Elastomer composition and film thereof

The elastomer composition, featuring a copolymerized α-olefin and diene with a photopolymerization initiator, addresses the lack of suitability in soft and transparent products by enhancing flexibility and heat resistance, making it suitable for automotive decorative films and other applications.

JP2024168842APending Publication Date: 2024-12-05RIKEN TECHNOS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023085844
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing copolymer elastomers of α-olefin and diene lack suitability as materials for soft and transparent products, particularly in applications requiring flexibility, transparency, and heat resistance.

Method used

A specific elastomer composition comprising a copolymerized elastomer of α-olefin and diene, combined with a photopolymerization initiator, which does not contain intramolecularly cleavable initiators, and is formulated to achieve high total light transmittance and controlled crosslinking for improved flexibility and heat resistance.

Benefits of technology

The resulting films exhibit excellent flexibility, transparency, and heat resistance, making them suitable for automotive decorative films and other soft, transparent applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168842000001
    Figure 2024168842000001
Patent Text Reader

Abstract

To provide an elastomer composition suitable as a material for a soft and transparent product, and a film thereof.SOLUTION: The present invention provides an elastomer composition that contains (A) 100 pts.mass of a copolymer elastomer of α-olefin and diene, preferably a copolymer elastomer of α-olefin and non-conjugated diene and (B) 0.01-30 pts.mass of a photopolymerization initiator, preferably a hydrogen-abstraction photopolymerization initiator, and a film thereof. The film is subjected to irradiation with active energy rays, resulting in enhanced heat resistance.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an elastomeric composition and a film thereof. [Background technology]

[0002] Copolymer elastomers of α-olefins and dienes, such as copolymer elastomers of ethylene, propylene, and dienes (EPDM), have no double bonds in the main chain, and therefore have features such as heat resistance, aging resistance, ozone resistance, and weather resistance, and have been widely used in various elastomer products for automobiles, industrial use, and construction. In addition, copolymer elastomers of α-olefins and dienes are soft and highly transparent, and therefore are considered to be suitable as materials for soft or soft and transparent products or components, such as surface protection films for automobiles, such as chipping films, and decorative films for automobiles, such as dressing films, marking films, tail lamp seals, and emblem seals, as well as materials for umbrellas, raincoats, bags, and badges. However, they have not been proposed as materials for soft products, particularly soft and transparent products. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-180370 A [Patent Document 2] JP 2005-019315 A [Patent Document 3] International Publication No. 2021 / 060446 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide an elastomer composition suitable as a material for soft products, and a film thereof. [Means for solving the problem]

[0005] As a result of extensive research, the present inventors have found that the above object can be achieved by using a specific elastomer composition.

[0006] That is, the various aspects of the present invention are as follows. [1]. (A) 100 parts by mass of a copolymer elastomer of an α-olefin and a diene; and (B) Photopolymerization initiator 0.01 to 30 parts by mass 1. An elastomer composition comprising: [2]. The elastomer composition according to item [1], wherein the component (A) copolymer elastomer of an α-olefin and a diene includes a copolymer elastomer of an α-olefin and a non-conjugated diene. [3]. The elastomer composition according to item [1], wherein the component (A) copolymerized elastomer of an α-olefin and a diene includes a copolymerized elastomer of ethylene, propylene, and one or more dienes selected from the group consisting of 5-ethylidene-2-norbornene, tricyclo[4.3.0.12,5]deca-3,7-diene, and 1,4-hexadiene. [4]. The elastomer composition according to item [2], wherein the component (B) photopolymerization initiator contains a hydrogen abstraction type photopolymerization initiator. [5]. The elastomer composition according to item [4], which does not contain an intramolecular cleavage type photopolymerization initiator. [6]. A film comprising the elastomer composition according to any one of [1] to [5]. [7]. Item 6. The film according to item 6, having a total light transmittance of 70% or more as measured according to JIS K7136:2000. [8]. The film according to item [6], having a loss tangent of 0.70 or less at a temperature of 140°C: The loss tangent mentioned above is the loss tangent value at a temperature of 140°C on a temperature-loss tangent curve obtained by measuring a sample of 25 mm in length and 10 mm in width taken from the film using a dynamic viscoelasticity measuring device, setting the chuck distance to 5 mm, and measuring under the following temperature program conditions: tensile mode, frequency of 1 Hz, and temperature of -80°C, holding the sample for 1 minute, and then heating the sample to 250°C at a heating rate of 5°C / min. [9]. A method for producing the film according to item [6], (1) a step of obtaining an elastomer composition comprising: (A) 100 parts by mass of a copolymer elastomer of an α-olefin and a diene; and (B) 0.01 to 30 parts by mass of a photopolymerization initiator; (2) forming a film from the elastomer composition obtained in the step (1) using a T-die film-forming apparatus equipped with an extruder, a T-die, and a take-up device; and (3) A step of irradiating the film-shaped molded body obtained in the above step (2) with active energy rays. A method for producing the film.

