Oxidation neutralization treatment method of aqueous nickel chloride solution
By using chlorine gas and nickel carbonate in the oxidative neutralization of nickel chloride solutions with controlled conditions, the method addresses the high cost issue of neutralizing agents, achieving efficient and cost-effective impurity removal in the hydrometallurgical process.
Patent Information
- Application Number
- JP2023085088
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
The high cost of oxidizing and neutralizing agents, particularly nickel carbonate, in the oxidative neutralization treatment of nickel chloride solutions in the hydrometallurgical process is a significant economic burden, as purchased sodium carbonate is often used, leading to increased consumption and operational costs.
The method employs chlorine gas as an oxidizing agent and nickel carbonate as a neutralizing agent, with controlled amounts of chlorine gas (1.5 kg/(m³·h) and adjusted redox potential (600 to 1,200 mV) to optimize the oxidative neutralization process, reducing the consumption of neutralizing agents.
This approach enhances the reaction efficiency of the neutralizing agent to 85% or more, thereby reducing the amount of neutralizing agent required and lowering operational costs.
Smart Images

Figure 2024168414000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for oxidizing and neutralizing an aqueous solution of nickel chloride, and more particularly to a method for removing impurities contained in an aqueous solution of nickel chloride by an oxidizing and neutralizing method. [Background technology]
[0002] In the nickel hydrometallurgical process, nickel sulfide is leached with chlorine, impurities are removed from the resulting nickel chloride aqueous solution, and electrolytic nickel is recovered by electrowinning. The oxidation neutralization method is known as a method for removing impurities from nickel chloride aqueous solution. For example, Patent Document 1 describes the removal of impurities such as lead contained in nickel chloride aqueous solution by the oxidation neutralization method. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-171972 A Summary of the Invention [Problem to be solved by the invention]
[0004] The oxidation neutralization treatment of the nickel chloride aqueous solution requires an oxidizing agent and a neutralizing agent, and the cost of these chemicals accounts for the majority of the operation cost. In particular, when nickel carbonate is used as a neutralizing agent in the oxidation neutralization treatment performed in the nickel hydrometallurgical process, nickel carbonate is produced using purchased sodium carbonate as a carbonating agent, so the more nickel carbonate is consumed, the higher the chemical cost. Therefore, from the viewpoint of economy, it is preferable to reduce the consumption of the neutralizing agent.
[0005] In view of the above circumstances, an object of the present invention is to provide a method for oxidizing and neutralizing an aqueous nickel chloride solution using chlorine gas as an oxidizing agent in order to reduce the consumption of a neutralizing agent. [Means for solving the problem]
[0006] The first aspect of the oxidation neutralization treatment method for an aqueous nickel chloride solution is a method for producing a neutralized precipitate containing impurities by an oxidation neutralization reaction by blowing chlorine gas as an oxidizing agent into an aqueous nickel chloride solution containing impurities in a reaction vessel and adding a neutralizing agent, and the amount of chlorine gas blown per unit volume of the aqueous nickel chloride solution in the reaction vessel is 1.5 kg / (m 3 h) is characterized in that: The oxidation / neutralization treatment method for an aqueous nickel chloride solution of the second aspect is the method of the first aspect, characterized in that the aqueous nickel chloride solution has an oxidation-reduction potential (Ag / AgCl electrode standard) of 600 to 1,200 mV. The oxidation neutralization treatment method for an aqueous nickel chloride solution of a third aspect is characterized in that in the first or second aspect, the neutralizing agent is nickel carbonate. The oxidation neutralization treatment method for an aqueous nickel chloride solution of a fourth aspect is characterized in that in any one of the first to third aspects, the aqueous nickel chloride solution has a nickel concentration of 90 to 130 g / L. A fifth aspect of the method for oxidizing and neutralizing an aqueous nickel chloride solution is a method for oxidizing and neutralizing an aqueous nickel chloride solution, comprising the steps of: continuously supplying the aqueous nickel chloride solution to a plurality of reaction tanks connected in series; and blowing an amount of the chlorine gas per unit volume of the aqueous nickel chloride solution in the most upstream reaction tank among the plurality of reaction tanks of 1.5 kg / (m 3 h) is characterized in that: Effect of the Invention
[0007] According to the present invention, the amount of chlorine is 1.5 kg / (m 3 By keeping the reaction efficiency of the neutralizing agent at or below 1.0 h, the reaction efficiency of the neutralizing agent can be increased and the amount of the neutralizing agent consumed can be reduced. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is an overall flow diagram of a nickel hydrometallurgical process. [Diagram 2] FIG. 2 is a detailed process diagram of the lead removal process. [Diagram 3] FIG. [Figure 4] 1 is a graph showing the relationship between the amount of chlorine and the neutralizing agent reaction efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Next, an embodiment of the present invention will be described with reference to the drawings. The oxidation neutralization treatment method according to one embodiment of the present invention is a method for removing impurities contained in an aqueous nickel chloride solution by an oxidation neutralization method. Impurities contained in an aqueous nickel chloride solution include iron, lead, manganese, and cobalt. The aqueous nickel chloride solution is subjected to an oxidation neutralization treatment to remove the impurities. However, impurities that cannot be completely removed may remain in the aqueous nickel chloride solution after the treatment.
