Production method for aluminum alloy ingot, continuously cast aluminum alloy rod, and forged aluminum alloy product
A method with controlled composition and two-step melting process addresses the issue of coarsely grown Al-Fe-Mn-Si compounds in aluminum alloy production, enhancing mechanical properties and corrosion resistance of ingots and forged products.
Patent Information
- Application Number
- JP2023084135
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
AI Technical Summary
The utilization of aluminum alloy scrap in producing aluminum alloys results in the formation of coarsely grown Al-Fe-Mn-Si compounds during melting and casting, which deteriorates the mechanical properties of the final product.
A method involving specific composition ranges of Cu, Mg, Si, Mn, Fe, Cr, Ti, B, and Zr in the aluminum alloy, combined with a two-step melting and casting process, including a primary and secondary melting process, to control the growth of Al-Fe-Mn-Si compounds and improve mechanical properties.
The method effectively suppresses the coarsening of Al-Fe-Mn-Si compounds, resulting in aluminum alloy ingots, continuously cast rods, and forged products with enhanced mechanical properties and corrosion resistance.
Smart Images

Figure 2024167799000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an aluminum alloy ingot, a continuously cast aluminum alloy rod, and an aluminum alloy forged product. [Background technology]
[0002] In recent years, amid the global trend toward carbon neutrality, reducing CO2 emissions from manufacturing processes has become an issue. In order to reduce CO2 emissions during aluminum production, it is important to utilize scrap aluminum alloys, which have a lower melting point than pure aluminum (purity of 99.0% or more), in order to improve the energy consumption rate during melting.
[0003] Methods for manufacturing aluminum alloys and aluminum alloy products using aluminum alloy scrap as a raw material are known (e.g., Patent Documents 1 to 3). Aluminum alloy scrap is recovered from used aluminum products, and is produced as a recycled raw material by melting and adjusting the composition, and is used as the raw material for aluminum alloys. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2020-514556 [Patent Document 2] Special Publication No. 2020-527653 [Patent Document 3] JP 2022-137762 A Summary of the Invention [Problem to be solved by the invention]
[0005] When utilizing scrap aluminum alloys as raw materials for aluminum alloys derived from recycled materials, for example, when using scrap for 6000 series alloys, it is preferable to use scrap with a high purity, such as 6063 sash scraps generated from building materials. However, impurities such as Si, Fe, and Mn are mixed in from the scrap. If these compounds (e.g. Al-Fe-Mn-Si) grow coarsely and are present in the cast rod during the melting and casting process, the mechanical properties of the product will decrease.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing a 6000 series aluminum alloy ingot, which can utilize aluminum alloy scrap available on the market in the production of aluminum alloys while suppressing coarsening of Al-Fe-Mn-Si compounds generated by elements mixed in from the aluminum alloy scrap, a continuously cast aluminum alloy rod, and an aluminum alloy forged product. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention provides the following means.
[0008] A first aspect of the present invention is an aluminum alloy for producing an aluminum alloy ingot containing additive elements in the range of 0.30 mass% to 1.0 mass%, Cu in the range of 0.80 mass% to 1.8 mass%, Si in the range of 0.90 mass% to 1.9 mass%, Mn in the range of 0.30 mass% to 1.2 mass%, Fe in the range of 0.20 mass% to 0.65 mass%, Zn in the range of 0.25 mass% or less, Cr in the range of 0.050 mass% to 0.30 mass%, Ti in the range of 0.01 mass% to 0.1 mass%, B in the range of 0.0010 mass% to 0.030 mass%, and Zr in the range of 0.0010 mass% to 0.050 mass%, with the balance being Al and unavoidable impurities. The method for producing an aluminum alloy ingot includes a primary casting step in which the primary molten metal obtained in the primary melting step is used to solidify an ingot into an ingot, the primary casting step being performed at a cooling rate from the liquidus temperature to the solidus temperature of a final solidification portion of the ingot of 10° C. / sec or more, and a secondary melting step in which metallic Si or a Si-containing alloy is added to the molten metal obtained in the primary casting step to melt the ingot obtained in the primary casting step, thereby adjusting the Si content to within the range of 0.90% by mass or more and 1.9% by mass or less.
