Laminated film and workpiece obtained by sealing laminated film

The laminated film with specific resin layers and properties addresses the issue of easily torn seals and improves production efficiency, offering high elongation, strength, and odor resistance for bags.

JP2024169841APending Publication Date: 2024-12-06OKURA INDUSTRIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023086637
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Laminated films used for making bags often have seals that are easily torn, especially when using fusing seals, and there is a need for improved production efficiency and odor resistance.

Method used

A laminated film structure comprising an inner layer of polyethylene resin, an intermediate layer of polybutylene terephthalate resin, and an outer layer of polyethylene resin, with an adhesive resin layer in between, where the intermediate layer has a modified resin with a Vicat softening point of 40°C to 53°C, and the polyethylene resin has a melt tension of 5.0 g to 20.0 g at 190°C, allowing for high elongation and strength in the seal portion.

Benefits of technology

The laminated film achieves high elongation and strength in the seal portion, making it difficult to tear, while maintaining excellent odor resistance and enabling faster sealing with improved production efficiency, suitable for making bags with enhanced deodorizing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169841000001_ABST
    Figure 2024169841000001_ABST
Patent Text Reader

Abstract

To provide a laminated film in which a seal part is hardly torn when the laminated film is sealed to form a bag and to provide a workpiece in which a thermally-cut seal part is hardly torn even when the laminated film is sealed by thermal-cut sealing.SOLUTION: A laminated film comprises an inner layer (A), an intermediate layer (B) and an outer layer (C), wherein the inner layer (A) and the outer layer (C) are mainly composed of a polyethylene-based resin, the intermediate layer (B) is mainly composed of a polybutylene terephthalate-based resin, and the interlayers between the inner layer (A) and the intermediate layer (B) and between the intermediate layer (B) and the outer layer (C) are laminated via an adhesive resin layer (D) mainly composed of a modified resin having a Vicat softening point of 40°C to 53°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film and a processed product obtained by sealing the laminated film. [Background technology]

[0002] Patent Document 1 describes an invention relating to an odor-barrier co-extruded multilayer film that is easy to process for use in packaging materials filled with food, miscellaneous goods, etc., to prevent deterioration of the contents due to erosion by volatile components from the outside during storage, and a packaging material and packaging container that use the same (Patent Document 1

[0001] ).

[0003] In the examples of Patent Document 1, a coextruded multilayer film having a structure of LLDPE / adhesive resin / PBT copolymer / adhesive resin / LLDPE is described. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-11741 A Summary of the Invention [Problem to be solved by the invention]

[0005] Generally, when making a bag from a laminated film, the bag is often made by sealing the sides and bottom of the bag, but bags made in this manner tend to have a tendency to tear at the sealed parts, resulting in the bag breaking.

[0006] Therefore, an object of the present invention is to provide a film whose seal portion is unlikely to tear when the laminated film is sealed to form a bag. [Means for solving the problem]

[0007] As a result of thorough investigation into the above-mentioned problems, the inventors have found that in order to make a sealed portion resistant to tearing, the sealed portion needs to be stretchable. Specifically, they have found that by giving the sealed portion the property of stretching (hereinafter sometimes referred to as extensibility), even if stress is applied to the sealed portion, the applied stress can be dispersed, and a bag with a sealed portion resistant to tearing can be obtained.

[0008] Furthermore, the present inventors have studied a method of making a bag using a fusion seal for the purpose of improving the production efficiency when sealing a laminated film to make a bag. However, when sealing a laminated film using a fusion seal, the sealed portion is more likely to break than when sealing with a hot plate. This is because, while sealing with a fusion seal allows for faster sealing, the sealing time is shorter than that of hot plate sealing, and the sealing pressure is also smaller, so that the laminated films may not be sufficiently fused together. Furthermore, the fusion seal portion where the laminated film is fusion-sealed has a smaller fusion area than the hot plate sealing portion where the hot plate sealing is performed, so that the laminated films may not be sufficiently fused together.

