Manufacturing method of crystalline film, vapor phase growth apparatus, and β-gallium oxide crystalline film
By combining trimethyl gallium, oxygen, and silicon dopant gases at controlled temperatures, the method addresses the challenge of producing high-purity β-Ga2O3 crystalline films, achieving low impurity levels and stable electron concentration for high-voltage power devices.
Patent Information
- Application Number
- JP2023084641
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional MOCVD methods face challenges in producing high-purity β-Ga2O3 crystalline films, which are essential for high-voltage power devices.
A method involving the combination of trimethyl gallium, oxygen, and silicon dopant gases in argon, heated to 850 to 1100°C, is used to form a β-gallium oxide crystal film, with a vapor phase growth apparatus that includes specific gas flow paths and heating devices to control impurity incorporation.
This approach enables the production of high-purity β-gallium oxide crystal films with low impurity levels, suitable for high-voltage power devices by minimizing carbon, hydrogen, and nitrogen content, and allowing stable electron concentration control.
Smart Images

Figure 2024168184000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a crystal film, a vapor phase growth apparatus, and a β-gallium oxide crystal film. [Background technology]
[0002] Vapor deposition is a thin-film formation method in which thin-film raw materials are turned into a gaseous state and supplied onto a substrate, where they are deposited on the substrate surface through chemical reactions. For example, gallium nitride semiconductor thin films, which are used to make blue light-emitting diodes, green light-emitting diodes, and purple laser diodes, are manufactured by MOCVD (Metal Organic Chemical Vapor Deposition), which uses organic metals as raw materials.
[0003] An example of a vapor phase growth apparatus for forming a semiconductor thin film using a vapor phase growth method is disclosed in Patent Document 1. The vapor phase growth apparatus in Patent Document 1 heats the vicinity of the substrate, while cooling the source gas flow path with a cooling device to prevent the source gas from forming a film in the flow path before reaching the substrate. In addition, the source gas flow path and the vicinity of the substrate are separated by a heat insulating plate to prevent the source gas flow path from being heated together with the vicinity of the substrate.
[0004] In recent years, gallium oxide has been attracting attention as a new semiconductor material. Gallium oxide has different crystal structures, which are designated as α, β, γ, δ, and ε types. Of these, the β type is considered to be the most thermally stable. β-Gallium oxide (β-Ga2O3) has excellent physical properties, such as a band gap of approximately 5 eV and a breakdown electric field of approximately 8 MV / cm, and is expected to be applied to high-voltage power devices. Non-Patent Document 1 reports that a film of β-gallium oxide crystals was formed by MOCVD. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 4542860 [Non-patent literature]
[0006] [Non-Patent Document 1] F.Alema,B.Hertog,A.Osinsky,P.Mukhopadhyay,M.Toporkov,and WVSchoenfeld,J.Cryst.Growth 475(2017)77-82 Summary of the Invention [Problem to be solved by the invention]
[0007] To realize high-voltage power devices, it is necessary to grow high-purity β-Ga2O3 crystalline films, but it has been difficult to obtain high-purity β-Ga2O3 crystalline films using conventional MOCVD methods. The present invention has been made in view of the above circumstances, and provides a crystal film manufacturing method, a vapor phase growth apparatus, and a β-gallium oxide crystal film that are capable of producing a high-purity β-Ga2O3 crystal film. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention employs the following configuration. [1] A plurality of source gases are joined at a joining position to obtain a mixed gas containing trimethylgallium, oxygen, and a silicon dopant in argon, and the obtained mixed gas is heated from the joining position; The heated gas mixture is then introduced onto a substrate surface, and a β-gallium oxide crystal film is grown on the substrate surface. [2] The method for producing a crystal film according to [1], wherein the joining point is heated to a temperature of 850 to 1100°C. [3] The method for producing a crystal film according to [1] or [2], wherein the plurality of source gases are a first source gas containing trimethylgallium and a silicon dopant in argon, and a second source gas containing oxygen in argon. [4] A vapor phase growth apparatus for growing a β-gallium oxide crystal film by vapor phase growth by supplying a mixed gas containing trimethylgallium, oxygen, and a silicon dopant in argon to a substrate placed in a reaction furnace, A source gas flow path for leading each of a plurality of source gases to a joining position, and a mixed gas flow path for leading the mixed gas obtained at the joining position from the joining position to the substrate surface and then discharging the mixed gas are formed in the reaction furnace, The vapor phase growth apparatus includes a heating device that heats the joining position so that the temperature is 850 to 1100°C. [5] The heating device is disposed around the part of the reactor surrounding the joining position, [4 ] The vapor phase growth apparatus according to claim 1 . [6] The vapor phase growth apparatus according to [4] or [5], wherein the source gas flow path comprises a first source gas flow path containing trimethylgallium and a silicon dopant in argon, and a second source gas flow path containing oxygen in argon. [7] The total carbon, hydrogen, and nitrogen content is 2×10 17 cm -3 and is doped with silicon, a β-gallium oxide crystalline film. [8] Donor concentration N d and the acceptor concentration N a Difference from [N d -N a ] is 10 15 cm -3 Over 10 19 cm -3 The β-gallium oxide crystal film according to [7], [9] Mobility is 30 cm 2 / Vs or more. Effect of the Invention
