Method for producing wax solution
A simple propeller-type stirrer-based method for producing wax solution liquid with smaller particles addresses the need for cost-effective and safer manufacturing, enhancing its industrial applicability across diverse fields.
Patent Information
- Application Number
- JP2023086440
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing water-based wax emulsions require specialized equipment like pressure vessels, homomixer-type stirrers, and chiller water, limiting their applicability and necessitating a simpler manufacturing method for smaller wax particles to expand their use in various industrial applications.
A method using two production tanks and a simple propeller-type stirrer to produce a wax solution liquid with oxidized polyethylene wax, nonionic and anionic surfactants, alkanolamine, and water, without requiring homogenizers or chillers, by heating and mixing the raw materials in separate tanks before combining and cooling.
Enables the production of a wax solution liquid with smaller particle sizes using basic equipment, reducing costs, maintaining worker safety, and expanding its applicability to industries like cosmetics and lubrication without affecting product appearance.
Smart Images

Figure 2024169185000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a wax solution having smaller wax particles than a wax emulsion using only simple production equipment. [Background technology]
[0002] The production of a water-based wax emulsion liquid requires special production equipment such as a pressure vessel, a homomixer-type agitator, a homogenizer-type agitator, and chiller water for cooling, so there has been a demand for a simple production method that does not require such special production equipment.
[0003] Furthermore, in order to expand the range of applications beyond that of existing wax emulsions, there was a demand for the commercialization of a wax solution with smaller wax particles than those of wax emulsions.
[0004] Patent Document 1 discloses a method for producing an aqueous wax emulsion by using polyethylene wax as a main raw material and a high-pressure homogenizer.
[0005] Furthermore, Patent Document 2 discloses a method for producing a wax emulsion for toner by using various waxes as raw materials, subjecting them to homogenization while stirring with a homomixer, and cooling with cold water.
[0006] Patent Document 3 discloses a method for producing a soap-free wax emulsion by first crudely emulsifying oxidized wax and a basic substance using a phase inversion method, and then using a high-speed homomixer and a high-pressure homogenizer.
[0007] Patent Document 4 discloses a method for producing a wax emulsion by softening wax and using a dispersant consisting of a saponified emulsion polymer of an anionic unsaturated monomer, a hydrophobic unsaturated monomer, and an unsaturated monomer copolymerizable therewith, and using a mixing high-pressure discharge type emulsifier or homogenizer.
[0008] The methods disclosed in the above patent documents require a homomixer-type agitator, a homogenizer-type agitator, and a special cooling device for obtaining cold water when producing a wax emulsion, and do not mention the production of a wax solution liquid having a smaller wax particle size than that of a wax emulsion liquid. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent Publication No. 2002-69302 [Patent Document 2] Patent Publication No. 2014-106474 [Patent Document 3] Patent Publication No. 2003-147088 [Patent Document 4] Patent Publication No. 2002-308994 Summary of the Invention [Problem to be solved by the invention]
[0010] Water-based wax emulsion liquids are used in many industrial fields, such as cosmetic bases, floor polishes, lubricants, release agents, anti-agglomeration agents, fabric softeners, and thickeners. However, their production requires special production equipment, such as pressure vessels, homomixer-type agitators, homogenizer-type agitators, and chiller water for cooling. Therefore, a simple production method that does not require such special production equipment is required.
[0011] Furthermore, in order to expand the range of applications beyond that of existing wax emulsions, there is a demand for the commercialization of wax solutions with smaller wax particles than those of wax emulsions.
[0012] In order to produce a water-based wax solution, which has a wider range of applications than existing wax emulsions, using only simple manufacturing equipment, it is necessary to select optimal raw materials and establish optimal manufacturing conditions. [Means for solving the problem]
[0013] In order to solve the above problems, the present inventors have selected optimal raw materials and established optimal manufacturing conditions, and have completed the present invention. That is, the present invention relates to a method for producing a wax solution liquid using the following simple manufacturing equipment.
[0014] [1] A method for producing a water-based wax solution that can be carried out using only two production tanks and a simple propeller stirrer.
[0015] [2] A method for producing a wax solution liquid according to [1], using as raw materials (A) oxidized polyethylene wax, (B) a nonionic surfactant, (C) an anionic surfactant, (D) an alkanolamine, and (E) water.
[0016] [3] The method for producing a wax solution liquid described in [2], wherein the nonionic surfactant is one or more types selected from the group consisting of alcohol ether type, polyoxyalkylene glycol type, fatty acid ester type, alkanolamide type, polyether amine type, and polyoxyalkylene alkyl amine type.
[0017] [4] The method for producing a wax solution liquid described in [2] or [3], wherein the anionic surfactant is one or more types selected from the group consisting of carboxylic acid type, sulfonate type, and sulfate type.
