Layered aluminosilicate, method for producing layered aluminosilicate, method for recovering amphiphilic low molecular compound, device for concentrating amphiphilic low molecular compound, and method for reducing concentration of amphiphilic low molecular compound
A layered aluminosilicate selectively adsorbs and concentrates ethanol from low-concentration solutions, addressing the inefficiencies of existing methods and enabling sustainable bioethanol production by reducing energy and cost.
Patent Information
- Application Number
- JP2023084490
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Current ethanol concentration methods, such as distillation and membrane separation, are energy-intensive and costly, and existing adsorption technologies require high ethanol concentrations or complex equipment, making it difficult to achieve sustainable and regionally distributed bioethanol production.
A layered aluminosilicate is produced using a specific raw material mixture and process, allowing it to selectively adsorb and concentrate ethanol from low-concentration solutions, even as low as 3% by weight, and efficiently desorb it for recovery.
The layered aluminosilicate enables low-cost, efficient concentration of ethanol from low-concentration solutions, reducing energy consumption and equipment complexity, facilitating sustainable and regionally distributed bioethanol production.
Smart Images

Figure 2024168085000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a layered aluminosilicate and a method for producing the layered aluminosilicate. The present invention also relates to a method for concentrating an amphipathic low molecular weight compound, an apparatus for concentrating an amphipathic low molecular weight compound, and a method for reducing the concentration of an amphipathic low molecular weight compound. [Background technology]
[0002] Bioethanol, a type of renewable energy, is a carbon-neutral energy obtained by fermenting the sugars in plant-derived biomass resources. In Southeast Asian countries where biomass resources are easily available, bioethanol production is carried out as a national policy, and it is being produced commercially around the world, and research and development is also being actively conducted to expand the use of non-edible biomass as a raw material.
[0003] In Japan, from the perspective of both creating a recycling-oriented society and revitalizing local areas, demonstration experiments have been conducted on locally distributed ethanol production that utilizes various local biomass resources, such as using sorghum in Shinjo City, Yamagata Prefecture, and food waste in Kitakyushu City, Fukuoka Prefecture, but none of these have led to continuous production (Agency for Natural Resources and Energy, "Present efforts and recent trends regarding the introduction of bioethanol").One of the reasons for this is the high cost of the process of concentrating the fermented alcohol obtained at a low concentration of around 5-10% into high-concentration ethanol of 99.5% or more.
[0004] Currently, ethanol is concentrated by distillation, but 6000 kJ of energy is required to obtain 1 kg of ethanol through distillation, meaning that much of the energy obtained from bioethanol is consumed at the point of production. A concentration method using a separation membrane has also been proposed, but separation using a membrane requires the creation of a pressure difference between the inside and outside of the membrane by pressurizing low-concentration alcohol, which increases the initial installation costs, such as equipment costs, and operating costs.
[0005] Ethanol is typically concentrated by distillation. There are only a limited number of techniques for concentration other than distillation, such as the following: Patent Document 1 discloses a method for producing high-concentration ethanol, characterized in that an ethanol-containing fermentation liquid obtained by ethanol fermentation of a carbohydrate raw material is passed through an activated carbon adsorption treatment step, a pH adjustment step, and then through an ethanol-selective hydrophobic pervaporation membrane separation device having a silylated silicalite membrane to produce high-concentration ethanol.
[0006] As another technique, Patent Document 2 discloses a method for producing bioethanol, which includes a saccharification and fermentation step of fermenting raw pulp in a saccharification and fermentation tank to produce a fermentation liquid containing bioethanol, an enzyme and yeast recovery step of contacting the fermentation liquid obtained in the saccharification and fermentation step with the raw pulp to be used for fermentation to transfer the enzymes and yeast contained in the fermentation liquid from the fermentation liquid to the raw pulp, and a concentration step of supplying the fermentation liquid in which the enzymes and yeast have been reduced in the recovery step to a concentrator and concentrating the bioethanol contained in the fermentation liquid with the concentrator, wherein in the saccharification and fermentation step, the raw pulp to which the enzymes and yeast have been transferred is supplied to the saccharification and fermentation tank and fermented, and in the concentration step, the fermentation liquid in which the enzymes and yeast have been reduced is supplied to the concentrator to concentrate the bioethanol contained in the fermentation liquid.
[0007] Non-Patent Document 1 is a document on a substance that the present inventors have studied. In this document, the present inventors have synthesized a layered silicate substance, KCS-11, which has a unique interlayer adsorption ability, and have found that this substance can selectively adsorb ethanol between its layers from low-concentration ethanol, and that the adsorbed ethanol is easily desorbed in the air. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2007-63259 A [Patent Document 2] JP 2018-64514 A [Non-patent literature]
[0009] [Non-Patent Document 1] Materials Letters 288 (2021) 129332 Summary of the Invention [Problem to be solved by the invention]
[0010] Patent Document 1 deals with a method for producing high-concentration bioethanol using a separation membrane. However, the separation ability is limited. In addition, concentration using a separation membrane inevitably requires high pressure, which increases the equipment and operating costs.
[0011] In Patent Document 2, low-concentration alcohol is concentrated by turning it into mist using ultrasonic vibrations. However, the concentrating device becomes complicated due to the ultrasonic vibrations, and water is also turned into mist at the same time by the ultrasonic vibrations, so it is considered that in principle it is not possible to concentrate it to a high concentration.
[0012] Furthermore, in order for the material in Non-Patent Document 1 to adsorb ethanol between the layers, the ethanol concentration must be 10 wt % or more, and the conditions under which it can be used are limited.