[0009] According to the crystal film manufacturing method and vapor phase growth apparatus of the present invention, a high-purity β-Ga2O3 crystal film can be manufactured. Furthermore, the β-gallium oxide crystal film of the present invention is highly pure and is expected to be used in high-voltage power devices. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic configuration diagram of a vapor phase growth apparatus according to a first embodiment, as viewed from the front. [Diagram 2] 1 is a schematic configuration diagram of a vapor phase growth apparatus according to a first embodiment, as viewed from above. [Diagram 3] FIG. 11 is a schematic configuration diagram of a vapor phase growth apparatus according to a second embodiment, as viewed from the front. [Figure 4] FIG. 1 is a diagram showing the results of Experimental Example 1. [Diagram 5] FIG. 13 is a diagram showing the results of Experimental Example 4. [Figure 6] FIG. 13 is a diagram showing the results of Experimental Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] First Embodiment [Vapor phase growth equipment] 1 and 2 show a vapor phase growth apparatus according to a first embodiment of the present invention. The vapor phase growth apparatus in Fig. 1 is an apparatus for forming a β-gallium oxide crystal film by vapor phase growth, and includes a reaction tube 1 in which a substrate 2 is placed, and a zone heater 10 for heating the reaction tube 1. In this embodiment, the zone heater 10 corresponds to the heating device of the present invention. Also, the reaction tube 1 corresponds to the reactor of the present invention.
[0012] In the reaction tube 1, an upstream flow channel 20, an intermediate flow channel 26, and a downstream flow channel 29 are formed. The upstream flow channel 20 corresponds to the source gas flow path of the present invention, which guides a plurality of source gases to a joining position. The intermediate flow channel 26 and the downstream flow channel 29 are flow paths that guide the mixed gas from the joining position to the substrate surface and then discharge it, and correspond to the mixed gas flow path of the present invention.
[0013] In the upstream flow channel 20, three flow paths are formed, in order from the top: a top channel 21, a middle channel 22, and a bottom channel 23. The middle channel 22 serves as a source gas flow path for supplying a first source gas to the substrate 2, and the top channel 21 and the bottom channel 23 serve as source gas flow paths for supplying a second source gas to the substrate 2.
[0014] 1 and 2, upstream flow channel 20 in this embodiment has a vertical cross section that decreases in diameter from upstream to downstream, and a horizontal cross section that increases in diameter from upstream to downstream. The downstream end has a flat shape that expands in the horizontal direction, and the first source gas flows out from the vertical center, and the second source gas flows out from above and below.
[0015] Intermediate flow channel 26 is connected to the downstream side of upstream flow channel 20, and this connection point, i.e., the upstream end of intermediate flow channel 26, corresponds to the junction position of the present invention where a plurality of source gases join together. At the joining position, the first source gas flowing out from the middle channel 22 and the second source gas flowing out from the top channel 21 and the bottom channel 23 join together, and the resulting mixed gas flows through the intermediate flow channel 26. Point A, indicated by a black circle in the figure, is the center of the joining position.
[0016] An upper opening 27 is formed in the upper pipe wall of intermediate flow channel 26, and suspended type substrate holder 3 is fitted into this upper opening 27. Suspended type substrate holder 3 has a plurality of claws for supporting substrate 2 on its underside facing the interior of intermediate flow channel 26. By placing substrate 2 on this suspended type substrate holder 3, the underside surface of substrate 2 is exposed to the mixed gas in intermediate flow channel 26. By adopting a so-called face-down type in which the lower surface of the substrate 2 is exposed to the mixed gas, it is easy to prevent unexpected adhesion of particles, etc.
[0017] The downstream flow channel 29 is connected to the downstream side of the intermediate flow channel 26, and the mixed gas that has passed through the intermediate flow channel 26 is discharged to the outside of the reaction tube 1 from the downstream side of the downstream flow channel 29.
[0018] A source gas supply pipe is connected to the upstream side of the upstream flow channel 20 . Specifically, the first source gas supply pipe 31 is connected to the middle channel 22 and supplies the first source gas to the middle channel 22. The second source gas supply pipe 32a is connected to the top channel 21 and supplies the second source gas to the top channel 21. The second source gas supply pipe 32b is connected to the bottom channel 23 and supplies the second source gas to the bottom channel 23.
