Oxidation neutralization treatment method of aqueous nickel chloride solution

By optimizing the nickel concentration and oxidation-reduction potential in the oxidative neutralization process, the method effectively suppresses side reactions, reducing agent consumption and lowering costs while enhancing impurity removal in nickel chloride solutions.

JP2024168413APending Publication Date: 2024-12-05SUMITOMO METAL MINING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023085087
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The high consumption of oxidizing and neutralizing agents in the oxidative neutralization treatment of nickel chloride solutions due to side reactions, leading to increased costs, is a challenge in the nickel hydrometallurgical process.

Method used

The method involves adjusting the nickel concentration of the nickel chloride solution to 121 to 130 g/L and controlling the oxidation-reduction potential to 600 to 1,200 mV, using chlorine gas as the oxidizing agent and nickel carbonate as the neutralizing agent, to suppress side reactions and optimize the oxidative neutralization process.

Benefits of technology

This approach reduces the consumption of oxidizing and neutralizing agents, thereby lowering operational costs and improving the efficiency of impurity removal in the nickel chloride solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168413000001_ABST
    Figure 2024168413000001_ABST
Patent Text Reader

Abstract

To provide an oxidation neutralization treatment method of an aqueous nickel chloride solution, the method enabling reduction of consumption of chlorine gas as an oxidant and reduction of consumption of a neutralizer.SOLUTION: An oxidation neutralization treatment method of an aqueous nickel chloride solution is provided in which chlorine gas as an oxidant is blown into an aqueous nickel chloride solution including impurities, then a neutralizer is added to the solution, and neutralized sediment including impurities is produced by an oxidation neutralization reaction, wherein nickel concentration of aqueous nickel chloride solution is set to be 121 to 130 g / L. Since the nickel concentration of the aqueous nickel chloride solution is 121 g / L or more, a side reaction in which chlorine oxidizes water to thereby produce a hydrochloric acid and oxygen, can be suppressed. As a result, consumption of chlorine gas as an oxidant and a neutralizer can be reduced, and chemical cost can be reduced.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for oxidizing and neutralizing an aqueous solution of nickel chloride, and more particularly to a method for removing impurities contained in an aqueous solution of nickel chloride by an oxidizing and neutralizing method. [Background technology]

[0002] In the nickel hydrometallurgical process, nickel sulfide is leached with chlorine, impurities are removed from the resulting nickel chloride aqueous solution, and electrolytic nickel is recovered by electrowinning. The oxidation neutralization method is known as a method for removing impurities from nickel chloride aqueous solution. For example, Patent Document 1 describes the removal of impurities such as lead contained in nickel chloride aqueous solution by the oxidation neutralization method. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-171972 A Summary of the Invention [Problem to be solved by the invention]

[0004] The oxidation and neutralization treatment of the nickel chloride aqueous solution requires an oxidizing agent and a neutralizing agent, and the cost of these chemicals accounts for the majority of the operation costs. Therefore, from the viewpoint of economy, it is preferable to reduce the consumption of the oxidizing agent and the neutralizing agent.

[0005] In particular, in the oxidation neutralization treatment using chlorine as an oxidizing agent, not only the main reaction of producing a neutralized precipitate occurs, but also the following side reaction of oxidizing water with chlorine to produce hydrochloric acid and oxygen. (Side reactions) Cl 2 +H 2 O → 2HCl + (1 / 2)O 2

[0006] The side reaction consumes the oxidizing agent chlorine, and the hydrochloric acid produced by the side reaction consumes the neutralizing agent. In other words, some of the oxidizing agent and neutralizing agent do not contribute to the production of neutralized precipitate, resulting in a loss of chemicals. Therefore, the side reaction causes an increase in the consumption of the oxidizing agent and neutralizing agent, leading to an increase in chemical costs.

