Optical element, optical system, imaging apparatus, and method for manufacturing optical element

The optical element with a three-layer antireflection film, composed of organic compounds with specific refractive indices and thickness ratios, addresses film unevenness and refractive index mismatches, ensuring consistent antireflection performance across different base materials.

JP2024169306AActive Publication Date: 2024-12-05CANON KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024039020
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-03-13
Publication Date
2024-12-05
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

Existing anti-reflection films on optical elements, particularly those with a first layer containing alumina, suffer from film unevenness and insufficient antireflection performance due to the refractive index mismatch between the base material and the second layer, leading to reduced reflectance across the lens surface.

Method used

An optical element with a base material and an antireflection film comprising three layers, each containing an organic compound, where the third layer has a refractive index of 1.10 ≤ n3 ≤ 1.28, and specific thickness ratios and ranges are maintained to ensure uniform antireflection performance regardless of the base material's refractive index.

Benefits of technology

The solution effectively reduces reflectance across the optical element, maintaining high antireflection performance even with varying base material refractive indices, thereby improving optical clarity and reducing flare and ghosting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169306000001_ABST
    Figure 2024169306000001_ABST
Patent Text Reader

Abstract

To provide an optical element that can sufficiently reduce its reflectance regardless of the refractive index of a base material.SOLUTION: An optical element (300) has a base material (200) and an anti-reflection film (100). The anti-reflection film comprises a first layer (01) formed on the base material, a second layer (02) formed on the first layer, and a third layer (03) formed on the second layer. The first to third layers each include an organic compound. When the refractive index of the third layer at a wavelength of 550 nm is defined as n3, the conditional expression of 1.10≤n3≤1.28 is satisfied.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical element, an optical system, an imaging device, and a method for manufacturing an optical element. [Background technology]

[0002] In order to prevent flare and ghosting caused by unnecessary reflection, dielectric multilayer films (anti-reflection films) with anti-reflection properties are often formed on the surfaces of optical elements such as lenses and filters in optical systems. If a material with a low refractive index is used for the top layer of an anti-reflection film, high anti-reflection performance can be obtained. As materials with a low refractive index, inorganic materials such as silica and magnesium fluoride, and organic materials such as silicon resin and amorphous fluororesin are known to be used. The refractive index of these materials can be reduced by forming voids within the layer.

[0003] Patent Document 1 discloses an antireflection coating having a two-layer structure composed of a first layer mainly composed of alumina and a second layer which is a silica aerogel having a refractive index of 1.27, which is formed on a substrate having a refractive index of 1.70 to 1.95. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-162989 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the anti-reflection coating disclosed in Patent Document 1 has a first layer mainly composed of alumina formed by vapor deposition. Therefore, in a large aperture lens, film unevenness occurs within the lens surface, and the anti-reflection performance (reduction of reflectance) is insufficient over the entire lens surface. In addition, since the refractive index of the second layer, which is the uppermost layer, is about 1.27, the anti-reflection performance is insufficient when a substrate with a lower refractive index is used.

[0006] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide an optical element capable of sufficiently reducing the reflectance regardless of the refractive index of the substrate. [Means for solving the problem]

[0007] An optical element according to one aspect of the present invention is an optical element having a substrate and an antireflection coating, the antireflection coating comprising a first layer formed on the substrate, a second layer formed on the first layer, and a third layer formed on the second layer, each of the first to third layers containing an organic compound, wherein n3 is a refractive index of the third layer at a wavelength of 550 nm, 1.10≦n3≦1.28 The following condition is satisfied.

[0008] Other objects and features of the present invention are illustrated in the following examples. Effect of the Invention

[0009] According to the present invention, it is possible to provide an optical element capable of sufficiently reducing the reflectance regardless of the refractive index of the substrate. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram of optical elements in Examples 1 to 14. [Diagram 2] 1 is a schematic cross-sectional view of optical elements in Examples 1, 2, 5, 7, 8, 11, and 13 and Comparative Examples 1 and 2. [Diagram 3] 1 is a schematic cross-sectional view of the optical elements in Examples 3, 4, 6, 9, 10, 12, and 14. [Figure 4] 13 shows reflectance characteristics at position C of the optical element in Example 1 at angles of incidence of 0, 15, 30, 45, and 60 degrees. [Diagram 5] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 1 at an incident angle of 0 degree. [Figure 6]13 shows reflectance characteristics at position C of the optical element in Example 2 at angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 7] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 2 at an incident angle of 0 degree. [Figure 8] The reflectance characteristics are shown for the incident angles of 0, 15, 30, 45, and 60 degrees at position C of the optical element in Example 3. [Figure 9] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 3 at an incident angle of 0 degree. [Figure 10] 13 shows reflectance characteristics at position C of the optical element in Example 4 at angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 11] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 4 at an incident angle of 0 degree. [Figure 12] 13 shows the reflectance characteristics at position C of the optical element in Example 5 at angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 13] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 5 at an incident angle of 0 degree. [Figure 14] 13 shows the reflectance characteristics of the optical element in Example 6 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 15] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 6 at an incident angle of 0 degree. [Figure 16] 13 shows the reflectance characteristics at position C of the optical element in Example 7 at angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 17] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 7 at an incident angle of 0 degree. [Figure 18] The reflectance characteristics of the optical element in Example 8 at position C are shown for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 19] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 8 at an incident angle of 0 degree. [Figure 20] The reflectance characteristics of the optical element in Example 9 at position C are shown for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 21]13 shows the reflectance characteristics at positions C and Q of the optical element in Example 9 at an incident angle of 0 degree. [Figure 22] The reflectance characteristics of the optical element in Example 10 at position C are shown for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 23] 13 shows the reflectance characteristics at positions C and Q of the optical element in Example 10 at an incident angle of 0 degree. [Figure 24] 13 shows the reflectance characteristics of the optical element in Example 11 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Diagram 25] 13 shows the reflectance characteristics of the optical element in Example 11 at positions C and Q at an incident angle of 0 degree. [Figure 26] 13 shows the reflectance characteristics of the optical element in Example 12 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 27] 13 shows the reflectance characteristics of the optical element in Example 12 at positions C and Q at an incident angle of 0 degree. [Figure 28] The reflectance characteristics of the optical element in Example 13 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 29] 13 shows the reflectance characteristics of the optical element in Example 13 at positions C and Q at an incident angle of 0 degree. [Diagram 30] 16 shows the reflectance characteristics of the optical element in Example 14 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Diagram 31] 16 shows the reflectance characteristics of the optical element in Example 14 at positions C and Q at an incident angle of 0 degree. [Diagram 32] FIG. 23 is a cross-sectional view of an optical system in Example 15. [Diagram 33] FIG. 23 is an external perspective view of an imaging device according to a sixteenth embodiment. [Diagram 34] The reflectance characteristics of the optical element of Comparative Example 1 at position C are shown for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Diagram 35] 13 shows the reflectance characteristics of the optical element of Comparative Example 1 at positions C and Q at an incident angle of 0 degree. [Diagram 36]The reflectance characteristics of the optical element of Comparative Example 2 at position C are shown for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 37] FIG. 2 is a schematic diagram of the optical elements in Examples 17 to 25. [Figure 38] 1 is a schematic cross-sectional view of optical elements in Examples 17, 19, 21, and 22 and Comparative Examples 1 and 2. FIG. [Figure 39] 1 is a schematic cross-sectional view of the optical elements in Examples 18, 20, and 23. FIG. [Diagram 40] FIG. 21 is a schematic cross-sectional view of an optical element in Example 24. [Diagram 41] FIG. 21 is a schematic cross-sectional view of an optical element in Example 25. [Diagram 42] 16 shows the reflectance characteristics of the optical element in Example 17 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Diagram 43] 16 shows the reflectance characteristics of the optical element in Example 17 at positions C and Q at an incident angle of 0 degree. [Diagram 44] 18 shows the reflectance characteristics at position C of the optical element in Example 18 at angles of incidence of 0, 15, 30, 45, and 60 degrees. [Diagram 45] 18 shows the reflectance characteristics of the optical element in Example 18 at positions C and Q at an incident angle of 0 degree. [Diagram 46] The reflectance characteristics of the optical element in Example 19 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 47] 23 shows the reflectance characteristics of the optical element in Example 19 at positions C and Q at an incident angle of 0 degree. [Figure 48] The reflectance characteristics of the optical element in Example 20 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 49] 20 shows the reflectance characteristics at positions C and Q of the optical element in Example 20 at an incident angle of 0 degree. [Figure 50] 21 shows the reflectance characteristics at position C of the optical element in Example 21 at angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 51] 23 shows the reflectance characteristics of the optical element in Example 21 at positions C and Q at an incident angle of 0 degree. [Figure 52] 23 shows the reflectance characteristics of the optical element in Example 22 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Diagram 53] 23 shows the reflectance characteristics of the optical element in Example 22 at positions C and Q at an incident angle of 0 degree. [Figure 54] The reflectance characteristics of the optical element in Example 23 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 55] 23 shows the reflectance characteristics of the optical element at positions C and Q at an incident angle of 0 degree in Example 23. [Figure 56] The reflectance characteristics of the optical element in Example 24 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 57] 26 shows the reflectance characteristics of the optical element in Example 24 at positions C and Q at an incident angle of 0 degree. [Figure 58] The reflectance characteristics of the optical element in Example 25 at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 59] 25 shows the reflectance characteristics of the optical element at positions C and Q at an incident angle of 0 degree in Example 25. [Figure 60] The reflectance characteristics of the optical element of Comparative Example 3 at position C are shown for angles of incidence of 0, 15, 30, 45, and 60 degrees. [Figure 61] 13 shows the reflectance characteristics of the optical element of Comparative Example 3 at positions C and Q at an incident angle of 0 degree. [Figure 62] The reflectance characteristics of the optical element of Comparative Example 4 at position C are shown for angles of incidence of 0, 15, 30, 45, and 60 degrees. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.

[0012] First, an outline of an optical element 300 in Examples 1 to 14 will be described with reference to FIG. 1. FIG. 1 is a schematic diagram of the optical element 300. The optical element 300 has a transparent substrate (base material) 200 and an anti-reflection film 100 consisting of three layers. Note that a "layer" here refers to a group of parts consisting of the same material. In other words, two adjacent layers are made of different materials, and an interface exists at the boundary between them. The anti-reflection film 100 consists of a thin film layer (first layer) 01, a thin film layer (second layer) 02, and a thin film layer (third layer) 03, in that order from the transparent substrate 200 toward the air side.

[0013] In each embodiment, the thin film layers 01, 02, and 03 of the optical element 300 are preferably made of a material containing an organic compound. Here, the organic compound refers to a compound containing carbon, excluding compounds with simple structures such as carbon monoxide and carbon dioxide. The material containing an organic compound can be easily formed by a wet coating method.

[0014] In each embodiment, when the reference wavelength λ is 550 nm and the refractive index of the thin film layer 03 at the wavelength of 550 nm is n3, it is preferable to satisfy the following conditional expression (1).

[0015] 1.10≦n3≦1.28 …(1) In each embodiment, the refractive index of thin film layer 01 at a wavelength of 550 nm is n1, the refractive index of thin film layer 02 at a wavelength of 550 nm is n2, and the refractive index of thin film layer 03 at a wavelength of 550 nm is n3. The physical thickness of thin film layer 01 is d1 (nm), the physical thickness of thin film layer 02 is d2 (nm), and the physical thickness of thin film layer 03 is d3 (nm). In this case, it is preferable to satisfy the following conditional expressions (2) to (8).

[0016] 1.30≦n1≦1.50 …(2) 1.56≦n2≦1.70 …(3) 1.10≦n3≦1.28 …(4) 10≦n1d1≦155 …(5) 10≦n2d2≦155 …(6) 100≦n3d3≦155 …(7) 200≦n1d1+n2d2+n3d3≦300 …(8) If the refractive index or physical thickness of each material is outside the range of conditional expressions (2) to (8), sufficient antireflection performance cannot be obtained.

[0017] More preferably, the numerical range of conditional formula (1) or conditional formula (4) is set as in the following conditional formula (9).

[0018] 1.12≦n3≦1.22 …(9) More preferably, the numerical range of conditional formula (1) or conditional formula (4) is set as in the following conditional formula (9a).

[0019] 1.15≦n3≦1.22 …(9a) Next, optical elements 300 (301, 302) in which antireflection films 100 (101, 102) are formed on transparent substrates 200 (201, 202) will be described with reference to Fig. 2 and Fig. 3. Fig. 2 is a schematic cross-sectional view of optical elements 301 in Examples 1, 2, 5, 7, 8, 11, and 13 and Comparative Examples 1 and 2 described below. Fig. 3 is a schematic cross-sectional view of optical elements 302 in Examples 3, 4, 6, 9, 10, 12, and 14 described below.

[0020] In the optical element 301 shown in Fig. 2, the transparent substrate 201 has a concave shape, and an antireflection film 101 consisting of a thin film layer (first layer) 11, a thin film layer (second layer) 12, and a thin film layer (third layer) 13 is formed on the concave surface of the transparent substrate 201. In the optical element 302 shown in Fig. 3, the transparent substrate 202 has a convex shape, and an antireflection film 102 consisting of a thin film layer (first layer) 21, a thin film layer (second layer) 22, and a thin film layer (third layer) 23 is formed on the convex surface of the transparent substrate 202. The optical element 301 shown in Fig. 2 will be described below, but the same applies to the optical element 302 shown in Fig. 3.

