Method of producing photosensitive resin coated film, method of manufacturing display, method of producing color filter, and photosensitive resin composition
By optimizing post-baking conditions through defined tangents of inclination angles, the method addresses residual film rate and baking temperature issues, ensuring uniformity and adhesion in photosensitive resin coatings for large-area products.
Patent Information
- Application Number
- JP2023084273
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods fail to address the relationship between residual film rate and baking temperature during post-baking after exposure and development, leading to inconsistent coating film thickness and adhesion issues, particularly in large-area products like displays and color filters, due to in-plane temperature variations.
A method for producing a photosensitive resin coating film that involves specific post-baking conditions defined by tangents of inclination angles in residual film rate, light transmittance, and exposure curves, ensuring uniform film thickness and adhesion by optimizing post-bake temperatures and exposure amounts.
This method reduces in-plane temperature variations, improves coating film uniformity, enhances productivity, and maintains quality in large-area products by stabilizing the post-baking process.
Smart Images

Figure 2024167940000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a photosensitive resin coating film, which comprises coating a substrate with a photosensitive resin composition and then exposing and developing the composition to form a pattern. In particular, the present invention relates to a method for producing a photosensitive resin coating film, which focuses on the relationship between the post-bake remaining film rate of the photosensitive resin coating film and the post-bake temperature in the post-bake step following the exposure and development to form a pattern. [Background technology]
[0002] Previously, there were inventions in cited documents 1 and 2 that focused on the relationship between the remaining film rate of the coating film and the bake temperature. The invention in cited document 1 is an invention of a method for revealing and evaluating the heat treatment effect actually received by the resist film in the resist film baking process. Area B in Figure 1 is an area where the effect of the in-plane temperature variation is small, and especially point C where the relationship between the two shows an extreme value. It is described that the effect of in-plane temperature variation is smallest at this temperature, and that by adopting this temperature as the actual process baking temperature, a good resist pattern can be formed.
[0003] The invention in Cited Document 2 relates to a resist processing method for baking a resist and a method for manufacturing a substrate with a resist, and describes a process for performing pre-exposure baking under predetermined pre-exposure bake temperature conditions, performing a development process on the test resist layer after performing post-exposure baking under predetermined post-exposure bake temperature conditions, and obtaining a residual film ratio for each pre-exposure bake temperature condition and post-exposure bake temperature condition, and performing pre-exposure baking and post-exposure baking on a resist layer having the same composition as the test resist layer and formed on a substrate under temperature conditions in which the residual film ratio is 95% or more on a graph having a pre-exposure bake temperature axis and a post-exposure bake temperature axis, thereby maintaining a high residual film ratio in the unexposed part of the chemically amplified resist layer, and providing a high pattern contrast and high resolution in the exposed part after development relative to the unexposed part. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-189303 A [Patent Document 2] JP 2012-47828 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the content of the cited document 1 is a method for determining the resist pattern formation conditions in the process of cooling the resist film baked in the resist film baking process to room temperature and then exposing and developing the resist film, and there is no description whatsoever about the relationship between the remaining film rate of the coating film and the bake temperature, etc., in the post-bake process after exposure and development.
[0006] Similarly, the invention described in D2 also relates to a method for a pre-exposure bake (PB) treatment performed after the formation of a resist layer and before pattern exposure, and a post-exposure bake (PEB) treatment performed after pattern exposure and before development, but there is no description whatsoever of the relationship between the remaining film rate of the coating film and the bake temperature, etc., in the post-bake after exposure and development.
[0007] On the other hand, in a coating film formed by coating a photosensitive resin composition containing a polymerizable compound, some unreacted polymerizable compound remains even after heat treatment and development by the resist film baking step in the above-mentioned cited document 1 or the baking step before and after exposure in the above-mentioned cited document 2. If this remains, the desired performance cannot be obtained due to defects such as insufficient adhesion strength and resistance, and cracks are likely to occur due to changes over time. Therefore, it is desirable to reduce the remaining unreacted polymerizable compound as much as possible by performing a post-bake treatment.
[0008] However, even when post-baking is performed, if there is a large variation in temperature within the surface, unreacted polymerizable compound may remain locally, or the thickness of the final coating film may vary within the surface, resulting in problems of reduced productivity and quality. In particular, when manufacturing products such as displays and color filters, which have a larger substrate size than semiconductors and have strict tolerances for the thickness of the coating film, the yield rate is significantly reduced, and the above problem is serious. Furthermore, since post-baking takes time, in order to increase efficiency, each product is often stacked on a rack and baked all at once, which further increases the temperature variation, making the above problem even more serious.
[0009] The present invention focuses on the post-bake process after exposure and development, and aims to clarify the relationship between the post-bake film remaining rate after post-bake and the post-bake temperature, find a temperature range that is less affected by variations in in-plane temperature, and adopt that temperature range as the post-bake temperature in the actual manufacturing process, thereby providing a manufacturing method that can stably produce a good coating film. [Means for solving the problem]
[0010] In order to solve the above problems, the method for producing a photosensitive resin coating film of the present invention has the following features: That is, the first feature of the present invention is to coat a substrate with a photosensitive resin composition to form a coating film, and to heat the formed coating film at 700 mJ / cm 2 This is a method for producing a photosensitive resin coating film, which comprises exposing the coating film to the following exposure amount, developing the exposed coating film to form a pattern, and then post-baking the patterned coating film under the following conditions. -0.05≦α≦0.12 (α: a value defined as the tangent of the inclination angle of the tangent of a curve of post-bake film remaining rate vs. post-bake temperature, the curve being plotted with post-bake temperature as the horizontal axis and post-bake film remaining rate as the vertical axis) A second aspect of the present invention is a method for producing a photosensitive resin coating film, which comprises post-baking the patterned coating film under the following conditions: -0.010≦β≦0.015 (β: a value defined as the tangent of the inclination angle of the tangent of a curve of light transmittance after post-baking vs. post-baking temperature, the curve being obtained by plotting light transmittance after post-baking on the vertical axis and post-baking temperature on the horizontal axis) A third aspect of the present invention is a method for producing a photosensitive resin coating film, which comprises exposing the formed coating film under the following conditions: -0.8≦γ≦0.3 (γ: a value defined as the tangent of the inclination angle of the tangent of a curve plotted as a function of the post-bake residual film ratio vs. exposure amount, the curve being obtained by plotting the post-bake residual film ratio on the vertical axis and the exposure amount during the exposure on the horizontal axis) The fourth aspect of the present invention is a method for producing a photosensitive resin coating film in which the residual film ratio after post-baking is 0 to 0.5% at an exposure dose of 0.1% of the saturated exposure dose (the minimum exposure dose at which the residual film ratio after post-baking is 85% or more).The fifth aspect of the present invention is a method for producing a photosensitive resin coating film in which the color difference ΔEab before and after baking is 5.0 or less when the film is additionally baked at 100°C for 240 minutes after post-baking.