[0009] A second aspect of the present invention is the method for producing an aluminum alloy ingot according to the first aspect, wherein the aluminum alloy scrap is one or more of scrap containing a 3000 series alloy, scrap containing a 4000 series alloy, scrap containing a 5000 series alloy, and scrap containing a 6000 series alloy.
[0010] A third aspect of the present invention is a continuously cast aluminum alloy rod obtained by using an aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to the first or second aspect, and having a 0.2% yield strength of 350 MPa or more.
[0011] A fourth aspect of the present invention is an aluminum alloy forging obtained by using the continuously cast aluminum alloy rod according to the third aspect, and having a 0.2% yield strength of 370 MPa or more. Effect of the Invention
[0012] According to the manufacturing method of an aluminum alloy ingot of the present invention, it is possible to provide a manufacturing method of a 6000 series aluminum alloy ingot that can utilize aluminum alloy scrap available on the market while suppressing coarsening of Al-Fe-Mn-Si compounds generated by elements mixed in from the aluminum alloy scrap. [Brief description of the drawings]
[0013] [Figure 1] (a) is a conceptual diagram of the case where the primary molten metal obtained in the primary melting process is solidified into an ingot and then the ingot is fed into the secondary melting process, and (b) is a conceptual diagram of the case where the primary molten metal obtained in the primary melting process is fed directly into the secondary melting process. [Diagram 2] FIG. 2 is a cross-sectional schematic view of a continuous casting mold for a vertical continuous casting apparatus. [Diagram 3] FIG. 2 is a cross-sectional schematic view of a horizontal continuous casting device. [Figure 4] FIG. 1( a ) is a schematic diagram illustrating a portion of a continuously cast aluminum alloy rod according to the present embodiment where the structure is observed, and FIG. 1( b ) is a schematic diagram illustrating a portion of a continuously cast aluminum alloy rod according to the present embodiment where the tensile properties are evaluated. [Diagram 5] FIG. 2 is a schematic diagram for explaining the preparation of a forging for evaluating the tensile properties of the aluminum alloy forging of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In addition, the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality. Furthermore, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not necessarily limited to them, and may be appropriately modified and implemented within the scope that does not change the effects of the present invention.
[0015] [Method of manufacturing aluminum alloy ingots] An aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to this embodiment will be described. The aluminum alloy ingot of this embodiment contains additive elements in the range of 0.30 mass% or more and 1.0 mass% or less, Cu in the range of 0.80 mass% or more and 1.8 mass% or less, Si in the range of 0.90 mass% or more and 1.9 mass% or less, Mn in the range of 0.30 mass% or more and 1.2 mass% or less, Fe in the range of 0.20 mass% or more and 0.65 mass% or less, Zn in the range of 0.25 mass% or less, Cr in the range of 0.050 mass% or more and 0.30 mass% or less, Ti in the range of 0.01 mass% or more and 0.1 mass% or less, B in the range of 0.0010 mass% or more and 0.030 mass% or less, Zr in the range of 0.0010 mass% or more and 0.050 mass% or less, with the balance being Al and unavoidable impurities.
[0016] The aluminum alloy ingot of this embodiment corresponds to a forged product of a 6000 series aluminum alloy in that it contains Mg and Si.
[0017] (Cu: 0.30 mass% or more, 1.0 mass% or less) Cu has the effect of finely dispersing Mg-Si compounds in the aluminum alloy and the effect of improving the tensile strength of the aluminum alloy by precipitating as Al-Cu-Mg-Si compounds including the Q phase. By keeping the Cu content within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.
[0018] (Mg: 0.80 mass% or more, 1.8 mass% or less) Mg has the effect of improving the tensile strength of aluminum alloys. Mg contributes to strengthening of aluminum alloys by dissolving in the aluminum parent phase or precipitating as Mg-Si compounds (Mg2Si) such as β” phase, or Al-Cu-Mg-Si compounds (AlCuMgSi) such as Q phase. Mg2Si also has the effect of suppressing the formation of CuAl2 phase in the aluminum alloy. Suppressing the formation of CuAl2 phase improves the corrosion resistance of aluminum alloy ingots. By keeping the Mg content within the above range, it is possible to improve the corrosion resistance as well as the mechanical properties at room temperature of the aluminum alloy ingot.