[0010] The oxidation neutralization method of the present embodiment is preferably applied to the de-iron step and the de-leading step, particularly the de-leading step, of the nickel hydrometallurgical process described below. Therefore, the de-leading step will be described below as an example. However, the oxidation neutralization method of the present embodiment is not limited to the de-leading step, and may be applied to any process step.
[0011] As shown in Figure 1, in the nickel hydrometallurgical process, the raw material nickel sulfide is first treated in the leaching process to obtain leachate. Nickel matte and nickel-cobalt mixed sulfide can be used as nickel sulfide.
[0012] The leaching process includes a chlorine leaching process and a cementation process. In the chlorine leaching process, the metals contained in the solid matter in the raw slurry are substantially all leached into the liquid by the oxidizing power of the chlorine gas blown into the leaching tank. In the cementation process, the chlorine leaching solution is brought into contact with nickel sulfide, preferably nickel matte, to carry out a substitution reaction between copper and nickel. As a result, for example, nickel in the nickel matte is leached into the liquid, and copper ions in the liquid are precipitated in the form of copper sulfide or metallic copper. The leaching solution obtained in the leaching process is mainly composed of an aqueous nickel chloride solution, and contains impurities such as copper, iron, and lead in addition to cobalt.
[0013] In the iron removal process, impurities such as iron and arsenic are removed from the leachate (nickel chloride aqueous solution) by oxidation neutralization. In the iron removal process, an oxidizing agent is applied to the leachate to adjust the oxidation-reduction potential (based on Ag / AgCl electrode, the same applies below) to 400-1,100 mV, while a neutralizing agent is added to adjust the pH to 1.5-3. Chlorine gas, for example, is used as the oxidizing agent. Nickel carbonate, for example, is used as the neutralizing agent. Impurities such as iron and arsenic contained in the leachate are precipitated as hydroxides or oxides by the oxidation neutralization reaction. The precipitate is removed by solid-liquid separation to obtain a deironized final solution from which impurities have been removed.
[0014] In the solvent extraction step, the cobalt contained in the iron-removal final solution is separated by solvent extraction to obtain an aqueous nickel chloride solution and an aqueous cobalt chloride solution. Hereinafter, for the sake of convenience, the aqueous nickel chloride solution and the aqueous cobalt chloride solution obtained in the solvent extraction step are referred to as an aqueous crude nickel chloride solution and an aqueous crude cobalt chloride solution, respectively. The nickel concentration in the aqueous crude nickel chloride solution is 160 to 200 g / L. The aqueous crude nickel chloride solution contains impurities such as lead, manganese, cobalt, and zinc. The cobalt contained in the aqueous crude nickel chloride solution is extracted into an organic solvent and selectively separated from the nickel chloride in the aqueous crude nickel chloride solution, but a very small amount of cobalt still remains in the extraction residue (aqueous crude nickel chloride solution).
[0015] The crude cobalt chloride aqueous solution is purified in a purification process to remove impurities, and the resulting high-purity cobalt chloride aqueous solution is sent to the cobalt electrolysis process, where electrolytic cobalt is produced by electrowinning.
[0016] The crude nickel chloride aqueous solution is subjected to a deleading process to remove impurities, resulting in a high-purity nickel chloride aqueous solution. The deleading process will be described in detail later. After the deleading process, other solution purification treatments may be performed as necessary. For example, trace amounts of zinc remaining in the nickel chloride aqueous solution may be removed by adsorbing them onto an anion exchange resin. The high-purity nickel chloride aqueous solution is sent to a nickel electrolysis process. In the nickel electrolysis process, electrolytic nickel is produced by electrowinning.