[0019] The zone heater 10 is provided in an annular shape along the outer wall of the reaction tube 1. The zone heater 10 is composed of an upstream heater 11, an intermediate heater 12, and a downstream heater 13, and the temperatures of the upstream heater 11, the intermediate heater 12, and the downstream heater 13 can be set individually.
[0020] The upstream heater 11 is disposed within the outer wall of the reaction tube 1 around the portion surrounding point A so as to heat the vicinity of point A where the first raw material gas and the second raw material gas join (the upstream portion of the intermediate flow channel 26). The intermediate heating heater 12 is disposed within the outer wall of the reaction tube 1 around the portion surrounding the location where the upper opening 27 of the intermediate flow channel 26 is provided, i.e., the location where the substrate 2 is placed, so as to heat the location where the upper opening 27 is provided. The downstream heater 13 is disposed around a portion of the inner wall of the reaction tube 1 surrounding the downstream side of the upper opening 27 so as to heat the downstream side of the intermediate flow channel 26 and the downstream flow channel 29.
[0021] Furthermore, the downstream side (near point A) of upstream flow channel 20 is covered with a heat insulating box 5. Heat insulating box 5 can be constructed, for example, by sealing an alumina heat insulating material inside a hollow annular box made of quartz. By providing the heat insulating box 5, it is possible to prevent the source gas from being thermally decomposed in the upstream flow channel 20 and gallium or the like from adhering to the inside of the upstream flow channel 20.
[0022] In place of the heat insulating box 5, a heat insulating mat or the like may be wrapped around the downstream side of the upstream flow channel 20. When the insulating box 5 is used, it is possible to move the insulating box 5 in the direction of the flow of the raw material gas while maintaining the overall shape, so that it becomes easy to adjust the temperature in the vicinity of point A.
[0023] [Method of manufacturing crystal film] To produce a crystal film using the vapor phase growth apparatus of the first embodiment, the substrate 2 is suspended by the hanging-type substrate holder 3, and a mixed gas is brought into contact with the lower surface of the substrate 2 under predetermined heating conditions.
[0024] The substrate 2 is not particularly limited as long as it is plate-shaped and can support the crystal film, and may be a known substrate. It may be an insulating substrate, a conductive substrate, or a semiconductor substrate. In this embodiment, the substrate is preferably a crystal substrate.
[0025] The crystalline substrate is not particularly limited as long as it is a substrate containing a crystalline substance as a main component, and may be a known substrate. It may be an insulating substrate, a conductive substrate, or a semiconductor substrate. It may be a single crystal substrate or a polycrystalline substrate. Examples of the crystalline substrate include a substrate containing a crystalline substance having a corundum structure as a main component, a substrate containing a crystalline substance having a β-gallium structure as a main component, and a substrate having a hexagonal crystal structure. The "main component" refers to a substrate containing the crystalline substance in a composition ratio of 50% or more, preferably 70% or more, and more preferably 90% or more.
[0026] Examples of substrates containing crystals with a corundum structure as a main component include sapphire substrates and α-type gallium oxide substrates. Examples of substrates containing crystals with a β-gallium structure as a main component include β-Ga2O3 substrates and mixed crystal substrates containing β-Ga2O3 and Al2O3. Examples of substrates with a hexagonal crystal structure include SiC substrates, ZnO substrates, and GaN substrates. Examples of other crystal substrates include Si substrates.
[0027] In this embodiment, the crystal substrate is preferably a sapphire substrate. Examples of the sapphire substrate include a c-plane sapphire substrate, an m-plane sapphire substrate, and an a-plane sapphire substrate. In this embodiment, the crystal substrate is preferably a c-plane sapphire substrate. In this embodiment, the crystal substrate is also preferably an m-plane sapphire substrate, and the sapphire substrate may have an off-angle. The off-angle is not particularly limited, but is preferably 0° to 15° in the a-axis or m-axis, or in a direction including both of them. The thickness of the crystal substrate is not particularly limited, but is preferably 50 to 2000 μm, and more preferably 200 to 800 μm.
[0028] The gas mixture includes trimethylgallium vaporized in argon gas, oxygen gas, and silicon dopant gas. Trimethylgallium is the source of gallium atoms, oxygen (oxygen molecules) is the source of oxygen atoms, and argon is the carrier. Silicon dopants include monosilane, tetramethylsilane, and tetraethylsilane.
[0029] It is preferable that the trimethylgallium and oxygen contained in the mixed gas are supplied separately up to the joining point, which makes it possible to prevent the trimethylgallium and oxygen from reacting with each other before joining. It is preferable that trimethylgallium and silicon dopant are mixed in advance and then supplied to the joining position, whereby the supply ratio of silicon dopant to trimethylgallium can be stably controlled.