[0013] In the distillation and membrane separation processes, costs can be reduced by achieving economies of scale through large-scale scale expansion. However, this requires the transport and consolidation of widely dispersed biomass resources or low-concentration bioethanol produced in various regions. This creates a dilemma in that the larger the scale, the greater the energy consumption for transportation. In other words, if a low-cost ethanol concentration process that can be operated on a small scale can be developed, bioethanol production can be shifted from a highly intensive model to a locally distributed model, thereby realizing sustainable bioethanol production.
[0014] Under these circumstances, an object of the present invention is to provide a layered aluminosilicate or the like capable of selectively adsorbing an amphiphilic low-molecular-weight compound such as ethanol. [Means for solving the problem]
[0015] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the following invention meets the above object, thereby completing the present invention.
[0016] <1> The present invention relates to a method for producing a layered aluminosilicate, the method comprising: a mixing step of preparing a raw material mixture containing the following raw materials (A) to (D); a hydrolysis step of hydrolyzing the raw material mixture to obtain a hydrolysate; and a hydrothermal synthesis step of heating the hydrolysate to synthesize an aluminosilicate. Raw Material (A) Vinyltrialkoxysilanes and / or Vinyltrichlorosilane Raw material (B) Aluminum compounds Raw Material (C) Alkali Metal Hydroxide and / or Organic Quaternary Ammonium Hydroxide Raw material (D) water <2> In the raw material mixture, a molar ratio of the raw material (A): the aluminum element of the raw material (B): the raw material (C): the raw material (D) is 1:0.2-0.5:0.5-8:2-40. <1> The manufacturing method described in <3> The raw material (A) is vinyltrimethoxysilane, the raw material (B) is alumina and / or aluminum hydroxide, and the raw material (C) is sodium hydroxide. <1> or <2> The manufacturing method described in <4> the hydrolysis step is carried out at 10 to 50° C. for 24 hours or more while stirring, the hydrothermal synthesis step is carried out at 80° C. or higher for 72 hours or more, and the method further comprises a recovery step of filtering and drying the aluminosilicate after the hydrothermal synthesis step, to recover the aluminosilicate. <1> ~ <3> 13. The method for producing a semiconductor device according to any one of the preceding claims. <5> A layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane. <6> A method for concentrating an amphiphilic low molecular weight compound, comprising the steps of contacting a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane with a treatment object containing an amphiphilic low molecular weight compound, and adsorbing the amphiphilic low molecular weight compound contained in the treatment object onto the layered aluminosilicate. <7> The amphiphilic low molecular weight compound is an alcohol and / or a carbonyl compound. <6> The concentration method according to claim 1. <8> The device for concentrating an amphiphilic low molecular weight compound has an adsorption vessel containing a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane. <9> The present invention further includes a tank for accommodating an object to be treated that contains an amphipathic low molecular weight compound, and a first liquid delivery line for delivering the object to be treated from the tank for the object to be treated to the adsorption tank. <8> 2. A device for concentrating an amphiphilic low molecular weight compound according to claim 1. <10> a second liquid sending line for sending the liquid in the treatment tank from the adsorption tank to the tank for the material to be treated, and a concentration line for concentrating the amphiphilic low molecular weight compound adsorbed by the layered aluminosilicate in the adsorption tank from the adsorption tank, the tank for the material to be treated being a fermentation tank for fermenting bioethanol; <9> The concentrating device according to claim 1 . <11> A method for reducing the concentration of an amphipathic low molecular weight compound in a treatment object, comprising the steps of contacting a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane with the treatment object containing an amphipathic low molecular weight compound, and adsorbing the amphipathic low molecular weight compound contained in the treatment object onto the layered aluminosilicate. Effect of the Invention
[0017] The layered aluminosilicate of the present invention is capable of selectively adsorbing amphiphilic low-molecular-weight compounds such as ethanol, and further relates to the concentration of ethanol using such a layered aluminosilicate. [Brief description of the drawings]
[0018] [Figure 1] 1 is an example of a flow of a manufacturing method of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of the reaction in each step of the production method of the present invention. [Diagram 3] FIG. 1 is a schematic diagram of the structure of the layered aluminosilicate of the present invention. [Figure 4] 1 is a powder X-ray diffraction pattern of the layered aluminosilicate of the present invention. [Diagram 5] 1 shows powder X-ray diffraction patterns of the layered aluminosilicate of the present invention in various states. [Figure 6] FIG. 1 is a schematic diagram showing an example of a concentrating device of the present invention. [Figure 7] FIG. 1 shows the results of an ethanol adsorption test in an example. [Figure 8] 1 is an image showing a test of the liquid dispersibility of an example. [Figure 9] FIG. 2 is a diagram showing a desorption test from a layered aluminosilicate after ethanol adsorption in an example. [Figure 10] 1 is an ethanol vapor adsorption isotherm of the layered aluminosilicate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The following is a detailed description of the embodiments of the present invention, but the following description of the constituent elements is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to the following content as long as the gist of the present invention is not changed. Note that in this specification, when the expression "~" is used, it is used as an expression including the numerical values before and after it.
[0020] [Method for producing the layered aluminosilicate of the present invention (the method for producing the layered aluminosilicate of the present invention)] The method for producing a layered aluminosilicate of the present invention includes a mixing step of preparing a raw material mixture containing raw materials (A) to (D), a hydrolysis step of hydrolyzing the raw material mixture to obtain a hydrolysate, and a hydrothermal synthesis step of heating the hydrolysate to synthesize an aluminosilicate. In the present application, the method for producing a layered aluminosilicate of the present invention may be simply referred to as the "production method of the present invention."
[0021] The raw materials (A) to (D) are as follows. Raw material (A): Vinyltrialkoxysilanes and / or vinyltrichlorosilane Raw material (B): Aluminum compound Raw material (C): alkali metal hydroxide and / or organic quaternary ammonium hydroxide Ingredients (D): Water
[0022] [Layered aluminosilicate of the present invention] The layered aluminosilicate of the present invention is a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane.