[0011] In a sixth aspect of the present invention, the area of the substrate is 0.4 to 16.0 m 2 The seventh and eighth aspects of the present invention are methods for producing displays and color filters to which the above-mentioned photosensitive resin coating film production method is applied.
[0012] The ninth aspect of the present invention is a photosensitive resin composition containing a specific polymerizable compound (A) and a specific polymerizable compound (B). The tenth to thirteenth aspects of the present invention are photosensitive resin compositions in which the total contents, weight average molecular weights, double bond equivalents, and weight part ratios of the specific polymerizable compound (A) and the specific polymerizable compound (B) are specified. The fourteenth and fifteenth aspects of the present invention are photosensitive resin compositions containing a specific photopolymerization initiator, which is further specified. Effect of the Invention
[0013] According to the method for producing a photosensitive resin coating film of the present invention, it is possible to reduce the temperature variation in the surface during post-baking, and the variation in the thickness of the final coating film in the surface can be reduced, which has the effect of improving productivity and quality. As a result, it is also applicable to the production of products in fields where the tolerance range for the thickness of the coating film is strict and the area is large.
[0014] Furthermore, according to the method for producing a photosensitive resin coating film of the present invention, the optimal and minimum post-bake temperature during post-baking and the optimal and minimum exposure dose during exposure can be accurately determined, making it possible to save on the amount of post-baking energy and the amount of exposure energy, which has the effect of enabling the method to be used as an ecological production method that leads to energy savings. [Brief description of the drawings]
[0015] [Figure 1] 1 is an example showing steps of a method for producing a photosensitive resin coating film in the first configuration of the present invention. [Diagram 2] 1 is an example of a curve of film remaining rate after post-bake versus post-bake temperature in the first configuration of the present invention. [Diagram 3] 1 is an example of a curve of light transmittance after post-baking versus post-baking temperature in the second configuration of the present invention. [Figure 4] 11 is another example of a curve of film remaining rate after post-bake versus post-bake temperature in the first configuration of the present invention. [Diagram 5] 1 is an example of a curve of light transmittance after post-baking versus post-baking temperature in the second configuration of the present invention. [Figure 6] 13 is an example of a post-post-bake residual film ratio vs. exposure curve in the third configuration of the present invention. [Figure 7] 13 is an example of a post-post-bake residual film ratio vs. exposure curve in the third configuration of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below with reference to the drawings. The first aspect of the present invention is a method for producing a photosensitive resin coating film 23, which comprises coating a substrate 1 with a photosensitive resin composition to form a coating film 20 (FIG. 1(a)), placing a photomask 3 on top of the coating film 20, and applying 700 mJ / cm 2 The method is characterized in that the coating film 21 is exposed to light at the following exposure dose (FIG. 1(b)), the exposed coating film 21 is developed to form a pattern (FIG. 1(c)), and then the patterned coating film 22 is post-baked under the following conditions (FIG. 1(d)). -0.05≦α≦0.12 (α: a value defined as the tangent of the inclination angle of the tangent of a curve of post-bake film remaining rate vs. post-bake temperature, the curve being plotted with post-bake temperature as the horizontal axis and post-bake film remaining rate as the vertical axis) The post-bake of the present invention refers to baking performed to thermally crosslink any unreacted polymerizable compound remaining after exposure and development to form a pattern, thereby improving adhesion and durability to the substrate, the post-bake temperature refers to the processing temperature during post-bake, and the remaining film rate (%) after post-bake refers to {(average thickness of photosensitive resin coating film 23 after post-bake / average thickness of coating film 20 before exposure)×100}. The average thickness of coating film 20 is the average value of values obtained by measuring five arbitrary points on the same surface of the target coating film 20 with a contact thickness gauge Dektak150 manufactured by Vecco.
[0017] The film remaining rate after post-bake versus post-bake temperature curve is obtained by plotting each measurement value with the film remaining rate after post-bake on the vertical axis and the post-bake temperature on the horizontal axis, and approximating the curve with a third-order polynomial, for example, as shown by the dotted lines in FIG. 2 and FIG. 4.
[0018] FIG. 2 is an example of a curve of film remaining rate after post-bake versus post-bake temperature in the first configuration of the present invention, and is an example of a curve of film remaining rate after post-bake versus post-bake temperature when the post-bake temperature is from 40° C. to 220° C.
[0019] FIG. 4 shows another example of the curve of the film remaining rate after post-bake versus the post-bake temperature in the first configuration of the present invention, which is an example of the curve of the film remaining rate after post-bake versus the post-bake temperature when the post-bake temperature is from 210° C. to 310° C.
[0020] This third-order polynomial approximation curve is a curve obtained by measuring at equal intervals under 5 to 10 temperature conditions, and measurement values showing performance deficiencies or obvious abnormalities, such as peeling of the photosensitive resin coating film 23 after post-baking, are excluded.
[0021] The tangent to the curve of film remaining rate after post-bake vs. post-bake temperature is the tangent T that touches each point on the curve as shown in Figures 2 and 4. The inclination angle of the tangent is the value of θ in Figures 2 and 4 (variation in film remaining rate after post-bake / variation in post-bake temperature), and the value α defined as the tangent of θ (i.e., tan θ) is positive on the curves that slope downward to the right in Figures 2 and 4, and is negative on the curves that slope upward to the right, with the value of α being 0 at the maximum point of the curve.
[0022] As a result of the verification, it was found that in the post-bake temperature range where α is from -0.05 to 0.12, the film remaining ratio after post-bake is maintained at a high value, and the change in the film remaining ratio is small even if the post-bake temperature fluctuates slightly. Therefore, if the post-bake temperature is set within this range during manufacturing, it is possible to form the photosensitive resin coating film 23 with a uniform and thick final thickness even if there is some variation in the in-plane temperature.
[0023] The post-baking device may be any device capable of controlling the temperature, such as a high-temperature dryer, oven, or hot plate, and is preferably equipped with a fan.
[0024] Next, the second aspect of the present invention is a method for producing a photosensitive resin coating film 23, which is characterized in that the coating film 22 on which the pattern has been formed (FIG. 1(c)) is post-baked under the following conditions (FIG. 1(d)).
[0025] -0.010≦β≦0.015 (β: a value defined as the tangent of the inclination angle of the tangent of a curve of light transmittance after post-baking vs. post-baking temperature, the curve being obtained by plotting light transmittance after post-baking on the vertical axis and post-baking temperature on the horizontal axis) The light transmittance (%) after post-baking is the average value obtained by measuring any five points on the same surface of the photosensitive resin coating film 23 after post-baking using a CF substrate optical inspection device (LCF-100MA_SF;) manufactured by Otsuka Electronics Co., Ltd.