[0009] Therefore, as a means for solving the above problems of the present invention, (1) A laminated film having an inner layer (A), an intermediate layer (B), and an outer layer (C), The inner layer (A) and the outer layer (C) each contain a polyethylene resin as a main component, The intermediate layer (B) is mainly composed of a polybutylene terephthalate resin, the inner layer (A) and the intermediate layer (B), and the intermediate layer (B) and the outer layer (C) are laminated with an adhesive resin layer (D) interposed therebetween; the adhesive resin layer (D) is a laminated film comprising, as a main component, a modified resin having a Vicat softening point of 40° C. or more and 53° C. or less; (2) The laminated film according to (1), wherein the polyethylene resin has a melt tension of 5.0 g or more and 20.0 g or less at 190° C.; (3) The laminate film according to (1) or (2), characterized in that the laminate film has a total thickness of 50 μm or less; (4) The laminate film according to any one of (1) to (3), wherein the laminate film is a coextruded air-cooled inflation film. (5) A processed product having a sealed portion formed by sealing the laminated film according to any one of (1) to (4); (6) The processed product according to (5), characterized in that the elongation of the seal portion is 100% or more; (7) The processed product according to (5) or (6), characterized in that the strength of the seal portion is 2N / 15mm or more; (8) The workpiece according to any one of (5) to (7), characterized in that the seal portion is a melt-cut seal; (9) The processed product according to any one of (5) to (8) is a bag obtained by making a bag; (10) The processed product according to any one of (5) to (8) is a deodorizing bag produced by bagging; The gist of this paper is as follows. Effect of the Invention

[0010] According to the first invention, the film has an excellent deodorizing property because it has a layer mainly composed of polybutylene terephthalate resin. In addition, by using a modified resin having a Vicat softening point of 40°C or more and 53°C or less as a main component between the intermediate layer (B) mainly composed of polybutylene terephthalate resin and the inner layer (A) and outer layer (C) mainly composed of polyethylene resin, the layers can be bonded sufficiently, and when the obtained laminated film is sealed by melt-cutting to form a processed product, the sealed part has extensibility, so that the sealed part is difficult to tear. According to the second invention, a laminated film with good film formation stability and suitability for welding seal can be obtained by using a polyethylene resin for the inner layer (A) and outer layer (C) that has a melt tension of 5.0 g or more and 20.0 g or less at 190°C, which is higher than that of general polyethylene resins. To explain the suitability for welding seal in detail, the high melt tension makes it difficult for whiskers to occur during welding seal, and reduces variations in seal strength and seal elongation. According to the third invention, when sealing the laminated film to make a processed product, sealing is possible even with a small amount of heat required to melt the laminated film, so that the sealing speed can be increased and production efficiency can be improved. Furthermore, a laminated film with excellent suitability for melt-cutting and sealing can be obtained. In addition, since the layer thickness is thin at 50 μm or less, when the laminated film is made into a bag (preferably an odor-proof bag), the opening of the bag can be easily tied. According to the fourth aspect of the present invention, a tubular film can be obtained, so that bags can be made with fewer sealing points. In addition, the width can be easily changed to any desired width, so that bags of different sizes can be easily made. Furthermore, since the strength of the film is well balanced in the length direction and width direction, a bag that is difficult to tear can be obtained when the laminated film 1 is used to make a bag. According to the fifth aspect of the present invention, a processed product having excellent odor prevention properties can be obtained. Also, a processed product having a sealed portion that is difficult to tear can be obtained. According to the sixth aspect of the present invention, the seal portion has sufficient extensibility, so that the seal portion is unlikely to tear. According to the seventh aspect of the present invention, the seal portion has sufficient strength, so that the seal portion is unlikely to be broken. According to the eighth aspect of the present invention, the sealing speed can be increased compared to hot plate sealing, improving production efficiency. Also, it is easier to respond to changes in the specifications of the workpiece than hot plate sealing. According to the ninth aspect of the present invention, the sealed portion has sufficient extensibility, so that the sealed portion is less likely to tear. According to the tenth aspect of the present invention, the sealed portion has sufficient extensibility, so that the sealed portion is difficult to tear. Also, since the bag is made of a laminated film having an intermediate layer (B) mainly composed of a polybutylene terephthalate resin, the odor-proof bag has excellent odor-proofing properties. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional view illustrating one embodiment of a laminated film according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram for explaining in detail a method for measuring the elongation and strength of a sealed portion where a laminated film according to the present invention is sealed. [Diagram 3] 1A is a schematic perspective view showing a bag made by welding sealing using the laminated film of the present invention, FIG. 1B is a schematic side view, and FIG. 1C is a schematic partial cross-sectional view showing an enlarged view of the sealed portion. [Figure 4] 1A is a schematic perspective view showing a bag made by hot plate sealing using the laminated film of the present invention, FIG. 1B is a schematic side view, and FIG. 1C is a schematic partial cross-sectional view showing an enlarged view of the sealed portion. [Diagram 5] 1A to 1C are schematic plan views showing a method for producing a bag by heat-cutting and sealing a laminated film according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below, but the present invention is not limited thereto, and various forms can be adopted within the scope of the present invention as long as the same effects are achieved, without departing from the gist of the present invention.

[0013] In this specification, the term "main component" means a component that constitutes a layer and accounts for 50% by weight or more, preferably 60% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, and particularly preferably 95% by weight or more.