[0007] In view of the above circumstances, an object of the present invention is to provide a method for oxidizing and neutralizing an aqueous nickel chloride solution, which can reduce the consumption of chlorine gas as an oxidizing agent and a neutralizing agent. [Means for solving the problem]

[0008] The oxidation neutralization treatment method for an aqueous nickel chloride solution of the first embodiment is a method in which chlorine gas as an oxidizing agent is blown into an aqueous nickel chloride solution containing impurities, a neutralizing agent is added, and a neutralized precipitate containing the impurities is produced by an oxidation neutralization reaction, and is characterized in that the aqueous nickel chloride solution has a nickel concentration of 121 to 130 g / L. The second embodiment of the method for oxidizing and neutralizing an aqueous nickel chloride solution is the same as the first embodiment, except that the amount of chlorine gas blown per unit amount of the aqueous nickel chloride solution is 0.8 to 2.2 kg / m 3 It is characterized in that: The oxidation / neutralization treatment method for an aqueous nickel chloride solution of a third aspect is characterized in that, in the first or second aspect, the aqueous nickel chloride solution has an oxidation-reduction potential (based on an Ag / AgCl electrode) of 600 to 1,200 mV and a pH of 4 to 6. Effect of the Invention

[0009] According to the present invention, since the nickel concentration of the nickel chloride aqueous solution is 121 g / L or more, the side reaction in which chlorine oxidizes water to generate hydrochloric acid and oxygen can be suppressed. As a result, the consumption of chlorine gas as an oxidizing agent and a neutralizing agent can be reduced, and the cost of chemicals can be reduced. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is an overall flow diagram of a nickel hydrometallurgical process. [Diagram 2] FIG. 2 is a detailed process diagram of the lead removal process. [Diagram 3] FIG. [Figure 4] 1 is a graph showing the relationship between the nickel concentration in an aqueous crude nickel chloride solution and the amount of oxygen generated. [Diagram 5] 1 is a graph showing the relationship between the amount of chlorine and the amount of oxygen generated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Next, an embodiment of the present invention will be described with reference to the drawings. The oxidation neutralization treatment method according to one embodiment of the present invention is a method for removing impurities contained in an aqueous nickel chloride solution by an oxidation neutralization method. Impurities contained in an aqueous nickel chloride solution include iron, lead, manganese, and cobalt. The aqueous nickel chloride solution is subjected to an oxidation neutralization treatment to remove the impurities. However, impurities that cannot be completely removed may remain in the aqueous nickel chloride solution after the treatment.

[0012] The oxidation neutralization method of the present embodiment is preferably applied to the de-iron step and the de-leading step, particularly the de-leading step, of the nickel hydrometallurgical process described below. Therefore, the de-leading step will be described below as an example. However, the oxidation neutralization method of the present embodiment is not limited to the de-leading step, and may be applied to any process step.

[0013] As shown in Figure 1, in the nickel hydrometallurgy process, the raw material nickel sulfide is first treated in the leaching process to obtain leachate. Nickel matte and nickel-cobalt mixed sulfide can be used as nickel sulfide.

[0014] The leaching process includes a chlorine leaching process and a cementation process. In the chlorine leaching process, the metals contained in the solid matter in the raw slurry are substantially all leached into the liquid by the oxidizing power of the chlorine gas blown into the leaching tank. In the cementation process, the chlorine leaching solution is brought into contact with nickel sulfide, preferably nickel matte, to carry out a substitution reaction between copper and nickel. As a result, for example, nickel in the nickel matte is leached into the liquid, and copper ions in the liquid are precipitated in the form of copper sulfide or metallic copper. The leaching solution obtained in the leaching process is mainly composed of an aqueous nickel chloride solution, and contains impurities such as copper, iron, and lead in addition to cobalt.

[0015] In the iron removal process, impurities such as iron and arsenic are removed from the leachate (nickel chloride aqueous solution) by oxidation neutralization. In the iron removal process, an oxidizing agent is applied to the leachate to adjust the oxidation-reduction potential (based on Ag / AgCl electrode, the same applies below) to 400-1,100 mV, while a neutralizing agent is added to adjust the pH to 1.5-3. Chlorine gas, for example, is used as the oxidizing agent. Nickel carbonate, for example, is used as the neutralizing agent. Impurities such as iron and arsenic contained in the leachate are precipitated as hydroxides or oxides by the oxidation neutralization reaction. The precipitate is removed by solid-liquid separation to obtain a deironized final solution from which impurities have been removed.