[0021] The optical element 301 has a shape in which the optical surface on which the anti-reflection film 101 is formed has a rotational symmetry axis (a reference axis, for example, a surface normal passing through the origin (surface vertex)), that is, a rotationally symmetric shape. However, each embodiment is not limited to this, and the optical surface on which the anti-reflection film 101 is formed may not be rotationally symmetric, and may be, for example, a shape in which a part of a rotationally symmetric shape is cut out. In FIG. 2, position C is the rotation center of the lens surface of the transparent substrate 201 to which the anti-reflection film 101 is applied. That is, position C is the position (intersection) where the rotational symmetry axis (reference axis, optical axis L) of the lens surface intersects with the lens surface of the transparent substrate 201. On the other hand, position Q is located at a position farthest from position C within the optically effective area on the lens surface of the transparent substrate 201. Here, the optically effective area refers to an area (effective diameter) through which an effective light ray that contributes to image formation passes on the optical surface.

[0022] In other words, if the angle between the optical axis L and the normal to the position Q (hereinafter referred to as the half angle) is φ, the half angle φ will be the maximum value within the optically effective area. The anti-reflection film 101 is made up of thin film layers 11, 12, and 13 in this order from the transparent substrate 201. The physical thickness of the thin film layer 11 at the position C is d 1c (nm), the physical thickness of the thin film layer 22 is d 2c The physical thickness of the thin film layer 13 is d 3c (nm). The physical thickness of the thin film layer 11 at the position Q is d 1q (nm), the physical thickness of the thin film layer 12 is d 2q (nm), the physical thickness of the thin film layer 13 is d 3q In this case, it is preferable to satisfy the following conditional expressions (10) to (12).

[0023] 1.0 <d 1q / d 1c ≦1.3 …(10) 1.0 <d 2q / d 2c ≦1.3 …(11) 1.0 <d 3q / d 3c ≦1.3 …(12) In each embodiment, it is preferable that the film thicknesses of the thin film layers 11, 12, and 13 constituting the antireflection coating 101 are smallest at position C, which is the center (center of the optical axis) of the antireflection coating 101, and increase with increasing distance from the center of the optical axis. By satisfying conditional expressions (10) to (12), film unevenness can be further reduced.

[0024] In each embodiment, it is preferable that the half opening angle φ (°) at the position Q satisfies the following conditional expression (13).

[0025] φ≧25 …(13) In each embodiment, the reflectance of the antireflection film 101 for light incident on the intersection (position C) at an incident angle of 0 degrees is preferably 0.5% or less in the wavelength range of 450 nm or more and 650 nm or less. In each embodiment, the reflectance of the antireflection film 101 for light incident on the intersection at an incident angle of 30 degrees is preferably 1.0% or less.

[0026] The thin film layers 03, 13, and 23 preferably contain voids. Since the thin film layers 03, 13, and 23 contain voids, that is, air with a refractive index of 1.0, the refractive index can be reduced to a range that satisfies conditional expressions (1), (4), and (9). If the refractive index is less than 1.10, the ratio of voids contained in the layer is large, so the film strength is weakened. On the other hand, if the refractive index is greater than 1.30, sufficient anti-reflection performance cannot be obtained. In addition, an anti-soiling film or the like may be provided on the surface of the anti-reflection film of each embodiment (the surface of the thin film layers 03, 13, and 23) as necessary. Examples of the anti-soiling film include films containing fluoropolymers, fluorosilane monomolecules, titanium oxide particles, and the like.

[0027] In each embodiment, the thin film layers 03, 13, 23 are preferably made of solid particles, chain particles, or hollow particles. More preferably, the thin film layers 03, 13, 23 are made of hollow particles having holes inside. The holes may be either single or multiple holes, and can be selected appropriately. The material constituting the solid particles, chain particles, or hollow particles preferably has a low refractive index. For example, organic resins made of SiO2, MgF2, fluorine, silicon, etc. are listed, and SiO2, which is easy to manufacture, is more preferable. The average particle diameter of the hollow particles is preferably 15 nm or more and 100 nm or less, preferably 15 nm or more and 80 nm or less. If the average particle diameter of the hollow particles is less than 15 nm, it is difficult to stably produce core particles. On the other hand, if the average particle diameter of the hollow particles exceeds 100 nm, the size of the gap between the particles becomes large, so large voids are likely to occur, and scattering occurs due to the size of the particles, which is not preferable.

[0028] The thin film layers 01, 11, and 21 are preferably made of a material containing solid particles, particularly solid silica particles, bound by a binder such as a siloxane bond, or a material containing an acrylic resin, which is a "polymer of acrylic acid ester or methacrylic acid ester."

[0029] The thin film layers 02, 12, and 22 are preferably made of a material containing a polyimide resin, which is a polymer compound containing an imide (-CO-NR-CO-) bond, or an epoxy resin, which is a resin cured by crosslinking epoxy groups having oxacyclopropane (oxirane), a three-membered ring ether, in the structural formula.

[0030] In each embodiment, the optical element 300 is manufactured by forming a thin film layer 01 on a transparent substrate 200, forming a thin film layer 02 on the thin film layer 01, and forming a thin film layer 03 on the thin film layer 02. In each embodiment, the thin film layers 01, 11, 21, 02, 12, 22, and 03, 13, 23 are preferably formed by a wet film formation method in which a coating liquid containing a film material is applied, and then dried and baked. The wet film formation method can coat a large area at low cost. In particular, the spin coating method (spin coating method) is preferable because the coating is performed while rotating the coating surface around the rotation axis, thereby suppressing the in-plane film thickness distribution. In a dry film formation method such as a deposition method or a sputtering method, the film is formed in a positional relationship in which the evaporation source and the center of the lens face each other. In the case of a large opening angle lens, the incident angle of the deposition material to the lens surface is large in the peripheral part, so the film thickness is reduced compared to the center part. This causes film unevenness in the lens surface, resulting in bias in anti-reflection performance. To form a film without causing unevenness, it is necessary to set a mask and control the position and rotation of the substrate.

[0031] The organic solvent that can be used in the coating liquid is not particularly limited as long as it does not impair the coating properties or performance, and known solvents can be used. For example, as monohydric alcohols, there are methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methylpropanol, 1-pentanol, 2-pentanol, cyclopentanol, and 2-methylbutanol. Alternatively, 3-methylbutanol, 1-hexanol, 2-hexanol, 3-hexanol, 4-methyl-2-pentanol, 2-methyl-1-pentanol, and 2-ethylbutanol may be used. Alternatively, 2,4-dimethyl-3-pentanol, 3-ethylbutanol, 1-heptanol, 2-heptanol, 1-octanol, and 2-octanol may be used. Alternatively, dihydric or higher alcohols such as ethylene glycol and triethylene glycol may be used.

[0032] The alcohol may be an ether alcohol such as methoxyethanol, ethoxyethanol, propoxyethanol, isopropoxyethanol, butoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, or 1-propoxy-2-propanol. Alternatively, the alcohol may be an ether such as dimethoxyethane, diglyme, tetrahydrofuran, dioxane, diisopropyl ether, dibutyl ether, or cyclopentyl methyl ether. Alternatively, the alcohol may be an ester. For example, there are ethyl formate, ethyl acetate, n-butyl acetate, methyl lactate, ethyl lactate, and ethylene glycol monomethyl ether acetate. Alternatively, there are ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, and propylene glycol monomethyl ether acetate.

[0033] Alternatively, various aliphatic or alicyclic hydrocarbons such as n-hexane, n-octane, cyclohexane, cyclopentane, and cyclooctane may be used. Alternatively, various aromatic hydrocarbons such as toluene, xylene, and ethylbenzene may be used. Alternatively, various ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone may be used. Alternatively, various chlorinated hydrocarbons such as chloroform, methylene chloride, carbon tetrachloride, and tetrachloroethane may be used. Alternatively, aprotic polar solvents such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and ethylene carbonate may be used. Two or more of these solvents may be mixed and used.

[0034] Furthermore, when solid particles, chain particles, or hollow particles are used for the thin film layers 03, 13, and 23, and solid particles are used for the thin film layers 01, 11, and 21, it is preferable that they are bound by a binder in order to improve strength. It is preferable to use siloxane bonds as the binder. This is particularly suitable when using silica particles that have many hydroxyl groups on the surface.

[0035] In each embodiment, the thin film layers 01, 11, 02, 12, 03, 13 are made of materials that can be formed by a wet film forming method, and therefore the materials themselves or the binders contain organic compounds. In addition, the anti-reflection films of each embodiment are not baked at high temperatures in the drying process after coating. For this reason, it is possible to use plastics that are prone to thermal deformation or optical curable resins for the transparent substrates 200, 201, 202.

[0036] The refractive index of the transparent substrates 200, 201, and 202 is n S When this is set, it is preferable to satisfy the following conditional expression (14):

[0037] 1.45≦n S ≦2.10 …(14) Specific examples are given below. However, these are merely examples, and the present invention is not limited to the scope of each example. EXAMPLES

[0038] First, Example 1 will be described. FIG. 2 is a schematic cross-sectional view of an optical element 301 in this example. The optical element 301 in this example is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA) with a refractive index of 1.57 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of solid silica, the thin film layer 12 is made of a material mainly composed of polyimide resin, and the thin film layer 13 is made of a material mainly composed of hollow silica. Table 1 shows the details of the film configuration of the optical element 301 in this example. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), (10) to (12). In addition, each of the thin film layers 11, 12, and 13 contains an organic compound.

[0039] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0040] (Hollow silica coating liquid 1) 580 g of an isopropyl alcohol dispersion of hollow silica particles (Suluria 4110, manufactured by JGC Catalysts and Chemicals Co., Ltd., average particle diameter about 60 nm, shell thickness about 12 nm, solid content concentration 20.5% by mass) was used. 1-ethoxy-2-propanol (hereinafter abbreviated as 1E2P) was added to this isopropyl alcohol dispersion while heating and distilling off isopropyl alcohol. The isopropyl alcohol was distilled off until the solid content concentration became 19.5% by mass, and 610 g of 1E2P solvent replacement liquid of hollow silica particles (hereinafter referred to as solvent replacement 1) was prepared. A fluorine-containing organic acid (trifluoroacetic acid, manufactured by Tokyo Chemical Industry Co., Ltd., fluorine number 3) was added to the obtained solvent replacement liquid 1 so that the ratio of hollow silica particles: fluorine-containing organic acid components was 100 / 1, and hollow particle dispersion liquid 1 was obtained.

[0041] In a separate container, 3.6 g of phosphinic acid diluted to 0.1% concentration with pure water, 11.4 g of 1-propoxy-2-propanol, and 4.5 g of methyl polysilicate (Methyl Silicate 53A, manufactured by Colcoat Co., Ltd.) were slowly added and stirred at room temperature for 120 minutes, thereby preparing a silica sol with a solid content concentration of 12% by mass (hereinafter, Silica Sol 1).

[0042] Hollow particle dispersion liquid 1 was diluted with ethyl lactate to a solid content of 4.5% by mass, and then silica sol 1 was added to the mixture so that the ratio of hollow silica particles to silica sol components was 100 / 12. The mixture was further mixed and stirred at room temperature for 2 hours to obtain hollow silica coating liquid 1 containing hollow silica particles.

[0043] (Solid silica coating liquid 1) Solid silica coating solution 1 was prepared by adding 300 g of 1-methoxy-2-propanol and 4 g of silica sol 1 to 25 g of silica particle dispersion PL-1 (manufactured by Fuso Chemical).

[0044] (Polyimide coating liquid 1) 200 g of 4,4'-methylenebis(aminocyclohexane) (hereinafter referred to as DADCM, manufactured by Tokyo Chemical Industry Co., Ltd.) was refluxed while gradually adding hexane to completely dissolve it. After stopping heating and leaving it at room temperature for several days, the precipitate was filtered off and dried under reduced pressure. 58 g of the purified white solid alicyclic diamine DADCM was obtained.

[0045] A diamine solution was prepared by dissolving three types of diamines in N,N-dimethylacetamide (hereinafter abbreviated as DMAc) so that the total amount was 12 mmol. One of these three diamines is the alicyclic diamine DADCM. The other two are the aromatic diamine 4,4'-bis(4-aminophenoxy)biphenyl (product name BODA: manufactured by Wakayama Seika Kogyo Co., Ltd.) and the siloxane-containing diamine 1,3-bis(3-aminopropyl)tetramethyldisiloxane (product name PAM-E: manufactured by Shin-Etsu Chemical Co., Ltd.).

[0046] About 12 mmol of acid dianhydride was added to the diamine solution while cooling it with water. The acid dianhydride was 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride (product name TDA-100: manufactured by New Japan Chemical Co., Ltd.). Alternatively, the acid dianhydride was 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride (product name B-4400: manufactured by DIC). The amount of DMAc was adjusted so that the total mass of the diamine and acid dianhydride was 20% by weight.

[0047] The solution was stirred at room temperature for 15 hours to carry out the polymerization reaction. After diluting with DMAc to adjust the concentration to 8% by weight, 7.4 ml of pyridine and 3.8 ml of acetic anhydride were added and stirred at room temperature for 1 hour. The solution was then stirred for 4 hours while being heated to 60 to 70°C in an oil bath. The polymerization solution was reprecipitated in methanol or methanol to extract the polymer, which was then washed several times in methanol. After drying at 60°C for 24 hours, white to pale yellow powdery polyimide 1 was obtained.

[0048] The obtained polyimide 1 was dissolved in cyclohexanone so that the solid content concentration was 2.5% by mass, to prepare a polyimide coating solution 1.

