Separator, method for manufacturing the same, and secondary battery including the same
A separator with a coating layer of hollow conductive particles and inorganic particles addresses lithium dendrite issues, enhancing battery safety and performance by preventing dendrite formation and swelling, ensuring high capacity and conductivity.
Patent Information
- Application Number
- JP2024082869
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-05
AI Technical Summary
Lithium dendrites formed during charging and discharging processes increase internal resistance, reduce efficiency, and can cause internal short circuits and safety issues in secondary batteries.
A separator with a coating layer containing hollow conductive particles and inorganic particles is applied on both sides of a porous substrate, utilizing the difference in specific gravity to form a conductive layer that prevents lithium dendrite formation and accommodates swelling, thereby enhancing battery safety and performance.
The separator effectively suppresses lithium dendrite growth, maintains conductivity, and prevents swelling, ensuring high capacity and safety in secondary batteries.
Smart Images

Figure 2024169369000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a separator, a manufacturing method thereof, and a secondary battery including the same. In particular, the present disclosure relates to a separator including hollow conductive particles, a manufacturing method thereof, and a secondary battery including the same. [Background technology]
[0002] Recently, secondary batteries have become larger and have higher capacities in order to be used in electric vehicles and the like, and ensuring the safety of the batteries has become a very important factor.
[0003] A lithium secondary battery is a battery that is composed of a negative electrode, a positive electrode, and an electrolyte and a separator that provide a path for lithium ions to move between the negative electrode and the positive electrode. When lithium ions are inserted into and extracted from both the positive and negative electrodes, electrical energy is generated through oxidation and reduction reactions.
[0004] However, after several charge / discharge cycles, the electrical isolation of lithium ions and the accumulation of dead lithium ions form irregular needle-like dendrites. The growth of the dendrites not only increases the internal resistance of the battery and reduces the charge / discharge efficiency of the battery, but can also destroy the separator and cause an internal short circuit in the battery.
[0005] That is, lithium dendrites that grow during repeated charging and discharging can cause internal short circuits in the battery, resulting in fatal safety issues, the surface of newly formed and exposed lithium dendrites reacts with the electrolyte, causing the liquid electrolyte to quickly dry up, and there are problems such as significant changes in the total volume of the battery due to changes in the thickness of the electrode that occur during the charging and discharging process when lithium peels off / deposits.
[0006] Therefore, Korean Patent Publication No. 10-2019-0046237 prevents internal short circuits caused by dendrites by providing a metal ion receptor in a battery cell to absorb the generated dendrites. However, there is a disadvantage that the energy capacity is lower than that of existing batteries due to the additional space for receiving the dendrites, i.e., the space occupied by the metal ion receptor, and there is a problem that the manufacturing method for forming the metal ion receptor is complicated. There is a disadvantage that the capacity of the dendrites that the metal ion receptor can receive is limited, and the life of the secondary battery cannot be substantially extended. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] : Korean Patent Publication No. 10-2019-0046237 (May 7, 2019) Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present disclosure is to provide a separator that can suppress the formation and growth of dendrites and ensure the safety of the battery.
[0009] Another object of the present invention is to provide a new separator capable of internally accommodating swelling caused by an electrolyte or the like.
[0010] Another object of the present invention is to provide a new separator that can prevent the electrical isolation of lithium ions and the accumulation of dead lithium ions, and suppress the growth of lithium dendrites.
[0011] In addition, the present invention aims to provide a new separator that contains hollow conductive particles having a shell layer made of a conductive material on the surface, thereby preventing short circuits caused by electrical leakage and further improving the safety of batteries.
[0012] In addition, after preparing a coating composition containing hollow conductive particles and inorganic particles, a coating layer can be formed in a single coating process. In the process of forming the coating layer, the hollow conductive particles, which have a relatively low specific gravity compared to the inorganic particles, form the coating layer while floating, so that a separate coating process is not required. This is an object of the present invention to provide a new separator that can be manufactured in a single coating process.
[0013] Another object of the present invention is to provide a novel separator in which the hollow conductive particles function as a buffer capable of internally accommodating swelling caused by an electrolyte, thereby suppressing swelling and preventing elution of the electrolyte.
[0014] Another object of the present disclosure is to provide a secondary battery whose safety is ensured by including a separator according to an embodiment of the present disclosure. [Means for solving the problem]
[0015] One aspect of the present disclosure provides a separator comprising a porous substrate and a coating layer located on one or both sides of the porous substrate and containing inorganic particles and hollow conductive particles. The separator may be a separator used to separate a positive electrode and a negative electrode of a secondary battery. The coating layer may be directly disposed on the surface of the porous substrate. Alternatively, the coating layer may be indirectly disposed on the surface of the porous substrate, which means that there may be an additional inorganic particle layer between the surface of the porous substrate and the coating layer. The additional inorganic particle layer may be further included between the porous substrate and the coating layer, but may not contain hollow conductive particles, and conventionally refers to a layer formed of inorganic particles commonly used in the technical field of separators suitable for batteries, such as the ceramic coating layer of a ceramic coating separator (CCS). The separator has a flat form having two surfaces. When the coating layer is disposed / present on both sides of the porous substrate, the coating layer may be formed in two layers on opposite sides of the porous substrate. The properties of the two layers may be identical to each other.
[0016] In one embodiment, when the surface of the coating layer facing the porous substrate is defined as a first surface and the surface opposite to the first surface is defined as a second surface, the content of the hollow conductive particles in the second surface may be higher than that in the first surface. The content of the hollow conductive particles in the first surface and the second surface may be determined by any suitable method known to those skilled in the art. In the present disclosure, the following method may be applied: A focused ion beam milling (FIB) is applied to cut the coating layer of the separator to obtain a cross section of the coating layer. Then, the distribution of the hollow conductive particles in the thickness direction of the coating layer (i.e., the direction from the second surface to the first surface or the direction from the first surface to the second surface) may be determined using, for example, SEM, EDS or FTIR ("Fourier transform infrared spectroscopy"). When using SEM, the surface of the cut coating layer may be scanned to generate a sample image, and the image thus obtained may be observed. Using EDS and FTIR, the distribution of hollow conductive particles composed of polymers can be quantitatively confirmed by elemental analysis of Al, C, O, etc.
[0017] In one embodiment, the coating layer may have a gradient in which the content of the hollow conductive particles increases from the first surface to the second surface. The term "gradient" may refer to a general tendency for the content of the hollow conductive particles to increase on the side opposite the first surface, and the increase may be a continuous or linear structure, or the increase may be nonlinear, and may alternatively include a structure in which the hollow conductive particles have a predetermined content intermittently (but do not intermittently decrease).
[0018] In one embodiment, the coating layer may include an inorganic particle layer including inorganic particles, and a conductive layer formed by suspending hollow conductive particles on the inorganic particle layer.
[0019] In one embodiment, the coating layer may include an inorganic particle sub-layer including inorganic particles and a conductive sub-layer formed by hollow conductive particles. The inorganic particle sub-layer may be formed on a first surface facing the porous substrate, and the conductive sub-layer including hollow conductive particles may be formed on a second surface opposite to the first surface. In the sub-layer, the hollow conductive particles may be suspended on the inorganic particles of the inorganic particle sub-layer. In the present disclosure, the term "suspended" refers to a situation in which hollow conductive particles, which are present in the coating composition and a slurry for producing the same and generally have a lower specific gravity than the inorganic particles present in the coating composition and a slurry for producing the same due to their hollow structure, are arranged by themselves toward the surface of the coating layer according to gravity when the coating layer is formed. Therefore, the arrangement of each particle is based on the principle that the higher the specific gravity, the more such particles (inorganic particles) sink to the surface facing the porous substrate, while the lower the specific gravity, the more such particles (hollow conductive particles) rise toward the outer surface of the porous substrate.