[0023] [Method for concentrating amphiphilic low-molecular-weight compounds of the present invention] The method for concentrating an amphiphilic low molecular weight compound of the present invention comprises a step of contacting a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane with a treatment object containing an amphiphilic low molecular weight compound, and adsorbing the amphiphilic low molecular weight compound contained in the treatment object to the layered aluminosilicate. Note that in the present application, the method for concentrating an amphiphilic low molecular weight compound of the present invention may be simply referred to as the "concentration method of the present invention."
[0024] [Concentration device for amphiphilic low molecular weight compounds of the present invention] The device for concentrating an amphiphilic low molecular weight compound of the present invention has an adsorption tank containing a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane. Note that in the present application, the device for concentrating an amphiphilic low molecular weight compound of the present invention may be simply referred to as the "concentration device of the present invention."
[0025] [Method of reducing amphiphilic low molecular weight compounds of the present invention] The method for reducing amphipathic low molecular weight compounds of the present invention is a method for reducing the concentration of amphipathic low molecular weight compounds in a treatment target, comprising the steps of contacting a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane with a treatment target containing an amphipathic low molecular weight compound, and adsorbing the amphipathic low molecular weight compounds contained in the treatment target to the layered aluminosilicate. Note that in the present application, the method for reducing amphipathic low molecular weight compounds of the present invention may be simply referred to as the "reduction method of the present invention".
[0026] In the present application, the layered aluminosilicate of the present invention can be produced by the production method of the present invention. Furthermore, the layered aluminosilicate of the present invention and the layered aluminosilicate produced by the production method of the present invention can be used in the concentrating device of the present invention, the concentrating method of the present invention, and the reduction method of the present invention. Furthermore, the concentrating device of the present invention can be used to carry out the concentrating method of the present invention and the reduction method of the present invention. In the present application, configurations corresponding to each of these can be used mutually.
[0027] The present inventors have found that a layered aluminosilicate produced using a specific raw material can selectively adsorb amphiphilic low molecular weight compounds such as ethanol. This is a characteristic that allows selective separation of only ethanol having amphiphilic properties from a mixture of water and ethanol. For example, it has been found that ethanol can be efficiently adsorbed between layers from a low concentration ethanol aqueous solution of 5% by weight or less, and more surprisingly, it has been found that ethanol can be adsorbed between layers even from an extremely low concentration ethanol aqueous solution of about 3% by weight. In addition, after adsorption of ethanol, the adsorbed ethanol can be desorbed and recovered from the layered aluminosilicate. The present invention relates to a layered aluminosilicate having such extremely special physical properties, a method for producing the same, and a method for using the same.
[0028] [Production of layered aluminosilicate] FIG. 1 is an example of a flow chart of the production method of the present invention. The layered aluminosilicate of the present invention can be produced, for example, by the following steps. Step S11 is a step of mixing the raw materials. Step S21 is a step of hydrolyzing a part of the raw materials. Step S31 is a step of hydrothermally synthesizing an aluminosilicate from the hydrolyzed material. Step S41 is a step of appropriately recovering the aluminosilicate. FIG. 2 is a schematic diagram of the reaction in each step of the production method of the present invention. Each step will be described in more detail below.
[0029] [Mixing process] The mixing step is a step of preparing a raw material mixture containing the raw materials (A) to (D). The raw material mixture is used to produce a layered aluminosilicate.
[0030] [Raw material (A)] The raw material (A) is vinyltrialkoxysilanes and / or vinyltrichlorosilane. The raw material (A) is a material that forms a structure that becomes the skeleton of the layered aluminosilicate by hydrolysis. Examples of the vinyltrialkoxysilanes include vinyltrimethoxysilane (hereinafter sometimes abbreviated as "VTMS"), vinyltriethoxysilane, and vinyltriisopropoxysilane. Vinyltrichlorosilane can also be used in the same way. Among these, VTMS, which has an appropriate hydrolysis rate, is the most suitable.
[0031] [Raw material (B)] The raw material (B) is an aluminum compound. The aluminum compound may be alumina, aluminum hydroxide, sodium aluminate, aluminum nitrate, or the like. The aluminum derived from the aluminum compound becomes aluminate ions in the alkaline water of the raw material mixture because water derived from the raw material (D) is used. These aluminate ions form layered aluminosilicate. In particular, it is preferable to use alumina as the aluminum compound from the viewpoint of pH setting for hydrolysis, and it is particularly preferable to use fumed alumina, which has a large surface area and excellent reactivity.
[0032] [Raw materials (C)] The raw material (C) is an alkali metal hydroxide and / or an organic quaternary ammonium hydroxide. The raw material (C) is used to adjust the raw material mixture to a pH suitable for hydrolysis. The alkali metal hydroxide may be sodium hydroxide, lithium hydroxide, potassium hydroxide, or the like. The organic quaternary ammonium hydroxide may be tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, or the like. The alkali metal ions and organic quaternary ammonium ions of the raw material (C) are expected to become cations and function as counter ions of the layered aluminosilicate. The raw material (C) is preferably sodium hydroxide, which provides the most crystalline material when made into a layered aluminosilicate.
[0033] [Raw materials (D)] The raw material (D) is water. Water functions as a dispersion medium suitable for providing a place for mixing, dispersing, arranging, synthesizing, etc., of the raw materials (A) to (C) for hydrolysis and hydrothermal synthesis. The water may be ordinary water with few impurities, but it is preferable to use ultrapure water or distilled water with fewer ions in the water so that design based on the components derived from the raw materials (A) to (C) can be more easily performed.