[10] . A method for producing the film according to item [6], (1) a step of obtaining an elastomer composition comprising: (A) 100 parts by mass of a copolymer elastomer of an α-olefin and a diene; and (B) 0.01 to 30 parts by mass of a photopolymerization initiator; (2) forming a film from the elastomer composition obtained in the step (1) using a calender roll rolling machine and a calender roll film forming apparatus equipped with a take-up device; and (3) A step of irradiating the film-shaped molded body obtained in the above step (2) with active energy rays. A method for producing the film. Effect of the Invention

[0007] Molded articles such as films obtained by using the elastomer composition of the present invention have excellent flexibility. Molded articles such as films obtained by using the preferred composition of the present invention also have good transparency, heat resistance, and color tone. Therefore, the elastomer of the present invention can be suitably used as a material for substrate films such as surface protection films and decorative films, for example, surface protection films for automobiles such as chipping films, and decorative films for automobiles such as dressing films, marking films, tail lamp seals, and emblem seals. Therefore, the elastomer of the present invention can be suitably used as a material for umbrellas, raincoats, bags, and badges. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In this specification, the term "resin (including elastomer; the same applies hereinafter)" is used to include a resin mixture containing two or more types of resins, and a resin composition containing components other than resin.

[0009] In this specification, the term "film" is used interchangeably or interchangeably with "sheet." In this specification, the terms "film" and "sheet" are used for those that can be industrially wound into a roll. The term "plate" is used for those that cannot be industrially wound into a roll. In addition, in this specification, laminating a certain layer and another layer in order includes both directly laminating the layers and laminating the layers with one or more other layers, such as an anchor coat, interposed between the layers.

[0010] In this specification, the term "more than" in relation to a numerical range means a certain number or more than a certain number. For example, 20% or more means 20% or more than 20%. The term "less than" in relation to a numerical range means a certain number or less than a certain number. For example, 20% or less means 20% or less than 20%. Furthermore, the symbol "~" in relation to a numerical range means a certain number, more than a certain number and less than another certain number, or another certain number. Here, the other certain number is a number larger than the certain number. For example, 10 to 90% means 10%, more than 10% and less than 90%, or 90%. Furthermore, the upper and lower limits of the numerical range can be arbitrarily combined, and an embodiment in which the values ​​are arbitrarily combined can be read. For example, from a statement regarding the numerical range of a certain characteristic such as "usually 10% or more, preferably 20% or more. On the other hand, it is usually 40% or less, preferably 30% or less" or "usually 10 to 40%, preferably 20 to 30%," it can be read that the numerical range of the certain characteristic is 10 to 40%, 20 to 30%, 10 to 30%, or 20 to 40% in one embodiment.

[0011] Other than in the examples, or where otherwise specified, all numerical values ​​used in the specification and claims should be understood to be modified by the term "about." Without attempting to limit the application of the doctrine of equivalents to the scope of the claims, each numerical value should be construed in light of the number of significant digits and by applying ordinary rounding techniques.

[0012] In this specification, terms specifying shapes or geometric conditions, such as parallel, orthogonal, and perpendicular, are intended to include substantially the same state in addition to their strict meanings.

[0013] In this specification, when it is explained that "comprises a certain substance", it is to be understood that in one embodiment, it contains a certain substance, consists of a certain substance, or consists only of a certain substance. For example, from the explanation that "composition A comprises substance a1 and substance a2", it is to be understood that in one embodiment, composition A comprises substance a1 and substance a2, composition A consists of substance a1 and substance a2, or composition A consists only of substance a1 and substance a2.

[0014] 1. Elastomer composition: The elastomer composition of the present invention comprises: (A) a copolymer elastomer of an α-olefin and a diene; and (B) a photopolymerization initiator. Each component will be described below.

[0015] (A) Copolymer elastomer of α-olefin and diene: The elastomer composition of the present invention contains the above-mentioned component (A), a copolymerized elastomer of an α-olefin and a diene. The above-mentioned component (A) is a copolymer of an α-olefin and a diene, and is a non-crystalline or low-crystalline copolymer. Since the above-mentioned component (A) is non-crystalline or low-crystalline, it has elastomeric properties and serves to impart excellent flexibility to a molded article such as a film obtained by using the elastomer composition of the present invention. Furthermore, since the above-mentioned component (A) is non-crystalline or low-crystalline, it has transparency and serves to impart good transparency to a molded article such as a film obtained by using the preferred elastomer composition of the present invention.

