Diaper and method for manufacturing diaper
The diaper design with a backsheet made of crimped fibers and elastomers addresses the issue of poor fit and discomfort by controlling stretchability and thickness change, enhancing comfort and motion tracking.
Patent Information
- Application Number
- JP2023086642
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
AI Technical Summary
Existing diapers with stretchable parts around the legs and torso have high expansion stress in areas without elastic members, leading to poor fit and discomfort during movements, especially when bending or standing up, due to uneven body shape and stiffness.
A diaper design utilizing a backsheet composed of nonwoven fabric with crimped fibers and elastomers, where different areas around the torso and legs have varying stretchability and thickness change rates, ensuring a comfortable fit and motion tracking by controlling elongation characteristics.
The diaper provides excellent surface touch, fit, and motion followability by using crimped fibers and elastomers with controlled stretchability, reducing discomfort during movements and maintaining a snug fit.
Smart Images

Figure 2024169844000004 
Figure 2024169844000005 
Figure 2024169844000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a diaper and a method for making a diaper. [Background technology]
[0002] In disposable diapers, the waist and leg sections have a stretchable structure, which plays a role in preventing leakage of excrement and slippage of the diaper. Generally, these stretchable sections are made of a nonwoven material in which stretched elastic threads are attached to the nonwoven material, and the elastic threads return to their original length, forming pleated gathers in the nonwoven material. However, in order to prevent leakage of excrement, the gathered nonwoven fabric needs to be compressed when worn, which means that the elastic threads have to be tightly tightened around the body, and the high thickness of the gathers results in low flexibility.
[0003] In recent years, there has been an increasing demand for improved comfort in sanitary materials such as disposable diapers, and in light of the above-mentioned issues, improvements in materials for stretchable parts have been actively studied. In addition to basic properties such as stretchability and good breathability, materials that are thin and highly flexible are required for stretchable parts so that the material can fit the uneven shape of the body. In addition, since the feel also affects comfort, the material that comes into contact with the skin in the stretchable parts is required to have an excellent surface touch.
[0004] Another important aspect of the design is to ensure that the diaper does not feel tight when the wearer moves. It is known that the wearer's skin deforms significantly in both the front and back of the body, especially when bending over or standing up, so the comfort of wearing the diaper can be optimized by controlling the stretch characteristics in the front and back direction of the body at each part of the diaper.
[0005] In response to this, Patent Document 1 proposes a pants-type disposable wearing article in which elastic members and a stretchable outer sheet are bonded together around the legs and torso so that the shrinkage dimensions of the elastic members in the leg direction after the stretching of the elastic members is released are adjusted to be approximately the same, thereby making the material stretchable but essentially flat without undulating in the thickness direction. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-148607 A Summary of the Invention [Problem to be solved by the invention]
[0007] In the technology of Patent Document 1, the leg and torso circumferences are stretchable without gathers, so the fitting is excellent in the relevant areas, but the stretching stress is high in the areas without elastic members, so it is difficult to fit the unevenness of the body. Furthermore, when making large movements such as bending or standing up, the movement tracking is poor, and the material is tight, reducing wearing comfort.
[0008] Therefore, the object of the present invention has been made in consideration of the above circumstances, and is to provide a diaper having excellent wearing comfort, in which the back sheet in the diaper has good elasticity and flexibility, has an excellent surface touch, and has movement tracking ability, and to provide a method for manufacturing the same. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to achieve the above object. As a result, they have discovered that by using a thin and stretchable nonwoven fabric having a specific structure for the back sheet of a diaper and further designing the back sheet so that different parts have different stretch characteristics, it is possible to obtain a diaper that is comfortable to wear and can achieve both good fit, surface touch, and motion tracking. The present invention has been completed based on these findings.
[0010] The present invention and its preferred embodiments comprise the following: [1] A diaper comprising a top sheet, an absorbent body, and a back sheet, the back sheet being composed of a waist section and a leg section, at least one of the waist section and the leg section being (1) At least 30% of the surface area is made of nonwoven fabric that is made of crimped fibers and has an elastomer; and (2) The thickness change rate at 30% elongation is 20.0% or less compared to the thickness at no load. a diaper in which if only one of the waist and leg portions satisfies the above (1) and (2), then that part is called part A, and the other part is called part B; and if both the waist and leg portions satisfy the above (1) and (2), then the part which has a lower elongation load when the diaper is elongated 50% in the vertical direction is called part A, and the other part is called part B, and the elongation load when the diaper is elongated 50% in the vertical direction is 0.90 or less times the elongation load when the diaper is elongated 50% in the vertical direction. [2] The part B is The nonwoven fabric is made of crimped fibers and has an elastomer in an area ratio of 30% or more, and The thickness change rate when elongated by 30% is 20.0% or less compared to the thickness when no load is applied The diaper according to the above [1] satisfies the above. [3] A method for producing the diaper according to [1] or [2] above, The method for producing the diaper includes the steps of: a back sheet manufacturing process for manufacturing a back sheet; a lamination step of laminating an absorbent body and a top sheet on the back sheet; Including, The back sheet manufacturing process includes: a fabric-making process in which the crimp-producing composite fibers are collected on a collecting belt to form a spunbonded nonwoven fabric layer, and at least one elastomer layer is laminated thereon and then integrated to obtain a laminated nonwoven fabric; A stretching process in which at least a part of the laminated nonwoven fabric obtained in the fabric-making process is stretched in at least one direction by a geared roller; a bonding step of bonding the stretched laminated nonwoven fabric as the part A sheet so that a portion of the part A sheet and a portion of the part B sheet overlap each other; Including, A method for manufacturing diapers. [4] A method for producing a diaper as described in [3] above, wherein the stretched laminated nonwoven fabric is used as a sheet for the waist area so that the stretching direction in the stretching step is the left-right direction of the diaper. [5] A method for producing a diaper as described in [3] above, wherein the stretched laminated nonwoven fabric is used as a sheet for the leg surrounding portions so that the stretching direction in the stretching step is the vertical direction of the diaper. [6] A method for producing a diaper as described in [5] above, wherein the stretched laminated nonwoven fabric is used as a sheet for the leg surrounding portions so that the stretching direction in the stretching step is the vertical direction of the diaper. Effect of the Invention
[0011] According to the present invention, a diaper having an excellent surface touch, excellent fitting property and excellent movement followability can be obtained. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a perspective view of a pants-type diaper, which is an example of the diaper of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the crotch portion (XX' portion) of FIG. [Diagram 3] FIG. 3 is a schematic view showing the back sheet of the diaper of the present invention when developed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The diaper of the present invention comprises a top sheet, an absorbent body, and a back sheet. The components are described in detail below, but the present invention is not limited to the embodiments described below without departing from the gist of the present invention.