[0030] In this embodiment, the first raw material gas is a gas containing trimethylgallium and silicon dopant in argon, and can be supplied to the joining position via the middle channel 22. The second raw material gas is a gas containing oxygen in argon, and can be supplied to the joining position via the top channel 21 and the bottom channel 23.
[0031] The supply ratio of silicon dopant to trimethylgallium can be adjusted according to the amount of silicon to be doped in the crystal film. -9 ~10 -4 It is preferable to set the above. According to this embodiment, it is possible to prevent silicon from being unintentionally contained in the mixed gas as an impurity, and therefore it is easy to adjust the amount of silicon to be doped by adjusting the supply ratio of the silicon dopant to trimethylgallium.
[0032] The growth temperature, that is, the temperature of the mixed gas when it comes into contact with the surface of the substrate 2, is preferably 575 to 1100° C. By keeping the growth temperature at or above the preferred lower limit, the concentration of impurities incorporated into the crystal film can be reduced. The growth temperature is preferably approximately constant over the entire extent of the upstream and downstream surfaces of the substrate 2 .
[0033] The temperature at point A is preferably 850 to 1100°C, more preferably 870 to 1080°C, further preferably 890 to 1060°C, and particularly preferably 900 to 1050°C. When the temperature at point A is equal to or higher than the preferred lower limit, the concentration of impurities incorporated into the crystal film can be reduced. When the temperature at point A is equal to or lower than the preferred upper limit, it can be avoided that the temperature exceeds an appropriate growth temperature before contacting the surface of the substrate 2.
[0034] The temperature of the mixed gas before contacting the surface of substrate 2, including point A, is preferably equal to or lower than the growth temperature, and is preferably lower than the growth temperature. This makes it possible to prevent the mixed gas before reaching the surface of substrate 2 from being thermally decomposed, and to prevent gallium, gallium oxide, etc. from adhering to the inside of upstream flow channel 20 or the upstream side of intermediate flow channel 26. It is preferable that the temperature of the mixed gas from point A until it contacts the most upstream side of the surface of the substrate 2 gradually increases.
[0035] The temperature within the intermediate flow channel 26, such as at point A, can be ascertained by inserting a thermocouple 4 within the flow path. When measuring the temperature at point A, insert the tip of thermocouple 4 until it reaches point A. When measuring the temperature at point B (the position indicated by the white circle in the figure), insert the tip of thermocouple 4 until it reaches point B. Figures 1 and 2 show the state in which the tip of thermocouple 4 is retracted slightly downstream of point B.
[0036] However, if the thermocouple 4 is inserted during the actual film formation, problems such as the adhesion of the gallium oxide film to the thermocouple 4 occur. Therefore, nitrogen that does not contain trimethylgallium, silicon dopant, or oxygen is flowed for the measurement using the thermocouple 4. Then, the thermocouple 4 is pulled out from the reaction tube 1 during the film formation.
[0037] <Second embodiment> Fig. 3 shows a vapor phase growth apparatus according to a second embodiment of the present invention. The vapor phase growth apparatus in Fig. 3 is similar to that of the first embodiment, except that it is a so-called face-up type in which the upper surface of the substrate 2 is exposed to a mixed gas. In Fig. 3, the same components as those in the first embodiment are denoted by the same reference numerals as in Fig. 1, and detailed description thereof will be omitted.
[0038] Since the vapor phase growth apparatus of this embodiment is a so-called face-up type, a bottom opening 28 is formed in the lower pipe wall of the intermediate flow channel 26, and a top-mounted substrate holder 6 is fitted into this bottom opening 28. The top-loading type substrate holder 6 has a recess formed on its upper surface for placing the substrate 2 thereon, and by placing the substrate 2 on this top-loading type substrate holder 6, the upper surface of the substrate 2 is exposed to the mixed gas in the intermediate flow channel 26. The method for producing a crystal film using the vapor phase growth apparatus of this embodiment is similar to the method for producing a crystal film using the vapor phase growth apparatus of the first embodiment, except that the substrate 2 is placed on the top-mounted substrate holder 6.
[0039] <Other embodiments> In each of the above embodiments, the upstream flow channel 20 is configured to have the middle channel 22 for supplying the first source gas, and the top channel 21 and the bottom channel 23 for supplying the second source gas, but may further have a fourth channel for supplying the third source gas. In this case, the silicon dopant is not included in the first source gas, and a gas containing the silicon dopant in argon can be used as the third source gas.
[0040] Moreover, both the hanging type substrate holder 3 and the overlying type substrate holder 6 may be attached to the intermediate flow channel 26 to form an apparatus capable of simultaneously forming films by two methods, the face-down type and the face-up type. In addition, various modifications are possible without departing from the spirit and scope of the present invention.
[0041] <Mechanism of action> According to each of the above-described embodiments, a β-gallium oxide crystal film with few impurities can be efficiently obtained. The reasons for this are considered to be as follows. First, in the above embodiment, trimethylgallium is used as the gallium source.
