Polyamide composition and molding

The polyamide composition with an acid-modified elastomer and specific structural units addresses rigidity and paintability issues in humid conditions, ensuring both properties are maintained in molded articles.

JP2024168252APending Publication Date: 2024-12-05ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023084758
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Polyamides used in sports equipment face challenges in maintaining rigidity and paintability in humid environments due to moisture absorption, with long chain skeletons reducing rigidity and hydrophilicity affecting paintability.

Method used

A polyamide composition is developed by incorporating a small amount of acid-modified elastomer with a high melting point and aromatic skeleton, along with specific dicarboxylic acid units and a C/N ratio, to suppress rigidity loss and enhance paintability.

Benefits of technology

The composition maintains rigidity and improves paintability in moisture-absorbed states, achieving both properties in molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168252000001
    Figure 2024168252000001
Patent Text Reader

Abstract

To provide a polyamide composition excellent in rigidity reduction inhibition when absorbing moisture, and coating property, and a molding obtained by molding the polyamide composition.SOLUTION: A polyamide composition includes a polyamide and an acid-modified elastomer, wherein the polyamide includes a dicarboxylic acid unit, a content percentage of an aromatic dicarboxylic acid unit to a total mole amount of the dicarboxylic acid units is 50 mol% or more, a C / N ratio of a polymer unit is greater than 6.0 and less than 8.0, a melting peak temperature of the polyamide composition is 310°C or higher in differential scanning calorimetry according to JIS-K7121, and an amount of the acid-modified elastomer is less than 6 mass% based on 100 mass% of the polyamide composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide composition and a molded article. [Background technology]

[0002] Traditionally, metal parts have been used for sports equipment that requires strength, such as bicycle parts, but in recent years, polyamides, which have high mechanical properties, have been widely used as replacements for metal parts to reduce weight.

[0003] Known uses for sporting goods include not only bicycle parts, but also rackets, spinning reels, etc. After production, parts for these applications take several weeks to several months to be delivered to the user due to transportation, etc. In addition, parts used around water, such as spinning reels, are exposed to humid environments.

[0004] In general, polyamides are known to be prone to moisture absorption due to the presence of hydrophilic amide groups, which reduces their rigidity. For this reason, efforts have been made to reduce water absorption by using skeletons containing long chains or aromatic ring skeletons (Patent Documents 1 and 2).

[0005] On the other hand, sporting goods are often painted because design is also important, and the more hydrophilic the resin used in the parts is, the better the paintability, since the solvent will more easily blend into the surface. For this reason, polyamides with long chain skeletons that have low moisture absorption have poor paintability, and it has been an issue to balance maintaining rigidity in a hygroscopic state with good paintability. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 672065 [Patent Document 2] JP 2009-215514 A Summary of the Invention [Problem to be solved by the invention]

[0007] Generally, when used in humid environments, heat resistance is not required, so polyamides with long chain skeletons and low amide group concentration have been used, even if they have low melting points. It is also known that polyamides with aromatic skeletons have low moisture absorption due to the hydrophobicity derived from aromatics. However, polyamides with short chain skeletons have higher moisture absorption than polyamides with long chain skeletons, and their physical properties tend to be worse when absorbing moisture.

[0008] Therefore, an object of the present invention is to provide a polyamide composition which is excellent in terms of suppressing a decrease in rigidity upon moisture absorption and in terms of paintability, and a molded article obtained by molding the polyamide composition. [Means for solving the problem]

[0009] In the present invention, it was found that by adding a small amount of acid-modified elastomer to a high melting point polyamide having a short chain skeleton, which has a high amide group concentration and an aromatic skeleton, it is possible to suppress the decrease in rigidity when absorbing moisture. It was also found that by having a high amide group concentration and moderate moisture absorption, the paintability, which was an issue with long chain skeleton polyamide, becomes good, and it is possible to achieve both rigidity retention in a hygroscopic state and good paintability. That is, the present invention includes the following aspects. [1] Polyamide, An acid-modified elastomer; A polyamide composition comprising: The polyamide comprises dicarboxylic acid units, the content of aromatic dicarboxylic acid units relative to the total molar amount of the dicarboxylic acid units is greater than 50 mol %; The C / N ratio of the polymer unit is greater than 6.0 and less than 8.0; In a differential scanning calorimetry measurement according to JIS-K7121, the polyamide composition has a melting peak temperature of 310° C. or higher; A polyamide composition, wherein the amount of the acid-modified elastomer is less than 6% by mass, based on 100% by mass of the polyamide composition. [2] The polyamide composition according to [1], wherein the polyamide contains a diamine unit, and the diamine unit has 4 to 6 carbon atoms. [3] The polyamide composition according to [2], wherein the diamine units include tetramethylenediamine units. [4] The polyamide composition according to any one of [1] to [3], wherein the aromatic dicarboxylic acid unit is a terephthalic acid unit. [5] The polyamide composition according to [4], wherein the content of the terephthalic acid units is 90 to 100 mol % based on the total molar amount of the dicarboxylic acid units. [6] The polyamide composition according to any one of [1] to [5], further comprising a filler, the filler being a fibrous filler. [7] The polyamide composition according to any one of [1] to [6], further comprising a filler, the filler being glass fiber or carbon fiber. [8] The polyamide composition according to any one of [1] to [7], further comprising a filler, the filler being carbon fiber. [9] The polyamide composition according to any one of [1] to [8], wherein the peak melting temperature is 325° C. or higher.

