Components for producing lithium-containing composite oxide, method for producing the same, and firing furnace for producing lithium-containing composite oxide
A coating film with high aluminum content on metal containers addresses temperature non-uniformity and corrosion issues in lithium-containing composite oxide production, ensuring consistent reaction conditions and preventing battery degradation.
Patent Information
- Application Number
- JP2023084475
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-23
AI Technical Summary
Existing methods for producing lithium-containing composite oxides for lithium ion secondary batteries face issues with temperature non-uniformity, corrosion resistance, and thermal shock resistance, leading to variations in solid phase reactions and potential battery degradation due to unreacted lithium hydroxide and oxygen deficiencies.
A coating film containing at least 60 atomic % aluminum and one or more of nickel, rhenium, and cobalt is applied to the surface of metal or alloy containers used in the production process, enhancing corrosion resistance and temperature uniformity during heating and cooling.
The solution provides excellent corrosion resistance and temperature uniformity, ensuring consistent reaction conditions and preventing battery degradation by maintaining uniform temperature distribution during the synthesis of lithium-containing composite oxides.
Smart Images

Figure 2024168076000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a member for producing a lithium-containing composite oxide, a method for producing the same, and a sintering furnace for producing a lithium-containing composite oxide, and is suitably applied to, for example, the production of a positive electrode active material for a lithium ion secondary battery. [Background technology]
[0002] The positive electrode active material of the lithium ion secondary battery is a lithium-containing composite oxide (for example, a lithium transition metal composite oxide such as a lithium cobalt composite oxide, a lithium nickel composite oxide, a lithium manganese composite oxide, a lithium manganese cobalt composite oxide, a lithium nickel cobalt composite oxide, or a lithium nickel cobalt manganese composite oxide). This positive electrode active material is produced by putting a raw material powder into a container and firing it.
[0003] Ceramic saggers are widely used as containers for firing positive electrode active materials (see, for example, Patent Documents 1 to 3). Raw material powder is placed in the ceramic sagger, which is then placed in a firing furnace and heated to perform firing.
[0004] The atmosphere inside the sintering furnace varies depending on the type of powder, but a resistance heater is widely used as the heating means. The resistance heater is installed on the ceiling of the furnace and radiates heat to the sagger and raw powder. Since the atmosphere inside the furnace is also heated, convection heating is also performed inside the furnace.
[0005] The thickness of the powder layer in the ceramic sagger is usually about 50 to 100 mm, and heating is mainly performed from the surface layer. The thermal conductivity of the ceramic sagger is low, and the thermal conductivity of the powder is also not very high. For this reason, the powder on the surface of the ceramic sagger rises in temperature easily, but the powder inside rises in temperature slowly, and a temperature difference inevitably occurs during the heating process. The powder on the surface is kept at the maximum temperature for a relatively long period of time, while the powder inside is kept at the maximum temperature for a shorter period of time, which causes variation in the progress of the solid-phase reaction.
[0006] When attempting to sinter a positive electrode active material, if a ceramic container such as a crucible or sagger is used, there is a problem that the crucible or sagger will deteriorate and break with repeated use because it has low thermal shock resistance.
[0007] Also, for example, in the synthesis of lithium nickel composite oxide using lithium hydroxide and nickel composite oxide as raw materials, the reaction between lithium hydroxide and nickel composite oxide starts at around 450°C. If oxygen is not sufficiently diffused to the bottom of the ceramic sagger, unreacted molten lithium hydroxide may remain. The remaining lithium hydroxide may react with carbon dioxide gas to produce lithium carbonate (Li2CO3). If lithium carbonate is produced, gas caused by this lithium carbonate may be generated at high temperatures during use of the battery, which may lead to the problem of battery expansion.
[0008] In addition, in the synthesis reaction of lithium nickel composite oxide, when the temperature is further increased to 650°C, if unreacted lithium hydroxide and nickel composite oxide are present and oxygen is insufficient, for example, Li2Ni8O 10 Such a side reaction occurs to generate a different phase, and the different phases that hinder the movement of lithium ions during the battery reaction occur in the generated lithium nickel composite oxide crystal, which may lead to deterioration of battery performance.
[0009] In order to obtain a positive electrode active material having excellent battery characteristics, many proposals have been made so far regarding the synthesis conditions by calcination of lithium metal composite oxides.
[0010] In the synthesis reaction of lithium-containing composite oxides, saggers and related parts made of metals or alloys are desirable because they have excellent temperature tracking ability and temperature uniformity when heating and cooling the inside of the sagger. However, they are not currently in practical use because of their poor corrosion resistance.
[0011] Against this background, a sagger has recently been proposed in which at least the surface that comes into contact with the lithium positive electrode material powder is formed from a nickel-based alloy with an aluminum content of 1% by weight or more and 10% by weight or less (see Patent Document 4). [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Patent No. 3552210 specification [Patent Document 2] JP 2003-165767 A [Patent Document 3] JP 2015-218098 A [Patent Document 4] Patent No. 7090784 specification Summary of the Invention [Problem to be solved by the invention]
[0013] However, according to the investigations of the present inventors, in the sagger proposed in Patent Document 4, the aluminum content of the nickel-based alloy is low, at 1% by weight or more and 10% by weight or less, so that protective alumina is not formed during use, resulting in poor corrosion resistance and the Cr contained in the nickel-based alloy being oxidized, which ultimately has the disadvantage of adversely affecting the charge / discharge characteristics of the lithium-ion secondary battery.
[0014] Therefore, an object of the present invention is to provide a member for producing a lithium-containing composite oxide, including various containers such as saggers and related members, which can obtain excellent corrosion resistance against a synthesis reaction of a lithium-containing composite oxide and have excellent temperature follow-up properties and temperature uniformity during heating and cooling, and a method for producing the same.
[0015] Another problem to be solved by the present invention is to provide a sintering furnace for producing a lithium-containing composite oxide, which can obtain excellent corrosion resistance when sintering a powder of a raw material for the lithium-containing composite oxide, and which is excellent in temperature follow-up ability and temperature uniformity during heating and cooling. [Means for solving the problem]
[0016] In order to solve the above problems, the present invention provides: A substrate made of a metal or alloy; a coating film provided on at least a surface of the substrate with which the powder of the raw material of the lithium (Li)-containing composite oxide comes into contact, the coating film containing at least aluminum (Al) and at least one metal selected from nickel (Ni), rhenium (Re) and cobalt (Co), and having a maximum Al concentration of 60 atomic % or more and less than 100 atomic %; The lithium-containing composite oxide manufacturing member has the following structure.
[0017] The metal or alloy constituting the substrate is not particularly limited as long as it does not lose mechanical strength even when heated to the firing temperature of the powder of the raw material of the Li-containing composite oxide, and is selected as necessary, for example, Ni, Ni-based alloy, iron (Fe)-based alloy, etc. Among them, Ni-based alloys are, for example, MA47P (Ni-2Cr-4Al-1.5Si-0.5Mn), Inconel, Hastelloy, Alloy-X, etc. Also, Fe-based alloys are, for example, stainless steel (SUS304, SUS310, etc.). The shape of the substrate is selected according to the application of the Li-containing composite oxide production member. When the Li-containing composite oxide production member is a container such as a sagger, it has, for example, a bowl shape, and a coating film is provided on the inner surface of the container. When the Li-containing composite oxide production member is a tube, it is a circular tube, a square tube, etc., and a coating film is provided on the outer surface and inner surface of the tube. When the member for producing a lithium-containing composite oxide is a rod, it may be a square rod, a round rod, or the like, and a coating film is provided on the outer surface of the rod.
[0018] When the maximum Al concentration of the coating film is 60 atomic % or more and less than 100 atomic %, protective alumina (Al2O3) can be maintained on the surface of the member for producing a Li-containing composite oxide for a long period of time, and corrosion resistance can be obtained. The maximum Al concentration of the coating film is preferably 70 atomic % or more and less than 100 atomic %. The maximum Al concentration of the coating film is typically 81 atomic % or less. If necessary, the coating film further contains at least one metal selected from the group consisting of tungsten (W), molybdenum (Mo) and niobium (Nb). The coating film may contain other metals that are inevitably mixed in.
[0019] The coating film is composed of a single layer or multiple layers. In the coating film, Al, Ni, Re, and Co exist as various alloys such as Ni(Re, Co)-Al in which a part of Ni in Ni-Al is replaced with Re and Co, Ni(Re)-Al in which a part of Ni in Ni-Al is replaced with Re, Co(Ni, Re)-Al in which a part of Co in Co-Al is replaced with Ni and Re, Co(Ni)-Al in which a part of Co in Co-Al is replaced with Ni, Ni-Al, Re-Al, Co-Al, etc. The coating film may contain metals other than Al, Ni, Re, and Co, and in this case, these alloys may contain one or more of these metals. When the coating film is composed of multiple layers, typically, each layer contains one of these alloys.
[0020] The present invention also provides A step of forming a raw material coating containing at least nickel (Ni) and at least one metal selected from rhenium (Re) and cobalt (Co) on a substrate made of a metal or alloy; a step of performing an aluminum (Al) diffusion treatment on the base material on which the raw coating is formed to form a coating film containing at least aluminum (Al) and at least one metal selected from the group consisting of nickel (Ni) and rhenium (Re) and cobalt (Co), and having a maximum aluminum (Al) concentration of 60 atomic % or more and less than 100 atomic %; The present invention relates to a method for producing a member for producing a lithium-containing composite oxide having the above structure.