[0014] [Top sheet] The top sheet is preferably a nonwoven fabric from the viewpoint of liquid permeability and surface touch. The form of the nonwoven fabric can be selected from known nonwoven fabrics such as spunbond nonwoven fabrics, meltblown nonwoven fabrics, and staple fiber nonwoven fabrics. Among them, spunbond nonwoven fabrics are preferable from the viewpoint of liquid permeability and flexibility. Furthermore, staple fiber nonwoven fabrics are preferable from the viewpoint of cushioning.
[0015] [Absorbent] From the viewpoint of absorption speed and absorption capacity, the absorbent body preferably has a structure in which pulp and / or absorbent polymer is wrapped in a sheet, and the sheet is preferably a hydrophilized nonwoven fabric or paper.
[0016] [Back seat] The backsheet is composed of a waistline part and a leg-around part. In Fig. 1, when the upper ends of leg openings 1-2A and 1-2B are designated as Y and Y', respectively, and the backsheet is divided into two or more parts by a line segment connecting Y-Y' in front of the wearer and a line segment connecting Y-Y' behind the wearer, the leg-around part is a part that is surrounded by the two line segments Y-Y' and the contour of the backsheet and includes a line segment X-X'.
[0017] The waist portion refers to the entire area of the back sheet other than the leg portions.
[0018] The waist portion is further divided into a ventral waist portion, which is the part on the wearer's ventral side, and a dorsal waist portion, which is the part on the wearer's back side.
[0019] At least one of the waist portion and the leg portion is (1) The nonwoven fabric is made of crimped fibers and has an elastomer in an area ratio of 30% or more, and (2) The thickness change rate at 30% elongation is 20.0% or less compared to the thickness at no load. Satisfy.
[0020] Regarding the waist portion, if at least one of the ventral waist portion or the rear waist portion satisfies the above condition, the waist portion satisfies the above condition. If one part of the ventral waist portion or the rear waist portion satisfies the condition, the area ratio is the area ratio relative to the area of the part that satisfies the condition.
[0021] When only one of the waist and leg portions satisfies the above conditions, that part is called Part A and the other is called Part B. When both the waist and leg portions satisfy the above conditions (1) and (2), the part which has a lower elongation load when the diaper is elongated by 50% in the vertical direction (hereinafter also referred to as "vertical elongation load") is called Part A and the other is called Part B.
[0022] If one of the ventral waist part or the posterior waist part satisfies the above conditions and the leg parts do not, the part of the waist part that satisfies the conditions is designated as part A, and the leg parts are designated as part B.
[0023] In addition, if one of the parts of the ventral waist portion or the posterior waist portion satisfies the above conditions and the leg portions also satisfy the conditions, the vertical elongation load is compared between the part of the waist portion that satisfies the conditions and the leg portions to determine part A and part B.
[0024] Furthermore, when the ventral waist portion, the rear waist portion, and the leg portions all satisfy the above conditions, the vertical extension loads are compared among these three parts. If the vertical extension load of the leg portion is the lowest, the leg portion is designated as part A, and the part with the higher extension load, either the ventral waist portion or the rear waist portion, is designated as part B. If the vertical extension load of either the ventral waist portion or the rear waist portion is the lowest, the part is designated as part A, and the leg portion is designated as part B.
[0025] In addition, if both the ventral waist portion and the posterior waist portion do not satisfy the above condition but exhibit different vertical elongation loads, and the leg portions satisfy the above condition, the part of the waist portion having the higher elongation load is designated as part B.
[0026] The crimped fiber is a fiber having a certain degree of crimping. By using the crimped fiber, the size of the gaps formed by the fibers in the nonwoven fabric can be increased, and the touch of the surface of the nonwoven fabric can be improved according to the number of crimps.
[0027] From the viewpoint of productivity, the crimped fibers are preferably fibers made of a thermoplastic resin.
[0028] Examples of the thermoplastic resin include: Aromatic polyester polymers and copolymers thereof, such as polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, and polyhexamethylene terephthalate; Aliphatic polyester polymers and copolymers thereof, such as polylactic acid, polyethylene succinate, polybutylene succinate, polybutylene succinate adipate, polyhydroxybutyrate-polyhydroxyvalerate copolymers, and polycaprolactone; Aliphatic polyamide polymers such as polyamide 6, polyamide 66, polyamide 610, polyamide 10, polyamide 12, polyamide 6-12, and copolymers thereof; Polyolefin polymers such as polypropylene, polyethylene, polybutene, polymethylpentene, and copolymers thereof; Examples of the polymer include water-insoluble ethylene-vinyl alcohol copolymer-based polymers containing 25 mol % to 70 mol % of ethylene units, polystyrene-based, polydiene-based, chlorine-based, polyolefin-based, polyester-based, polyurethane-based, polyamide-based, and fluorine-based elastomer polymers, and any of these can be selected and used.
[0029] In particular, the thermoplastic resins not belonging to the last group of elastomer polymers, i.e., the aromatic polyester polymers and their copolymers, the aliphatic polyester polymers and their copolymers, the aliphatic polyamide polymers and their copolymers, the polyolefin polymers and their copolymers, and the ethylene-vinyl alcohol copolymer polymers, are preferred because they have a rubber-like feel (rubber touch) and are unlikely to deform easily and have recovery power. Among them, since olefin-based nonwoven fabrics are often used for materials other than the backsheet of diapers, it is more preferable to use olefin-based thermoplastic resins for the crimped fibers from the viewpoint of adhesion.