[10] A molded article obtained by molding the polyamide composition according to any one of [1] to [9]. Effect of the Invention

[0010] The polyamide composition of the present invention, when formed into a molded article, exhibits excellent suppression of decrease in rigidity upon moisture absorption and excellent paintability. The molded article of the present invention exhibits excellent suppression of decrease in rigidity upon moisture absorption and excellent paintability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out with appropriate modifications within the scope of its gist.

[0012] In this specification, polyamide means a polymer having an amide bond (-NHCO-) ​​in the main chain.

[0013] In this specification, semi-aromatic polyamide means a polyamide having aliphatic units and aromatic units. The aliphatic units refer to units derived from aliphatic monomers. The aromatic units refer to units derived from aromatic monomers.

[0014] Unless otherwise specified, the materials, components, compounds, resins and solvents described in this specification may be used alone or in combination of two or more.

[0015] In this specification, unless otherwise specified, any numerical range is intended to include the upper and lower limits of the range, for example, 90 to 100 mol% means a range of 90 mol% or more and 100 mol% or less.

[0016] In the present embodiment, the melting peak temperature of the polyamide composition is a value measured by the measurement method described in the Examples.

[0017] Polyamide Composition The polyamide composition of the present embodiment contains a polyamide and an acid-modified elastomer, which makes it possible to produce a molded article that is inhibited from decreasing in rigidity upon moisture absorption and has excellent paintability.

[0018] Hereinafter, each of the components of the polyamide composition of the present embodiment will be described in detail.

[0019] polyamide The polyamide contained in the polyamide composition of the present embodiment is preferably composed of only semi-aromatic polyamide from the viewpoints of suppressing a decrease in rigidity upon moisture absorption and of paintability.

[0020] Semi-aromatic polyamide The constituent units of the semi-aromatic polyamide preferably satisfy at least one of the following conditions (1) and (2): It is particularly preferable that the constituent units of the semi-aromatic polyamide satisfy (1). (1) It contains aromatic dicarboxylic acid units, aliphatic dicarboxylic acid units and aliphatic diamine units. (2) It contains an aromatic dicarboxylic acid unit and an aliphatic diamine unit.

[0021] Aromatic dicarboxylic acid unit The aromatic dicarboxylic acid unit may be a terephthalic acid unit or an isophthalic acid unit, and preferably a terephthalic acid unit. The aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit other than the terephthalic acid unit may be, for example, a dicarboxylic acid having an aromatic group such as a phenyl group or a naphthyl group. The aromatic group of the aromatic dicarboxylic acid may be unsubstituted or may have a substituent.

[0022] The substituent is not particularly limited, but examples thereof include an alkyl group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, an arylalkyl group having 7 to 10 carbon atoms, an alkylaryl group having 7 to 10 carbon atoms, a halogen group, a silyl group having 1 to 6 carbon atoms, a sulfonic acid group, and a salt thereof (such as a sodium salt).

[0023] Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group.

[0024] Examples of the aryl group having 6 to 10 carbon atoms include a phenyl group and a naphthyl group.

[0025] Examples of the arylalkyl group having 7 to 10 carbon atoms include a benzyl group.

[0026] Examples of the alkylaryl group having 7 to 10 carbon atoms include a tolyl group and a xylyl group.

[0027] Examples of the halogen group include a fluoro group, a chloro group, a bromo group, and an iodo group.

[0028] Examples of the silyl group having 1 to 6 carbon atoms include a trimethylsilyl group and a tert-butyldimethylsilyl group.

[0029] The aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit other than the isophthalic acid unit is preferably an aromatic dicarboxylic acid having 8 to 20 carbon atoms which is unsubstituted or substituted with a predetermined substituent.