[0049] The solid silica coating liquid 1, the polyimide coating liquid 1, and the hollow silica coating liquid 1 form an anti-reflection film 101.

[0050] 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the hollow silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0051] FIG. 4 shows the reflectance characteristics at the incidence angles of 0, 15, 30, 45, and 60 degrees at position C of the optical element 301 in this embodiment. In FIG. 4, the horizontal axis shows the wavelength (nm) and the vertical axis shows the reflectance (%). This is the same for the other reflection characteristic diagrams. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. FIG. 5 shows the reflectance characteristics at the incidence angle of 0 degrees at positions C and Q of the optical element 301 in this embodiment. According to Table 1, the film thickness of each thin film layer at position Q is about 6% higher than that at position C, but the reflectance characteristic is 0.2% or less at wavelengths of 420 nm to 680 nm, which is good.

[0052] [Table 1] EXAMPLES

[0053] Next, a second embodiment of the present invention will be described. FIG. 2 is a schematic cross-sectional view of an optical element 301 in this embodiment. The optical element 301 in this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-LAL12 (manufactured by OHARA) with a refractive index of 1.68 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 70 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of solid silica, the thin film layer 12 is made of a material mainly composed of polyimide resin, and the thin film layer 13 is made of a material mainly composed of hollow silica. Table 2 shows the details of the film configuration of the optical element in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), (10) to (12). In addition, each of the thin film layers 11, 12, and 13 contains an organic compound.

[0054] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0055] (Hollow silica coating liquid 2) The methods for preparing hollow particle dispersion 1 and silica sol 1 were the same as those for hollow particle coating liquid 1. Hollow particle dispersion 1 was diluted with ethyl lactate to a solid content of 4.5% by mass, and then silica sol 1 was added so that the ratio of hollow silica particles:silica sol components was 100 / 9. The mixture was further mixed and stirred at room temperature for 2 hours to obtain hollow silica coating liquid 2 containing hollow silica particles.

[0056] The solid silica coating liquid 1, the polyimide coating liquid 1, and the hollow silica coating liquid 2 form an anti-reflection film 101.

[0057] 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the hollow silica coating liquid 2 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0058] FIG. 6 shows the reflectance characteristics at the incidence angles of 0, 15, 30, 45, and 60 degrees at position C of the optical element 301 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. FIG. 7 shows the reflectance characteristics at the incidence angle of 0 degrees at positions C and Q of the optical element 301 in this embodiment. According to Table 2, the film thickness of each thin film layer at position Q is 20% greater than that at position C, but the reflectance at wavelengths of 420 nm to 680 nm is 0.2% or less, which is good.

[0059] [Table 2] EXAMPLES

[0060] Next, a third embodiment of the present invention will be described. FIG. 3 is a schematic cross-sectional view of an optical element 302 in this embodiment. The optical element 302 in this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH53 (manufactured by OHARA) with a refractive index of 1.81 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed has a convex shape. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of acrylic resin, and the thin film layer 22 is made of a material mainly composed of hollow silica. Table 3 shows the details of the film configuration of the optical element 302 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), (10) to (12). The thin film layers 21, 22, and 23 contain an organic compound.

[0061] The method for forming the anti-reflection film 102 of this embodiment is as follows.

[0062] (Chain Silica Coating Liquid 1) A 2-propanol (IPA) dispersion of chain-shaped silica particles (IPA-ST-UP manufactured by Nissan Chemical Industries, Ltd., average particle size 12 nm, solid content concentration 15 mass%) was evaporated to replace the 2-propanol solvent with 1-propoxy-2-propanol (manufactured by Sigma). This produced a 1-propoxy-2-propanol dispersion (solid content concentration 17 wt%). This was named dispersion 2. Next, 18.5 g of tetraethoxysilane (TEOS, manufactured by Tokyo Chemical Industry Co., Ltd.) and 16.0 g of 0.1 wt% phosphinic acid (10 equivalents to TEOS) as catalytic water were added, and the mixture was mixed and stirred in a water bath at 20°C for 60 minutes to obtain binder solution 2.

[0063] To 251.3 g of the dispersion liquid 2, 33.4 g of the binder solution 2 were added. Then, 174.5 g of 1-propoxy-2-propanol and 546.5 g of ethyl lactate were added and stirred for 60 minutes to obtain a chain silica coating liquid 1.

[0064] (Acrylic coating liquid) 6.1g of N-cyclohexylmaleimide (hereinafter, CHMI) and 4.0g of 2,2,2-trifluoroethyl methacrylate (product name M-3F: manufactured by Kyoeisha Chemical) were used. Furthermore, 0.45g of 3-(methacryloyloxy)propyltrimethoxysilane (product name LS-3380: manufactured by Shin-Etsu Chemical Co., Ltd.) was used. In addition, 0.08g of 2,2'-azobis(isobutyronitrile) (hereinafter, AIBN) was used. These were stirred and dissolved in 24.8g of toluene to obtain a solution. This solution was repeatedly degassed and substituted with nitrogen while cooling with ice water, and then stirred at 60 to 70 ° C for 7 hours while flowing nitrogen. The polymerization solution was slowly poured into strongly stirred methanol, and the precipitated polymer was filtered, and then stirred and washed several times in methanol. The polymer recovered by filtration was vacuum dried at 80 to 90 ° C. A white powder of maleimide copolymer with a maleimide copolymerization ratio of 0.57 was obtained (8.3 g, 81% yield). 2.2 g of the maleimide copolymer 1 powder was dissolved in 97.8 g of a cyclopentanone / cyclohexanone mixed solvent to prepare a maleimide copolymer 1 solution, and an acrylic coating solution was prepared.

[0065] (Polyimide coating liquid 2) 4,4'-methylenebis(aminocyclohexane) (hereinafter referred to as DADCM, manufactured by Tokyo Chemical Industry Co., Ltd.) was purified to obtain 50 g of white solid alicyclic diamine DADCM. Three types of diamines were dissolved in N,N-dimethylacetamide (hereinafter referred to as DMAc) so that the total amount was 12 mmol. One of the three diamines is the alicyclic diamine DADCM. The other two are the aromatic diamine 4,4'-bis(4-aminophenoxy)biphenyl (product name BODA, manufactured by Wakayama Seika Kogyo Co., Ltd.) and the siloxane-containing diamine 1,3-bis(3-aminopropyl)tetramethyldisiloxane (product name PAM-E, manufactured by Shin-Etsu Chemical Co., Ltd.).

[0066] The following procedure was the same as for Polyimide Coating Liquid 1. Polyimide 2 was obtained, which had a different ratio of three types of diamine from Polyimide Coating Liquid 1. The obtained Polyimide 2 was dissolved in cyclohexanone so that the solid content concentration was 2.5 mass %, to prepare Polyimide Coating Liquid 2.

[0067] The anti-reflection film 102 is formed from the acrylic coating liquid, the polyimide coating liquid 2, and the chain silica coating liquid 1.

[0068] 0.2 ml of the acrylic coating liquid was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 2 was continuously dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the chain silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0069] Fig. 8 shows the reflectance characteristics at the incidence angles of 0, 15, 30, 45, and 60 degrees at position C of the optical element 302 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 9 shows the reflectance characteristics at the incidence angle of 0 degrees at positions C and Q of the optical element 302 in this embodiment. According to Table 3, the film thickness of each thin film layer at position Q is about 2% higher than at position C, but the reflectance characteristics are good, being 0.2% or less at wavelengths of 420 nm to 680 nm.

[0070] [Table 3] EXAMPLES

[0071] Next, a fourth embodiment of the present invention will be described. FIG. 3 is a schematic cross-sectional view of an optical element 302 in this embodiment. The optical element 302 in this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH79 (manufactured by OHARA) with a refractive index of 2.00 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed is a convex shape. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of solid silica, the thin film layer 12 is made of a material mainly composed of polyimide resin, and the thin film layer 13 is made of a material mainly composed of hollow silica. Table 4 shows the details of the film configuration of the optical element in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), (10) to (12). The thin film layers 21, 22, and 23 contain an organic compound.

[0072] The method for forming the anti-reflection film 102 of this embodiment is as follows.

[0073] The solid silica coating liquid 2, the polyimide coating liquid 2, and the hollow silica coating liquid 1 form an anti-reflection film 102.

[0074] 0.2 ml of the solid silica coating liquid 2 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 2 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the hollow silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0075] Fig. 10 shows the reflectance characteristics at the incidence angles of 0, 15, 30, 45, and 60 degrees at position C of the optical element 302 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 11 shows the reflectance characteristics at the incidence angle of 0 degrees at positions C and Q of the optical element 302 in this embodiment. According to Table 4, the film thickness of each thin film layer at position Q is about 6% higher than at position C, but it can be confirmed that the reflectance is 0.2% or less at wavelengths of 420 nm to 680 nm, which is good.

[0076] [Table 4] EXAMPLES

[0077] Next, a fifth embodiment of the present invention will be described. FIG. 2 is a schematic cross-sectional view of an optical element 301 in this embodiment. The optical element 301 in this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-LAH53 (manufactured by OHARA) with a refractive index of 1.81 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of acrylic resin, the thin film layer 12 is made of a material mainly composed of polyimide resin, and the thin film layer 13 is made of a material mainly composed of hollow silica. Table 5 shows the details of the film configuration of the optical element in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), (10) to (12). In addition, the thin film layers 11, 12, and 13 contain an organic compound.

[0078] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0079] The anti-reflection film 101 is formed by the acrylic coating liquid, the polyimide coating liquid 1, and the hollow silica coating liquid 2. 0.2 ml of the acrylic coating liquid was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the hollow silica coating liquid 2 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0080] Fig. 12 shows the reflectance characteristics at the incidence angles of 0, 15, 30, 45, and 60 degrees at position C of the optical element 301 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 13 shows the reflectance characteristics at the incidence angle of 0 degrees at positions C and Q of the optical element 301 in this embodiment. According to Table 5, although the film thickness of each thin film layer at position Q is about 6% higher than at position C, it can be confirmed that the reflectance characteristics are good, being 0.2% or less at wavelengths of 420 nm to 680 nm.

[0081] [Table 5] EXAMPLES

[0082] Next, a sixth embodiment of the present invention will be described. FIG. 3 is a schematic cross-sectional view of an optical element 302 in this embodiment. The optical element 302 in this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH66 (manufactured by OHARA) with a refractive index of 1.77 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed has a convex shape. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 60 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of solid silica, the thin film layer 22 is made of a material mainly composed of epoxy resin, and the thin film layer 23 is made of a material mainly composed of hollow silica. Table 6 shows the details of the film configuration of the optical element 302 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), (10) to (12). The thin film layers 21, 22, and 23 contain an organic compound.

[0083] The method for forming the anti-reflection film 102 of this embodiment is as follows.

[0084] (Epoxy coating fluid) Intermediate layer coating solution 3 was prepared by adding 500 g of 1-methoxy-2-propanol to 25 g of epoxy resin jER828 (manufactured by Mitsubishi Chemical).

[0085] The solid silica coating liquid 2, the epoxy coating liquid, and the hollow silica coating liquid 1 form an anti-reflection film 102.

[0086] 0.2 ml of the solid silica coating liquid 2 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the epoxy coating liquid was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the hollow silica coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at a room temperature of 23°C.

[0087] Fig. 14 shows the reflectance characteristics at incident angles of 0, 15, 30, 45, and 60 degrees at position C of optical element 302 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 15 shows the reflectance characteristics at incident angle of 0 degrees at positions C and Q of optical element 302 in this embodiment. According to Table 6, although the film thickness of each thin film layer at position Q is about 12% higher than at position C, it can be confirmed that the reflectance characteristics are good, being 0.2% or less at wavelengths of 420 nm to 680 nm.

[0088] [Table 6] EXAMPLES

[0089] Next, a seventh embodiment of the present invention will be described. FIG. 2 is a schematic cross-sectional view of an optical element 301 in this embodiment. The optical element 301 in this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is ZEONEX K22R (manufactured by Zeon Corporation) with a refractive index of 1.54 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is a concave shape. The half-open angle φ at a position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of solid silica, the thin film layer 12 is made of a material mainly composed of polyimide resin, and the thin film 13 is made of a material mainly composed of hollow silica. Table 7 shows the details of the film configuration of the optical element 301 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), (10) to (12). In addition, the thin film layers 11, 12, and 13 contain an organic compound.

[0090] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0091] The anti-reflection film 101 is formed by the solid silica coating liquid 1, the polyimide coating liquid 1, and the hollow silica coating liquid 1. 0.2 ml of the solid silica coating liquid 1 is dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 1 is dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the hollow silica coating liquid 1 is continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate is dried for 24 hours or more in a clean room at room temperature of 23°C.

[0092] Fig. 16 shows the reflectance characteristics at incident angles of 0, 15, 30, 45, and 60 degrees at position C of optical element 301 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 17 shows the reflectance characteristics at an incident angle of 0 degrees at positions C and Q of optical element 301 in this embodiment. According to Table 7, the film thickness of each thin film layer at position Q is about 2% higher than at position C, but it can be confirmed that the reflectance is 0.2% or less at wavelengths of 420 nm to 680 nm, which is good.

[0093] [Table 7] EXAMPLES

[0094] Next, an eighth embodiment of the present invention will be described. FIG. 2 is a schematic cross-sectional view of an optical element 301 in this embodiment. The optical element 301 in this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is EP-5000 (manufactured by Mitsubishi Gas Chemical Company, Inc.) with a refractive index of 1.64 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at a position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of solid silica, the thin film layer 12 is made of a material mainly composed of polyimide resin, and the thin film layer 13 is made of a material mainly composed of hollow silica. Table 8 shows the details of the film configuration of the optical element 301 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8) and (10) to (12). Moreover, the thin film layers 11, 12, and 13 contain an organic compound.