[0020] In one embodiment, the hollow conductive particles may have a void ratio of 5 to 97%, 50 to 95%, 60 to 90%, 70 to 85%, or 75 to 85%, but is not limited thereto.
[0021] In one embodiment, the hollow conductive particles may have an average outer diameter of 10 nm to 10 μm, 500 nm to 2 μm, or 700 nm to 1200 nm, but is not limited thereto. The average outer diameter refers to the average diameter of two or more particles.
[0022] In one embodiment, the hollow conductive particle may include a hollow core having a hollow structure with an open interior, and a shell layer made of at least one conductive material selected from the group consisting of metals and conductive polymers.
[0023] In one embodiment, the hollow conductive particle may further include a structural material layer between the hollow core and the shell layer to maintain the hollow structure.
[0024] In one embodiment, the structure material layer may include at least one selected from an inorganic material and a crosslinked polymer.
[0025] In one embodiment, the inorganic material may be an oxide, a carbon material, or a mixture thereof, and the crosslinked polymer may include at least one selected from a styrene-based, an acrylic-based, and a fluorine-based polymer, but is not limited thereto.
[0026] In one embodiment, an inorganic particle layer may be further included between the porous substrate and the coating layer. Here, the inorganic particle layer means a layer made of inorganic particles, i.e., a ceramic layer, which is generally used in the art to distinguish it from the coating layer. Specifically, for example, it may be a layer made of only inorganic particles and having pores formed therebetween, or a layer in which inorganic particles are bound by a binder and have pores formed therebetween. Here, the inorganic particle layer may not include the hollow conductive particles.
[0027] Yet another aspect of the present disclosure provides a method for manufacturing a separator, the method including: applying a coating composition including inorganic particles and hollow conductive particles onto one or both sides of a porous substrate to form a coating layer; and drying the coating layer.
[0028] In one embodiment, the method may further include a step of applying vibration before or simultaneously with the drying step.
[0029] In one embodiment, the method may further include a step of leaving the separator coated with the coating composition unattended after the coating step and before drying.
[0030] In one embodiment, the coating composition can be applied multiple times on one or both sides of the porous substrate, and for this purpose, the coating process can be performed by applying the coating to each surface, allowing the applied coating to stand, and then applying a second coating after the first coating has dried.
[0031] In one aspect, after the coating step and the drying step, the hollow conductive particles may float on the surface of the coating layer to form a gradient, or a conductive layer made of the hollow conductive particles may be formed on the surface.
[0032] In one embodiment, the coating layer may have a gradient formed by hollow conductive particles formed on the surface of the coating layer after the coating and drying steps. The coating layer may form a conductive sublayer formed by hollow conductive particles formed on the surface. In such a sublayer, the hollow conductive particles may be suspended above the inorganic particles forming the inorganic particle sublayer.
[0033] In one embodiment, the coating composition may have a solid content of 10 to 60% by weight, 20 to 50% by weight, or 20 to 40% by weight, but is not limited thereto.
[0034] In one embodiment, the coating composition may include, but is not limited to, 0.2 to 20 parts by weight, 0.2 to 10 parts by weight, 0.5 to 10 parts by weight, or 0.5 to 5 parts by weight of the hollow conductive particles relative to 100 parts by weight of the inorganic particles.
[0035] In one embodiment, the drying may be performed with hot air at 25 to 100° C., 25 to 80° C., or 30 to 60° C. In general, drying is performed until there is no further detectable change in weight.
[0036] Yet another aspect of the present disclosure provides a secondary battery including the separator according to the above aspect.
[0037] Also provided is a method for manufacturing a secondary battery, the method including the steps of: positioning the separator according to the embodiment between a positive electrode and a negative electrode; and then applying heat, pressure, or both to integrate the separator and the electrodes. Effect of the Invention
[0038] A separator according to an embodiment of the present disclosure contains hollow conductive particles, and the hollow conductive particles are present on the surface of the separator, and thus act as a conductive layer in contact with an electrode, preventing electrical isolation of lithium ions and accumulation of dead lithium ions, thereby suppressing the formation and growth of lithium dendrites, thereby ensuring the safety of the battery.
[0039] Furthermore, the separator according to one embodiment of the present disclosure can prevent electrical short circuits by imparting conductivity to the surface layer.
[0040] Moreover, according to one embodiment of the present disclosure, it is possible to provide a new separator that can suppress swelling by functioning as a buffer that can internally accommodate swelling of a battery caused by an electrolyte or the like.
[0041] Furthermore, since swelling can be suppressed and adhesive strength with the electrode can be well maintained, loss of adhesive strength due to swelling can be prevented, and a new separator and a battery using the same can be provided in which the alignment of the electrode module is well maintained even when the electrodes and separators are stacked many times.
[0042] In addition, the method for manufacturing a separator according to an embodiment of the present disclosure can easily manufacture a separator capable of suppressing the formation and growth of dendrites by simply forming a coating layer containing hollow conductive particles on a porous substrate. In addition, inorganic particles forming a ceramic layer for imparting heat resistance and hollow conductive particles can be mixed and applied, and even with just one application, the hollow conductive particles can be formed more on the surface due to the difference in specific gravity between the inorganic particles and the hollow conductive particles.
[0043] Furthermore, a secondary battery including a separator according to an embodiment of the present disclosure can have a high capacity and a large size because safety is ensured, and can provide the effect of having extremely high industrial applicability. [Brief description of the drawings]
[0044] [Figure 1] FIG. 1 illustrates one embodiment of a hollow conductive particle consisting of a hollow core 11 and a shell layer 12 made of a conductive material. [Diagram 2] This is a diagram illustrating one embodiment of a hollow conductive particle consisting of a hollow core 11, a structural material layer 13 for forming and maintaining the hollow structure, and a shell layer 12 made of a conductive material. [Diagram 3] 1A to 1C are diagrams illustrating one embodiment of a method for manufacturing a separator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045] Unless otherwise defined, technical and scientific terms used in this specification have the meanings commonly understood by a person of ordinary skill in the art to which this disclosure belongs, and in the following description and the accompanying drawings, descriptions of known functions and configurations that may obscure the gist of this disclosure will be omitted.
[0046] Also, as used herein, the singular forms "a," "an," and "the" can be intended to include the plural forms as well, unless the context indicates otherwise.
[0047] Furthermore, in this specification, units used without special reference are based on weight, and as an example, a unit of % or ratio means % by weight or weight ratio, and % by weight means the weight % that any one component of the total composition occupies in the composition, unless otherwise defined.
[0048] In addition, the numerical ranges used herein include lower and upper limits, all values within the range, increments logically derived from the form and width of the ranges defined, all values that are doubly limited, and all possible combinations of upper and lower limits of numerical ranges that are limited in different forms. Unless otherwise specified in the specification of this disclosure, values outside the numerical ranges that may occur due to experimental error or rounding of values are also included in the defined numerical ranges.
[0049] As used herein, the term "comprising" is an open-ended term having the same meaning as expressions such as "comprising," "containing," "having," or "characterized by," and does not exclude further unrecited elements, materials, or steps.