[0026] The post-post-bake light transmittance vs. post-bake temperature curve is a curve as shown by the dotted lines in Figs. 3 and 5, which is obtained by plotting each measured value with the post-post-bake light transmittance on the y-axis and the post-bake temperature on the x-axis, and approximating the curve with a third-order polynomial.
[0027] FIG. 3 is an example of a curve of light transmittance after post-baking vs. post-baking temperature in the second configuration of the present invention, in which the curve shows light transmittance after post-baking vs. post-baking temperature at post-baking temperatures of 40° C. to 220° C.
[0028] FIG. 5 is an example of a curve of light transmittance after post-baking vs. post-baking temperature in the second configuration of the present invention, and is an example of a curve of light transmittance after post-baking vs. post-baking temperature in the post-baking temperature range of 210° C. to 310° C.
[0029] This third-order polynomial approximation curve is also a curve obtained by measuring at equal intervals under 5 to 10 temperature conditions, and measurement values showing performance deficiencies or obvious abnormalities, such as peeling of the photosensitive resin coating film 23 after post-baking, are excluded.
[0030] Moreover, the tangent T of the curve of light transmittance after post-bake vs. post-bake temperature is the tangent that touches each point on the curve as shown in Figures 3 and 5. The inclination angle of the tangent is the value of θ in Figures 3 and 5 (fluctuation in light transmittance after post-bake / fluctuation in post-bake temperature), and the value β defined as the tangent of θ (i.e., tan θ) is positive on the curve that slopes downward to the right in Figures 3 and 5, and α is negative on the curve that slopes upward to the right, with the value of β being 0 at the maximum point of the curve.
[0031] As a result of the verification, it was found that in the post-bake temperature range where β is -0.010 or more and 0.015 or less, the light transmittance after post-bake is maintained at a constant high value, and the change in the value of the light transmittance is small even if the post-bake temperature fluctuates slightly. Therefore, if the post-bake temperature is set within this range during production, the light transmittance of the photosensitive resin coating film 23 can be formed to be uniform and high even if there is some variation in the in-plane temperature. In particular, when the photosensitive resin coating film 23 is applied to products for which high transparency is required, such as pixels and overcoats of displays and color filters, the effect of greatly contributing to improvement of productivity and performance is achieved.
[0032] Next, the manufacturing method of the photosensitive resin coating film 23 of the third aspect of the present invention is characterized in that the coating film 20 formed by coating a photosensitive resin composition (FIG. 1(a)) is exposed to light under the following conditions (FIG. 1(b)).
[0033] -0.8≦γ≦0.3 (γ: a value defined as the tangent of the inclination angle of the tangent of a curve plotted as a function of the post-bake residual film ratio vs. exposure amount, the curve being obtained by plotting the post-bake residual film ratio on the vertical axis and the exposure amount during the exposure on the horizontal axis) The post-post-bake film remaining rate vs. exposure curve is a curve as shown by the dotted lines in Figures 6 and 7, which is obtained by plotting the post-post-bake film remaining rate on the vertical axis and the exposure dose during exposure on the horizontal axis, and is fitted with a third-order polynomial.
[0034] FIG. 6 is an example of a post-baking residual film ratio vs. exposure curve in the third configuration of the present invention, where the exposure dose is 20 mJ / cm 2 to 80 mJ / cm 2 4 is an example of a post-bake residual film ratio vs. exposure curve.
[0035] FIG. 7 is an example of a post-baking residual film ratio vs. exposure curve in the third configuration of the present invention, where the exposure dose is 100 mJ / cm 2 to 700 mJ / cm 2 4 is an example of a post-bake residual film ratio vs. exposure curve.
[0036] This third-order polynomial approximation curve is also a curve obtained by measuring at equal intervals under 5 to 10 exposure conditions, and excludes measured values of insufficient performance or obvious abnormalities such as peeling of the photosensitive resin coating film 23 after post-baking. Therefore, although Figures 6 and 7 are exactly the same except for the exposure dose, they are treated as different curves because the interval width of the exposure dose is different.
[0037] Moreover, the tangent to the post-post-bake remaining film ratio vs. exposure curve is the tangent that touches the curve as shown in Figures 6 and 7. The inclination angle of the tangent is the value of θ in Figures 6 and 7 (variation in post-post-bake remaining film ratio / variation in exposure dose), and the value γ defined as the tangent of θ (i.e., tan θ) is positive on the curves that slope downward to the right in Figures 6 and 7, is negative on the curves that slope upward to the right, and is 0 at the maximum point of the curve.
[0038] The inclination angle of the tangent is the value of θ in Figures 6 and 7, and the value γ defined as the tangent of θ (i.e., tan θ) is preferably -0.8 to 0.3. If exposure is performed under conditions where γ is -0.8 to 0.3, even if there is some variation in the amount of exposure, the effect on the thickness of the patterned coating film 22 after post-baking is small, and there is an effect that the photosensitive resin coating film 23 can be applied to large-area sizes, such as pixel patterns of displays and color filters.
[0039] Next, the manufacturing method of the photosensitive resin coating film 23 according to the fourth aspect of the present invention is characterized in that the post-bake residual film ratio is 0 to 0.5% at an exposure dose of 0.1% of the saturated exposure dose. The saturated exposure dose is the minimum exposure dose at which the post-bake residual film ratio is 85% or more. For example, in the case of FIG. 6, the minimum exposure dose at which the post-bake residual film ratio is 85% or more is an exposure dose of 45 mJ / cm2. 2 The exposure amount of 0.1% of the saturated exposure amount is 0.045 mJ / cm in the case of FIG. 2 This corresponds to an exposure level of about
[0040] Therefore, the fourth configuration of the present invention has a luminance of 0.045 mJ / cm in the case of FIG. 2 This means that the residual film rate after post-baking is 0 to 0.5% with an exposure dose of about 100 nm or less. Even if the unexposed parts are completely shielded with a photomask during exposure, the diffraction effect of the exposure light causes some of the exposure light to penetrate and expose parts that should be unexposed, and even after development, some of the exposed coating film 21 remains as a residual film. As a result, there is a problem that the boundary between the exposed and unexposed parts becomes blurred, reducing the resolution.
[0041] However, as a result of verification, it was found that the amount of exposure that penetrates and is exposed is about 0.1% of the saturated exposure amount, so that if the remaining film rate after post-baking is set to 0 to 0.5% at that amount of exposure as in the fourth configuration of the present invention, the remaining film rate will be 0.5% or less, improving the resolution. As a result, there is an effect that the photosensitive resin coating film 23 can be applied to high-definition semiconductor patterns, high-definition display and pixel patterns of color filters, etc.