[0095] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0096] The solid silica coating liquid 2, the polyimide coating liquid 2, and the hollow silica coating liquid 2 form an anti-reflection film 101.

[0097] 0.2 ml of the solid silica coating liquid 2 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 2 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the hollow silica coating liquid 2 was continuously dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0098] Fig. 18 shows the reflectance characteristics at incident angles of 0, 15, 30, 45, and 60 degrees at position C of optical element 301 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 19 shows the reflectance characteristics at incident angle of 0 degrees at positions C and Q of optical element 301 in this embodiment. According to Table 8, the film thickness of each thin film layer at position Q is 6% higher than at position C, but the reflectance characteristics are 0.2% or less at wavelengths of 420 nm to 680 nm, which is good.

[0099] [Table 8] EXAMPLES

[0100] Next, a ninth embodiment of the present invention will be described. FIG. 3 is a schematic cross-sectional view of an optical element 302 in this embodiment. The optical element 302 in this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is EP-9000 (manufactured by Mitsubishi Gas Chemical Company, Inc.) with a refractive index of 1.64 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed has a convex shape. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of solid silica, the thin film layer 22 is made of a material mainly composed of polyimide resin, and the thin film layer 23 is made of a material mainly composed of hollow silica. Table 9 shows the details of the film configuration of the optical element 302 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), (10) to (12). In addition, the thin film layers 21, 22, and 23 contain an organic compound.

[0101] The method for forming the anti-reflection film 102 of this embodiment is as follows.

[0102] The anti-reflection film 102 is formed by the solid silica coating liquid 1, the polyimide coating liquid 1, and the chain silica coating liquid 1. 0.2 ml of the solid silica coating liquid 1 is dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 1 is dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the chain silica coating liquid 1 is continuously dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Then, drying is performed for 24 hours or more in a clean room at room temperature of 23°C.

[0103] Fig. 20 shows the reflectance characteristics at incident angles of 0, 15, 30, 45, and 60 degrees at position C of optical element 302 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 21 shows the reflectance characteristics at incident angle of 0 degrees at positions C and Q of optical element 302 in this embodiment. According to Table 9, although the film thickness of each thin film layer at position Q is 2% higher than at position C, it can be confirmed that the reflectance characteristics are good, being 0.2% or less at wavelengths of 420 nm to 680 nm.

[0104] [Table 9] EXAMPLES

[0105] Next, a tenth embodiment of the present invention will be described. FIG. 3 is a schematic cross-sectional view of an optical element 302 in this embodiment. The optical element 302 in this embodiment is an optical element in which an anti-reflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is an optical element called a replica element in which the transparent substrate 202 is formed on the surface of a glass base material (not shown in the figure) that serves as a base material. The transparent substrate 202 is LPQ-1500 (manufactured by Mitsubishi Gas Chemical Co., Ltd.) with a refractive index of 1.59 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the anti-reflection film 102 is formed has a convex shape. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of solid silica, the thin film layer 22 is made of a material mainly composed of polyimide resin, and the thin film layer 23 is made of a material mainly composed of hollow silica. Table 10 shows the details of the film configuration of the optical element 302 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8) and (10) to (12). Furthermore, the thin film layers 21, 22, and 23 contain an organic compound.

[0106] The method for forming the anti-reflection film 102 of this embodiment is as follows.

[0107] The anti-reflection film 102 is formed by the solid silica coating liquid 1, the polyimide coating liquid 2, and the hollow silica coating liquid 1. 0.2 ml of the solid silica coating liquid 1 is dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 2 is dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the hollow silica coating liquid 1 is continuously dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Then, it is dried for 24 hours or more in a clean room at room temperature of 23°C.

[0108] Fig. 22 shows the reflectance characteristics at incident angles of 0, 15, 30, 45, and 60 degrees at position C of optical element 302 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 23 shows the reflectance characteristics at incident angle of 0 degrees at positions C and Q of optical element 302 in this embodiment. According to Table 10, the film thickness of each thin film layer at position Q is 2% higher than at position C, but the reflectance characteristics are good, being 0.2% or less at wavelengths of 420 nm to 680 nm.

[0109] [Table 10] EXAMPLES

[0110] Next, an eleventh embodiment of the present invention will be described. FIG. 2 is a schematic cross-sectional view of an optical element 301 in this embodiment. The optical element 301 in this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-LAH66 (manufactured by OHARA) with a refractive index of 1.77 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of polyimide resin, the thin film layer 12 is made of a material mainly composed of solid silica, and the thin film layer 13 is made of a material mainly composed of hollow silica. Table 11 shows the details of the film configuration of the optical element in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1), (10) to (12). In addition, the thin film layers 11, 12, and 13 contain an organic compound.

[0111] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0112] The anti-reflection film 101 is formed by the polyimide coating liquid 1, the solid silica coating liquid 1, and the hollow silica coating liquid 1. 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the hollow silica coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0113] Fig. 24 shows the reflectance characteristics at the incidence angles of 0, 15, 30, 45, and 60 degrees at position C of the optical element 301 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 25 shows the reflectance characteristics at the incidence angle of 0 degrees at positions C and Q of the optical element 301 in this embodiment. According to Table 11, the film thickness of each thin film layer at position Q is 6% higher than at position C, but the reflectance characteristics are 0.2% or less at wavelengths of 420 nm to 680 nm, which is good.

[0114] [Table 11] EXAMPLES

[0115] Next, a twelfth embodiment of the present invention will be described. FIG. 3 is a schematic cross-sectional view of an optical element 302 in this embodiment. The optical element 302 in this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-TIH53 (manufactured by OHARA) with a refractive index of 1.85 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed is a concave shape. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of polyimide resin, the thin film layer 22 is made of a material mainly composed of solid silica, and the thin film layer 23 is made of a material mainly composed of hollow silica. Table 12 shows the details of the film configuration of the optical element 302 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1), (10) to (12). The thin film layers 21, 22, and 23 contain an organic compound.

[0116] The method for forming the anti-reflection film 102 of this embodiment is as follows.

[0117] The anti-reflection film 102 is formed by the polyimide coating liquid 2, the solid silica coating liquid 1, and the hollow silica coating liquid 2. 0.2 ml of the polyimide coating liquid 2 is dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 is dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. 0.2 ml of the hollow silica coating liquid 2 is continuously dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate is dried for 24 hours or more in a clean room at room temperature of 23°C.

[0118] Fig. 26 shows the reflectance characteristics at incident angles of 0, 15, 30, 45, and 60 degrees at position C of optical element 302 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 27 shows the reflectance characteristics at incident angle of 0 degrees at positions C and Q of optical element 302 in this embodiment. According to Table 12, the film thickness of each thin film layer at position Q is 2% higher than at position C, but the reflectance characteristics are good, being 0.2% or less at wavelengths of 420 nm to 680 nm.

[0119] [Table 12] EXAMPLES

[0120] Next, a thirteenth embodiment of the present invention will be described. FIG. 2 is a schematic cross-sectional view of an optical element 301 in this embodiment. The optical element 301 in this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA) with a refractive index of 1.57 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half aperture angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of magnesium fluoride, the thin film layer 12 is made of a material mainly composed of alumina, and the thin film layer 13 is made of a material mainly composed of hollow silica. Table 13 shows the details of the film configuration of the optical element 301 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8) and (10) to (12).

[0121] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0122] The thin film layers 11 and 12 were formed by deposition. An electron beam was used to heat the evaporation material. In order to form a denser film, an ion beam assisted deposition method was used. The inside of the vacuum chamber of the deposition device was filled with 2×10 -3The vacuum chamber was evacuated without heating until it reached a high vacuum of approximately 1×10 Pa. After it was confirmed that the inside of the vacuum chamber had reached a high vacuum state, Ar was introduced into the ion gun as an inert gas, and the ion gun was made to discharge. After the ion gun reached a stable state, oxygen was introduced into the vacuum chamber until the vacuum pressure reached 1×10 -2 Ion-assisted deposition was performed using oxygen ions at about 1000 nm (Pa). In general, in the case of a lens with a large half aperture angle, the deposition method has a problem that the film thickness decreases toward the periphery. In Example 13, in order to prevent the film thickness from decreasing in the periphery, a mask of an arbitrary shape was placed on the film-forming surface side of the transparent substrate 201 before deposition, so that the film thickness distribution within the surface was approximately the same.

[0123] After the thin film layer 11 and then the thin film layer 12 were formed by vapor deposition, 0.2 ml of the hollow silica coating solution 1 was dropped onto the lens surface of the transparent substrate 202 on which the thin films 11 and 12 were formed, and spin-coated at 4000 rpm for 20 seconds. Then, the film was dried for 24 hours or more in a clean room at a room temperature of 23°C.

[0124] Fig. 28 shows the reflectance characteristics at incident angles of 0, 15, 30, 45, and 60 degrees at position C of optical element 301 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 29 shows the reflectance characteristics at incident angle of 0 degrees at positions C and Q of optical element 301 in this embodiment. According to Table 13, the film thickness of each thin film layer at position Q is 6% higher than at position C, but the reflectance characteristics are 0.2% or less at wavelengths of 420 nm to 680 nm, which is good.

[0125] [Table 13] EXAMPLES

[0126] Next, a fourteenth embodiment of the present invention will be described. FIG. 3 is a schematic cross-sectional view of an optical element 302 in this embodiment. The optical element 302 in this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH79 (manufactured by OHARA) with a refractive index of 2.00 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed is a concave shape. The half aperture angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of magnesium fluoride, the thin film layer 22 is made of a material mainly composed of zirconia oxide and alumina, and the thin film layer 23 is made of a material mainly composed of hollow silica. Table 14 shows the details of the film configuration of the optical element 302 in this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8) and (10) to (12).

[0127] The method for forming the anti-reflection film 102 in this embodiment is as follows. The thin film layers 21 and 22 were formed by vapor deposition. The vapor deposition method was the same as in Example 13. In this embodiment, a mask was used so that the film thickness distribution was approximately the same in the plane. After the thin film layer 22 was formed by vapor deposition following the thin film layer 21, 0.2 ml of the hollow silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 202 on which the thin film layers 21 and 22 were formed, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at a room temperature of 23°C.

[0128] Fig. 30 shows the reflectance characteristics at incident angles of 0, 15, 30, 45, and 60 degrees at position C of optical element 302 in this embodiment. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. Fig. 31 shows the reflectance characteristics at incident angle of 0 degrees at positions C and Q of optical element 302 in this embodiment. According to Table 13, the film thickness of each thin film layer at position Q is 2% higher than at position C, but the reflectance characteristics are good, being 0.2% or less at wavelengths of 420 nm to 680 nm.

[0129] [Table 14] EXAMPLES

[0130] Next, an optical system 401 in Example 15 will be described with reference to FIG. 32. FIG. 32 is a cross-sectional view of the optical system 401. The optical system 401 has a plurality of optical elements G401 to G416. 402 is a diaphragm (aperture stop), and 403 is an image forming surface. The optical elements G401 to G411 are lenses. An anti-reflection film according to any one of Examples 1 to 14 is applied to at least one of the entrance surface and the exit surface. That is, the optical system 401 has a plurality of optical elements G401 to G411, and the plurality of optical elements G403, G412, and G143 include the optical element 301 or the optical element 302 on which the anti-reflection film according to any one of Examples 1 to 14 is formed.

[0131] The optical system 400 of this embodiment is not limited to an imaging optical system used in an imaging device described later, but can be applied to optical systems for various purposes such as binoculars, projectors, and telescopes. EXAMPLES

[0132] Next, an imaging device in Example 16 will be described with reference to FIG. 33. FIG. 33 is an external perspective view of an imaging device (digital camera 500). The digital camera 500 has a camera body 502 and a lens device 501 that is integrally configured with the camera body 502. However, this example is not limited to this, and the lens device 501 may be an interchangeable lens that is detachable from the camera body 502, such as for a single-lens reflex camera or a mirrorless camera. The lens device 501 has the optical system 401 of any one of Examples 1 to 15. The camera body 502 has an imaging element 503 such as a CMOS sensor or a CCD sensor. The imaging element 503 is disposed on the imaging plane 403 of the optical system 401. Comparative Example 1 Next, Comparative Example 1 of the present invention will be described. FIG. 2 is a schematic cross-sectional view of the optical element in this comparative example. The optical element 301 in this comparative example is an optical element in which the antireflection film 101 is formed on the transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA) with a refractive index of 1.57 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of magnesium fluoride, the thin film layer 12 is made of a material mainly composed of alumina, and the thin film layer 13 is made of a material mainly composed of hollow silica. Table 15 shows the details of the film configuration of the optical element in this comparative example. The refractive index and film thickness of each material satisfy the conditional expressions (1) to (8), but do not satisfy the conditional expressions (10) and (11).

[0133] The method for forming the anti-reflection film 101 in this comparative example is as follows. The thin film layer 11 and the thin film layer 12 were formed by a vapor deposition method. The vapor deposition method was the same as in Example 13. In this comparative example, no mask was used to make the film thickness distribution uniform within the surface. After the thin film layer 12 was formed by vapor deposition following the thin film layer 11, 0.2 ml of the hollow silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201 on which the thin films 11 and 12 were formed, and spin-coated at 4000 rpm for 20 seconds. Then, the film was dried for 24 hours or more in a clean room at a room temperature of 23°C.