[0019] (Si: 0.90 mass% or more, 1.9 mass% or less) Like Mg, Si has the effect of improving the mechanical properties and corrosion resistance of an aluminum alloy ingot at room temperature. However, if an excessive amount of Si is added to an aluminum alloy, coarse primary crystal Si grains may crystallize, which may reduce the tensile strength of the aluminum alloy. By keeping the Si content within the above range, it is possible to improve the mechanical properties and corrosion resistance of an aluminum alloy ingot at room temperature while suppressing the crystallization of primary crystal Si.
[0020] (Mn: 0.30 mass% or more, 1.2 mass% or less) Mn has the effect of improving the tensile strength of the aluminum alloy by forming fine granular precipitates including intermetallic compounds such as Al-Mn-Fe-Si and Al-Mn-Cr-Fe-Si in the aluminum alloy. By keeping the Mn content within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.
[0021] (Fe: 0.20 mass% or more, 0.65 mass% or less) Fe has the effect of improving the tensile strength of the aluminum alloy by crystallizing in the aluminum alloy as fine crystals including intermetallic compounds such as Al-Mn-Fe-Si, Al-Mn-Cr-Fe-Si, Al-Fe-Si, Al-Cu-Fe, and Al-Mn-Fe. By keeping the Fe content within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved. The Fe / Mn relationship is less than 1.4. By having the Fe / Mn relationship be less than 1.4, crystallization of AlFeSi-based compounds having sizes of 2.0 μm or more can be suppressed, and mechanical properties can be improved.
[0022] (Cr: 0.050 mass% or more, 0.30 mass% or less) Cr has the effect of improving the tensile strength of the aluminum alloy by forming fine granular crystallized products containing intermetallic compounds such as Al-Mn-Cr-Fe-Si and Al-Fe-Cr in the aluminum alloy. By keeping the Cr content within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.
[0023] (Ti: 0.010 mass% or more, 0.10 mass% or less) Ti has the effect of refining the crystal grains of an aluminum alloy and improving the wrought workability. If the Ti content is less than 0.010% by mass, the effect of refining the crystal grains may not be sufficiently obtained. On the other hand, if the Ti content exceeds 0.10% by mass, coarse crystallized products may be formed, and the wrought workability may be deteriorated. In addition, if a large amount of coarse crystallized products containing Ti are mixed into an aluminum alloy ingot, the toughness may be deteriorated. Therefore, the Ti content is set to 0.010% by mass or more and 0.10% by mass or less. The Ti content is preferably 0.015% by mass or more and 0.050% by mass or less.
[0024] (B: 0.0010 mass% or more, 0.030 mass% or less) B has the effect of refining the crystal grains of the aluminum alloy and improving the wrought workability. By adding B to the aluminum alloy together with Ti, the effect of refining crystal grains is improved. If the content of B is less than 0.0010% by mass, the effect of refining crystal grains may not be sufficiently obtained. On the other hand, if the content of B exceeds 0.030% by mass, coarse crystallized matter may be formed and may be mixed into the aluminum alloy ingot as inclusions. In addition, if a large amount of coarse crystallized matter containing B is mixed into the final product of the aluminum alloy, the toughness may decrease. Therefore, the content of B is set to 0.0010% by mass or more and 0.030% by mass. The content of B is preferably 0.0050% by mass or more and 0.025% by mass.
[0025] (Zr: 0.0010 mass% or more, 0.050 mass% or less) When the Zr content is 0.050% by mass or less, it precipitates in the form of Al3Zr and Al-(Ti,Zr), which contributes to improving the strength of the aluminum alloy ingot through recrystallization suppression effect and precipitation strengthening. However, when the Zr content exceeds 0.050% by mass, it crystallizes as coarse Zr compounds, which may lead to a decrease in the corrosion resistance of the aluminum alloy ingot. For this reason, the Zr content is set to 0.050% by mass or less. In order to obtain the above-mentioned recrystallization suppression effect and the effect of improving the strength of the forged product through precipitation strengthening, the Zr content is preferably 0.0010% by mass or more.
[0026] (Zn: 0.250% by mass or less) The Zn content may be 0.250% by mass or less. If the Zn content exceeds 0.250% by mass, MgZn2 is generated and precipitates from the Al matrix to the grain boundaries, causing intergranular corrosion and leading to a decrease in the corrosion resistance of the aluminum alloy ingot. For this reason, it is preferable that the Zn content is 0.250% by mass or less, or that it is not contained at all.
