Polyamide resin support

A polyamide resin support with controlled polymer chain tension and specific manufacturing processes addresses the issue of resin support deterioration, providing long-term structural reinforcement by maintaining dimensional stability and preventing peeling.

JP2024169840AInactive Publication Date: 2024-12-06TORAY MONOFILAMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023086635
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing resin supports for mortar reinforcement, such as those made of polyester, deteriorate quickly in alkaline environments and lack long-term dimensional stability, posing challenges for structural reinforcement over time.

Method used

A polyamide resin support with a network structure composed of filaments, manufactured through specific heat treatment and net-making processes, to control polymer chain tension and ensure dimensional stability, with a dimensional change rate of -1.0 to 1.5% and a Raman spectrum full width at half maximum of 15-43 cm⁻¹, enhancing long-term use.

Benefits of technology

The polyamide resin support maintains excellent dimensional stability, preventing peeling and ensuring a sustained reinforcing effect over time, suitable for mortar reinforcement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169840000010
    Figure 2024169840000010
  • Figure 2024169840000011
    Figure 2024169840000011
  • Figure 2024169840000001
    Figure 2024169840000001
Patent Text Reader

Abstract

To provide a polyamide resin support excellent in dimension stability as a mortar reinforcement material.SOLUTION: A polyamide resin support has a network structure formed of a filament body mainly made of a polyamide resin and has -1.0 to 1.5% of a dimensional change rate (%) expressed by a formula (1). A dimensional change rate (%)=(Support porosity under atmosphere at 20°C-support porosity after dry heat processing at 140°C)÷support porosity under atmosphere at 20°C×100 (1)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide resin support that can be suitably used as a mortar reinforcing material. [Background technology]

[0002] In recent years, cracks in exterior walls and sloped walls due to deterioration of existing structures, and associated rock falls, have become a problem. Mortar made of cement, water, and sand, or concrete made of mortar mixed with gravel, are used for reinforcement work for existing structures that have deteriorated.

[0003] When applying mortar to existing structures, metal supports have traditionally been used as reinforcing materials; however, metal supports are heavy and difficult to install, and rust causes their volume to expand, causing the mortar to peel off from the support, reducing the reinforcing effect over time.

[0004] For this reason, in recent years, lightweight, rust-resistant resin supports have been available as an alternative to metal supports, and one known example is a mortar reinforcing net with tortoiseshell-shaped net loops made of synthetic fiber yarn (Patent Document 1).

[0005] Resin supports are generally produced by preheating the filaments that make up the resin support to a temperature above the glass transition temperature and below the melting point, and then subjecting them to a net-making process (Patent Document 2). Polyester resin supports, which are one type of general-purpose resin (Patent Document 3), have excellent strength, durability, and acid resistance, but deteriorate significantly over time in an alkaline environment where mortar is used.

[0006] It is known that a support using polyamide resin, which is one of the general-purpose resins, has alkali resistance, is easy to install due to its moderate rigidity, and provides a sufficient reinforcing effect (Patent Document 4). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2003-74160 A [Patent Document 2] Special Publication No. 61-52259 [Patent Document 3] Special Publication No. 7-30495 [Patent Document 4] Patent No. 3918030 Summary of the Invention [Problem to be solved by the invention]

[0008] In recent years, from the viewpoint of reducing the burden on the global environment and reducing the workload by reducing the number of construction operations, there has been a demand for polyamide resin supports that can be used for a longer period than the resin supports listed in Patent Document 4.

[0009] An object of the present invention is to provide a polyamide resin support which, when used as a mortar reinforcing material, has excellent dimensional stability and can be used for a long period of time. [Means for solving the problem]

[0010] The inventors investigated the reason why the shape of the support becomes unstable over long periods of use when the resin support is used as a mortar reinforcing material, and concluded that this is because the polymer chains inside the filaments that make up the resin support are in a state of tension immediately after production of the support, and structural relaxation occurs over time. Based on this idea, the inventors discovered that by producing a polyamide resin support having a network structure made up of filaments whose main component is polyamide resin using a specific production method, it is possible to control the state of the polymer chains inside the filaments that make up the polyamide resin support, thereby obtaining a polyamide resin support that has excellent dimensional stability and can be used for long periods of time.