[0021] The raw coating may contain at least one metal selected from the group consisting of W, Mo and Nb, in addition to Ni and at least one metal selected from Re and Co, and may also contain Al in some cases. If necessary, the raw coating may be formed in a plurality of separate steps. In this case, it is sufficient that the raw coating finally obtained as a whole contains at least one metal selected from Ni, Re and Co, and each raw coating does not have to contain all of them. The method for forming the raw coating is not particularly limited and is selected as necessary, and examples of the method include plating (electroplating), thermal spraying, and electron beam vacuum deposition.
[0022] The Al diffusion treatment is carried out, for example, by immersing the substrate on which the raw coating has been formed in a mixed powder containing an Al-containing powder (e.g., Al powder), NH4Cl powder, and Al2O3 powder, and heating it in an inert gas atmosphere, preferably an argon (Ar) + 3 vol% hydrogen (H2) atmosphere, at a temperature of 950°C to 1150°C for 1 hour to 10 hours.
[0023] If necessary, after the formation of the raw coating, the substrate on which the raw coating is formed is heat-treated before the Al diffusion treatment. The metals constituting the raw coating are diffused and homogenized by this heat treatment. The temperature and time of this heat treatment are selected as necessary, but the temperature is, for example, 950°C or more and 1150°C or less, and the time is, for example, 30 minutes to 20 hours, typically 1 hour to 10 hours. This heat treatment is preferably performed in an inert gas atmosphere similar to that described above. This heat treatment is typically performed by embedding the substrate on which the raw coating is formed in, for example, Cr powder or a mixed powder of Al powder and Al2O3 powder, and heating it in an inert gas atmosphere similar to that described above. When the raw coating is formed in multiple steps, for example, a heat treatment may be performed after the formation of the first raw coating, and then a second raw coating may be formed to form the desired raw coating. In addition, if necessary, a Cr diffusion treatment may be performed after the formation of the first raw coating, and then a second raw coating may be formed to form the desired raw coating. The Cr diffusion treatment is performed, for example, by immersing the substrate on which the raw material coating has been formed in a mixed powder containing a powder containing Ni and Cr, NH4Cl powder, and Al2O3 powder, and heating it in an inert gas atmosphere similar to that described above at a temperature of 950°C to 1150°C for 1 hour to 10 hours.
[0024] In this invention, with respect to matters other than those mentioned above, what has been explained in relation to the invention of the above-mentioned member for producing a lithium-containing composite oxide holds true, unless it is contrary to the nature of the invention.
[0025] The present invention also provides A substrate made of a metal or alloy; a coating film provided on a surface of the substrate that comes into contact with a substance generated during firing of at least the powder of the lithium (Li)-containing composite oxide raw material, the coating film containing at least aluminum (Al) and at least one metal selected from nickel (Ni), rhenium (Re) and cobalt (Co), and having a maximum aluminum (Al) concentration of 60 atomic % or more and less than 100 atomic %; The calcination furnace for producing a lithium-containing composite oxide has the following structure.
[0026] The substrate includes all substrates used in various structural members in a sintering furnace, such as furnace walls including the ceiling, supports, structural materials, etc. In this invention, with respect to matters other than those mentioned above, what has been explained in relation to the invention of the above-mentioned member for producing a Li-containing composite oxide is valid, unless it is contrary to the nature of the invention. Effect of the Invention
[0027] According to the invention, a coating film containing at least Al and Ni and at least one metal selected from Re and Co, and having a maximum Al concentration of 60 atomic % or more and less than 100 atomic %, is provided on at least the surface of a substrate made of a metal or alloy, with which the raw material powder of the lithium-containing composite oxide comes into contact, thereby making it possible to obtain excellent corrosion resistance when the raw material powder of the lithium-containing composite oxide is sintered, and since the substrate is made of a metal or alloy having excellent thermal conductivity and the coating film is also made of an alloy having excellent thermal conductivity, it is possible to realize various members for producing lithium-containing composite oxides, which have excellent temperature tracking ability and temperature uniformity when the powder is heated and cooled during sintering. Furthermore, a coating film containing at least Al and Ni and at least one metal selected from Re and Co, and having a maximum Al concentration of 60 atomic % or more and less than 100 atomic %, is provided on at least the surface of the base material made of a metal or alloy, which comes into contact with a substance generated during sintering of the raw material powder of the lithium-containing composite oxide. This makes it possible to obtain excellent corrosion resistance when sintering the raw material powder of the lithium-containing composite oxide, and also to realize a sintering furnace for producing a lithium-containing composite oxide, which has excellent temperature tracking ability and temperature uniformity during heating and cooling during sintering. [Brief description of the drawings]
[0028] [Figure 1A] 1 is a plan view showing a Li-containing composite oxide producing vessel according to a first embodiment of the present invention. [Figure 1B] 1 is a cross-sectional view showing a Li-containing composite oxide producing vessel according to a first embodiment of the present invention. [Figure 2A]FIG. 1 is a plan view for explaining a method of using a lithium-containing composite oxide producing vessel according to a first embodiment of the present invention. [Figure 2B] FIG. 1 is a cross-sectional view illustrating a method of using a lithium-containing composite oxide producing vessel according to a first embodiment of the present invention. [Figure 3A] FIG. 4 is a plan view showing a tube for producing a lithium-containing composite oxide according to a second embodiment of the present invention. [Figure 3B] FIG. 4 is a cross-sectional view showing a tube for producing a Li-containing composite oxide according to a second embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view illustrating a method of using a tube for producing a lithium-containing composite oxide according to a second embodiment of the present invention. [Figure 5A] FIG. 11 is a plan view showing a rod for producing a lithium-containing composite oxide according to a third embodiment of the present invention. [Figure 5B] FIG. 4 is a cross-sectional view showing a rod for producing a lithium-containing composite oxide according to a third embodiment of the present invention. [Figure 6] FIG. 11 is a sectional view for illustrating a method of using a rod for producing a lithium-containing composite oxide according to a third embodiment of the present invention. [Figure 7A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 1 after an Al diffusion treatment. [Figure 7B] 7B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 7A. [Figure 8A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 1 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 8B] 8B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 8A. [Figure 9A] 8B is a drawing-substitute photograph showing an enlarged portion of the Ni base material shown in FIG. 8A. [Figure 9B] 9B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 9A. [Figure 10A]1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 1 after it was immersed in molten Li2CO3 at 950°C in air for 40 hours. [Figure 10B] 10B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 10A. [Figure 11A] 10B is a drawing-substitute photograph showing an enlarged portion of the Ni base material shown in FIG. 10A. [Figure 11B] 11B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 11A. [Figure 12A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 1 after it was immersed in molten Li2CO3 at 950°C in air for 80 hours. [Figure 12B] 12B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 12A. [Figure 13A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 1 after it was immersed in molten Li2CO3 at 950°C in air for 100 hours. [Figure 13B] 13B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 13A. [Figure 14] 1 is a schematic diagram showing the relationship between the Al concentration and thickness of the coating film of the Ni substrate in Example 1 and the immersion time in molten Li 2 CO 3 . [Figure 15] 1 is a schematic diagram showing the relationship between the concentration of each element in the coating film of the Ni substrate in Example 1 and the immersion time in molten Li 2 CO 3 . [Figure 16A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 2 after an Al diffusion treatment. [Figure 16B] 16B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 16A. [Figure 17A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 2 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 17B] 17B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 17A. [Figure 18A] 17B is a photograph showing an enlarged view of a part of the Ni base material shown in FIG. 17A. [Figure 18B] 18B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 18A. [Figure 19A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 2 after it was immersed in molten Li2CO3 at 950°C in air for 40 hours. [Figure 19B] 19B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 19A. [Figure 20A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 2 after it was immersed in molten Li2CO3 at 950°C in air for 80 hours. [Figure 20B] 20B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 20A. [Figure 21A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 2 after it was immersed in molten Li2CO3 at 950°C in air for 100 hours. [Figure 21B] 21B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 21A. [Figure 22] FIG. 13 is a schematic diagram showing the relationship between the Al concentration and thickness of the coating film of the Ni substrate in Example 2 and the immersion time in molten Li2CO3. [Diagram 23] 13 is a schematic diagram showing the relationship between the concentration of each element in the coating film of the Ni substrate in Example 2 and the immersion time in molten Li2CO3. FIG. [Figure 24A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 3 after an Al diffusion treatment. [Figure 24B] 24B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 24A. [Figure 25A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 3 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 25B]25B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 25A. [Figure 26A] 25B is a drawing-substitute photograph showing an enlarged portion of the Ni base material shown in FIG. 25A. [Figure 26B] 26B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 26A. [Figure 27A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 4 after an Al diffusion treatment. [Figure 27B] 27B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 27A. [Figure 28A] 1 is a drawing-substitute photograph showing a cross-sectional structure of the Ni base material of Example 4 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 28B] 28B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 28A. [Figure 29A] 1 is a drawing-substitute photograph showing a cross-sectional structure of a SUS304 substrate of Example 5 after an Al diffusion treatment. [Figure 29B] 29B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 base material shown in FIG. 29A. [Figure 30A] 11 is a drawing-substitute photograph showing a cross-sectional structure of a SUS304 substrate of Example 5 after it was immersed in molten Li2CO3 at 950°C in air for 40 hours. [Figure 30B] 30B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 base material shown in FIG. 