[0014] Regarding the term "sealed portion" in this specification, a sealed portion sealed by melt-cutting may be referred to as a "melt-cutting sealed portion", and a sealed portion sealed by a hot plate may be referred to as a "hot plate sealed portion".

[0015] A typical structure of the laminated film in the present invention is an inner layer (A) mainly composed of a polyethylene-based resin / adhesive resin layer (D) / intermediate layer (B) mainly composed of a polybutylene terephthalate-based resin / adhesive resin layer (D) / outer layer (C) mainly composed of a polyethylene-based resin.

[0016] FIG. 1 shows a schematic cross-sectional view of the representative configuration described above.

[0017] <Inner layer (A)> The inner layer (A) is mainly composed of a polyethylene resin, which allows the laminated film 1 to have excellent sealing properties.

[0018] The density of the polyethylene resin used for the inner layer (A) is not particularly limited, but is preferably 0.880 to 0.930 g / cm. 3 is preferable, and more preferably 0.915 to 0.925 g / cm 3 It is.

[0019] Density 0.915g / cm 3 By doing so, the crystallinity of the polyethylene resin can be increased, and the laminate film 1 can have excellent blocking resistance. In addition, the laminate film 1 can have excellent strength, and when the laminate film 1 is sealed to form a processed product, the sealed portion is unlikely to break.

[0020] Density 0.925g / cm 3By setting the following, it is possible to obtain a laminated film 1 that is excellent in flexibility and easy to stretch. As a result, when the laminated film 1 is sealed to form a processed product, the sealed portion can be made to be difficult to tear. Furthermore, since the laminated film 1 has excellent flexibility, when the laminated film 1 is sealed to form a processed product, the processed product can be made to be easy to handle, and further, when the laminated film 1 is made into a bag (preferably an odor-proof bag), the opening of the bag can be easily tied.

[0021] The melt tension at 190°C of the polyethylene resin used for the inner layer (A) is not particularly limited, but is preferably 5.0 g or more and 20.0 g or less, more preferably 6.0 g or more and 15.0 g or less, and even more preferably 7.0 g or more and 10.0 g or less. The melt tension at 190° C. is measured using a Capillograph 1C manufactured by Toyo Seiki Seisakusho Co., Ltd. under the following measurement conditions. <Measurement conditions> Nozzle used: L = 8,000 mm, D = 2.095 mm, barrel diameter: 9.55 mm, measurement temperature: 190°C, resin extrusion speed: 15 mm / min, resin take-up speed: 10 m / min.

[0022] A laminated film with good film formation stability and suitability for welding seal can be obtained by using a polyethylene resin with a melt tension of 5.0 g to 20.0 g at 190° C. for the inner layer and the outer layer described below. To explain the suitability for welding seal in detail, high melt tension makes it difficult for whiskers to form during welding seal, and reduces variations in seal strength and seal elongation.

[0023] Specific examples of polyethylene resins include ultra-low density polyethylene, low density polyethylene, high density polyethylene, linear low density polyethylene, etc., among which linear low density polyethylene is preferably used. Linear low density polyethylene has an appropriately low melting point, and therefore can be used to form a laminate film 1 with excellent sealability.

[0024] From the viewpoint of mechanical strength and processability, the melt flow rate (MFR) value of the polyethylene resin at 190° C. is preferably 1.0 to 10.0 g / 10 min, more preferably 1.0 to 5.0 g / 10 min, and particularly preferably 1.0 to 3.0 g / 10 min.

[0025] The polyethylene resin may be one type or two or more types, and when two or more types are used, the combination and ratio thereof can be selected arbitrarily according to the purpose. For example, a blend of linear low-density polyethylene and low-density polyethylene can be exemplified, but those skilled in the art can appropriately select a preferred form, and there is no particular limitation.

[0026] The melting point of the polyethylene resin used in the inner layer (A) is not particularly limited, but is preferably 80 to 135° C., more preferably 90 to 130° C., and particularly preferably 100 to 120° C. By keeping the melting point within the above range, a laminate film 1 with excellent sealability can be obtained.

[0027] Furthermore, additives may be added to the inner layer (A) as necessary, and those skilled in the art can add suitable additives as desired.

[0028] Furthermore, the inner layer (A) may contain other resins, and is not particularly limited, so long as it contains a polyethylene resin as the main component.

[0029] The thickness of the inner layer (A) is not particularly limited, but is preferably 1 to 20 μm, and more preferably 3 to 10 μm. If the inner layer (A) is in the above range, high-speed sealing is possible even when the laminated film 1 is sealed to form a processed product, and the strength of the seal portion formed by sealing the laminated film 1 can be made sufficient.

[0030] <Middle layer (B)> The intermediate layer (B) is mainly composed of polybutylene terephthalate resin. This allows the laminated film 1 to have excellent odor prevention properties. In addition, when the laminated film 1 is sealed and processed, it can be made into a processed product with excellent odor prevention properties.