[0030] The thermoplastic resins may be used alone or in combination of two or more.
[0031] For the purpose of improving the surface feel of the backsheet, it is preferable that at least a portion of the crimped fibers contains a fatty acid amide compound.
[0032] Examples of the fatty acid amide compound include saturated fatty acid monoamide compounds, saturated fatty acid diamide compounds, unsaturated fatty acid monoamide compounds, and unsaturated fatty acid diamide compounds. The carbon number in the present invention means the number of carbon atoms contained in the molecule. Specific examples of the fatty acid amide compound include palmitic acid amide, palmitoleic acid amide, stearic acid amide, oleic acid amide, elaidic acid amide, vaccenic acid amide, linoleic acid amide, linolenic acid amide, pinolenic acid amide, eleostearic acid amide, stearidonic acid amide, bosseopentaenoic acid amide, arachidic acid amide, gadoleic acid amide, eicosenoic acid amide, eicosadienoic acid amide, mead acid amide, eicosatrienoic acid amide, arachidonic acid amide, eicosatetraenoic acid amide, eicosapentaenoic acid amide, henicosyl acid amide, behenic acid amide, erucic acid amide, docosadienoic acid amide, adrenic acid amide, osbondoic acid amide, sardine acid amide, docosahexaenoic ... amide, lignoceric acid amide, nervonic acid amide, tetracosapentaenoic acid amide, nisinic acid amide, cerotic acid amide, montanic acid amide, melissic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, methylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, ethylene biserucic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, distearyl adipic acid amide, distearyl sebacic acid amide, and hexamethylene bisoleic acid amide. Also, a combination of a plurality of these can be used.
[0033] By setting the carbon number of the fatty acid amide compound to preferably 15 or more, more preferably 23 or more, and even more preferably 30 or more, it is possible to suppress excessive precipitation of the fatty acid amide compound on the fiber surface, and to achieve excellent spinnability and processing stability and high productivity. In addition, by setting the carbon number of the fatty acid amide compound to preferably 50 or less, more preferably 45 or less, and even more preferably 42 or less, the fatty acid amide compound is appropriately precipitated on the fiber surface, resulting in a laminated nonwoven fabric with excellent touch.
[0034] The content of the fatty acid amide compound in the crimped fiber is preferably 0.5% by mass or more, more preferably 0.7% by mass or more, and even more preferably 1.0% by mass or more, so that the fatty acid amide compound acts as a lubricant on the fiber surface, and the backsheet can have an excellent feel. From the viewpoint of cost and productivity, the content of the fatty acid amide compound is preferably 5.0% by mass or less.
[0035] The crimped fibers may also contain various additives, such as inorganic substances such as titanium oxide, silica, and barium oxide, colorants such as carbon black, dyes, and pigments, flame retardants, fluorescent whitening agents, antioxidants, and ultraviolet absorbing agents.
[0036] Examples of the crimped fibers include conjugate fibers such as side-by-side conjugate fibers and eccentric core-sheath conjugate fibers, and single-component crimped fibers having a modified cross section. Among these, conjugate fibers that allow easy control of the number of crimps are preferred.
[0037] The feel of the backsheet can be designed according to the crimp number of the crimped fiber, with a larger crimp number indicating finer crimping of the crimped fiber.
[0038] For example, when the back sheet is to have excellent bending flexibility, the number of crimps of the crimped fiber is preferably 50 pieces / 25 mm or more and 1000 pieces / 25 mm or less. By making the number of crimps of the crimped fiber 50 pieces / 25 mm or more, more preferably 85 pieces / 25 mm or more, and even more preferably 100 pieces / 25 mm or more, the extensibility of the crimped fiber is improved, and the fiber is not tensed when the nonwoven fabric is bent, so that the bending flexibility of the back sheet can be improved. In addition, by making the number of crimps of the crimped fiber 1000 pieces / 25 mm or less, more preferably 500 pieces / 25 mm or less, the size of the gap between the fibers is not too small, and a suitable surface touch can be obtained.
[0039] On the other hand, if the back sheet is to have excellent cushioning properties, the number of crimps of the crimped fibers is preferably 10 pieces / 25 mm or more and 50 pieces / 25 mm or less. By setting the number of crimps to 10 pieces / 25 mm or more and 50 pieces / 25 mm or less, more preferably 20 pieces / 25 mm or more and 45 pieces / 25 mm or less, the gaps between the fibers can be made large, and cushioning properties can be improved.
[0040] The crimp number can be determined as follows. An image of the surface of the backsheet is taken with a scanning electron microscope (SEM) at a magnification where 10 or more crimped fibers can be observed. The image is used to measure the apparent length of the crimped fibers in the measurement area. The number of peaks and valleys of the crimped fibers present within the apparent length is counted, and the total number of peaks and valleys is divided by 2. The total number is converted to the number per 25 mm. The same operation is performed on 20 different fibers, and the simple number average is calculated, and the value rounded off to the nearest tenth is the crimp number referred to in the present invention.
[0041] In the present invention, the elastomer refers to a polymer compound having a hard segment and a soft segment at room temperature. One of the characteristics of the elastomer is that it can be deformed by a small force.
[0042] By using the elastomer in the nonwoven fabric of the backsheet, the backsheet exhibits elasticity and can suitably fit the unevenness of the wearer's body. Furthermore, by making the backsheet from the nonwoven fabric containing the crimped fiber and the elastomer, both the fit and the surface touch can be achieved.
[0043] From the viewpoint of productivity, the elastomer is preferably a thermoplastic resin. When the elastomer is a thermoplastic resin, the surface morphology can be easily controlled. The thermoplastic resin that is the elastomer exhibits thermoplastic properties when heated to a melting point or higher, but can be deformed by a weak force at room temperature.