[0050] Unless otherwise specified in this specification, when a layer or member is said to be "on" another layer or member, this includes not only the case where a layer or member is in contact with the other layer or member, but also the case where another layer or member exists between two layers or two members.
[0051] In the present specification, the term "hollow conductive particle" refers to a particle that is hollow inside and has conductivity. Specifically, as shown in FIG. 1 and FIG. 2, the hollow conductive particle is composed of a hollow core 11 that is hollow inside and a shell layer 12 made of a conductive material, and the shell layer may have at least one layer. Also, as shown in FIG. 2, a structure material layer 13 for forming and maintaining a hollow structure may be further included between the hollow core 11 and the shell layer 12. FIG. 1 and FIG. 2 are intended to specifically illustrate the hollow conductive particle according to one embodiment of the present disclosure, and the present disclosure is not limited thereto.
[0052] In the conductive particles, "conductive" means that the conductive material forming the shell layer has a surface resistance of 10,000 ohm / sq or less when coated on a glass substrate or silicon wafer to a thickness of 200 nm or more, more specifically, when coated to a thickness of 200 nm.
[0053] In conventional secondary batteries, irregular needle-shaped dendrites protrude from the surfaces of the electrodes and separators due to the electrical isolation of lithium ions and the accumulation of dead lithium ions during repeated charging and discharging. Not only do these dendrites increase the internal resistance of the battery and reduce the charge and discharge efficiency of the battery, but the needle-shaped dendrites can also destroy the separator, causing an internal short circuit in the battery.
[0054] In order to solve this problem, the inventors have conducted extensive research and found that by forming a coating layer containing conductive particles having a hollow structure with a shell layer coated on the surface of the separator and hollow conductive particles having an open interior, it is possible to prevent the formation of lithium dendrites, suppress the volume change of the battery, suppress the decomposition of the electrolyte, suppress the increase in the resistance of the battery, and improve the cycle life of the battery, leading to the completion of the present disclosure. In addition, the inventors have found that by mixing inorganic particles for heat resistance to form a coating layer, the conductive particles having a hollow structure float in the surface layer due to the difference in specific gravity with the inorganic particles, making it unnecessary to add a separate coating process, and providing a separator with less change in the air permeability of the separator and excellent lithium ion conductivity compared to the case of forming a separate conductive coating layer, leading to the completion of the present disclosure.
[0055] Specifically, the inventors have found that the above problems can be solved by providing a separator including a porous substrate and a coating layer that is located on one or both sides of the porous substrate and includes inorganic particles and hollow conductive particles, and have thus completed the present disclosure.
[0056] That is, in a conventional separator having a porous substrate and a ceramic layer (hereinafter also referred to as a "coating layer") in which inorganic particles formed on one or both sides of the porous substrate are connected to each other and pores are formed by the connection of the inorganic particles, the inventors have found that the above problems can be solved by manufacturing the ceramic layer containing hollow conductive particles together with the inorganic particles, and have thus completed the present disclosure.
[0057] The hollow conductive particles have a hollow structure and therefore have a relatively low specific gravity compared to the inorganic particles, and can float on the surface. As a result, it is not necessary to form a separate conductive coating layer, and the hollow conductive particles can be mixed with the inorganic particles and applied simultaneously to form a coating layer, and the hollow conductive particles naturally float on the surface layer to provide conductivity.
[0058] In this way, by including hollow conductive particles in the coating layer, the hollow conductive particles have a lower specific gravity than inorganic particles due to their hollow structure, so that the hollow conductive particles can be easily guided to the surface of the coating layer when the coating layer is formed. As a result, it is not necessary to separately form a conductive coating layer, and therefore conductivity can be achieved even with a smaller amount of conductive material, i.e., a smaller amount of hollow conductive particles.
[0059] In addition, when swelling occurs due to an electrolyte, etc., the coating layer can internally accommodate the electrolyte, thereby preventing external swelling. In addition, a secondary battery including a separator according to an embodiment of the present disclosure can prevent various problems such as an increase in resistance or a decrease in cycle life during charging and discharging, and can prevent separation between the electrodes and the separator, thereby preventing an increase in resistance due to the separation between the electrodes and the separator, and preventing the swelling phenomenon of the battery.
[0060] That is, when the coating layer includes the hollow conductive particles, it is possible to provide a new separator that can prevent lithium ion dendrites from being formed on the separator and electrodes, suppress an increase in resistance, and internally accommodate swelling caused by electrolytes, etc., without causing external swelling. The hollow conductive particles of the coating layer can be uniformly distributed in the coating layer, but due to the difference in specific gravity between the hollow conductive particles and the inorganic particles, the hollow conductive particles are distributed more on the surface in contact with the electrode, thereby more effectively preventing electrical isolation of lithium ions emitted from the electrode and accumulation of dead lithium ions, and more effectively preventing the formation and growth of dendrites.
[0061] In addition, the separator suppresses swelling caused by the electrolyte and minimizes loss of adhesion to the electrodes, i.e., prevents loss of adhesion caused by swelling, so that the alignment of the electrode module is well maintained even when the electrodes and separators are stacked many times. Also, the suppression of swelling and dissolution can improve the electrode performance.
[0062] In addition, due to the difference in specific gravity between the hollow conductive particles and the inorganic particles in the coating layer, the hollow conductive particles having a low specific gravity or density may be concentrated on the surface in contact with the electrode, and thus the content of the hollow conductive particles exhibiting conductivity may be minimized. As a result, compared to the case where a conductive coating layer is formed separately, the content of the conductive particles may be minimized, and the problem of deterioration of battery performance may be prevented.
[0063] In a separator according to one embodiment of the present disclosure, when a surface facing the porous substrate is designated as a first surface and a surface opposite the first surface is designated as a second surface, the content of the hollow conductive particles can be greater in the second surface than in the first surface.
[0064] In addition, the coating layer may have a gradient in which the content of the hollow conductive particles increases from the first surface to the second surface.
[0065] Also, the coating layer may be composed of an inorganic particle layer containing inorganic particles and a conductive layer formed by hollow conductive particles suspended on the inorganic particle layer. That is, as shown in Fig. 3, the hollow conductive particles may be suspended to form a layer separate from the layer composed of the inorganic particles.
[0066] In the coating layer, the hollow conductive particles have a lower specific gravity than the inorganic particles, so that the coating layer may have a gradient in which the concentration of the hollow conductive particles increases as the coating layer gets farther from the porous substrate. As described above, such a separator may have high conductivity relative to the amount of conductive material added, since the conductive material is concentrated on the surface of the coating layer.
[0067] In the present disclosure, the separator may include a single coating layer. Alternatively, a plurality of coating layers may be laminated. In this case, by laminating a plurality of layers, the content of hollow conductive particles relative to inorganic particles may be varied for each layer, and the content of hollow conductive particles may be increased on the surface that adheres to the electrode, thereby further improving conductivity.