[0042] Next, the manufacturing method of the photosensitive resin coating film 23 of the fifth aspect of the present invention is characterized in that the color difference ΔEab before and after additional baking for 240 minutes at 100° C. after post-baking is 5.0 or less. The color difference ΔEab is a value that represents the difference in color calculated by the CIE (International Commission on Illumination) in 1976 as the distance between two points on the L*a*b* color space, and in the present invention, it is a value measured using a microsurface spectrophotometer VSS400 manufactured by Nippon Denshoku Industries Co., Ltd.
[0043] Although the unreacted polymerizable compound is almost completely eliminated by the post-bake of the present invention, the photosensitive resin coating film 23 may discolor when subjected to a heavy heat load since the photosensitive resin coating film 23 is composed of a cured film of a photosensitive resin composition. If the color difference ΔEab before and after the additional baking at 100° C. for 240 minutes is 5.0 or less, discoloration is unlikely to be a problem unless the film is used in a harsh environment. Therefore, the coating film produced by the method for producing the photosensitive resin coating film 23 according to the fifth aspect of the present invention is effective in being applied to semiconductors, displays, color filters, and the like used in environments where people live.
[0044] Next, in the sixth aspect of the present invention, a method for producing the photosensitive resin coating film 23 is provided in which the area of the substrate 1 is 0.4 to 16.0 m 2 It is characterized by its small size, which is 0.4 m2, like a typical semiconductor substrate with a diameter of 300 mm. 2 Of course, the present invention is effective even with a substrate 1 of less than this size, but the problem of in-plane variation itself does not occur much with such a small-sized substrate 1. On the other hand, based on the favorable test results with a substrate 1 of 2,160 mm x 2,460 mm, the effects of the present invention can be obtained sufficiently even when expanded to a large area of 4 m square.
[0045] The material of the substrate 1 is not particularly limited, but examples thereof include a sheet of glass, resin, etc. Examples of glass include soda glass, non-alkali glass, borate glass, etc., and the thickness is preferably 0.5 to 2 mm. Examples of resin include polyester, polyvinyl chloride, polystyrene, polyurethane, polycarbonate, polyimide, cyclic olefin, polyacrylate, acrylic, etc., and the thickness is preferably 50 to 500 μm.
[0046] Next, the seventh aspect of the present invention is a manufacturing method for a display, characterized in that any one of a luminescent pixel pattern, a spacer pattern, and an overcoat pattern is formed using the photosensitive resin coating film 23 manufactured by the manufacturing method for the photosensitive resin coating film 23. As described above, the present invention can reduce temperature variations within a surface even in a large area, and is therefore suitable for manufacturing luminescent pixel patterns, spacer patterns, and overcoat patterns of displays that are often formed in large areas.
[0047] The eighth aspect of the present invention is a manufacturing method for a color filter, characterized in that a pixel pattern or a black matrix pattern is formed using the photosensitive resin coating film 23 manufactured by the manufacturing method for the photosensitive resin coating film 23. As in the seventh aspect, since it is often formed in a large area, the present invention is also suitable for manufacturing pixel patterns and black matrix patterns of color filters.
[0048] Next, the photosensitive resin composition used in the manufacturing method of the photosensitive resin coating film 23 will be described. The photosensitive resin composition is a composition that enables pattern formation by exposure and development, and is composed of a binder resin, a polymerizable compound, a photopolymerization initiator, a solvent, and other additives. Examples of the other additives include a chain transfer agent, a sensitizer, a polymer dispersant, an adhesion improver, a surfactant, and a dispersant.
[0049] The binder resin is not particularly limited as long as it is a component that can be easily diluted with an organic solvent, and examples of the binder resin include acrylic resin, epoxy resin, polyimide resin, urethane resin, urea resin, polyvinyl alcohol resin, melamine resin, polyamide resin, polyamideimide resin, polyester resin, polyolefin resin, etc. Two or more of these may be contained.
[0050] In particular, acrylic resins are preferably used in terms of ease of dissolution in the above organic solvents, transparency, and stability.As the acrylic resin, a copolymer of an unsaturated carboxylic acid and an ethylenically unsaturated compound is preferable.As the unsaturated carboxylic acid, for example, monocarboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, or vinylacetic acid, or dicarboxylic acids such as itaconic acid, maleic acid, or fumaric acid, or their acid anhydrides can be mentioned.
[0051] Among them, it is preferable to contain a unit derived from acrylic acid or methacrylic acid. Specifically, it is preferable to use a resin having a tricyclodecane skeleton or a dicyclopentadiene skeleton, such as tricyclodecanyl (meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, dicyclopentenyl (meth)acrylate, or dicyclopentenyloxyethyl (meth)acrylate.
[0052] The polymerizable compound is a reactive monomer that is polymerized by the action of a photopolymerization initiator in an exposure step, and examples of the polymerizable compound include a polymerizable compound (A) containing a unit represented by the following chemical formula 1 and a hydroxyl group, and a polymerizable compound (B) containing a unit represented by the following chemical formula 1 and a unit represented by the following chemical formula 2.
[0053] [ka]
[0054] [ka]
[0055] Examples of the polymerizable compound (A) include the following compounds (a) to (i).
[0056] [ka]
[0057] [ka]
[0058] Examples of the polymerizable compound (B) include the following compounds (i) to (o). Compound (i) is a compound having a structure that belongs to both the polymerizable compound (A) and the polymerizable compound (B).
[0059] [ka]
[0060] [ka]
[0061] Furthermore, as shown in the ninth aspect of the present invention, it is preferable to incorporate both the polymerizable compound (A) and the polymerizable compound (B) in the photosensitive resin composition. By incorporating both, the post-baking temperature range that satisfies the conditions of -0.05≦α≦0.12 and -0.010≦β≦0.015 can be set broadly, the post-baking temperature can be relatively lowered, and the exposure dose required for pattern formation can also be relatively reduced, so that from both of these viewpoints, the effects of energy saving and productivity improvement can be obtained.
[0062] The total content of the polymerizable compound (A) and the polymerizable compound (B) is preferably 20 to 70 parts by weight, with the total solid content being 100 parts by weight, as shown in the tenth aspect of the present invention. By containing 20% by weight or more of the polymerizable compound, a tough layer excellent in adhesion and free from cohesive failure can be formed, and by containing 70% by weight or less of the polymerizable compound, the influence of unreacted double bonds can be prevented.
[0063] Furthermore, as shown in the eleventh aspect of the present invention, the weight average molecular weight of the polymerizable compound (A) is preferably 100 to 800, and the weight average molecular weight of the polymerizable compound (B) is preferably 300 to 1,000. By setting the weight average molecular weight of the polymerizable compound within this range, it is possible to easily adjust the viscosity to a level suitable for coating.