[0044] Examples of the thermoplastic resin that is the elastomer include polyurethane-based elastomers, polypropylene-based elastomers, polyethylene-based elastomers, polyester-based elastomers, polystyrene-based elastomers, and polybutadiene-based elastomers. The thermoplastic resin that is the elastomer may be used alone or in combination. For the nonwoven fabric of the diaper backsheet of the present invention, any of these may be appropriately selected and used in consideration of the adhesiveness with the crimped fibers.
[0045] The elastomer preferably has a stress of 50 MPa or less when tensile at 100% tension, the stress being measured based on JIS K7311:1995 "Testing methods for polyurethane thermoplastic elastomers".
[0046] The elastomer may be in the form of a fiber or a film, of which the fiber form is preferred from the viewpoint of providing suitable breathability and flexibility for a back sheet of a diaper.
[0047] In the backsheet, the mass ratio of the crimped fiber to the elastomer (crimped fiber: elastomer) is preferably 10: 90 to 90: 10. By setting the mass ratio of the crimped fiber to the elastomer in this range, it is possible to achieve both surface touch and stretchability.
[0048] The backsheet is preferably a composite nonwoven fabric in which the spunbond nonwoven fabric layer made of the crimped fibers and the elastomer layer are integrated together, where "integration" means that these layers are bonded together by entangling the fibers, fixing with an adhesive or other component, or fusing the thermoplastic resins that make up each layer together.
[0049] It is preferable that the mass ratio of the crimped fibers is higher than that of the elastomer on at least one surface of the backsheet. This can suppress the surface exposure of the rubber-touch elastomer, improving the surface touch. This embodiment can also be obtained by a composite nonwoven fabric in which a nonwoven fabric layer made of the crimped fibers and a layer made of the elastomer are laminated and integrated.
[0050] The form of the composite nonwoven fabric can be selected from known nonwoven fabrics such as spunbond nonwoven fabrics, meltblown nonwoven fabrics, staple fiber nonwoven fabrics, etc. From the viewpoint of productivity, preferred embodiments include a spunbond nonwoven fabric made of the crimped fibers integrated with a spunbond nonwoven fabric made of the elastomeric fibers, and a spunbond nonwoven fabric made of the crimped fibers integrated with a meltblown nonwoven fabric made of the elastomeric fibers.
[0051] The lamination structure of the laminated nonwoven fabric may be, for example, (S) / (E) for a two-layer structure, (S) / (E) / (S) for a three-layer structure, (S) / (E) / (E) / (S) for a four-layer structure, and (S) / (E) / (E) / (S) / (S) / (S) for a five-layer structure. Among these, a structure in which spunbonded nonwoven fabric layers are laminated on both sides of an elastomer layer, i.e., (S) / (E) / (S) or (S) / (E) / (S) / (E) / (S), is more preferable. This lamination structure may be selected depending on the purpose of use.
[0052] As a means for integrating the laminated nonwoven fabrics, for example, thermal bonding or ultrasonic bonding is preferable.
[0053] At least one of the waist and leg portions satisfies the requirement that an area ratio of 30% or more of the nonwoven fabric is made up of the nonwoven fabric (also referred to as "condition (1)"). The crimped fibers in the nonwoven fabric are structurally stretchable, and the stretching of the nonwoven fabric is not easily hindered when the nonwoven fabric is stretched, so that it is possible to achieve both low elongation load and surface touch characteristic of elastomers. By setting the area ratio to 30% or more, preferably 40% or more, and more preferably 50% or more, the surface touch and fit of the nonwoven fabric can provide a suitable wearing comfort for the diaper.
[0054] It is also preferable that part B is composed of a nonwoven fabric having an elastomer and an area ratio of 30% or more of the crimped fibers. Part B, which is a part of the backsheet that has a relatively high elongation load in the vertical direction of the diaper and fits the body, should have an area ratio of 30% or more, preferably 40% or more, and more preferably 50% or more, so that the good surface touch of the crimped fibers and the flexibility of the elastomer can improve wearing comfort.
[0055] At least one of the waist and leg portions satisfies the requirement that the thickness change rate at 30% elongation is 20.0% or less relative to the thickness at no load (also referred to as "condition (2)"). Since the waist and leg portions of the diaper stretch when the wearer moves, a thickness change rate of 20.0% or less, preferably 18.0% or less, and more preferably 15.0% or less will prevent the diaper from shifting from the wearer's body even when the wearer moves, providing an excellent fit. On the other hand, a thickness change rate of 1.0% or more is preferable in order to prevent the diaper from becoming tight when the wearer moves.
[0056] The rate of change in thickness when elongated by 30% relative to the thickness when no load is applied is determined as follows. (1) Separate the backsheet from the diaper. (2) Take a square test piece measuring 50 mm in both the vertical and horizontal directions of the diaper from any location on the backsheet. (3) For the test pieces taken, measure the thickness to two decimal places in mm based on Method A of JIS L1913:2010 "General nonwoven fabric test methods", 6.1 "Thickness (ISO method)", to determine the unstretched thickness (T0). (4) Fix the test piece in a state where it is stretched 30%. The direction in which the test piece is stretched is the vertical direction of the diaper or the horizontal direction of the diaper, whichever direction gives the lower stress at 30% stretch. The stress at 30% stretch here is the value calculated to two decimal places in units of N / 25mm by stretching the test piece and obtaining a tensile strength-elongation graph based on 6.3 of JIS L1913:2010 "General nonwoven fabric test method". Using a test piece taken from the backsheet separately from the thickness measurement, the 30% stretch is measured in the vertical and horizontal directions of the diaper, and the direction with the lower value is defined as the stretched direction. (5) With respect to the test piece fixed in a 30% elongated state, measure the thickness at 30% elongation (T30) in mm to two decimal places based on Method A of JIS L1913:2010 "General nonwoven fabric test methods", 6.1 "Thickness (ISO method)". (6) Using these values, calculate the rate of change in thickness (ΔT) when stretched 30% relative to the unstretched thickness using Equation 1. ΔT=100×(T0-T30) / T0...Equation 1 (7) Repeat steps (1) to (6) for 10 different test pieces, calculate the simple average of the results, and round off to the first decimal place. This value is the thickness change rate at 30% elongation.