[0018] [5] A process of adding the raw materials (A) oxidized polyethylene wax, (B) nonionic surfactant, and (C) anionic surfactant to a production tank 1 and mixing them while heating with a simple propeller-type agitator; A step of adding raw materials (D) alkanolamine and (E) water to a production tank 2 and mixing them while heating them with a simple propeller-type agitator; A step of pouring the raw materials mixed in the manufacturing tank 1 into the manufacturing tank 2; A method for producing a wax solution comprising: Effect of the Invention
[0019] The wax solution liquid manufacturing method of the present invention makes it possible to manufacture wax solution liquid using simple manufacturing equipment without using special manufacturing equipment such as pressure vessels, homomixer-type agitators, homogenizer-type agitators, or chiller water for cooling, thereby making it possible to keep manufacturing equipment costs and equipment maintenance costs low.
[0020] Furthermore, the wax solution liquid manufacturing method of the present invention makes it possible to manufacture wax solution liquid using simple manufacturing equipment, thereby reducing the burden on manufacturing workers, such as "danger," "hard work," and "dirtiness."
[0021] Furthermore, in the method for producing a wax solution of the present invention, raw materials that are easy to procure are selected, so there is less concern about raw material procurement, and problems such as delays in product supply can be alleviated. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic diagram of a manufacturing facility of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The method for producing a wax solution liquid of the present invention uses only two production tanks and a simple propeller-type agitator. Here, the simple propeller-type agitator means a propeller-type agitator that is not a special agitator such as a homomixer type or a homogenizer type, and does not use blades with a special shape. The production tank 1 is used to heat and dissolve the raw materials, and the production tank 2 is used to mix the raw materials heated and dissolved in the production tank 1 with water. Therefore, it is necessary to install piping to send the raw materials from the production tank 1 to the production tank 2.
[0024] A simple propeller-type agitator is installed in each of the two manufacturing tanks to dissolve the raw materials evenly.
[0025] Manufacturing tank 1 is equipped with a heating device for heating and dissolving the raw materials, and manufacturing tank 2 is equipped with a heating device for heating and dissolving the raw materials and a simple cooling device such as a cooling pipe that uses industrial water to cool the product.
[0026] First, the raw materials (A) oxidized polyethylene wax, (B) nonionic surfactant, and (C) anionic surfactant are charged into manufacturing tank 1, and while heating to 130°C to 150°C, they are stirred and dissolved using a simple propeller stirrer. (Process in manufacturing tank 1)
[0027] Simultaneously with the process in manufacturing tank 1, raw materials (D) alkanolamine and (E) water are added to manufacturing tank 2, and while heating to 80°C to 90°C, they are stirred and dissolved using a simple propeller stirrer. (Process in manufacturing tank 2)
[0028] After the raw materials put into manufacturing tanks 1 and 2 are uniformly dissolved, the raw materials from manufacturing tank 1 are put into manufacturing tank 2. At this time, stirring is continued in manufacturing tank 2. Also, at this time, if the raw materials in manufacturing tank 2 foam significantly, a defoaming agent, which is also a raw material, can be added.
[0029] The raw materials in manufacturing tank 1 are poured into manufacturing tank 2, and after the liquid in manufacturing tank 2 becomes uniform, cooling begins using a cooling pipe that uses ordinary industrial water.
[0030] After the liquid temperature has been cooled to below 50°C, the raw material (E) water is added and the volume of the liquid is adjusted to produce the product.
[0031] As the (A) oxidized polyethylene wax, those called oxidized type or acid-modified type can be used, such as the Hiwax series (Mitsui Chemicals, Inc.), the NPS (registered trademark) series (Nippon Seiro Co., Ltd.), the Sanwax (registered trademark) series (Sanyo Chemical Industries, Ltd.), and the AC series (Honeywell International, Inc.).
[0032] The content of the oxidized polyethylene wax (A) in the wax solution of the present invention is preferably 1 to 30 mass %, and more preferably 10 to 20 mass %, when the total mass of the wax solution is taken as 100 mass %.
[0033] If the content of (A) oxidized polyethylene wax is less than 1% by mass, the wax solution may not be sufficiently effective. If the content of (A) oxidized polyethylene wax is more than 30% by mass, it may become difficult to ensure the stability of the solution.
[0034] As the (B) nonionic surfactant, alcohol ether type, polyoxyalkylene glycol type, fatty acid ester type, alkanolamide type, polyether amine type, polyoxyalkylene alkyl amine type, etc. can be used.