[0134] FIG. 34 shows the reflectance characteristics at the incidence angles of 0, 15, 30, 45, and 60 degrees at position C of the optical element 301 in this comparative example. It is seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. However, when comparing the reflectance characteristics at the incidence angle of 0 degrees at positions C and Q in FIG. 35, it can be seen that the reflectance characteristic at position Q is deteriorated compared to position C. According to Table 14, the film thickness of the thin film layer 12 at position Q is 6% higher than that at position C, but the film thickness of the thin film layers 11 and 12 at position Q is 30% lower than that at position C. For this reason, it can be said that the reflectance characteristic at position Q is deteriorated.

[0135] [Table 15]

[0136] Comparative Example 2 Next, Comparative Example 2 of the present invention will be described. FIG. 2 is a schematic cross-sectional view of an optical element in this comparative example. An optical element 301 in this comparative example is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA) with a refractive index of 1.57 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed has a concave shape. The half-open angle φ at a position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of solid silica, the thin film layer 12 is made of a material mainly composed of polyimide resin, and the thin film layer 13 is made of a material mainly composed of hollow silica.

[0137] Table 16 shows the details of the film configuration of the optical element 301 of this comparative example. The refractive index of the thin film layer 13 does not satisfy the conditional expressions (1) and (4).

[0138] The method for forming the anti-reflection film 101 of this comparative example is as follows. (Chain Silica Coating Liquid 2) The methods for preparing chain particle dispersion 2 and binder solution 2 were the same as those for hollow particle coating solution 1. 78.0 g of binder solution 2 was added to 251.3 g of chain particle dispersion 2. Then, 174.5 g of 1-propoxy-2-propanol and 510.8 g of ethyl lactate were added and stirred for 60 minutes to obtain chain silica coating solution 2.

[0139] The solid silica coating liquid 1, the polyimide coating liquid 1, and the chain silica coating liquid 2 form an anti-reflection film 101.

[0140] 0.2 ml of the solid silica coating liquid was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the chain silica coating liquid 2 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at a room temperature of 23°C.

[0141] 36 shows the reflectance characteristics of optical element 301 in this comparative example at angles of incidence of 0, 15, 30, 45, and 60 degrees at position C. The reflectance is 0.2% or more at 0 degree incidence and wavelengths of 420 nm to 680 nm, which means that sufficient anti-reflection characteristics are not obtained.

[0142] [Table 16]

[0143] According to each embodiment, it is possible to provide an optical element, an optical system, an imaging device, and a method for manufacturing an optical element that are capable of sufficiently reducing the reflectance regardless of the refractive index of the base material.

[0144] Next, an overview of the optical element 300 in Examples 17 to 25 will be described with reference to Fig. 37. Fig. 37 is a schematic diagram of the optical element 300. The optical element 300 has a transparent substrate (base material) 200 and an antireflection film 100 consisting of four layers of film. The antireflection film 100 consists of, in order from the transparent substrate 200 toward the air side, a thin film layer (first layer) 01, a thin film layer (second layer) 02, a thin film layer (third layer) 03, and a thin film layer (fourth layer) 04.

[0145] At a wavelength of 550 nm, the refractive index of thin film layer 01 is n1, the refractive index of thin film layer 02 is n2, the refractive index of thin film layer 03 is n3, and the refractive index of thin film layer 04 is n4. Furthermore, assuming that the physical thickness of thin film layer 01 is d1 (nm), the physical thickness of thin film layer 02 is d2 (nm), the physical thickness of thin film layer 03 is d3 (nm), and the physical thickness of thin film layer 04 is d4 (nm), it is preferable that at least one of the following conditional expressions (15) to (22) is satisfied.

[0146] 1.56≦n1≦1.70 …(15) 1.30≦n2≦1.50 …(16) 1.56≦n3≦1.70 …(17) 1.10≦n4≦1.28 …(18) 40≦n1d1≦250 …(19) 10≦n2d2≦100 …(20) 10≦n3d3≦100 …(21) 100≦n4d4≦155 …(22) 200≦n1d1+n2d2+n3d3+n4d4≦550 …(23) If the refractive index or physical thickness of each material falls outside the range of conditional expressions (15) to (23), sufficient antireflection performance cannot be obtained.

[0147] More preferably, the numerical range of conditional expression (18) is set as in the following conditional expression (24).

[0148] 1.12≦n4≦1.22 …(24) It is more preferable that the numerical range of condition (18) be set as in the following condition (24a).

[0149] 1.15≦n4≦1.22 …(24a) The thin film layers 02, 03, and 04 of the optical element 300 in each embodiment are preferably made of a material containing an organic compound. In this embodiment, the term "organic compound" refers to a compound containing carbon, excluding compounds with simple structures such as carbon monoxide and carbon dioxide. The material containing the "organic compound" can be easily formed by a wet coating method.

[0150] Optical elements 301 and 302 according to one embodiment of the present invention shown in Figures 38 and 39 are schematic diagrams showing the case where the surfaces of transparent substrates 201 and 202 on which antireflection films 101 and 102 are formed are concave and convex. Only the concave shape shown in Figure 38 will be described below, but the same is true for the convex shape shown in Figure 39.

[0151] The optical element 301 has a shape in which the optical surface on which the anti-reflection film 101 is formed has a rotational symmetry axis (a reference axis, for example, a surface normal passing through the origin (surface vertex)), that is, a rotationally symmetric shape. However, each embodiment is not limited to this, and the optical surface on which the anti-reflection film 101 is formed may not be rotationally symmetric. In FIG. 38, position C is the rotation center of the lens surface of the transparent substrate 201 to which the anti-reflection film 101 is applied. That is, position C is the position (intersection) where the rotational symmetry axis (optical axis L) of the lens surface intersects with the lens surface of the transparent substrate 201. On the other hand, position Q is located at the farthest position from position C within the optically effective area on the lens surface of the transparent substrate 201. Here, the optically effective area refers to the area (effective diameter) through which effective light rays that contribute to image formation pass on the optical surface.

[0152] In other words, if the angle between the optical axis L and the normal to position Q (hereinafter referred to as the half angle) is φ, the half angle φ will be the maximum value within the optically effective area. The anti-reflection coating 101 is composed of a thin film layer (first layer) 11, a thin film layer (second layer) 12, a thin film layer (third layer) 13, and a thin film layer (fourth layer) 14, in that order from the transparent substrate 201. The physical film thickness of the thin film layer 12 at position C is d 2c (nm), the physical thickness of the thin film layer 13 is d 3c , the physical thickness of the thin film layer 14 is d 4c The physical thickness of the thin film layer 12 at the position Q is d 2q (nm), the physical thickness of the thin film layer 13 is d 3q (nm), the physical thickness of the thin film layer 14 is d 4q In this case, it is preferable to satisfy at least one of the following conditional expressions (25) to (27).

[0153] 1.0 <d2q / d 2c ≦1.3 …(25) 1.0 <d 3q / d 3c ≦1.3 …(26) 1.0 <d 4q / d 4c ≦1.3 …(27) In each embodiment, it is desirable that the film thicknesses of the thin film layers 12, 13, and 14 constituting the antireflection coating 101 are smallest at position C which is the center (center of the optical axis) of the antireflection coating 101 and increase with increasing distance from the center of the optical axis.

[0154] In each embodiment, it is preferable that the half opening angle φ (°) at the position Q satisfies the following conditional expression (28).

[0155] 25≦φ<90 …(28) The refractive index of the transparent substrate 201 is n S When this is set, it is preferable to satisfy the following conditional expression (29):

[0156] 1.45≦n S ≦2.10 …(29) 38 and 39, thin film layer 11 of antireflection coating 101 and thin film layer 21 of antireflection coating 102 are desirably made of a material containing an organic compound, similar to thin film layers 12, 13, 14 and thin film layers 22, 23, 24. Similarly, a wet film formation method, particularly a spin coating method, is desirably used as the formation method.

[0157] Although only the concave shape shown in FIG. 38 will be described below, the same applies to the convex shape shown in FIG.

[0158] In the thin film layer 11, the physical thickness of the thin film layer 11 at the position C is d 1c (nm), and the physical thickness of the thin film layer 11 at the position Q is d 1q When (nm), it is preferable to satisfy the following conditional expression (30):

[0159] 1.0 <d 1q / d 1c≦1.3 …(30) It is preferable that the thin film layers 11 and 13 satisfy the following conditional formula (31).

[0160] 0.9≦d1 / d3≦1.1 …(31) Moreover, the thin film layer 11 is preferably made of a material containing a polyimide resin, which is a "polymer compound containing an imide (-CO-NR-CO-) bond". Imide bonds are planar structures, and thin film layers having these structures tend to have molecular chains oriented parallel to the substrate when formed. Therefore, the adhesion in the vertical direction is weaker than the adhesion in the horizontal direction, and the thin film layer can be easily peeled off by applying an appropriate amount of an abrasive containing an alumina-based mineral to a cloth and rubbing it. In one embodiment of the present invention, the thin film layers 12, 13, and 14, which are the upper layers of the thin film layer 11, that is, the anti-reflection film 101, can be peeled off from the transparent substrate 201, making it easy to perform a regeneration process during the manufacturing process.

[0161] 40 and 41 show optical elements 303 and 304, which are one embodiment of the present invention. Optical elements 303 and 304 are schematic diagrams in which the surfaces of transparent substrates 203 and 204 on which antireflection films 103 and 104 are formed are concave and convex. Only the concave shape shown in Fig. 40 will be described below, but the same applies to the convex shape shown in Fig. 41.

[0162] The antireflection coating 103 is composed of, in order from the transparent substrate 203, a thin film layer 31, a thin film layer 32, a thin film layer 33, and a thin film layer 34. Like the thin film layers 12, 13, and 14 in the antireflection coating 101 described above, the thin film layers 32, 33, and 34 are desirably made of a material containing an organic compound, and satisfy the conditional expressions (25) to (27).

[0163] The thin film layer 31 may be made of a material containing aluminum oxide. Aluminum oxide has excellent barrier properties against water vapor and can prevent the substrate surface from becoming discolored. In this case, it is preferable that the following conditional formula (19a) is satisfied.

[0164] 120≦n1d1≦250 …(19a) When the thin film layer 31 is formed by a dry film forming method such as vapor deposition or sputtering, the incident angle of the vapor deposition material to the lens surface is large at the periphery of the large aperture lens, so the film thickness is smaller than that at the center. 31c (nm) and the physical thickness d of the thin film layer 31 at the position Q 31q It is preferable that (nm) satisfy the following conditional expression (32).

[0165] 0.5≦d 31q / d 31c <1.0 …(32) The refractive index of the transparent substrate 203 at a wavelength of 550 nm is n s When this is set, it is preferable to satisfy the following condition (33):

[0166] -0.1≦n s -n1≦0.1 …(33) The interface reflection is small when the difference in refractive index between the transparent substrate 203 and the thin film layer 31 is small. Even if the film thickness of the thin film layer 31 is uneven within the lens surface, the reflectance performance is unlikely to be biased.

[0167] The glass transition temperature T of the transparent substrate 203 g (° C.), it is preferable to satisfy the following conditional expression (34):

[0168] 450≦T g ≦550 …(34) Glass materials with low glass transition temperatures are prone to problems caused by the glass material, such as discoloration. By using aluminum oxide as the layer applied directly to the glass material, it is possible to suppress the decrease in reflectance caused by discoloration.

[0169] It is desirable that the thin film layers 04, 14, 24, 34, and 44 contain voids. Since the thin film layers 04, 14, 24, 34, and 44 contain voids, that is, air with a refractive index of 1.0, the refractive index can be reduced to the conditional formula (18) and the conditional formula (24). If the refractive index is less than 1.10, the ratio of voids contained in the layer is large, so the film strength is weakened. If the refractive index is greater than 1.28, sufficient anti-reflection performance cannot be obtained. In addition, an anti-soiling film or the like may be provided on the surface of the anti-reflection film of each embodiment (the surface of the thin film layers 04, 14, 24, 34, and 44) ​​as necessary. Examples of the anti-soiling film include films containing fluoropolymers, fluorosilane monomolecules, titanium oxide particles, and the like.

[0170] In each embodiment, the thin film layers 04, 14, 24, 34, and 44 are preferably made of solid particles, chain particles, or hollow particles. More preferably, they are made of hollow particles having holes inside. The holes may be either single-hole or multi-hole and can be selected appropriately. The material constituting the solid particles, chain particles, or hollow particles is preferably one with a low refractive index. For example, organic resins made of SiO2, MgF2, fluorine, silicon, etc. are listed, but SiO2 is more preferable because it is easy to manufacture the particles. The average particle diameter of the hollow particles is 15 nm or more and 100 nm or less, preferably 15 nm or more and 80 nm or less. If the average particle diameter of the hollow particles is less than 15 nm, it is difficult to stably produce the core particles. Also, if it exceeds 100 nm, the size of the gap between the particles becomes large, so large voids are likely to occur, and scattering occurs due to the size of the particles, which is not preferable.

[0171] The thin film layers 02, 12, 22, 32, and 42 are preferably made of a material containing solid particles, particularly solid silica particles, bound by a binder such as a siloxane bond, or a material containing an acrylic resin, which is a "polymer of acrylic acid ester or methacrylic acid ester."

[0172] The thin film layers 03, 13, 23, 33, and 43 are preferably made of a material containing a polyimide resin, which is a polymer compound containing an imide (-CO-NR-CO-) bond, or a material containing an epoxy resin, which is a resin cured by crosslinking epoxy groups having an oxacyclopropane (oxirane) structure, which is a three-ring ether.