[0027] (Inevitable impurities) Inevitable impurities are impurities that are inevitably mixed into the aluminum alloy from the raw materials or manufacturing process of the aluminum alloy ingot. Examples of inevitable impurities include Ni, Sn, Be, etc. The content of these inevitable impurities preferably does not exceed 0.1 mass%.
[0028] [Method of manufacturing aluminum alloy ingots] Next, a method for producing an aluminum alloy ingot according to this embodiment will be described. The aluminum alloy ingot of this embodiment can be manufactured by, for example, a method including a melting (molten metal formation) step and a casting step. Here, the aluminum alloy ingot of this embodiment is characterized in that the melting step has two sub-steps (a first melting step and a second melting step) and the casting step also has two sub-steps (a first casting step and a second casting step (main casting step)). These sub-steps are performed in the order of the first melting step → the first casting step → the second melting step → the second casting step.
[0029] Both the primary casting process and the secondary melting process have in common that they are processes for forming molten aluminum alloy. Both the primary and secondary casting processes have in common the fact that they are processes for producing aluminum alloy ingots (rods).
[0030] <1st dissolution process> In the primary melting step, a raw material containing aluminum alloy scrap, in which the content ratio of the above-mentioned additive elements (Cu, Mg, Mn, Fe, Zn, Cr, Ti, B, Zr) is within the same composition range as that of the aluminum alloy ingot to be produced, except that the content ratio of Si is 0.60 mass% or more and 0.90 mass% or less, is melted to obtain a primary molten metal.
[0031] FIG. 1 is a diagram conceptually showing a part of the method for producing an aluminum alloy ingot according to the present embodiment. Specifically, this is a diagram conceptually illustrating a flow in which raw materials including blended aluminum alloy scrap are prepared, the raw materials are then charged into a primary melting furnace to carry out a primary melting process to obtain a primary molten metal, the primary molten metal is temporarily solidified into an ingot, and the ingot is used as a raw material to carry out a secondary melting process in a secondary melting furnace to obtain a secondary molten metal.
[0032] The primary melting process is carried out under conditions such that the input raw materials (ingredients) are completely melted. The raw materials include aluminum alloy scrap, aluminum ingot, Cu scrap, mother alloy, etc., and are melted at, for example, 780 to 850°C. Examples of aluminum alloy scrap include scrap of Al-Mn-based (3000 series) alloys, such as aluminum cans and recycled aluminum can blocks, scrap of Al-Si-based (4000 series) alloys, such as ADC12 and A356, scrap of Al-Mg-based (5000 series) alloys, such as 5052 and 5083, and scrap of Al-Mg-Si-based (6000 series) alloys, such as 6063 and 6061. Aluminum bullion (pure aluminum) is classified into normal purity bullion, high purity bullion, and alloy bullion based on its purity and composition, and can be divided into ingots (cast metal for general raw material use), slabs (cast metal prepared for rolling), billets (cast metal prepared for extrusion), etc. based on its shape and use.
[0033] When the Si content is less than 0.60 mass%, for example, the Si content is adjusted to within the range of 0.60 mass% to 0.90 mass% by adding metal Si or a Si-containing alloy. Metal Si is preferred as the additive material because it is easy to adjust. When the Si content exceeds 0.90% by mass, aluminum ingot or aluminum alloy scrap with a low Si content is added to adjust the Si content to within a range of 0.60% to 0.90% by mass. Examples of aluminum alloy scrap with a low Si content include 3000 series alloy scrap, scrap containing 5000 series alloy, and scrap containing 6000 series alloy. The Si content (component analysis) can be carried out, for example, by emission spectrometry.
[0034] When Si, Fe, and Mn are mixed in scrap and melted, Al-Fe-Mn-Si compounds are generated at a certain temperature range during the melting process. The amount of this compound is particularly affected by the amount of Si. If the amount of compound increases, it is necessary to set the melting temperature to 850°C or higher in order to melt them. This is not desirable because it increases the energy used during melting. Furthermore, if the Si content falls below 0.6 mass%, the amount of Si added in the secondary melting step will be too large, and it will take time for all the added Si to melt, resulting in energy loss. Therefore, the Si content of the alloy composition obtained in the primary melting step must be 0.60 mass% or more and 0.90 mass% or less.