[0030] Examples of the unsubstituted or substituted aromatic dicarboxylic acid having 8 to 20 carbon atoms include terephthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, and 5-sodium sulfoisophthalic acid.

[0031] In a preferred embodiment, the content of terephthalic acid units relative to the total molar amount of dicarboxylic acid units is 90 to 100 mol %.

[0032] Aliphatic dicarboxylic acid unit Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit include linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms. Examples of linear saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane diacid, and diglycolic acid. Examples of branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms include dimethylmalonic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid.

[0033] As the aliphatic dicarboxylic acid, a linear saturated aliphatic dicarboxylic acid having 6 or more carbon atoms is preferred because the polyamide composition tends to have better heat resistance, fluidity, toughness, low water absorption, rigidity, etc. As the linear saturated aliphatic dicarboxylic acid having 6 or more carbon atoms, adipic acid, sebacic acid, or dodecanedioic acid is preferred from the viewpoint of the heat resistance, etc. of the polyamide composition.

[0034] Aliphatic diamine units Examples of the aliphatic diamine constituting the aliphatic diamine unit include linear saturated aliphatic diamines having 2 to 20 carbon atoms, and branched saturated aliphatic diamines having 3 to 20 carbon atoms. Examples of the linear saturated aliphatic diamines having 2 to 20 carbon atoms include ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, and tridecamethylenediamine. Examples of branched saturated aliphatic diamines having 3 to 20 carbon atoms include 2-methylpentamethylenediamine (also referred to as 2-methyl-1,5-diaminopentane), 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,8-octanediamine (also referred to as 2-methyloctamethylenediamine), and 2,4-dimethyloctamethylenediamine.

[0035] The carbon number of the aliphatic diamine is preferably 4 to 12, and more preferably 4 to 10. When the carbon number of the aliphatic diamine constituting the aliphatic diamine unit is 4 or more, the heat resistance of the obtained molded article is more excellent. On the other hand, when the carbon number is 12 or less, the crystallinity and releasability of the obtained molded article are more excellent. In one embodiment, the carbon number of the aliphatic diamine unit is 4 to 6.

[0036] Specific examples of preferred linear or branched saturated aliphatic diamines having 4 to 12 carbon atoms include tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 2-methylpentamethylenediamine, and 2-methyl-1,8-octanediamine. Preferred linear or branched saturated aliphatic diamines having 4 to 12 carbon atoms are tetramethylenediamine, hexamethylenediamine, and 2-methylpentamethylenediamine. By including such an aliphatic diamine unit, the rigidity of a molded article obtained from the polyamide composition is improved.

[0037] In addition, the semi-aromatic polyamide may further contain units derived from a trivalent or higher polyvalent aliphatic amine, if necessary, within a range that does not impair the effects of the polyamide composition of the present embodiment. Examples of trivalent or higher polyvalent aliphatic amines include bishexamethylenetriamine.

[0038] In one embodiment, the semi-aromatic polyamide is one or more selected from the group consisting of polyamide 4T / 6T, polyamide 4T / 6T / 66 and polyamide 6T / 6I, where 4 represents tetramethylenediamine units, 6 represents hexamethylenediamine units, T represents terephthalic acid units and I represents isophthalic acid units.

[0039] As the semi-aromatic polyamide, from the viewpoint of mechanical properties and heat resistance, polyamides containing dicarboxylic acid units and diamine units are preferred, and polyamide 4T / 6T is more preferred. Polyamide 4T / 6T is considered to be a suitable material for automobile parts because of its excellent mechanical properties, heat resistance, moldability and toughness.

[0040] The polyamide composition has a peak melting temperature of 310°C or higher. The polyamide composition has a peak melting temperature of 310°C or higher, which tends to provide excellent heat resistance. The polyamide composition has a peak melting temperature of, for example, 310 to 332°C. In one embodiment, the polyamide composition has a peak melting temperature of 325°C or higher. In another embodiment, the polyamide composition has a peak melting temperature of 315 to 330°C.

[0041] The content of the semi-aromatic polyamide can be, for example, 50 to 100 mass%, for example, 55 to 100 mass%, for example, 57 to 100 mass%, relative to the total mass of polyamide in the polyamide composition.

[0042] The C / N ratio of a polymer unit is calculated by dividing the number of carbon atoms contained in the monomer unit of the polyamide by the number of nitrogen atoms. In the case of polyamides made of diamines and dicarboxylic acids, the monomer unit is a 1:1 condensation of diamines and dicarboxylic acids. The C / N ratio of the polymer unit is more than 6.0 and less than 8.0, so that the moisture absorption rate falls within an appropriate range. In one embodiment, the C / N ratio of the polymer unit is 6.4 to 7.0.