[0035] For example, commercially available alcohol ether products include Noigen (registered trademark) (Dai-ichi Kogyo Seiyaku Co., Ltd.) and Braunon (registered trademark) (Aoki Oil Industry Co., Ltd.); commercially available polyoxyalkylene glycol products include Epan (registered trademark) (Dai-ichi Kogyo Seiyaku Co., Ltd.), Pronon (registered trademark) (NOF Corporation), and Newpol (registered trademark) (Sanyo Chemical Industries Co., Ltd.); commercially available fatty acid ester products include Nonion (NOF Corporation) and Ionet (registered trademark) (Sanyo Chemical Industries Co., Ltd.); commercially available alkanolamide products include Stahome (registered trademark) (NOF Corporation) and Takesurf (registered trademark) (Takemoto Oil Industry Co., Ltd.); commercially available polyoxyalkylene alkylamine products include Braunon (registered trademark) (Aoki Oil Industry Co., Ltd.) and Puremeal (registered trademark) (Sanyo Chemical Industries Co., Ltd.), and the like.
[0036] The content of the nonionic surfactant (B) in the wax solution of the present invention is preferably 0.5 to 10 mass %, and more preferably 1 to 5 mass %, when the total mass of the wax solution is taken as 100 mass %.
[0037] (B) If the content of the nonionic surfactant is less than 0.5% by mass, the effect of turning the polyethylene wax into a solution may not be fully exerted. On the other hand, if the content exceeds 10% by mass, secondary problems such as excessive foaming may occur, making it difficult to prepare the wax solution.
[0038] As the (C) anionic surfactant, a carboxylic acid type, a sulfonate type, a sulfate type, etc. can be used.
[0039] For example, commercially available carboxylate-type products include Viewlite (registered trademark) (Sanyo Chemical Industries, Ltd.) and Nonsal (registered trademark) (NOF Corporation), commercially available sulfonate-type products include Takesurf (registered trademark) (Takemoto Oil Co., Ltd.) and Sulfol (registered trademark) (MORESCO Corporation), and a commercially available sulfate-type product includes Sandet (registered trademark) (Sanyo Chemical Industries, Ltd.), etc.
[0040] The content of the anionic surfactant (C) in the wax solution of the present invention is preferably 1 to 20 mass %, and more preferably 1 to 10 mass %, when the total mass of the wax solution is taken as 100 mass %.
[0041] (C) If the content of the anionic surfactant is less than 1% by mass, the effect of turning the polyethylene wax into a solution may not be fully exerted. On the other hand, if the content of the anionic surfactant exceeds 20% by mass, it becomes difficult to ensure the stability of the wax solution, and there is a risk of separation of the original solution or cloudiness of the original solution.
[0042] (D) Examples of alkanolamines that can be used include monoethanolamine, diglycolamine, monoisopropanolamine, 2-amino-2-methylpropanol, diethanolamine, diisopropanolamine, N-methylethanolamine, N-ethylethanolamine, 2-(butylamino)ethanolamine, 2-((1-methylpropyl)amino)ethanol, triethanolamine, and triisopropanolamine.
[0043] The content of the (D) alkanolamine in the wax solution of the present invention is an amount that allows the wax solution to have a set pH.
[0044] (E) Water that can be used includes industrial water, tap water, distilled water, ion-exchanged water, pure water, and the like.
[0045] The content of water (E) in the wax solution liquid of the present invention is preferably 50 to 90% by mass, and more preferably 60 to 80% by mass, taking into consideration performance and liquid stability, when the total mass of the wax solution liquid is 100% by mass.
[0046] In addition to the above components, additives such as preservatives and antifoaming agents may be added to the wax solution of the present invention, if necessary. EXAMPLES
[0047] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to these examples.
[0048] In addition, the example produced is judged to be a wax solution liquid rather than a wax emulsion liquid because the liquid is transparent and objects and patterns behind it can be seen through the liquid, and the average particle size of the liquid is considered to be approximately 0.1 μm or less.
[0049] The wax solution of the present invention was prepared on a laboratory scale by mixing the components shown in Table 1 and following the procedure below.
[0050] (A) oxidized polyethylene wax, (B) nonionic surfactant a, and (C) anionic surfactant are placed in container 1, and then heated to 130°C to 150°C using a simple propeller stirrer while stirring until completely dissolved.
[0051] (D) Triethanolamine, which is an alkanolamine, and (E) water are placed in container 2, and completely dissolved while heating to 80° C. to 90° C. using a simple propeller stirrer.
[0052] After the raw materials charged into vessel 1 and vessel 2 are uniformly dissolved at a predetermined temperature, the raw materials from vessel 1 are gradually charged into vessel 2. At this time, the mixture in manufacturing tank 2 is kept stirred.