[0016] In this specification, being non-crystalline or low crystalline means that in a crystallization curve measured according to JIS K7121-1987 using a Diamond DSC type differential scanning calorimeter manufactured by PerkinElmer Japan Co., Ltd., with a temperature program of holding at 190°C for 5 minutes and cooling to -50°C at a temperature drop rate of 10°C / min, no peak associated with crystallization (hereinafter referred to as "crystallization peak") is observed, or the peak top temperature of the crystallization peak (hereinafter referred to as "crystallization temperature") is 60°C or lower. Here, when there are two or more crystallization peaks, the peak top temperature of the crystallization peak with the highest peak height is taken as the crystallization temperature. The crystallization temperature of the component (A) copolymerized elastomer of α-olefin and diene may be preferably 50°C or lower, more preferably 40°C or lower. In one preferred embodiment, the component (A) copolymerized elastomer of α-olefin and diene may be one in which no crystallization peak is observed.

[0017] The α-olefin is an alkene having a carbon-carbon double bond at the α-position. Examples of the α-olefin include ethylene, propylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-pentene-1. The α-olefin may be one or more of these.

[0018] The diene is an alkene having two carbon-carbon double bonds in one molecule. Examples of the diene include non-conjugated dienes (dienes in which two carbon-carbon double bonds are separated by two or more carbon-carbon single bonds), conjugated dienes (dienes in which two carbon-carbon double bonds are separated by one carbon-carbon single bond), and allenes (dienes in which two carbon-carbon double bonds are adjacent to each other). Among these, the non-conjugated dienes are preferred from the viewpoint of making the component (A) copolymer elastomer of α-olefin and diene have no double bonds in the main chain.

[0019] Examples of the non-conjugated dienes include 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, 1,7-octadiene, bicyclo[2.2.1]hepta-2-ene (norbornene), 5-ethylidene-2-norbornene (ethylidenenorbornene), and tricyclo[4.3.0.12,5]deca-3,7-diene (dicyclopentadiene).

[0020] As the diene, one or more of these can be used.

[0021] The component (A) copolymerized elastomer of an α-olefin and a diene may preferably include a copolymerized elastomer of an α-olefin and a non-conjugated diene. The component (A) copolymerized elastomer of an α-olefin and a diene may more preferably include a copolymerized elastomer of ethylene, propylene, and one or more dienes selected from the group consisting of 5-ethylidene-2-norbornene (ethylidene norbornene), tricyclo[4.3.0.12,5]deca-3,7-diene (dicyclopentadiene), and 1,4-hexadiene.

[0022] The Mooney viscosity (ML) of the component (A) copolymer elastomer of α-olefin and diene was measured according to ASTM D1646 using an L-shaped rotor under the conditions of a preheating time of 1 minute, a rotor rotation time of 4 minutes, and a test temperature of 125°C. 1+4 125° C.) may be preferably 70 or less, more preferably 50 or less, even more preferably 40 or less, and most preferably 30 or less, from the viewpoint of film formability. On the other hand, it may be preferably 10 or more, more preferably 15 or more, from the viewpoint of mechanical strength.

[0023] The component (A) copolymer elastomer of α-olefin and diene may contain a structural unit derived from a monomer other than α-olefin and diene (hereinafter referred to as "other monomer"), to the extent that it does not contradict the object of the present invention. Examples of the other monomer include unsaturated carboxylic acids such as (meth)acrylic acid, (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, acid anhydrides of unsaturated carboxylic acids such as maleic anhydride, aromatic vinyl compounds such as styrene, and compounds having a polymerizable carbon-carbon double bond such as vinyl acetate. As the other monomer, one or more of these may be used. The content of the structural unit derived from the other monomer in the component (A) copolymer elastomer of α-olefin and diene may be usually 10% by mass or less, preferably 6% by mass or less, and more preferably 0 to 3% by mass, based on the sum of all structural units of the component (A) being 100% by mass.

[0024] In one preferred embodiment, the copolymer elastomer of α-olefin and diene (A) may not contain any of the other monomers. Here, "not containing any of the other monomers" means that the other monomers are not used intentionally. Therefore, "not containing any of the other monomers" can be rephrased as the content of the structural unit derived from the other monomer in the component (A) is usually 0.1% by mass or less, preferably 0.05% by mass or less, more preferably 0 to 0.01% by mass.

[0025] As the component (A), the copolymer elastomer of an α-olefin and a diene, one or a mixture of two or more of these can be used.

[0026] (B) Photopolymerization initiator: The elastomer composition of the present invention contains the above-mentioned component (B) photopolymerization initiator, which generates radicals when irradiated with active energy rays, thereby crosslinking the above-mentioned component (A) copolymer elastomer of an α-olefin and a diene, thereby improving heat resistance.

[0027] The component (B) photopolymerization initiator is roughly classified into (B1) hydrogen abstraction type photopolymerization initiator and (B2) intramolecular cleavage type photopolymerization initiator. The component (B1) hydrogen abstraction type photopolymerization initiator is a compound that absorbs light of a specific wavelength to become excited and abstracts hydrogen from surrounding hydrogen donors to generate radicals. The component (B2) intramolecular cleavage type photopolymerization initiator is a compound that absorbs light of a specific wavelength to break a bond at a specific site of the photopolymerization initiator itself to generate radicals.

