Method for producing oxygen reduction catalyst

By heating Fe-N-C compounds to 700 to 1200°C using microwave or induction heating, the method suppresses hydrogen peroxide production, enhancing catalyst stability and performance in oxygen reduction reactions.

JP2024168122AInactive Publication Date: 2024-12-05HOKKAIDO UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023084553
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Nitrogen-containing carbon materials with Fe, Co, or Mn as transition metals exhibit high oxygen reduction activity but produce large amounts of hydroxyl radicals during oxygen reduction, leading to catalyst deactivation.

Method used

Heating Fe-N-C compounds to a temperature range of 700 to 1200°C using microwave or induction heating to suppress hydrogen peroxide production, which involves rapid temperature increase and short heating times to minimize catalyst deactivation.

Benefits of technology

The method effectively reduces hydrogen peroxide generation during oxygen reduction, maintaining catalyst performance by heating the Fe site and its surroundings to higher temperatures than the average compound temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168122000001_ABST
    Figure 2024168122000001_ABST
Patent Text Reader

Abstract

To provide a method for producing an oxygen reduction catalyst that suppresses generation of H2O2 during oxygen reduction.SOLUTION: A method for producing an oxygen reduction catalyst involves heating an Fe-N-C compound having one or more peaks with peak tops in the 1550-1620 cm-1 range in the Raman spectrum to 700-1200°C through microwave or induction heating.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing an oxygen reduction catalyst. [Background technology]

[0002] Currently, expensive and rare platinum is used as an oxygen reduction catalyst in solid polymer fuel cells, etc. Meanwhile, in order to reduce costs, active research is being conducted on oxygen reduction catalysts that can replace platinum.

[0003] Patent Document 1 discloses a method for producing a specific nitrogen-containing carbon material. According to Patent Document 1, the nitrogen-containing carbon material contains a transition metal and has high oxygen reduction activity. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-256093 A Summary of the Invention [Problem to be solved by the invention]

[0005] Among the nitrogen-containing carbon materials disclosed in Patent Document 1, those containing Fe, Co, or Mn as a transition metal exhibit high oxygen reduction activity, and among these, Fe materials (hereinafter also referred to as "Fe-NC compounds") can exhibit particularly high oxygen reduction activity. However, oxygen reduction catalysts consisting of Fe-NC compounds have the problem that they generate a large amount of H2O2 during oxygen reduction, and the decomposition products (hydroxyl radicals) deactivate the catalyst.

[0006] The present disclosure has been made in light of these circumstances, and one of its objectives is to provide a method for producing an oxygen reduction catalyst that can suppress the generation of H2O2 during oxygen reduction more than conventional methods. [Means for solving the problem]

[0007] Aspect 1 of the present invention is In the Raman spectrum, 1550-1620 cm -1 and heating an Fe-NC compound having one or more peaks with a peak apex in the range of 700 to 1200°C by microwave heating or induction heating.

[0008] Aspect 2 of the present invention is 2. The method of claim 1, comprising heating the Fe-NC compound to the temperature by microwave heating.

[0009] Aspect 3 of the present invention is 3. The method according to claim 1 or 2, wherein the average heating rate to the temperature is 2° C. / sec or more.

[0010] A fourth aspect of the present invention is The method according to any one of aspects 1 to 3, wherein the heating time at the temperature is 300 seconds or less. Effect of the Invention

[0011] According to an embodiment of the present invention, it is possible to provide a method for producing an oxygen reduction catalyst that can suppress the generation of H2O2 during oxygen reduction more than ever before. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 shows LSV (linear sweep voltammetry) curves obtained using the oxygen reduction catalysts of Samples No. 1 to 5 during oxygen reduction. [Diagram 2] FIG. 2 is a graph showing the amount of hydrogen peroxide produced during oxygen reduction using the oxygen reduction catalysts of Samples No. 1 to 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present inventors have carried out investigations from various angles in order to realize a method for producing an oxygen reduction catalyst that can suppress the generation of H2O2 during oxygen reduction more than conventional methods.