30A. [Figure 31A] 30B is a drawing substitute photograph showing an enlarged portion of the SUS304 base material shown in FIG. 30A. [Figure 31B] 31B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 base material shown in FIG. 31A. [Figure 32A] 1 is a drawing-substitute photograph showing a cross-sectional structure of a SUS304 substrate of Example 6 after an Al diffusion treatment. [Figure 32B]32B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 base material shown in FIG. 32A. [Figure 33A] 11 is a drawing-substitute photograph showing a cross-sectional structure of a SUS304 substrate of Example 6 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 33B] FIG. 33B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 base material shown in FIG. 33A. [Figure 34A] 33B is a drawing substitute photograph showing an enlarged portion of the SUS304 base material shown in FIG. 33A. [Figure 34B] FIG. 34B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 base material shown in FIG. 34A. [Figure 35A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 7 after an Al diffusion treatment. [Figure 35B] FIG. 35B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 35A. [Figure 36A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 7 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 36B] FIG. 36B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 36A. [Figure 37A] 36B is a drawing substitute photograph showing an enlarged portion of the SUS310 base material shown in FIG. 36A. [Figure 37B] FIG. 37B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 37A. [Figure 38A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 8 after an Al diffusion treatment. [Figure 38B] FIG. 38B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 38A. [Figure 39A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 8 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 39B] FIG. 39B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 39A. [Figure 40A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 9 after an Al diffusion treatment. [Figure 40B] FIG. 40B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 40A. [Figure 41A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 9 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 41B] 41B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 41A. [Diagram 42] 41B is a drawing substitute photograph showing an enlarged portion of the SUS310 base material shown in FIG. 41A. [Figure 43A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 10 after an Al diffusion treatment. [Figure 43B] FIG. 43B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 43A. [Figure 44A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 10 after immersion in molten Li2CO3 at 950°C in air for 20 hours. [Figure 44B] FIG. 44B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 44A. [Diagram 45] 44B is a drawing substitute photograph showing an enlarged portion of the SUS310 base material shown in FIG. 44A. [Figure 46A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 11 after an Al diffusion treatment. [Figure 46B] FIG. 46B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 46A. [Figure 47A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 11 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 47B] FIG. 47B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 47A. [Figure 48A] 47B is a drawing substitute photograph showing an enlarged portion of the SUS310 base material shown in FIG. 47A. [Figure 48B] FIG. 48B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 48A. [Figure 49A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 12 after an Al diffusion treatment. [Figure 49B] FIG. 49B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 49A. [Figure 50A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 12 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 50B] 50B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 50A. [Figure 51A] 50B is a drawing substitute photograph showing an enlarged portion of the SUS310 base material shown in FIG. 50A. [Figure 51B] 51B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 51A. [Figure 52A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 13 after an Al diffusion treatment. [Figure 52B] FIG. 52B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 52A. [Figure 53A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 13 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 53B] FIG. 53B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 53A. [Figure 54A] 53B is a drawing substitute photograph showing an enlarged portion of the SUS310 base material shown in FIG. 53A. [Figure 54B] FIG. 54B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 54A. [Figure 55A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 14 after an Al diffusion treatment. [Figure 55B] FIG. 55B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 55A. [Figure 56A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 14 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 56B] FIG. 56B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 56A. [Figure 57A] 56B is a drawing substitute photograph showing an enlarged portion of the SUS310 base material shown in FIG. 56A. [Figure 57B] FIG. 57B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 57A. [Figure 58A] 13 is a drawing-substitute photograph showing a cross-sectional structure of a SUS310 substrate of Example 15 after an Al diffusion treatment. [Figure 58B] FIG. 58B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 58A. [Figure 59A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 15 after it was immersed in molten Li2CO3 at 950°C in air for 20 hours. [Figure 59B] FIG. 59B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 59A. [Figure 60A] 13 is a drawing-substitute photograph showing a cross-sectional structure of the SUS310 substrate of Example 15 after it was immersed in molten Li2CO3 at 950°C in air for 60 hours. [Figure 60B] 60B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 60A. [Figure 61A]60B is a drawing substitute photograph showing an enlarged portion of the SUS310 base material shown in FIG. 60A. [Figure 61B] 61B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in FIG. 61A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, a mode for carrying out the invention (hereinafter simply referred to as "embodiment") will be described.
[0030] First Embodiment [Container for manufacturing Li-containing composite oxide] 1A and 1B show a Li-containing composite oxide manufacturing container 10 (hereinafter, referred to as "container 10" as necessary) according to a first embodiment, in which FIG. 1A is a plan view and FIG. 1B is a cross-sectional view (longitudinal cross-sectional view). This container 10 is used to sinter raw material powder of lithium-containing composite oxide used for a positive electrode active material of a lithium ion secondary battery. As shown in FIG. 1A and FIG. 1B, this container 10 is made of a metal or an alloy, and a coating film 12 is provided on the entire inner surface of a bowl-shaped base material 11 having a flat bottom. The boundary between the flat bottom surface and the inner side surface of the base material 11 is rounded, and reflecting this, the coating film 12 is also rounded at the same position. In this way, the raw material powder of the lithium-containing composite oxide put into the container 10 can be heated uniformly regardless of location and sintered. The coating film 12 contains at least Al and Ni and at least one metal selected from Re and Co, with the maximum Al concentration being 60 atomic % or more, preferably 70 atomic % or more, and typically 81 atomic % or less. As described above, the coating film 12 is made of various alloys such as Ni(Re,Co)-Al. If necessary, the coating film 12 may be provided on not only the inner surface but also the outer surface of the container 10. Alternatively, the coating film 12 may be provided only on the inner surface of the container 10, and a coating film made of an Al-containing alloy with an Al concentration of, for example, 20 atomic % or more may be provided on the outer surface.
[0031] The substrate 10 is selected as necessary, for example, from those already mentioned, and specifically, for example, it is made of Ni, Ni-based alloy, Fe-based alloy, etc. The Ni-based alloy is, for example, Alloy-X, etc. The Fe-based alloy is various stainless steels, for example, SUS304, SUS310, etc.
[0032] [How to use the Li-containing composite oxide manufacturing vessel] 2A and 2B, a container 10 is filled with raw material powder 20 of the Li-containing composite oxide, which is then placed in a firing furnace (not shown) and fired at a high temperature by a heating means (not shown). In this way, the desired Li-containing composite oxide is produced.
[0033] [Method of manufacturing a vessel for producing Li-containing composite oxide] A method for manufacturing this container 10 will now be described.
[0034] (1) Manufacturing method 1 First, a raw material coating containing at least Ni and at least one metal selected from Re and Co is formed on the inner surface of the substrate 11 by plating, thermal spraying, electron beam vacuum deposition, or the like. The raw material coating may be formed multiple times, for example, twice, as necessary. In this case, it is sufficient that the entire raw material coating containing at least Ni and at least one metal selected from Re and Co.
[0035] Next, the substrate 11 on which the base film is formed is subjected to an Al diffusion treatment (Al pack), so that a coating film 12 is formed on the inner surface of the substrate 11, as shown in Figures 1A and 1B. In this way, the container 10 is manufactured. The Al diffusion treatment is performed by the method described above.
[0036] (2) Manufacturing method 2 First, as in manufacturing method 1, a raw material coating containing at least Ni and at least one metal selected from Re and Co is formed on the inner surface of the substrate 11. The raw material coating may be formed multiple times, for example, twice, as necessary. In this case, it is sufficient that the entire raw material coating containing at least Ni and at least one metal selected from Re and Co.
[0037] Next, the base material 11 on which the raw material coating is formed is subjected to a heat treatment to homogenize the raw material coating. The heat treatment is performed by the method described above.
[0038] Next, the base material 11 thus heat-treated is subjected to an Al diffusion treatment, thereby forming a coating film 12 on the inner surface of the base material 11. In this manner, the container 10 is manufactured.
[0039] (3) Manufacturing method 3 First, in the same manner as in Production Method 1, a first layer raw material coating containing at least Ni and at least one metal selected from the group consisting of Re and Co is formed on the inner surface of the substrate 11 .
[0040] Next, the base material 11 on which the first layer of the raw material coating is formed is subjected to a heat treatment to homogenize the raw material coating. The heat treatment is performed by the method described above.
[0041] Next, a second layer of raw film is formed on the first layer of raw film that has been heat-treated in this manner.
[0042] Thereafter, the substrate 11 on which the second-layer base film has been formed is subjected to an Al diffusion treatment, thereby forming a coating film 12 on the inner surface of the substrate 11. In this manner, the container 10 is manufactured.
[0043] (4) Manufacturing method 4 First, in the same manner as in Production Method 1, a first layer raw material coating containing at least Ni and at least one metal selected from the group consisting of Re and Co is formed on the inner surface of the substrate 11 .
[0044] Next, the substrate 11 on which the first layer of the base coating is formed is subjected to a Cr diffusion treatment (Cr pack). The Cr diffusion treatment is performed by the method described above.
[0045] Next, a second layer of raw film is formed on the first layer of raw film that has been subjected to the Cr diffusion treatment.
[0046] Thereafter, the substrate 11 on which the second-layer base film has been formed is subjected to an Al diffusion treatment, thereby forming a coating film 12 on the inner surface of the substrate 11. In this manner, the container 10 is manufactured.