[0068] That is, when the coating layer has a single layer structure, the hollow conductive particles may naturally rise to the surface to have a concentration gradient or form a separate conductive layer during the process of coating the surface of the porous substrate with a slurry in which the hollow conductive particles and the inorganic particles are mixed and drying the slurry, depending on the difference in specific gravity between the hollow conductive particles and the inorganic particles. Alternatively, after coating the slurry, a process of maintaining the slurry for a predetermined time so that the hollow conductive particles rise sufficiently to the surface and the inorganic particles sink toward the porous substrate may be introduced, and the concentration gradient of the hollow conductive particles may be intentionally formed by adjusting the time of standing. That is, when the surface of the coating layer facing the porous substrate is defined as a first surface and the surface opposite to the first surface is defined as a second surface, the concentration of the hollow conductive particles may be continuously increased from the first surface to the second surface, or the standing time may be adjusted so that more hollow conductive particles are distributed on the second surface. Alternatively, a conductive layer may be formed in which hollow conductive particles are suspended on the second surface. The coating layers may have different coating compositions. For example, the coating compositions may differ in the inorganic particles and / or hollow conductive particles used. Or, the amount of inorganic particles and / or hollow conductive particles used may differ from each other. Each coating layer (first, second, Nth) included in (i.e., forming) the coating layer may be distinguished from each other since each surface of the layer has a different concentration of hollow conductive particles depending on the manufacturing method. For example, the first surface of the first layer may have a smaller concentration (amount) of hollow conductive particles than the second surface of the first layer. The third surface of the second layer may have a smaller concentration (amount) of hollow conductive particles than the second surface of the first layer. Thus, the first coating layer may be distinguished from the second coating layer. This means that N coating layers may be applied in the same way.
[0069] The coating layer may have a multi-layer structure in which at least one layer is laminated.
[0070] For example, the coating layer may have a multi-layer structure in which the content of the inorganic particles and the hollow conductive particles is changed to form a plurality of layers with different contents of the hollow conductive particles. In particular, the coating layer may have a structure divided into n (n≧2, a natural number) layers with different concentrations of the hollow conductive particles. Specifically, n may be 2 to 5.
[0071] The coating layer may include a first coating layer having a first surface in contact with the porous substrate and a second surface opposite to the first surface, the first coating layer containing a first amount of hollow conductive particles, a third surface in contact with the second surface and a fourth surface opposite to the third surface, the second coating layer containing a second amount of hollow conductive particles, and an nth coating layer containing an nth amount of hollow conductive particles. For example, when the coating layer is divided into two layers, the first coating layer may contain a first amount of hollow conductive particles and the second coating layer may contain a second amount of hollow conductive particles. The respective coating layers may be in direct contact with each other.
[0072] In the present disclosure, the separator has a porous structure, and thus may have pores and porosity. The size and porosity of the pores formed in the separator may be appropriately adjusted according to the porosity of the porous substrate and the thickness of the coating layer. As an example, the average size of the pores formed in the separator, i.e., the average diameter of the pores, may be 0.001 to 10 μm, and the porosity may be 10 to 70%.
[0073] The separator according to one embodiment of the present disclosure may have a gas permeability of 500sec / 100cc or less, 400sec / 100cc or less, 300sec / 100cc or less, 200sec / 100cc or less, or 100sec / 100cc or less. The gas permeability is measured using a Densometer manufactured by Toyoseiki Co., Ltd. in accordance with the ASTM D 726 standard. In addition, the change in Gurley permeability ΔG according to the following formula may be 50sec / 100cc or less, 45sec / 100cc or less, 40sec / 100cc or less, 35sec / 100cc or less, or 30sec / 100cc or less.
[0074] ΔG=G1-G2
[0075] In the above formula, G1 is the Gurley permeability of a separator having coating layers formed on both sides of a porous substrate, and G2 is the Gurley permeability of the porous substrate itself. The Gurley permeability was measured using a Densometer manufactured by Toyoseiki Co., Ltd. in accordance with the ASTM D 726 standard, and the unit is sec / 100cc.
[0076] The heat shrinkage rate can be 8% or less, 7% or less, 6% or less, 5% or less, 4% or less, 3% or less, 2% or less, or 1% or less at 150° C. The heat shrinkage rate can be 8% or less, 7% or less, 6% or less, 5% or less, 4% or less, 3% or less, or 2% or less at 170° C.
[0077] Furthermore, a separator according to one embodiment of the present disclosure can have an average capacity retention rate of 60 cycles or more, 65 cycles or more, 68 cycles or more, 70 cycles or more, 75 cycles or more, 80 cycles or more, or 85 cycles or more, for example, 60 to 95 cycles, 65 to 90 cycles.
[0078] In addition, the separator according to one embodiment of the present disclosure has a surface resistance of 1×10 7 Ω / sq or less, 1×10 6 Ω / sq or less, 1×10 5 Ω / sq or less, 1×10 4Ω / sq or less, 1×10 2 Ω / sq or more, 1×10 3 Ω / sq or more and can be any value within the ranges described above. For example, 1×10 2 Ω / sq or more 1×10 7 Ω / sq or less, 1×10 2 Ω / sq or more 1×10 6 Ω / sq or less, 1×10 2 Ω / sq or more 1×10 5 Ω / sq or less, 1×10 2 Ω / sq or more 1×10 4 The surface resistance of the separator may be Ω / sq or less. The surface resistance of the coating layer is measured using a four-point probe method under conditions of a temperature of 25±5° C. and a relative humidity of 30±5%, and an applied voltage of 5V.
[0079] [Porous base material] As an example, the porous substrate of the separator is not limited as long as it is a substrate that has been used in the past for separators. Specifically, it may be a film, sheet, nonwoven fabric, or woven fabric made of a polymeric material. Specifically, the porous substrate may include a porous substrate made of a polyolefin-based resin. The polyolefin-based resin may be, but is not limited to, one or more selected from the group consisting of high-density polyethylene, low-density polyethylene, linear low-density polyethylene, ultra-high molecular weight polyethylene, polypropylene, and copolymers thereof.
[0080] The thickness of the porous substrate is not particularly limited, but may be in the range of 1 to 100 μm, 5 to 60 μm, 5 to 40 μm, 5 to 20 μm, or 5 to 10 μm. The porous substrate may be in the form of a porous film.
[0081] The pores formed in the porous substrate are not limited as long as they are of a size that allows smooth movement of lithium ions, but an average diameter of 0.01 to 20 μm, or 0.05 to 5 μm, or 0.05 to 1 μm can be advantageous in terms of smooth movement of lithium ions and impregnation of the electrolyte. In addition, although not particularly limited, the porosity can be 5 to 95%, or 30 to 60%. The porosity can be calculated by cutting a sample into a rectangle (thickness T μm) of A cm x B cm, measuring the mass, and calculating the ratio of the weight of the resin and the weight of the separator (Mg) of the same volume according to the following formula: Porosity (%) = 100 x {1-M x 10000 / (A x B x T x ρ)}, where ρ (g / cm 2 ) is the density of the resin.
[0082] [Coating layer] For example, the coating layer may be formed on one or both sides of the porous substrate, and may be a layer having a porous structure in which inorganic particles and hollow conductive particles are connected to each other to form pores. Alternatively, the coating layer may be a laminated structure in which an inorganic particle layer in which inorganic particles are connected to each other to form pores and a conductive layer in which hollow conductive particles are suspended on the inorganic particle layer are formed. The coating layer may be formed in direct contact with the porous substrate. Alternatively, another layer that is usually used in a separator, specifically an inorganic particle layer in which pores are formed between inorganic particles, may be further provided between the porous substrate and the coating layer, but is not limited thereto.
[0083] As described above, the coating layer allows the hollow conductive particles to be concentrated on the surface that contacts the electrode, thereby solving the problems of the conventional separator.