[0035] The higher the usage ratio (mixture ratio) of aluminum alloy scrap in the raw materials, the more preferable it is in terms of improving the energy consumption rate during melting. The blending ratio of the aluminum alloy scrap can be, for example, 50% or more. For example, it can be 60% or more, 70% or more, 80% or more, 90% or more, or 100%. On the other hand, the blending ratio of the aluminum alloy scrap can be less than 50%, for example, 40%, 30%, 20%, or 10%, although the effect of improving the energy consumption rate during melting is reduced.
[0036] The melting point of pure aluminum ingot is approximately 660°C. In contrast, ADC12, for example, has a melting point of 570°C, and even other aluminum alloys have melting points below 650°C, which is more than 10°C lower. This makes it easier to melt, and by utilizing this, the energy consumption during melting can be improved.
[0037] The aluminum alloy scrap can be used within the composition range of Al-Si (4000 series) alloys such as ADC12 and A356 containing 4 mass% to 12 mass% Si and 0.01 mass% to 3.0 mass% Cu, Al-Mn (3000 series) alloys containing 0.7 mass% to 1.4 mass% Mn and 0.5 mass% to 1.4 mass% Mg such as other aluminum cans and recycled aluminum can chunks, Al-Mg (5000 series) alloys such as 5052 and 5083 containing 2.0 mass% to 5.0 mass% Mg, and Al-Mg-Si (6000 series) alloys such as 6063 and 6061 containing 0.2 mass% to 0.8 mass% Si and 0.45 mass% to 1.2 mass% Mg. Aluminum can scraps are usually used after undergoing a heat treatment process at 400 to 500 degrees Celsius to remove the paint from the surface of the cans before being melted down. By adding an Al-Si alloy, the amount of Si added in the secondary melting process can be reduced, so it is preferable to use this in combination with scrap of other alloys.
[0038] <First casting process> The primary casting process is a process in which the primary molten metal obtained in the primary melting process is solidified into an ingot. During this process, the cooling rate from the liquidus temperature to the solidus temperature of the final solidification part of the ingot is 10°C / sec or more. The cooling rate of the final solidification part was measured by using a thermocouple to measure the temperature at the center of the ingot, which is the final solidification part. The cooling rate from the liquidus temperature to the solidus temperature was calculated. For example, a K type thermocouple (positive electrode: chromel, negative electrode: alumel) can be used.
[0039] Here, as is well known, the "finally solidified portion" of the ingot refers to the portion of the molten metal where solidification is complete. When the molten metal is poured into a mold, it is cooled and solidifies from the vicinity of the wall surface of the mold, and the molten metal at the opening surface of the mold is the last to solidify. This last solidified portion is the "finally solidified portion." In this specification, the "finally solidified portion" refers to the portion of the molten metal remaining in the mold that finally solidifies after 95% of the volume of the molten metal has solidified.
[0040] The approximate position of the "final solidification part" is shown using the vertical continuous casting apparatus shown in FIG. 2 and the horizontal (horizontal) continuous casting apparatus shown in FIG.
[0041] The continuous casting mold 200 of the vertical continuous casting machine shown in FIG. 2 is cylindrical with both ends of the molding hole 11 having a circular cross section and is composed of a cylindrical mold body 200A and a cylindrical carbon ring 200B on the inner peripheral surface 200Aa of the mold body 200A, which is fitted into the molding hole 11. One end of the molding hole 11 is an inlet 12 for the molten metal M, and the other end is a casting outlet 13 for the ingot S. The mold body 200A has a cavity 21 for circulating cooling water C inside, an inlet 22 to the cavity 21 is provided at the top, and an outlet 23 is provided surrounding the casting outlet 13. The cooling water C introduced from the inlet 22 is primarily cooled and solidified through the carbon ring 200B, and is sprayed onto the ingot S being cast from the outlet 23 to perform secondary cooling of the ingot S. Further, a recess 26 having a thickness equivalent to that of the carbon ring 200B is formed in an area of the inner peripheral surface 200Aa of the mold body 200A excluding a part on the casting outlet 13 side. In FIG. 2, the symbol S fは The final solidification part is indicated by the symbol T h indicates the location where the temperature is measured with a thermocouple to measure the cooling rate of the final solidification portion.