[0031] The intermediate layer (B) is mainly composed of a polybutylene terephthalate resin. The polybutylene terephthalate resin may be one type or two or more types. When two or more types are used, the combination and ratio of the resins may be selected according to the purpose.

[0032] Specific examples of polybutylene terephthalate resins include homopolymers and copolymers. Examples of the acid component of the copolymer include, but are not limited to, terephthalic acid, isophthalic acid, and adipic acid.

[0033] The thickness of the intermediate layer (B) is not particularly limited as long as it can impart deodorizing properties to the laminated film 1, but is preferably 1 μm to 10 μm. Furthermore, the intermediate layer (B) exhibits sufficient deodorizing properties if its thickness is 2 μm or more, 3 μm or more, 4 μm or more, or 5 μm or more, and 9 μm or less, 8 μm or less, 7 μm or less, or 6 μm or less.

[0034] Furthermore, additives may be added to the intermediate layer (B) as necessary, and those skilled in the art can add suitable additives as desired.

[0035] Furthermore, the intermediate layer (B) may contain other resins as long as it contains polybutylene terephthalate resin as the main component, and is not particularly limited.

[0036] <Outer layer (C)> The outer layer (C) can be made of the same resin as described in the section on inner layer (A). By using the same resin for the inner layer (A) and the outer layer (C), the laminated film can be used without worrying about the front and back. It also makes the laminated film less prone to curling.

[0037] <Adhesive resin layer (D)> As shown in the representative configuration described above, the adhesive resin layer (D) is located between the inner layer (A) and the intermediate layer (B), and between the intermediate layer (B) and the outer layer (C).

[0038] When a laminated film is produced by a co-extrusion method, the polyester resin such as polybutylene terephthalate resin used in the intermediate layer (B) does not have good adhesion to the polyethylene resin used in the inner layer (A) and outer layer (C), so an adhesive resin layer (D) is required. The resin used in the adhesive resin layer (D) is often a modified resin. However, there are only a few modified resins that have good adhesion to polyester-based resins, and many modified resins are laminated in a state where the intermediate layer (B) and the adhesive resin layer (D) are easily peeled off from each other. As a result, when the laminated film is melt-cut and sealed to measure the seal strength, peeling occurs between the intermediate layer (B) and the adhesive resin layer (D), and high seal strength and seal elongation are not obtained in some cases. In the present invention, therefore, after trying many adhesive resins, it was found that a modified resin having a Vicat softening point of 40° C. or more and 53° C. or less should be used. The Vicat softening point is measured based on ASTM D 1525.

[0039] By setting the Vicat softening point of the modified resin to 40°C or higher and 53°C or lower, it is possible to firmly bond the intermediate layer (B) and the adhesive resin layer (D) together, and to obtain a laminated film with elongation properties in the sealed portion when heat-sealed. It is presumed that the modified resin has an anchor effect on the polybutylene terephthalate resin during film formation, which affects the adhesive strength, seal elongation, and seal strength. Modified resins with a Vicat softening point of less than 40°C are difficult to handle because their Vicat softening point is close to room temperature, and if the Vicat softening point exceeds 53°C, the desired elongation characteristics of the sealed portion cannot be obtained when melt-cut sealing is performed. The Vicat softening point of the modified resin is preferably 41° C. or higher, 42° C. or higher, or 43° C. or higher, and is preferably 52° C. or lower, 50° C. or lower, 48° C. or lower, or 46° C. or lower.

[0040] The modified resin according to the present invention is a resin modified by unsaturated carboxylic acid, its anhydride or derivative, etc., which is a resin in which the type or arrangement of a part of the molecular chain is changed without changing the basic structure of the resin. Examples of unsaturated carboxylic acid include maleic acid, itaconic acid, and fumaric acid, and examples of derivatives thereof include esters and anhydrides such as maleic acid monoester, maleic acid diester, maleic anhydride, itaconic acid monoester, itaconic acid diester, itaconic anhydride, fumaric acid monoester, fumaric acid diester, and fumaric anhydride. Examples of the above resin include ethylene-based polymers such as linear polyethylene, very low density polyethylene, high density polyethylene, ethylene-vinyl acetate (VA) copolymer, ethylene-ethyl acrylate (EA) copolymer, and ethylene-methacrylate copolymer, propylene-based polymers, and styrene-based elastomers. Among these, polyolefin-based resins including ethylene-based polymers and propylene-based polymers are preferred, and ethylene-based polymers are particularly preferred.

[0041] Furthermore, additives may be added to the adhesive resin layer (D) as necessary, and those skilled in the art can add suitable additives as desired.