[0011] That is [1] The present invention relates to a polyamide resin support having a network structure made of filaments containing a polyamide resin as a main component, and having a dimensional change rate (%) represented by formula (1) of −1.0 to 1.5%.

[0012]

number

[0013] [2] 3300 cm in the Raman spectrum of the filament -1 The full width at half maximum of the peak is 15 to 43 cm -1 The polyamide resin support according to [1] above, [3] The polyamide resin support according to [1] or [2] above, wherein the filament is a monofilament. [4] The polyamide resin support according to any one of [1] to [3] above, wherein the filament has a fineness of 1,000 to 350,000 dtex. [5] The polyamide resin support according to any one of [1] to [4] above, wherein the network structure is a tortoiseshell network. [6] A method for producing a polyamide resin support, comprising forming a filament made mainly of polyamide resin into a mesh and then heat-treating the filament, in which the atmospheric temperature is set to the melting point plus 15 to 60°C and the heat treatment is performed while maintaining a fixed length. [7] The method for producing a polyamide resin support according to [6] above, wherein the filament containing polyamide resin as a main component is a monofilament. [8] The method for producing a polyamide resin support according to the above [6] or [7], wherein the filament containing a polyamide resin as a main component has a fineness of 1,000 to 350,000 dtex. [9] The method for producing a polyamide resin support according to any one of the above [6] to [8], further comprising forming a filament having a polyamide resin as a main component into a tortoiseshell net. Effect of the Invention

[0014] According to the present invention, it is possible to obtain a polyamide resin support which is excellent in dimensional stability and can be used for a long period of time when used as a mortar reinforcing material. [Brief description of the drawings]

[0015] [Figure 1]FIG. 2 is a diagram for explaining a method for measuring a Raman spectrum in a cross section perpendicular to the longitudinal fiber direction of a filament in the present invention. [Diagram 2] FIG. 2 is a diagram for explaining a method for calculating the full width at half maximum at 3300 cm −1 of a Raman spectrum in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below.

[0017] The polyamide resin support of the present invention has a network structure made of filaments containing polyamide resin as a main component, and has a dimensional change rate (%) represented by the formula (1) of −1.0 to 1.5%.

[0018]

number

[0019] The polyamide resin support of the present invention has a network structure made of filaments mainly composed of polyamide resin. Examples of polyamide resins that can be used in the present invention include polyamide 6 (hereinafter referred to as N6), polyamide 66 (hereinafter referred to as N66), polyamide 6 / 10 (hereinafter referred to as N610), polyamide 6 / 12 (hereinafter referred to as N612), polyamide 11 (hereinafter referred to as N11), and polyamide 12 (hereinafter referred to as N12), among which N6 or N610 is preferably used. The filaments mainly composed of polyamide resin means that the filaments contain polyamide resin at a ratio of more than 50% of the components other than inorganic components among the components constituting the filaments.

[0020] The form of the filament is not particularly limited and may be any of spun yarn, multifilament, monofilament, etc., but monofilament is preferred because its rigidity makes it easy to feed the filament to a net-making machine and because no fluffing occurs during the manufacturing process.

[0021] The polyamide resin support of the present invention has a net structure, and although the shape and size of the net are not particularly limited, it is preferably a tortoiseshell net. Since the tortoiseshell net has no knots or fusions at the intersections of the net, the strength of the filament does not decrease and the mortar reinforcing effect is high. In addition, the net is difficult to deform after the support is manufactured, has excellent shape stability, and is easy to apply when applying mortar, making it easy to handle.

[0022] The polyamide resin support of the present invention preferably has a dimensional change rate (%) represented by the above formula (1) of -1.0 to 1.5%, more preferably -0.5 to 1.0%, and further preferably 0.0 to 0.5%. Here, the dimensional change rate (%) represented by the above formula (1) is a value obtained based on the support porosity obtained as follows.

[0023] The porosity (%) of the support shown in formula (1) can be calculated by formula (2).

[0024]

number

[0025] The support after the 140°C dry heat treatment was a 1 m x 1 m support that had been left in a hot air circulating dryer whose temperature was adjusted to 140°C for 30 minutes.