[0057] In the diaper of the present invention, the vertical extension load of the waist and leg portions of the backsheet is suitably controlled. Specifically, when one of the waist and leg portions is called part A and the other is called part B, provided that the above-mentioned conditions (1) and (2) are satisfied, the vertical extension load F50A of part A is 0.90 times or less the vertical extension load F50B of part B. In other words, the ratio F50A / F50B between the two is 0.90 or less.
[0058] The smaller F50A / F50B indicates that part A is made of a material that easily stretches in the vertical direction of the diaper. It is known that the skin of the lower abdomen / buttocks, which are the parts where the diaper is worn, stretches significantly in the vertical direction of the body when the wearer makes a large movement such as bending over. By disposing part A, which has a relatively low vertical extension load, in the back sheet of the diaper and setting F50A / F50B to 0.90 or less, preferably 0.85 or less, and more preferably 0.80 or less, the diaper can follow the movement without being stretched. In addition, the vertical extension load of part B is relatively high, so that the diaper can be prevented from shifting due to movement. On the other hand, by setting F50A / F50B to preferably 0.01 or more, more preferably 0.05 or more, the decrease in strength can be suppressed.
[0059] The vertical extension load and F50A / F50B are calculated as follows. (1) Separate the backsheet from the diaper. (2) Take a rectangular test piece measuring 40 mm in the vertical direction and 25 mm in the horizontal direction from any point around the waist of the backsheet. (3) Based on JIS L1913:2010 "General nonwoven fabric testing method" 6.3, the collected test specimen is stretched in the vertical direction of the diaper to obtain a tensile strength-elongation graph. (4) Using the graph created in (3), calculate the elongation load at 50% elongation, in units of N / 25 mm, to two decimal places. (5) Repeat steps (1) to (4) for 10 different test pieces. Calculate the simple average of the results and round off to one decimal place. This value is the vertical extension load. (6) For the leg-around portion of the back seat, calculate the vertical extension load using steps (1) to (5). (7) If the part with a relatively low vertical extension load is part A and the part with a relatively high vertical extension load is part B, calculate the ratio of their respective vertical extension loads (F50A, F50B), F50A / F50B, and round off to the third decimal place.
[0060] The nonwoven fabric constituting part A preferably has a stretch recovery rate of 80% or more when stretched 100% in at least one direction.
[0061] By setting the elongation recovery rate to 80% or more, and more preferably 90% or more, the material of part A has a suitable contractile force, and the fit of the portion of the diaper covered by part A can be suitably controlled.
[0062] The elongation recovery rate at 100% elongation is determined as follows. (1) Cut out a sample from any part in the top-to-bottom and left-to-right directions of the diaper. Based on JIS L1913:2010 "General nonwoven fabric test methods", stretch the test piece and determine the direction with the lowest 50% elongation load as the tensile direction. (2) A test piece is cut out from any point of the part in the tensile direction determined in (1). (3) Measure the elongation recovery rate as measured by 8.16.2 Method A of JIS L1096:2010 "Testing methods for woven and knitted fabrics."
[0063] As long as the effect of the diaper of the present invention is not adversely affected, an elastic material may be attached to the part A and the part B. By doing so, the stretchability can be further improved.
[0064] [Diaper composition] The diaper of the present invention will be described with reference to Figures 1 and 2. Figure 1 is a perspective view of a pants-type diaper which is an example of the diaper of the present invention, and Figure 2 is a cross-sectional view of the crotch portion (X-X' portion) of Figure 1.
[0065] 1, the diaper of the present invention has an opening 1-1 around the waist and openings 1-2A and 1-2B around the legs. The edge of the opening around the waist in the diaper of the present invention is referred to as the upper end of the diaper.
[0066] In the present invention, when the lower ends of the leg openings 1-2A and 1-2B are designated as X and X', respectively, the direction of the line segment connecting X-X' is referred to as the left-right direction of the diaper, and the direction perpendicular to this is referred to as the up-down direction of the diaper.
[0067] FIG. 2 is a cross-sectional view of the diaper of the present invention taken along the line XX', with the upper side of the figure being the wearer side.
[0068] The top sheet 2-1 is disposed closest to the wearer when the diaper is worn. The top sheet 2-1 may cover the entire area of the diaper that comes into contact with the wearer's skin, or may cover only a part of it.
[0069] The absorbent body 2-2 is disposed in the crotch area when the diaper is worn, and has a structure in which an absorbent material is wrapped in a sheet. The absorbent body is preferably disposed between the top sheet 2-1 and the back sheet 2-4 described below.
[0070] The back sheet 2-4 is disposed on the outer side farthest from the wearer when the diaper is worn. The back sheet 2-4 can be separated independently by heating. When an elastic material is attached to the back sheet 2-4, the sheet in the attached state is defined as the back sheet.
[0071] The term "elastic material" here refers to a material that has elasticity. In the case of sheet-like materials, this means that the elongation recovery rate measured in at least one direction according to 8.16.2 A method of JIS L1096:2010 "Testing methods for woven and knitted fabrics" is 80% or more. In the case of fibrous materials, this means that the elongation elasticity measured in accordance with 8.9 B method of JIS L1013:2021 "Testing methods for chemical fiber filament yarns" is 80% or more.
[0072] In a structure in which an elastic material is bonded, the back sheet 2-4 has a high thickness change rate at 30% elongation, as described later, and therefore, from the viewpoint of fit, it is preferable to use a structure in which no elastic material is bonded.
[0073] The diaper of the present invention may further include a liquid-impermeable sheet 2-3 from the viewpoint of preventing the liquid absorbed by the absorbent body 2-2 from leaking out to the outside. In this case, the liquid-impermeable sheet 2-3 is preferably disposed between the absorbent body 2-2 and the back sheet 2-4.