[0042] Furthermore, the adhesive resin layer (D) may contain a resin other than the adhesive resin, and is not particularly limited. For example, the adhesive resin layer (D) may be a blend of an adhesive resin and a polybutylene terephthalate resin.

[0043] <Laminated film 1> The total thickness of the laminated film 1 is preferably from 1 to 50 μm, more preferably from 5 to 30 μm, and particularly preferably from 10 to 25 μm. By setting the thickness within the above range, the laminate film 1 can be made soft and easy to handle by reducing the thickness while providing appropriate stiffness and strength to the laminate film 1. Furthermore, when the thickness is within the above range, the laminate film 1 can be sealed to form a processed product even if the amount of heat required to melt the laminate film 1 is small. This allows for a high-speed sealing process, improving production efficiency. Furthermore, when the laminate film 1 is made into a deodorizing bag, it is possible to easily tie the opening of the deodorizing bag.

[0044] The laminated film 1 of the present invention is preferably a co-extruded air-cooled inflation film. By using a co-extruded air-cooled inflation film, a tubular film can be obtained, which allows bags to be made with fewer sealing points. In addition, the width can be easily changed to any desired width, which allows bags of different dimensions to be made easily. Furthermore, since the film has an excellent balance of strength in the length direction and width direction, when the laminated film 1 is used to make a bag, a bag that is difficult to tear can be obtained.

[0045] The laminated film 1 of the present invention is not limited to the above-mentioned typical configuration, and layers other than the inner layer (A), intermediate layer (B), outer layer (C), and adhesive resin layer (D) may be provided as necessary.

[0046] As shown in the above representative structure, by forming the layers symmetrically in the thickness direction, the laminate film 1 can be made less prone to curling.

[0047] <Processed product> By sealing the laminated film of the present invention, a processed product having a sealed portion can be obtained.

[0048] The laminated film of the present invention has excellent elongation. Therefore, even when the laminated film is sealed to provide a sealed portion, it is possible to obtain a processed product that has excellent elongation and is difficult to tear. In addition, because of the excellent elongation, when the laminated film is sealed to form a bag, it is possible to obtain a processed product in which the sealed portion is difficult to tear. Specifically, even if stress is applied to the sealed portion, the applied stress can be dispersed, and a bag in which the sealed portion is difficult to tear can be obtained.

[0049] The processed product obtained by the present invention has a sealed portion, and if the sealed portion has sufficient extensibility and strength, the sealed portion can be made to be resistant to tearing.

[0050] Specifically, the elongation of the sealed portion is preferably 100% or more, 120% or more, 140% or more, 160% or more, 180% or more, 200% or more, 250% or more, or 300% or more. By stretching the sealed portion, the sealed portion can be made into a processed product that is difficult to tear. Furthermore, when the laminated film is sealed to make a bag, the sealed portion can be made into a bag that is difficult to tear. There is no particular upper limit to the elongation of the sealed portion.

[0051] FIG. 2 is a schematic diagram for explaining in detail a method for measuring the elongation and strength of a sealed portion formed by sealing a laminated film according to the present invention.

[0052] The method for measuring the elongation of the seal portion will be explained in detail below with reference to FIG. (1) The laminated film 1 is sealed to produce a processed product having a sealed portion. (2) A rectangular test piece 4 (width 15 mm) is prepared from a workpiece having a seal portion. At this time, the test piece is prepared so that the seal portion 3 is positioned in the center in the longitudinal direction of the test piece, as shown in FIG. (3) The test piece 4 is attached to a tensile testing machine. The distance between the chucks is 40 mm. (4) The tensile test is performed at a speed of 500 mm / min in the tensile direction shown in FIG. 2 until the seal portion 3 breaks. (5) Calculate the elongation (%) of the seal part. The calculation method is as follows: Elongation (%) = ([Chuck distance at break] - [Chuck distance before tensile test (40 mm)]) / [Chuck distance before tensile test (40 mm)] × 100.

[0053] In addition, the strength of the sealed portion is preferably 2N / 15mm or more, 3N / 15mm or more, 5N / 15mm or more, 6N / 15mm or more, 7N / 15mm or more, 9N / 15mm or more, or 11N / 15mm or more. When the strength of the sealed portion is within the above range, the sealed portion can be made into a processed product that is difficult to tear. Furthermore, when the laminated film is sealed to make a bag, the sealed portion can be made into a bag that is difficult to tear. The upper limit of the strength of the sealed portion is not particularly limited. In addition, there is a correlation between the elongation and strength of the sealed portion, and when the sealed portion has elongation, the strength of the sealed portion tends to increase.

