Manufacturing method of submount, and manufacturing method of laser module
By heating and pressing the submount with a multi-metal layer to reduce warpage and surface irregularities, the method addresses issues of warping and void formation, ensuring consistent laser beam emission and improved reliability in semiconductor laser devices.
Patent Information
- Application Number
- JP2023086280
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
The warping of submounts and the formation of voids between the submount and laser diode bars due to mismatched coefficients of linear expansion and surface unevenness during bonding, which affect the optical output and reliability of semiconductor laser devices.
A method involving heating and pressing the submount with a metal layer to reduce warpage and surface irregularities, using a composite material with a first metal layer composed of multiple metals to enhance bonding and thermal conductivity, and aligning the laser diode bar with precision to minimize void formation.
Reduces warpage and voids, maintaining consistent laser beam emission points, improving beam quality, and enhancing the operational reliability and heat dissipation of semiconductor laser modules.
Smart Images

Figure 2024169090000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a submount and a method for manufacturing a laser module. [Background technology]
[0002] In recent years, expectations for laser processing have been rising for various materials such as copper, gold, and resin. For example, in the automobile industry, motorization, miniaturization, high rigidity, improved design freedom, and improved productivity are required, and expectations for laser processing are high. To achieve highly productive processing, a laser light source that can generate a highly efficient and high-power laser light is required. A semiconductor laser element is known as a laser light source suitable for this requirement. In particular, to increase the output of laser light, a laser module equipped with a laser diode bar having a plurality of emitters that emit laser light is useful.
[0003] Incidentally, semiconductor laser elements in the broad sense, whether single-emitter or multiple-emitter, are usually mounted on a submount for use. The submount is usually a plate-shaped component that mechanically supports the semiconductor laser element and also serves as a thermal stress buffer, dissipating heat generated by the semiconductor laser element during operation to the outside. In addition, the semiconductor laser element and the submount are generally joined together using metal solder to maximize heat dissipation.
[0004] In addition, the submount is required to have not only high heat dissipation but also a linear expansion coefficient close to that of the main semiconductor material that constitutes the semiconductor laser element. The semiconductor laser element generates heat during operation, and the temperature rise at that time causes thermal expansion of both the semiconductor laser element and the submount. If the linear expansion coefficients of the two differ significantly, thermal stress due to the difference in thermal expansion force is applied to the semiconductor laser element, causing a decrease in optical output characteristics and a decrease in reliability.
[0005] In order to achieve both high heat dissipation and matching of the linear expansion coefficient with the semiconductor laser element, it has been proposed to use a composite material, a mixture of multiple materials, as the material of the submount. For example, Patent Document 1 discloses a submount made of an aluminum-diamond composite. Patent Document 2 discloses a submount made of a composite material in which diamond particles are mixed into a metal matrix, and the surface of the diamond particles is coated with a coating layer made of the same material as the matrix. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2010 / 007922 [Patent Document 2] JP 2005-175006 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, when the above-mentioned laser diode bar is joined to the submount using metal solder, the following problems may occur.
[0008] First, since a laser diode bar has a plurality of emitters, it is often rectangular when viewed from above, and the shape of the submount is also rectangular to match this.
[0009] However, in this case, the submount is likely to warp along the longitudinal direction. When a laser diode bar is bonded to a warped submount, the laser diode bar will warp according to the amount of warping of the submount. When the laser diode bar warps, the emission points of the laser light from each emitter vary.
[0010] In addition, a metal layer is usually formed on the surface of the submount to bond it to the metal solder. This metal layer has the same composition as the metal solder or contains the same type of metal to improve compatibility with the metal solder. For example, an electrolytic plating method is used to form the metal layer on the surface of the submount.
[0011] However, when the metal layer is formed by a method with a high film formation rate such as electrolytic plating, the surface unevenness of the metal layer may become large. When the surface unevenness becomes large, a gap may be generated between the metal solder and the metal layer, and after the metal layer and the metal solder are joined, voids due to the gap may remain inside the metal solder. If such voids exist, heat dissipation from the laser diode bar to the submount is hindered during operation of the laser diode bar.
[0012] The present disclosure has been made in consideration of these points, and its purpose is to provide a method for manufacturing a submount and a method for manufacturing a laser module that can reduce warping of the submount and suppress the occurrence of voids in the metal solder interposed between the submount and the laser diode bar in a simple manner. [Means for solving the problem]
[0013] In order to achieve the above-mentioned object, a manufacturing method of a submount according to the present disclosure includes at least a first step of preparing a submount having a first surface and a second surface opposite to the first surface in a thickness direction; a second step of mounting the submount on a first mounting surface of a first mounting stand; a third step of heating the first mounting stand to a first temperature and applying a first load to the first surface or the second surface of the submount to press it; a fourth step of mounting the submount on a second mounting surface of a second mounting stand after performing the third step; and a fifth step of heating the second mounting stand to a second temperature and applying a second load to at least the first surface of the submount to press it; at least the first surface and the second surface of the submount are covered with a first metal layer, and the first metal layer includes at least a first adhesion layer in contact with at least the first surface and the second surface of the submount and a first bonding layer covering the first adhesion layer, and the first bonding layer includes two or more types of metals.