[0016] In the solvent extraction step, the cobalt contained in the iron-removal final solution is separated by solvent extraction to obtain an aqueous nickel chloride solution and an aqueous cobalt chloride solution. Hereinafter, for the sake of convenience, the aqueous nickel chloride solution and the aqueous cobalt chloride solution obtained in the solvent extraction step are referred to as an aqueous crude nickel chloride solution and an aqueous crude cobalt chloride solution, respectively. The nickel concentration in the aqueous crude nickel chloride solution is 160 to 200 g / L. The aqueous crude nickel chloride solution contains impurities such as lead, manganese, cobalt, and zinc. The cobalt contained in the aqueous crude nickel chloride solution is extracted into an organic solvent and selectively separated from the nickel chloride in the aqueous crude nickel chloride solution, but a very small amount of cobalt still remains in the extraction residue (aqueous crude nickel chloride solution).

[0017] The crude cobalt chloride aqueous solution is purified in a purification process to remove impurities, and the resulting high-purity cobalt chloride aqueous solution is sent to the cobalt electrolysis process, where electrolytic cobalt is produced by electrowinning.

[0018] The crude nickel chloride aqueous solution is subjected to a deleading process to remove impurities, resulting in a high-purity nickel chloride aqueous solution. The deleading process will be described in detail later. After the deleading process, other solution purification treatments may be performed as necessary. For example, trace amounts of zinc remaining in the nickel chloride aqueous solution may be removed by adsorbing them onto an anion exchange resin. The high-purity nickel chloride aqueous solution is sent to a nickel electrolysis process. In the nickel electrolysis process, electrolytic nickel is produced by electrowinning.

[0019] As shown in Fig. 2, the deleading process has three sub-processes: a dilution process, an oxidation / neutralization process, and a solid-liquid separation process. In the following description, the term "crude nickel chloride aqueous solution" is used to mean not only the starting liquid of the deleading process, but also the water to be treated in the dilution process and the oxidation / neutralization process.

[0020] In the dilution step, a diluent is added to the crude nickel chloride aqueous solution to dilute it, thereby decreasing the nickel concentration. Nickel electrolysis waste liquid is preferably used as the diluent. Nickel electrolysis waste liquid is obtained as waste liquid after using a high-purity nickel chloride aqueous solution as an electrolyte in the nickel electrolysis step. By using nickel electrolysis waste liquid as a diluent, it is possible to prevent the total amount of liquid in the system of the hydrometallurgical process from increasing. Industrial water may be used as the diluent instead of nickel electrolysis waste liquid. If industrial water is used, the crude nickel chloride aqueous solution can be diluted to the desired nickel concentration with a smaller amount of liquid than if nickel electrolysis waste liquid is used.

[0021] The diluted crude nickel chloride aqueous solution is sent to the oxidation neutralization step. In the oxidation neutralization step, an oxidizing agent is applied to the crude nickel chloride aqueous solution to adjust the redox potential to 600 to 1,200 mV, while a neutralizing agent is added to adjust the pH to 4 to 6. Impurities such as lead, manganese, and cobalt contained in the crude nickel chloride aqueous solution are coprecipitated with nickel precipitate by the oxidation neutralization reaction. Hereinafter, the nickel precipitate containing impurities is referred to as neutralized precipitate.

[0022] Chlorine gas is used as the oxidizing agent. Nickel carbonate, sodium carbonate, calcium carbonate, nickel hydroxide, sodium hydroxide, calcium hydroxide, etc. can be used as the neutralizing agent. Among these, nickel carbonate and nickel hydroxide are preferred because they do not increase the impurities in the nickel chloride aqueous solution.