[0064] Furthermore, as shown in the twelfth aspect of the present invention, the double bond equivalent of the polymerizable compound (A) is preferably 50 to 150, and the double bond equivalent of the polymerizable compound (B) is preferably 30 to 200. By setting the double bond equivalent of the polymerizable compound within this range, the exposure sensitivity is improved, making it possible to form a pattern with a relatively small amount of exposure light, and energy saving can be facilitated.
[0065] The weight ratio of the polymerizable compound (A) to the polymerizable compound (B) is preferably 30:70 to 70:30 as shown in the thirteenth aspect of the present invention. By using this weight ratio, the composition can be easily diluted with an organic solvent, and the dispersibility is excellent when a coloring material such as a pigment is contained, making it easy to apply the composition to pixel patterns of displays and color filters.
[0066] The solvent preferably has a boiling point of 150° C. or less. Solvents with a boiling point exceeding 150° C. are likely to remain as residual solvent in the photosensitive resin coating film 23, and if there is a large amount of residual solvent, radicals are likely to be deactivated and the polymerization reaction is likely to be inhibited. Examples of solvents with a boiling point of 150° C. or less include aliphatic ester solvents, aliphatic alcohol solvents, ketone solvents, hydrocarbon solvents, acetate solvents, and glycol ether solvents. Two or more of these may be contained.
[0067] The photopolymerization initiator is a compound that decomposes and / or reacts with light (including ultraviolet light or electron beam) to generate radicals, and examples of the photopolymerization initiator include oxime ester compounds, benzophenone compounds, acetophenone compounds, oxanthone compounds, anthraquinone compounds, imidazole compounds, benzothiazole compounds, benzoxazole compounds, carbazole compounds, triazine compounds, phosphorus compounds, and titanocene compounds.
[0068] The photopolymerization initiator acts as a trigger for the reaction of the unsaturated double bonds present in the binder resin and the polymerizable compound, improving the sensitivity during patterning and preventing the adverse effects of unreacted double bonds. That is, the photocuring proceeds sufficiently to reduce the residues of the double bonds, suppressing the deterioration of stability over time due to the residues. For this purpose, a photopolymerization initiator that allows the exposure light to reach not only the surface but also the deep parts uniformly is preferred.
[0069] In particular, when post-baking is performed at a low temperature, double bond residues are likely to remain, but by including a photopolymerization initiator having this function, it is possible to prevent variation in the degree of photocuring between the surface and the depth of the photosensitive resin coating film 23, thereby reducing the possibility of double bond residues remaining. Photopolymerization initiators having such a function include photobleach-type photopolymerization initiators.
[0070] Photobleach-based photopolymerization initiators are photopolymerization initiators in which the light absorption decreases due to cleavage of the double bond as the reaction progresses.Specific examples include monoacylphosphine oxide-based photopolymerization initiators, bisacylphosphine oxide-based photopolymerization initiators, metallocene (titanocene)-based photopolymerization initiators, polysilane-based photopolymerization initiators, and oxime ester-based initiators.
[0071] A plurality of types of photopolymerization initiators may be contained, for example, an oxime ester-based photopolymerization initiator and an alkylphenone-based photopolymerization initiator may be contained as shown in the 14th configuration of the present invention. In addition, as the melting point of the photopolymerization initiator increases, the absorbance in the visible region increases and the photopolymerization initiator is likely to take on a yellowish hue, and therefore, in order to maintain the colorless transparency of the photosensitive resin coating film 23, a photopolymerization initiator having a melting point of 115° C. or less is preferred as shown in the 15th configuration of the present invention.
[0072] Examples of oxime ester photopolymerization initiators having a melting point of 115°C or lower include "Irgacure 369", "Irgacure OXE-03", and "Irgacure OXE-04" manufactured by BASF Japan Ltd., "P0211" manufactured by Tokyo Chemical Industry Co., Ltd., and "ADEKA CRUISE NCI-930", "ADEKA CRUISE NCI-803", and "ADEKA CRUISE NCI-730" manufactured by ADEKA Corporation.
[0073] From the viewpoints of sensitivity, patterning ability, and processability, the content of the photopolymerization initiator is preferably from 1 mass % to 30 mass % of the solid content of the photosensitive resin composition, more preferably from 2 mass % to 20 mass %, and even more preferably from 5 mass % to 15 mass %.
[0074] In order to apply the photosensitive resin coating film produced by the present invention to pixel patterns, black matrix patterns, etc., the photosensitive resin composition may contain coloring materials such as organic pigments, inorganic pigments, dyes, etc., such as red, blue, green, yellow, and black. Examples of red coloring materials include CI Pigment Red (hereinafter, "PR") 9, PR48, PR97, PR122, PR123, PR144, PR, 149, PR166, PR168, PR177, PR179, PR180, PR192, PR209, PR215, PR216, PR217, PR220, PR223, PR224, PR226, PR227, PR228, PR240, PR254, and diketopyrrolopyrrole coloring materials having a bromine group.
[0075] Examples of green colorants include CI Pigment Green (hereinafter referred to as "PG") PG1, PG2, PG4, PG7, PG8, PG10, PG13, PG14, PG15, PG17, PG18, PG19, PG26, PG36, PG38, PG39, PG45, PG48, PG50, PG51, PG54, PG55, PG58, PG59 (all numbers are color index numbers), etc.
[0076] Examples of yellow colorants include CI Pigment Yellow (hereinafter referred to as "PY") 12, PY13, PY17, PY20, PY24, PY83, PY86, PY93, PY95, PY109, PY110, PY117, PY125, PY129, PY137, PY139, PY147, PY148, PY150, PY153, PY154, PY166, and PY168 (all numbers are Color Index Nos.).
[0077] Examples of blue coloring materials include CI Pigment Blue (hereinafter, "PB") 15, PB15:3, PB15:4, PB15:6, PB21, PB22, PB60, and PB64. Examples of black coloring materials include carbon black and titanium black. The content of the coloring material is preferably 10% by mass or more and 40% by mass or less, and more preferably 20% by mass or more and 35% by mass or less, based on the solid content of the photosensitive resin composition.
[0078] Examples of methods for coating the photosensitive resin composition include gravure coating, spin coating, dip coating, curtain flow coating, roll coating, spray coating, slit die coating, ink jet coating, and nozzle coating.
[0079] The drying method for evaporating the solvent of the coated photosensitive resin composition to form the coating film 20 is not particularly limited, but reduced pressure drying at room temperature is preferable to reduce the influence of heat. The reduced pressure drying pressure is preferably equal to or lower than the vapor pressure of the solvent contained in the layer, and is preferably 1 to 1000 Pa. The reduced pressure drying time is preferably 10 to 600 seconds.
[0080] In the exposure step, a photomask 3 is placed on the top of the coating film 20 formed as shown in Fig. 1(b), and exposure is performed. A negative exposure step is then preferred in which the exposed parts are cured as shown in Fig. 1(c), and developed with an alkaline developer in the development step, thereby removing the unexposed parts to form a pattern.