[0014] The manufacturing method of a laser module according to the present disclosure is characterized by comprising at least a sixth step of fabricating the submount using the submount manufacturing method, a seventh step of providing a first metal solder on the first surface of the submount after performing the sixth step, an eighth step of preparing a laser diode bar having a plurality of emitters provided along the longitudinal direction, and a ninth step of placing the laser diode bar on an upper surface of the first metal solder after aligning it with the first metal solder, and joining the submount and the laser diode bar. Effect of the Invention
[0015] According to the present disclosure, it is possible to reduce warping of the submount and suppress the occurrence of voids in the metal solder interposed between the submount and the laser diode bar in a simple manner. [Brief description of the drawings]
[0016] [Figure 1A] 1 is a perspective view of a laser module according to an embodiment; [Figure 1B] FIG. 1B is a cross-sectional view taken along line IB-IB in FIG. 1A. [Figure 2A] 5A to 5C are schematic diagrams illustrating one manufacturing process of the laser module. [Figure 2B] FIG. 2B is a schematic diagram illustrating a step subsequent to the step shown in FIG. 2A. [Figure 2C] FIG. 2C is a schematic diagram illustrating a step subsequent to the step shown in FIG. 2B. [Diagram 3] 1 is a flowchart showing a manufacturing process of a submount. [Figure 4] 1A to 1C are schematic diagrams illustrating a process for reducing warpage of a submount. [Diagram 5] 1A to 1C are schematic diagrams illustrating a process for reducing surface irregularities of a submount. [Figure 6] 4 is a schematic cross-sectional view of the vicinity of a first surface of a submount before a warpage reduction step is performed. FIG. [Figure 7] 11 is a schematic cross-sectional view of the vicinity of the first surface of the submount after the surface irregularity reducing step has been performed. FIG. [Figure 8] FIG. 2 is a schematic cross-sectional view of a laser module according to an embodiment. [Figure 9] 11 is an ultrasonic inspection photograph of a laser module according to a comparative example. [Figure 10] 1 is a photograph showing an ultrasonic inspection of a laser module according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. Note that the following description of the preferred embodiments is merely illustrative in nature and is not intended to limit the present disclosure, its application, or its uses.
[0018] (Embodiment) [Laser module configuration] Fig. 1A shows a perspective view of the laser module according to this embodiment, and Fig. 1B shows a cross-sectional view taken along line IB-IB in Fig. 1A. In order to make it easier to understand the shape of the laser diode bar 10, the p-side electrode 14 (see Fig. 8) is omitted in Figs. 1A and 1B. For ease of explanation, the shapes of the emitters 11 and the separation grooves 12 shown in Figs. 1A and 1B, as well as the number of these, are different from the actual ones.
[0019] In the following description, the arrangement direction of the emitters 11 in the laser diode bar 10 is referred to as the X direction, and the thickness direction of the submount 20 is referred to as the Y direction. The Y direction is also the direction in which the laser diode bar 10, the submount 20, and the base 40 are stacked. A direction perpendicular to the X direction and the Y direction is referred to as the Z direction. The Z direction is the longitudinal direction of the emitters 11, and is also the optical axis direction of the laser light emitted from each of the multiple emitters 11.
[0020] In the Y direction, the side where the laser diode bar 10 is arranged is called the top or upper side, and the side where the base 40 is arranged is called the bottom or lower side. In the Z direction, the side where the end face of the emitter 11 from which the laser light is emitted is called the front or front, and the side where the end face opposite to the said end face is called the rear or rear. In addition, the laser module 100 and each of its components viewed from the Y direction is called a plan view.
[0021] In this specification, "orthogonal," "parallel," or "the same" means orthogonal, parallel, or the same, including manufacturing tolerances of each component that makes up laser module 100 and assembly tolerances between the components, and does not mean that the objects being compared are strictly orthogonal, parallel, or the same.
[0022] As shown in FIGS. 1A and 1B, the laser module 100 is configured by stacking a base 40, a submount 20, and a laser diode bar 10 in this order from the bottom.
[0023] In addition, in the submount 20, the surface on which the laser diode bar 10 is mounted is called a first surface 20a, and the surface opposite to the first surface 20a in the Y direction is called a second surface 20b.
[0024] In addition, in members other than the laser diode bar 10 and the submount 20, the surface on which the laser diode bar 10 or the submount 20 is mounted is referred to as the upper surface, and the surface opposite to the upper surface in the Y direction is referred to as the lower surface.
[0025] The base 40 is a component having a cooling water passage 41 therein, and a second metal layer 50 is formed on the upper surface. The base 40 itself is made of, for example, insulating ceramics. When the laser module 100 is in operation, cooling water is circulated through the cooling water passage 41 by a circulation mechanism (not shown).
[0026] 1B, the submount 20 is joined to the second metal layer 50 via a second metal solder 70. The second metal solder 70 is an alloy solder containing silver (Ag), tin (Sn), and copper (Cu). However, the second metal solder 70 is not particularly limited thereto, and may be any material having a melting point lower than that of the first metal solder 60.