[0074] Furthermore, the diaper of the present invention may have side gathers 2-5 for the purpose of preventing leakage of urine or feces by the wearer. The side gathers 2-5 of the diaper of the present invention are sheets that are arranged so as to overlap part of the top sheet 2-1 and can rise up three-dimensionally relative to the top sheet when the diaper is worn.
[0075] In the case of the diaper of the present invention being of the tape type, it is necessary to connect the waist part of the diaper to the abdominal part of the wearer, so that it is preferable to attach ear parts to the upper end part of the diaper. In the diaper of the present invention, the ear parts include the engagement parts for connecting the waist part and the abdominal part.
[0076] It is also preferable that the garment includes a sheet for engaging with the engaging portion when worn.
[0077] [Diaper manufacturing method] The method for producing a diaper of the present invention comprises a backsheet production step of producing a backsheet, and a lamination step of laminating an absorbent body and a top sheet onto the backsheet. The backsheet production step comprises a fabric-making step of collecting crimp-producing composite fibers on a collecting belt to form a spunbond nonwoven fabric layer, laminating at least one elastomer layer thereon and integrating the layers to obtain a laminated nonwoven fabric, a stretching step of stretching at least a portion of the laminated nonwoven fabric obtained in the fabric-making step in at least one direction with a geared roller, and a lamination step of laminating the stretched laminated nonwoven fabric as the part A sheet so that a portion of the part A sheet and a portion of the part B sheet overlap each other.
[0078] [Backsheet manufacturing process] (cloth making process) In the fabric-making process, the crimp-producing conjugate fibers are collected on a collecting belt to form a spunbond nonwoven fabric layer, and at least one elastomer layer is laminated thereon and then integrated to obtain a laminated nonwoven fabric.
[0079] In order to obtain the crimp-producing composite fiber, it is preferable to separately melt a plurality of polymer raw materials having different melt viscosities and / or polymer types and extrude them from the spinneret as a composite polymer stream. By making the melt viscosities and / or polymer types of the polymer raw materials of the crimp-producing composite fiber different, the fiber can exhibit crimp due to the difference in elastic modulus between the polymer raw materials.
[0080] Since the number of crimps of the crimp-expressing conjugate fiber affects the surface touch of the diaper, it is preferable to appropriately select the polymer raw material and melt viscosity so as to obtain the number of crimps necessary to obtain the desired surface touch.
[0081] In order to increase the number of crimps in the crimp-producing conjugate fiber and improve bending flexibility, it is preferable to provide a difference in melt viscosity between the polymer raw materials. In this case, it is preferable that the ratio of the melt viscosity of the polymer raw material with the highest melt viscosity to the polymer raw material with the lowest melt viscosity among the polymer raw materials constituting the crimp-producing conjugate fiber is 1.20 or more.
[0082] By setting the melt viscosity ratio to 1.20 or more, more preferably 1.30 or more, the difference in elastic modulus between the polymer raw materials can be increased, and the number of crimps can be improved. On the other hand, by setting the melt viscosity ratio to preferably 8.00 or less, it is possible to prevent the composite polymer flow discharged from the spinneret from bending significantly, which makes it impossible to spin the fibers.
[0083] The melt viscosity in this invention is the shear rate of 31.4 s at the spinning temperature. -1 This refers to the melt viscosity at 100° C. and is measured by the method described below. (1) Using a rotational rheometer (for example, "Rheosol-G3000" manufactured by UBM), the temperature is raised to a temperature equivalent to the spinning temperature. (2) A polymer is sandwiched between parallel plates of φ20 mm, and after melting, the gap between the plates is set to 0.5 mm. (3) 31.4rad / s -1 The strain is applied at a rate such that (4) Measure the melt viscosity under the above conditions (unit: Pa s).
[0084] A spinneret for suitably obtaining the crimp-expressing conjugate fiber is preferably equipped with a mechanism capable of forming a side-by-side type conjugate cross section or an eccentric core-sheath type conjugate cross section. In this case, the shape of the nozzle hole of the spinneret may be freely selected as long as it does not impair the effects of the present invention, but from the viewpoint of spinning stability, a round hole is preferable.
[0085] The spunbond method is a method for producing a nonwoven fabric in which a thermoplastic resin as a raw material is melted, spun from a spinneret, cooled and solidified to obtain a filament, which is then pulled and stretched by an air pulling unit such as an ejector, collected on a moving collection belt to form a nonwoven fiber web, and then thermally bonded. By producing a nonwoven fabric layer made of the crimp-expressing composite fiber by the spunbond method, molecular orientation is promoted by air pulling, and the fibers are firmly fixed to each other by thermal bonding, so that sufficient strength can be obtained.
[0086] In order to increase the number of crimps in the crimp-producing composite fiber, the crimp-producing composite fiber may be subjected to a heat treatment after being collected on a collecting belt. The heat treatment is preferably performed before laminating and integrating with the elastomer layer. The heat treatment temperature is preferably set to a temperature of Tm-100°C or higher, where Tm is the lowest melting point of the polymer raw materials constituting the crimp-producing composite fiber, as measured by differential scanning calorimetry (DSC) according to JIS K7121:1987 "Method for measuring transition temperature of plastics".
[0087] The step of laminating the elastomer layer may be, for example, a method of continuously collecting an elastomer layer in-line on the spunbonded nonwoven fabric layer formed on the collecting belt as described above by a conventional method including a known method, and integrating the layers by heating and pressing, or a method of laminating a spunbonded nonwoven fabric layer and an elastomer layer obtained separately offline, and integrating the layers by heating and pressing, etc. Among these, a method of continuously collecting an elastomer layer in-line on the spunbonded nonwoven fabric layer formed on the collecting belt, and integrating the layers by heating and pressing is preferred because of its excellent productivity. Examples of the integration method include a method of entangling the fibers by a method such as needle punching, and a method of bonding the fibers using an adhesive, etc.