[0042] A horizontal continuous casting apparatus 2000 shown in Fig. 3 includes a molten metal receiving section (not shown) having a tap port on its side wall, a molten metal pouring nozzle 20 having a molten metal pouring passage having a circular cross section, and a continuous casting mold 400 having a cylindrical mold body 400A having a molding hole 41 having a circular cross section. The continuous casting mold 400 shown in Fig. 3 includes a cylindrical mold body 400A having an injection port 12 for molten metal at one end and an outlet 13 for casting an ingot at the other end, and a carbon ring 400B disposed on an inner peripheral surface 400Aa of the mold body 400A so as to be fitted into the molding hole 41. A lubricating oil supply pipe 43 opening into the molding hole 41 is provided on the inlet side of the molding hole 41. The mold body 400A has a cavity 42 through which cooling water C flows, and a jet outlet 44 is provided surrounding the casting outlet 13. The cooling water C introduced from an inlet (not shown) flows through the cavity 42, primarily cooling and solidifying the molten metal M in the forming hole 41 via the mold body 400A and the carbon ring 400B, and is sprayed onto the ingot S being cast out from the jet outlet 44, thereby secondary cooling the ingot S. In addition, a recess corresponding to the thickness of the carbon ring 400B is formed in an area of the inner peripheral surface 400Aa of the mold body 400A excluding a part on the casting outlet 13 side. In FIG. 3, the symbol S fは The final solidification part is indicated by the symbol T h indicates the location where the temperature is measured with a thermocouple to measure the cooling rate of the final solidification portion.
[0043] Specifically, the first casting process is a process in which the molten metal obtained in the first melting process is poured into a mold such as cast iron to cast the ingot when the molten metal obtained in the first melting process is solidified into an ingot. At this time, the temperature of the mold is controlled so that the cooling rate of the final solidification part of the ingot is 10°C / sec or more. Casting may be performed by pouring the molten metal into a stationary mold to solidify it, or vertical continuous casting may be performed. When the molten metal is cast into a stationary mold, the mold temperature can be 200°C or less, and preferably 100°C or less. If the cooling rate exceeds 10°C / sec, Al-Fe-Mn-Si-based compounds grow coarsely in the final solidification part, and these compounds will not decompose unless they are melted at a temperature exceeding 800°C in the second melting process. If the secondary melting process and casting are carried out without disassembling the material, unmelted Al-Fe-Mn-Si compounds will remain in the product and impair its mechanical properties. When melting is performed at a temperature exceeding 800°C, oxidation consumption during melting is accelerated, resulting in large material loss.
[0044] <Secondary melting process> The secondary melting process is a process in which metal Si or a Si-containing alloy is added to the molten metal obtained by melting the ingot obtained in the primary casting process to adjust the Si content to 0.90% by mass or more and 1.9% by mass. Metal Si is preferable as the additive material because it is easy to adjust.
[0045] The composition adjustment here is carried out at a temperature of 700°C or higher and 800°C or lower. If the temperature is below 700°C, the Al-Fe-Mn-Si compounds will grow coarsely due to the temperature drop in the molten metal path when the molten metal is cast, impairing the mechanical properties of the product. Also, if the temperature exceeds 800°C, the amount of hydrogen dissolved in the air increases in the molten aluminum, increasing the amount of hydrogen gas in the molten metal, resulting in porosity in the cast product and impairing the mechanical properties. Therefore, the temperature should be between 700°C and 800°C.
[0046] <Secondary casting process (main casting process)> The molten metal obtained in the secondary melting process is flux-treated, then undergoes GBF (gas bubbling filtration) treatment before being poured into a casting mold. The poured molten metal is continuously cast by either vertical continuous casting or horizontal continuous casting to obtain an aluminum alloy continuously cast rod.
[0047] [Aluminum alloy continuous casting rod] The continuously cast aluminum alloy rod of this embodiment is produced by carrying out continuous casting using an aluminum alloy ingot obtained by the method for producing an aluminum alloy ingot of this embodiment, by either vertical continuous casting or horizontal continuous casting, and has a 0.2% yield strength of 350 MPa or more.