[0023] The slurry containing the neutralized precipitate is separated into a high-purity nickel chloride aqueous solution and the neutralized precipitate in the solid-liquid separation process. The main components of the neutralized precipitate are nickel hydroxide and oxide. Therefore, the neutralized precipitate is used as a raw material for nickel sulfate.

[0024] In the oxidation neutralization step, a reaction tank shown in FIG. 3 is used. A crude nickel chloride aqueous solution is continuously supplied to the reaction tank. The flow rate of the crude nickel chloride aqueous solution is, for example, 2,200 to 3,000 L / min. An oxidizing agent (chlorine gas) and a neutralizing agent are continuously supplied to the reaction tank. Chlorine gas is blown as an oxidizing agent into the crude nickel chloride aqueous solution in the reaction tank, and a neutralizing agent is added to generate a neutralized precipitate by an oxidation neutralization reaction. The reaction tank is equipped with an agitator for stirring the crude nickel chloride aqueous solution, the oxidizing agent (chlorine gas), and the neutralizing agent. A slurry containing the neutralized precipitate is continuously discharged from the reaction tank.

[0025] In addition, a plurality of reaction tanks may be connected in series to carry out the oxidation neutralization treatment stepwise. In this case, the crude nickel chloride aqueous solution is continuously supplied to the most upstream reaction tank and flows in sequence to the downstream reaction tanks. The dilution step may be carried out in a concentration adjustment tank, or the dilution step and the oxidation neutralization step may be carried out in the same reaction tank. In the latter case, both the crude nickel chloride aqueous solution before dilution and the diluent may be supplied to the reaction tank. In this case, the dilution rate of the crude nickel chloride aqueous solution may be adjusted using the nickel concentration of the crude nickel chloride aqueous solution in the slurry continuously discharged from the reaction tank, or the nickel concentration of the crude nickel chloride aqueous solution before dilution and the nickel concentration of the diluent as an index.

[0026] Chlorine gas supplied as an oxidant is absorbed into the crude nickel chloride aqueous solution, and almost the entire amount contributes to the oxidation neutralization reaction. Nevertheless, to prevent chlorine gas, which is a toxic gas, from leaking outside the reaction tank, a circulating collection pipe is connected to the gas phase of the reaction tank, and the inside of the reaction tank is kept at negative pressure by an induced draft fan. The gas drawn by the induced draft fan (hereinafter referred to as "circulating collection gas") is sent to the detoxification tower through the circulating collection pipe. The circulating collection gas includes the gas generated in the reaction tank as well as the atmosphere (free air) that flows in through the gaps in the reaction tank.

[0027] When chlorine gas is blown into an aqueous solution of crude nickel chloride as an oxidizing agent and basic nickel carbonate is added as a neutralizing agent, nickel precipitate is produced by the following main reaction: At the same time, impurities such as lead and manganese contained in the aqueous solution of crude nickel chloride are precipitated as hydroxides or oxides. (Main reaction) 3NiCl 2 +Cl 2 +(4 / 3)Ni 3 (CO 3 )(OH) 4 4H 2 O →Ni 3 O 2 (OH) 4 +4NiCl 2 +(4 / 3)CO 2 +6H 2 O

[0028] When a carbonate such as nickel carbonate, sodium carbonate, or calcium carbonate is used as a neutralizing agent, carbon dioxide is generated, which is discharged as reflux gas.

[0029] In addition to the main reaction, the oxidation neutralization treatment using chlorine as an oxidizing agent may also cause the following side reaction in which chlorine oxidizes water to generate hydrochloric acid and oxygen. The oxygen generated by the side reaction is discharged as reflux gas. (Side reactions) Cl 2 +H 2 O → 2HCl + (1 / 2)O 2

[0030] The side reaction consumes the oxidizing agent chlorine, and the hydrochloric acid produced by the side reaction consumes the neutralizing agent. In other words, some of the oxidizing agent and neutralizing agent do not contribute to the production of neutralized precipitate, resulting in a loss of chemicals. Therefore, the side reaction causes an increase in the consumption of the oxidizing agent and neutralizing agent, leading to an increase in chemical costs.