[0027] The submount 20 is a rectangular plate-shaped conductive member in a plan view, and is made of a metal, which is the main material, for example, a composite of copper and diamond. However, the material of the submount 20 is not particularly limited to this, and may be, for example, a composite of copper and tungsten (W). The main material constituting the submount 20 may be called the first material. In the above case, copper is the first material, and diamond or tungsten is the second material. In addition, the thermal conductivity of the first material is usually different from that of the second material, and in the case of a composite of copper and diamond, the thermal conductivity of copper is lower than that of diamond. On the other hand, in the case of a composite of copper and tungsten, the thermal conductivity of copper is higher than that of tungsten.
[0028] It goes without saying that if the submount 20 is a composite made of three types of materials, the submount 20 includes a third material.
[0029] Moreover, it is preferable that the submount 20 has a linear expansion coefficient close to that of the main semiconductor material constituting the laser diode bar 10 so as not to apply stress to the laser diode bar 10 .
[0030] As shown in FIG. 1B, the entire surface of the submount 20, that is, the first surface 20a, the second surface 20b, and the four side surfaces continuous with the first surface 20a and the second surface 20b, are covered with the first metal layer 30. However, from the viewpoint of ensuring bonding with other members, it is sufficient that at least the first surface 20a and the second surface 20b are covered with the first metal layer 30. The first metal layer 30 is a conductive film having a structure in which a first adhesion layer 31 and a first bonding layer 32 are laminated in this order on the surface of the submount 20. For example, the first adhesion layer 31 is made of platinum (Pt). The first bonding layer 32 is made of an alloy containing gold (Au) and another metal, for example, tin. Note that a first diffusion prevention layer (not shown) may be provided between the first adhesion layer 31 and the first bonding layer 32.
[0031] The laser diode bar 10 has multiple emitters 11 and is a rectangular member in plan view, with its long sides in the X direction and its short sides in the Z direction. The multiple emitters 11 are separated by separation grooves 12. The multiple emitters 11 are formed at intervals from one another along the X direction.
[0032] As shown in FIG. 1B, an n-side electrode 13 is formed on the lower surface of the laser diode bar 10. Although not shown, a p-side electrode 14 (see FIG. 8) is formed on the upper surface of each of the emitters 11. The p-side electrode 14 includes an ohmic electrode that makes ohmic contact with the upper surface of the emitter 11, and a bonding electrode (neither of which is shown) that covers the upper surface of the emitter 11 including the upper surface of the ohmic electrode and the separation groove 12 and is used for connection to the outside. The laser diode bar 10 shown in this embodiment is a so-called junction-up type in which the light-emitting point of the emitter 11 is on the upper surface side far from the submount 20, but is not particularly limited to this. It may also be a junction-down type (see FIG. 8) that will be described later.
[0033] Laser light in a predetermined wavelength range is emitted from each emitter 11 in the laser diode bar 10. The wavelength of the laser light is determined depending on the composition and layer thickness of an active layer (not shown) of the laser diode bar 10. Furthermore, the emission points of the laser light from each emitter 11 are located at the same height with the lower surface of the laser diode bar 10 as a reference.
[0034] The laser diode bar 10 is electrically connected to the submount 20 via the first metal solder 60 and the first metal layer 30. The first metal solder 60 is an alloy solder containing gold and tin. However, the first metal solder 60 is not particularly limited thereto, and any material having a melting point higher than that of the second metal solder 70 may be used.
[0035] Furthermore, the laser diode bar 10 is electrically connected to a second metal layer 50 provided on the upper surface of the base 40 via the submount 20 and the first metal layer 30. For example, by providing a connection electrode to an external power supply (not shown) on the upper surface of the second metal layer 50, the laser diode bar 10 can be electrically connected to the external power supply via the second metal solder 70, the first metal solder 60, the submount 20, and the first metal layer 30. When the second metal layer 50 is used as a type of electrical wiring, it is necessary to appropriately set the width in the X direction and the thickness in the Y direction of the second metal layer 50 in order to set the electrical resistance to a predetermined value or less.
[0036] [Laser module manufacturing method] FIG. 2A is a schematic diagram illustrating one manufacturing process of a laser module, FIG. 2B is a schematic diagram illustrating a process subsequent to the process shown in FIG. 2A, and FIG. 2C is a schematic diagram illustrating a process subsequent to the process shown in FIG. 2B.
[0037] As shown in Fig. 2A, a first metal solder 60 having a rectangular shape in plan view is provided on the first surface 20a of the submount 20 on which the first metal layer 30 is formed. Note that the submount 20 before the first metal solder 60 is provided has undergone steps (see Figs. 3 to 5) described later to reduce warping and surface irregularities. In plan view, one side of the first metal solder 60 coincides with the front side surface of the submount 20 on which the laser diode bar 10 is mounted, or is located a predetermined distance behind the front side surface.
[0038] Next, the laser diode bar 10 is prepared, aligned with the first metal solder 60, and then the laser diode bar 10 is placed on the upper surface of the first metal solder 60. At this time, the n-side electrode 13 of the laser diode bar 10 is abutted against the upper surface of the first metal solder 60. If the laser diode bar 10 is of the junction-down type (see FIG. 8), the p-side electrode 14 of the laser diode bar 10 is abutted against the upper surface of the first metal solder 60.
[0039] Furthermore, in this state, the submount 20 and the laser diode bar 10 are heated to bond them together via the first metal solder 60 .