[0043] End-capping agent The terminals of the polyamide contained in the polyamide composition of the present embodiment may be capped with a known terminal capping agent. By blocking the terminals of the polyamide with a terminal capping agent, the thermal stability of the molded product obtained from the polyamide composition tends to be better. Such terminal capping agents can also be added as molecular weight regulators when producing polyamide from dicarboxylic acid and diamine, or from at least one selected from the group consisting of lactam and aminocarboxylic acid.

[0044] Examples of the terminal blocking agent include monocarboxylic acid, monoamine, acid anhydride (phthalic anhydride, etc.), monoisocyanate, monoesters, monoalcohols, etc. The terminal blocking agent is preferably monocarboxylic acid or monoamine.

[0045] The monocarboxylic acid that can be used as the terminal blocking agent may be any one that is reactive with the amino group that may be present at the terminal of the polyamide. Examples of the monocarboxylic acid include aliphatic monocarboxylic acids, alicyclic monocarboxylic acids, and aromatic monocarboxylic acids. Examples of the aliphatic monocarboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecyl acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid. Examples of the alicyclic monocarboxylic acids include cyclohexane carboxylic acid. Examples of the aromatic monocarboxylic acids include benzoic acid, toluic acid, α-naphthalene carboxylic acid, β-naphthalene carboxylic acid, methylnaphthalene carboxylic acid, and phenyl acetic acid. In particular, it is preferable that the terminals of the semi-aromatic polyamide are blocked with acetic acid from the viewpoints of fluidity and mechanical strength.

[0046] The monoamine that can be used as the terminal blocking agent may be any monoamine that has reactivity with the carboxyl group that may be present at the terminal of the polyamide. Examples of the monoamine include aliphatic monoamines, alicyclic monoamines, and aromatic monoamines. Examples of the aliphatic monoamines include methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine. Examples of the alicyclic monoamines include cyclohexylamine and dicyclohexylamine. Examples of the aromatic monoamines include aniline, toluidine, diphenylamine, and naphthylamine.

[0047] Polyamide compositions containing polyamide end-capped with an end-capping agent tend to have better heat resistance, flowability, toughness, low water absorption, and rigidity.

[0048] Polyamide manufacturing method When producing the polyamide (semi-aromatic polyamide) contained in the polyamide composition of the present embodiment, the amount of dicarboxylic acid added and the amount of diamine added are preferably approximately the same molar amount. Taking into consideration the amount of diamine that escapes to the outside of the reaction system during the polymerization reaction, the molar amount of the total diamine relative to the molar amount of the total dicarboxylic acid is preferably 0.9 to 1.2, more preferably 0.95 to 1.10, and even more preferably 0.98 to 1.05.

[0049] The method for producing polyamide includes, for example, the following polymerization step (1) or (2). (1) A step of polymerizing a combination of a dicarboxylic acid constituting a dicarboxylic acid unit and a diamine constituting a diamine unit to obtain a polymer. (2) A step of polymerizing one or more members selected from the group consisting of lactam constituting the lactam unit and aminocarboxylic acid constituting the aminocarboxylic acid unit to obtain a polymer.

[0050] The method for producing polyamide preferably further includes, after the polymerization step, an increasing step of increasing the degree of polymerization of the polyamide. If necessary, the method may include, after the polymerization step and the increasing step, a capping step of capping the ends of the obtained polymer with a terminal capping agent.

[0051] Specific examples of the method for producing polyamide include various methods such as the following first to fourth methods. The first method is to heat an aqueous solution or suspension of one or more selected from the group consisting of a dicarboxylic acid-diamine salt, a mixture of a dicarboxylic acid and a diamine, a lactam, and an aminocarboxylic acid, and polymerize the resulting solution while maintaining the molten state (hereinafter, this may be referred to as the "thermal melt polymerization method"). Second: A method in which the degree of polymerization of polyamide obtained by the hot melt polymerization method is increased while maintaining the polyamide in a solid state at a temperature below the melting point (hereinafter sometimes referred to as "hot melt polymerization / solid-state polymerization method"). Third: A method of polymerizing one or more selected from the group consisting of dicarboxylic acid-diamine salts, mixtures of dicarboxylic acids and diamines, lactams, and aminocarboxylic acids while maintaining the solid state (hereinafter, sometimes referred to as "solid-state polymerization method"). Fourth: A method of polymerization using a dicarboxylic acid halide component equivalent to a dicarboxylic acid and a diamine component (hereinafter, sometimes referred to as a "solution method").