[0031] Therefore, it is considered to select operating conditions that suppress the side reactions and reduce the consumption of the oxidizing agent and neutralizing agent. In this regard, the inventors of the present application have found that the higher the nickel concentration in the aqueous solution of crude nickel chloride, the more the side reactions are suppressed. Specifically, if the nickel concentration of the aqueous solution of crude nickel chloride in the reaction tank is set to 121 g / L or more, the side reactions can be sufficiently suppressed. As a result, the consumption of the oxidizing agent and neutralizing agent can be reduced, and the chemical costs can be reduced.

[0032] From the viewpoint of suppressing side reactions, there is no upper limit to the nickel concentration of the crude nickel chloride aqueous solution. However, the nickel concentration of the crude nickel chloride aqueous solution is preferably 130 g / L or less. If the nickel concentration of the crude nickel chloride aqueous solution is 130 g / L or less, the chloride ion concentration is low, so that the chloro complex becomes unstable, and impurities, especially cobalt, tend to precipitate in the oxidation neutralization step. In addition, if the nickel concentration of the crude nickel chloride aqueous solution is 130 g / L or less, the nucleus growth of the precipitate particles is promoted, and the particle size becomes large, thereby improving the filterability in the solid-liquid separation step. EXAMPLES

[0033] Next, an embodiment will be described. The nickel hydrometallurgical smelting process shown in Figure 1 was carried out. In the deleading process shown in Figure 2, impurities contained in the crude nickel chloride aqueous solution were removed by the oxidation neutralization method. In the oxidation neutralization process, three reaction tanks connected in series were used, and the oxidation neutralization treatment was carried out in stages. Chlorine gas was used as the oxidizing agent, and basic nickel carbonate was used as the neutralizing agent.

[0034] In order to monitor the extent to which the above-mentioned side reactions were occurring, the amount of oxygen generated by the side reactions was determined using the following method. First, the oxygen and carbon dioxide concentrations in the collected gas from the reaction tank were measured using a gas analyzer. The nitrogen concentration was calculated by subtracting the oxygen and carbon dioxide concentrations from 100%. It is known that the components of the atmosphere are 78.1% nitrogen, 20.9% oxygen, 0.9% argon, and 0.1% other trace components. Therefore, the value obtained by subtracting the oxygen and carbon dioxide concentrations from 100% is, precisely, the total concentration of nitrogen, argon, and other trace components (excluding carbon dioxide).

[0035] Next, the calculated nitrogen concentration (including argon, etc.) is multiplied by the ratio of nitrogen (including argon, etc.) to oxygen in the atmosphere, 0.264 (=20.9% / 79.1%) to calculate the oxygen concentration originating from the atmosphere (hereinafter referred to as "atmospheric oxygen concentration"). Since no nitrogen is generated in the reaction tank, all of the nitrogen contained in the collected gas is from the atmosphere. Therefore, the atmospheric oxygen concentration can be obtained by multiplying the nitrogen concentration in the collected gas by the ratio of nitrogen to oxygen in the atmosphere.

[0036] Next, the oxygen concentration derived from the reaction (hereinafter referred to as "generated oxygen concentration") is calculated by subtracting the atmospheric oxygen concentration from the oxygen concentration in the collected gas. The amount of generated oxygen is then calculated by multiplying the generated oxygen concentration by the mass (flow rate) of the collected gas.

[0037] The amount of oxygen generated is the amount of oxygen generated by a side reaction. Therefore, the amount of oxygen generated is an index of the extent to which a side reaction is occurring. In other words, the amount of side reaction occurring can be monitored based on the amount of oxygen generated.