[0014] Generally, in the positive electrode reaction of a solid polymer fuel cell or the like, the reactions of the following formulas (1) and (2) can occur. O2+4H + +4e - →2H2O ···(1) O2+2H + +2e - →H2O2···(2)

[0015] When platinum is used as an oxygen reduction catalyst, the four-electron reaction shown in formula (1) above occurs. On the other hand, when an Fe-NC compound is used as an oxygen reduction catalyst, in addition to the four-electron reaction, the two-electron reaction shown in formula (2) above occurs, producing hydrogen peroxide. It is believed that this hydrogen peroxide reacts mainly with the Fe sites in the Fe-NC compound that may have oxygen reduction activity, deteriorating the catalytic performance.

[0016] In response to the above, the present inventors have found that hydrogen peroxide generation can be suppressed by heating to a predetermined temperature by microwave heating or induction heating. This is believed to be due to the following mechanism. The reaction of the above formula (2) is believed to occur mainly in oxygen functional groups (C=O, CO, etc.) that may be present around the Fe site in the Fe-NC compound. Therefore, by heating the Fe-NC compound by microwave heating or induction heating, the Fe site and its periphery can be heated to a higher temperature than the average temperature of the entire Fe-NC compound (for example, the average temperature of the entire Fe-NC compound is 700 to 1200°C, while the Fe site and its periphery can be heated to a higher temperature (sometimes more than 1200°C)). This makes it possible to reduce oxygen functional groups that may be present around the Fe site while maintaining the main skeleton of the Fe-NC compound, thereby suppressing the generation of hydrogen peroxide. However, the technical scope of the present invention is not limited by the above mechanism. Each of the requirements of the embodiment of the present invention will be described in detail below.

[0017] The method for producing an oxygen reduction catalyst according to an embodiment of the present invention is characterized in that the catalytic activity of the catalyst is 1550 to 1620 cm -1 The method includes heating an Fe-NC compound having one or more peaks with a peak apex in the range of 700 to 1200°C by microwave heating or induction heating. This makes it possible to suppress the generation of H2O2 during oxygen reduction more than ever before.

[0018] The Fe-NC compound contains Fe, N, and C and has a Raman spectrum of 1550–1620 cm -1 The peak is considered to be derived from a six-membered ring structure. Such a compound may have good oxygen reduction activity.

[0019] The Fe-NC compound preferably contains Fe at 0.001 mass% or more. The Fe content is more preferably 0.01 mass% or more, even more preferably 0.1 mass% or more, and even more preferably 1.0 mass% or more. This can further improve the oxygen reduction activity of the Fe-NC compound. The upper limit of the Fe content is not particularly limited, but may be, for example, 20 mass % or less. The Fe content can be determined by the method described in the Examples below.

[0020] The Fe-NC compound preferably contains 1 to 20 atomic % of N. This can further improve the oxygen reduction activity of the Fe-NC compound. The N content can be determined by the method described in the Examples below.

[0021] The Fe-NC compound contains C in addition to Fe and N. The C content is not particularly limited, but may be, for example, 50% by mass or more and 95% by mass or less. The C content may be determined by a known measurement method.

[0022] The Fe-NC compound may contain, for example, more than 0 atomic % or 0.1 atomic % or more of O in addition to F, N, and C. If there is too much O, it may contribute to the generation of hydrogen peroxide during oxygen reduction, so it is preferable that the content is, for example, 10 atomic % or less. Other elements include H, S, etc., which are usually contained in raw materials, and their contents are not particularly limited, but may be 10 atomic % or less in total.

[0023] The Fe-NC compound may be prepared by a known method, for example, as described in Chem. Rev. 2018, 118, 2313-2339 (particularly Figure 2), for example, by a method including a step of heating a precursor containing Fe, N, and C to 700 to 1200 °C (hereinafter also referred to as the "first heating step").

[0024] The precursor is not particularly limited as long as it is a material capable of forming an Fe-NC compound, for example, as described in Chem. Rev. 2018, 118, 2313-2339 (particularly Figure 2). The precursor may be, for example, a mixture of compounds containing Fe, N, and C, a mixture of a nitrogen-containing organic compound and an Fe compound (Fe salt), or a compound containing Fe, N, and C that does not have a 6-membered ring structure (or has few 6-membered ring structures). As the precursor, ZIF-8 (zeolitic imidazole framework-8, also called a porous metal complex) containing Fe or polyaniline (or a polyaniline derivative) containing Fe is preferred.