[0042] When triethylgallium is used as a gallium source, triethylgallium, which has a low decomposition temperature, easily reacts with silicon dioxide contained in the materials (quartz, etc.) of components that come into contact with the raw material gas, such as flow channels. As a result, there is a problem that a large amount of thermally decomposed silicon is incorporated into the crystal film. In addition, triethylgallium has a low vapor pressure, making it difficult to supply high-concentration gallium to the reactor.
[0043] In the above embodiment, trimethylgallium, which has a high decomposition temperature and is not prone to self-thermal decomposition, is used as the gallium source, thereby suppressing reaction with quartz, etc., and reducing the amount of silicon unintentionally incorporated into the crystal film. In addition, trimethylgallium has a high vapor pressure, so that a high concentration of gallium can be supplied to the reactor, enabling a crystal film to be grown at high speed.
[0044] Furthermore, when an organometallic material is used as a metal source, carbon and hydrogen from the hydrocarbon group generally tend to be incorporated into the crystalline film. In each of the above embodiments, the mixed gas is heated sufficiently from the joining position. This allows the hydrocarbons generated by the decomposition of trimethylgallium to be sufficiently combusted and reacted with oxygen before reaching the substrate. This makes it possible to prevent carbon and hydrogen derived from the hydrocarbon groups from being incorporated into the crystal film.
[0045] In the above embodiment, argon is used as the carrier. If nitrogen gas is used as the carrier, nitrogen will be taken into the film and form an acceptor. Argon does not form donors or acceptors in the film.
[0046] In this manner, in the above embodiment, the amount of impurities unintentionally mixed into the β-gallium oxide crystal film can be reduced, and therefore, by adjusting the supply ratio of silicon dopant to trimethylgallium, it is possible to stably control the electron concentration in the crystal film.
[0047] Conventionally, the raw gas flow path is cooled by a cooling device to prevent the raw gas from forming a film in the flow path before reaching the substrate. In contrast, in the above embodiment, not only is cooling not performed, but the mixed gas is intentionally heated from the joining position, and film formation in the flow path is sufficiently suppressed for practical use. This is thought to be because the hydrocarbon group portion reacts more easily with oxygen than the gallium derived from trimethylgallium. The crystal film obtained in the above embodiment will now be described in detail.
[0048] <Crystalline film> The crystal film of this embodiment is a β-type gallium oxide crystal film. The crystal film of this embodiment has a total content of carbon, hydrogen, and nitrogen of 2×10 17 cm -3 The total content of carbon, hydrogen, and nitrogen is 10 17 cm -3 It is preferable that the number of the particles is less than 10. 16 cm -3 It is more preferable that:
[0049] The carbon content is 10 17 cm -3 It is preferable that the number of the particles is less than 10. 16 cm -3 More preferably, it is 10 15 cm -3 It is more preferable that the hydrogen content is 10 17 cm -3 It is preferable that the number of the particles is less than 10. 16 cm -3 More preferably, it is 10 15 cm -3 It is more preferable that the nitrogen content is 10 17 cm -3 It is preferable that the number of the particles is less than 10. 16 cm -3 More preferably, it is 10 15 cm -3 It is even more preferable that:
[0050] In addition, the content of silicon not contained as a dopant, i.e., not derived from an intentionally used silicon dopant, is 10 16 cm -3 It is preferable that the number of the particles is less than 10. 15 cm -3 It is more preferable that: The carbon, hydrogen, nitrogen and silicon contents are the average values of the concentrations in the range of 1 to 3 μm from the film surface, measured by secondary ion mass spectrometry (SIMS).
[0051] The crystal film of this embodiment is doped with silicon to be of n-type. The donor concentration N d and the acceptor concentration N a Difference from [N d -N a ] is 10 15 cm -3 Over 10 19 cm -3 The following is the result. In addition, the difference [N d -N a ] is the average value of the values in the range of 2 to 3 μm from the film surface calculated by capacitance-voltage (CV) measurement using a mercury probe. Difference [N d -N a ] is 10 15 cm -3 Over 10 19 cm -3 It is preferable that:
[0052] The crystal film of this embodiment has a mobility of 30 cm 2 / Vs or more is preferable, and 50cm 2 / Vs or more is more preferable, and 100 cm 2 It is more preferable that the mobility is equal to or higher than Vs. High mobility can suppress power loss during operation of the semiconductor device. The thickness of the crystal film in this embodiment is preferably 0.5 to 100 μm.