[0047] As described above, according to the first embodiment, the Li-containing composite oxide producing container 10 is constructed by providing the coating film 12, which contains at least Al and Ni and at least one metal selected from Re and Co and has a maximum Al concentration of 60 atomic % or more, on the entire inner surface of the base material 11 made of a metal or alloy such as Ni, a Ni-based alloy, or an Fe-based alloy. Therefore, excellent corrosion resistance can be obtained when firing the powder of the raw material of the lithium-containing composite oxide, and since the base material 11 is made of a metal or alloy with excellent thermal conductivity and the coating film 12 is also made of an alloy with similarly excellent thermal conductivity, the lithium-containing composite oxide producing container 12 can be realized that has excellent temperature follow-up ability and temperature uniformity in heating and cooling the powder when firing.
[0048] Second embodiment [Li-containing composite oxide production tube] 3A and 3B show a tube 30 for producing a Li-containing composite oxide according to a second embodiment (hereinafter referred to as "tube 30" as necessary), with FIG. 3A being a plan view and FIG. 3B being a cross-sectional view (longitudinal cross-sectional view). This tube 30 is an associated member used together with the container 10 according to the first embodiment. As shown in FIGS. 3A and 3B, in this tube 10, a coating film 32 is provided on the entire outer and inner surfaces as well as the lower end surface of a cylindrical substrate 31 made of a metal or alloy. The coating film 32 is the same as the coating film 12. The substrate 31 is also the same as the substrate 10 except for its shape.
[0049] [How to use the tube for manufacturing Li-containing composite oxides] 4, powder 20, which is the raw material of the Li-containing composite oxide, is charged into a container 10, and calcination is carried out with a tube 30 inserted inside the powder 20, thereby producing the desired Li-containing composite oxide. In this case, carbon dioxide (CO2), which is generated as a reaction by-product during calcination, is efficiently discharged to the outside of the container 10 through the tube 30.
[0050] [Method of manufacturing tubes for producing Li-containing composite oxides] The method for manufacturing the tube 30 is basically the same as the method for manufacturing the container 10 .
[0051] According to the second embodiment, it is possible to obtain excellent corrosion resistance when calcining the powder of the raw material of the lithium-containing composite oxide, and further to realize a tube 30 for producing a lithium-containing composite oxide that is excellent in temperature followability and temperature uniformity in heating and cooling the powder when calcining.
[0052] Third embodiment [Rod for producing Li-containing composite oxide] 5A and 5B show a rod 40 for producing a Li-containing composite oxide according to a third embodiment (hereinafter referred to as "rod 40" as necessary), with FIG. 5A being a plan view and FIG. 5B being a cross-sectional view (longitudinal cross-sectional view). This rod 40 is an associated member used together with the container 10 according to the first embodiment. As shown in FIGS. 5A and 5B, in this rod 40, a coating film 42 is provided on the entire outer surface of a round bar-shaped substrate 41 made of a metal or alloy. The coating film 42 is the same as the coating film 12. The substrate 41 is also the same as the substrate 11 except for its shape.
[0053] [How to use the tube for manufacturing Li-containing composite oxides] 6, a powder 20 as a raw material for the Li-containing composite oxide is put into a container 10, and sintering is carried out with a rod 40 inserted inside the powder 20 to produce the desired Li-containing composite oxide. In general, a tube 30 is inserted into the powder 20 in addition to the rod 40 before use.
[0054] According to the third embodiment, it is possible to obtain excellent corrosion resistance when sintering the powder of the raw material of the lithium-containing composite oxide, and further to realize a lithium-containing composite oxide manufacturing rod 40 having excellent temperature follow-up ability and temperature uniformity in heating and cooling the powder when sintering. EXAMPLES
[0055] An embodiment will be described.
[0056] The following three types of substrates were used in the following Examples 1 to 15. The nominal composition (mass %) of each substrate is shown below.
[0057] (1)Ni base material (2) SUS304 base material (3) SUS310 base material
[0058] The nominal composition (mass%) of each base material is as follows:
[0059] (1)Ni base material C Si Mn Cr Ni Fe Cu Al 0.02 or less 0.35 or less 0.35 or less none 99 or more 0.40 or less 0.25 or less none (2) SUS304 base material C Si Mn Cr Ni Fe Cu Al 0.08 or less 1.5 or less 2.0 or less 24.00-26.00 19.00-22.00 Remaining none none (3) SUS310 base material C Si Mn Cr Ni Fe Cu Al 0.08 or less 1.0 or less 2.0 or less 18.00-20.00 8.00-10.50 Remaining none none
[0060] Example 1 A coating film was formed on a Ni substrate by Manufacturing Method 2.
[0061] First, the surface of the Ni base material was polished to be smooth and degreased, and then a Ni strike film, a Re(Ni) film, and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by plating in that order. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was performed at 60 mA / cm for 1 min. The composition of the plating solution was 0.1 atomic % Co and 99.9 atomic % Ni. The plating of the Re(Ni) film was performed at a current density of 60 mA / cm 2 The plating was performed for 60 minutes at 6000 K, and the composition of the plating solution was 0.2 atomic % Co, 59.2 atomic % Ni, and 40.3 atomic % Re. The plating of the Co-containing Re(Ni) film was performed at a current density of 60 mA / cm 2 The plating was carried out for 90 minutes at room temperature, and the composition of the plating solution was 10.5 atomic % Co, 60.7 atomic % Ni, and 28.5 atomic % Re.
[0062] Next, the Ni base material on which the plating film was formed was subjected to a heat treatment by embedding the Ni base material on which the plating film was formed in a mixed powder of 10 g of Cr powder and 100 g of Al2O3 powder, and heating it at 1100°C for 2 hours in an Ar + 3 vol% H2 atmosphere.
[0063] Next, the heat-treated Ni substrate was subjected to an Al diffusion treatment by embedding the heat-treated Ni substrate in a mixture of 8 g of Al powder, 2 g of NH4Cl powder, and 100 g of Al2O3 powder, and heating it at 1100°C for 2 hours in an Ar + 3 vol% H2 atmosphere.
[0064] A part of the Ni substrate / coating surface after Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured using a SEM-EDX (scanning electron microscope-energy dispersive spectroscopy) device. Figures 7A and 7B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 7A) measured using EDX, respectively. Figures 7A and 7B show that a coating film made of Ni(Re,Co)-Al is formed on the Ni substrate. The maximum Al concentration of this coating film is about 77 atomic %, and the Al concentration is 60 atomic % or more in most parts in the thickness direction except for the part on the Ni substrate side. Such a high Al concentration is obtained because the coating film contains Re and Co. Re is concentrated in the part of this coating film on the Ni substrate side, and this part becomes a diffusion barrier layer.
[0065] The Ni substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for four periods: 20 hours, 40 hours, 80 hours, and 100 hours.
[0066] After the 20-hour immersion test, a part of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 8A and 8B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 8A), respectively. Figures 8A and 8B show that the coating film made of Ni(Re,Co)-Al is maintained, the maximum value of the Al concentration is 50 atomic % or more, and the Al concentration is 40 atomic % or more in most parts in the thickness direction except for the part on the Ni substrate side. It can be seen that the Re in the diffusion barrier layer is further aggregated to have a high Re concentration. The Al concentration in the diffusion barrier layer is reduced. The Ni concentration is higher than the Co concentration in the entire coating film. Figures 9A and 9B show a cross-sectional SEM photograph of an enlarged part of the cross-sectional structure (surface side part) shown in Figure 8A, and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 9A), respectively. 9A and 9B show that an oxide made of Al2O3 is formed in close contact with the surface of the Ni(Re,Co)-Al layer. The (Ni,CoAl) oxide is observed on the top surface of the oxide.
[0067] After the 40-hour immersion test, a part of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 10A and 10B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG1 in the photograph shown in Figure 10A), respectively. As shown in Figures 10A and 10B, no significant changes were observed in the coating film compared to the Ni substrate that had been immersed for 20 hours. The maximum Al concentration of the coating film was 40 atomic % or more, and the Al concentration was 40 atomic % or more in most parts in the thickness direction except for the part on the Ni substrate side. Figures 11A and 11B show a cross-sectional SEM photograph of an enlarged part of the cross-sectional structure shown in Figure 10A (the part on the surface side) and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 11A), respectively. As shown in Figures 11A and 11B, an oxide made of Al2O3 was formed in close contact with the surface of the Ni(Re,Co)-Al layer. On the outermost surface of the oxide, (Al, Ni, Co) oxides are observed.
[0068] After the 80-hour immersion test, a portion of the Ni substrate / coating surface was cut to observe its cross-sectional structure and measure the concentration distribution of each element. Figures 12A and 12B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 12A), respectively. Figures 12A and 12B show that the maximum Al concentration is 40 atomic % or more. An oxide made of Al2O3 is formed in close contact with the surface of the Ni(Re, Co)-Al layer. An (Al, Ni, Co) oxide is observed on the top surface of the oxide.
[0069] After the 100-hour immersion test, a portion of the Ni substrate / coating surface was cut to observe its cross-sectional structure and measure the concentration distribution of each element. Figures 13A and 13B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 13A), respectively. Figures 13A and 13B show that an oxide made of Al2O3 is formed in close contact with the surface of the Ni(Re, Co)-Al layer. The maximum Al concentration of the coating film is 40 atomic % or more. (Al, Ni, Co) oxides are observed on the outermost surface of the oxide. The diffusion barrier layer of the coating film is maintained.