[0034] [Raw material mixture] The raw material mixture is a mixture of these raw materials (A) to (D). There are no particular limitations on the mixing method used to obtain the raw material mixture, but it may be simply mixed by stirring at room temperature and normal pressure. Since water or the like is used as a raw material, the raw material mixture is in the form of a suspension in which the raw materials (A) to (C) are dissolved and dispersed in water.
[0035] [Mixing ratio] The mixing ratio of the raw materials (A) to (D) in the raw material mixture can be appropriately set in consideration of the type of each component, the conditions of downstream processes such as the hydrolysis process and the hydrothermal synthesis process, the quality of the layered aluminosilicate to be produced, etc. In addition, since the layered aluminosilicate corresponding to the mixing ratio in the raw material mixture, that is, the feeding conditions, is produced, the mixing ratio may be set according to the allowable state of the layered aluminosilicate.
[0036] The molar ratio of raw material (A): aluminum element of raw material (B): raw material (C): raw material (D) can be about 1:0.2-0.5:0.5-8:2-40. That is, the molar ratio of each raw material can be set as follows, with 1 mole of the main raw material (A) that forms the layered aluminosilicate structure as the standard. Raw material (A): 1 mole Aluminum element in raw material (B): 0.2 to 0.5 mol Raw material (C): 0.5 to 8 moles Raw materials (D): 2~40
[0037] The raw material (B) is an aluminum compound. The aluminum compound is used based on the number of moles of aluminum element per mole of the raw material depending on the type of aluminum compound. For example, in the case of alumina, Al 2 O 3 Therefore, 2 moles of aluminum element are contained per mole of alumina. Therefore, the amount of raw material (B) is controlled by the molar amount of aluminum element relative to the molar amount of raw material (A). From the structure of layered aluminosilicate, it is considered that layered aluminosilicate requires 0.5 moles of aluminum element per mole of raw material (A). Therefore, if the aluminum element of raw material (B) is small, raw material (A) may not be fully used up, but if it is 0.2 moles or more, stable formation of layered aluminosilicate can be expected. Also, if the aluminum element of raw material (B) is too large, the yield is considered to be rate-limiting due to a shortage of raw material (A). From the viewpoint of more reliably using up raw material (A), the upper limit of the aluminum element of raw material (B) can be about 0.5 moles.
[0038] The raw material (C) is important in the raw material mixture, particularly for maintaining the alkalinity required for hydrolysis of the raw material (A). In addition, in the layered aluminosilicate, the alkali metal and ammonium ions of the raw material (C) are considered to be used as counter ions. From this viewpoint, it is preferable to set the pH to be sufficiently alkaline and to supply counter ions of the layered aluminosilicate at 0.5 moles or more. If it is below this lower limit, hydrolysis may be difficult or the counter ions may be insufficient. On the other hand, when the amount of the raw material (D) described later is large, it is more preferable to use up to 8 moles in order to maintain the alkalinity or to maintain the molar ratio of raw material (C) / raw material (D). There is no need to exceed this upper limit, and there is a possibility that excessive raw materials will be used.
[0039] The raw material (D) is water, and also adjusts the concentration of other raw materials in the mixed composition. If the raw material (D) is excessive, the concentration of the other raw materials will be low and dilute. In such a state, it is difficult to arrange the raw materials to form a layered aluminosilicate, and excessive reaction time may be required. On the other hand, if the raw material (D) is too little, the concentration of the other raw materials will be high and concentrated. In such a state, the movement of each component to form a layered aluminosilicate may not be sufficient. From experimental findings, it is possible to efficiently produce a layered aluminosilicate with excellent crystallinity by setting the raw material (D) within the above-mentioned range.
[0040] A typical example of mixing is, for example, 1 mole of VTMS as raw material (A), 0.2 moles of alumina as raw material (B), 1 mole of NaOH as raw material (C), and 5 moles of water as raw material (D). The order of mixing these is not particularly limited, and since the reactivity in a short time is limited and mixing is performed while stirring sufficiently in the subsequent hydrolysis step, etc., mixing may be performed in an order that is easy to handle depending on the raw materials to be adopted and the mixing vessel, etc.
[0041] [Hydrolysis process] The hydrolysis process is a process in which the raw material mixture is hydrolyzed to produce a hydrolysate. This hydrolysis refers to hydrolysis of a portion of the raw materials to be hydrolyzed in the raw material mixture. Since at least a portion of the raw material mixture is hydrolyzed, it is called a hydrolysate. In particular, the hydrolysis process is carried out in order to separate the alkyl group of the alkoxy group of raw material (A) and the chloro group into water. In addition, in the hydrolysis process, it is considered that the raw materials (A), (B), etc., for forming the layered aluminosilicate are arranged in water as a result of the hydrolysis.
[0042] The hydrolysis step is preferably carried out at 10 to 50°C for 24 hours or more while stirring. The hydrolysis step involves hydrolysis of the raw material (A) and arrangement for forming a layered aluminosilicate, which is considered to occur relatively slowly. For this reason, from the viewpoint of using the raw material (D), the hydrolysis step may be carried out without excessive cooling or heating. In the hydrolysis step, there is no reason to cool or heat, and from the viewpoint of reducing energy consumption associated with production, the temperature of the hydrolysis step can be about room temperature. If the hydrolysis step is excessively heated, hydrothermal synthesis may occur with insufficient arrangement for forming a layered aluminosilicate, so it is preferable not to heat the hydrolysis step. This temperature is more preferably about 20 to 40°C.