[0025] In the first heating step, if the heating temperature is less than 700°C, the Fe-NC compound may not be sufficiently formed from the precursor. On the other hand, if the heating temperature is more than 1200°C, Fe and N may be significantly desorbed, and / or Fe particles that may inhibit the oxygen reduction reaction may be significantly generated. More preferably, the heating temperature is 1100°C or less. There is no particular limitation on the rate of temperature rise to the above heating temperature. Note that the above heating temperature refers to the average temperature of the entire precursor (and / or the Fe-NC compound).

[0026] In the first heating step, the heating method is not particularly limited and can be performed by a known method. The atmosphere during heating can be an inert gas atmosphere, hydrogen, or an ammonia-containing gas atmosphere. The inert gas can be, but is not particularly limited, nitrogen, rare gas, vacuum, or the like.

[0027] In the first heating step, the heating time at the above heating temperature is preferably, for example, 5 minutes to 50 hours. By setting the heating time to 5 minutes or more, the reaction for forming the 6-membered ring structure can be sufficiently promoted. Furthermore, by setting the heating time to 50 hours or less, the elimination of Fe and N and the generation of Fe particles can be suppressed.

[0028] After the first heating step, other steps may be performed as necessary. For example, since Fe particles that may inhibit the redox reaction may be generated together with the Fe-NC compound after heating, the Fe particles may be removed by treating the heated FNC compound with an acid. The acid used for the treatment is not particularly limited, and any known acid may be used.

[0029] The Fe-NC compound prepared as described above is heated to a temperature of 700 to 1200°C by microwave heating or induction heating (hereinafter, also referred to as the "second heating step"). This makes it possible to suppress hydrogen peroxide generation during oxygen reduction more than in the past. Conventionally, heating has generally been performed by resistance heating or the like, but this method does not sufficiently suppress hydrogen peroxide generation because it is difficult to heat the Fe site and its surroundings to a higher temperature (after the average temperature of the entire Fe-NC compound is set to 700 to 1200°C).

[0030] Microwave heating and induction heating can be carried out by known methods. Microwave heating can use microwaves of 300 MHz to 300 GHz. Microwave heating can be preferred because it can heat even complex shapes relatively easily. Microwave heating can be performed in single mode or multimode, and can be appropriately selected. In single mode microwave heating, it is preferable to perform heating at a position where the electric field strength is maximum. The induction heating may be low-frequency induction heating using a low frequency of, for example, 0.05 to 3 kHz, or high-frequency induction heating using a high frequency of 3 kHz to 300 MHz (or 3 kHz to 30 MHz). High-frequency induction heating is preferable because it can increase the temperature rise rate more quickly than low-frequency induction heating.

[0031] If the heating temperature in the second heating step is less than 700°C, the Fe site and its surroundings may not be heated sufficiently to suppress the generation of hydrogen peroxide. On the other hand, if the heating temperature in the second heating step is more than 1200°C, Fe and N may be significantly desorbed, and / or Fe particles may be significantly generated. More preferably, the heating temperature is 1100°C or less. The above heating temperature refers to the average temperature of the entire Fe-NC compound. The above heating temperature can be measured with a radiation thermometer.

[0032] The average rate of temperature rise up to the heating temperature in the second heating step is preferably 0.2° C. / sec or more, and more preferably 2° C. / sec or more, which can suppress the generation of Fe particles.

[0033] The heating time at the above heating temperature in the second heating step is preferably 3000 seconds or less, more preferably 300 seconds or less, even more preferably 100 seconds or less, and even more preferably 5 seconds or less. This makes it possible to suppress the generation of Fe particles. The lower limit of the heating time at the above heating temperature is not particularly limited and may be more than 0 seconds.

[0034] The method for producing an oxygen reduction catalyst according to an embodiment of the present invention may include other steps without departing from the object of the present invention. EXAMPLES

[0035] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all of these are included in the technical scope of the embodiments of the present invention.