[0054] The method for measuring the strength of the seal portion is explained in detail below with reference to FIG. (1) The laminated film 1 is sealed to produce a processed product having a sealed portion. (2) A rectangular test piece 4 (15 mm wide) is made from a workpiece having a seal part. At this time, the test piece is made so that the seal part 3 is located in the center of the length direction of the test piece, as shown in Figure 2. (3) The test piece 4 is attached to a tensile testing machine. The distance between the chucks is 40 mm. (4) The tensile test speed is 500 mm / min, and the tensile test is performed in the tensile direction shown in FIG. 2 until the seal portion 3 breaks. (5) The strength of the seal (N / 15mm) is the maximum load at which the seal breaks.

[0055] In addition, the laminated film of the present invention has an intermediate layer (B) mainly composed of a polybutylene terephthalate resin, and therefore has excellent odor prevention properties. Therefore, when the laminated film of the present invention is sealed to produce a processed product, a processed product having excellent odor prevention properties can be obtained.

[0056] The processed product can be, for example, a bag made by sealing a laminated film. The bag made by the present invention has an odor-proof property and can be used as an odor-proof bag.

[0057] The odor-proof bag obtained by the present invention can contain odorous substances and can seal the odor of the odorous substances inside the odor-proof bag. Examples of odorous substances include human or animal excrement, used diapers, food waste, etc. Also examples include foods with strong odors such as kimchi and natto. Furthermore, odor-resistant items that are prone to absorbing odors can be stored in the odor-resistant bag, and the contents can be protected from odors outside the bag. For example, when storing items that contain volatile chemicals such as insect repellents, deodorants, and air fresheners in a location close to these items, the contents can be stored in the odor-resistant bag to protect them from the volatile chemicals. As described above, the contents to be contained in the odor-proof bag and the method of using the odor-proof bag are not particularly limited, and those skilled in the art can select a suitable preferred form.

[0058] In addition, the laminated film can be sealed to be processed into gloves. In this way, the form of the processed product can be appropriately determined by those skilled in the art as desired, and is not particularly limited.

[0059] Specific examples of the sealing method include melt-cutting sealing, hot plate sealing, ultrasonic sealing, and high-frequency sealing, and among these, it is preferable to employ melt-cutting sealing and hot plate sealing.

[0060] The laminated film of the present invention is very excellent in suitability for welding and sealing because the laminated films can be sufficiently fused together even when sealed at high speed. Furthermore, since welding and sealing is easier to respond to changes in the specifications of the processed products than other sealing methods, welding and sealing using the laminated film of the present invention can improve production efficiency.

[0061] FIG. 3 is a schematic perspective view (A) of a bag made by melt-cutting and sealing using the laminated film of the present invention, a schematic cross-sectional view (B), and a schematic partial side view (C) showing an enlarged view of the sealed portion.

[0062] 3A, the laminated film 1 can be used to make a bag by melt-sealing the sides and bottom of the bag to form melt-sealed parts 31. Alternatively, a bag can be made by folding a sheet of laminated film 1, making the crease the bottom of the bag, and melt-sealing the parts that will become the sides of the bag.

[0063] The method for producing the bag by welding and sealing can be a conventionally known method, and is not particularly limited.

[0064] FIG. 4 is a schematic perspective view (A), a schematic side view (B), and a schematic partial cross-sectional view (C) showing an enlarged view of the sealed portion, showing a bag made by hot plate sealing using the laminated film of the present invention.

[0065] As shown in the schematic perspective view (A) of Fig. 4, the laminated film can be made into a bag by sealing the sides and bottom of the bag with a hot plate to form hot plate sealed parts 32. Alternatively, a bag can be made by folding a sheet of laminated film, using the crease as the bottom of the bag, and sealing the parts that will become the sides of the bag with a hot plate.

[0066] The method for making bags by hot plate sealing can be any conventionally known method, and is not particularly limited.

[0067] Although the method of making a bag from a laminated film by melt-cutting or hot plate sealing has been described above, the bag can be made by a conventionally known method, and a person skilled in the art can appropriately select a preferred form. For example, a bag can be made by sealing the bottom of the bag with a hot plate and melt-cutting the sides of the bag, and then using melt-cutting and hot plate sealing. EXAMPLES

[0068] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples in any way.