[0043] The time for the hydrolysis step is preferably 24 hours or more. As mentioned above, it is considered preferable to carry out the hydrolysis step relatively slowly. If the time is shorter than this, the crystallinity of the layered aluminosilicate may decrease. The hydrolysis step is most preferably carried out for about 4 days (96 hours). Even if the hydrolysis step is carried out for an excessively long period of time, it is considered that the crystallinity and the like will not be improved any more, so the hydrolysis step may be carried out with an upper limit of 200 hours or less, 150 hours or less, 120 hours or less, or the like.
[0044] The hydrolysis step is preferably carried out with stirring from the viewpoints of dispersing the raw materials, hydrolysis, and ensuring an opportunity for arrangement for forming the layered aluminosilicate, etc. By carrying out the hydrolysis step with stirring, the crystallinity of the produced layered aluminosilicate is improved.
[0045] [Hydrothermal synthesis process] The hydrothermal synthesis process is a process in which the hydrolysate is heated to synthesize an aluminosilicate. By carrying out the hydrothermal synthesis process, the raw material of the hydrolysate is synthesized to become an aluminosilicate. This aluminosilicate is considered to be layered, and is therefore called a layered aluminosilicate.
[0046] The hydrothermal synthesis step is preferably carried out at 80° C. or higher for 72 hours or longer. At this time, stirring may be performed or not.
[0047] The hydrothermal synthesis step is carried out in the presence of water, which originates from the raw material mixture and is also contained in the hydrolyzate. The step is also carried out by heating to near the boiling point of water. This allows the synthesis of a layered aluminosilicate that will crystallize from the state in which the arrangement for forming the layered aluminosilicate is being carried out in the hydrolysis step.
[0048] The temperature of the hydrothermal synthesis step is preferably 80°C or higher. If the temperature is too low, the rate at which the layered aluminosilicate is synthesized by hydrothermal synthesis may decrease, or the layered aluminosilicate may not be synthesized at all. The temperature may be 90°C or higher, or 95°C or higher. In addition, the temperature may be higher than 100°C, for example, about 120°C or 150°C, by appropriately carrying out the process under pressure. If the process is heated excessively, other reactions may occur, so the process is preferably carried out at 180°C or lower, or 150°C or lower. In particular, the process may be carried out at about 100°C, which can be achieved by heating at normal pressure.
[0049] The hydrothermal synthesis step is preferably performed for 72 hours or more. If this time is shorter, the synthesis of the layered aluminosilicate may not be sufficient, resulting in a decrease in yield. This time may be 120 hours or more, or 144 hours or more. In particular, it is preferable to perform the hydrothermal synthesis step at 100°C for about 168 hours (7 days). Since it is considered that the yield will not improve even if the hydrothermal synthesis step is performed excessively, the time may be set to an upper limit of 250 hours or less, or 200 hours or less. Note that the hydrolysis step and hydrothermal synthesis step can be performed in a container with a high level of airtightness, such as by being appropriately covered, so that the concentration does not change significantly due to evaporation of water.
[0050] [Recovery process] The recovery step is a step of filtering and drying the aluminosilicate after the hydrothermal synthesis step, and recovering the aluminosilicate. This aluminosilicate is considered to be layered, and is therefore called layered aluminosilicate. This allows the production of layered aluminosilicate.
[0051] The aluminosilicate synthesized in the hydrothermal synthesis step is crystalline and becomes a powdery solid in water, etc. By filtering this solid from liquids such as water that are unreacted substances derived from the raw material mixture after the hydrothermal synthesis, layered aluminosilicate can be selectively obtained.
[0052] [Layered aluminosilicate] The layered aluminosilicate of the present invention has a structure derived from vinyltrialkoxysilanes or vinyltrichlorosilane. Since the structures derived from vinyltrialkoxysilanes and vinyltrichlorosilane are considered to be similar, they may be simply described as "structures derived from vinyltrialkoxysilanes, etc." Figure 3 is a schematic diagram of the structure of the layered aluminosilicate of the present invention. As shown in Figure 3, the layered aluminosilicate is an aluminosilicate having a structure derived from vinyltrialkoxysilanes, etc. The layered aluminosilicate has a structure similar to that of RUB-15 (U. Oberhagemann et al., Angew. Chem. Int. Ed. 35, 2869 (1997) and HUS-1 (T. Ikeda et al., Inorg. Chem. 50, 2294 (2011)). It also has a layered structure. It is believed that vinyl groups are arranged between the layers, and that this molecular structure allows amphiphilic low molecular weight compounds such as ethanol to selectively enter between the layers.
[0053] 4 is a powder X-ray diffraction pattern by a reflection method using Cu Kα radiation according to a manufacturing example of the layered aluminosilicate of the present invention. The layered aluminosilicate of this manufacturing example shows such a crystalline powder X-ray diffraction pattern in a dry state. The details of this manufacturing example will be described in the examples below.
[0054] This layered aluminosilicate has X-ray diffraction peaks and the like as shown in Table 1. Table 1 shows the positions (2θ) and peak intensities of the main peaks, and the indices (hkl) of each peak. The layered aluminosilicate of the present invention can also be identified by performing such matching of powder X-ray diffraction patterns. Note that the peak positions and simulation intensities in Table 1 are ideal positions and intensities simulated from the crystal structure.
[0055] [Table 1]
[0056] FIG. 5 shows X-ray diffraction patterns of the layered aluminosilicate of the present invention in a number of states. In data obtained by actually measuring the layered aluminosilicate, the intensity ratio may differ from that of the simulation due to reasons such as crystal orientation. In addition, the interlayer distance may change depending on the manufacturing conditions and storage conditions, and the peak position may also change partially. In addition, the actual sample may contain impurities. FIG. 5 shows a number of measurement examples as reference information.
[0057] It is considered that the layered aluminosilicate may show a partially different X-ray diffraction pattern depending on the raw materials and production conditions. In addition, due to the complex structure, it may be impossible or impractical to directly identify the substance by its structure or characteristics, and it may be necessary to identify the layered aluminosilicate of the present invention by its production method in some cases.