[0070] The results of the above immersion tests show that by forming a coating film consisting of Ni(Re,Co)-Al on a Ni substrate with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0071] Figure 14 shows the change in the Al concentration (maximum value) in the coating film and the thickness of the coating film versus the immersion time in molten Li2CO3. As shown in Figure 14, both the Al concentration in the coating film and the thickness of the coating film rapidly decrease from the start of immersion until 20 hours have elapsed, but the decrease thereafter becomes gradual, and even after 100 hours have elapsed, the Al concentration (maximum value) is approximately 40 atomic % or more. Figure 15 shows the change in the Al concentration (maximum value) and the concentrations (maximum values) of Co, Ni, and Re in the coating film versus the immersion time in molten Li2CO3. As shown in Figure 15, Ni increases rapidly from the start of immersion until 20 hours have elapsed, but the increase thereafter becomes gradual.
[0072] Example 2 A coating film was formed on a Ni substrate by Manufacturing Method 1.
[0073] First, the surface of the Ni base material was polished to be smooth and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by a plating method. The plating conditions of the Ni strike film and the composition of the plating solution were the same as in Example 1. The plating conditions of the Co-containing Re(Ni) film and the composition of the plating solution were the same as in Example 1. Then, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed by a plating method. The plating of the Ni strike film was performed in the same manner as above. The plating conditions of the Co-containing Re(Ni) film and the composition of the plating solution were the same as in Example 1.
[0074] Next, the Ni base material having the plating film formed thereon was subjected to a heat treatment under the same conditions as in Example 1.
[0075] Next, the Ni base material thus heat-treated was subjected to an Al diffusion treatment under the same conditions as in Example 1.
[0076] After the Al diffusion treatment, a portion of the Ni substrate / coating surface was cut to observe its cross-sectional structure and to measure the concentration distribution of each element. Figures 16A and 16B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG5 in the photograph shown in Figure 16A), respectively. Figures 16A and 16B show that a coating film made of Ni(Re,Co)-Al has been formed on the Ni substrate. The maximum Al concentration of this coating film is approximately 77 atomic %, and the Al concentration is 60 atomic % or more in most parts in the thickness direction, except for the part on the Ni substrate side.
[0077] The Ni substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for four periods: 20 hours, 40 hours, 80 hours, and 100 hours.
[0078] After the 20-hour immersion test, a part of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 17A and 17B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 17A), respectively. From Figures 17A and 17B, it can be seen that the maximum value of the Al concentration of the coating film is 40 atomic % or more. Figures 18A and 18B show a cross-sectional SEM photograph of an enlarged part of the cross-sectional structure shown in Figure 17A, and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG5 in the photograph shown in Figure 18A), respectively. From Figures 18A and 18B, it can be seen that an oxide made of Al2O3 is formed in close contact with the surface of the Ni(Re,Co)-Al layer. (Al,Ni,Co) oxides are observed on the outermost surface of the oxide.
[0079] After the 40-hour immersion test, a portion of the Ni substrate / coating surface was cut to observe its cross-sectional structure and measure the concentration distribution of each element. Figures 19A and 19B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 19A), respectively. Figures 19A and 19B show that the maximum Al concentration of the coating film was 40 atomic % or more.
[0080] After the 80-hour immersion test, a portion of the Ni substrate / coating surface was cut to observe its cross-sectional structure and measure the concentration distribution of each element. Figures 20A and 20B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 20A), respectively. Figures 20A and 20B show that the maximum Al concentration of the coating film is still 40 atomic % or more. An oxide made of Al2O3 is formed in close contact with the surface of the Ni(Re,Co)-Al layer. An (Al,Ni,Co) oxide is observed on the top surface of the oxide.
[0081] After the 100-hour immersion test, a portion of the Ni substrate / coating surface was cut to observe its cross-sectional structure and measure the concentration distribution of each element. Figures 21A and 21B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG6 in the photograph shown in Figure 21A), respectively. Figures 21A and 21B show that the maximum Al concentration of the coating film is still 40 atomic % or more. An oxide made of Al2O3 is formed in close contact with the surface of the Ni(Re,Co)-Al layer. An (Al,Ni,Co) oxide is observed on the top surface of the oxide.
[0082] The results of the above immersion tests show that by forming a coating film consisting of Ni(Re,Co)-Al on a Ni substrate with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0083] Figure 22 shows the change in the Al concentration (maximum value) in the coating film and the thickness of the coating film versus the immersion time in molten Li2CO3. As shown in Figure 22, both the Al concentration in the coating film and the thickness of the coating film rapidly decrease from the start of immersion until 20 hours have elapsed, but the decrease thereafter becomes gradual, and even after 100 hours the Al concentration (maximum value) remains high at approximately 40 atomic %. Figure 23 shows the change in the Al concentration (maximum value) and the concentrations (maximum values) of Co, Ni, and Re in the coating film versus the immersion time in molten Li2CO3. As shown in Figure 23, Ni increases rapidly from the start of immersion until 20 hours have elapsed, but the increase thereafter becomes gradual.
[0084] Example 3 A coating film was formed on a Ni substrate by Manufacturing Method 2.
[0085] First, the surface of the Ni base material was polished to be smooth and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 50 mass% Co were formed on the surface by plating. The plating conditions for the Ni strike film and the composition of the plating solution were the same as in Example 1. The plating of the Co-containing Re(Ni) film was performed at a current density of 60 mA / cm. 2 The plating was carried out for 60 minutes at 85.5 atomic % Co, 3.2 atomic % Ni, and 11.2 atomic % Re. Next, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass % Co were formed in that order by plating. The Ni strike film was plated in the same manner as above. The Co-containing Re(Ni) film was plated at a current density of 60 mA / cm. 2 The plating was carried out for 90 minutes using a plating solution having the same composition as in Example 1.
[0086] Next, the Ni base material having the plating film formed thereon was subjected to a heat treatment under the same conditions as in Example 1.
[0087] Next, the Ni base material thus heat-treated was subjected to an Al diffusion treatment under the same conditions as in Example 1.
[0088] A part of the Ni substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 24A and 24B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG6 in the photograph shown in Figure 24A), respectively. Figures 24A and 24B show that a coating film made of Co(Ni, Re)-Al is formed on the Ni substrate. The maximum Al concentration of this coating film is about 76 atomic %, and the Al concentration is 60 atomic % or more in most parts in the thickness direction except for the part on the Ni substrate side. Co contained in Co(Ni, Re)-Al contributes to obtaining such a high Al concentration.
[0089] The Ni substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0090] After the 20-hour immersion test, a part of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 25A and 25B show a cross-sectional SEM photograph and the measurement result of the concentration distribution of each element (concentration distribution along the analysis line of the photograph shown in Figure 25A) measured by EDX, respectively. From Figures 25A and 25B, it can be seen that a Co(Ni, Re)-Al layer and a Ni(Co, Re)-Al layer are formed in sequence on the Ni substrate to form a coating film. The maximum value of the Al concentration of this coating film is 60 atomic % or more. Figures 26A and 26B show a cross-sectional SEM photograph in which a part of the cross-sectional structure (the part on the surface side) shown in Figure 25A is enlarged, and the measurement result of the concentration distribution of each element (concentration distribution along the analysis line LG5 of the photograph shown in Figure 26A) is shown, respectively. From Figures 26A and 26B, it can be seen that an oxide made of Al2O3 is formed in close contact with the surface of the Ni(Re, Co)-Al layer. On the outermost surface of the oxide, (Al, Ni, Co) oxides are observed.
[0091] The results of the above immersion tests show that by forming a coating film consisting of Ni(Re,Co)-Al on a Ni substrate with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0092] Example 4 A coating film was formed on a Ni substrate by Manufacturing Method 3.
[0093] First, the surface of the Ni base material was polished to be smooth and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by a plating method. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was performed for 3 minutes at a current density of 60 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 120 minutes using the same plating solution composition as in Example 1.
[0094] Next, the Ni substrate on which the plating film was formed was subjected to a heat treatment by embedding the Ni substrate on which the plating film was formed in a mixture of 2 g of Al powder and 100 g of Al2O3 powder, and heating it at 1100°C for 1.5 hours in an Ar + 3 vol% H2 atmosphere.
[0095] Next, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed in this order by plating again. The Ni strike film was plated in the same manner as above. The Co-containing Re(Ni) film was plated at a current density of 60 mA / cm 2 The plating was carried out for 75 minutes using a plating solution having the same composition as in Example 1.
[0096] Next, the Ni substrate on which the second-layer plating film was formed was subjected to an Al diffusion treatment by burying the Ni substrate on which the second-layer plating film was formed in a mixture of 7 g of Al powder, 2 g of NH4Cl powder, and 100 g of Al2O3 powder, and heating it at 1100°C for 1.5 hours in an Ar + 3 vol% H2 atmosphere.
[0097] After the Al diffusion treatment, a portion of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 27A and 27B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 27A), respectively. Figures 27A and 27B show that a coating film consisting of Co, Ni, Re layers, Re-Al layers, and Co, Ni-Al layers was formed on the Ni substrate. The maximum Al concentration of this coating film was approximately 64 atomic %.
[0098] The Ni substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0099] After the 20-hour immersion test, a portion of the Ni substrate / coating surface was cut to observe its cross-sectional structure and to measure the concentration distribution of each element. Figures 28A and 28B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG2 in the photograph shown in Figure 28A), respectively. Figures 28A and 28B show that the maximum Al concentration of the coating film is approximately 55 atomic %, and that the Al concentration is 40 atomic % or more in most parts in the thickness direction, except for the part on the Ni substrate side. An oxide made of Al2O3 is formed in close contact with the surface of the Co and Ni-Al layers.