[0052] A specific method for producing polyamide is preferably a method including a hot melt polymerization method. When producing polyamide by hot melt polymerization, it is preferable to maintain the molten state until the polymerization is completed. In order to maintain the molten state, it is necessary to produce the polyamide composition under polymerization conditions suitable for the composition. Examples of the polymerization conditions include the following conditions. First, the polymerization pressure in the hot melt polymerization method is set to 14 to 25 kg / cm. 2 (gauge pressure) and continue heating. Next, the pressure in the vessel is controlled to atmospheric pressure (gauge pressure is 0 kg / cm 2 ) over 30 minutes or more until the blood pressure drops to 0.

[0053] In the method for producing polyamide, the polymerization form is not particularly limited, and may be a batch type or a continuous type. The polymerization apparatus used for producing polyamide is not particularly limited, and a known apparatus may be used. Specific examples of the polymerization apparatus include an autoclave type reactor, a tumbler type reactor, and an extruder type reactor (such as a kneader).

[0054] As a method for producing polyamide, a method for producing polyamide by a batch-type hot melt polymerization method will be specifically exemplified below.

[0055] First, an aqueous solution containing about 40 to 60% by mass of raw material components of polyamide (a combination of dicarboxylic acid and diamine, and at least one selected from the group consisting of lactam and aminocarboxylic acid, if necessary) is prepared. Then, the aqueous solution is concentrated to about 65 to 90% by mass in a concentration tank operated at a temperature of 110 to 180°C and a pressure of about 0.035 to 0.6 MPa (gauge pressure) to obtain a concentrated solution. Then, the concentrated solution obtained is transferred to an autoclave, and heating is continued until the pressure in the autoclave becomes about 1.2 to 2.2 MPa (gauge pressure). Then, in the autoclave, the pressure is maintained at about 1.2 to 2.2 MPa (gauge pressure) while removing at least one of water and gas components. Then, when the temperature reaches about 220 to 260°C, the pressure is reduced to atmospheric pressure (gauge pressure is 0 MPa). After the pressure in the autoclave is reduced to atmospheric pressure, the pressure can be reduced as necessary to effectively remove by-product water. The autoclave is then pressurized with an inert gas such as nitrogen, and the polyamide melt is extruded from the autoclave as a strand. The extruded strand is cooled and cut to obtain polyamide pellets.

[0056] Polyamide properties Polyamide polymer end The polymer ends of the polyamide contained in the polyamide composition of the present embodiment are not particularly limited, but can be classified and defined as follows into the following first to fourth types: First: amino end, Second: carboxy end, Third: end due to a capping agent, Fourth: other end. The first: amino terminus is a polymer terminus having an amino group (-NH2 group) and is derived from a diamine unit. The second: carboxyl end is a polymer end having a carboxy group (-COOH group) and is derived from a dicarboxylic acid unit. The third terminal formed by a capping agent is a terminal formed when a capping agent is added during polymerization. Examples of the capping agent include the above-mentioned terminal capping agents. Fourth: Other terminals are polymer terminals that are not classified into the above-mentioned first to third types. Specific examples of other terminals include terminals generated by deammonia reaction of amino terminals, terminals generated by decarboxylation of carboxyl terminals, etc.

[0057] Acid-modified elastomer The acid-modified elastomer has the function of improving the hydrophobicity of the polyamide composition. The acid-modified elastomer contained in the polyamide composition of this embodiment is, for example, an elastomer such as ethylene vinyl acetate (EVA), ethylene acrylate copolymer (EEA), polyethylene (PE), polypropylene (PP), or a styrene-based elastomer (styrene-ethylenebutylene-styrene copolymer: SEBS, styrene-ethylenepropylene-styrene copolymer: SEPS, etc.) modified with maleic anhydride. From the viewpoint of heat resistance, the acid-modified elastomer is particularly preferably an acid-modified polyolefin, SEBS, or SEPS. In one embodiment, the acid-modified elastomer is one or more types of acid-modified elastomers selected from the group consisting of EVA, EEA, PE, PP, SEBS, and SEPS. In another embodiment, the acid-modified elastomer is one or more types of maleic anhydride-modified elastomers selected from the group consisting of EVA, EEA, PE, PP, SEBS, and SEPS.

[0058] In this embodiment, the amount of the acid-modified elastomer is less than 6% by mass, based on 100% by mass of the polyamide composition. The amount of the acid-modified elastomer is preferably 2.0% by mass or more and less than 6.0% by mass, more preferably 2.5 to 5.5% by mass, and particularly preferably 3.0 to 5.0% by mass, based on 100% by mass of the polyamide composition. In one embodiment, the amount of the acid-modified elastomer is 3.0 to 4.5% by mass.