[0053] The crystal film of this embodiment is particularly suitable for use in semiconductor devices, and is particularly useful in power devices. Examples of semiconductor devices formed using the crystal film of this embodiment include transistors and TFTs such as MIS and HEMT, Schottky barrier diodes using semiconductor-metal junctions, PN or PIN diodes combined with other P layers, and light-receiving and light-emitting devices. The crystal film of this embodiment may be used in a semiconductor device or the like as it is formed on a substrate, or may be applied to a semiconductor device or the like after using a known method such as peeling it off from the substrate. The semiconductor device can be suitably used as a power module, an inverter or a converter by using known means, and can also be suitably used in, for example, a semiconductor system using a power supply device. EXAMPLES
[0054] <Substrate> The following substrates were used in the following experimental examples: Substrate A: (010) surface, 0.50 mm thick, Sn-doped Ga2O3 substrate (Novel Crystal Technology Co., Ltd.). Substrate B: (0001) surface, thickness 0.43 mm, m-axis off angle 0.15°, sapphire substrate (manufactured by Orbray Corporation).
[0055] <Raw materials> The following raw materials were used in the following experimental examples: TMGa: Trimethylgallium (manufactured by Taiyo Nippon Sanso Corporation). O2: Oxygen (manufactured by Taiyo Nippon Sanso Corporation). Ar: Argon (manufactured by Taiyo Nippon Sanso Corporation). TMSi: Tetramethylsilane (manufactured by Taiyo Nippon Sanso Corporation).
[0056] <Measurement method> The content of each of the impurities carbon, hydrogen, and nitrogen was measured at 64 points every 0.031 μm in the range of 1 to 3 μm from the film surface using a CAMECA secondary ion mass spectrometer IMS-6f. The content was calculated as the average of the 64 measurement results. The silicon content was measured at 53 points every 0.038 μm in the range of 1 to 3 μm from the film surface using the same device as used for measuring carbon, hydrogen, and nitrogen. The content was calculated as the average of the 53 measurement results.
[0057] Difference [N d -N a ] was measured at six points every 0.2 μm in the range of 2 to 3 μm from the film surface using a Materials Development Corporation (CV) measuring device Model 802B equipped with a mercury probe. The average of the six measurement results was calculated as the difference [N d -N a ]. The electron concentration and mobility were determined by AC Hall measurement (alternating current electromagnetic field method) using ResiTest8300 manufactured by Toyo Corporation.
[0058] The Ar, O2, and TMGa gas flow rates were measured using Fujikin FCST1030MZDTC-4J1-F5L-AR-R6-D28, FCST1005MZDTC-4J1-F1L-O2-R5-D28, and FCST1005MZDTC-4J1-F1L-AR-R4-D28, respectively. The pressure after the merging was measured using a diaphragm type vacuum gauge. The flow rate of the mixed gas was calculated from the temperature and pressure after the merging and the mixed gas flow rate.
[0059] <Experimental Example 1> The temperature distribution was confirmed for the same device as in Figure 1, except that an alumina insulation material with a volume similar to that of the insulation box was wrapped around the upstream flow channel 20 instead of the insulation box 5. The distance from point A to point B was 200 mm. The height and width of the intermediate flow channel 26 were 10 mm and 80 mm, respectively.
[0060] In order to confirm the temperature distribution using the thermocouple 4, only N2 was introduced into the apparatus. The flow rates of N2 supplied from each of the first raw material gas supply pipe 31, the second raw material gas supply pipe 32a, and the second raw material gas supply pipe 32b were each 3.0 L / min, the total flow rate was 9.0 L / min, and the pressure after merging was 1.4 kPa. As a result, when the temperature was 1000° C., the flow velocity of the mixed gas was 63.2 m / sec, and the time it took for the mixed gas to reach the center of the substrate holder from point A was 0.0019 sec.
[0061] The set temperatures of the zone heaters 10 were 600° C. for the upstream heater 11 and 960° C. for the intermediate heater 12 and downstream heater 13 . As a result, the temperature distribution shown in Figure 4 was obtained. As shown in Figure 4, the temperature at point A was 903°C, and the temperature near the substrate was kept constant at approximately 1000°C.
[0062] <Experimental Example 2> Using the same apparatus as in Experimental Example 1, a β-Ga2O3 crystal film having a thickness of 5 μm was grown on the substrate A. The thermocouple 4 was not used. The gas supplied from the first source gas supply pipe 31 was a gas containing TMGa in Ar, and the gas supplied from the second source gas supply pipes 32a and 32b was a gas containing O in Ar. TMSi was not used as a dopant.
[0063] The supply rate of TMGa was set to 182 μmol / min, and the supply rate of O2 was set to 178571 μmol / min (2.0 L / min). The supply ratio of oxygen to trimethylgallium at this time, expressed as the molar ratio of oxygen molecules to trimethylgallium, was 981. The growth time was 60 minutes. The set temperature of the zone heater 10 was the same as in Experimental Example 1. The total flow rate of the mixed gas (total flow rate after merging), the pressure after merging, the flow velocity of the mixed gas at a temperature of 1000° C., and the time it took for the mixed gas to reach the center of the substrate holder from point A were 8.4 L / min, 2.4 kPa, 34.4 m / sec, and 0.0035 sec, respectively.