[0088] In one preferred embodiment of the method for producing the elastomer layer of the diaper of the present invention, the elastomer layer is formed by a spunbonding method, which is preferred because it allows a laminated nonwoven fabric having high strength to be obtained.
[0089] Another preferred embodiment of the method for producing the elastomer layer of the diaper of the present invention is to form the elastomer layer by a melt-blowing method. The melt-blowing method allows for more stable sheet formation than the spunbonding method. Another advantage is that the fiber diameter can be made smaller than in the spunbonding method, which further improves bending flexibility.
[0090] In addition, the method for producing the elastomer layer of the diaper of the present invention only requires that the above-mentioned spunbonded nonwoven fabric layer and at least one elastomer layer are laminated, and the number and combination of layers can be any configuration depending on the purpose.
[0091] (Stretching process) In the stretching step, at least a part of the laminated nonwoven fabric obtained in the fabric-making step is stretched in at least one direction by a geared roller.
[0092] By subjecting the laminated nonwoven fabric to a stretching process, it is possible to improve the stretchability in the stretching direction, and the thickness change rate of the laminated nonwoven fabric at 30% elongation can be suitably controlled. Furthermore, the stretching process can loosen the tensed fibers in the nonwoven fabric, so that the stretchability in the direction perpendicular to the stretching direction can also be improved.
[0093] The geared roller in the present invention is a roller having at least a portion of its surface formed with projections and recesses. A preferred embodiment of the geared roller is a pair of rollers in which the recesses of one roller mesh with the projections of the other roller. When a nonwoven fabric is processed with a roller having such a configuration, the nonwoven fabric is stretched in a small section between adjacent recesses of one roller, and the laminated nonwoven fabric can be uniformly stretched.
[0094] The stretching ratio in the stretching step is preferably adjusted appropriately depending on the desired physical properties. The stretching ratio may be adjusted by the height of the concave and convex portions or by the distance between the rolls.
[0095] In the stretching step, the laminated nonwoven fabric may be stretched in either the machine direction (MD) or the cross direction (CD), depending on the properties of the diaper to be produced. Furthermore, the laminated nonwoven fabric may be stretched in both the machine direction (MD) and the cross direction (CD).
[0096] The method for producing the backsheet of the present invention may include a step of heat treating the stretched laminated nonwoven fabric for the purpose of suppressing tearing due to stretching and adjusting dimensional stability.
[0097] (Laminating process) In the bonding step, the stretched laminated nonwoven fabric is used as part A, and the parts A and B are bonded together such that a part of the part A overlaps a part of the part B.
[0098] As the bonding means in the bonding step, from the viewpoint of strength when made into a diaper, a bonding method using a hot melt adhesive, a bonding method by heat pressing, or a bonding method by ultrasonic waves is preferable.
[0099] In the lamination step, the part A sheet and the part B sheet may be cut into a suitable shape in advance and then laminated together, or a continuous part A sheet and part B sheet may be laminated together.
[0100] When part A is set as the sheet for the waist area, it is preferable to laminate the stretched laminated nonwoven fabric as part A to part B so that the stretching direction in the stretching step is the left-right direction of the diaper. By laminating part A in this manner, it is possible to lower the elongation load in the up-down direction of the diaper compared to part B, while increasing the stretchability in the left-right direction of the diaper required in the waist area of the wearer, thereby obtaining a suitable fit.
[0101] On the other hand, when part A is set as a sheet for the leg surrounding portions, it is preferable to bond the stretched laminated nonwoven fabric as part A to part B so that the stretching direction in the stretching step is the vertical direction of the diaper. Since the leg surrounding portions are areas that significantly elongate in the vertical direction due to the wearer's movements, bonding part A in the above-mentioned direction allows for a design that can suitably follow the wearer's movements.
[0102] Furthermore, when part A is set as the sheet for the leg-surrounding portions, it is preferable that the stretched laminated nonwoven fabric is used as part B of the backsheet so that the stretching direction in the stretching step is the left-right direction of the diaper. By bonding part B in the above-mentioned direction, it is possible to increase the stretchability in the left-right direction of the diaper, which is necessary for the leg-surrounding portions, as described above, and therefore obtain a suitable fit.
[0103] [Lamination process] In the lamination step, an absorbent body and a top sheet are laminated on the back sheet. A liquid-impermeable sheet, side gathers, etc. may also be placed on the back sheet.
[0104] In the lamination step, it is preferable to bond the respective constituent materials to each other. As a bonding method, from the viewpoint of adhesive strength, a method of bonding using a hot melt adhesive, a method of bonding by heat pressing, or a method of bonding by ultrasonic waves are preferable.
[0105] After the respective constituent materials are bonded together, they are cut into the shape of the product to produce the diaper of the present invention. EXAMPLES
[0106] The present invention will now be described in detail with reference to examples, although the present invention is not limited to these examples.
[0107] [Measurement method] The respective property values in the examples were determined by the following methods. Unless otherwise specified, the measurements were carried out according to the above-mentioned methods.
[0108] (1) Thickness change rate at 30% elongation Square test pieces measuring 50 mm in each of the vertical and horizontal directions of the diaper were taken from any location of the waist or leg areas of the backsheet, and the thickness change rate at 30% elongation was measured using the measurement procedure for "thickness change rate at 30% elongation relative to the thickness at no load" described above.
[0109] (2) Vertical tension load and F50A / F50B Rectangular test pieces measuring 40 mm in the vertical direction and 25 mm in the horizontal direction were taken from any point of the waist and leg areas of the backsheet, and the vertical extension loads of parts A and B that make up the backsheet were measured using the measurement procedure described above for "the ratio of the extension load when part A is stretched 50% in the vertical direction of the diaper to the extension load when part B is stretched 50% in the vertical direction of the diaper", and the ratio F50A / F50B was calculated.