[0069] <Examples 1 to 2, Comparative Examples 1 to 3> Using the resins listed below, a laminated film having a structure of inner layer (A) / adhesive resin layer (D) / middle layer (B) / adhesive resin layer (D) / outer layer (C) was obtained by coextrusion. The thickness of each layer is shown in Table 1. <Inner layer (A) and outer layer (C)> · Linear low density polyethylene (LLDPE) Density: 0.923g / cm 3 Melting point: 118℃, MFR: 1.5g / 10min(190℃), Melt tension(190℃): 8.1g <Middle layer (B)> Polybutylene terephthalate (PBT) Homopolymer, density: 1.310g / cm 3 Melting point: 223℃, MFR=5g / 10min 6-6,6 copolymer nylon (6-66 copolymer Ny) Copolymer, density: 1.14g / cm 3 <Adhesive resin layer (D)> Modified resin 1: Maleic anhydride modified polyolefin Density: 0.88g / cm 3 , MFR: 2.6 / 10min., Vicat softening point: 43℃ Modified resin 2: Maleic anhydride modified ethylene methyl acrylate Density: 0.93g / cm 3 , MFR: 1.6g / 10min., Vicat softening point: 52℃ Modified resin 3: Maleic anhydride modified polyolefin Density: 0.90g / cm 3 , MFR: 3.5g / 10min., Vicat softening point: 55℃ Modified resin 4: Acid-modified LLDPE Density: 0.90g / cm 3 , MFR: 1.0g / 10min., Vicat softening point: 74℃ Modified resin 5: Acid-modified LLDPE Density: 0.914g / cm 3 , MFR: 6.5g / 10min., Vicat softening point: 46℃

[0070] <<Stretchability and strength of laminated film>> The elongation and strength of the obtained laminated film were evaluated. Specifically, the elongation and strength of the laminated film in the MD and TD directions were measured. The measurement method was performed with reference to JIS K 7127 (1989), and the measured value was the average of five samples excluding the maximum and minimum values ​​of seven samples. The chuck distance was 80 mm, and the tensile test speed was 500 mm / min. The measurement results are shown in Table 1.

[0071] The obtained laminated film was then heat-cut and sealed to produce a workpiece having a heat-cut and sealed portion. The heat-cut and sealed method is described below.

[0072] [Fusing seal] The obtained laminated film was heat-cut and sealed to produce a bag by the following method. The specific production method is described in detail below with reference to Fig. 5. Fig. 5 is a schematic plan view showing the production method of producing a bag by heat-cutting and sealing the laminated film according to the present invention. (i) A laminate film 1 is prepared. (ii) The laminated film 1 is folded along the center in the width direction to produce a laminated film 1' having a crease 5. (iii) The laminated film 1' having the fold 5 is fusion-cut and sealed using a fusion-cutting and sealing device 6 to produce the bag 7. At this time, the laminated film 1' having the fold 5 in the direction perpendicular to the conveying direction shown in Fig. 5 is fusion-cut and sealed to produce the bag 7. In this way, the bottom of the bag 7 is formed by the fold 5, and the sides of the bag 7 are formed by the fusion-cut and sealed portions 31, making it possible to produce the bag 7. The sealing temperature of the welding sealing device 6 in the welding sealing machine was 300° C., and the contact time between the welding sealing device 6 and the laminated film 1′ having the fold 5 was 0.1 seconds, allowing the production of 45 bags per minute.

[0073] [Seal stretch] The elongation of the weld-sealed part of the bag produced by the weld-sealing method was measured. Since the produced bag had two weld-sealed parts (see Figure 5 (iii)), the elongation of the two weld-sealed parts (parts P and Q) was measured. The measurement results are shown in Table 1. The method for measuring the elongation of the seal portion will be explained in detail below with reference to FIG. (1) A rectangular test piece 4 (15 mm wide) is prepared from a workpiece or bag with a sealed portion. At this time, the test piece is prepared so that the sealed portion is located in the center of the length of the test piece, as shown in Figure 2. (2) The test piece 4 is attached to a tensile testing machine. The distance between the chucks is set to 40 mm. (3) The tensile test speed is 500 mm / min, and the tensile test is performed in the tensile direction shown in FIG. 2 until the seal portion 3 breaks. (4) Calculate the elongation (%) of the seal at the time of breakage. The calculation method is as follows: Elongation (%) = ([Chuck distance at break] - [Chuck distance before tensile test (40 mm)]) / [Chuck distance before tensile test (40 mm)] × 100.

[0074] [Seal strength] The strength of the weld-sealed parts of the bags produced by the weld-sealing method was measured. As the bags produced had two weld-sealed parts, the strength of the two weld-sealed parts (parts P and Q) was measured. The evaluation results are shown in Table 1. The method for measuring the strength of the sealed parts is explained in detail below with reference to Figure 2. (1) A rectangular test piece 4 (15 mm wide) is prepared from a workpiece or bag with a sealed portion. At this time, the test piece is prepared so that the sealed portion is located in the center of the length of the test piece, as shown in Figure 2. (2) The test piece 4 is attached to a tensile testing machine. The distance between the chucks is set to 40 mm. (3) The tensile test speed is 500 mm / min, and the tensile test is performed in the tensile direction shown in FIG. 2 until the seal portion 3 breaks. (4) The strength of the seal (N / 15mm) is the maximum load that can be applied until the seal breaks.