[0058] [Form / physical properties] Layered aluminosilicates have an ideal molar composition of (CH 2 CH-Si) 2 NaAlO 5 When structural defects exist, the abundance of each element may be as low as 1 mol %.
[0059] [Form / physical properties] The layered aluminosilicate is a powdery solid, etc. Also, the layered aluminosilicate is a crystalline substance in which the crystallites have a tabular shape.
[0060] [Optional ingredients] The layered aluminosilicate can be used as it is as an adsorbent for amphiphilic low molecular weight compounds. It may also be used as a molded product of any shape, such as a plate or block, by using a binder or the like. It can also be attached to various molded products, or can be housed in a package using a filter having air and liquid permeability.
[0061] [Concentrator] Fig. 6 is a schematic diagram showing an example of the concentrating apparatus of the present invention. The concentrating apparatus has a fermentation tank, which is an example of a tank for a material to be treated, a plurality of adsorption tanks, and a concentrating tank. These tanks are connected by a liquid transfer line for transporting liquids, etc. By using the concentrating apparatus, it is possible to selectively concentrate an amphipathic low molecular weight compound.
[0062] [Adsorption tank] The adsorption tank is a tank containing a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane. That is, the adsorption tank is a tank containing the layered aluminosilicate of the present invention. This layered aluminosilicate adsorbs the amphiphilic low molecular weight compound contained in the object to be treated. The concentrating device of the present invention has at least this adsorption tank. The object to be treated is placed in the adsorption tank, and the object to be treated after adsorption and the layered aluminosilicate are separated by filtration or the like, and the amphiphilic low molecular weight compound contained in the object to be treated is desorbed from the layered aluminosilicate, thereby concentrating the amphiphilic low molecular weight compound. In addition, the other object to be treated after adsorption that has been separated by filtration has a reduced concentration of the amphiphilic low molecular weight compound. Therefore, it can also be used as a device for reducing the concentration of the amphiphilic low molecular weight compound.
[0063] [Treated material tank] The tank for the object to be treated is a tank that contains the object to be treated, which contains an amphipathic low molecular weight compound. The tank for the object to be treated is a tank that is selected according to the object to be treated. The object to be treated may be any object that contains an amphipathic low molecular weight compound. The tank for the object to be treated may be a tank that stores a mixture containing the object to be treated, or may be a reaction tank in which an amphipathic low molecular weight compound is produced while reacting in the tank. For example, a fermentation tank can be used as shown in FIG. 6, and this fermentation tank can be a tank in the middle of a reaction in which alcohol fermentation is performed using alcohol fermentation bacteria or the like with sugars or the like as a raw material. Typically, the tank for the object to be treated can be a fermentation tank that ferments bioethanol.
[0064] [Liquid delivery] The concentrating device may have a first liquid transfer line for transferring the material to be treated from a tank for the material to be treated to the adsorption tank. By transferring the liquid in this manner, the liquid is transferred in accordance with the state of the tank for the material to be treated, such as a fermenter, and the adsorption tank. For example, after the liquid in the fermenter has reached a state in which it contains a certain amount of alcoholic fermentation, the liquid in the fermenter is transferred to the adsorption tank.
[0065] [Return] The concentrating apparatus may further include a second liquid transfer line for transferring the liquid in the adsorption tank from the adsorption tank to the tank for the material to be treated. The liquid obtained after the amphiphilic low molecular weight compound is adsorbed from the material to be treated onto the layered aluminosilicate in the adsorption tank may be returned to the tank for the material to be treated, such as a fermentation tank, and may be used again for fermentation or for mixing with the residual liquid.
[0066] [Concentration line] The concentrating device may also have a concentration line for concentrating the amphipathic low molecular weight compound adsorbed by the layered aluminosilicate in the adsorption tank from the adsorption tank. This concentration line is a pipe or the like for selectively transferring and concentrating the amphipathic low molecular weight compound in a high concentration state that has been desorbed from the layered aluminosilicate. Since the desorbed amphipathic low molecular weight compound may be desorbed as a gas, a gas or liquid may be transferred according to the state. The high concentration of the amphipathic low molecular weight compound can be recovered by transferring it to the concentration tank via the concentration line.
[0067] [Amphiphilic low molecular weight compounds] The amphiphilic low molecular weight compounds to be concentrated using the layered aluminosilicate of the present invention are low molecular weight compounds having amphiphilicity. These compounds are selectively adsorbed between the layers of the layered aluminosilicate. The amphiphilic low molecular weight compounds can be, for example, alcohols and / or carbonyl compounds. Examples of alcohols include benzyl alcohol (molar mass 108.1), butanol (molar mass 74.1), and ethanol (molar mass 46.1). Examples of carbonyl compounds include acetone (molar mass 58.1) and methyl ethyl ketone (molar mass 72.1). The molecular weight can be about 150 or less, or about 120 or less.
[0068] Layered aluminosilicates do not adsorb hydrophobic compounds such as toluene, or extremely polar compounds such as water. The fact that layered aluminosilicates have adsorbed a compound can be confirmed by the fact that the largest peak in the 2θ of the dry layered aluminosilicate, which is around 10°, shifts after coming into contact with the target compound, thereby changing the crystal structure.
[0069] [Adsorption process] The concentration method of the present invention can be carried out using the concentration apparatus of the present invention having an adsorption tank. This concentration method includes a step of contacting a layered aluminosilicate with a treatment object containing an amphiphilic low molecular weight compound, and adsorbing the amphiphilic low molecular weight compound contained in the treatment object onto the layered aluminosilicate.