[0038] FIG. 4 shows the relationship between the nickel concentration in the crude nickel chloride aqueous solution and the amount of oxygen generated. The horizontal axis of the graph in FIG. 4 is the nickel concentration in the crude nickel chloride aqueous solution after dilution. The vertical axis is the amount of oxygen generated as determined by the method described above. As can be seen from the graph in FIG. 4, the higher the nickel concentration in the crude nickel chloride aqueous solution, the lower the amount of oxygen generated. It is known that the higher the nickel chloride concentration of the aqueous solution, the lower the water activity. It is presumed that when the nickel concentration of the crude nickel chloride aqueous solution is high, the water activity decreases and the equilibrium potential of the water oxidation reaction increases, suppressing the oxidation of water, i.e., the side reaction.

[0039] If the nickel concentration of the crude nickel chloride aqueous solution is 121 g / L or more, the amount of oxygen generated will be 16 kg / h or less, and side reactions can be sufficiently suppressed. As a result, the consumption of oxidizing agents and neutralizing agents can be reduced, and chemical costs can be reduced.

[0040] FIG. 5 shows the relationship between the amount of chlorine and the amount of oxygen generated. The horizontal axis of the graph in FIG. 5 is the amount of chlorine gas blown per unit amount of the aqueous nickel chloride solution (hereinafter referred to as the "amount of chlorine"), which is the value obtained by dividing the flow rate of chlorine gas into the reaction tank by the flow rate of the aqueous crude nickel chloride solution into the reaction tank. The vertical axis is the amount of oxygen generated calculated by the method described above. As can be seen from the graph in FIG. 5, when the nickel concentration of the aqueous crude nickel chloride solution is low, particularly when it is 111 g / L or less, the amount of oxygen generated changes depending on the amount of chlorine. On the other hand, when the nickel concentration of the aqueous crude nickel chloride solution is 121 g / L or more, the amount of oxygen generated is almost constant regardless of whether the amount of chlorine increases or decreases.

[0041] The amount of chlorine is adjusted so that the oxidation-reduction potential of the crude nickel chloride aqueous solution becomes a value suitable for the oxidation neutralization treatment. When the nickel concentration of the crude nickel chloride aqueous solution is low, the amount of oxygen generated increases or decreases depending on the amount of chlorine adjusted using the oxidation-reduction potential as an index. On the other hand, when the nickel concentration of the crude nickel chloride aqueous solution is 121 g / L or more, even if the amount of chlorine is adjusted using the oxidation-reduction potential as an index, the effect on the amount of oxygen generated is small, and the amount of oxygen generated can be constantly suppressed. From the graph of FIG. 5, it can be seen that at least the amount of chlorine is 0.8 to 2.2 kg / m 3 From this viewpoint, it is preferable that the nickel concentration of the aqueous solution of crude nickel chloride is 121 g / L or more.

Claims

1. A method for producing a neutralized precipitate containing impurities by an oxidation-neutralization reaction, comprising blowing chlorine gas as an oxidizing agent into an aqueous nickel chloride solution containing impurities, and adding a neutralizing agent to the aqueous nickel chloride solution, the method comprising the steps of: The nickel concentration of the aqueous nickel chloride solution is 121 to 130 g / L.

2. A method for oxidizing and neutralizing an aqueous nickel chloride solution.

2. The amount of chlorine gas blown per unit amount of the nickel chloride aqueous solution is 0.8 to 2.2 kg / m 3 is 2. The method for oxidizing and neutralizing an aqueous nickel chloride solution according to claim 1.

3. The nickel chloride aqueous solution has an oxidation-reduction potential (based on an Ag / AgCl electrode) of 600 to 1,200 mV and a pH of 4 to 6.

3. The method for oxidizing and neutralizing an aqueous nickel chloride solution according to claim 1 or 2.

Citation Information

Patent Citations

  • Method for removing lead in chloride solution

    JP1994306503A

  • Method for removing lead from nickel solution

    JP1996295965A

  • Method for controlling oxidization and neutralization of aqueous nickel chloride solution

    JP2010168258A

  • Method of oxidative neutralizing treatment of aqueous nickel chloride solution

    JP2014062303A

  • Purification method of nickel chloride solution

    JP2015209551A