[0028] Examples of the hydrogen abstraction type photopolymerization initiator, component (B1), include benzophenone-based compounds, anthraquinone-based compounds, thioxanthone-based compounds, and hexaarylbisimidazoles.

[0029] Examples of the benzophenone compounds include benzophenone, methyl-o-benzoylbenzoate, 4-methylbenzophenone, 4,4'-bis(diethylamino)benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.

[0030] Examples of the anthraquinone compounds include methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, and 2-amylanthraquinone.

[0031] Examples of the thioxanthone compounds include thioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone.

[0032] Among these, as the component (B1) hydrogen abstraction photopolymerization initiator, a benzophenone-based compound is preferred from the viewpoint of suppressing coloration of the molded article.

[0033] Examples of the component (B2) intramolecular cleavage type photopolymerization initiator include alkylphenone compounds, acylphosphine oxide compounds, and oxime ester compounds.

[0034] Examples of the alkylphenone compounds include 1-hydroxycyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-methylpropanone, 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, and 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone.

[0035] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0036] Examples of the oxime ester compounds include 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(o-benzoyloxime), and ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime).

[0037] In the case where the component (A) copolymerized elastomer of α-olefin and diene contains the copolymerized elastomer of α-olefin and non-conjugated diene, the component (B) photopolymerization initiator may preferably contain the component (B1) hydrogen abstraction type photopolymerization initiator from the viewpoint of heat resistance. In the case where the component (A) copolymerized elastomer of α-olefin and diene contains the copolymerized elastomer of α-olefin and non-conjugated diene, the component (B) photopolymerization initiator may more preferably contain the component (B1) hydrogen abstraction type photopolymerization initiator and not contain the component (B2) intramolecular cleavage type photopolymerization initiator from the viewpoint of heat resistance.

[0038] Without intending to be bound by theory, the reason why it is preferable to use the component (B1) hydrogen abstraction type photopolymerization initiator in the case where the component (A) copolymerized elastomer of an α-olefin and a diene contains the copolymerized elastomer of the α-olefin and a non-conjugated diene from the viewpoint of heat resistance is considered as follows. The component (B1) hydrogen abstraction type photopolymerization initiator requires a hydrogen supply source in the carbon-carbon double bond in the component (A) copolymerized elastomer of an α-olefin and a diene, and does not require a hydrogen supply source in other places. In the case of the copolymerized elastomer of an α-olefin and a non-conjugated diene, the carbon-carbon double bond does not exist in the main chain, but only in the side chain composed of a structural unit derived from the non-conjugated diene. Therefore, the crosslinking reaction proceeds exclusively, and the main chain is not cut. As a result, the degree of crosslinking is increased, and heat resistance is sufficiently improved. On the other hand, the radicals generated by the component (B2) intramolecular cleavage type photopolymerization initiator act on random positions of the component (A) copolymer elastomer of α-olefin and diene. Therefore, even in the case of the copolymer elastomer of α-olefin and non-conjugated diene, the crosslinking reaction and the main chain scission compete with each other. As a result, the degree of crosslinking is suppressed, and the improvement of heat resistance is also suppressed.

[0039] As the component (B) photopolymerization initiator, one or a mixture of two or more of these can be used.

[0040] The amount of the photopolymerization initiator (B) may be, from the viewpoint of heat resistance, usually 0.01 parts by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, and most preferably 0.3 parts by mass or more, based on 100 parts by mass of the copolymer elastomer (A) of α-olefin and diene, while from the viewpoint of suppressing coloration of the molded product, it may be usually 30 parts by mass or less, preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and most preferably 3 parts by mass or less.

[0041] (C)Lubricant: In one of the preferred embodiments, the elastomer composition of the present invention may further contain a lubricant (C). By including the component (C) in the elastomer composition of the present invention, moldability is improved, and a molded product having good transparency can be easily obtained. By including the component (C) in the elastomer composition of the present invention, film formability is improved, and a film having good transparency can be easily obtained.

[0042] Examples of the lubricant (C) include fatty acid-based lubricants, metal soaps, fatty acid amides, fatty alcohols, ester-based lubricants, hydrocarbon-based lubricants, and silicone oils.

[0043] Examples of the fatty acid-based lubricants include saturated higher fatty acids such as capric acid, lauric acid, palmitic acid, and stearic acid, unsaturated higher fatty acids such as oleic acid, linoleic acid, ricinoleic acid, behenic acid, and erucic acid, and hydroxy higher fatty acids such as 12-hydroxystearic acid.

[0044] The metal soap is a salt of an aliphatic carboxylic acid such as a fatty acid or a hydroxy fatty acid with a metal such as calcium, zinc, or barium. Examples of the metal soap include higher fatty acid metal salts. Examples of the higher fatty acid metal salts include metal stearates such as calcium stearate, zinc stearate, and barium stearate, metal laurates such as calcium laurate, zinc laurate, and barium laurate, and metal ricinoleates such as calcium ricinoleate, zinc ricinoleate, and barium ricinoleate.