[0100] The results of the above immersion tests show that by forming a coating film consisting of a Co, Ni, Re layer, a Re-Al layer, and a Co, Ni-Al layer on a Ni substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0101] Example 5 A coating film was formed on a SUS304 substrate by Manufacturing Method 1.
[0102] First, the surface of the SUS304 substrate was polished to be smooth and degreased, and then a Ni strike film, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed on the surface by plating in this order. The Ni strike film was plated under the same conditions as in Example 1, and the composition of the plating solution was the same as in Example 1. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm. 2 The plating was performed for 60 minutes at a current density of 40 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 20 minutes at room temperature, and the composition of the plating solution was 99.1 atomic % Co and 0.5 atomic % Ni.
[0103] Next, the SUS304 substrate on which the plating film was formed was subjected to an Al diffusion treatment by embedding the SUS304 substrate on which the plating film was formed in a mixture of 7 g of Al powder, 2 g of NH4Cl powder, and 90 g of Al2O3 powder, and heating it at 1000°C for 6 hours in an Ar + 3 vol% H2 atmosphere.
[0104] After the Al diffusion treatment, a portion of the SUS304 substrate / coating surface was cut to observe its cross-sectional structure and measure the concentration distribution of each element. Figures 29A and 29B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 29A), respectively. Figures 29A and 29B show that a coating film consisting of a (Co, Ni, Re)-Al layer and a Co-Al layer is formed on the SUS304 substrate. The maximum Al concentration of this coating film is approximately 76 atomic %, and the Al concentration is 60 atomic % or more in most parts in the thickness direction, except for the part on the SUS304 substrate side.
[0105] The Ni substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 40 hours.
[0106] After the 40-hour immersion test, a portion of the SUS304 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 30A and 30B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 30A), respectively. From Figures 30A and 30B, it can be seen that the Al concentration of the coating film remains around 50 atomic % even after 40 hours of immersion. Protective Al2O3 is formed inside the outermost Co-Al layer. Fe in the SUS304 substrate diffuses to the vicinity of the outer layer. Figures 31A and 31B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure shown in Figure 30A (the surface side portion) and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 31A), respectively. From Figures 31A and 31B, it can be seen that the Al concentration of the Co-Al layer has decreased to around 30 atomic %. The top layer of the coating film is made of an oxide of Al2O3.
[0107] The results of the above immersion tests show that by forming a coating film consisting of a (Co, Ni, Re)-Al layer and a Co-Al layer on a SUS304 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0108] Example 6 Example 6 corresponds to the first embodiment.
[0109] A coating film was formed on a SUS304 substrate by Manufacturing Method 1.
[0110] First, the surface of a SUS304 substrate was polished to be smooth and degreased, and then a Ni strike film, a Ni film using a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were successively formed on the surface by plating. The Ni strike film was plated under the same conditions as in Example 1, and the composition of the plating solution was the same as in Example 1. The Ni film was plated using a Watts bath at a current density of 40 mA / cm. 2The plating was performed for 10 minutes at a current density of 40 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was performed for 90 minutes at a current density of 40 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 60 minutes using a plating solution having the same composition as in Example 5.
[0111] Next, the SUS304 substrate on which the plating film was formed was subjected to an Al diffusion treatment by embedding the SUS304 substrate on which the plating film was formed in a mixture of 8 g of Al powder, 2 g of NH4Cl powder, and 90 g of Al2O3 powder, and heating it at 1000°C for 4 hours in an Ar + 3 vol% H2 atmosphere.
[0112] After the Al diffusion treatment, a portion of the SUS304 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 32A and 32B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG1 in the photograph shown in Figure 32A), respectively. Figures 32A and 32B show that a coating film consisting of Co, Ni, Re-Al layers, and Co-Al layers was formed on the SUS304 substrate. The maximum Al concentration of this coating film was approximately 77 atomic %, and the Al concentration was 60 atomic % or more in most parts in the thickness direction, except for the part on the SUS304 substrate side.
[0113] The Ni substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0114] After the 20-hour immersion test, a portion of the SUS304 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 33A and 33B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 33A), respectively. From Figures 33A and 33B, it can be seen that even after 20 hours of immersion, the maximum value of the Al concentration of the coating film remains at 60 atomic % or more, and the Al concentration is 40 atomic % or more in most parts in the thickness direction except for the part on the SUS304 substrate side. Figures 34A and 34B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure shown in Figure 33A (the part on the surface side) and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG7 in the photograph shown in Figure 34A), respectively. From Figures 34 and 34B, it can be seen that dense protective Al2O3 is formed on the surface of the Co-Al layer.
[0115] The above immersion test results show that by forming a coating film consisting of Co, Ni, Re-Al layers, and Co-Al layers on a SUS304 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0116] Example 7 A coating film was formed on a SUS310 substrate by manufacturing method 3.
[0117] First, the surface of the SUS310 substrate was polished to be smooth and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by a plating method. The Ni strike film was plated under the same conditions as in Example 1, and the composition of the plating solution was the same as in Example 1. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm 2 The plating was performed for 60 minutes using a plating solution having the same composition as in Example 1.
[0118] Next, the SUS310 substrate on which the plating film was formed was subjected to a heat treatment by embedding the SUS310 substrate on which the plating film was formed in a mixture of 2 g of Al powder and 100 g of Al2O3 powder, and heating it at 1100°C for 2 hours in an Ar + 3 vol% H2 atmosphere.
[0119] Next, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed in this order on the heat-treated SUS310 substrate by plating. The Ni strike film was plated at a current density of 0.5 A / cm 2 The plating was performed for 3 minutes at a current density of 60 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was performed for 60 minutes using a plating solution having the same composition as in Example 1.
[0120] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment by embedding the heat-treated SUS310 substrate in a mixture of 10 g of Al powder, 2 g of NH4Cl powder, and 100 g of Al2O3 powder, and heating it at 1100°C for 2 hours in an Ar + 3 vol% H2 atmosphere.
[0121] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 35A and 35B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 35A), respectively. Figures 35A and 35B show that a coating film consisting of Co, Re, Fe, Cr, Ni layers and a Co(Ni, Re)-Al layer was formed on the SUS310 substrate. The maximum Al concentration of this coating film was approximately 67 atomic %.
[0122] The SUS310 substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0123] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 36A and 36B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG1 in the photograph shown in Figure 36A), respectively. From Figures 36A and 36B, it can be seen that even after 20 hours of immersion, the maximum Al concentration of the coating film was around 60 atomic %, and the Al concentration was 40 atomic % or more in most parts of the Co(Ni, Re)-Al layer in the thickness direction. Figures 37A and 37B show a cross-sectional SEM photograph of an enlarged portion (surface side portion) of the cross-sectional structure shown in Figure 36A, and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG1 in the photograph shown in Figure 37A), respectively. From Figures 37A and 37B, it can be seen that dense protective Al2O3 is formed on the surface of the Co(Ni, Re)-Al layer.
[0124] The results of the above immersion tests show that by forming a coating film consisting of Co, Re, Fe, Cr, Ni layers and a Co(Ni, Re)-Al layer on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0125] Example 8 A coating film was formed on a SUS310 substrate by manufacturing method 3.
[0126] First, the surface of the SUS310 substrate was polished to be smooth and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by plating. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was performed for 3 minutes at a current density of 60 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 120 minutes using the same plating solution composition as in Example 1.
[0127] Next, the SUS310 substrate on which the plating film was formed was subjected to a heat treatment by embedding the SUS310 substrate on which the plating film was formed in a mixture of 2 g of Al powder and 100 g of Al2O3 powder, and heating it at 1100°C for 1.5 hours in an Ar + 3 vol% H2 atmosphere.
[0128] Next, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed in this order on the heat-treated SUS310 substrate by plating. The Ni strike film was plated at a current density of 0.5 A / cm 2 The plating was performed for 3 minutes at a current density of 60 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 75 minutes using a plating solution having the same composition as in Example 1.
[0129] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment by embedding the heat-treated SUS310 substrate in a mixture of 7 g of Al powder, 2 g of NH4Cl powder, and 100 g of Al2O3 powder, and heating it at 1100°C for 1.5 hours in an Ar + 3 vol% H2 atmosphere.
[0130] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut to observe the cross-sectional structure and measure the concentration distribution of each element. Figures 38A and 38B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG1 in the photograph shown in Figure 38A), respectively. Figures 38A and 38B show that a coating film consisting of Co, Re, Fe, Cr, Ni layers and Co, Ni, Re-Al layers has been formed on the SUS310 substrate. The maximum Al concentration of the coating film is approximately 64 atomic %.
[0131] The SUS310 substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0132] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut to observe the cross-sectional structure and measure the concentration distribution of each element. Figures 39A and 39B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG1 in the photograph shown in Figure 39A), respectively. Figures 39A and 39B show that even after 20 hours of immersion, the maximum Al concentration of the coating film is approximately 66 atomic %. Only the outermost Co, Ni, and Re-Al layers of the coating film are corroded. Protective Al2O3 is formed in close contact with the surface of the outermost Co, Ni, and Re-Al layers.
[0133] The results of the above immersion tests show that by forming a coating film consisting of Co, Re, Fe, Cr, Ni layers and Co, Ni, Re-Al layers on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0134] Example 9 A coating film was formed on a SUS310 substrate by Manufacturing Method 4.
[0135] First, the surface of the SUS310 substrate was polished and degreased, and then a Ni strike film and a Re(Ni) film were formed on the surface by plating. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was performed for 3 minutes at a current density of 60 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 90 minutes using a plating solution having the same composition as in Example 1.