[0081] Examples of exposure devices include steppers, mirror projection mask aligners (MPA), parallel light mask aligners (PLA), lens scans, etc. Examples of exposure light sources include ultraviolet rays such as i-lines, h-lines, and g-lines, KrF (wavelength 248 nm) lasers, and ArF (wavelength 193 nm) lasers.
[0082] The exposure dose was 700 mJ / cm 2 Set the exposure to 700 mJ / cm 2 By keeping the exposure dose at 300 mJ / cm or less, the exposure time can be shortened, productivity can be improved, and the amount of energy required for exposure can be saved. 2 More preferably, the exposure dose is 100 mJ / cm or less. 2 The lower the exposure dose, the shorter the exposure time, improving productivity and saving energy for exposure.
[0083] Examples of the developing method include showering, dipping, and puddling. By immersing the exposed coating film 21 in the developer for 5 seconds to 10 minutes, a coating film 22 having a predetermined pattern can be formed as shown in FIG. 1(c). Examples of the developing solution include inorganic alkalis such as hydroxides, carbonates, phosphates, silicates, and borates of alkali metals such as sodium hydroxide and potassium hydroxide; amines such as 2-diethylaminoethanol, monoethanolamine, and diethanolamine; and alkaline developers such as aqueous solutions containing quaternary ammonium salts such as tetramethylammonium hydroxide and choline. After development, it is preferable to rinse with water. EXAMPLES
[0084] <Example 1 of post-bake residual film rate vs. post-bake temperature curve and post-bake light transmittance vs. post-bake temperature curve> A photosensitive resin composition having the following composition was applied by slit die coating onto soda lime glass substrates each having a thickness of 1 mm and a length of 10 cm square, and then dried under reduced pressure to form a coating film having a thickness of 5.0 μm and a light transmittance of 85%. A photomask was then set on the coating film, and ultraviolet i-line was irradiated from above the photomask at an exposure dose of 60 mJ / cm. 2 The exposed coating film was exposed by irradiation with 100 .mu.m, and the unexposed areas of the exposed coating film were developed with an aqueous sodium carbonate solution to form a pattern.
[0085] (Composition of photosensitive resin composition) Alkali-soluble resin Tricyclodecanyl (meth)acrylate 40 parts by weight Polymerizable compound (A) (B) Compound (i) (weight average molecular weight: 298, double bond equivalent: 99) 30 parts by weight Polymerizable compound (B) Compound (n) (weight average molecular weight: 579, double bond equivalent: 96) 30 parts by weight Photopolymerization initiator BASF Irgacure 369 (melting point 110°C, α-aminoalkylphenone polymerization initiator) 1 part by weight Photopolymerization initiator Adeka Cruise NCI-930 (melting point 96°C, oxime ester polymerization initiator 1 part by weight Solvent: Polyethylene glycol monomethyl ether acetate 120 parts by weight Next, the patterned coating film was post-baked for 30 minutes at each of the temperatures of 40°C, 60°C, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, and 220°C, and the thickness of each coating film after post-baking was measured to calculate the post-baking residual film ratio of each coating film, and the post-baking light transmittance of each coating film was measured. A post-baking residual film ratio vs. post-baking temperature curve shown in Figure 2, in which the post-baking residual film ratio is plotted on the vertical axis and the post-baking temperature on the horizontal axis, and a post-baking light transmittance vs. post-baking temperature curve shown in Figure 3, in which the post-baking light transmittance is plotted on the vertical axis and the post-baking temperature on the horizontal axis, were created.
[0086] Next, a tangent line T was drawn at an arbitrary point on each curve, and the angles 4θ and 20θ between the tangent line at that arbitrary point and a line parallel to the horizontal axis were measured, from which the inclination angle θ was obtained, and the values of α and β at that arbitrary point were calculated. The results are shown in Table 1. It can be seen from Table 1 that if the post-bake temperature is 40 to 160°C, the condition of -0.05≦α≦0.12 is satisfied, and if the post-bake temperature is 40 to 140°C, the condition of -0.010≦β≦0.015 is satisfied.
[0087] [Table 1]
[0088] <Example 2 of post-bake residual film rate vs. post-bake temperature curve and post-bake light transmittance vs. post-bake temperature curve> The patterned coating film was formed in the same manner as in Preparation Example 1, except that the composition of the photosensitive resin composition was as follows and the post-bake temperatures were changed to 190°C, 210°C, 230°C, 250°C, 270°C, 290°C, and 310°C.
[0089] (Composition of photosensitive resin composition) Alkali-soluble resin Dicyclopentenyloxyethyl (meth)acrylate 30 parts by weight Polymerizable compound (B) Compound (n) (weight average molecular weight: 579, double bond equivalent: 96) 40 parts by weight Photopolymerization initiator BASF Irgacure 369 (melting point 110°C, α-aminoalkylphenone polymerization initiator) 1 part by weight Solvent: Polyethylene glycol monoethyl ether acetate 120 parts by weight Next, in the same manner as in Preparation Example 1, a curve of post-baking residual film ratio vs. post-baking temperature and a curve of post-baking light transmittance vs. post-baking temperature were prepared. Next, a tangent line T was drawn at an arbitrary point on each curve, and angles 4θ and 5θ between the tangent line at the arbitrary point and a line parallel to the horizontal axis were measured, and an inclination angle θ was obtained from the angles, and values of α and β at the arbitrary point were calculated. The results are shown in Table 2. From Table 2, it can be seen that if the post-baking temperature is 210 to 250°C, the condition of -0.05≦α≦0.12 is satisfied, and if the post-baking temperature is 230°C, the condition of -0.010≦β≦0.015 is satisfied.
[0090] [Table 2]
[0091] <Post-bake remaining film ratio vs. exposure curve creation example 3> The exposure dose of ultraviolet i-line irradiated from above the photomask is 60 mJ / cm 2 and 20 mJ / cm 2 , 40mJ / cm 2 , 80mJ / cm 2 , 100mJ / cm 2 , 200mJ / cm 2 , 300mJ / cm 2 , 400mJ / cm 2 , 500mJ / cm 2 , 600mJ / cm 2 , 700mJ / cm 2 A patterned coating film was formed in the same manner as in Preparation Example 1, except that the above-mentioned changes were made.