[0173] In each embodiment, the thin film layers 11, 21, 12, 22, 32, 42, 13, 23, 33, 43, and 14, 24, 34, 44 are preferably formed by a wet film formation method in which a coating liquid containing a film material is applied and then dried or baked. The wet film formation method can coat a large area inexpensively. In particular, the spin coating method is preferable because the coating is performed while rotating the coating surface on a rotation axis, thereby suppressing the in-plane film thickness distribution.

[0174] The organic solvent that can be used in the coating liquid is not particularly limited as long as it does not impair the coating properties or performance, and known solvents can be used. For example, as a monohydric alcohol, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methylpropanol, 1-pentanol, 2-pentanol, and cyclopentanol can be used. Alternatively, for example, 2-methylbutanol, 3-methylbutanol, 1-hexanol, 2-hexanol, 3-hexanol, 4-methyl-2-pentanol, 2-methyl-1-pentanol, and 2-ethylbutanol can be used. Alternatively, for example, 2,4-dimethyl-3-pentanol, 3-ethylbutanol, 1-heptanol, 2-heptanol, 1-octanol, and 2-octanol can be used.

[0175] Alternatively, divalent or higher alcohols such as ethylene glycol and triethylene glycol may be used. Alternatively, ether alcohols may be used. For example, methoxyethanol, ethoxyethanol, propoxyethanol, isopropoxyethanol, butoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 1-propoxy-2-propanol, etc. Alternatively, ethers such as dimethoxyethane, diglyme, tetrahydrofuran, dioxane, diisopropyl ether, dibutyl ether, and cyclopentyl methyl ether may be used.

[0176] Alternatively, esters such as ethyl formate, ethyl acetate, n-butyl acetate, methyl lactate, ethyl lactate, ethylene glycol monomethyl ether acetate, and ethylene glycol monoethyl ether acetate may be used. Alternatively, esters such as ethylene glycol monobutyl ether acetate and propylene glycol monomethyl ether acetate may be used. Alternatively, various aliphatic or alicyclic hydrocarbons such as n-hexane, n-octane, cyclohexane, cyclopentane, and cyclooctane may be used. Alternatively, various aromatic hydrocarbons such as toluene, xylene, and ethylbenzene may be used.

[0177] Alternatively, various ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, etc. Various chlorinated hydrocarbons such as chloroform, methylene chloride, carbon tetrachloride, tetrachloroethane, etc. Alternatively, aprotic polar solvents such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, ethylene carbonate, etc. may be used. Two or more of these solvents may be mixed and used.

[0178] Furthermore, when solid particles, chain particles, or hollow particles are used in the fourth thin film layer 04, 14, 24, 34, 44, and when solid particles are used in the second thin film layer 02, 12, 22, 32, 42, it is preferable that they are bound by a binder in order to improve strength. It is preferable to use a siloxane bond as the binder. This is particularly suitable when using silica particles having many hydroxyl groups on the surface.

[0179] In each embodiment, the thin film layers 11, 21, 12, 22, 13, 23, and 14, 24 are made of materials that can be formed by a wet film-forming method, and therefore the materials themselves or the binder contain organic compounds. In addition, the anti-reflection films of each embodiment are not baked at high temperatures in the drying process after coating. For this reason, it is possible to use plastics that are easily deformed by heat or optical curable resins for the transparent substrates 201, 202, all of which can be formed by a wet film-forming method.

[0180] On the other hand, the thin film layers 31 and 41 are preferably formed by a dry film forming method such as a vapor deposition method or a sputtering method. In a dry film forming method such as a vapor deposition method or a sputtering method, the film is formed in a positional relationship in which the evaporation source and the center of the lens face each other. In the case of a large-angle lens, the incidence angle of the evaporated material to the lens surface is large in the peripheral part, so the film thickness is smaller than that in the central part. This causes film unevenness in the lens surface, and causes bias in the anti-reflection performance. However, when the conditional formula (19) is satisfied, the interface reflection between the transparent substrate 200 and the thin film layers 31 and 41 is small. Therefore, even if there is in-plane variation in the film thickness of the thin film layers 31 and 41, the bias in the reflectance performance is small.

[0181] Specific examples are given below. However, these are merely examples, and the present invention is not limited to the scope of the examples. EXAMPLES

[0182] FIG. 38 is a schematic cross-sectional view of an optical element 301 according to a seventeenth embodiment of the present invention. The optical element 301 of this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA) having a refractive index of 1.57 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of polyimide resin, the thin film layer 12 is made of a material mainly composed of solid silica, the thin film layer 13 is made of a material mainly composed of polyimide resin, and the thin film layer 14 is made of a material mainly composed of hollow silica. Table 1 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (37), and (30). Additionally, the thin film layers 11, 12, 13, and 14 contain an organic compound.

[0183] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0184] The solid silica coating liquid 1, the polyimide coating liquid 1, and the hollow silica coating liquid 1 form an anti-reflection film 101.

[0185] 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 2000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the polyimide coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0186] Figure 42 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths from 420 nm to 680 nm, which is an extremely good reflectance characteristic. Figure 43 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 17, the film thickness of each thin film layer at position Q is about 6% higher than at position C, but the reflectance characteristics are good, being 0.2% or less at wavelengths from 420 nm to 680 nm.

[0187] [Table 17] EXAMPLES

[0188] FIG. 39 is a schematic cross-sectional view of an optical element 302 according to an eighteenth embodiment of the present invention. The optical element 302 of this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-LAH66 (manufactured by OHARA) having a refractive index of 1.77 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed is convex. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 60 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of polyimide resin, the thin film layer 22 is made of a material mainly composed of solid silica, the thin film layer 23 is made of a material mainly composed of polyimide resin, and the thin film layer 24 is made of a material mainly composed of hollow silica. Table 18 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (27), and (30). Additionally, the thin film layers 21, 22, 23, and 24 contain an organic compound.

[0189] The method for forming the anti-reflection film 102 in this embodiment is as follows.

[0190] The solid silica coating liquid 1, the polyimide coating liquid 1, and the hollow silica coating liquid 1 form an anti-reflection film 102.

[0191] 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 3000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the polyimide coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating liquid was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0192] Figure 44 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths from 420 nm to 680 nm, which is an extremely good reflectance characteristic. Figure 45 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 18, the film thickness of each thin film layer at position Q is about 12% greater than at position C, but the reflectance at wavelengths from 420 nm to 680 nm is 0.2% or less, which is good.

[0193] [Table 18] EXAMPLES

[0194] FIG. 38 is a schematic cross-sectional view of an optical element 301 according to a nineteenth embodiment of the present invention. The optical element 301 of this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIH53 (manufactured by OHARA) with a refractive index of 1.85 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of polyimide resin, the thin film layer 12 is made of a material mainly composed of solid silica, the thin film layer 13 is made of a material mainly composed of polyimide resin, and the thin film layer 14 is made of a material mainly composed of hollow silica. Table 19 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (27), and (30). Additionally, the thin film layers 11, 12, 13, and 14 contain an organic compound.

[0195] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0196] The solid silica coating liquid 1, the polyimide coating liquid 2, and the hollow silica coating liquid 1 form an anti-reflection film 101.

[0197] 0.2 ml of the polyimide coating liquid 2 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 3000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the polyimide coating liquid 2 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the hollow silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0198] Figure 46 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths from 420 nm to 680 nm, which is an extremely good reflectance characteristic. Figure 47 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 19, the film thickness of each thin film layer at position Q is about 2% higher than at position C, but the reflectance characteristics are good, being 0.2% or less at wavelengths from 420 nm to 680 nm.

[0199] [Table 19] EXAMPLES

[0200] FIG. 39 is a schematic cross-sectional view of an optical element 302 according to a 20th embodiment of the present invention. The optical element 302 of this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is LPQ-1500 (manufactured by Mitsubishi Gas Chemical Company, Inc.) with a refractive index of 1.59 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed is a convex shape. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of polyimide resin, the thin film layer 22 is made of a material mainly composed of solid silica, the thin film layer 23 is made of a material mainly composed of polyimide resin, and the thin film layer 24 is made of a material mainly composed of hollow silica. Table 20 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (27), and (30). Additionally, the thin film layers 11, 12, 13, and 14 contain an organic compound.

[0201] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0202] The solid silica coating liquid 1, the polyimide coating liquid 2, and the hollow silica coating liquid 1 form an anti-reflection film 102.

[0203] 0.2 ml of the polyimide coating liquid 2 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 3500 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 2 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the hollow silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0204] Figure 48 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths from 420 nm to 680 nm, which is an extremely good reflectance characteristic. Figure 49 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 20, the film thickness of each thin film layer at position Q is about 3% higher than at position C, but it can be confirmed that the reflectance is 0.2% or less at wavelengths from 420 nm to 680 nm, which is good.

[0205] [Table 20] EXAMPLES

[0206] FIG. 38 is a schematic cross-sectional view of an optical element 301 according to a twenty-first embodiment of the present invention. The optical element 301 of this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is EP-9000 (manufactured by Mitsubishi Gas Chemical Company, Inc.) with a refractive index of 1.68 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. The thin film layer 11 is made of a material mainly composed of polyimide resin, the thin film layer 12 is made of a material mainly composed of solid silica, the thin film layer 13 is made of a material mainly composed of polyimide resin, and the thin film layer 14 is made of a material mainly composed of hollow silica. Table 21 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (27), (30), and (31). Additionally, the thin film layers 11, 12, 13, and 14 contain an organic compound.

[0207] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0208] The solid silica coating liquid 1, the polyimide coating liquid 1, and the hollow silica coating liquid 1 form an anti-reflection film 101.

[0209] 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0210] Figure 50 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths from 420 nm to 680 nm, which is an extremely good reflectance characteristic. Figure 51 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 21, the film thickness of each thin film layer at position Q is about 6% higher than at position C, but the reflectance characteristics are 0.2% or less at wavelengths from 420 nm to 680 nm, which is good.

[0211] [Table 21] EXAMPLES

[0212] FIG. 38 is a schematic cross-sectional view of an optical element 301 according to a twenty-second embodiment of the present invention. The optical element 301 of this embodiment is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-BSL7 (manufactured by OHARA) with a refractive index of 1.52 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 30 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of polyimide resin, the thin film layer 12 is made of a material mainly composed of solid silica, the thin film layer 13 is made of a material mainly composed of polyimide resin, and the thin film layer 14 is made of a material mainly composed of hollow silica. Table 22 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (27), (30), and (31). Additionally, the thin film layers 11, 12, 13, and 14 contain an organic compound.

[0213] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0214] The solid silica coating liquid 1, the polyimide coating liquid 2, and the hollow silica coating liquid 1 form an anti-reflection film 101.

[0215] 0.2 ml of the polyimide coating liquid 2 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the polyimide coating liquid 2 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0216] Figure 52 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is an extremely good reflectance characteristic. Figure 53 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 22, the film thickness of each thin film layer at position Q is about 3% greater than at position C, but the reflectance characteristics are good, being 0.2% or less at wavelengths of 420 nm to 680 nm.

[0217] [Table 22] EXAMPLES

[0218] FIG. 39 is a schematic cross-sectional view of an optical element 302 according to a twenty-third embodiment of the present invention. The optical element 302 of this embodiment is an optical element in which an antireflection film 102 is formed on a transparent substrate 202. The transparent substrate 202 is S-BAM12 (manufactured by OHARA) with a refractive index of 1.64 (wavelength 550 nm). The lens surface of the transparent substrate 202 on which the antireflection film 102 is formed is convex. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 21 is made of a material mainly composed of polyimide resin, the thin film layer 22 is made of a material mainly composed of solid silica, the thin film layer 23 is made of a material mainly composed of polyimide resin, and the thin film 24 is made of a material mainly composed of hollow silica. Table 23 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (27), (30), and (31). Moreover, the thin film layers 21, 22, 23, and 24 contain an organic compound.

[0219] The method for forming the anti-reflection film 102 in this embodiment is as follows.

[0220] The solid silica coating liquid 1, the polyimide coating liquid 1, and the hollow silica coating liquid 1 form an anti-reflection film 102.

[0221] 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0222] Figure 54 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths from 420 nm to 680 nm, which is an extremely good reflectance characteristic. Figure 55 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 23, the film thickness of each thin film layer at position Q is about 6% higher than at position C, but it can be confirmed that the reflectance is 0.2% or less at wavelengths from 420 nm to 680 nm, which is good.

[0223] [Table 23] EXAMPLES

[0224] 40 is a schematic cross-sectional view of an optical element 303 according to Example 24 of the present invention. The optical element 303 of this example is an optical element in which an antireflection film 103 is formed on a transparent substrate 203. The transparent substrate 203 is L-BAL43 (manufactured by OHARA Co., Ltd.) having a refractive index of 1.59 (wavelength 550 nm). The glass transition temperature T g The temperature (°C) is 493°C. The lens surface of the transparent substrate 203 on which the antireflection film 103 is formed has a concave shape. The half aperture angle φ at the position Q on the maximum effective beam diameter is 30 degrees. As for the layer materials, the thin film layer 31 is made of a material mainly composed of aluminum oxide, the thin film layer 32 is made of a material mainly composed of solid silica, the thin film layer 33 is made of a material mainly composed of polyimide resin, and the thin film layer 34 is made of a material mainly composed of hollow silica. Table 24 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (27), and (32) to (34). The thin film layers 32, 33, and 34 contain an organic compound.

[0225] The method for forming the anti-reflection film 103 in this embodiment is as follows.