[0026] The basis weight described in formula (2) is the mass per unit area under standard conditions as specified in JIS L 1096:2010, 8.3.2. a) According to the provisions of Method A, the mass measured on a 50 cm x 50 cm test piece is multiplied by 1 m 2 Mass per unit (g / m 2 ) and calculate the average value. The thickness shown in formula (2) is the thickness measured according to the provisions of JIS L 1096:2010, 8.4 Thickness, a) Method A, and the density is the density of the polyamide resin used in the support.

[0027] On the other hand, when a polyamide resin support having a dimensional change rate (%) represented by the above formula (1) below -1.0% or above 1.5% is used as a mortar reinforcing material, peeling may occur at the interface between the mortar and the polyamide resin support, and the reinforcing effect may decrease over time, which is not preferable.

[0028] In addition, since the dimensions of a polyamide resin support change most at 140°C, which is approximately the crystallization temperature of polyamide resin, the dimensional change over time of a polyamide resin support, which should essentially be observed over a long period of time, can be observed in an accelerated manner using the dimensional change rate (%) expressed by the above formula (1).

[0029] The polyamide resin filament (hereinafter sometimes abbreviated as polyamide resin filament) constituting the polyamide resin support of the present invention has a peak at 3300 cm in Raman spectrum. -1 The full width at half maximum of the peak is 15 to 43 cm -1 It is preferable that the thickness is 15 to 40 cm. -1 and more preferably 15 to 37 cm -1 3300 cm in the Raman spectrum -1 The peak at 3300 cm in the Raman spectrum is due to the NH group of the polyamide resin. -1 The smaller the full width at half maximum of the peak, the higher the crystallinity inside the polyamide resin filament and the more stable the internal structure.

[0030] On the other hand, the 3300 cm -1 The full width at half maximum of the peak is 43 cm -1 When a polyamide resin support having a thickness exceeding 100 mm is used as a mortar reinforcing material, the crystals present inside the polyamide resin filament do not grow sufficiently, and the structure inside the polyamide resin filament changes over time, resulting in a large change in the dimensions of the polyamide resin support, which is undesirable because peeling occurs at the interface between the mortar and the polyamide resin support, and the reinforcing effect decreases over time.

[0031] The fineness of the polyamide resin filament of the present invention is preferably 1,000 to 350,000 dtex, more preferably 8,000 to 150,000 dtex, and further preferably 20,000 to 80,000 dtex.

[0032] On the other hand, when a polyamide resin support having a polyamide resin filament fineness of less than 1000 dtex is used as a mortar reinforcing material, the mesh space volume for holding the mortar becomes small, which is not preferable because the mortar may not be held sufficiently during construction. Also, when the polyamide resin filament fineness exceeds 350000 dtex, the rigidity of the support becomes high, which is not preferable because it may cause gaps between the wall surface to be constructed and the support, making handling difficult.

[0033] The method for producing the polyamide resin support of the present invention includes a method for melt-spinning a monofilament and then forming a monofilament into a mesh, a method for melt-spinning a multifilament and then forming a multifilament into a mesh, and a method for entangling and fusing filament-like resins extruded from an extruder into a three-dimensional net shape to form a long filament three-dimensional bond in the product flow direction. Among the above-mentioned production methods, the method for melt-spinning a monofilament and then forming a monofilament into a mesh is preferred because it is easy to make the mesh size of the polyamide resin support uniform and the monofilament is easy to supply to a mesh machine due to the rigidity of the monofilament. As mentioned above, the mesh shape of the polyamide resin support of the present invention is preferably a tortoiseshell mesh, and the following is an example of a method for melt-spinning a monofilament and a method for forming a tortoiseshell mesh using a monofilament. However, the production method is not limited to this.

[0034] A monofilament mainly composed of polyamide resin can be produced by measuring and mixing polyamide resin and any other raw materials such as pigments, feeding the mixture to a known melt spinning machine, melt-kneading the mixture, and then extruding the mixture through a spinneret hole. Note that a monofilament mainly composed of polyamide resin means that the monofilament contains polyamide resin in a proportion of more than 50% of the components other than inorganic components that constitute the monofilament.

[0035] The molten material extruded from the spinneret holes is cooled and solidified in a cooling medium to obtain an undrawn yarn. Examples of the cooling medium include water and polyethylene glycol, but there is no particular limitation as long as it can be easily removed from the surface of the monofilament after cooling and solidification.