[0092] (Composition of photosensitive resin composition) Alkali-soluble resin Dicyclopentenyloxyethyl (meth)acrylate 30 parts by weight Polymerizable compound (B) Compound (n) (weight average molecular weight: 579, double bond equivalent: 96) 40 parts by weight Photopolymerization initiator BASF Irgacure 369 (melting point 110°C, α-aminoalkylphenone polymerization initiator) 1 part by weight Solvent: Polyethylene glycol monoethyl ether acetate 120 parts by weight Next, in the same manner as in Preparation Example 1, the patterned coating film was post-baked at 100° C. for 30 minutes, the thickness after post-baking was measured, and the post-baking remaining film ratio was calculated. The post-baking remaining film ratio vs. exposure dose curves shown in FIG. 6 and FIG. 7 were created by plotting the post-baking remaining film ratio on the ordinate and the exposure dose on the abscissa.
[0093] Next, a tangent line T was drawn at an arbitrary point on each curve, and the angles θ and 20θ between the tangent line at the arbitrary point and a line parallel to the horizontal axis were measured, and the inclination angle θ was calculated from the angles, and the γ value at the arbitrary point was calculated. The results are shown in Table 3. From Table 3, it can be seen that when the exposure dose was 60 mJ / cm 2 More than 700mJ / cm 2 It can be seen that the condition -0.8≦γ≦0.3 is satisfied up to this range.
[0094] [Table 3]
[0095] <Examples 1 to 5, Comparative Examples 1 to 2> A photosensitive resin composition having the following composition was applied by slit die coating onto 700 soda lime glass substrates each having a thickness of 1 mm, a length of 2.16 m and a width of 2.46 m, and then dried under reduced pressure to form a coating film having a thickness of 5.0 μm and a light transmittance of 85%. A photomask was then set on the coating film, and ultraviolet i-line was irradiated from above the photomask at an exposure dose of 80 mJ / cm. 2 The exposed coating film was then developed with an aqueous sodium carbonate solution to remove the unexposed areas, forming a pattern.
[0096] (Composition of photosensitive resin composition) Alkali-soluble resin Tricyclodecanyl (meth)acrylate 40 parts by weight Polymerizable compound (A) (B) Compound (i) (weight average molecular weight: 298, double bond equivalent: 99) 30 parts by weight Polymerizable compound (B) Compound (n) (weight average molecular weight: 579, double bond equivalent: 96) 30 parts by weight Photopolymerization initiator Adeka Cruise NCI-930 (melting point 96°C, oxime ester polymerization initiator) 2 parts by weight Solvent: Polyethylene glycol monomethyl ether acetate 120 parts by weight Next, 100 of each of the patterned coating films were post-baked for 30 minutes at temperatures of 40° C., 60° C., 100° C., 140° C., 160° C., 180° C., and 200° C., and the light transmittance (%) after post-baking was measured. In addition, the thickness after post-baking of the patterned coating film and the thickness after post-baking of the remaining film after development (corresponding to the coating film thickness at an exposure amount of 0.1% of the saturated exposure amount) were measured, and the remaining film ratio after post-baking of the patterned coating film and the remaining film ratio after post-baking of the remaining film after development were calculated.
[0097] Next, the α and β values at each post-bake temperature were calculated from the post-bake residual film rate and post-bake light transmittance (%) of the patterned coating film. After that, the patterned coating film was additionally baked for 240 minutes at 100°C, and the color difference ΔEab of the patterned coating film before and after baking was measured. The results are shown in Tables 4 and 5. Tables 4 and 5 show that if the product is manufactured under conditions that satisfy the condition -0.05≦α≦0.12, the yield rate will be 97% or more, and if the product is manufactured under conditions that also satisfy the condition -0.010≦β≦0.015, the yield rate will be 99% or more.
[0098] <Examples 6 to 8, Comparative Examples 3 to 4> Patterned coating films were formed in the same manner as in Examples 1 to 5, except that a photosensitive resin composition having the following composition was applied onto 500 soda-lime glass substrates each having a thickness of 1 mm, a length of 2.16 m, and a width of 2.46 m.
[0099] (Composition of photosensitive resin composition) Alkali-soluble resin Dicyclopentenyloxyethyl (meth)acrylate 30 parts by weight Polymerizable compound (B) Compound (n) (weight average molecular weight: 579, double bond equivalent: 96) 40 parts by weight Photopolymerization initiator BASF Irgacure 369 (melting point 110°C, α-aminoalkylphenone polymerization initiator) 1 part by weight Solvent: Polyethylene glycol monoethyl ether acetate 120 parts by weight Next, the same procedure as in Example 1 was carried out, except that 100 pieces of each pattern-formed coating film were post-baked at temperatures of 190° C., 210° C., 230° C., 250° C., and 270° C. The results are shown in Tables 4 and 5. It can be seen from Tables 4 and 5 that if production is carried out under conditions that satisfy the condition -0.05≦α≦0.12, the yield rate will be 95% or more, and if production is carried out under conditions that also satisfy the condition -0.010≦β≦0.015, the yield rate will be 99%.
[0100] [Table 4]
[0101] [Table 5]
[0102] <Example 9> (Preparation of overcoat film for organic electroluminescence display) A sealing film was formed on an organic electroluminescence pixel pattern having a thickness of 1 mm, a length of 2.88 m, and a width of 3.13 m. A photosensitive resin composition having the following composition was applied onto the sealing film by a slit die coating method, and then dried under reduced pressure to form an overcoat coating film. Next, a photomask was set on the coating film, and ultraviolet i-line was irradiated from above the photomask at an exposure dose of 80 mJ / cm. 2 The exposed coating film was then developed with an aqueous sodium carbonate solution to remove the unexposed areas, thereby forming an overcoat pattern.
[0103] (Composition of photosensitive resin composition) Alkali-soluble resin Dicyclopentenyloxyethyl (meth)acrylate 40 parts by weight Polymerizable compound (A) Compound (b) (weight average molecular weight: 116, double bond equivalent: 116) 30 parts by weight Polymerizable compound (B) Compound (k) (weight average molecular weight: 212, double bond equivalent: 106) 30 parts by weight Photopolymerization initiator Adeka Cruise NCI-930 (melting point 96°C, oxime ester polymerization initiator) 2 parts by weight Photopolymerization initiator Adeka Cruise NCI-730 (melting point 85°C, oxime ester polymerization initiator) 2 parts by weight Solvent: Polyethylene glycol monomethyl ether acetate 120 parts by weight The patterned coating film was then post-baked for 30 minutes at 40° C. to form an organic electroluminescence element with an overcoat pattern. The post-baked light transmittance (%), the post-baked thickness of the patterned coating film, and the post-baked thickness of the remaining film after development (corresponding to the coating film thickness at an exposure dose of 0.1% of the saturated exposure dose) were measured, and the post-baked remaining film ratio of the patterned coating film and the post-baked remaining film ratio of the remaining film after development were calculated.
[0104] Next, the α and β values at the post-bake temperature were calculated from the post-bake residual film rate and post-bake light transmittance (%) of the patterned coating film. After that, the patterned coating film was additionally baked for 240 minutes at 100°C, and the color difference ΔEab of the patterned coating film before and after baking was measured. The results are shown in Table 6. From Table 6, it can be seen that the post-bake conditions satisfied the conditions of -0.05≦α≦0.12 and -0.010≦β≦0.015.