[0226] The thin film layer 31 was formed by deposition. An electron beam was used to heat the evaporation material. In order to form a denser film, an ion beam assisted deposition method was used. The inside of the vacuum chamber of the deposition device was filled with 2×10 -3 The vacuum chamber was evacuated without heating until it reached a high vacuum of approximately 1×10 Pa. After it was confirmed that the inside of the vacuum chamber had reached a high vacuum state, Ar was introduced into the ion gun as an inert gas, and the ion gun was made to discharge. After the ion gun reached a stable state, oxygen was introduced into the vacuum chamber until the vacuum pressure reached 1×10 -2 Ion-assisted deposition was performed using oxygen ions at approximately 100 Pa. In the deposition method, when the half aperture angle is large, the film thickness decreases toward the periphery.

[0227] After the thin film layer 31 was formed by vapor deposition, 0.2 ml of the solid silica coating solution 1 was dropped onto the lens surface of the transparent substrate 203 on which the thin film 31 was formed, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating solution 1 was dropped onto the lens surface of the transparent substrate 202, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating solution 1 was continuously dropped onto the lens surface of the transparent substrate 203, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0228] FIG. 56 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. FIG. 57 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 24, at position Q, the film thickness of thin film layer 31 is about 13% less than at position C, and the film thicknesses of thin film layers 32, 33, and 34 are about 3% more than at position C, but the reflectance characteristics are 0.2% or less at wavelengths of 420 nm to 680 nm, which is good.

[0229] [Table 24] EXAMPLES

[0230] FIG. 41 is a schematic cross-sectional view of an optical element 304 according to a twenty-fifth embodiment of the present invention. The optical element 304 of this embodiment is an optical element in which an antireflection film 104 is formed on a transparent substrate 204. The transparent substrate 204 is L-TIL28 (manufactured by OHARA) having a refractive index of 1.69 (wavelength 550 nm). The lens surface of the transparent substrate 204 on which the antireflection film 104 is formed is convex. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 40 degrees. As for the layer materials, the thin film layer 41 is made of a material mainly composed of aluminum oxide, the thin film layer 42 is made of a material mainly composed of solid silica, the thin film layer 43 is made of a material mainly composed of polyimide resin, and the thin film layer 44 is made of a material mainly composed of hollow silica. Table 25 shows the details of the film configuration of the optical element of this embodiment. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), (25) to (27), and (32) to (34). The thin film layers 42, 43, and 44 each contain an organic compound. The method for forming the anti-reflection film 104 of this embodiment is as follows.

[0231] The thin film layer 41 was formed by a deposition method similar to that for the thin film layer 31 in Example 8.

[0232] After the thin film layer 41 was formed by vapor deposition, 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 204 on which the thin film 41 was formed, and spin-coated at 4000 rpm for 20 seconds. Next, 0.2 ml of the polyimide coating liquid 2 was continuously dropped onto the lens surface of the transparent substrate 204, and spin-coated at 4000 rpm for 20 seconds. Finally, 0.2 ml of the hollow silica coating liquid 1 was continuously dropped onto the lens surface of the transparent substrate 204, and spin-coated at 4000 rpm for 20 seconds. Then, the substrate was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0233] FIG. 58 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. FIG. 59 shows the reflectance characteristics at positions C and Q for an incident angle of 0 degrees. According to Table 25, at position Q, the film thickness of thin film layer 41 is about 23% less than at position C, and the film thickness of thin film layers 32, 33, and 34 is 5% more than at position C, but the reflectance characteristics are 0.2% or less at wavelengths of 420 nm to 680 nm, which is good.

[0234] [Table 25]

[0235] The optical elements of Examples 17 to 25 are also applicable to the optical system 401 of Example 15 described with reference to Fig. 32. The optical system 400 includes optical elements 301, 302, 303, and 304 on which the antireflection film of any one of Examples 17 to 25 is formed. The optical elements of Examples 17 to 25 are also applicable to the imaging device (digital camera 500) of Example 16 described with reference to Fig. 33.

[0236] Comparative Example 3 FIG. 38 shows a schematic cross-sectional view of an optical element according to Comparative Example 3 of the present invention. The optical element 301 of this comparative example is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA) with a refractive index of 1.57 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of aluminum oxide, the thin film layer 12 is made of a material mainly composed of magnesium fluoride, the thin film layer 13 is made of a material mainly composed of aluminum oxide, and the thin film layer 14 is made of a material mainly composed of hollow silica. Table 26 shows the details of the film configuration of the optical element of this comparative example. The refractive index and film thickness of each material satisfy the conditional expressions (15) to (23), but do not satisfy the conditional expressions (25) to (27).

[0237] The method for forming the anti-reflection film 101 of this comparative example is as follows. The thin film layers 11, 12, and 13 were formed by vapor deposition. The vapor deposition method was the same as in Example 8. After the thin film layers 11, 12, and 13 were formed by vapor deposition in this order, 0.2 ml of the hollow silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201 on which the thin films 11, 12, and 13 had been formed, and spin-coated at 4000 rpm for 20 seconds. Then, the film was dried for 24 hours or more in a clean room at a room temperature of 23°C.

[0238] FIG. 60 shows the reflectance characteristics at position C for angles of incidence of 0, 15, 30, 45, and 60 degrees. It can be seen that the reflectance is 0.2% or less at 0 degree incidence and wavelengths of 420 nm to 680 nm, which is a very good reflectance characteristic. However, when comparing the reflectance characteristics at positions C and Q for an incident angle of 0 degree in FIG. 61, it can be seen that the reflectance characteristic at position Q is lower than that at position C. According to Table 26, the film thickness of thin film layer 14 at position Q is 6% higher than that at position C, but the film thickness of thin film layers 11, 12, and 13 at position Q is 30% lower than that at position C. For this reason, it can be said that the reflectance characteristic at position Q has decreased.

[0239] [Table 26]

[0240] Comparative Example 4 FIG. 62 shows a schematic cross-sectional view of an optical element according to Comparative Example 4 of the present invention. The optical element 301 of this comparative example is an optical element in which an antireflection film 101 is formed on a transparent substrate 201. The transparent substrate 201 is S-TIL26 (manufactured by OHARA) with a refractive index of 1.57 (wavelength 550 nm). The lens surface of the transparent substrate 201 on which the antireflection film 101 is formed is concave. The half-open angle φ at the position Q on the maximum effective diameter of the light beam is 45 degrees. As for the layer materials, the thin film layer 11 is made of a material mainly composed of polyimide resin, the thin film layer 12 is made of a material mainly composed of solid silica, the thin film layer 13 is made of a material mainly composed of polyimide resin, and the thin film layer 14 is made of a material mainly composed of chain silica. Table 27 shows the details of the film configuration of the optical element of this comparative example. The refractive index of the thin film layer 13 does not satisfy conditional formula (18).

[0241] The method for forming the anti-reflection film 101 of this embodiment is as follows.

[0242] (Chain Silica Coating Liquid 2) The solid silica coating liquid 1, the polyimide coating liquid 1, and the chain silica coating liquid 2 form an anti-reflection film 101.

[0243] 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 3000 rpm for 20 seconds. Next, 0.2 ml of the solid silica coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the polyimide coating liquid 1 was dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. Furthermore, 0.2 ml of the chain silica coating liquid 2 was continuously dropped onto the lens surface of the transparent substrate 201, and spin-coated at 4000 rpm for 20 seconds. After that, it was dried for 24 hours or more in a clean room at room temperature of 23°C.

[0244] 62 shows the reflectance characteristics for angles of incidence of 0, 15, 30, 45, and 60 degrees at position C. The reflectance is 0.2% or more at 0 degree incidence and wavelengths of 420 nm to 680 nm, which indicates that sufficient anti-reflection characteristics are not obtained.

[0245] [Table 27]

[0246] The disclosure of each embodiment includes the following configurations and methods. (Configuration 1) An optical element having a substrate and an anti-reflection coating, the antireflection coating comprises a first layer formed on the substrate, a second layer formed on the first layer, and a third layer formed on the second layer; each of the first to third layers contains an organic compound; When the refractive index of the third layer at a wavelength of 550 nm is n3, 1.10≦n3≦1.28 An optical element characterized by satisfying the following conditional expression: (Configuration 2) An optical element having a substrate and an anti-reflection coating, the antireflection coating comprises a first layer formed on the substrate, a second layer formed on the first layer, and a third layer formed on the second layer; When the refractive index of the first layer at a wavelength of 550 nm is n1, the refractive index of the second layer at a wavelength of 550 nm is n2, the refractive index of the third layer at a wavelength of 550 nm is n3, the physical thickness of the first layer is d1 (nm), the physical thickness of the second layer is d2 (nm), and the physical thickness of the third layer is d3 (nm), 1.30≦n1≦1.50 1.56≦n2≦1.70 1.10≦n3≦1.28 10≦n1d1≦155 10≦n2d2≦155 100≦n3d3≦155 200≦n1d1+n2d2+n3d3≦300 An optical element characterized by satisfying the following conditional expression: (Configuration 3) 3. The optical element according to claim 2, wherein each of the first to third layers contains an organic compound. (Configuration 4) The physical thickness of the first layer, the physical thickness of the second layer, and the physical thickness of the third layer at the intersection of a reference axis passing through the vertex of the optical surface on which the antireflection film is formed in the base material and the optical surface are respectively defined as d 1c , d 2c , and d 3c year, In the effective area of ​​the optical surface, the physical thickness of the first layer, the physical thickness of the second layer, and the physical thickness of the third layer at the position farthest from the intersection are respectively defined as d 1q , d 2q , and d 3q When 1.0 <d 1q / d 1c ≦1.3 1.0 <d 2q / d 2c ≦1.3 1.0 <d 3q / d 3c ≦1.3 4. The optical element according to any one of configurations 1 to 3, which satisfies the following conditional expression: (Configuration 5) 5. The optical element according to any one of configurations 1 to 4, wherein the physical film thickness of each of the first layer and the second layer is smallest at the center of the antireflection film and increases with increasing distance from the center. (Configuration 6) 6. The optical element according to any one of configurations 1 to 5, wherein the first layer contains an acrylic resin. (Configuration 7) 6. The optical element of any one of configurations 1 to 5, wherein the first layer includes solid particles. (Configuration 8) 8. The optical element according to any one of configurations 1 to 7, wherein the second layer contains an epoxy resin or a polyimide resin. (Configuration 9) The refractive index of the substrate at a wavelength of 550 nm is n s When 1.45≦n s <= 2.10 9. The optical element according to any one of configurations 1 to 8, which satisfies the following conditional expression: (Configuration 10) An optical element having a substrate and an anti-reflection coating, the antireflection coating comprises a first layer formed on the substrate, a second layer formed on the first layer, a third layer formed on the second layer, and a fourth layer formed on the third layer; each of the second to fourth layers contains an organic compound; When the refractive index of the fourth layer at a wavelength of 550 nm is n4, 1.10≦n4≦1.28 An optical element characterized by satisfying the following conditional expression: (Configuration 11) An optical element having a substrate and an anti-reflection coating, the antireflection coating comprises a first layer formed on the substrate, a second layer formed on the first layer, a third layer formed on the second layer, and a fourth layer formed on the third layer; Let n1 be the refractive index of the first layer at a wavelength of 550 nm, n2 be the refractive index of the second layer at a wavelength of 550 nm, n3 be the refractive index of the third layer at a wavelength of 550 nm, n4 be the refractive index of the fourth layer at a wavelength of 550 nm, d1 (nm) be the physical thickness of the first layer, d2 (nm) be the physical thickness of the second layer, d3 (nm) be the physical thickness of the third layer, and d4 (nm) be the physical thickness of the fourth layer. 1.56≦n1≦1.70 1.30≦n2≦1.50 1.56≦n3≦1.70 1.10≦n4≦1.28 40≦n1d1≦250 10≦n2d2≦100 10≦n3d3≦100 100≦n4d4≦155 200≦n1d1+n2d2+n3d3+n4d4≦550 An optical element characterized by satisfying the following conditional expression: (Configuration 12) 12. The optical element according to claim 11, wherein each of the second to fourth layers contains an organic compound. (Configuration 13) 13. The optical element according to any one of configurations 10 to 12, wherein the first layer contains an organic compound. (Configuration 14) The physical thickness of the second layer, the physical thickness of the third layer, and the physical thickness of the fourth layer at the intersection of a reference axis passing through the vertex of the optical surface on which the antireflection film is formed in the base material and the optical surface are respectively defined as d 2c , d 3c , and d 4c year, In the effective area of ​​the optical surface, the physical thickness of the second layer, the physical thickness of the third layer, and the physical thickness of the fourth layer at the position farthest from the intersection are respectively defined as d 2q , d 3q , and d 4q When 1.0 <d 2q / d 2c ≦1.3 1.0 <d 3q / d 3c ≦1.3 1.0 <d 4q / d 4c ≦1.3 14. The optical element according to any one of configurations 10 to 13, which satisfies the following conditional expression: (Configuration 15) 15. The optical element according to any one of configurations 10 to 14, wherein the first layer contains a polyimide resin. (Configuration 16) The physical thickness of the first layer at the intersection of a reference axis passing through the vertex of the optical surface on which the antireflection film is formed in the base material and the optical surface is defined as d 1c year, The physical thickness of the first layer at the position farthest from the intersection in the effective area of ​​the optical surface is d 1q When 1.0 <d 1q / d 1c ≦1.3 16. The optical element according to claim 15, wherein the following condition is satisfied: (Configuration 17) 0.9≦d1 / d3≦1.1 13. The optical element according to claim 2, 3, 11, or 12, which satisfies the following condition: (Configuration 18) 18. The optical element of any one of configurations 10 to 17, wherein the first layer contains aluminum oxide. (Configuration 19) The physical thickness of the first layer at the intersection of a reference axis passing through the vertex of the optical surface on which the antireflection film is formed in the base material and the optical surface is defined as d 31c year, The physical thickness of the first layer at the position farthest from the intersection in the effective area of ​​the optical surface is d 31q When 0.5≦d 31q / d 31c <1.0 19. The optical element according to embodiment 18, which satisfies the following condition: (Configuration 20) The refractive index of the substrate at a wavelength of 550 nm is n s When 1.55≦n s ≦1.70 20. The optical element according to any one of structures 1 to 19, which satisfies the following conditional expression: (Configuration 21) The glass transition temperature of the substrate is T g (℃), 450≦T g <=550 21. The optical element according to any one of Structures 1 to 20, which satisfies the following conditional expression: (Configuration 22) 20. The optical element of configuration 4, 14, 16, or 19, wherein the reflectance of the antireflection coating for light incident on the intersection at an incident angle of 0 degrees is 0.5% or less in a wavelength range of 450 nm or more and 650 nm or less, and the reflectance of the antireflection coating for light incident on the intersection at an incident angle of 30 degrees is 1.0% or less. (Configuration 23) 1.12≦n3≦1.25 23. The optical element according to any one of structures 1 to 22, which satisfies the following conditional expression: (Configuration 24) An optical element described in any one of structures 10 to 23, characterized in that the physical film thicknesses of the second layer, the third layer, and the fourth layer are smallest at the center of the antireflection film and increase with increasing distance from the center. (Configuration 25) 25. The optical element according to any one of configurations 1 to 24, wherein the layer in the antireflection coating farthest from the substrate contains voids. (Configuration 26) 26. The optical element according to any one of configurations 1 to 25, wherein the layer in the antireflection coating that is farthest from the substrate contains at least one of solid particles, chain particles, and hollow particles. (Configuration 27) 27. The optical element of claim 26, wherein at least one of the solid particles, the chain particles, and the hollow particles is made of silica. (Configuration 28) 17. The optical element of any one of claims 10 to 16, wherein the second layer comprises solid particles. (Configuration 29) 29. The optical element according to any one of structures 1 to 28, further comprising a film containing a fluororesin formed on the antireflection film. (Configuration 30) 30. An optical system comprising a plurality of optical elements including the optical element according to any one of claims 1 to 29. (Configuration 31) When the half aperture angle at the position of the effective diameter of the optical surface on which the antireflection film is formed in the base material is φ (degrees), 25≦φ<90 31. The optical system according to claim 30, wherein the following condition is satisfied: (Configuration 32) An optical system including the optical element according to configuration 30; and an image sensor for capturing an image of a subject via the optical system. (Method 1) A method for manufacturing an optical element having a substrate and an antireflection film including first to third layers, comprising the steps of: forming the first layer on the substrate by a wet coating method; forming the second layer on the first layer by a wet coating method; forming the third layer on the second layer by a wet coating method; When the refractive index of the third layer at a wavelength of 550 nm is n3, 1.10≦n3≦1.28 The manufacturing method is characterized in that the following conditional expressions are satisfied. (Method 2) A method for manufacturing an optical element having a substrate and an antireflection film including first to fourth layers, comprising the steps of: forming the first layer on the substrate; forming the second layer on the first layer by a wet coating method; forming the third layer on the second layer by a wet coating method; forming the fourth layer on the third layer by a wet coating method; When the refractive index of the fourth layer at a wavelength of 550 nm is n4, 1.10≦n4≦1.28 The manufacturing method is characterized in that the following conditional expressions are satisfied. (Method 3) 3. The manufacturing method according to method 1 or 2, wherein the wet coating method is a spin coating method.