[0084] The thickness of the coating layer is not particularly limited, but for example, the thickness of the coating layer formed on one side of the porous substrate may be 0.1 μm or more, 0.5 μm or more, 1 μm or more, 1.5 μm or more, 2 μm or more, 3 μm or more, or 5 μm or more, for example, 0.1 to 10 μm, 0.2 to 5 μm, or 0.2 to 3 μm, but is not limited thereto. In addition, the coating layer may include a conductive layer formed by suspending the hollow conductive particles, and the thickness of the conductive layer may be, but is not limited to, 0.01 to 20 μm. The thickness of the conductive layer may be adjusted by adjusting the content of the hollow conductive particles used, but is not limited thereto.
[0085] As an example, the thickness ratio of the porous substrate of the separator to the coating layer may be, but is not limited to, 1:0.01-1, or 1:0.05-0.5, as long as the object of the present disclosure can be achieved. This range is preferable because excellent battery stability, suppression of swelling, improvement of battery performance, and conductivity can be ensured within the above range, but is not limited thereto. As an example, the coating layer may be formed on 90% or more of the total area of each surface of the porous substrate, and 95% or more, or 100% of the total area of each surface of the porous substrate, except in cases where microdefects occur.
[0086] The coating layer may further include other commonly known additives in addition to the inorganic particles and hollow conductive particles, such as dispersants, lubricants, antifoaming agents, thickeners, etc., and the content thereof may be about the same as that of commonly used additives.
[0087] In addition, the coating layer may further include an adhesive resin, if necessary, in order to provide a bond between the inorganic particles and provide adhesion to the electrode. The adhesive resin may be a water-based binder or a particulate binder, and is not limited as long as it is one that is generally used in the field. In addition, the adhesive resin may be used in an amount significantly less than that used conventionally so as not to interfere with the suspension of the hollow conductive particles. Such a conventional adhesive resin is not particularly limited, and may include, for example, any one or a mixture of two or more selected from acrylic polymers, styrene polymers, vinyl alcohol polymers, vinylpyrrolidone polymers, and fluorine polymers.
[0088] For example, the polyacrylamide, poly(meth)acrylate, acrylic acid-methacrylic acid copolymer, polystyrene, polyvinyl alcohol, polyvinyl acetate, polyvinyl acetate-polyvinyl alcohol copolymer, polyvinylpyrrolidone, polyvinylidene fluoride, polytetrafluoroethylene, polyhexafluoropropylene, hexafluoropropylene, polyvinylidene fluoride-hexafluoropropylene, polychlorotrifluoroethylene, etc., or a mixture of two or more thereof, or a copolymer thereof, may be used, but is not limited thereto.
[0089] The adhesive resin and additives may be further included in an appropriate minimum amount, and as a non-limiting example, the adhesive resin may be 0.1 to 5 parts by weight and the additives may be 0.1 to 3 parts by weight per 100 parts by weight of inorganic particles. This is an example and is not limited thereto.
[0090] The inorganic particles contained in the coating layer may be, for example, any one or more selected from metal oxides, metal nitrides, metal carbides, metal carbonates, metal hydrates, and metal carbonitrides, etc. For example, they may be one or more selected from boehmite, Ga2O3, SiC, SiC2, quartz, NiSi, Ag, Au, Cu, Ag-Ni, ZnS, Al2O3, TiO2, CeO2, MgO, NiO, Y2O3, CaO, SrTiO3, SnO2, ZnO, and ZrO2, etc., but are not necessarily limited thereto as long as they are electrochemically unstable and do not significantly affect the performance of the battery.
[0091] The shape of the inorganic particles is not particularly limited as long as the purpose of improving the durability and heat resistance of the porous substrate is achieved. Specifically, the inorganic particles may have one or more shapes selected from the group consisting of spherical, angular, and amorphous.
[0092] The size of the inorganic particles is not limited as long as the above-mentioned object is achieved, and specifically, the size of the inorganic particles, i.e., the average diameter, can be 0.001 to 100 μm, specifically 0.01 to 50 μm, and more specifically 0.01 to 10 μm. Within the above range, it is preferable to have the above-mentioned separator porosity, but it is not necessarily limited thereto.
[0093] The hollow conductive particles used in the coating layer may have a lower density and buoyancy than inorganic particles by forming a hollow inside as shown in FIG. 1 and FIG. 2. The hollow ratio of the hollow conductive particles is not particularly limited as long as it achieves the above-mentioned purpose, i.e., the purpose of forming a lower density than inorganic particles. As an example, the hollow ratio of the hollow conductive particles may be 5 to 97%, 10 to 97%, 15 to 97%, 20 to 97%, or 50 to 95%, but is not limited thereto. The hollow ratio can be calculated from the outer diameter and inner diameter of the hollow conductive particles according to the following formula. The outer diameter and inner diameter refer to the average particle diameter and can be measured using SEM, etc. Hollow ratio (%) = inner diameter / outer diameter x 100, the outer diameter refers to the average particle diameter of the hollow conductive particles, i.e., the average outer diameter, and the inner diameter is calculated by subtracting the thickness of the shell layer from the average particle diameter by measuring the thickness of the shell layer using SEM, TEM, etc. In addition, when the hollow conductive particles have a non-uniform hollow shape, the hollowness can be calculated based on the correlation between the density (apparent density) measured using a powder density measurement method and the theoretical density. In this case, the hollowness (%) can be calculated as (1-apparent density / theoretical density) x 100. The thickness of the porous substrate or the porous film can be measured using a thickness meter manufactured by Mitutoyo. In addition, the thickness of the shell layer, the core layer, or the diameter of the hollow particles can be measured using an electron microscope such as SEM or TEM.
[0094] The hollow conductive particles provide conductivity to the coating layer, thereby preventing the electrical isolation of lithium ions and the accumulation of dead lithium ions. As shown in Fig. 1, the battery is composed of a hollow core 11 with a hole therein and a shell layer 12 made of an adhesive material, and the shell layer may be composed of at least one layer. Also, as shown in Fig. 2, the battery may further include a structural material layer 13 between the hollow core 11 and the shell layer 12 for forming and maintaining the hollow structure of the hollow core.
[0095] The shell layer of the hollow conductive particle may be made of any material having conductivity. For example, the shell layer may be made of at least one conductive material selected from the group consisting of metals and conductive polymers. The metal may be, for example, metal nanoparticles. That is, any material having a shell layer made of a metal or conductive polymer and a hollow structure with a void inside may be used without limitation.
[0096] The hollow conductive particles are not particularly limited as long as they have a surface resistance of 10,000 Ω / sq or less and are hollow with a space inside.
[0097] As an example of a method for producing the hollow conductive particles, as described in “Uniform hollow conductive polymer microspheres synthesized with the sulfonated polystyrene template”, July 2005, Materials Chemistry and Physics 92(1):164-171, polystyrene microspheres are sulfonated to produce sulfonated polystyrene (sulfonated PS), and conductive materials such as aniline and pyrrole are oxidatively polymerized to form a shell layer, and then the sulfonated polystyrene inside is dissolved and removed.
[0098] In addition, there are various methods for manufacturing the hollow conductive particles, such as manufacturing hollow polymer particles by a method such as that described in Korean Patent Publication No. 10-2020-0138213 (Publication date: December 9, 2020, Zeon Corporation), and then coating the surface with a binder slurry composition in which conductive metal nanoparticles or microparticles are dispersed on the surface, or a conductive polymer resin solution composition, and then drying to manufacture the particles, which will not be described below.
[0099] The structural material layer may be any material capable of maintaining the hollow core structure, including, but not limited to, SiO2, Al2O3, ZnO, TiO2, SnO2, carbon, polystyrene, polyacrylate, and PVDF.