[0105] <Example 10> (Fabrication of red color filters for reflective LCD displays) A red photosensitive resin composition having the following composition was applied by slit die coating onto a soda lime glass substrate having a thickness of 1 mm, a length of 1 m and a width of 1.2 m, and then dried under reduced pressure to form a red photosensitive resin coating film. Next, a photomask was set on the coating film, and ultraviolet i-line was irradiated from above the photomask at an exposure dose of 100 mJ / cm. 2The exposed coating film was then developed with an aqueous sodium carbonate solution and the unexposed areas were peeled off to form a pattern of a red photosensitive resin coating film.
[0106] (Composition of photosensitive resin composition) Colorant: CI Pigment Red 220 15 parts by weight Alkali-soluble resin Tricyclodecanyl (meth)acrylate 40 parts by weight Polymerizable compound (A) (B) Compound (i) (weight average molecular weight: 298, double bond equivalent: 99) 30 parts by weight Polymerizable compound (B) Compound (n) (weight average molecular weight: 579, double bond equivalent: 96) 30 parts by weight Photopolymerization initiator Adeka Cruise NCI-803 (melting point 72°C, oxime ester polymerization initiator) 1 part by weight Photopolymerization initiator Adeka Cruise NCI-730 (melting point 85°C, oxime ester polymerization initiator) 1 part by weight Solvent: Polyethylene glycol monomethyl ether acetate 120 parts by weight Next, the patterned coating film was post-baked for 30 minutes at a temperature of 80° C. to produce a red color filter for a reflective liquid crystal display. In addition, the light transmittance after post-baking (%), the thickness after post-baking of the patterned coating film, and the thickness after post-baking of the remaining film after development (corresponding to the coating film thickness at an exposure amount of 0.1% of the saturated exposure amount) were measured, and the remaining film ratio after post-baking of the patterned coating film and the remaining film ratio after post-baking of the remaining film after development were calculated.
[0107] Next, the α and β values at the post-bake temperature were calculated from the post-bake residual film rate and post-bake light transmittance (%) of the patterned coating film. After that, the patterned coating film was additionally baked for 240 minutes at 100°C, and the color difference ΔEab of the patterned coating film before and after baking was measured. The results are shown in Table 6. From Table 6, it can be seen that the post-bake conditions satisfied the conditions of -0.05≦α≦0.12 and -0.010≦β≦0.015.
[0108] [Table 6] [Explanation of symbols]
[0109] 1: Base material 20: Paint film 21: Exposed coating 22: Patterned coating 23: Photosensitive resin coating 3: Photomask E: Exposure P: Post bake
Claims
1. A photosensitive resin composition is coated on a substrate to form a coating film, and the coating film is subjected to irradiation with 700 mJ / cm 2 A method for producing a photosensitive resin coating film, comprising exposing the coating film to an exposure amount as described below, developing the exposed coating film to form a pattern, and then post-baking the patterned coating film under the conditions as described below. -0.05≦α≦0.12 (α: a value defined as the tangent of the inclination angle of the tangent of a curve of the film remaining rate after post-bake vs. the post-bake temperature, the curve being plotted with the film remaining rate after post-bake on the vertical axis and the post-bake temperature on the horizontal axis)
2. 2. The method for producing a photosensitive resin coating film according to claim 1, wherein the patterned coating film is post-baked under the following conditions: -0.010≦β≦0.015 (β is a value defined as the tangent of the inclination angle of the tangent of a curve of light transmittance after post-baking vs. post-baking temperature, the curve being obtained by plotting light transmittance after post-baking on the vertical axis and post-baking temperature on the horizontal axis.)
3. 3. The method for producing a photosensitive resin coating film according to claim 1, wherein the formed coating film is exposed under the following conditions: −0.8≦γ≦0.3 (γ: a value defined as the tangent of the inclination angle of the tangent of a curve of post-bake residual film ratio vs. exposure, the curve being a plot of the post-bake residual film ratio on the vertical axis and the exposure dose during the exposure on the horizontal axis)
4. 3. The method for producing a photosensitive resin coating film according to claim 1 or 2, wherein the post-bake residual film ratio is 0 to 0.5% at an exposure amount of 0.1% of a saturated exposure amount (the minimum exposure amount at which the post-bake residual film ratio is 85% or more).
5. 3. The method for producing a photosensitive resin coating film according to claim 1, wherein the color difference ΔEab before and after additional baking at 100° C. for 240 minutes after post-baking is 5.0 or less.
6. The area of the substrate is 0.4 to 16.0 m 2 The method for producing a photosensitive resin coating film according to claim 1 or 2,
7. A method for producing a display, comprising forming any one of a light-emitting pixel pattern, a spacer pattern, and an overcoat pattern using a photosensitive resin coating film produced by the method for producing a photosensitive resin coating film according to claim 1 or 2.
8. A method for producing a color filter, comprising forming a pixel pattern or a black matrix pattern using a photosensitive resin coating film produced by the method for producing a photosensitive resin coating film according to claim 1 or 2.
9. A photosensitive resin composition comprising: a polymerizable compound (A) containing a unit represented by the following chemical formula 1 and a hydroxyl group; and a polymerizable compound (B) containing a unit represented by the following chemical formula 1 and a unit represented by the following chemical formula 2: 【Chemistry 1】 【Chemistry 2】
10. 10. The photosensitive resin composition according to claim 9, wherein the total amount of the polymerizable compound (A) and the polymerizable compound (B) is 20 to 70 parts by weight, based on 100 parts by weight of the total solid content.
11. 11. The photosensitive resin composition according to claim 9, wherein the polymerizable compound (A) has a weight average molecular weight of 100 to 800, and the polymerizable compound (B) has a weight average molecular weight of 300 to 1,000.
12. 11. The photosensitive resin composition according to claim 9, wherein the polymerizable compound (A) has a double bond equivalent of 50 to 150, and the polymerizable compound (B) has a double bond equivalent of 30 to 200.
13. 11. The photosensitive resin composition according to claim 9, wherein the weight ratio of the polymerizable compound (A) to the polymerizable compound (A) is 30:70 to 70:
30.
14. The photosensitive resin composition according to claim 9 or 10, comprising a photopolymerization initiator having a melting point of 115° C. or less.
15. The photosensitive resin composition according to claim 9 or 10, comprising an alkylphenone-based photopolymerization initiator and an oxime ester-based photopolymerization initiator.
Citation Information
Patent Citations
Method of evaluating heat treating effect and method of evaluating resist baking apparatus
JP2002189303A
Resist processing method and method of manufacturing resist-attached substrate
JP2012047828A