[0136] Next, the SUS310 substrate on which the plating film was formed was subjected to a Cr diffusion treatment (Cr pack). The Cr diffusion treatment was performed by embedding the SUS310 substrate on which the plating film was formed in a mixture of 5 g of (Ni+Cr) powder, 2 g of NH4Cl powder, and 100 g of Al2O3 powder, and heating it at 1100°C for 2 hours in an Ar+3 vol% H2 atmosphere.
[0137] Next, a Ni strike film and a Re(Ni) film were formed in this order on the SUS310 substrate that had been subjected to the Cr diffusion treatment by plating. The Ni strike film was plated at a current density of 0.5 A / cm 2 The plating was performed for 1 minute at a current density of 60 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 90 minutes using a plating solution having the same composition as in Example 1.
[0138] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment by burying the SUS310 substrate on which the plating film was formed in a mixture of 7 g of Al powder, 2 g of NH4Cl powder, and 100 g of Al2O3 powder, and heating it at 1100°C for 2 hours in an Ar + 3 vol% H2 atmosphere.
[0139] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut to observe its cross-sectional structure and measure the concentration distribution of each element. Figures 40A and 40B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 40A), respectively. Figures 40A and 40B show that a coating film consisting of a Ni, Re, Fe, Cr layer and a Ni, Re-Al layer has been formed on the SUS310 substrate. The maximum Al concentration of the coating film is approximately 67 atomic %.
[0140] The SUS310 substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 6 hours.
[0141] After the 6-hour immersion test, a portion of the SUS310 substrate / coating surface was cut to observe the cross-sectional structure and measure the concentration distribution of each element. Figures 41A and 41B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 41A), respectively. Figure 42 shows a cross-sectional SEM photograph in which a portion (the surface side portion) of the cross-sectional structure shown in Figure 41A is enlarged. Figures 41A, 41B, and 42 show that even after immersion for 6 hours, the maximum Al concentration of the coating film is about 70 atomic %. Only the outermost Ni and Re-Al layers are corroded. Protective Al2O3 is formed in close contact with the surface of the outermost Ni and Re-Al layers.
[0142] The results of the above immersion tests show that by forming a coating film consisting of a Ni, Re, Fe, Cr layer and a Ni, Re-Al layer on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0143] Example 10 A coating film was formed on a SUS310 substrate by Manufacturing Method 4.
[0144] First, the surface of the SUS310 substrate was polished to be smooth and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by plating. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was performed for 3 minutes at a current density of 60 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 90 minutes using a plating solution having the same composition as in Example 1.
[0145] Next, the SUS310 substrate on which the plating film was formed was subjected to a Cr diffusion treatment (Cr pack). The Cr diffusion treatment was performed by embedding the SUS310 substrate on which the plating film was formed in a mixture of 5 g of (Ni+Cr) powder, 2 g of NH4Cl powder, and 100 g of Al2O3 powder, and heating it at 1100°C for 2 hours in an Ar+3 vol% H2 atmosphere.
[0146] Next, a Ni strike film and a Re(Ni) film were formed in this order on the SUS310 substrate that had been subjected to the Cr diffusion treatment by plating. The Ni strike film was plated at a current density of 0.5 A / cm 2 The plating was performed for 1 minute at a current density of 60 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 90 minutes using a plating solution having the same composition as in Example 1.
[0147] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was performed in the same manner as in Example 8.
[0148] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 43A and 43B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 43A), respectively. Figures 43A and 43B show that a coating film consisting of a Co, Re, Fe, Cr layer and a Ni, Re-Al layer was formed on the SUS310 substrate. The maximum Al concentration of the coating film was approximately 65 atomic %.
[0149] The SUS310 substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 6 hours.
[0150] After the 6-hour immersion test, a portion of the SUS310 substrate / coating surface was cut to observe the cross-sectional structure and measure the concentration distribution of each element. Figures 44A and 44B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG5 in the photograph shown in Figure 44A), respectively. Figure 45 shows a cross-sectional SEM photograph in which a portion (the surface side portion) of the cross-sectional structure shown in Figure 44A is enlarged. Figures 44A, 44B, and 45 show that even after immersion for 6 hours, the maximum Al concentration of the coating film is about 66 atomic %. Only the outermost Ni and Re-Al layers are corroded. Protective Al2O3 is formed in close contact with the surface of the outermost Ni and Re-Al layers.
[0151] The results of the above immersion tests show that by forming a coating film consisting of a Co, Re, Fe, Cr layer and a Ni, Re-Al layer on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0152] Example 11 A coating film was formed on a SUS310 substrate by manufacturing method 3.
[0153] First, the surface of the SUS310 substrate was polished to be smooth and degreased, and then a Ni strike film, a Ni film using a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were successively formed on the surface by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film was plated in the Watts bath in the same manner as in Example 6. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm 2 The plating was performed for 30 minutes at a current density of 40 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was performed for 30 minutes using a plating solution having the same composition as in Example 5.
[0154] Next, the SUS310 substrate on which the plating film was formed was subjected to a heat treatment by embedding the SUS310 substrate on which the plating film was formed in a mixture of 10 g of Cr powder and 90 g of Al2O3 powder, and heating it at 1000°C for 4 hours in an Ar + 3 vol% H2 atmosphere.
[0155] Next, on the SUS310 substrate thus heat-treated, a Ni strike film, a Ni film by a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed in this order by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film was plated by a Watts bath at a current density of 40 mA / cm. 2 The plating was performed for 10 minutes at 4000 K, and the composition of the plating solution was 0.1 atomic % Co and 99.9 atomic % Ni. The plating of the Co-containing Re(Ni) film was performed at a current density of 40 mA / cm 2 The plating was performed for 60 minutes at a current density of 40 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating solution had the same composition as in Example 5.
[0156] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment by embedding the SUS310 substrate on which the plating film was formed in a mixture of 8 g of Al powder, 2 g of NH4Cl powder, and 90 g of Al2O3 powder, and heating it at 1000°C for 4 hours in an Ar + 3 vol% H2 atmosphere.
[0157] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 46A and 46B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 46A), respectively. Figures 46A and 46B show that a coating film consisting of Co, Ni, Re-Al layers, and Co-Al layers is formed on the SUS310 substrate. The maximum Al concentration of this coating film is 80 atomic %, and the Al concentration is 60 atomic % or more in most parts in the thickness direction, except for the part on the SUS310 substrate side.
[0158] The SUS310 substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0159] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 47A and 47B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 47A), respectively. From Figures 47A and 47B, it can be seen that even after 20 hours of immersion, the maximum Al concentration of the coating film was about 78 atomic %, and the overall Al concentration was 40 atomic % or more. Figures 48A and 48B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure shown in Figure 47A (the portion on the surface side) and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG6 in the photograph shown in Figure 48A), respectively. From Figures 48A and 48B, it can be seen that dense protective Al2O3 is formed in close contact with the surface of the Co(Ni)-Al layer.
[0160] The results of the above immersion tests show that by forming a coating film consisting of Co, Ni, Re-Al layers and Co-Al layers on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0161] Example 12 A coating film was formed on a SUS310 substrate by manufacturing method 3.
[0162] First, the surface of the SUS310 substrate was polished to be smooth and degreased, and then a Ni strike film, a Ni film using a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were successively formed on the surface by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film was plated in the Watts bath in the same manner as in Example 11. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm 2The plating was performed for 30 minutes at 4000 K, the composition of the plating solution was 10.5 atomic % Co, 60.7 atomic % Ni, and 28.5 atomic % Re. The plating of the Co film was performed at a current density of 40 mA / cm 2 The plating was performed for 30 minutes using a plating solution having the same composition as in Example 5.
[0163] Next, the SUS310 base material having the plating film formed thereon was subjected to a heat treatment in the same manner as in Example 10.
[0164] Next, on the SUS310 substrate thus heat-treated, a Ni strike film, a Ni film by a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed in this order by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film by a Watts bath was plated in the same manner as in Example 11. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm. 2 The plating was performed for 60 minutes at a current density of 40 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating solution had the same composition as in Example 5.
[0165] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was performed in the same manner as in Example 10.
[0166] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 49A and 49B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 49A), respectively. Figures 49A and 49B show that a coating film consisting of Co, Re, Ni-Al layers, and Co(Ni)-Al layers is formed on the SUS310 substrate. The maximum Al concentration of this coating film is approximately 78 atomic %, and the Al concentration is 60 atomic % or more in most parts in the thickness direction, except for the part on the SUS310 substrate side.
[0167] The Ni substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0168] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 50A and 50B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG1 in the photograph shown in Figure 50A), respectively. From Figures 50A and 50B, it can be seen that even after 20 hours of immersion, the maximum Al concentration of the coating film was about 75 atomic %, and the overall Al concentration was 40 atomic % or more. Figures 51A and 51B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure shown in Figure 50A (the portion on the surface side) and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG5 in the photograph shown in Figure 51A), respectively. From Figures 51A and 51B, it can be seen that dense protective Al2O3 is formed in close contact with the surface of the Co(Ni)-Al layer.
[0169] The results of the above immersion tests show that by forming a coating film consisting of a Co, Re, Ni-Al layer and a Co(Ni)-Al layer on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0170] (Example 13) A heat-resistant metal member was produced by Manufacturing Method 1 using a SUS310 substrate.