[0036] <Sample preparation> A precursor of the Fe-NC compound (Fe-containing ZIF-8) powder was obtained by a known method such as that disclosed in Chem.Rev.2018,118,2313-2339 (particularly Figure 2). Specifically, 6.25 parts by mass of zinc nitrate hexahydrate (FUJIFILM Wako Pure Chemicals, purity 99.9%), 43.75 parts by mass of 2-methylimidazole (Sigma Aldrich, purity 99%), and 6.25 parts by mass of iron (III) acetylacetonate (FUJIFILM Wako Pure Chemicals, purity 99%) were mixed by stirring in methanol (FUJIFILM Wako Pure Chemicals, purity 99.8%) for 24 hours, and the obtained powder was washed by centrifugation and then dried overnight at 60 ° C. The dried powder was heated in nitrogen at 350°C for 1 hour using an electric furnace (Asahi Rika Seisakusho, ARF-30KC) while introducing nitrogen gas (Air Water Corporation, purity 99.99%) at 50 mL / min, and then further heated to 900°C and heated at 900°C for 3 hours to obtain a powder of the Fe-NC compound. The heated powder was treated with acid (stirred in 0.5M H2SO4) to remove Fe particles. The crystallinity of the Fe-NC compound powder after the acid treatment was evaluated using a Raman microscope system (inVia Reflex, RENISHAW). The measurement conditions were an excitation laser wavelength of 532 nm, objective lens magnification of 20 times, exposure time of 10 seconds, number of integrations of 1 time, and laser power of 10%. As a result, in the obtained Raman spectrum, a peak was observed at 1550-1620 cm -1 The peak had one apex in the range of

[0037] The Fe-NC compound powder after the acid treatment was heated by irradiating it with microwaves (frequency: 2.45 GHz). The Fe-NC compound powder was heated by using a single-mode microwave irradiation device having a semiconductor oscillator (Wattsine, SOLID STATE MICROWAVE GENERATOR, WSPS-2450-1500, 2.45 GHz). The Fe-NC compound powder was placed in a position in a sample chamber (quartz tube) where the electric field strength of the microwaves was maximum, and nitrogen gas (Air Water Inc., purity >99.99%) was introduced into the sample chamber at 15 mL / min. The average temperature of the powder was measured using a radiation thermometer (Japan Sensor Co., Ltd., PWCX). The heating temperature was set to 900°C (±10°C). As shown in Table 1 below, the heating rate to the heating temperature and the heating time at the heating temperature were changed to obtain oxygen reduction catalysts of Samples No. 1 to 4. For comparison, the Fe-NC compound powder after the acid treatment was heated (resistance heating) for 1 hour at 900°C (±10°C) using an electric furnace as a conventional heating method to obtain an oxygen reduction catalyst of sample No. 5.

[0038] <Evaluation of oxygen reduction reaction (ORR) activity and hydrogen peroxide production> First, in order to remove adsorbed water before evaluation, the samples were dried under vacuum conditions at 150 °C for 12 h or more. After drying, 2.5 mass parts of each catalyst were mixed with 120 μL each of distilled water and ethanol per 1 mg of catalyst, and 10 μL of Nafion dispersion liquid (Sigma-Aldrich, solvent: 1-propanol 48 ± 3 mass%, water 45 ± 3 mass%, ethanol < 4 mass%). The mixture was subjected to ultrasonic treatment for 30 minutes while cooling on ice, and the resulting solution was dropped onto a glassy carbon electrode (BAS Co., Ltd., electrode diameter 4 mm) and dried at room temperature for about 30 minutes while rotating at 700 rpm, resulting in an oxygen reduction catalyst amount of 255 μg / cm. 2 A working electrode having the above structure was fabricated.

[0039] The above working electrode was attached to a rotating electrode apparatus (BAS, RRDE-3A). The reference electrode was Ag / AgCl (BAS, RE-1CP saturated KCl silver-silver chloride reference electrode), the counter electrode was Pt wire (diameter 0.20 mm, Nilaco), and the electrolyte was 0.5 M H2SO4 solution (Wako Pure Chemical Industries, f = 0.999 (293 K)). The oxygen reduction reaction (ORR) activity and the amount of hydrogen peroxide produced were evaluated by LSV linear sweep voltammetry (LSV) measurement.