[0040] Next, as shown in FIG. 2B, a second metal solder 70 having a rectangular shape in plan view is provided in a predetermined region on the upper surface of the base 40. In plan view, one side of the second metal solder 70 coincides with the front side surface of the base 40 on which the submount 20 is installed, or is located behind the front side surface with a predetermined gap. Furthermore, as shown in FIG. 2C, the second metal solder 70 is aligned, and then the submount 20 with the laser diode bar 10 bonded to the upper surface of the second metal solder 70 is installed. In this state, the submount 20 and the base 40 are heated, and the two are bonded via the second metal solder 70. In this way, the n-side electrode 13 of the laser diode bar 10 and the second metal layer 50 are electrically connected via the first metal solder 60, the submount 20, and the second metal solder 70.
[0041] 2C, the second metal layer 50 is electrically connected to an external power supply (not shown). Also, the p-side electrode 14 of the laser diode bar 10 is electrically connected to the external power supply.
[0042] If a cooling means for the laser diode bar 10 is separately prepared, the base 40 can be omitted in the laser module 100. In other words, the laser module 100 may be composed of the laser diode bar 10, the submount 20, and the first metal solder 60.
[0043] [Submount manufacturing method] Fig. 3 is a flow chart showing the manufacturing process of the submount. Fig. 4 is a schematic diagram explaining the warpage reduction process of the submount. Fig. 5 is a schematic diagram explaining the surface irregularity reduction process of the submount. Fig. 6 is a schematic cross-sectional view of the vicinity of the first surface of the submount before the warpage reduction process is performed. Fig. 7 is a schematic cross-sectional view of the vicinity of the first surface of the submount after the surface irregularity reduction process is performed.
[0044] Hereinafter, a method for manufacturing the submount 20 of this embodiment will be described with reference to FIGS.
[0045] First, the submount 20 having the first metal layer 30 formed on its surface is prepared (step S1), and the submount 20 is placed on the first mounting surface 211 of the first mounting table 210 (step S2).
[0046] 4, the first mounting base 210 has a recess 212 recessed inward from the first mounting surface 211. Therefore, the submount 20 is mounted on the first mounting base 210 with both longitudinal end portions abutting the first mounting surface. In this state, the center of the first surface 20a of the submount 20 protrudes upward, causing warping of the submount 20. The amount of warping of the submount 20 with respect to the first mounting surface 211 is denoted as L0.
[0047] Next, the first mounting table 210 is heated to a first temperature T1 (step S3). After heating, the roller 200 is brought into contact with the first surface 20a of the submount 20, and the roller 200 applies a first load G1 to the submount 20 to press it downward (step S4). The roller 200 is also moved back and forth along the longitudinal direction of the submount 20 to press the submount 20.
[0048] This reduces the warpage of the submount 20. The first temperature T1 (°C) and the first load G1 (kgf) are set appropriately depending on the material and thickness of the submount 20 and the amount of warpage L0. Steps S3 and S4 may be referred to as a warpage reduction process.
[0049] 4, the first surface 20a is the upper surface of the submount 20. Furthermore, with the center of the first surface 20a protruding upward, warping occurs in the submount 20. For this reason, with the roller 200 in contact with the first surface 20a of the submount 20, the roller 200 presses the submount 20 downward, thereby reducing the warping of the submount 20.
[0050] However, there may be cases where the center of the first surface 20a of the submount 20 protrudes downward, causing warping of the submount 20. In this case, the roller 200 is brought into contact with the second surface 20b of the submount 20 and presses the submount 20 downward with the roller 200. In this case, the second surface 20b is the upper surface of the submount 20. In this way, warping of the submount 20 can be reduced.
[0051] Next, the submount 20 is placed on the second mounting surface 221 of the second mounting table 220 (step S5).
[0052] As shown in FIG. 5, the second mounting surface 221 of the second mounting base 220 is a flat surface. After step 5 is performed, the submount 20 still has some warping. In this case, the amount of warping of the submount 20 based on the second mounting surface 221 is L1 (L1 <L0)とする。
[0053] Next, the second mounting table 220 is heated to a second temperature T2 (step S6). After heating, the roller 200 is brought into contact with the first surface 20a of the submount 20, and the roller 200 applies a second load G2 to the submount 20, pressing it downward (step S7). The roller 200 is also moved back and forth along the longitudinal direction of the submount 20 to press the submount 20. Note that steps S6 and S7 may be referred to as a surface irregularity reducing process.
[0054] As shown in Fig. 6, before the warpage reduction step is performed, the first metal layer 30 formed on the surface of the submount 20, particularly the surface of the first bonding layer 32, has irregularities, in other words, a predetermined surface roughness. Looking at the maximum peak height Sp, which is one of the parameters representing the surface roughness, the maximum peak height Sp1 of the first metal layer 30 shown in Fig. 6 is about several tens of µm. The maximum peak height Sp is a parameter representing the maximum value of the height of the convex portion in a region having irregularities.