[0045] The fatty acid amide is a compound obtained by amidating an aliphatic carboxylic acid such as a fatty acid or a hydroxy fatty acid with an amine compound. Examples of the fatty acid amide include saturated higher fatty acid amides such as capric acid amide, palmitic acid amide, and stearic acid amide, unsaturated higher fatty acid amides such as oleic acid amide, linoleic acid amide, and erucic acid amide, and bis-higher fatty acid amides such as ethylene bis-stearic acid amide, ethylene bis-oleic acid amide, and ethylene bis-erucic acid amide.

[0046] Examples of the fatty alcohol include stearyl alcohol, lauryl alcohol, and palmityl alcohol.

[0047] Examples of the ester-based lubricants include glycerin monostearate, glycerin monooleate, and butyl stearate.

[0048] Examples of the hydrocarbon lubricant include paraffin wax and polyethylene wax.

[0049] As the component (C) lubricant, one of these may be used alone or a mixture of two or more of them may be used.

[0050] In the case where the component (C) lubricant is used, the amount of the component (C) lubricant may be, from the viewpoint of reliably obtaining the effect of using the component (C) lubricant, preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, based on 100 parts by mass of the component (A) copolymer elastomer of α-olefin and diene, while from the viewpoint of suppressing troubles due to bleeding out of the component (C) lubricant, the amount may be preferably 2 parts by mass or less, more preferably 1 part by mass or less.

[0051] The elastomer composition of the present invention may further contain other optional components other than the component (A) copolymerized elastomer of α-olefin and diene and the component (B) photopolymerization initiator, to the extent that it does not contradict the object of the present invention. Examples of the other optional components include resins (including elastomers) other than the component (A) copolymerized elastomer of α-olefin and diene, heat stabilizers, antioxidants, weathering stabilizers, light resistance stabilizers, ultraviolet absorbers (excluding compounds corresponding to the component (B) photopolymerization initiator), antifouling agents, nucleating agents, antistatic agents such as glycerin fatty acid esters, flame retardants, inorganic particles, organic particles, inorganic colorants, and organic colorants. As the other optional components, one or a mixture of two or more of these may be used. The amount of the other optional components is not particularly limited, as long as it does not contradict the object of the present invention, since they are optional components. The amount of the other optional components may be typically 50 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, 10 parts by mass or less, 5 parts by mass or less, 0 to 1 part by mass, or about 0.01 to 50 parts by mass, relative to 100 parts by mass of the component (A) copolymer elastomer of an α-olefin and a diene.

[0052] In one embodiment, the elastomer composition of the present invention may not contain any one or more of the other optional components. Here, not containing any of the other optional components means that the component is not intentionally blended. Therefore, not containing any of the other optional components can also be rephrased as the content of the component is usually less than 0.01 parts by mass, preferably 0.001 parts by mass or less, more preferably 0.0001 parts by mass or less, relative to 100 parts by mass of the copolymer elastomer of α-olefin and diene, component (A).

[0053] 2. Method for producing elastomer composition: The elastomer composition of the present invention can be obtained by using any melt kneader, simultaneously or in any order introducing the component (A) copolymerized elastomer of an α-olefin and a diene, the component (B) photopolymerization initiator, and the other optional components used as desired, and melt kneading them, preferably at a resin temperature of 60 to 200°C.

[0054] Examples of the melt kneader include batch kneaders such as pressure kneaders and mixers, extrusion kneaders such as single-screw extruders, co-rotating twin-screw extruders, and counter-rotating twin-screw extruders, and calendar roll kneaders. These may be used in any combination.

[0055] The resulting elastomer composition can be pelletized by any method and then molded into any article by any method, such as hot cutting, strand cutting, and underwater cutting.

[0056] In another embodiment, the elastomer composition in the form of chunks, rods, or strands discharged from the melt kneader may be sent directly to any molding machine to mold an article.

[0057] 3.Film: The film of the present invention is a film containing the elastomer composition of the present invention. In one typical embodiment, the film of the present invention is a film made of the elastomer composition of the present invention. In one preferred embodiment, the film of the present invention is a film made of the elastomer composition of the present invention, and in which the component (B) photopolymerization initiator acts upon irradiation with active energy rays to crosslink the component (A) copolymer elastomer of α-olefin and diene. In one embodiment, the film of the present invention may be a multilayer film having one or more layers made of the elastomer composition of the present invention. In another preferred embodiment, the film of the present invention is a multilayer film having one or more layers made of the elastomer composition of the present invention, and in which the layer made of the elastomer composition of the present invention is a multilayer film in which the component (B) photopolymerization initiator acts upon irradiation with active energy rays to crosslink the component (A) copolymer elastomer of α-olefin and diene.