[0040] The rotating electrode device is divided into a disk electrode and a ring electrode. The disk electrode was used to detect the reactions of the above formulas (1) and (2) by LSV measurement, and the ring electrode was used to detect the oxidation reaction of hydrogen peroxide generated at the disk electrode by applying a constant potential. Specifically, N2 bubbling was first performed for 30 minutes to remove dissolved oxygen. In this state, the electrodes were rotated at 1700 rpm, and the potential was swept in the potential range of 1.0 to -0.2 V (vs. Ag / AgCl) at the disk electrode side at a sweep rate of 1 mV / sec, and a constant potential of 0.98 V (vs. Ag / AgCl) was applied to the ring electrode side, and the current value was recorded. The electrolyte was then saturated with oxygen by bubbling oxygen gas (Air Water, purity 99.5%) at a flow rate of 10 mL / min for approximately 30 minutes, and the potential was swept in the range of 1.0 to -0.2 V (vs. Ag / AgCl) at the disk electrode side at a sweep rate of 1 mV / sec, and a constant potential of 0.98 V (vs. Ag / AgCl) was applied at the ring electrode side to record the current value. The current values ​​obtained by removing dissolved oxygen as background were subtracted from the results for both the disk electrode side and the ring electrode side. In addition, the obtained results were converted from the potential (E (vs. Ag / AgCl)) based on Ag / AgCl to a standard electrode potential (E (vs. RHE)) using the following formula (3). E(vs.RHE)=E(vs.Ag / AgCl)+0.198+0.059×pH ···(3) Here, the pH was set to 0.293.

[0041] In addition, the LSV curve on the disk electrode side shows that the current density value is 10 μA / cm for the first time. 2 The potential at which the potential exceeded was determined as the ORR onset potential. The amount of hydrogen peroxide produced (%) was calculated based on the following formula (4). H2O2(%)=200×I R / (NI D +I R ) ···(4) Here, I R is the current at the ring electrode side (mA), I D is the current on the disk electrode side (mA), and N is the capture rate (=0.425).

[0042] Furthermore, a Tafel plot was created from the LSV curve on the disk electrode side, with the x-axis representing the common logarithm of the current density, log|i|, and the y-axis representing the potential V (vs. RHE). Linear approximation was performed on the obtained Tafel plot at 50 points before and after the ORR onset potential, and the obtained slope was taken as the Tafel gradient.

[0043] Figure 1 shows the LSV curves on the disk electrode side during oxygen reduction when the oxygen reduction catalysts of Samples No. 1 to 5 were used. As shown in Figure 1, when the oxygen reduction catalysts of Samples No. 1 to 5 were used, the ORR onset potentials all showed similar values.

[0044] 2 is a graph showing the amount of hydrogen peroxide generated during oxygen reduction using the oxygen reduction catalysts of samples Nos. 1 to 5. Compared to the case where sample No. 5 prepared by conventional resistance heating was used, the amount of hydrogen peroxide generated during oxygen reduction was significantly lower when samples Nos. 1 to 4 prepared by heating according to the embodiment of the present invention were used. The above results are summarized in Table 1.

[0045] [Table 1]

[0046] From Table 1, the following can be seen. Samples Nos. 1 to 4 are examples that satisfy all the requirements of the embodiment of the present invention, and compared with sample No. 5, which corresponds to the prior art, the amount of hydrogen peroxide generated was reduced. Generally, the more the amount of oxygen reduction catalyst, the more the hydrogen peroxide generation can be suppressed. In this example, 2 This demonstrated the remarkable effect of reducing the amount of hydrogen peroxide produced to a sufficiently low level (for example, 1.5% or less, a minimum of 0.4%) with such a very small amount of catalyst. Furthermore, since Samples No. 1 to No. 3 satisfied the average heating rate of 2° C. / sec or more as a preferable requirement according to the embodiment of the present invention, the absolute values ​​of the current density at 0.5 V and 0.6 V (vs. RHE) were higher. In addition, comparing Samples No. 1 to No. 3, the shorter the heating time, the higher the absolute value of the current density. This is considered to be because the increase in the average heating rate and the shortening of the heating time suppressed the generation of Fe particles that may inhibit the oxygen reduction reaction. On the other hand, sample No. 5 is an example that does not satisfy the requirements of the embodiment of the present invention, and generated a large amount of aqueous hydrogen peroxide. In addition, although the average heating rate of sample No. 5 was extremely slow and the heating time was long, the absolute value of the current density was higher than that of sample No. 4. This is thought to be because the Fe site and its surroundings were not heated to a high temperature by resistance heating of sample No. 5, and the generation of Fe particles is less likely to occur compared to microwave heating.