[0070] [Mixing ratio] The amount of amphipathic low molecular weight compound adsorbed relative to the mass of layered aluminosilicate (adsorbed amount of amphipathic low molecular weight compound (g) / mass of layered aluminosilicate (g)) can be approximately 0.1 g / g. Based on this guideline, the mixing ratio of layered aluminosilicate to the object to be treated and the contact time are set, taking into consideration the concentration of the amphipathic low molecular weight compound contained in the object to be treated. The desorption rate and filtration frequency can also be set as appropriate.
[0071] The contact time between the layered aluminosilicate and the object to be treated can be approximately several hours. For example, it can be 30 minutes or more, 1 hour or more, or 2 hours or more. The content of the amphiphilic low molecular weight compound in the object to be treated, the amount of the layered aluminosilicate that can be adsorbed, the production speed, transfer speed, concentration speed, and the like can be designed. Since the object may be stored in an adsorbed state, there is no need to set an upper limit on the contact time. When performing continuous operation, the upper limit may be set to 24 hours or less, 12 hours or less, 8 hours or less, or the like.
[0072] [Reduction] The present invention can also be provided as a method for reducing the concentration of an amphiphilic low molecular weight compound in a treatment object, comprising a step of contacting the layered aluminosilicate of the present invention with the treatment object containing an amphiphilic low molecular weight compound and adsorbing the amphiphilic low molecular weight compound contained in the treatment object onto the layered aluminosilicate.
[0073] The concentration method of the present invention can be used, for example, to concentrate bioethanol. Conventionally, in order to increase the concentration of bioethanol, the processes of distillation and membrane separation themselves require a large amount of energy and cost. In addition, in order to scale up the concentration to reduce costs, it is necessary to transport and collect the raw biomass and low-concentration fermented alcohol, which requires additional energy and cost. For these reasons, there is a demand for the development of a process that can concentrate low-concentration fermented alcohol of about 5 to 10% at low cost.
[0074] Separation and concentration by adsorption is a low-cost process that can be performed using simple equipment. However, because ethanol has a very high affinity for water, no adsorbent has been developed to selectively adsorb only ethanol from a low-concentration aqueous ethanol solution.
[0075] KCS-11, which was developed by the present inventors and described in Non-Patent Document 1, was able to interlayer adsorb only ethanol from an ethanol aqueous solution with a low concentration of 10% by weight, but bioethanol is often obtained at a lower concentration, and there are cases in which KCS-11 cannot be used.
[0076] The layered aluminosilicate of the present invention can adsorb ethanol between its layers even from an aqueous solution of ethanol with a very low concentration of about 3% by weight, and is therefore considered to be applicable to the low-cost concentration of bioethanol.
[0077] In addition, by utilizing this adsorption ability, it is possible to remove ethanol from relatively low-concentration alcoholic beverages such as wine and sake. Because it selectively adsorbs ethanol, it is possible to produce beverages that meet the recent trend for low-alcohol beverages without compromising the flavor of the alcoholic beverage. EXAMPLES
[0078] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples unless the gist of the present invention is changed.
[0079] [Raw materials] ·VTMS: Vinyltrimethoxysilane (Tokyo Chemical Industry Co., Ltd. >98%) Alumina: Fumed alumina (AEROXIDE Alu C manufactured by Evonik) NaOH: Sodium hydroxide (Fujifilm Wako Pure Chemical Industries, Ltd., special grade) Water: Distilled and ion-exchanged water ·MTMS: Methyltrimethoxysilane (Tokyo Chemical Industry Co., Ltd. >98%) Ethanol: Ethanol (Fujifilm Wako Pure Chemical Industries, Ltd., special grade)
[0080] [Measurement method] ·XRD (Reflection X-ray Powder Diffraction Pattern) Malvern Panalytical X´Pert PRO Bragg-Brentano method (concentrated reflection method) Light source: Cu Kα line
[0081] Ethanol vapor adsorption isotherm Microtrack-Bell Belsorp Max Pretreatment conditions: 150℃, 4 hours Adsorption temperature: 25°C (ethanol saturated vapor pressure 7.958 kPa) Adsorption equilibrium judgment time: 1200 seconds
[0082] [Example 1] Preparation of layered aluminosilicate (1) 1)Mixture A raw material mixture was prepared by mixing 1 mole of VTMS, 0.2 moles of alumina, 1 mole of NaOH, and 5 moles of water at room temperature. 2) Hydrolysis The raw material mixture was stirred at room temperature for 4 days to hydrolyze VTMS and the like. 3) Hydrothermal synthesis After the hydrolysis, the mixture was sealed and left to stand for 7 days at 100°C for hydrothermal synthesis to synthesize layered aluminosilicate in water. 4) Solid-liquid separation After the hydrothermal synthesis, solid-liquid separation was performed by filtration to obtain layered aluminosilicate (1).
[0083] [Reference Example 1] Production of layered aluminosilicate (a) Layered aluminosilicate (a) was produced in the same manner as in Example 1, except that MTMS was used in place of VTMS.
[0084] [Example 2] Evaluation of layered aluminosilicate (XRD) The X-ray diffraction pattern of the layered aluminosilicate (1) was evaluated by XRD. The evaluation results are shown in FIG.
[0085] [Example 3] Evaluation of layered aluminosilicate (adsorption of ethanol) Ethanol was mixed with water to prepare ethanol mixtures of various concentrations. The ethanol mixtures were brought into contact with the layered aluminosilicates of Example 1 and Reference Example 1 to evaluate the adsorption of ethanol between the layers. FIG. 7 shows the results of the ethanol adsorption test in the examples. FIG. 7 shows the evaluation conditions and evaluation results of ethanol adsorption. FIG. 7 shows the evaluation by XRD, and when adsorption occurs, the XRD peak before treatment shifts to the left.