[0017] As shown in Fig. 2, the deleading process has three sub-processes: a dilution process, an oxidation / neutralization process, and a solid-liquid separation process. In the following description, the term "crude nickel chloride aqueous solution" is used to mean not only the starting liquid of the deleading process, but also the water to be treated in the dilution process and the oxidation / neutralization process.
[0018] In the dilution step, the crude nickel chloride aqueous solution is diluted with a diluent to reduce the nickel concentration. For example, the crude nickel chloride aqueous solution (nickel concentration 160 to 200 g / L) obtained in the solvent extraction step is diluted so that the nickel concentration becomes 90 to 130 g / L. Since the main component of the crude nickel chloride aqueous solution is nickel chloride, the nickel concentration can be used as an index showing the chloride ion concentration of the crude nickel chloride aqueous solution.
[0019] If the nickel concentration of the crude nickel chloride aqueous solution is 130g / L or less, the chloride ion concentration is low, which makes the chloro complex unstable and makes it easier for impurities, especially cobalt, to precipitate in the oxidation neutralization process. Also, if the nickel concentration of the crude nickel chloride aqueous solution is 130g / L or less, the nucleus growth of the precipitate particles is promoted and the particle size increases, improving the filterability in the solid-liquid separation process. If the nickel concentration of the crude nickel chloride aqueous solution is 90g / L or more, the amount of diluent added can be reduced and a significant increase in the volume of the crude nickel chloride aqueous solution can be suppressed, making it unnecessary to increase the facility capacity.
[0020] It is preferable to use nickel electrolysis waste liquid as the diluent. Nickel electrolysis waste liquid is obtained as waste liquid after using a high-purity nickel chloride aqueous solution as an electrolyte in the nickel electrolysis process. By using nickel electrolysis waste liquid as a diluent, it is possible to prevent an increase in the total amount of liquid in the system of the hydrometallurgical process. Industrial water may be used as the diluent instead of nickel electrolysis waste liquid. If industrial water is used, the crude nickel chloride aqueous solution can be diluted to the target nickel concentration with a smaller amount of liquid than if nickel electrolysis waste liquid is used.
[0021] The diluted crude nickel chloride aqueous solution is sent to the oxidation neutralization step. In the oxidation neutralization step, an oxidizing agent is applied to the crude nickel chloride aqueous solution to adjust the redox potential to 600 to 1,200 mV, while a neutralizing agent is added to adjust the pH to 4 to 6. Impurities such as lead, manganese, and cobalt contained in the crude nickel chloride aqueous solution are coprecipitated with nickel precipitate by the oxidation neutralization reaction. Hereinafter, the nickel precipitate containing impurities is referred to as neutralized precipitate.
[0022] Chlorine gas is used as the oxidizing agent. Nickel carbonate, sodium carbonate, calcium carbonate, nickel hydroxide, sodium hydroxide, calcium hydroxide, etc. can be used as the neutralizing agent. Among these, nickel carbonate and nickel hydroxide are preferred because they do not increase the impurities in the nickel chloride aqueous solution.
[0023] The slurry containing the neutralized precipitate is separated into a high-purity nickel chloride aqueous solution and the neutralized precipitate in the solid-liquid separation process. The main components of the neutralized precipitate are nickel hydroxide and oxide. Therefore, the neutralized precipitate is used as a raw material for nickel sulfate.
[0024] In the oxidation neutralization step, a reaction tank shown in FIG. 3 is used. A crude nickel chloride aqueous solution is continuously supplied to the reaction tank. The flow rate of the crude nickel chloride aqueous solution is, for example, 2,200 to 3,000 L / min. An oxidizing agent (chlorine gas) and a neutralizing agent are continuously supplied to the reaction tank. Chlorine gas is blown as an oxidizing agent into the crude nickel chloride aqueous solution in the reaction tank, and a neutralizing agent is added to generate a neutralized precipitate by an oxidation neutralization reaction. The reaction tank is equipped with an agitator for stirring the crude nickel chloride aqueous solution, the oxidizing agent (chlorine gas), and the neutralizing agent. A slurry containing the neutralized precipitate is continuously discharged from the reaction tank.