[0055] On the other hand, the thickness of the first metal solder 60 is about several tens of μm to several hundreds of μm. Therefore, if the maximum peak height Sp1 on the surface of the first bonding layer 32 is about several tens of μm, a gap of a certain size will be generated between the first metal layer 30 and the first metal solder 60 when the first metal solder 60 is provided on the first surface 20a of the submount 20. If this gap remains as a void inside the first metal solder 60 when the submount 20 and the laser diode bar 10 are bonded, the void will hinder the dissipation of heat from the laser diode bar 10 to the submount 20 as described above.
[0056] 3 is performed to make the first bonding layer 32 easily deformable, and then step S7 is performed to reduce the surface unevenness of the submount 20, and more specifically, the surface unevenness of the first metal layer 30. In this manner, it is possible to prevent voids from remaining inside the first metal solder 60 when the submount 20 and the laser diode bar 10 are bonded. Note that the maximum peak height Sp is reduced to about several μm on the surface of the first bonding layer 32 shown in FIG.
[0057] The second temperature T2 (° C.) and the second load G2 (kgf) are appropriately set according to the material and thickness of the first bonding layer 32.
[0058] After the surface irregularity reducing step is performed, the warpage of the submount 20 is further reduced, and the warpage amount L2 of the submount 20 shown in FIG. 5 becomes smaller than the above-mentioned warpage amount L1.
[0059] By setting the amount of warpage L2 to a predetermined value, for example, 10 μm or less, the variation in height of the emission point of the laser light from each emitter of the laser diode bar 10 can be reduced to within an allowable range.
[0060] If it is desired to reduce the surface irregularities on the second surface 20b of the submount 20, the above-described surface irregularity reducing step may be performed on the second surface 20b of the submount 20.
[0061] In this case, it is possible to prevent voids from remaining inside the second metal solder 70 when the submount 20 and the base 40 are joined.
[0062] [Effects, etc.] As described above, the method for manufacturing the submount 20 according to this embodiment includes at least the first to fifth steps described below.
[0063] In a first step (step S1 in FIG. 3), a submount 20 having a first surface 20a and a second surface 20b opposing the first surface 20a in the Y direction is prepared.
[0064] In a second step (step S2 in FIG. 3), the submount 20 is placed on the first mounting surface 211 of the first mounting table 210.
[0065] In a third step (steps S3 and S4 in FIG. 3), the first mounting table 210 is heated to a first temperature T1, and a first load G1 is applied to the first surface 20a or the second surface 20b of the submount 20 to press it.
[0066] In a fourth step (step S5 in FIG. 3), the submount 20 is placed on the second mounting surface 221 of the second mounting table 220.
[0067] In a fifth step (steps S6 and S7 in FIG. 3), the second mounting table 220 is heated to a second temperature T2, and at least the first surface 20a of the submount 20 is pressed with a second load G2.
[0068] At least the first surface 20a and the second surface 20b of the submount 20 are covered with a first metal layer 30. The first metal layer 30 includes at least a first adhesion layer 31 in contact with at least the first surface 20a and the second surface 20b of the submount 20 and a first bonding layer 32 covering the first adhesion layer 31, and the first bonding layer 32 includes two or more types of metals.
[0069] In the third step, the warpage of the submount 20 in the longitudinal direction is reduced, and in the fifth step, the surface irregularities of the submount 20 including the first metal layer 30 are reduced.
[0070] According to this embodiment, the warpage of the submount 20 in the longitudinal direction can be reduced and the surface irregularities of the submount 20 including the first metal layer 30 can be reduced by the simple method of pressing the submount 20 in a heated state. The effects of reducing the warpage and the surface irregularities will be further described below.
[0071] When a laser diode bar 10 having multiple emitters 11 is used as a laser light source, a method of combining the laser beams emitted from each emitter 11 into one laser beam is often adopted in order to achieve high output. However, if the height of the emission point of the laser beam varies from emitter 11 to emitter 11, problems such as poor combination of the laser beams and complicated shapes of optical components arranged for combination occur. In this case, problems such as deterioration of the beam quality of the combined laser beam and increase in the cost of the laser device having the laser diode bar 10 occur.
[0072] According to this embodiment, by reducing the warpage of the submount 20 in the longitudinal direction, it is possible to suppress the warpage of the laser diode bar 10 mounted on the first surface 20a of the submount 20 via the first metal solder 60 in the longitudinal direction. This makes it possible to reduce the variation in height of the emission point of the laser light from each emitter 11 of the laser diode bar 10. Furthermore, it is possible to suppress the deterioration of the beam quality of the laser light obtained by combining the laser lights emitted from each emitter 11. In addition, it is possible to simplify the optical components for combining the laser lights, and it is possible to suppress the increase in the cost of the laser device having the laser diode bar 10.
[0073] Furthermore, according to this embodiment, by reducing the surface unevenness of the submount 20 including the first metal layer 30, it is possible to suppress the generation of gaps between the first metal layer 30 and the first metal solder 60 when the submount 20 and the laser diode bar 10 are joined. In addition, the size of the gaps can be reduced. This makes it possible to suppress the gaps from becoming voids and remaining inside the first metal solder 60 when the submount 20 and the laser diode bar 10 are joined. In addition, the size and density of the voids can be reduced.