[0059] filling material The polyamide composition of the present embodiment may further contain a filler in addition to the polyamide and the acid-modified elastomer. By containing the filler, the polyamide composition can have more excellent mechanical properties such as toughness and rigidity.

[0060] Examples of the filler contained in the polyamide composition of the present embodiment include glass fiber and carbon fiber. In addition, for example, the filler described in JP-A-2023-035802 may be used. As the filler, glass fiber or carbon fiber is more preferable, and glass fiber is further preferable.

[0061] The number average fiber diameter and weight average fiber length of the filler can be measured using the method described in JP 2023-035802 A.

[0062] The content of the filler in the polyamide composition is preferably 1 to 80 mass%, more preferably 5 to 70 mass%, further preferably 10 to 60 mass%, particularly preferably 15 to 55 mass%, and most preferably 20 to 50 mass%, based on the total mass of the polyamide composition. When the content of the filler is 1 mass% or more, the mechanical properties such as strength and rigidity of the polyamide composition tend to be further improved. On the other hand, when the content of the filler is 80 mass% or less, a polyamide composition having better moldability tends to be obtained.

[0063] Other additives The polyamide composition of the present embodiment may contain other additives commonly used in polyamides, such as moldability improvers, deterioration inhibitors, nucleating agents, and heat stabilizers, within the range that does not impair the effects of the polyamide composition of the present embodiment.

[0064] Moldability improver Examples of the moldability improver include those described in JP-A-2022-115097.

[0065] Deterioration inhibitor Examples of the deterioration inhibitor include those described in JP-A-2021-050323.

[0066] Nucleating Agent Examples of nucleating agents include those described in JP-A-2021-050323.

[0067] Heat stabilizer Examples of the heat stabilizer include those described in JP-A-2023-028935 and JP-A-2021-050323.

[0068] Method for producing polyamide composition The method for producing the polyamide composition of the present embodiment is not particularly limited as long as it is a method for mixing a polyamide, an acid-modified elastomer, and an optional component. For example, the method described in JP-A-2023-035802 can be mentioned. The blending amount of each component when producing the polyamide composition of the present embodiment is the same as the content of each component in the polyamide composition described above.

[0069] When the polyamide contains a semi-aromatic polyamide, the melt kneading temperature is preferably about 1 to 100° C. higher than the melting point of the semi-aromatic polyamide, and more preferably about 10 to 50° C. higher than the melting point of the semi-aromatic polyamide.

[0070] The shear rate in the mixer is 100 sec -1 The average residence time during kneading is preferably about 0.5 to 5 minutes.

[0071] The melt-kneading apparatus may be any known apparatus, and examples of the apparatus include the method described in JP-A-2023-028935.

[0072] molded product The molded article of the present embodiment is produced by molding a polyamide composition.

[0073] The method for obtaining a molded product is not particularly limited, and a known molding method can be used. Examples of the known molding method include the method described in JP-A-2022-115097.

[0074] Purpose The molded article of the present embodiment is obtained by molding a polyamide composition, and has excellent elastic modulus retention in a wet state and excellent paintability, and can be used in various applications. The molded article can be suitably used in, for example, humid environment applications such as sporting goods, the automotive field, the electrical and electronic field, the mechanical and industrial field, the office equipment field, and the aviation and space field. EXAMPLES

[0075] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.

[0076] Each of the components of the polyamide composition used in the present examples and comparative examples will be described below.

[0077] polyamide Polyamide 4T / 6T, synthesized as described below, indicated as "4T / 6T" in the table Polyamide 4T / 6T / 66, synthesized as described below, indicated as "4T / 6T / 66" in the table Polyamide 6T / 6I, synthesized as described below, indicated as "6T / 6I" in the table Polyamide 9T / 2Me8T (Kuraray, Genestar TM N1000, indicated as "9T / 2Me8T" in the table Polyamide 610, synthesized as described below, indicated as "610" in the table

[0078] Acid-modified elastomer Acid-modified polyolefin (manufactured by Mitsui Chemicals, Inc., model number: TAFMER (registered trademark) MH5020), indicated as "MH5020" in the table Acid-modified hydrogenated styrene-based thermoplastic elastomer (Tuftec (registered trademark) M1911, manufactured by Asahi Kasei Corporation), indicated as "M1911" in the table Maleic anhydride modified polyphenylene ether (m-PPE) (manufactured by Asahi Kasei Corporation) (oxygen index: 28%, molecular weight: 54,000), indicated as "m-PPE" in the table.