[0025] In addition, a plurality of reaction tanks may be connected in series to carry out the oxidation neutralization treatment stepwise. In this case, the crude nickel chloride aqueous solution is continuously supplied to the most upstream reaction tank and flows in sequence to the downstream reaction tanks. The dilution step may be carried out in a concentration adjustment tank, or the dilution step and the oxidation neutralization step may be carried out in the same reaction tank. In the latter case, both the crude nickel chloride aqueous solution before dilution and the diluent may be supplied to the reaction tank. In this case, the dilution rate of the crude nickel chloride aqueous solution may be adjusted using the nickel concentration of the crude nickel chloride aqueous solution in the slurry continuously discharged from the reaction tank, or the nickel concentration of the crude nickel chloride aqueous solution before dilution and the nickel concentration of the diluent as an index.
[0026] When chlorine gas is blown into an aqueous solution of crude nickel chloride as an oxidizing agent and basic nickel carbonate is added as a neutralizing agent, nickel precipitate is produced by the following main reaction: At the same time, impurities such as lead and manganese contained in the aqueous solution of crude nickel chloride are precipitated as hydroxides or oxides. (Main reaction) 3NiCl2+Cl2+(4 / 3)Ni3(CO3)(OH)4·4H2O →Ni3O2(OH)4+4NiCl2+(4 / 3)CO2+6H2O
[0027] The inventors of the present application have found that in such an oxidation neutralization treatment, the reaction efficiency of the neutralizing agent can be increased by reducing the amount of chlorine gas blown into the reaction tank. Specifically, the amount of chlorine gas blown into the reaction tank per unit volume of the aqueous solution of crude nickel chloride (hereinafter referred to as the "chlorine amount") is reduced to 1.5 kg / (m 3 ·h), the reaction efficiency of the neutralizing agent can be sufficiently increased. As a result, the consumption of the neutralizing agent can be reduced. The amount of chlorine is determined by dividing the amount of chlorine gas blown into the reaction tank (kg / h) by the volume of the crude nickel chloride aqueous solution in the reaction tank (m 3 ) is the value divided by
[0028] In particular, when nickel carbonate is used as a neutralizing agent, the amount of chlorine is 1.5 kg / (m 3 By keeping the reaction efficiency of the neutralizer at 85% or more, the reaction efficiency of the neutralizer can be increased to 85% or more. Here, the reaction efficiency of the neutralizer is a value calculated by the following formula, assuming the above-mentioned main reaction. Reaction efficiency of neutralizing agent = (theoretical amount of neutralizing agent required for the production of nickel hydroxide in the neutralized precipitate) ÷ (actual amount of neutralizing agent consumed) × 100%
[0029] The reason why the reaction efficiency of the neutralizing agent increases when the amount of chlorine is reduced is presumed to be as follows: In the oxidation neutralization treatment using chlorine as an oxidizing agent, in addition to the above-mentioned main reaction, the following side reaction may occur in which chlorine oxidizes water to generate hydrochloric acid and oxygen. (Side reactions) Cl2+H2O→2HCl+(1 / 2)O2
[0030] It is believed that if the amount of chlorine is large, the area of high chlorine concentration in the aqueous solution of crude nickel chloride increases, making side reactions more likely to occur. If a side reaction occurs, the generated hydrochloric acid consumes the neutralizing agent, so that part of the neutralizing agent does not contribute to the production of neutralized precipitate, and the reaction efficiency of the neutralizing agent decreases. Conversely, if the amount of chlorine is small, it is believed that side reactions are suppressed and the reaction efficiency of the neutralizing agent increases.
[0031] In a continuous reactor, rather than a batch reactor, multiple reaction tanks may be connected in series to carry out the oxidation neutralization treatment in stages. By carrying out the oxidation neutralization treatment in stages, the efficiency of the oxidation neutralization treatment can be improved and the impurity concentration of the treated liquid can be reduced. For example, the lead concentration of the high-purity nickel chloride aqueous solution obtained in the lead removal process can be reduced. In such an apparatus with multiple reaction tanks connected in series, the amount of chlorine in the most upstream reaction tank (first tank) must be at least 1.5 kg / (m 3 h) The following should suffice.
[0032] In a system in which multiple reaction tanks are connected in series, the majority of the oxidation and neutralization reaction basically takes place in the first tank. In other words, the amount of chlorine in the first tank is determined by the amount of impurities such as lead and cobalt, so the first tank is operated with a larger amount of chlorine than the other tanks. Therefore, the amount of chlorine in the first tank must be at least 1.5 kg / (m 3 If the above ratio is less than or equal to h), the generation of hydrochloric acid due to a side reaction can be effectively suppressed, and the consumption of the neutralizing agent can be reduced.