[0100] The size of the hollow conductive particles is not limited as long as the above-mentioned object is achieved, and the size of the hollow conductive particles, i.e., the average outer diameter, may be, but is not necessarily limited to, 10 nm to 10 μm, or 50 nm to 5 μm, or 0.1 to 5 μm, or 0.2 to 2 μm.
[0101] The coating layer may include hollow conductive particles of unitary structure or hollow particles having multiple shell layers, such as bilayers or triple layers, that are open inside.
[0102] The thickness of the shell layer of the hollow conductive particles is not particularly limited as long as it satisfies the above-mentioned hollow ratio. Specifically, the thickness of the shell layer may be within 0.0001R to 0.8R, more specifically 0.001R to 0.5R, or 0.2R, relative to the average outer diameter R of the hollow conductive particles, but is not limited thereto.
[0103] The coating layer may contain more inorganic particles than the hollow conductive particles. The hollow conductive particles may be used in a small amount that can exhibit conductivity and adhesiveness, and may contain, for example, 0.1 parts by weight or more, 0.2 parts by weight or more, 0.3 parts by weight or more, 0.4 parts by weight or more, 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, 0.8 parts by weight or more, 0.9 parts by weight or more, or 1.0 parts by weight or more of the hollow conductive particles relative to 100 parts by weight of the inorganic particles, and may contain 20 parts by weight or less, 19 parts by weight or less, 18 parts by weight or less, 17 parts by weight or less, 16 parts by weight or less, or 15 parts by weight or less, and may be used within these ranges. For example, the inorganic particles may contain 0.1 to 20 parts by weight, 0.2 to 20 parts by weight, 1 to 20 parts by weight, 1 to 15 parts by weight, 1 to 10 parts by weight, 1 to 8 parts by weight, or 1 to 5 parts by weight, but are not limited thereto, and sufficient conductivity and electrode adhesive strength can be exhibited even within the above ranges. In addition, the inorganic particles may further contain 0.1 to 5 parts by weight of a non-hollow polymer binder and 0.1 to 5 parts by weight of an additive, if necessary, but are not limited thereto.
[0104] It is needless to say that the coating layer may further include a binder that connects and fixes the inorganic particles and the hollow conductive particles to each other and provides adhesion between the coating layer and the porous substrate layer.
[0105] The binder is not particularly limited, and may include, for example, any one or a mixture of two or more selected from acrylic polymers, styrene polymers, esters, amides, imides, amide-imides, vinyl alcohol polymers, vinylpyrrolidone polymers, and fluorine-based polymers.
[0106] Specifically, the binder may be any one or a mixture of two or more selected from polyacrylamide, polymethacrylate, polyacrylate, polybutyl acrylate, sodium polyacrylate, acrylic acid-methacrylic acid copolymer, polystyrene, polyvinyl alcohol, polyvinyl acetate, polyvinyl acetate-polyvinyl alcohol copolymer, polyvinylpyrrolidone, polyvinylidene fluoride, polytetrafluoroethylene, polyhexafluoropropylene, hexafluoropropylene, polyvinylidene fluoride-hexafluoropropylene, and polychlorotrifluoroethylene, but is not limited thereto.
[0107] The content of the binder is not particularly limited, but as a non-limiting example, the binder may be contained in an amount of 0.1 to 10 parts by weight and the additive in an amount of 0.1 to 5 parts by weight per 100 parts by weight of the inorganic particles.
[0108] [Separator manufacturing method] The method for producing the separator will be described in detail below.
[0109] In the present disclosure, a method for producing a separator includes a coating step of applying a coating composition including inorganic particles and hollow conductive particles onto one or both sides of a porous substrate to form a coating layer, and a drying step of drying the coating layer.
[0110] 3, a coating composition including the inorganic particles 20 and hollow conductive particles 10 may be applied to one side of a porous substrate 100 and then dried to produce a coating layer 200 having a higher content of the hollow conductive particles on the surface, i.e., the surface not in contact with the porous substrate. Alternatively, the hollow conductive particles may be substantially guided to the surface to form a conductive layer.
[0111] As an example, when the surface facing the porous substrate is designated as a first surface and the surface opposite the first surface is designated as a second surface, the second surface may have a higher content of the hollow conductive particles than the first surface.
[0112] For example, the coating layer may be manufactured to have a gradient in which the content of the hollow conductive particles increases from the first surface to the second surface, or the coating layer may be composed of an inorganic particle layer including inorganic particles and a conductive layer in which hollow conductive particles are suspended on the inorganic particle layer.
[0113] In one embodiment, before the drying step, in order to artificially induce the formation of a gradient or another conductive layer due to the difference in specific gravity between the hollow conductive particles and the inorganic particles, the coating may be left to stand for a predetermined time, vibrated, or both may be applied simultaneously or successively, and then dried. That is, the coating composition may be applied and then left to stand for a predetermined time, and then dried. Alternatively, the coating composition may be applied and then left to stand for a predetermined time, and then vibrated, and then dried. Alternatively, the coating composition may be applied and then left to stand for a predetermined time, and then vibrated and then dried. Alternatively, the coating composition may be applied and then vibrated, and then dried. Alternatively, the coating composition may be applied and then vibrated, and then dried. In one embodiment, the time for leaving to stand for a predetermined time may be adjusted to adjust the gradient of the hollow conductive particles, or a conductive layer formed by hollow conductive particles floating may be formed.
[0114] In one embodiment, when the coating layer is formed on both sides of the porous substrate, a coating layer may be formed on one side and then a coating layer may be formed on the other side. Although both sides may be simultaneously coated, it is preferable to coat each side on the side on which the hollow conductive particles are guided as intended in the present disclosure.
[0115] As described above, the hollow conductive particles migrate to the air surface (the surface opposite to the surface in contact with the porous substrate) due to the difference in specific gravity and dry, so that the hollow conductive particles having conductivity and adhesiveness are present in large amounts on the surface, and even if a small amount of hollow conductive particles is used, the surface resistance can be further reduced and the growth of dendrites can be suppressed.
[0116] In this method for manufacturing a separator, simply by forming a coating layer containing the hollow conductive particles on a porous substrate, it is possible to easily manufacture a separator that has improved adhesion to an electrode, suppresses the generation of dendrites, and has excellent resistance to expansion.
[0117] In the manufacturing method, the porous substrate, the inorganic particles, the hollow conductive particles, and the manufactured separator have been described above, and detailed description will be omitted below, and each step will be described in detail.
[0118] The coating composition may be a slurry in which inorganic particles and hollow conductive particles are dispersed in a solvent. In addition, the coating composition may further include an adhesive resin as necessary, and may further include additives that are commonly used in the relevant field.
[0119] The solvent is not particularly limited as long as it can disperse the solid inorganic particles and hollow conductive particles. For example, the solvent may be water, lower alcohol such as ethanol, methanol, propanol, dimethylformamide, acetone, tetrahydrofuran, diethyl ether, methylene chloride, N-methyl-2-pyrrolidone, hexane, cyclohexane, or a mixture thereof, but is not necessarily limited thereto.