[0079] filling material Carbon fiber (CF) (manufactured by Teijin Ltd., product name "HT C413"), indicated as "HT C413" in the table

[0080] Polyamide manufacturing The methods for producing the semi-aromatic polyamides are described in detail below. The aliphatic polyamides and semi-aromatic polyamides obtained by the following methods were dried in a nitrogen stream to adjust the moisture content to about 0.2% by mass, and then used as raw materials for the polyamide compositions in the following examples and comparative examples.

[0081] Synthesis Example 1: Synthesis of polyamide 4T / 6T The compound was synthesized by the method described in paragraph

[0052] of JP2020-513438A.

[0082] Synthesis Example 2: Synthesis of polyamide 4T / 6T / 66 The compound was synthesized according to the method described in paragraph

[0055] of JP-T-2009-524711.

[0083] Synthesis Example 2: Synthesis of polyamide 6T / 6I The compound was synthesized by the method described in paragraph

[0081] of JP 2018-145292 A.

[0084] Synthesis Example 3: Synthesis of Polyamide 610 Polyamide 610 was obtained by the method described in paragraph

[0043] of JP2016-030787A.

[0085] Preparation of polyamide compositions Example 1 Using a TEM 35mm twin-screw extruder (set temperature: 350°C, screw rotation speed: 300 rpm) manufactured by Toshiba Machine Co., Ltd., a mixture of polyamide 4T / 6T and acid-modified elastomer MH5020 was fed from the top feed port provided at the most upstream part of the extruder. A filler was also fed from the side feed port on the downstream side of the extruder (in a state where the resin fed from the top feed port was fully melted). Next, the molten kneaded product extruded from the die head was cooled in a strand shape and pelletized to obtain pellets of a polyamide composition. The blending amounts are shown in Table 1. The blending amount of each component is in mass%.

[0086] In addition, the obtained polyamide composition pellets with the adjusted moisture content were molded into multipurpose test pieces (A-type, dumbbell-shaped tensile test pieces) in accordance with ISO3167 using an injection molding machine (PS-40E, manufactured by Nissei Plastics Co., Ltd.). The dimensions of the multipurpose test piece are: total length ≧170 mm, distance between tabs 109.3±3.2 mm, length of parallel part 80±2 mm, radius of shoulder 24±1 mm, width of end 20±0.2 mm, width of central parallel part 10±0.2 mm, and thickness 4±0.2 mm. Specific injection molding conditions were set as follows: injection and pressure holding time: 5 seconds, cooling time: 5 seconds, mold temperature: 120°C, and cylinder temperature: 350°C.

[0087] Molded products were produced by the above method, and various physical properties were measured and evaluated. The evaluation results are shown in Table 1.

[0088] Examples 2 to 5, Comparative Examples 1 to 5 Polyamide compositions were produced in the same manner as in Example 1, except for the composition shown in Table 1. The evaluation results are shown in Table 1. In Examples 4 to 5 and Comparative Example 2, the extruder temperature setting was changed to 330°C, and in Comparative Example 3, the extruder temperature setting was changed to 250°C.

[0089] Properties and Evaluation First, the pellets of the polyamide compositions obtained in the Examples and Comparative Examples were dried in a nitrogen stream to reduce the moisture content in the polyamide compositions to 500 ppm or less. Next, the pellets of each polyamide composition with the adjusted moisture content were used to measure various physical properties and perform various evaluations using the following methods.

[0090] [Physical Properties 1] The C / N ratio of polyamide was calculated using the following formula. C / N = number of carbon atoms in a monomer unit ÷ number of nitrogen atoms in a monomer unit

[0091] [Physical Property 2] Melting peak temperature of polyamide composition The measurement was performed using Diamond-DSC manufactured by PERKIN-ELMER in accordance with JIS-K 7121. In a nitrogen atmosphere, about 10 mg of the polyamide composition was heated to 280°C or more and 370°C or less according to the melting point (Tm) of the sample at a heating rate of 20°C / min (first heating), and the highest endothermic peak (melting peak) melting peak temperature was determined as Tm1 (°C). The melting peak temperature Tm2 of the polyamide composition was measured as follows. After the first heating, the temperature was kept in a molten state at the highest temperature of the heating for 1 minute, then the temperature was lowered to 30°C at a heating rate of 20°C / min and held at 30°C for 1 minute. After that, the temperature was raised in the same manner at a heating rate of 20°C / min (second heating), and the highest endothermic peak temperature was determined as the melting peak temperature Tm2 of the polyamide composition.