[0064] The impurity concentration in the resulting crystal film was measured and found to be 3×10 16 cm -3 , hydrogen concentration is 7×10 16 cm -3 , the nitrogen concentration is 9×10 15 cm -3 , silicon concentration is 1×10 15 cm -3 Both values were extremely low, comparable to the background levels of SIMS measurements. The total content of carbon, hydrogen, and nitrogen is 2 × 10 17 cm -3 The results were as follows. In addition, the difference obtained by (CV) measurement [N d -N a ] is 2 x 10 15 cm -3 It was. This confirmed that impurities could be kept at an extremely low concentration when the temperature at the junction point was set at 903°C.
[0065] <Experimental Example 3> Using the same apparatus as in Experimental Example 1, a β-Ga2O3 crystal film having a thickness of 5 μm was grown on a substrate shown in Table 1. Thermocouple 4 was not used. The gas supplied from the first source gas supply pipe 31 was a gas containing TMGa in Ar, and the gas supplied from the second source gas supply pipes 32a and 32b was a gas containing O in Ar. TMSi was not used as a dopant.
[0066] The supply rate of TMGa was set to 182 μmol / min, and the supply rate of O2 was set to 178571 μmol / min (2.0 L / min). The supply ratio of oxygen to trimethylgallium at this time, expressed as the molar ratio of oxygen molecules to trimethylgallium, was 981. The growth time was 60 minutes.
[0067] The total flow rate, pressure, and flow rate of the mixed gas at a temperature of 1000° C., as well as the time it takes for the mixed gas to reach the center of the substrate holder from point A, were changed for each example as shown in Table 1. The set temperature of the zone heater 10 was the same as in Experimental Example 1.
[0068] The carbon concentration in the resulting crystal film was measured, and the results shown in Table 1 were obtained. From this, it was confirmed that, under the condition that the temperature at the junction point is 903°C, the impurity concentration can be kept lower by reducing the flow rate of the mixed gas and lengthening the time it takes for the mixed gas to reach the center of the substrate from point A.
[0069] [Table 1]
[0070] <Experimental Example 4> Using the same apparatus as in Experimental Example 1, a β-Ga2O3 crystal film having a thickness of 5 μm was grown on a substrate shown in Table 1. Thermocouple 4 was not used. The gas supplied from the first source gas supply pipe 31 was a gas containing TMGa and TMSi in Ar, and the gas supplied from the second source gas supply pipes 32a and 32b was a gas containing O2 in Ar.
[0071] The supply amount of TMGa was fixed at 182 μmol / min, and the supply amount of TMSi was changed to change the TMSi / TMGa supply ratio (the supply molar ratio of tetramethylsilane to trimethylgallium) in the first source gas to 9.97×10 -5 From 4.98 x 10 -7 It has been changed to.
[0072] The supply amount of O2 was set to 178571 μmol / min (2.0 L / min). The supply ratio of oxygen to trimethylgallium at this time, expressed as the molar ratio of oxygen molecules to trimethylgallium, was 981. The growth time was 60 minutes. The total flow rate, pressure, and flow rate of the mixed gas at a temperature of 1000° C., the time it took for the mixed gas to reach the center of the substrate holder from point A, and the set temperature of the zone heater 10 were the same as in Experimental Example 1.
[0073] The results of measuring the electron concentration of the resulting crystal film are shown in Figure 5. As shown in Figure 5, the electron concentration changed linearly depending on the TMSi / TMGa supply ratio. From this, it was confirmed that, under the condition that the temperature at the joining point was 903°C, by changing the TMSi / TMGa supply ratio, the influence of impurities could be suppressed and the electron concentration could be stably controlled.
[0074] <Experimental Example 5> The temperature distribution was confirmed using the same device as in Fig. 1 (the position of the insulating box 5 was also the same as in Fig. 1). The distance from point A to point B was set to 200 mm. The height and width of the intermediate flow channel 26 were set to 10 mm and 80 mm, respectively.
[0075] In order to confirm the temperature distribution using the thermocouple 4, only N2 was introduced into the apparatus. The flow rates of N2 supplied from each of the first raw material gas supply pipe 31, the second raw material gas supply pipe 32a, and the second raw material gas supply pipe 32b were each 3.0 L / min, the total flow rate was 9.0 L / min, and the pressure after merging was 1.4 kPa. As a result, when the temperature was 1000° C., the flow velocity of the mixed gas was 63.2 m / sec, and the time it took for the mixed gas to reach the center of the substrate holder from point A was 0.0019 sec.