[0120] The content of the solid matter in the slurry-like coating composition can be appropriately adjusted so that the coating composition can be easily applied and can induce a layer separation phenomenon due to the difference in density between the inorganic particles and the hollow conductive particles when dried. Specifically, the content of the solid matter in the coating composition can be, but is not limited to, 10 to 60% by weight, or 20 to 50% by weight. The solid matter includes inorganic particles and hollow conductive particles, and can further include an adhesive resin as necessary. For example, the content of the solid matter can include 0.1 to 20 parts by weight, 0.1 to 15 parts by weight, 0.1 to 10 parts by weight, 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, or 0.1 to 2 parts by weight of hollow conductive particles relative to 100 parts by weight of inorganic particles. In addition, the coating composition can further include 0.1 to 5 parts by weight of adhesive resin and 0.1 to 5 parts by weight of additives relative to 100 parts by weight of inorganic particles as necessary, but is not limited thereto.
[0121] In addition, the coating composition may further include additives within a range that does not significantly deteriorate the coating property or the battery performance. Specifically, for example, the additives may include dispersants, lubricants, antifoaming agents, thickeners, etc., but are not limited thereto, and since they have been described above, further description will be omitted.
[0122] The coating method for coating the coating composition on one or both sides of the porous substrate is not limited, and specifically, may be a common coating method such as bar coating, dip coating, flow coating, knife coating, roll coating, gravure coating, spray coating, etc.
[0123] In the drying step, the drying means is not particularly limited as long as it can remove 90% or more of the solvent. The drying temperature can be changed depending on the solvent, for example, 20 to 200°C, and is not limited as long as the surface structure is not changed due to the sudden evaporation of the solvent or the hollow conductive particles are not melted and collapsed. As a specific example, it can be dried with hot air at 25°C to 100°C, and the drying time is not limited, but can be, for example, 5 seconds to 300 seconds. In addition, drying methods using infrared rays, near infrared rays, heat rolls, and hybrid forms thereof are also possible. Within the above range, the hollow conductive particles can be smoothly suspended, and a larger amount of the hollow conductive particles can be located in the upper region, the conductive layer, or the nth coating layer.
[0124] In one embodiment, the drying step may involve vibration or artificial standing time before drying, or these mixing means may be used to provide a concentration gradient of the hollow conductive particles.
[0125] When the vibration is further applied, the hollow conductive particles can be more smoothly suspended due to the difference in specific gravity between the inorganic particles and the hollow conductive particles. The vibration is not particularly limited as long as it can be applied to the coating composition. For example, the vibration can be applied directly to the coating composition by applying energy such as ultrasonic waves. Alternatively, the vibration can be applied to the coating composition by applying physical vibration such as a motor to the porous substrate.
[0126] In one embodiment, the method may further include a step of leaving the coating composition to allow the hollow conductive particles to have a sufficient gradient before the drying step. Specifically, the coating composition may be left to stand for about 30 seconds to 1 hour after being applied onto a porous substrate, so that the hollow conductive particles are sufficiently suspended on the surface of the coating layer. The temperature at which the coating composition is left to stand is 0 to 50°C, preferably at room temperature (25°C ± 5), but is not limited thereto.
[0127] [Secondary battery] The secondary battery will be described in detail below.
[0128] In the present disclosure, the secondary battery includes the above-mentioned separator, and specifically, the secondary battery can have a structure in which the above-mentioned separator is interposed between and bonded to a negative electrode and a positive electrode.
[0129] In particular, the positive and negative electrodes are not limited as long as they are materials normally used as positive and negative electrodes of secondary batteries.
[0130] A secondary battery including the above separator can inhibit the formation of lithium dendrites, thereby increasing the battery life, and can prevent the electrode and the separator from being separated during charging and discharging. This can solve various problems such as an increase in resistance or a decrease in cycle life due to the separation between the electrode and the separator, and can achieve high capacity and large size, making it practically highly industrially applicable. In addition, despite the high surface electrical conductivity, the conductive material is contained in a relatively small amount and is present only on the surface of the separator, preventing problems such as internal short circuit and deterioration of battery performance due to the conductive material.
[0131] The present disclosure will be described in more detail below based on examples and comparative examples. However, the following examples and comparative examples are merely examples for describing the present disclosure in more detail, and the present disclosure is not limited by the following examples and comparative examples.
[0132] The physical properties were measured as follows.
[0133] 1) Electrode manufacturing Preparation of positive electrode: 92 wt% of lithium cobalt composite oxide (LiCoO2) as a positive electrode active material, 4 wt% of carbon black as a conductive material, and 4 wt% of polyvinylidene fluoride (PVDF) as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent to prepare a positive electrode mixture slurry. The prepared slurry was applied to a 30 μm thick aluminum (Al) thin film, dried at a temperature of 120°C, and then roll-pressed to prepare a positive electrode with a thickness of 140 μm.
[0134] Preparation of negative electrode: A 20 μm-thick lithium foil was roll-pressed onto both sides of a 8 μm-thick copper (Cu) thin film to prepare a 48 μm-thick negative electrode.
[0135] 2) Gas permeability The gas permeability was measured using a Gurley type densometer manufactured by Toyoseiki Co., Ltd. in accordance with JIS P8117. The measured value was corrected to a thickness value and converted to a value that does not vary depending on the thickness.
[0136] 3) Change in Gurley transmittance The change in Gurley permeability, ΔG, is calculated as follows:
[0137] ΔG=G1-G2
[0138] In the above formula, G1 is the Gurley permeability of a separator having coating layers formed on both sides of a porous substrate, and G2 is the Gurley permeability of the porous substrate itself. The Gurley permeability was measured using a Densometer manufactured by Toyoseiki Co., Ltd. in accordance with the ASTM D 726 standard, and the unit is sec / 100cc.
[0139] 4) Heat shrinkage rate Separators of 10 cm×10 cm were left to stand at 130° C., 150° C. and 170° C. for 1 hour, respectively, and then the reduction in area was measured and the thermal shrinkage was calculated by the following formula.
[0140] Heat shrinkage rate (%) = ((length before heating - length after heating) / length before heating) x 100
[0141] 5) Battery performance and battery deformation rate The separator prepared between the positive and negative electrodes was used to assemble pouch-type batteries in a stacking manner, and an electrolyte solution of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) = 3:5:2 (volume ratio) in which 1M lithium hexafluorophosphate (LiPF6) was dissolved was injected into each assembled battery to manufacture a lithium secondary battery. As a result, a pouch-type lithium ion secondary battery with a capacity of 2000mAh was manufactured. The resistance (DC-IR) of the lithium secondary battery was evaluated using the J-pulse (Japan Electric Vehicle Association Standards, JEVS D 713) method, which evaluates discharge and charge characteristics for 10 seconds at 0.25C, 0.5C, 1.0C, 1.5C, 2.0C, and 2.5C. The average impedance of the three batteries was calculated using the above method, and the initial resistance value and its standard deviation were calculated. The relative comparison value of the initial resistance refers to the increased value relative to the initial resistance of the uncoated porous substrate (Comparative Example 2).
[0142] Relative comparison with Ref.(%)=((Impedance-Impedance 基材 ) / Impedance 基材 ) x 100
[0143] In the case of cycle capacity retention, the battery was charged / discharged from 2.7V (constant current) to 4.3V (constant current constant voltage) at 0.1C for the first cycle and 0.2C for the second cycle, and then charged / discharged at 0.5C from the third cycle onwards, and the number of cycles until the battery capacity retention rate fell to 50% or less was measured.
[0144] 6) Average particle size and average outer diameter According to the ISO 13320-1 standard, the average particle size (D 50 ), D 10 and D. 90 was measured.
[0145] 7) Conductivity The surface resistance of the coating layer was measured using a four-point probe method under the conditions of a temperature of 25±5°C and a relative humidity of 30±5%. The applied voltage was 5V.