[0058] The total light transmittance of the film of the present invention measured according to JIS K7136: 2000 may be preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, still more preferably 85% or more, and most preferably 88% or more. By having a total light transmittance of 70% or more, the film of the present invention can be suitably used in applications requiring transparency, such as the base film of a chip-resistant film.

[0059] From the viewpoint of heat resistance, the loss tangent (tan δ) of the film of the present invention at a temperature of 140° C. may be preferably 0.70 or less, more preferably 0.60 or less, even more preferably 0.50 or less, still more preferably 0.40 or less, even more preferably 0.30 or less, and most preferably 0.20 or less. Here, the loss tangent (tan δ) is the value of the loss tangent (tan δ) at a temperature of 140° C. in a temperature-loss tangent curve obtained by using a dynamic viscoelasticity measuring device, using a sample of 25 mm in length and 10 mm in width taken from the film, setting the sample so that the chuck distance is 5 mm, and measuring under the conditions of a tensile mode, a frequency of 1 Hz, and a temperature program in which the temperature is held at −80° C. for 1 minute and then increased to 250° C. at a heating rate of 5° C. / min. Without intending to be bound by theory, the loss tangent (tan δ) at a temperature of 140°C is believed to be an indicator of the degree of crosslinking of the copolymer elastomer of α-olefin and diene, component (A), in the film of the present invention (the smaller the loss tangent (tan δ) at a temperature of 140°C, the greater the degree of crosslinking).

[0060] The thickness of the film of the present invention can be appropriately determined taking into consideration the film-forming property, the use and the required properties thereof, and the handling property. When the film of the present invention is used as a base film of a chip-resistant film, the thickness of the film of the present invention may be usually 50 to 700 μm, preferably 100 to 600 μm, more preferably 150 to 500 μm.

[0061] 4. Film manufacturing method: The method for producing the film of the present invention is not particularly limited. For example, the method for producing the film of the present invention may include a method in which the elastomer composition of the present invention is obtained, then molded into a film by a known method, and irradiated with active energy rays. In one preferred embodiment, the film of the present invention can be obtained by a production method including: (1) a step of obtaining the elastomer composition of the present invention; (2) a step of forming a film using the elastomer composition obtained in the above step (1) using a film-forming device; and (3) a step of irradiating the film-shaped molded body obtained in the above step (2) with active energy rays.

[0062] The above step (1) is a step for obtaining the elastomer composition of the present invention. The elastomer composition of the present invention has been described in "1. Elastomer composition". The method for obtaining the elastomer composition of the present invention has been described in "2. Method for producing elastomer composition".

[0063] The above step (2) is a step of forming a film using a film-forming apparatus from the elastomer composition obtained in the above step (1). As the elastomer composition, a pelletized one may be used, or the elastomer composition in the form of a block, rod, or strand discharged from a melt kneader may be directly sent to the film-forming apparatus and used.

[0064] The film-forming apparatus is not particularly limited, and any film-forming apparatus can be used. Since the elastomer composition of the present invention is a composition having a relatively high viscosity, the film-forming apparatus may preferably be a T-die film-forming apparatus equipped with an extruder, a T-die, and a winding device, or a calender roll rolling film-forming apparatus equipped with a calender roll rolling machine and a winding device.

[0065] When a T-die film-forming apparatus equipped with an extruder, a T-die, and a take-up device is used as the film-forming apparatus, the T-die outlet resin temperature may be preferably 120° C. or higher, more preferably 135° C. or higher, and even more preferably 150° C. or higher, from the viewpoint of the transparency of the obtained film and from the viewpoint of melting and dispersing the component (B) photopolymerization initiator to reliably obtain the action of the component. On the other hand, the T-die outlet resin temperature may be preferably 300° C. or lower, more preferably 240° C. or lower, and even more preferably 200° C. or lower, from the viewpoint of suppressing consumption of the component (B) photopolymerization initiator before irradiation with active energy rays.

[0066] When a calendar roll film-forming apparatus equipped with a calendar roll rolling machine and a winding device is used as the film-forming apparatus, the resin temperature of the film-like molded product sent from the calendar roll rolling machine to the winding device may be preferably 120° C. or higher, more preferably 135° C. or higher, and even more preferably 150° C. or higher, from the viewpoint of the transparency of the obtained film and from the viewpoint of melting and dispersing the component (B) photopolymerization initiator to reliably obtain the action of the component. On the other hand, the resin temperature may be preferably 300° C. or lower, more preferably 240° C. or lower, and even more preferably 200° C. or lower, from the viewpoint of suppressing consumption of the component (B) photopolymerization initiator before irradiation with active energy rays.

[0067] The step (3) is a step of irradiating the film-like molded article obtained in the step (2) with active energy rays. In the step (3), the component (B) photopolymerization initiator acts by irradiating the film with active energy rays, and the component (A) α-olefin / diene copolymer elastomer is crosslinked.