[0047] The ORR onset potentials of samples No. 1 to 4 were comparable to that of sample No. 5. The Tafel slopes of each were also comparable to those of the known Tafel slopes obtained with oxygen reduction catalysts made of Fe-NC compounds prepared using Fe-containing ZIF-8 as a precursor. These results suggest that there is no deterioration of the Fe-NC compounds due to heating.

[0048] To further consider the above results, the compositions (Fe content, N content, O content) of Samples Nos. 1 to 5 were analyzed.

[0049] The Fe content (mass%) was measured using an ICP emission spectrometer (Shimadzu Corporation, ICPE-9000). First, 0.4 ml of HNO3 per 1 mg of sample was added to 5 to 10 mass parts of samples No. 1 to 5, and ultrasonic cleaning was performed for 10 seconds, followed by thermal decomposition at 100°C and ultrasonic cleaning again for 10 seconds. After cooling, ultrapure water was added to the sample so that the total amount was 10 ml per 1 mg of the sample, and the sample was passed through a 0.45 μm filter to prepare a measurement sample. Thereafter, the Fe content was measured under the following measurement conditions: High frequency power: 1.20 kW, plasma gas: 10 L / min, auxiliary gas: 0.60 L / min, carrier gas: 0.70 L / min, exposure time: 30 seconds, sensitivity: wide range, observation direction: axial, solvent rinse time: Low 60 seconds, High 0 seconds, sample rinse time: Low 60 seconds, High 0 seconds, peristaltic pump rotation speed: Low 20 rpm, High 60 rpm.

[0050] The N content and O content (atomic %) were measured using an X-ray photoelectron spectroscopy (XPS) analyzer (JPS-9200, JEOL Ltd.). Indium foil (NILACO, product number: IN-203260) was placed in an Al open-type sample container (Hitachi High-Tech Science, GAA-0068, φ5.2, H2.5mm), and each sample and a Ti plate (no brand, free plate (shearing cut), width, length, and thickness all 2mm) were placed on top of it, and then pressed with a tablet molder (Jasco Engineering, MP-1 Mini press) to prepare the measurement samples. The N content and O content were then measured under the following measurement conditions (Table 2): X-ray source: MgKα (1253.6 eV), X-ray source voltage: 10 kV, filament current value: 3.5 A, lens mode (measurement area diameter): 1.0 mmφ, wide scan pass energy: 50 eV, narrow scan pass energy: 10 eV, narrow scan step width: 0.1 eV, C scan range: 296 to 280 eV, C scan accumulation number: 30, O scan range: 540 to 525 eV, O scan accumulation number: 100, N scan range: 410 to 380 eV, N scan accumulation number: 100, measurement time: approximately 3 hours / sample

[0051] [Table 2]

[0052] Consider the results in Table 2. Samples No. 1 to 4, which were subjected to the heating according to the embodiment of the present invention, had lower contents of Fe, N, and O compared to sample No. 5, which was subjected to resistance heating. Although the detailed mechanism of these results is unclear, it is believed that they are due to the fact that the Fe site and its surroundings were heated to a higher temperature by the heating according to the embodiment of the present invention. In particular, it is believed that the heating according to the embodiment of the present invention was able to reduce oxygen functional groups that may be present around the Fe site and suppress the generation of hydrogen peroxide, and it is believed that the low oxygen contents of samples No. 1 to 3 shown in Table 2 reflect at least in part the reduction in oxygen functional groups around the Fe site.

Claims

1. In the Raman spectrum, 1550 to 1620 cm -1 and heating an Fe-N-C compound having one or more peaks with a peak apex in the range of 700 to 1200°C by microwave heating or induction heating.

2. The method of claim 1 , comprising heating said Fe—N—C compound to said temperature by microwave heating.

3. The method according to claim 1 or 2, wherein the average heating rate to the temperature is 2° C. / sec or more.

4. The method according to claim 1 or 2, wherein the heating time at said temperature is 300 seconds or less.

Citation Information

Patent Citations

  • Nitrogen-containing carbon material

    JP2011256093A