[0036] Then, in order to obtain the strength required for a monofilament, the undrawn yarn obtained by cooling and solidifying is heated and drawn in one or multiple stages, and then subjected to a relaxation heat treatment. In the present invention, the total draw ratio is 3.0 to 7.0 times, and the yarn can be obtained by performing one or multiple stage drawing with a draw ratio distribution ratio of 70 to 100% in the first stage, followed by heat treatment at 0.80 to 1.00 times. Here, the total draw ratio refers to the product of the draw ratios in the drawing process, and does not include the relaxation ratio in the heat treatment process.

[0037] The heat transfer medium used during the heat stretching or heat treatment may be air, hot water, steam, polyethylene glycol, glycerin, silicone oil, etc., but is not particularly limited as long as it can be easily removed from the surface of the monofilament after the heat stretching or heat treatment.

[0038] Depending on the type of heat medium, the stretching temperature can be 60 to 200°C, and the heat treatment temperature can be 110 to 200°C.

[0039] The monofilament thus obtained can be given a finishing oil, coated with a resin, or printed, if necessary.

[0040] The cross-sectional shape of the monofilament is not limited to a circular cross-section, but may be any cross-sectional shape, such as a flat, triangular, star-shaped, hollow, or other irregular cross-section, or a cross-section having a hollow portion, or a composite cross-section such as a core-sheath composite or sea-island type.

[0041] The monofilaments thus obtained can be successively treated in the steps described below to obtain tortoiseshell netting continuously.

[0042] First, in the tortoiseshell net making process, a plurality of monofilaments obtained by the melt spinning method are aligned and fed into a known tortoiseshell net manufacturing device, where the monofilaments are crossed with each other and continuously twisted together so that the straight and twisted parts of the monofilaments form the sides of a hexagonal tortoiseshell net. Next, the tortoiseshell net made from the above process is continuously heat-treated at an atmospheric temperature of 15 to 60°C above the melting point for 45 to 180 seconds while maintaining a fixed length, and then cooled to produce the tortoiseshell net.

[0043] The heat treatment has the effect of promoting the growth of crystals present in the polyamide resin filament and the relaxation of amorphous matter. By passing through the heat treatment process at the atmospheric temperature, the molecules present in the outermost layer of the polyamide resin filament relax and crystallization is promoted in the inner layer, so that a resin support body with a stable internal structure and small dimensional change over time can be obtained. The heat treatment temperature is particularly preferably in the range of the melting point plus 30 to 60°C.

[0044] On the other hand, when the heat treatment temperature is lower than the melting point plus 15°C, sufficient heat is not applied to the polyamide resin filament, and the heat treatment effect cannot be obtained, which may result in large dimensional changes in the polyamide resin support, which is not preferable. Also, when the heat treatment temperature is higher than the melting point plus 60°C, excessive heat is applied to the polyamide resin filament during the heat treatment, which may cause the center of the polyamide resin filament to reach the melting point or higher, which may result in melting.

[0045] The heat treatment time is preferably from 45 to 180 seconds, and more preferably from 60 to 120 seconds.

[0046] On the other hand, when the heat treatment temperature is 15 to 60°C above the melting point and the heat treatment time is less than 45 seconds, sufficient heat is not applied to the polyamide resin filament, the heat treatment effect is not obtained, and the dimensional change of the polyamide resin support may become large, which is not preferable. Also, when the heat treatment temperature is 15 to 60°C above the melting point and the heat treatment time is more than 180 seconds, excessive heat is applied to the polyamide resin filament during the heat treatment, and the center of the polyamide resin filament may reach the melting point or higher, which is not preferable, and the polyamide resin filament may melt.

[0047] In the present invention, the polyamide resin filament to be subjected to the net-making step preferably has a fineness of 1,000 to 350,000 dtex, more preferably 8,000 to 150,000 dtex, and further preferably 20,000 to 80,000 dtex.

[0048] On the other hand, when the fineness of the polyamide resin filament is less than 1000 dtex, the small fineness causes excessive heat to be applied to the polyamide resin filament during the heat treatment, and the central part of the polyamide resin filament may reach the melting point or higher and melt-cut, which is not preferable. Also, when the fineness of the polyamide resin filament is 350000 dtex or less, the rigidity of the polyamide resin filament falls within a range that is easy to handle during processing, which is preferable because stable processing can be performed.