[0146] [Example 1] 100 parts by weight of boehmite (γ-AlO(OH)) with an average particle size of 300 nm was added to water, and 3 parts by weight of polyacrylamide (Mw 150,000 g / mol, Sigma Aldrich) was added. 0.7 parts by weight of dispersant (BYK-2018) was added to the boehmite, and the mixture was stirred to produce a uniform aqueous slurry with a solid content of 30 wt%. 1 part by weight of polyaniline hollow particles with an average outer diameter of 1 μm and a hollow ratio of 80%, which were produced by the experimental method described in “Uniform hollow conductive polymer microspheres synthesized with the sulfonated polystyrene template” July 2005, Materials Chemistry and Physics 92(1):164-171, was added to the boehmite, and water was further added to produce a slurry composition with a final solid content of 25 wt%.
[0147] The prepared slurry composition was coated on both sides of a 9 μm thick polyolefin microporous membrane (ENPASS, SK Innovation, average pore size: 40 nm) at a speed of 10 m / min and dried with hot air at 45° C. Drying was continued until there was no further weight loss. Then, the membrane was wound up. After drying, the thickness of the coating layers on both sides was 3.0 μm. The physical properties of the prepared separator were evaluated and are shown in Table 1, and the physical properties of a cell using the prepared separator were evaluated and are shown in Table 2.
[0148] The manufactured separator was observed using an Energy Dispersive Spectrometer (EDS) attached to a SEM (scanning electron microscope), and it was confirmed that hollow particles were suspended on the surface and formed a conductive layer.
[0149] [Example 2] The same procedure as in Example 1 was repeated except that the slurry composition was applied to one side of a polyolefin microporous membrane fixed to a glass plate of 0.2 m x 0.2 m size using a bar coating method, and then the plate was left to stand for 3 minutes, and then ultrasonic vibration was applied to the glass plate, and the plate was dried with hot air at 45°C for a period of time until no further weight loss occurred. The physical properties of the produced separator were evaluated and are shown in Table 1, and the physical properties of a cell using the produced separator were evaluated and are shown in Table 2.
[0150] The manufactured separator was observed using an EDS attached to a SEM (scanning electron microscope), and it was confirmed that the hollow particles floated on the surface to form a conductive layer. In addition, it was confirmed that more hollow particles were floating on the surface compared to Example 1.
[0151] [Example 3] The same procedure was carried out as in Example 1, except that 2 parts by weight of hollow particles were added relative to the boehmite. The properties of the produced separator were evaluated and are shown in Table 1, and the properties of a cell using the produced separator were evaluated and are shown in Table 2.
[0152] [Example 4] The same procedure was carried out as in Example 1, except that the hollow particles were added in an amount of 5 parts by weight relative to the boehmite. The physical properties of the produced separator were evaluated and are shown in Table 1, and the physical properties of the cell using the produced separator were evaluated and are shown in Table 2.
[0153] [Comparative Example 1] A slurry was prepared in the same manner as in Example 1, except that hollow particles were not used, and a separator was prepared in the same manner. The physical properties of the produced separator were evaluated and are shown in Table 1, and the cell properties were evaluated using the produced separator and are shown in Table 2.
[0154] [Comparative Example 2] The properties of the polyolefin microporous membrane (ENPASS, SK Innovation, average pore size: 40 nm) used in Example 1 were evaluated and are shown in Table 1. That is, the properties of the polyolefin microporous membrane itself without forming a coating layer were measured and shown in Table 1, and the properties of the cell using the same were measured and shown in Table 2.
[0155] [Table 1]
[0156] [Table 2]
[0157] As described above, the present disclosure has been described by citing specific matters and limited examples and comparative examples. However, these are provided to aid in a more general understanding of the present disclosure, and the present disclosure is not limited to the above examples. A person having ordinary knowledge in the field to which the present disclosure pertains can make various modifications and variations from such descriptions.
[0158] Therefore, the idea of the present disclosure should not be limited to the above-described embodiments, and it can be said that not only the scope of the claims described below, but also all equivalent or similar variations to the scope of the claims fall within the scope of the idea of the present disclosure. [Explanation of symbols]
[0159] 10. Hollow conductive particles 20 Inorganic particles 11 Hollow-core 12 Shell layer 13 Structure material layer 100 Porous substrate 200 coating layers
Claims
1. A porous substrate; a coating layer disposed on one or both sides of the porous substrate, the coating layer including inorganic particles and hollow conductive particles.
2. 2. The separator according to claim 1, wherein a surface of the coating layer facing the porous substrate is defined as a first surface and a surface opposite to the first surface is defined as a second surface, and the second surface has a higher content of the hollow conductive particles than the first surface.
3. The separator according to claim 2 , wherein the coating layer has a gradient in which the content of the hollow conductive particles increases from the first surface to the second surface.
4. The separator according to claim 3 , wherein the coating layer comprises an inorganic particle layer including inorganic particles and a conductive layer formed by suspending hollow conductive particles on the inorganic particle layer.
5. The separator according to claim 1 , wherein the hollow conductive particles have a void ratio of 5 to 97%.
6. The separator according to claim 1 , wherein the hollow conductive particles have an average outer diameter of 10 nm to 10 μm.
7. The separator according to claim 1 , wherein the hollow conductive particle comprises a hollow core having a hollow structure with an open interior, and a shell layer made of at least one conductive material selected from the group consisting of metals and conductive polymers.
8. The separator according to claim 7 , wherein the hollow conductive particle further comprises a structural material layer between the hollow core and the shell layer for maintaining the hollow structure.
9. The separator of claim 7 , wherein the structural material layer comprises at least one selected from the group consisting of inorganic materials and cross-linked polymers.
10. The inorganic material is an oxide, a carbon material, or a mixture thereof; The separator according to claim 9 , wherein the crosslinked polymer includes at least one selected from a styrene-based polymer, an acrylic-based polymer, and a fluorine-based polymer.
11. The separator according to claim 1 , further comprising an inorganic particle layer between the porous substrate and the coating layer.
12. A coating step of applying a coating composition including inorganic particles and hollow conductive particles onto one or both sides of the porous substrate to form a coating layer; and drying the coating layer.
13. The method for producing a separator according to claim 12, further comprising the step of applying vibration prior to or simultaneously with the drying step.
14. The method for producing a separator according to claim 12, further comprising the step of leaving the separator coated with the coating composition undisturbed after the coating step and before drying.
15. 13. The method for manufacturing a separator according to claim 12, wherein after the coating step and the drying step, the hollow conductive particles float on the surface of the coating layer to form a gradient, or a conductive layer made of the hollow conductive particles is formed on the surface of the coating layer.
16. The method for producing a separator according to claim 12, wherein the coating composition has a solid content of 10 to 60 wt %.
17. The method for producing a separator according to claim 12, wherein the coating composition contains 0.2 to 20 parts by weight of the hollow conductive particles based on 100 parts by weight of the inorganic particles.
18. The method for producing a separator according to claim 12, wherein the drying is performed with hot air at 25 to 100°C.
19. A secondary battery comprising the separator according to any one of claims 1 to 11.
20. A method for manufacturing a secondary battery, comprising the steps of: positioning the separator according to claim 1 between a positive electrode and a negative electrode; and then applying heat, pressure, or heat and pressure to integrate the separator and the electrodes.
Citation Information
Patent Citations
Secondary battery preventing dendrite growth
KR1020190046237A