[0247] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these embodiments, and various modifications and changes are possible within the scope of the gist of the present invention. [Explanation of symbols]

[0248] 01, 11, 21 Thin film layer (first layer) 02, 12, 22 Thin film layer (second layer) 03, 13, 23 Thin film layer (third layer) 100, 102, 102 Anti-reflection coating 200, 201, 202 base material 300, 301, 302 Optical elements

Claims

1. An optical element having a substrate and an anti-reflection coating, the antireflection film comprises a first layer formed on the substrate, a second layer formed on the first layer, and a third layer formed on the second layer; each of the first to third layers contains an organic compound; The refractive index of the third layer at a wavelength of 550 nm is n 3 When 1.10≦n 3 ≦1.28 An optical element characterized by satisfying the following conditional expression:

2. An optical element having a substrate and an anti-reflection coating, the antireflection film comprises a first layer formed on the substrate, a second layer formed on the first layer, and a third layer formed on the second layer; The refractive index of the first layer at a wavelength of 550 nm is n 1 The refractive index of the second layer at a wavelength of 550 nm is n 2 The refractive index of the third layer at a wavelength of 550 nm is n 3 , the physical thickness of the first layer is d 1 (nm), the physical thickness of the second layer is d 2 (nm), the physical thickness of the third layer is d 3 (nm), 1.30≦n 1 ≦1.50 1.56≦n 2 ≦1.70 1.10≦n 3 ≦1.28 10≦n 1 d 1 ≦155 10≦n 2 d 2 ≦155 100≦n 3 d 3 ≦155 200≦n 1 d 1 +n 2 d 2 +n 3 d 3 ≦300 An optical element characterized by satisfying the following conditional expression:

3. 3. The optical element according to claim 2, wherein each of the first to third layers contains an organic compound.

4. The physical thickness of the first layer, the physical thickness of the second layer, and the physical thickness of the third layer at the intersection of a reference axis passing through the vertex of the optical surface on which the antireflection film is formed in the base material and the optical surface are respectively represented by d 1c , d 2c , and d 3c year, In the effective area of ​​the optical surface, the physical thickness of the first layer, the physical thickness of the second layer, and the physical thickness of the third layer at the position farthest from the intersection are respectively defined as d 1q , d 2q , and d 3q When 1.0<d 1q / d 1c ≦1.3 1.0<d 2q / d 2c ≦1.3 1.0<d 3q / d 3c ≦1.3 4. The optical element according to claim 1, which satisfies the following condition:

5. 4. The optical element according to claim 1, wherein the physical thickness of each of the first layer and the second layer is smallest at the center of the antireflection film and increases with increasing distance from the center.

6. 4. The optical element according to claim 1, wherein the first layer contains an acrylic resin.

7. 4. The optical element according to claim 1, wherein the first layer comprises solid particles.

8. 4. The optical element according to claim 1, wherein the second layer contains an epoxy resin or a polyimide resin.

9. The refractive index of the substrate at a wavelength of 550 nm is n s When 1.45≦n s ≦2.10 4. The optical element according to claim 1, which satisfies the following condition:

10. An optical element having a substrate and an anti-reflection coating, the antireflection coating comprises a first layer formed on the substrate, a second layer formed on the first layer, a third layer formed on the second layer, and a fourth layer formed on the third layer; each of the second to fourth layers contains an organic compound; The refractive index of the fourth layer at a wavelength of 550 nm is n 4 When 1.10≦n 4 ≦1.28 An optical element characterized by satisfying the following conditional expression:

11. An optical element having a substrate and an anti-reflection coating, the antireflection coating comprises a first layer formed on the substrate, a second layer formed on the first layer, a third layer formed on the second layer, and a fourth layer formed on the third layer; The refractive index of the first layer at a wavelength of 550 nm is n 1 The refractive index of the second layer at a wavelength of 550 nm is n 2 The refractive index of the third layer at a wavelength of 550 nm is n 3 The refractive index of the fourth layer at a wavelength of 550 nm is n 4 , the physical thickness of the first layer is d 1 (nm), the physical thickness of the second layer is d 2 (nm), the physical thickness of the third layer is d 3 (nm), the physical thickness of the fourth layer is d 4 (nm), 1.56≦n 1 ≦1.70 1.30≦n 2 ≦1.50 1.56≦n 3 ≦1.70 1.10≦n 4 ≦1.28 40≦n 1 d 1 ≦250 10≦n 2 d 2 ≦100 10≦n 3 d 3 ≦100 100≦n 4 d 4 ≦155 200≦n 1 d 1 +n 2 d 2 +n 3 d 3 +n 4 d 4 ≦550 An optical element characterized by satisfying the following conditional expression:

12. The optical element according to claim 11 , wherein each of the second to fourth layers contains an organic compound.

13. 13. The optical element according to claim 10, wherein the first layer comprises an organic compound.

14. The physical thickness of the second layer, the physical thickness of the third layer, and the physical thickness of the fourth layer at the intersection of a reference axis passing through the vertex of the optical surface on which the antireflection film is formed in the base material and the optical surface are respectively denoted by d 2c , d 3c , and d 4c year, In the effective area of ​​the optical surface, the physical thickness of the second layer, the physical thickness of the third layer, and the physical thickness of the fourth layer at the position farthest from the intersection are respectively defined as d 2q , d 3q , and d 4q When 1.0<d 2q / d 2c ≦1.3 1.0<d 3q / d 3c ≦1.3 1.0<d 4q / d 4c ≦1.3 13. The optical element according to claim 10, which satisfies the following condition:

15. 13. The optical element according to claim 10, wherein the first layer contains a polyimide resin.

16. The physical thickness of the first layer at the intersection of a reference axis passing through the vertex of the optical surface on which the antireflection film is formed in the base material and the optical surface is defined as d 1c year, The physical thickness of the first layer at the position farthest from the intersection in the effective area of ​​the optical surface is d 1q When 1.0<d 1q / d 1c ≦1.3 16. The optical element according to claim 15, which satisfies the following condition:

17. 0.9≦d 1 / d 3 ≦1.1 13. The optical element according to claim 2, 3, 11, or 12, which satisfies the following condition:

18. 13. The optical element according to claim 10, wherein the first layer comprises aluminum oxide.

19. The physical thickness of the first layer at the intersection of a reference axis passing through the vertex of the optical surface on which the antireflection film is formed in the base material and the optical surface is defined as d 31c year, The physical thickness of the first layer at the position farthest from the intersection in the effective area of ​​the optical surface is d 31q When 0.5≦d 31q / d 31c <1.0 20. The optical element according to claim 18, which satisfies the following condition:

20. The refractive index of the substrate at a wavelength of 550 nm is n s When 1.55≦n s ≦1.70 13. The optical element according to claim 1, wherein the following condition is satisfied:

21. The glass transition temperature of the substrate is T g (℃), 450≦T g ≦550 13. The optical element according to claim 1, wherein the following condition is satisfied:

22. 5. The optical element according to claim 4, wherein the reflectance of the anti-reflection film for light incident on the intersection at an incident angle of 0 degrees is 0.5% or less in a wavelength range of 450 nm or more and 650 nm or less, and the reflectance of the anti-reflection film for light incident on the intersection at an incident angle of 30 degrees is 1.0% or less.

23. 1.12≦n 3 ≦1.25 13. The optical element according to claim 1, wherein the following condition is satisfied:

24. 13. The optical element according to claim 10, wherein the physical thickness of each of the second layer, the third layer, and the fourth layer is smallest at the center of the anti-reflection film and increases with increasing distance from the center.

25. 13. The optical element according to claim 1, wherein the layer of the antireflection film farthest from the substrate contains a gap.

26. 13. The optical element according to claim 1, wherein a layer of the antireflection coating that is farthest from the substrate contains at least one of solid particles, chain particles, and hollow particles.

27. 27. The optical element according to claim 26, wherein at least one of the solid particles, the chain particles, and the hollow particles is made of silica.

28. 13. The optical element according to any one of claims 10 to 12, wherein the second layer comprises solid particles.

29. 13. The optical element according to claim 1, further comprising a film containing a fluororesin formed on the antireflection film.

30. An optical system comprising a plurality of optical elements including the optical element according to claim 1 .

31. When the half aperture angle at the position of the effective diameter of the optical surface of the base material on which the antireflection film is formed is φ (degrees), 25≦φ<90 31. The optical system according to claim 30, wherein the following condition is satisfied:

32. An optical system including the optical element according to claim 30; and an image sensor for capturing an image of a subject via the optical system.

33. A method for manufacturing an optical element having a substrate and an antireflection film including first to third layers, comprising the steps of: forming the first layer on the substrate by a wet coating method; forming the second layer on the first layer by a wet coating method; forming the third layer on the second layer by a wet coating method; The refractive index of the third layer at a wavelength of 550 nm is n 3 When 1.10≦n 3 ≦1.28 The manufacturing method is characterized in that the following conditional expressions are satisfied.

34. A method for manufacturing an optical element having a substrate and an antireflection film including first to fourth layers, comprising the steps of: forming the first layer on the substrate; forming the second layer on the first layer by a wet coating method; forming the third layer on the second layer by a wet coating method; forming the fourth layer on the third layer by a wet coating method; The refractive index of the fourth layer at a wavelength of 550 nm is n 4 When 1.10≦n 4 ≦1.28 The manufacturing method is characterized in that the following conditional expressions are satisfied.

35. 35. The method according to claim 33, wherein the wet coating method is a spin coating method.

Citation Information

Patent Citations

  • Coating compositions forming organic antireflection layer and antifouling layer, and article having organic antireflection layer and antifouling layer

    JP2007310053A

  • Optical article and method of manufacturing optical article

    JP2008096702A

  • Antireflection member, and polarizer, image display device and antireflection article including antireflection member

    JP2020166236A

  • Antireflection film and optical component having the same, interchangeable lens and imaging device

    JP2009162989A