[0049] In the present invention, the breaking strength of the polyamide resin filament to be subjected to the net-making step is preferably 300 to 3000N, more preferably 500 to 2500N, and further preferably 500 to 2000N.

[0050] On the other hand, if the breaking strength of the polyamide resin filament is less than 300 N, the polyamide resin filament may break during net making, which is not preferred. Also, if the breaking strength of the polyamide resin filament exceeds 3000 N, the rigidity of the polyamide resin filament becomes high, which is not preferred, since the polyamide resin filament may crack during net making. EXAMPLES

[0051] Examples of the present invention will be described below, but the present invention is not limited to these. Measurements of each characteristic were carried out as follows.

[0052] (1) Measurement of the basis weight of the substrate Mass per unit area under standard conditions as specified in JIS L1096:2010, 8.3.2 a) According to the provisions of Method A, the mass measured for two 50cm x 50cm test pieces is multiplied by 1m 2 Mass per unit (g / m 2 ) and the average value was calculated.

[0053] (2) Measurement of the thickness of the support Measurement was performed in accordance with the provisions of JIS L 1096:2010, 8.4 Thickness a) Method A.

[0054] (3) Measurement of dimensional change rate of support The dimensional change rate of the support was calculated by formula (1). Note that the support after the 140°C dry heat treatment described in formula (1) is a support of 1 m x 1 m that was left in a hot air circulating dryer whose temperature was adjusted to 140°C for 30 minutes.

[0055]

number

[0056] (4) Measurement of support porosity The porosity of the support was calculated by the formula (2). The density shown in the formula (2) is the density of the polyamide resin used in the support.

[0057]

number

[0058] (5) Raman spectrum of the striatum 3300cm -1 Measurement of full width at half maximum of peaks at Using a laser Raman spectrophotometer manufactured by JASCO Corporation, a beam with a diameter of 4 μm was irradiated at equal intervals (position 2b) so that a total of 30 points were irradiated from the center (position 2a) of the cross section perpendicular to the longitudinal direction of the filament constituting the resin support to the outermost layer (position 2c), as shown in FIG. 1. The resulting 90 to 3800 cm -1 In contrast to the Raman spectrum of -1 The full width at half maximum of the peak at was obtained as shown in Figure 2. The average value was calculated from the full width at half maximum obtained at each measurement point. Note that the outermost layer in the cross section of the filament is the position where the outer periphery of the 4 μm diameter beam comes into contact with the cross section of the filament.

[0059] (6) Measurement of fineness Measurements were taken in accordance with JIS L 1013:2010.

[0060] (7) Breaking strength measurement of polyamide resin filaments The measurement was performed using a tensile tester (Autograph AGX-10KNVD, manufactured by Shimadzu Corporation) in accordance with JIS L 1013:2010.

[0061] (8) Evaluation of mortar retention Install the polyamide resin support and raise it 60 degrees from the horizontal position. o 100mL of mortar, a mixture of cement, sand, and water in a ratio of 1:3:0.5, was poured onto a tilted 50cm x 50cm piece of wood, and the time the mortar was retained on the support without flowing off onto the floor was measured. Mortar retention times of 1 minute or more were rated as 'Good', and those of less than 1 minute were rated as 'Poor'.

[0062] [Example 1] The melt-spun polyamide resin monofilament with a fineness of 35,000 dtex was subjected to a tortoiseshell net making process to obtain a tortoiseshell net, which was then continuously heat-treated at the melting point plus 40°C for 60 seconds, cooled to solidify the shape, and wound up. The evaluation results of the polyamide resin support thus obtained are shown in Table 1.

[0063] [Examples 2 to 4] A net was produced in the same manner as in Example 1, except that the heat treatment temperature of the tortoiseshell net was adjusted as shown in Table 1. The evaluation results of the polyamide resin support thus obtained are shown in Table 1.

[0064] [Examples 5 to 6] A net was produced in the same manner as in Example 1, except that the fineness of the melt-spun polyamide resin monofilament was adjusted to be as shown in Table 1. The evaluation results of the polyamide resin support thus obtained are shown in Table 1.