[0086] 7, the notation "〇% EtOH" indicates that an aqueous ethanol solution with a concentration of % by weight indicated by the value in the circle was used. Also, the notation "〇h" indicates that the contact was performed for the time indicated by the value in the circle.
[0087] Fig. 8 is an image of the liquid dispersibility test of Example 1 and Reference Example 1. The layered aluminosilicate (a) of Reference Example 1 is not sufficiently dispersed even when mixed with an ethanol aqueous solution, and is separated into an upper layer of layered aluminosilicate and a lower layer of ethanol aqueous solution. On the other hand, it was confirmed that the layered aluminosilicate (1) of Example 1 becomes a sufficiently uniform dispersion when mixed with an ethanol aqueous solution.
[0088] [Example 4] Evaluation of layered aluminosilicate (elimination of ethanol) An ethanol desorption test was carried out using the sample after adsorption of 10 wt % ethanol in Example 3. Fig. 9 is a diagram showing the desorption test from the layered aluminosilicate after ethanol adsorption in the example.
[0089] When the layered aluminosilicate (a) of the reference example was used, it was confirmed that from about 3 hours, a peak corresponding to the layered aluminosilicate in a dry state due to desorption of ethanol coexisted with a peak in the state in which ethanol was adsorbed. As time passed, the peak in the state in which ethanol was adsorbed decreased, but even after 45 hours, the peak in the state in which ethanol was adsorbed remained, and it was confirmed that ethanol had not been completely desorbed.
[0090] When the layered aluminosilicate (1) of the embodiment was used, after about 2 hours, only a peak corresponding to the layered aluminosilicate in a nearly dry state was observed, and after about 4 hours, the peak in the state where ethanol was adsorbed became difficult to identify.
[0091] This confirms that the layered aluminosilicate (1) can easily desorb the adsorbed ethanol. The desorbed ethanol is considered to be vaporized. Therefore, the gas phase is collected when the ethanol is desorbed, and then cooled and pressure adjusted to condense it, allowing the ethanol to be selectively collected.
[0092] [Example 5] Evaluation of layered aluminosilicate (vapor adsorption isotherm) Figure 10 shows the ethanol vapor adsorption isotherm of the layered aluminosilicate (1). From the condition of low relative pressure, it was confirmed that the layered aluminosilicate (1) adsorbs ethanol. [Industrial Applicability]
[0093] INDUSTRIAL APPLICABILITY The present invention can be utilized for selective adsorption and recovery of ethanol, etc., and is therefore industrially useful.
Claims
1. A mixing step of preparing a raw material mixture containing the following raw materials (A) to (D); a hydrolysis step of hydrolyzing the raw material mixture to obtain a hydrolysate; a hydrothermal synthesis step of heating the hydrolyzate to synthesize an aluminosilicate; A method for producing a layered aluminosilicate having the above structure. Raw Material (A) Vinyltrialkoxysilanes and / or Vinyltrichlorosilane Raw material (B) Aluminum compound Raw Material (C) Alkali Metal Hydroxide and / or Organic Quaternary Ammonium Hydroxide Raw material (D) water
2. In the raw material mixture, the molar ratio of the raw material (A): the aluminum element of the raw material (B): the raw material (C): the raw material (D) is The method according to claim 1, wherein the ratio is 1:0.2-0.5:0.5-8:2-40.
3. The raw material (A) is vinyltrimethoxysilane, the raw material (B) is alumina and / or aluminum hydroxide, The method according to claim 2, wherein the raw material (C) is sodium hydroxide.
4. The hydrolysis step is carried out at 10 to 50° C. for 24 hours or more with stirring, The hydrothermal synthesis step is carried out at 80° C. or higher for 72 hours or longer; The method according to any one of claims 1 to 3, further comprising, after the hydrothermal synthesis step, a recovery step of filtering and drying the aluminosilicate to recover the aluminosilicate.
5. A layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane.
6. A method for concentrating an amphiphilic low molecular weight compound, comprising the steps of contacting a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane with a treatment object containing an amphiphilic low molecular weight compound, and adsorbing the amphiphilic low molecular weight compound contained in the treatment object onto the layered aluminosilicate.
7. The method according to claim 6 , wherein the amphiphilic low molecular weight compound is an alcohol and / or a carbonyl compound.
8. An apparatus for concentrating an amphiphilic low molecular weight compound, comprising an adsorption vessel containing a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane.
9. Further, a tank for a treatment object containing an amphipathic low molecular weight compound; 9. The apparatus for concentrating an amphipathic low-molecular-weight compound according to claim 8, further comprising: a first liquid transfer line for transferring the material to be treated from the material to be treated tank to the adsorption tank.
10. a second liquid transfer line for transferring the liquid in the treatment tank from the adsorption tank to the tank for the material to be treated; a concentration line extending from the adsorption tank to concentrate the amphiphilic low molecular weight compound adsorbed by the layered aluminosilicate in the adsorption tank, The concentrating apparatus according to claim 9 , wherein the tank for the material to be treated is a fermentation tank for fermenting bioethanol.
11. A method for reducing the concentration of an amphipathic low molecular weight compound in a treatment object, comprising the steps of contacting a layered aluminosilicate having a siloxane skeleton derived from vinyltrialkoxysilanes and / or vinyltrichlorosilane with the treatment object containing an amphipathic low molecular weight compound, and adsorbing the amphipathic low molecular weight compound contained in the treatment object onto the layered aluminosilicate.
Citation Information
Patent Citations
Method of producing high-concentration bioethanol by pervaporation separation process using silylated silicalite membrane
JP2007063259A
Production method and production equipment for bioethanol
JP2018064514A