[0075] <Seal tear evaluation> We evaluated the tear resistance of the weld-sealed part of the bag produced by the weld-sealing method. As shown in Figure 3(B), the weld-sealed part was placed in the center, and a point 1 cm away from the weld-sealed part (d in Figure 3(B)) was grasped with the hand and pulled in the pulling direction shown in the figure to evaluate the tear resistance of the weld-sealed part. Note that although there are two pulling directions in Figure 3(B), pulling was performed in both directions at the same time. The evaluation criteria are as follows: ◯: When pulled in the tensile direction, it does not break immediately and the melt-cut sealed part stretches in the tensile direction. ×: When pulled in the tensile direction, the melt-cut sealed portion immediately breaks. The evaluation results are shown in Table 1.

[0076] Deodorization evaluation First, the obtained laminated film was sealed to produce a bag. The specific bag-making method was to fold the obtained laminated film in half so that the crease would become the bottom of the bag. Then, the side of the bag was sealed using a sealing machine described below to produce the bag. Sealing machine: Fuji Impulse P-300 (product number: H6196259 / 01301D), adhesive temperature: 180℃ Next, the following odor prevention evaluation was performed to confirm the odor prevention performance of the prepared bag. First, 10 g of kimchi was placed in the prepared bag, and the opening of the bag was tied. Then, the bag containing the kimchi was placed in an aluminum pouch with a zipper for 24 hours. After 24 hours, the aluminum pouch was opened and the odor was confirmed. The evaluation criteria are as follows. A: I didn't notice any smell. ×: A strong odor was felt. The evaluation results are shown in Table 1.

[0077] [Table 1]

[0078] From Table 1, it can be seen that in Examples 1 and 2 and Comparative Example 3, the elongation of the sealed portion is 100% or more, and that these have sufficient elongation compared to Comparative Examples 1 and 2. Furthermore, in Examples 1 and 2 and Comparative Example 3, the "evaluation of the seal portion breaking" is all rated "good," and it can be seen that when the elongation of the sealed portion is 100% or more, the sealed portion is less likely to break.

[0079] In addition, when comparing Example 1 and Comparative Example 1, the seal strength was not significantly different, with an average of 6.2 N / 15 mm for Example 1 and 5.65 N / 15 mm for Comparative Example 1, but the tear evaluation was "good" for Example 1 and "poor" for Comparative Example 1. This is thought to be due to the difference in seal elongation.

[0080] In Examples 1 to 2 and Comparative Examples 1 and 2 in which the intermediate layer (B) was PBT, the odor prevention evaluation was all "Good", and it is clear that they have better odor prevention properties than Comparative Example 3 in which the intermediate layer (B) was 6-66 copolymerized Ny. [Explanation of symbols]

[0081] 1. Laminated film (A) Inner layer (A) (B) Middle layer (B) (C) Outer layer (C) (D) Adhesive resin layer (D) 1′ Laminated film with folds 2 Workpiece 3. Seal Part 31 Welding seal part 32 Hot plate seal section 4. Test specimens 5. Crease 6. Welding and sealing equipment 7 bags

Claims

1. A laminated film comprising an inner layer (A), an intermediate layer (B), and an outer layer (C), The inner layer (A) and the outer layer (C) each contain a polyethylene resin as a main component, The intermediate layer (B) is mainly composed of a polybutylene terephthalate resin, the inner layer (A) and the intermediate layer (B), and the intermediate layer (B) and the outer layer (C) are laminated with an adhesive resin layer (D) interposed therebetween; The adhesive resin layer (D) is a laminated film characterized in that it contains as a main component a modified resin having a Vicat softening point of 40° C. or more and 53° C. or less.

2. 2. The laminated film according to claim 1, wherein the polyethylene resin of the inner layer (A) and the outer layer (C) has a melt tension at 190° C. of 5.0 g or more and 20.0 g or less.

3. 2. The laminate film according to claim 1, wherein the laminate film has a total thickness of 50 [mu]m or less.

4. 2. The laminate film according to claim 1, which is a coextruded inflation film.

5. A processed product comprising a sealed portion formed by sealing the laminated film according to any one of claims 1 to 4.

6. 6. The workpiece of claim 5, wherein the elongation of the seal portion is 100% or greater.

7. 6. The workpiece according to claim 5, wherein the strength of the seal portion is 2N / 15mm or more.

8. 6. The workpiece according to claim 5, wherein the seal portion is a fusion seal.

9. The processed product according to claim 5 is a bag produced by bag manufacturing.

10. The processed product according to claim 5 is a deodorizing bag produced by bagging.

Citation Information

Patent Citations

  • Coextruded multilayer film with bad smell barrier property, packaging material using the same, and packaging container

    JP2012011741A