[0068] The cumulative dose of the irradiation can be appropriately selected and determined in consideration of the thickness of the film-like molded article obtained in the step (2) from the viewpoint of sufficient crosslinking (obtaining sufficient heat resistance) and preventing coloring (yellowing). The cumulative dose of the irradiation depends on the thickness of the film-like molded article obtained in the step (2), but is usually 100 mJ / cm from the viewpoint of sufficient crosslinking (obtaining sufficient heat resistance). 2 More than 400 mJ / cm 2 More preferably, 700 mJ / cm 2 On the other hand, from the viewpoint of preventing coloring (yellowing), it is usually 10000 J / cm 2 Less than 7000 mJ / cm 2 Less than or equal to 4000 mJ / cm 2 More preferably, 2000 mJ / cm 2 It may be the following:

[0069] After the above step (3), an aging treatment may be carried out, which can stabilize the properties of the film of the present invention.

[0070] 5. Goods: The article of the present invention includes the elastomer composition of the present invention. In one typical embodiment, the article of the present invention includes the film of the present invention. Examples of the article of the present invention include surface protection films, such as surface protection films for automobiles, such as chipping films, and decorative films, such as dressing films, marking films, tail lamp seals, and emblem seals, as well as umbrellas, raincoats, bags, and badges. EXAMPLES

[0071] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0072] Measurement method (a) Tensile test: In accordance with JIS K7127:1999, a tensile tester "Autograph AGS-1kNX (product name)" manufactured by Shimadzu Corporation was used to perform a tensile test at a tensile speed of 200 mm / min and a temperature of 23°C using a sample punched out from the film in the shape of the test piece type 5 (Figure 2 of the JIS standard) of the above JIS standard, with the machine direction of the film being the tensile direction, to obtain a stress-strain curve. Next, from the obtained stress-strain curve, the 5% strain tensile stress (referred to as "5% modulus" in the table, unit: MPa) and the 100% strain tensile stress (referred to as "100% modulus" in the table, unit: MPa) were calculated in accordance with Clause 10 of JIS K7161-1:2014. The tensile stress at the time when the sample broke was calculated as the tensile strength (unit: MPa), and the strain was calculated as the tensile elongation (unit: %).

[0073] (b) Total light transmittance: The total light transmittance (unit: %) of the film was measured using a turbidity meter "NDH4000 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K7136:2000.

[0074] (c) Loss tangent (tan δ): A dynamic viscoelasticity measuring device was used to obtain a sample 25 mm long and 10 mm wide taken from the film with the machine direction of the film being the tensile direction, the sample was set with a chuck distance of 5 mm, and a temperature-loss tangent curve was obtained under the following temperature program conditions: tensile mode, frequency of 1 Hz, temperature of -80°C, held for 1 minute, and then heated to 250°C at a heating rate of 5°C / min. The loss tangent at 140°C was then calculated from the obtained temperature-loss tangent curve.

[0075] (d) Yellowness index: The yellowness index of the film was measured using a colorimeter "SolidSpec-3700 (product name)" manufactured by Shimadzu Corporation in accordance with JIS K7105:1981.

[0076] Raw materials used (A) Copolymer elastomer of α-olefin and diene (A-1) Ethylene-propylene-ethylidene norbornene copolymer "Nodel 4725P (trade name)" from The Dow Chemical Company. Crystallization temperature: 30°C (low crystallinity), Mooney viscosity (ML 1+4 125°C) 25, content of structural units derived from ethylene 70% by mass, content of structural units derived from ethylidenenorbornene 4.9% by mass (A-2) Ethylene-propylene-ethylidene norbornene copolymer "Nodel 3720P (trade name)" from The Dow Chemical Company. Crystallization temperature: 38°C (low crystallinity), Mooney viscosity (ML 1+4 125°C)20, content of structural units derived from ethylene 70% by mass, content of structural units derived from ethylidenenorbornene 0.6% by mass

[0077] (B1) Hydrogen abstraction type photopolymerization initiator (B1-1) 4-Methylbenzophenone. CAS number 134-84-9 (B1-2) Benzophenone. CAS number 119-61-9 (B1-3) 2,4-Diethylthioxanthone. CAS number 82799-44-8

[0078] (B2) Intramolecular cleavage type photopolymerization initiator (B2-1) IGM Resins' alkylphenone photoinitiator (1-hydroxycyclohexyl-phenyl ketone) "Omnirad 184 (trade name)".