[0033] Also, from the viewpoint of maintaining good filterability of the generated neutralized sediment, the pH of the first tank is set to the highest, and the pH of the second tank and thereafter is gradually lowered, and no neutralizing agent is added to the most downstream reaction tank (final tank). In this case, since hydrochloric acid is likely to be generated in the first tank, which has the highest pH, it is particularly effective to limit the amount of chlorine in the first tank. On the other hand, in order to lower the pH of the second tank and thereafter, it is rather advantageous for hydrochloric acid to be generated. Therefore, it is not necessary to limit the amount of chlorine in the second tank and thereafter.
[0034] From the viewpoint of increasing the reaction efficiency of the neutralizing agent, there is no lower limit to the amount of chlorine. However, the amount of chlorine affects the redox potential of the crude nickel chloride aqueous solution. It is preferable to adjust the amount of chlorine so that the redox potential of the crude nickel chloride aqueous solution is in a range suitable for the oxidation neutralization treatment, 600 to 1,200 mV in the deleading step. EXAMPLES
[0035] Next, an embodiment will be described. The nickel hydrometallurgical smelting process shown in Figure 1 was operated. In the deleading process shown in Figure 2, impurities contained in the crude nickel chloride aqueous solution were removed by the oxidation neutralization method. In the oxidation neutralization process, three reaction tanks connected in series were used. Each reaction tank had a capacity of 50 m 3 The nickel concentration of the aqueous solution of crude nickel chloride supplied to the first tank is 90-130g / L. An oxidizing agent and a neutralizing agent were added to the first and second tanks. Only an oxidizing agent was added to the third tank. Chlorine gas was used as the oxidizing agent, and basic nickel carbonate was used as the neutralizing agent. The pH of the aqueous solution of crude nickel chloride in the first tank is 4.9-5.2. The pH of the aqueous solution of crude nickel chloride in the second tank is 4.7-4.9. The temperature of the aqueous solution of crude nickel chloride in all tanks is 50-60°C.
[0036] Figure 4 shows the relationship between the amount of chlorine in the first tank and the reaction efficiency of the neutralizing agent. The horizontal axis of the graph in Figure 4 is the amount of chlorine (the amount of chlorine gas blown into the first tank divided by the volume of the crude nickel chloride aqueous solution in the first tank), and the vertical axis is the reaction efficiency of the neutralizing agent in the entire deleading process. As can be seen from the graph in Figure 4, the lower the amount of chlorine, the higher the reaction efficiency of the neutralizing agent.
[0037] Chlorine content: 1.5kg / (m 3 If the reaction efficiency of the neutralizing agent is 85% or more, the consumption of the neutralizing agent can be reduced, and the chemical cost can be suppressed.
Claims
1. A method for producing a neutralized precipitate containing impurities by an oxidation-neutralization reaction by blowing chlorine gas as an oxidizing agent into an aqueous nickel chloride solution containing impurities in a reaction vessel and adding a neutralizing agent, comprising the steps of: The amount of chlorine gas blown per unit volume of the aqueous nickel chloride solution in the reaction tank is 1.5 kg / (m 3 h) is less than or equal to 2. A method for oxidizing and neutralizing an aqueous nickel chloride solution.
2. The oxidation-reduction potential of the nickel chloride aqueous solution (based on an Ag / AgCl electrode) is 600 to 1,200 mV.
2. The method for oxidizing and neutralizing an aqueous nickel chloride solution according to claim 1.
3. The neutralizing agent is nickel carbonate.
2. The method for oxidizing and neutralizing an aqueous nickel chloride solution according to claim 1.
4. The nickel concentration of the aqueous nickel chloride solution is 90 to 130 g / L.
2. The method for oxidizing and neutralizing an aqueous nickel chloride solution according to claim 1.
5. The nickel chloride aqueous solution is continuously supplied to a plurality of the reaction tanks connected in series, The amount of chlorine gas blown per unit volume of the aqueous nickel chloride solution in the most upstream reaction tank among the plurality of reaction tanks is 1.5 kg / (m 3 h) is less than or equal to 2. The method for oxidizing and neutralizing an aqueous nickel chloride solution according to claim 1.
Citation Information
Patent Citations
Technology for removing cobalt by dynamic wave chlorine oxidation
CN103361483A
Lead removal method for nickel chloride solution
CN114107697A
Method for removing lead in chloride solution
JP1994306503A
Method for removing lead from nickel solution
JP1996295965A
Method for controlling oxidization and neutralization of aqueous nickel chloride solution