[0074] As a result, the voids prevent heat from being discharged from the laser diode bar 10 to the submount 20, and heat buildup in the laser diode bar 10 during operation can be suppressed. This makes it possible to suppress a decrease in operational reliability during long-term use of the laser diode bar 10, and also to suppress fluctuations in the characteristics of the laser light emitted from each emitter 11 of the laser diode bar 10.
[0075] As a method for reducing the surface unevenness of the first bonding layer 32, for example, a method of polishing the surface of the first bonding layer 32 is considered. However, when the first bonding layer 32 contains multiple types of metals (gold and tin) as shown in this embodiment, the polishing speed differs depending on the type of metal. When this happens, the composition of the first bonding layer 32 becomes non-uniform in the plane and thickness direction.
[0076] When the first bonding layer 32 is heated to a predetermined temperature, it fuses with the first metal solder 60, bonding the first metal solder 60 to the submount 20. If the composition of the first bonding layer 32 is non-uniform, the fusion with the first metal solder 60 may not be successful in some areas, which may result in poor bonding between the first metal solder 60 and the submount 20, and ultimately poor bonding between the laser diode bar 10 and the submount 20.
[0077] On the other hand, according to this embodiment, the submount 20 is pressed while being heated, thereby reducing the surface irregularities of the first metal layer 30, and more specifically, the first bonding layer 32. This makes it possible to prevent the composition of the first bonding layer 32 from becoming non-uniform, and thus makes it possible to prevent poor bonding between the first metal solder 60 and the submount 20, and in turn, poor bonding between the laser diode bar 10 and the submount 20.
[0078] The submount 20 is a composite material including at least a first material as a main material and a second material, and the thermal conductivity of the first material is different from that of the second material. The first material is preferably a metal material having a specific electrical conductivity or less.
[0079] By using a composite material for the submount 20 and appropriately adjusting the compounding ratio of each material, it becomes easy to adjust the Young's modulus of the submount 20 and the linear expansion coefficient with the main semiconductor material constituting the laser diode bar 10. This makes it possible to suppress a decrease in the operational reliability of the laser diode bar 10 during long-term use, which is caused by thermal stress due to a difference in thermal expansion force being applied to the laser diode bar 10 during operation of the laser diode bar 10. In addition, it is possible to suppress fluctuations in the characteristics of the laser light emitted from each emitter 11 of the laser diode bar 10.
[0080] Furthermore, by adjusting the types and compounding ratios of the materials constituting the submount 20, the thermal conductivity of the submount 20 can be increased to a predetermined level or higher, and the heat dissipation properties of the submount 20 can be improved.
[0081] The first material is preferably a material having a Young's modulus that is large enough to deform the submount 20 when the first load G1 is applied to the submount 20. Taking into consideration the requirement for electrical conductivity, the first material is preferably copper or a copper alloy.
[0082] Moreover, it is preferable that a recess 212 is provided on the first mounting surface 211 of the first mounting base 210. In this case, in the second step, the submount 20 is mounted on the first mounting surface 211 so as to cover the recess 212.
[0083] By providing the recess 212 in the first mounting surface 211, the center of the submount 20 in the longitudinal direction is not prevented from deforming downward when the submount 20 is pressed downward in the second step. This makes it possible to reliably reduce warpage of the submount 20 in the longitudinal direction.
[0084] If the second mounting surface 221 of the second mounting stand 220 is flat, when the submount 20 is pressed downward in the fifth step, the entire submount 20 is pressed against the second mounting surface 221, and no part of the submount 20 is displaced downward. In other words, the second load G2 is applied to the entire surface of the first metal layer 30 without escaping, so that the surface unevenness can be reduced over the entire first metal layer 30.
[0085] The method for manufacturing the laser module 100 according to this embodiment includes at least the sixth to ninth steps described below.
[0086] In the sixth step, the submount 20 is fabricated by sequentially carrying out the first to fifth steps described above.
[0087] In the seventh step, after the sixth step is performed, a first metal solder 60 is provided in a predetermined area on the first surface 20a of the submount 20.
[0088] In the eighth step, the laser diode bar 10 is prepared. The laser diode bar 10 is provided with a plurality of emitters 11 along its longitudinal direction.
[0089] In the ninth step, the laser diode bar 10 is placed on the upper surface of the first metal solder 60 after being aligned with the first metal solder 60. Furthermore, in this state, the submount 20, the first metal solder 60, and the laser diode bar 10 are heated to a predetermined temperature, and the submount 20 and the laser diode bar 10 are joined via the first metal solder 60.
[0090] In this way, the warp in the longitudinal direction of the submount 20 can be reduced, and the surface irregularities of the submount 20 including the first metal layer 30 can be reduced. This can suppress the deterioration of the beam quality of the laser light obtained by combining the laser lights emitted from the emitters 11. In addition, the optical components for combining the laser lights can be simplified, and the cost increase of the laser device having the laser diode bar 10 can be suppressed. In addition, the generation of voids in the first metal solder 60 interposed between the laser diode bar 10 and the submount 20 can be suppressed. This can suppress the voids from hindering the heat dissipation from the laser diode bar 10 to the submount 20, and suppress the deterioration of the operational reliability of the laser diode bar 10 during long-term use. In addition, the characteristics of the laser light emitted from each emitter 11 of the laser diode bar 10 can be suppressed from fluctuating.