[0048] [Aluminum alloy forgings] The aluminum alloy forged product according to this embodiment is manufactured using the aluminum alloy continuously cast rod according to this embodiment, and has a 0.2% yield strength of 370 MPa or more. For example, the aluminum alloy continuously cast rod according to the present embodiment can be subjected to a homogenization heat treatment step, a forging step, a solution treatment step, a quenching treatment step, and an aging treatment step to produce the aluminum alloy forged product according to the present embodiment. EXAMPLES
[0049] Next, specific examples of the present invention will be described, but the present invention is not limited to these examples.
[0050] (Example of aluminum alloy scrap) The component analysis values (mass%) of each scrap obtained by optical emission spectroscopy of aluminum alloy scrap obtained from secondary alloy manufacturers and scrap manufacturers are shown in Table 1. The component analysis was carried out in accordance with the optical emission spectroscopy analysis of aluminum and aluminum alloys specified in JIS H1305 2005.
[0051] [Table 1]
[0052] (Examples 1 to 6, Comparative Examples 1 to 6) The compositions of the samples of Examples 1 to 6 and Comparative Examples 1 to 6 are as follows. In Examples 1 to 6, the combination (mixture) of aluminum alloy scrap and aluminum ingot shown in Table 1, or only aluminum alloy scrap was used as the raw material. In both the examples and comparative examples, the contents of additive elements other than Si were as follows: Cu was in the range of 0.30 mass% or more and 1.0 mass% or less, Mg was in the range of 0.80 mass% or more and 1.8 mass% or less, Mn was in the range of 0.30 mass% or more and 1.2 mass% or less, Fe was in the range of 0.20 mass% or more and 0.65 mass% or less, Zn was in the range of 0.25 mass% or less, Cr was in the range of 0.050 mass% or more and 0.30 mass% or less, Ti was in the range of 0.01 mass% or more and 0.1 mass% or less, B was in the range of 0.0010 mass% or more and 0.030 mass% or less, and Zr was in the range of 0.0010 mass% or more and 0.050 mass% or less, with the balance being Al and unavoidable impurities. Furthermore, in the examples, the Si content was blended so as to be within the range of 0.60 mass% or more and 0.90 mass% or less, whereas in the comparative examples, the Si content was blended so as to be outside the range of 0.60 mass% or more and 0.90 mass% or less.
[0053] In both the examples and comparative examples, the melting step and the casting step were carried out using a vertical continuous casting apparatus. In the examples, the molten metal obtained in the primary melting step was once poured into a cast iron mold to perform pouring casting to obtain an ingot. When casting into an ingot, casting was performed so that the cooling rate of the final solidified portion was 10°C / sec or more. Specifically, a 5 kg ingot was cast with a mold temperature of 200°C or less. On the other hand, in the comparative examples, when casting into an ingot from the molten metal obtained in the primary melting step, casting was performed so that the cooling rate of the final solidified portion exceeded 10°C / sec. Specifically, a 5 kg ingot was cast with a mold temperature exceeding 200°C. The cooling rate of the final solidification part was measured using a K-type thermocouple at the center of the ingot, which was the final solidification part, as shown in Figure 2, and the cooling rate from the liquidus temperature to the solidus temperature was calculated.
[0054] For each of the examples and comparative examples, the ingots obtained in the first casting process were used to carry out melting and component adjustment in the second melting process. The second melting was carried out at 780°C. After the raw materials were melted, a jig was used to check for the presence or absence of hearth sediment (residual matter at the hearth). The resulting molten metal was then used to carry out casting in the main casting process to obtain a continuously cast rod.
[0055] The casting conditions for this casting process were as follows; Casting diameter: φ82mm Casting speed: 230mm / min Cooling water amount: 30L / min Casting temperature: 720℃
[0056] <Evaluation after the second dissolution process> As mentioned above, the presence or absence of hearth bottom deposits (Al-Fe-Mn-Si compounds) was confirmed after the secondary melting at 780℃. Those without hearth bottom deposits were marked with an ◯, and those with deposits were marked with an X. An iron stirring tool was used to check for hearth bottom deposits. When the stirring tool came into contact with hearth bottom deposits, it felt like hitting a pebble.