[0092] [Evaluation 1] (Moisture absorption rate: Paintability evaluation) A test plate (60 mm x 60 mm x 3 mm) was molded according to the above molding method, and the obtained test plate was conditioned in accordance with JIS K-7143, and the weight of the test piece was measured. The moisture absorption rate was calculated using the following formula. Moisture absorption rate (%) = (weight of test piece when hydrated - weight of test piece when completely dry) ÷ weight of test piece when completely dry × 100

[0093] Paintability is correlated with the moisture absorption rate of the molded product. If the moisture absorption rate is too low, the surface of the molded product is not sufficiently invaded by the paint, making it difficult for the paint to adhere to the surface. On the other hand, if the moisture absorption rate is too high, the surface of the molded product is too invaded, causing the surface to become rough and the appearance to deteriorate. In the study of this invention, paintability is defined as both the ease of paint application and the appearance, and the closer the moisture absorption rate is to 1.2%, the better the paintability is, and the further away from 1.2%, the worse the paintability is.

[0094] [Evaluation 2] Tensile strength retention rate A multipurpose test piece (Type A) was subjected to a tensile test in the same manner as described above at a tensile speed of 5 mm / min in accordance with ISO 527, and each tensile strength before moisture absorption was measured. In addition, a multipurpose test piece (Type A) was immersed in warm water at 80°C, and when the weight became constant (saturated water absorption), a tensile test was performed in the same manner as described above to measure each tensile strength in a moisture-absorbed state. The tensile strength retention rate when moisture was absorbed was calculated using the following formula. Tensile strength retention rate at water saturation (%) = (tensile strength at water saturation ÷ tensile strength at bone dry) × 100

[0095] [Table 1]

[0096] As can be seen from Table 1, the polyamide composition of this embodiment containing a polyamide and an acid-modified elastomer gave molded articles that were able to achieve both appropriate water absorption and high elastic modulus retention.

[0097] In addition, the polyamide compositions of Examples 1 to 3 containing polyamide 4T / 6T, 4T / 6T / 66 or 6T / 6I had particularly good moisture absorption rates and elastic modulus retention rates. In Example 2, good results were obtained even when the amount of acid-modified polyolefin was increased.

[0098] On the other hand, the polyamide composition of Comparative Example 1, which did not contain the acid-modified elastomer, did not provide a molded article that could achieve both the moisture absorption rate and the elastic modulus retention rate. In addition, when 6 parts of the (B) acid-modified elastomer were added, the elastic modulus retention rate decreased.

[0099] In Example 1, since the moisture absorption rate was within a specific range, the molded product could be painted with an appropriate amount, and a molded product with a smooth surface appearance was obtained. On the other hand, in Comparative Example 5, since the moisture absorption rate was lower than the specific range, a larger amount of paint was required for painting than in Example 1. Furthermore, the paint became uneven on the surface of the molded product.

[0100] From the above, it has become clear that the polyamide composition of the present embodiment can provide a molded article that has good paintability and can retain a high elastic modulus when wet. [Industrial Applicability]

[0101] According to the polyamide composition of the present embodiment, it is possible to provide a polyamide composition that has good paintability and excellent elastic modulus retention rate when molded into a molded article. Therefore, the molded article of the present embodiment is used for humid environment applications such as sporting goods.

Claims

1. Polyamide, An acid-modified elastomer; A polyamide composition comprising: The polyamide comprises dicarboxylic acid units, The content of aromatic dicarboxylic acid units relative to the total molar amount of the dicarboxylic acid units is more than 50 mol %, The C / N ratio of the polymer unit is greater than 6.0 and less than 8.0; In a differential scanning calorimetry measurement according to JIS-K7121, the polyamide composition has a melting peak temperature of 310° C. or higher; A polyamide composition, wherein the amount of the acid-modified elastomer is less than 6% by mass, based on 100% by mass of the polyamide composition.

2. 2. The polyamide composition according to claim 1, wherein the polyamide comprises a diamine unit having 4 to 6 carbon atoms.

3. The polyamide composition of claim 2 , wherein the diamine units comprise tetramethylene diamine units.

4. 2. The polyamide composition of claim 1, wherein said aromatic dicarboxylic acid units are terephthalic acid units.

5. 5. The polyamide composition according to claim 4, wherein the content of the terephthalic acid units relative to the total molar amount of the dicarboxylic acid units is 90 to 100 mol %.

6. 10. The polyamide composition of claim 1, further comprising a filler, said filler being a fibrous filler.

7. 10. The polyamide composition of claim 1 further comprising a filler, said filler being glass fiber or carbon fiber.

8. 10. The polyamide composition of claim 1 further comprising a filler, said filler being carbon fiber.

9. 2. The polyamide composition according to claim 1, wherein the peak melting temperature is 325°C or higher.

10. A molded article obtained by molding the polyamide composition according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Polyamide resin composition

    JP2009215514A

  • JP672065B