[0091] The method for manufacturing the laser module 100 of this embodiment may further include a tenth step and an eleventh step described below.
[0092] In the tenth step, second metal solder 70 is provided in a predetermined area on the surface of base 40 .
[0093] In an eleventh step, the submount 20 to which the laser diode bar 10 is bonded is placed on the upper surface of the second metal solder 70 after being aligned with the second metal solder 70. Furthermore, in this state, the submount 20 to which the laser diode bar 10 is bonded, the second metal solder 70, and the base 40 are heated to a predetermined temperature, and the submount 20 and the base 40 are bonded via the second metal solder 70.
[0094] By providing the tenth and eleventh steps, the submount 20 to which the laser diode bar 10 is bonded can be bonded and fixed to the base 40. This makes it possible to reliably fix the positions of the submount 20 and, in turn, the laser diode bar 10.
[0095] Furthermore, as shown in this embodiment, when the base 40 is a cooler, the heat generated in the laser diode bar 10 during operation can be discharged to the outside of the laser module via the first metal solder 60, the submount 20, and the second metal solder 70. This makes it possible to suppress a decrease in the operational reliability of the laser diode bar 10 during long-term use. Also, it is possible to suppress a fluctuation in the characteristics of the laser light emitted from each emitter 11 of the laser diode bar 10.
[0096] If a cooling means for the laser diode bar 10 is separately prepared, the base 40 can be omitted in the laser module 100. In other words, the laser module 100 may be composed of the laser diode bar 10, the submount 20, and the first metal solder 60.
[0097] The base 40 may be made of a metal such as stainless steel. In that case, it is necessary to electrically insulate the base 40 and the submount 20 except for the second metal layer 50. It is also necessary to ensure electrical insulation between the cooling water flowing through the cooling water passage 41 and the base 40. The base 40 may be cooled by contacting a cooling water pipe with the back surface or side surface of the base 40. In that case, the internal cooling water passage 41 is omitted.
[0098] Furthermore, in this embodiment, an example has been shown in which the submount 20 is pressed using the rollers 200, but the mechanism for pressing the submount 20 is not particularly limited to this. EXAMPLES
[0099] Fig. 8 is a schematic cross-sectional view of a laser module according to an embodiment. Fig. 9 is an ultrasonic inspection photograph of a laser module according to a comparative example. Fig. 10 is an ultrasonic inspection photograph of a laser module according to an embodiment. Note that in the laser module 100 according to the comparative example and the embodiment, the base 40 and the second metal solder 70 are omitted. Also, for convenience of explanation, only the first metal solder 60 is shown in Figs. 9 and 10.
[0100] <Common structure> The laser module 100 shown in Fig. 8 differs from the laser module 100 of the embodiment shown in Fig. 1B in that the laser diode bar 10 is of a junction-down type. That is, the laser diode bar 10 and the submount 20 are joined via the first metal solder 60 with the p-side electrode 14 of the laser diode bar 10 in contact with the upper surface of the first metal solder 60. This structure is the same in the comparative example.
[0101] The submount 20 is a composite material of copper and diamond, and has a length in the longitudinal direction, i.e., the X direction, of 11 mm, a width in the Z direction of 4.5 mm, and a thickness in the Y direction of 0.3 μm, including the thickness of the first metal layer 30.
[0102] The first adhesive layer 31 in the first metal layer 30 is made of platinum, and the first bonding layer 32 is a gold-tin alloy layer. The average thickness of the first bonding layer 32 is about 5 μm to 7 μm. The first metal solder 60 is a gold-tin alloy solder.
[0103] The main semiconductor material constituting the laser diode bar 10 is a nitride semiconductor (GaN-based semiconductor). Laser light in the blue wavelength range is emitted from each emitter 11. The "blue wavelength range" refers to a wavelength range of 350 nm or more and 460 nm or less.
[0104] <Example> The steps shown in Fig. 3 were sequentially performed on the submount 20 having the first metal layer 30 formed on the surface. At this time, the first temperature T1 was 250 (°C), and the first load G1 was 50 (kgf). The second temperature T2 was 250 (°C), and the second load G2 was 50 (kgf).
[0105] In addition, the amount of warping L0 before step S1 shown in FIG. 3 was performed and the amount of warping L1 after step S4 was performed were each measured using a three-dimensional optical surface shape / roughness measuring device.
[0106] In addition, the surface irregularities of the submount 20 after step S7 was performed were measured using a three-dimensional optical surface shape / roughness measuring device, and the maximum peak height Sp2 was obtained from the results.
[0107] The amounts of warpage L0 and L1 are values in the state shown in Fig. 4. The maximum peak height Sp2 is a value in the state shown in Fig. 7.
[0108] Next, a first metal solder 60 having a rectangular shape in a plan view was provided on the first surface 20a of the submount 20, and after alignment with the first metal solder 60, the laser diode bar 10 was placed on the surface of the first metal solder 60. Furthermore, in this state, the submount 20, the first metal solder 60, and the laser diode bar 10 were heated to 250°C, and then cooled to room temperature.
[0109] Thereafter, the laser module 100 was inspected using an ultrasonic flaw detector, and the state of voids generated in the first metal solder 60 was evaluated.