[0057] <Evaluation of Continuously Cast Rods (Tensile Properties)> The tensile properties of the obtained continuously cast aluminum alloy rod 10 were measured by the following method. The tensile properties are evaluated in accordance with the ASTM-E8 standard. That is, referring to Fig. 4(a) and Fig. 4(b), a tensile test specimen having a gauge length of 25.4 mm and a parallel part diameter of 6.4 mm is taken from a central portion 10b extending in the casting direction of a continuously cast aluminum alloy rod 10. The obtained test specimen is subjected to a tensile test at room temperature (25°C) at a speed of 2 mm / min to measure the 0.2% proof stress. The results are shown in Table 2.
[0058] <Evaluation of forged products (tensile properties)> As shown in FIG. 5, a continuously cast aluminum alloy rod 10 having a diameter of φ82 mm was upset from its side to a thickness of 41 mm, and the 50% upset product was subjected to T6 treatment under the following conditions and then subjected to a tensile test: ·Forging conditions: Forging temperature 520℃ · T6 treatment conditions: 3 hours at 540℃ (solution treatment) → hardening process (water temperature 40℃) → 6 hours at 180℃ (aging treatment process). The tensile test piece was subjected to a tensile test at room temperature (25° C.) at a rate of 2 mm / min to measure the 0.2% yield strength. The results are shown in Table 2.
[0059] [Table 2]
[0060] As can be seen from Table 2, after the secondary melting process, no hearth deposits (Al-Fe-Mn-Si compounds) were found in any of the Examples, whereas hearth deposits (Al-Fe-Mn-Si compounds) were found in all of the Comparative Examples. Furthermore, all of the continuously cast aluminum alloy rods of Examples had a 0.2% yield strength of 350 MPa or more, whereas all of the continuously cast aluminum alloy rods of Comparative Examples had a 0.2% yield strength of less than 350 MPa. Moreover, all of the aluminum alloy forged products of the examples had a 0.2% yield strength of 370 MPa or more, whereas all of the aluminum alloy continuous forged products of the comparative examples had a 0.2% yield strength of less than 350 MPa. [Explanation of symbols]
[0061] 10. Aluminum alloy continuous cast rod
Claims
1. 1. A method for producing an aluminum alloy ingot comprising additive elements in the range of Cu from 0.30 to 1.0 mass%, Mg from 0.80 to 1.8 mass%, Si from 0.90 to 1.9 mass%, Mn from 0.30 to 1.2 mass%, Fe from 0.20 to 0.65 mass%, Zn from 0.25 mass%, Cr from 0.050 to 0.30 mass%, Ti from 0.01 to 0.1 mass%, B from 0.0010 to 0.030 mass%, and Zr from 0.0010 to 0.050 mass%, with the balance being Al and unavoidable impurities, a primary melting step of melting a raw material containing aluminum alloy scrap, the raw material having a Si content of 0.60% by mass or more and 0.90% by mass or less and other contents of the additive elements being in the same composition range as the aluminum alloy ingot, to obtain a primary molten metal; a primary casting process for solidifying the primary molten metal obtained in the primary melting process into an ingot, the primary casting process being performed at a cooling rate from a liquidus temperature to a solidus temperature of a final solidification portion of the ingot of 10° C. / sec or more; and a secondary melting step of adding metallic Si or a Si-containing alloy to the molten metal obtained by melting the ingot obtained in the primary casting step to adjust the Si content ratio to be within the range of 0.90% by mass or more and 1.9% by mass or less.
2. 2. The method for producing an aluminum alloy ingot according to claim 1, wherein the aluminum alloy scrap comprises at least one of scrap containing a 3000 series alloy, scrap containing a 4000 series alloy, scrap containing a 5000 series alloy, and scrap containing a 6000 series alloy.
3. 3. A continuously cast aluminum alloy rod obtained by using an aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to claim 1 or 2, and having a 0.2% yield strength of 350 MPa or more.
4. 4. An aluminum alloy forging obtained by using the aluminum alloy continuously cast rod according to claim 3, the aluminum alloy forging having a 0.2% yield strength of 370 MPa or more.
Citation Information
Patent Citations
Casting recycled aluminum scrap
JP2020514556A
High performance aluminum alloy with a large amount of recycled materials and method for making same
JP2020527653A
Manufacturing method of aluminum alloy forging material
JP2022137762A