[0053] After the liquid in vessel 2 becomes uniform, cooling is started, and after the liquid temperature falls to 50° C. or below, the raw material (E) water is added and the volume of the liquid is adjusted. Comparative Example 1 contained a different nonionic surfactant a from that in the examples, Comparative Example 2 contained a different amount of surfactant, and Comparative Example 3 contained a commercially available wax emulsion liquid MGP 055 (manufactured by Maruyoshi Chemical Industry Co., Ltd.).
[0054] [Manufacturing method] When producing the wax solution liquid of the present invention as a product, the equipment shown in FIG. 1 was used and the following procedure was followed.
[0055] (A) Oxidized polyethylene wax, (B) nonionic surfactant, and (C) anionic surfactant are charged into manufacturing tank 1 (volume 600 L) and stirred at 130°C to 150°C using a simple propeller stirrer (Shimazaki Manufacturing Co., Ltd., 1.5 kW, 360 rpm, propeller 200 φ mm) until completely dissolved. At this time, heating is performed using steam heating piping installed in manufacturing tank 1.
[0056] Simultaneously with the process in manufacturing tank 1, (D) triethanolamine, which is an alkanolamine, and (E) water are added to manufacturing tank 2 (volume 1,200 L) and stirred at 80°C to 90°C using a simple propeller mixer (manufactured by Satake Chemical Machinery Co., Ltd., 3.7 KW, 360 rpm, propeller 350 φ mm) until completely dissolved. At this time, heating is performed using steam heating piping installed in manufacturing tank 2.
[0057] After the raw materials put into manufacturing tanks 1 and 2 are uniformly dissolved at a specified temperature, the raw materials from manufacturing tank 1 are put into manufacturing tank 2. At this time, the raw materials in manufacturing tank 2 are kept stirred. Also, at this time, if the raw materials in manufacturing tank 2 foam significantly, a defoaming agent, which is also a raw material, can be added.
[0058] The raw materials in manufacturing tank 1 are poured into manufacturing tank 2, and after the liquid in manufacturing tank 2 becomes uniform, cooling using normal industrial water is started through the cooling pipes. At that time, heating is stopped.
[0059] After the liquid temperature drops below 50°C, the raw material (E) water is added and the volume of the liquid is adjusted to produce the product.
[0060] [Table 1] Liquid stability: If there is no separation of the liquid and no floating or settling of some components, it is marked as "○". If there is floating or settling of some components, it is marked as "×". Appearance: If the pattern behind the liquid can be clearly seen, it is rated as "transparent." If it can be seen but not clearly, it is rated as "semi-transparent." If it cannot be seen, it is rated as "cloudy." [Industrial Applicability]
[0061] Existing wax emulsion liquids are used in many industrial fields, such as cosmetic bases, floor polishes, lubricants for machine sliding surfaces, surface protectors for machine parts, anti-agglomeration agents, fabric softeners, and thickeners. However, the wax solution liquid of the present invention has a transparent appearance, and can impart the performance of wax to the products to which it is added while minimizing the impact on the appearance, making it suitable for use in a wider range of products than existing wax emulsion liquids.
Claims
1. A method for producing a water-based wax solution that can be carried out using only two production tanks and a simple propeller stirrer.
2. The method for producing a wax solution liquid according to claim 1, wherein the raw materials used are (A) oxidized polyethylene wax, (B) a nonionic surfactant, (C) an anionic surfactant, (D) an alkanolamine, and (E) water.
3. The method for producing a wax solution liquid according to claim 2, wherein the nonionic surfactant is one or more types selected from the group consisting of alcohol ether type, polyoxyalkylene glycol type, fatty acid ester type, alkanolamide type, polyether amine type, and polyoxyalkylene alkyl amine type.
4. 4. The method for producing a wax solution liquid according to claim 2 or 3, wherein the anionic surfactant is one or more types selected from the group consisting of carboxylic acid type, sulfonate type, and sulfate type anionic surfactants.
5. A step of adding raw materials (A) oxidized polyethylene wax, (B) a nonionic surfactant, and (C) anionic surfactant to a production tank 1 and mixing them while heating with a simple propeller type agitator; A step of adding (D) an alkanolamine and (E) water to a production tank 2 and mixing them while heating with a simple propeller type agitator; A step of pouring the raw materials mixed in the production tank 1 into the production tank 2; A method for producing a wax solution comprising:
Citation Information
Patent Citations
Method for preparing oxidic polyethylene wax microemulsion
CN101289540A
Microemulsion composite of polyethylene wax oxide
CN101942152A
Method for preparing modified magnesium hydroxide flame retardant
CN103965656A
Multifunctional lubricant and preparation method and application thereof
CN112500532A
Aqueous emulsion composition of acid-modified polyolefin
JP2015078331A