[0065] [Examples 7 to 8] A net was produced in the same manner as in Example 1, except that the heat treatment time of the tortoiseshell net was adjusted as shown in Table 1. The evaluation results of the polyamide resin support thus obtained are shown in Table 1.

[0066] [Comparative Example 1] A net was produced in the same manner as in Example 1, except that the heat treatment temperature of the tortoiseshell net was adjusted as shown in Table 2. The evaluation results of the polyamide resin support thus obtained are shown in Table 2.

[0067] [Comparative Example 2] A net was produced in the same manner as in Example 1, except that the heat treatment temperature of the tortoiseshell net was adjusted as shown in Table 2. However, due to melting of the polyamide resin monofilament during the heat treatment, a polyamide resin support was not obtained and evaluation was not possible.

[0068] [Comparative Example 3] A net was produced in the same manner as in Example 1, except that the fineness of the melt-spun polyamide resin monofilament was adjusted to be as shown in Table 2. However, because the fineness was small, the polyamide resin monofilament melted and broke during the heat treatment, and a polyamide resin support was not obtained, so that evaluation was not possible.

[0069] [Comparative Example 4] A net was made in the same manner as in Example 1, except that the fineness of the melt-spun polyamide resin monofilament was adjusted to be as shown in Table 2. However, since the fineness was large and the polyamide resin monofilament could not be stably fed to the net-making machine, a polyamide resin support was not obtained, and therefore evaluation was not possible.

[0070] [Comparative Example 5] A net was produced in the same manner as in Example 1, except that the heat treatment time of the tortoiseshell net was adjusted as shown in Table 2. The evaluation results of the polyamide resin support thus obtained are shown in Table 2.

[0071] [Comparative Example 6] A net was produced in the same manner as in Example 1, except that the heat treatment time of the tortoiseshell net was adjusted as shown in Table 2. However, due to melting of the polyamide resin monofilament during the heat treatment, a polyamide resin support was not obtained and evaluation was not possible.

[0072] [Table 1]

[0073] [Table 2] [Industrial Applicability]

[0074] According to the present invention, as described above, it is possible to obtain a polyamide resin support having an internal structure with excellent dimensional stability as a mortar reinforcing material, which can be used continuously for a long period of time in place of metal supports that have been conventionally used as mortar reinforcing materials. [Explanation of symbols]

[0075] 1. Cross-section of the striatum 2a Laser beam irradiated at the center of the striatum 2b Laser beams irradiated at equal intervals between 2a and 2b 2c Laser beam irradiated onto the outermost layer of the striatum

Claims

1. A polyamide resin support having a network structure made of filaments mainly composed of polyamide resin, the dimensional change rate (%) being represented by the formula (1) being −1.0 to 1.5%. [0010]

2. In the Raman spectrum of the filament, -1 The full width at half maximum of the peak is 15 to 43 cm -1 2. The polyamide resin support of claim 1,

3. 3. The polyamide resin support according to claim 1 or 2, wherein the filament is a monofilament.

4. 3. The polyamide resin support according to claim 1, wherein the filament has a fineness of 1,000 to 350,000 dtex.

5. 3. The polyamide resin support according to claim 1, wherein the network structure is a tortoiseshell network.

6. This method for producing a polyamide resin support comprises forming a filament made mainly of polyamide resin into a mesh and then heat-treating the filament, the filament being heated at an atmospheric temperature of 15 to 60°C above the melting point while maintaining a fixed length.

7. The method for producing a polyamide resin support according to claim 6, wherein the filament containing the polyamide resin as a main component is a monofilament.

8. The method for producing a polyamide resin support according to claim 6 or 7, wherein the filament containing a polyamide resin as a main component has a fineness of 1,000 to 350,000 dtex.

9. The method for producing a polyamide resin support according to claim 6 or 7, further comprising forming the filaments containing the polyamide resin as a main component into a tortoiseshell net.

Citation Information

Patent Citations

  • Dehydration of garlic

    JP1986052259A

  • Bidirectional optical communication equipment

    JP1995030495A

  • Net for reinforcing mortar

    JP2003074160A

  • Tunnel inner wall construction method

    JP3918030B2