[0079] (C)Lubricant: (C-1) Stearic acid. CAS number 57-11-4

[0080] Example 1 A mixture consisting of 100 parts by mass of the above component (A-1), 0.5 parts by mass of the above component (B1-1), and 0.5 parts by mass of the above component (C-1) was melt-kneaded at a temperature of 170°C to obtain an elastomer composition, which was then sent directly to a calendar roll rolling film-forming device equipped with a calendar roll rolling processor and a winding device, and the film-shaped molded product sent from the calendar roll rolling processor to the winding device was formed into a film under the condition of a resin temperature of 170°C to obtain a film-shaped molded product. Next, a high-pressure mercury lamp-type ultraviolet ray irradiation device was used on the film-shaped molded product, with an accumulated light amount of 750 mJ / cm. 2 The film was irradiated with ultraviolet rays under the above conditions to obtain a film having a thickness of 300 μm. The above tests (a) to (d) were carried out. The results are shown in Table 1.

[0081] Examples 2-5 A film was obtained in the same manner as in Example 1, except that the formulation of the elastomer composition was changed as shown in Table 1. The above tests (a) to (d) were carried out. The results are shown in Table 1.

[0082] Example 6 Accumulated light intensity of 1500mJ / cm 2 A film was obtained in the same manner as in Example 1, except for changing the above. The above tests (a) to (d) were carried out. The results are shown in Table 1.

[0083] [Table 1]

[0084] Example 7 The elastomer composition of Example 1 was dissolved in toluene to obtain a solution with a solid content concentration of 10% by mass. Next, the solution was used to form a wet coating film using an applicator on the surface of a biaxially oriented polyethylene terephthalate film that had been treated for easy peeling, so that the film thickness after drying would be 25 μm. Next, the film was dried in a drying oven set at a temperature of 110° C. Next, a high-pressure mercury lamp-type ultraviolet ray irradiation device was used from the coating surface side, and an integrated light amount of 750 mJ / cm was applied. 2 The film was irradiated with ultraviolet light under the above conditions to obtain a film having a thickness of 25 μm. The film had a very soft feel and high transparency. The above test (c) loss tangent (tan δ) was carried out. The loss tangent (tan δ) was 0.15.

[0085] It was found that the film made of the elastomer composition of the present invention has excellent flexibility. It was also found that the film made of the preferred elastomer composition of the present invention has good transparency, heat resistance, and color tone.

Claims

1. (A) 100 parts by mass of a copolymer elastomer of an α-olefin and a diene; and (B) Photopolymerization initiator: 0.01 to 30 parts by mass 1. An elastomer composition comprising:

2. 2. The elastomer composition according to claim 1, wherein the component (A) copolymerized elastomer of an α-olefin and a diene comprises a copolymerized elastomer of an α-olefin and a non-conjugated diene.

3. The elastomer composition according to claim 1, wherein the component (A) copolymerized elastomer of an α-olefin and a diene comprises a copolymerized elastomer of ethylene, propylene, and one or more dienes selected from the group consisting of 5-ethylidene-2-norbornene, tricyclo[4.3.0.12,5]deca-3,7-diene, and 1,4-hexadiene.

4. The elastomer composition according to claim 2 , wherein the component (B) photopolymerization initiator comprises a hydrogen abstraction type photopolymerization initiator.

5. The elastomer composition according to claim 4, which does not contain an intramolecular cleavage type photopolymerization initiator.

6. A film comprising the elastomer composition according to any one of claims 1 to 5.

7. The film according to claim 6, which has a total light transmittance of 70% or more as measured in accordance with JIS K7136:2000.

8. The film according to claim 6, having a loss tangent of 0.70 or less at a temperature of 140°C. The loss tangent mentioned above is the value of the loss tangent at a temperature of 140°C on a temperature-loss tangent curve obtained by measuring a sample of 25 mm in length and 10 mm in width taken from the film using a dynamic viscoelasticity measuring device, setting the chuck distance to be 5 mm, and measuring under the following temperature program conditions: tensile mode, frequency of 1 Hz, and temperature of -80°C, holding the sample for 1 minute, and then heating the sample to 250°C at a heating rate of 5°C / min.

9. A method for producing the film of claim 6, comprising the steps of: (1) a step of obtaining an elastomer composition comprising: (A) 100 parts by mass of a copolymer elastomer of an α-olefin and a diene; and (B) 0.01 to 30 parts by mass of a photopolymerization initiator; (2) forming a film from the elastomer composition obtained in the step (1) using a T-die film-forming apparatus equipped with an extruder, a T-die, and a take-up device; and (3) A step of irradiating the film-like molded article obtained in the above step (2) with active energy rays. A method for producing the film.

10. A method for producing the film of claim 6, comprising the steps of: (1) a step of obtaining an elastomer composition comprising: (A) 100 parts by mass of a copolymer elastomer of an α-olefin and a diene; and (B) 0.01 to 30 parts by mass of a photopolymerization initiator; (2) forming a film from the elastomer composition obtained in the step (1) using a calender roll rolling machine and a calender roll film forming apparatus equipped with a take-up device; and (3) A step of irradiating the film-like molded article obtained in the above step (2) with active energy rays. A method for producing the film.

Citation Information

Patent Citations

  • Electric wire binding tape

    JP2005019315A

  • Method for producing crosslinked rubber

    JP2010180370A