[0076] Regarding the set temperatures of the zone heaters 10, the upstream heater 11 was set to 600° C. in Experimental Example 5-1 and 960° C. in Experimental Example 5-2. The intermediate heater 12 and downstream heater 13 were set to 960° C. in both Experimental Example 5-1 and Experimental Example 5-2. As a result, the temperature distribution shown in Figure 6 was obtained. As shown in Figure 6, the temperature at point A was 923°C in Experimental Example 5-1 and 939°C in Experimental Example 5-2. The temperature near the substrate was able to be kept constant at approximately 1000°C in both Experimental Example 5-1 and Experimental Example 5-2.
[0077] <Experimental Example 6> Using the same apparatus as in Experimental Example 1, a β-Ga2O3 crystal film having a thickness of 5 μm was grown on the substrate A. The thermocouple 4 was not used. The gas supplied from the first source gas supply pipe 31 was a gas containing TMGa in Ar, and the gas supplied from the second source gas supply pipes 32a and 32b was a gas containing O in Ar. TMSi was not used as a dopant.
[0078] The supply rate of TMGa was set to 182 μmol / min, and the supply rate of O2 was set to 178571 μmol / min (2.0 L / min). The supply ratio of oxygen to trimethylgallium at this time, expressed as the molar ratio of oxygen molecules to trimethylgallium, was 981. The growth time was 60 minutes. The set temperature of the zone heater 10 was the same as that of Experimental Example 5-1 in Experimental Example 6-1, and was the same as that of Experimental Example 5-2 in Experimental Example 6-2. The total flow rate of the mixed gas (total flow rate after merging), the pressure after merging, the flow velocity of the mixed gas at a temperature of 1000° C., and the time it took for the mixed gas to reach the center of the substrate holder from point A were 8.4 L / min, 1.4 kPa, 59.0 m / sec, and 0.0020 sec, respectively.
[0079] When the carbon concentration in the obtained crystal film was measured, the carbon concentration in Experimental Example 6-1 was 6×10 17 cm -3 , the carbon concentration in Experimental Example 6-2 is 1×10 17 cm -3 It was. From this, it was confirmed that the carbon concentration could be kept lower by increasing the temperature at point A from 923°C to 939°C. [Explanation of symbols]
[0080] 1 Reaction tube 2. Board 3 Hanging PCB holder 4 Thermocouples 5. Insulation box 6 Top-mounted PCB holder 10 Zone Heater 11 Upstream heating heater 12 Intermediate heating heater 13 Downstream heating heater 20 Upstream Flow Channel 21 Top Channel 22 Middle Channel 23 Bottom Channel 26 Intermediate Flow Channel 27 Top opening 28 Bottom opening 29 Downstream Flow Channel 31 First raw gas supply pipe 32a Second raw material gas supply pipe 32b Second raw material gas supply pipe
Claims
1. A plurality of source gases are joined at a joining position to obtain a mixed gas containing trimethylgallium, oxygen, and a silicon dopant in argon, and the obtained mixed gas is heated from the joining position; The heated mixed gas is then introduced onto a substrate surface, and a β-gallium oxide crystal film is grown on the substrate surface.
2. 2. The method for producing a crystal film according to claim 1, wherein heating is performed so that the temperature at the joining point is 850 to 1100.degree.
3. 3. The method for producing a crystal film according to claim 1, wherein the plurality of source gases are a first source gas containing trimethylgallium and a silicon dopant in argon, and a second source gas containing oxygen in argon.
4. A vapor phase growth apparatus for growing a β-gallium oxide crystal film by vapor phase growth by supplying a mixed gas containing trimethylgallium, oxygen, and a silicon dopant in argon to a substrate placed in a reaction furnace, A source gas flow path for leading each of a plurality of source gases to a joining position, and a mixed gas flow path for leading the mixed gas obtained at the joining position from the joining position to the substrate surface and then discharging the mixed gas are formed in the reaction furnace, a vapor phase growth apparatus including a heating device for heating the joining position so that the temperature is 850 to 1100°C;
5. The vapor phase growth apparatus according to claim 4 , wherein the heating device is disposed around a portion of the reaction furnace surrounding the joining position.
6. 6. The vapor phase growth apparatus according to claim 4, wherein the source gas flow passage comprises a first source gas flow passage containing trimethylgallium and a silicon dopant in argon, and a second source gas flow passage containing oxygen in argon.
7. The total content of carbon, hydrogen, and nitrogen is 2 x 10 17 cm -3 and is doped with silicon.
8. Donor concentration N d and the acceptor concentration N a The difference between [N d -N a ] is 10 15 cm -3 More than 10 19 cm -3 The β-gallium oxide crystal film according to claim 7, wherein:
9. Mobility is 30 cm 2 The β-gallium oxide crystal film according to claim 7 or 8, wherein Vs is 0.1 V or more.
Citation Information
Patent Citations
Vapor phase growth apparatus
JP4542860B2