[0110] <Comparative Example> A submount 20 was prepared, with a first metal layer 30 formed on the surface thereof. However, unlike the example, the steps shown in FIG.
[0111] The amount of warpage L0 in this state was measured using a three-dimensional optical surface profile / roughness measuring instrument. The surface irregularities of the submount 20 were also measured using the three-dimensional optical surface profile / roughness measuring instrument, and the maximum peak height Sp1 was calculated from the results.
[0112] The amount of warpage L0 is a value in the state shown in FIG. 4. The maximum peak height Sp1 is a value in the state shown in FIG.
[0113] Next, a first metal solder 60 having a rectangular shape in a plan view was provided on the first surface 20a of the submount 20, and after alignment with the first metal solder 60, the laser diode bar 10 was placed on the surface of the first metal solder 60. Furthermore, in this state, the submount 20, the first metal solder 60, and the laser diode bar 10 were heated to 250°C, and then cooled to room temperature.
[0114] Thereafter, the laser module 100 was inspected using an ultrasonic flaw detector, and the state of voids generated in the first metal solder 60 was evaluated.
[0115] <Comparison of evaluation results between Examples and Comparative Examples> First, the amount of warping L0 in the example and comparative example was 60 μm, while the amount of warping L1 in the example was 20 μm. In other words, by carrying out the warping reduction step, the amount of warping of the submount 20 could be reduced to ⅓.
[0116] In addition, the maximum peak height Sp1 in the comparative example was 27 μm, whereas the maximum peak height Sp2 in the example was 4.6 μm. In other words, by carrying out the surface irregularity reducing step, the maximum peak height of the submount 20, in other words, the first metal layer 30, could be reduced to ⅕ or less.
[0117] Also, the number of white spots in the ultrasonic inspection photographs was significantly reduced in the case shown in Fig. 10 compared to the case shown in Fig. 9. The white spots in Fig. 9 and Fig. 10 are presumed to be the locations where voids have occurred. In other words, it was found that the number of voids that have occurred inside the first metal solder 60 interposed between the laser diode bar 10 and the submount 20 was significantly reduced in the example compared to the comparative example. [Industrial Applicability]
[0118] The submount manufacturing method disclosed herein can reduce warping of the submount and suppress the occurrence of voids in the metal solder interposed between the submount and the laser diode bar, and is therefore useful in achieving higher output and higher reliability of the laser diode bar mounted on the submount. [Explanation of symbols]
[0119] 10 Laser Diode Bar 11 Emitter 12 Separation groove 13 n-side electrode 14 p side electrode 20 Submount 20a Page 1 20b 2nd side 30 1st metal layer 31 First adhesive layer 32 1st bonding layer 40 Base 41 Cooling Channel 50 Second metal layer 60 First metal solder 70 Second metal solder 100 Laser Module 200 Roller 210 1st installation stand 211 1st installation surface 212 Recess 220 2nd installation stand 221 2nd installation surface
Claims
1. A first step of preparing a submount having a first surface and a second surface opposed to the first surface in a thickness direction; a second step of mounting the submount on a first mounting surface of a first mounting table; a third step of heating the first mounting table to a first temperature and applying a first load to the first surface or the second surface of the submount to press the first surface or the second surface of the submount; a fourth step of mounting the submount on a second mounting surface of a second mounting table after the third step is performed; and a fifth step of heating the second mounting table to a second temperature and applying a second load to at least the first surface of the submount to press the submount, At least the first surface and the second surface of the submount are covered with a first metal layer; the first metal layer includes at least a first adhesion layer in contact with at least the first surface and the second surface of the submount and a first bonding layer covering the first adhesion layer; A method for manufacturing a submount, wherein the first bonding layer contains two or more types of metals.
2. 2. The method for manufacturing a submount according to claim 1, In the third step, a warpage of the submount in a longitudinal direction is reduced; The method for manufacturing a submount, wherein the fifth step reduces surface unevenness of the submount including the first metal layer.
3. 2. The method for manufacturing a submount according to claim 1, the submount is a composite material including at least a first material as a main material and a second material, A method for manufacturing a submount, wherein the thermal conductivity of the first material is different from the thermal conductivity of the second material.
4. 2. The method for manufacturing a submount according to claim 1, The first mounting surface is provided with a recess, while the second mounting surface is flat; In the second step, the submount is mounted on the first mounting surface so as to cover the recess.
5. a sixth step of fabricating the submount by using the method for manufacturing the submount according to any one of claims 1 to 4; a seventh step, after performing the sixth step, of providing a first metal solder on the first surface of the submount; an eighth step of providing a laser diode bar having a plurality of emitters disposed along a longitudinal direction of the laser diode bar; and a ninth step of placing the laser diode bar on an upper surface of the first metal solder after aligning the submount with the first metal solder, and joining the submount and the laser diode bar.
6. 6. The method for manufacturing a laser module according to claim 5, a tenth step of providing a second metal solder on a surface of the base; a step 11 of placing the submount to which the laser diode bar is joined on an upper surface of the second metal solder after aligning the second metal solder with the upper surface of the second metal solder, and joining the submount to the base.
Citation Information
Patent Citations
Heatsink and power module
JP2005175006A
Aluminum-diamond composite and method for producing the same
WO2010007922A1