[0171] First, the surface of the SUS310 substrate was polished to be smooth and degreased, and then a Ni strike film, a Ni film, and a Co film were formed in that order on the surface by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film was plated at a current density of 40 mA / cm 2 The plating was performed for 30 minutes at a current density of 40 mA / cm. The composition of the plating solution was the same as in Example 1. 2 The plating was carried out for 60 minutes using a plating solution having the same composition as in Example 5.
[0172] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment by embedding the SUS310 substrate on which the plating film was formed in a mixture of 7 g of Al powder, 2 g of NH4Cl powder, and 90 g of Al2O3 powder, and heating it at 1000°C for 6 hours in an Ar + 3 vol% H2 atmosphere.
[0173] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 52A and 52B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 52A), respectively. Figures 52A and 52B show that a coating film consisting of Fe, Ni, Co-Al layers, and Co-Al layers was formed on the SUS310 substrate. The maximum Al concentration of this coating film was approximately 64 atomic %.
[0174] The SUS310 substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0175] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 53A and 53B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 53A), respectively. From Figures 53A and 53B, it can be seen that even after 20 hours of immersion, the maximum Al concentration of the coating film was about 60 atomic %, and the overall Al concentration was 40 atomic % or more except for the part on the SUS310 substrate side. Figures 54A and 54B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure shown in Figure 53A (the part on the surface side) and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG5 in the photograph shown in Figure 54A), respectively. From Figures 54A and 54B, it can be seen that dense protective Al2O3 is formed in close contact with the surface of the outermost Co-Al layer.
[0176] The results of the above immersion tests show that by forming a coating film consisting of Fe, Ni, Co-Al and Co-Al layers on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0177] Example 14 A coating film was formed on a SUS310 substrate by manufacturing method 2.
[0178] First, the surface of the SUS310 substrate was polished to be smooth and degreased, and then a Ni strike film, a Ni film, and a Co film were formed on the surface in this order by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film was plated in the same manner as in Example 13. The Co film was plated at a current density of 40 mA / cm 2 The plating was carried out for 60 minutes using a plating solution having the same composition as in Example 5.
[0179] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was performed in the same manner as in Example 12.
[0180] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 55A and 55B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 55A), respectively. Figures 55A and 55B show that a coating film consisting of Ni, Fe, Cr-Al layers, Ni-Al layers, and Co-Al layers has been formed on the SUS310 substrate. The maximum Al concentration of this coating film is approximately 75 atomic %.
[0181] The Ni substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for 20 hours.
[0182] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 56A and 56B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG6 in the photograph shown in Figure 56A), respectively. From Figures 56A and 56B, it can be seen that even after 20 hours of immersion, the Al concentration of the coating film is 40 atomic % or more in most parts except for the part on the SUS310 substrate side. Figures 57A and 57B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure shown in Figure 56A (the part on the surface side) and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG7 in the photograph shown in Figure 57A), respectively. From Figures 57A and 57B, it can be seen that dense protective Al2O3 is formed in close contact with the surface of the Co-Al layer.
[0183] The results of the above immersion tests show that by forming a coating film consisting of Ni, Fe, Cr-Al, Ni-Al and Co-Al layers on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0184] Example 15 A coating film was formed on a SUS310 substrate by Manufacturing Method 1.
[0185] First, the surface of the SUS310 substrate was polished to be smooth and degreased, and then a Ni strike film, a (Co+W) film, and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by plating in that order. The Ni strike film was plated in the same manner as in Example 1. The (Co+W) film was plated at a current density of 40 mA / cm. 2 The plating was performed for 60 minutes at 4000 K, with the composition of the plating solution being 90.3 atomic % Co, 1.7 atomic % Ni, and 7.7 atomic % W. The plating of the Co-containing Re(Ni) film was performed at a current density of 40 mA / cm 2 The plating was performed for 30 minutes using a plating solution having the same composition as in Example 1.
[0186] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment by embedding the SUS310 substrate on which the plating film was formed in a mixture of 7 g of Al powder, 2 g of NH4Cl powder, and 90 g of Al2O3 powder, and heating it at 1000°C for 4 hours in an Ar + 3 vol% H2 atmosphere.
[0187] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 58A and 58B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG of the photograph shown in Figure 58A), respectively. Figures 58A and 58B show that a coating film consisting of a Co, Ni, Fe-Al layer and a Co, Re-Al layer is formed on the SUS310 substrate. The maximum Al concentration of this coating film is approximately 79 atomic %, and the Al concentration is 60 atomic % or more in the majority of the thickness direction.
[0188] The SUS310 substrate after Al diffusion treatment was immersed in molten Li2CO3 at 950℃ in air for two periods of time, 20 hours and 60 hours.
[0189] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut to observe the cross-sectional structure and measure the concentration distribution of each element. Figures 59A and 59B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line of the photograph shown in Figure 59A), respectively. Figures 59A and 59B show that even after 20 hours of immersion, the maximum Al concentration of the coating film was approximately 77 atomic %, and the overall Al concentration was 40 atomic % or more. A protective Al2O3 was formed in close contact with the surface of the outermost Co-Re-Al layer.
[0190] After the 60-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 60A and 60B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 60A), respectively. From Figures 60A and 60B, it can be seen that even after 60 hours of immersion, the maximum Al concentration of the coating film was about 50 atomic %, and the Al concentration was 40 atomic % or more in a considerable part except for the part on the SUS310 substrate side. Figures 61A and 61B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure shown in Figure 60A (the part on the surface side) and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 61A), respectively. From Figures 61A and 61B, it can be seen that dense protective Al2O3 is formed in close contact with the surface of the Co(Ni)-Al layer.
[0191] The results of the above immersion tests show that by forming a coating film consisting of a Co, Ni, Fe-Al layer and a Co, Re-Al layer on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to achieve excellent corrosion resistance against molten Li2CO3.
[0192] Although the embodiment and examples of the present invention have been specifically described above, the present invention is not limited to the above-described embodiment and examples, and various modifications based on the technical concept of the present invention are possible. [Explanation of symbols]
[0193] 10...container, 11...substrate, 12...coating film, 20...powder, 30...tube, 31...substrate, 32...coating film, 40...rod, 41...substrate, 42...coating film
Claims
1. A substrate made of a metal or alloy; a coating film provided on at least a surface of the substrate with which the powder of the raw material of the lithium-containing composite oxide comes into contact, the coating film containing at least aluminum and at least one metal selected from the group consisting of nickel, rhenium, and cobalt, and having a maximum aluminum concentration of 60 atomic % or more and less than 100 atomic %; A member for producing a lithium-containing composite oxide comprising the above-mentioned compound.
2. 2. The member for producing a lithium-containing composite oxide according to claim 1, wherein said coating film further contains at least one metal selected from the group consisting of tungsten, molybdenum and niobium.
3. 2. The member for producing a lithium-containing composite oxide according to claim 1, wherein the maximum value of the aluminum concentration in the coating film is 70 atomic % or more and less than 100 atomic %.
4. 2. The member for producing a lithium-containing composite oxide according to claim 1, wherein the substrate is made of nickel, a nickel-based alloy or an iron-based alloy.
5. 2. The member for producing a lithium-containing composite oxide according to claim 1, wherein the member is a container, and the coating film is provided on the inner surface of the container.
6. 2. The member for producing a lithium-containing composite oxide according to claim 1, wherein the member for producing a lithium-containing composite oxide is a tube, and the coating film is provided on the outer and inner surfaces of the tube.
7. 2. The member for producing a lithium-containing composite oxide according to claim 1, wherein the member for producing a lithium-containing composite oxide is a rod, and the coating film is provided on an outer surface of the rod.
8. forming a raw coating containing at least nickel and at least one metal selected from the group consisting of rhenium and cobalt on a substrate made of a metal or alloy; a step of performing an aluminum diffusion treatment on the base material on which the raw material film has been formed, thereby forming a coating film, which contains at least aluminum and at least one metal selected from nickel, rhenium, and cobalt, and has a maximum aluminum concentration of 60 atomic % or more and less than 100 atomic %, on at least a surface of the base material that is in contact with the powder of the raw material of the lithium-containing composite oxide; The present invention relates to a method for producing a lithium-containing composite oxide.
9. 9. The method for producing a member for producing a lithium-containing composite oxide according to claim 8, wherein the raw material film contains nickel, rhenium and cobalt.
10. 10. The method for producing a member for producing a lithium-containing composite oxide according to claim 8 or 9, wherein the raw material film further contains at least one metal selected from the group consisting of tungsten, molybdenum and niobium.
11. 9. The method for producing a member for producing a lithium-containing composite oxide according to claim 8, wherein the raw material film is formed by a plating method, a thermal spraying method or an electron beam vacuum deposition method.
12. A substrate made of a metal or alloy; a coating film provided on at least a surface of the substrate on the side that comes into contact with a substance generated during firing of the raw material powder of the lithium-containing composite oxide, the coating film containing at least aluminum and at least one metal selected from nickel, rhenium, and cobalt, and having a maximum aluminum concentration of 60 atomic % or more and less than 100 atomic %; A calcination furnace for producing a lithium-containing composite oxide comprising:
Citation Information
Patent Citations
Wet type developing apparatus
JP1980050278A
JP1982028300U
Heat resistant metal member and method of manufacturing the same, and high-temperature device and method of manufacturing the same
JP2022065441A
High-temperature oxidation-resistant Ni alloy heat-resistant material and method for manufacturing the same
JP3916484B2
Nickel-base alloy, heat-resistant and corrosion resistant component, and component for heat-treatment furnace
WO2021132350A1