[0110] (3) Diaper wearing test The diapers were worn by healthy adults (a total of 30 people, 15 men and 15 women), who conducted a wear test in which they walked up and down a 30cm high step 30 times. During the test, the following items were scored on a three-point scale, and the total score was used to evaluate the wearability. (a) Surface touch The surface touch of the diapers produced was evaluated for the parts that came into contact with the skin when worn. 5: The surface is smooth and cushioned. 3: The surface is smooth but not cushioned. 1: The surface has a rubber touch. (b) Diaper fit The diapers were evaluated for their fit to the body when the subject was not moving and when the subject was moving up and down a step. 5: The diaper fits the body well even when moving. 3: When there is no movement, the diaper fits the body well, but when moving, a space opens up between the diaper and the body. 1: Even when not moving, there is space between the diaper and the body, and it does not fit the body properly. (c) Motion tracking We evaluated whether the diaper material felt tight when ascending and descending steps. 5: The diaper conforms to the body and there is no tightness. 3: I feel tightness in some parts of the diaper. 1: I feel tightness in part of the diaper.
[0111] [Diaper parts and materials] (Top sheet) The top sheet is made of 2.2 dtex short fibers with a polyethylene core and a polyethylene terephthalate sheath, and has a basis weight of 20 g / m. 2 An air-through nonwoven fabric was used.
[0112] (Absorbent) The absorbent material is a mixture of particles of highly absorbent polymer made of polyacrylic acid and fluff pulp, with a basis weight of 20 g / m. 2 The specimens were wrapped in paper.
[0113] (Elastic thread) The elastic yarn used was a fiber made of polyurethane resin with a single fiber fineness of 7.0 dtex.
[0114] [Nonwoven fabric A] (cloth making process) (First crimped fiber web) The first component has a shear rate of 31.4 s -1 The melt viscosity of homopolypropylene (PP) at a shear rate of 153 Pa s was used as the second component. -1 A crimped fiber web was prepared by the spunbond method using ethylene copolymerized polypropylene (coPP) with 2.7 mol% ethylene copolymerized and a melt viscosity of 270 Pa·s at room temperature.
[0115] The first and second components were melted in separate extruders and extruded from a rectangular spinneret at a spinning temperature of 230°C to obtain fibers with a side-by-side composite cross section (referred to as SbS in Table 1) at a throughput of 0.55 g / (min·hole) per hole and a mass ratio of component 1:component 2 of 50:50.
[0116] The spun filaments are cooled and solidified, then pulled and stretched in a rectangular ejector by compressed air at a pressure of 0.10 MPa, collected on a moving collection belt, and spun to a basis weight of 10 g / m. 2 The fibers in the crimped fibrous web layer had crimps, and the number of crimps was 120 per 25 mm.
[0117] (Elastomer layer) An elastomer layer was formed by the spunbond method using a polypropylene-based elastomer (PP-based EL) copolymerized with 15 wt% ethylene, with a melt viscosity of 423 Pa·s and a flexural modulus of 13 MPa.
[0118] The above PP-based EL was melted in an extruder and spun from a rectangular die at a spinning temperature of 230°C with a throughput of 0.20 g / (min·hole).
[0119] The spun filaments were cooled and solidified, then pulled and stretched in a rectangular ejector by compressed air at a pressure of 0.10 MPa, and collected on a first crimped fiber web with a basis weight of 30 g / m 2 Thus, an elastomer layer of
[0120] (Second crimped fiber web) Further, on the above-mentioned elastomer layer, a second crimped fibrous web was collected in the same manner as the above-mentioned first crimped fibrous web.
[0121] (integration) The upper roll was a metal embossing roll with circular convex parts arranged in a staggered pattern at the same pitch in both MD and CD, and the lower roll was a metal flat roll with a pair of upper and lower heating mechanisms. The laminate of the first crimped fiber web / elastomer layer / second crimped fiber web was heated and pressed at a linear pressure of 300 N / cm and a surface temperature of the embossing roll of 100°C to be integrated, to obtain a laminated nonwoven fabric with a three-layer structure (the laminate structure is indicated as C / EL / C in Table 2).
[0122] (Stretching process) In the stretching process, a stretching device was used, which was a pair of rolls, each having a gear with a groove depth of 4 mm and a groove pitch of 3 mm, arranged above and below each other so that the convex part of one roll meshes with the concave part of the other roll. The laminated nonwoven fabric was stretched in the CD direction at a stretch ratio of 2.4 times by the stretching device, to obtain nonwoven fabric A.
[0123] [Nonwoven fabric B] (cloth making process) (First PP fiber web) Shear rate 31.4s -1 A PP fiber web was prepared by the spunbond method using homopolypropylene (PP) with a melt viscosity of 153 Pa·s at room temperature.
[0124] The above PP was melted in an extruder and extruded from a rectangular die at a spinning temperature of 230°C with a throughput of 0.55 g / (min·hole).
[0125] The spun filaments are cooled and solidified, then pulled and stretched in a rectangular ejector by compressed air at a pressure of 0.10 MPa, collected on a moving collection belt, and spun to a basis weight of 10 g / m. 2The fibers in the PP fiber web layer had no crimp.
[0126] (Elastomer layer) An elastomer layer was formed on the first PP fiber web in the same manner as in the case of nonwoven fabric A.
[0127] (Second PP fiber web) On the above elastomer layer, a second PP fiber web was further collected in the same manner as the above first PP fiber web.
[0128] (integration) The above-mentioned first PP fiber web / elastomer layer / second PP fiber web laminate was heated and pressed to be integrated in the same manner as for nonwoven fabric A, to obtain a laminated nonwoven fabric with a three-layer structure (the lamination structure is indicated as S / EL / S in Table 2).
[0129] (Stretching process) The laminated nonwoven fabric was stretched in the CD direction at a stretch ratio of 1.8 times using the same stretching equipment as used for nonwoven fabric A, to obtain nonwoven fabric B.
[0130] [Nonwoven fabric C] (cloth making process) (PP fiber web) Shear rate 31.4s -1 A PP fiber web was prepared by the spunbond method using homopolypropylene (PP) with a melt viscosity of 153 Pa·s at room temperature.
[0131] The above PP was melted in an extruder and extruded from a rectangular die at a spinning temperature of 230°C with a throughput of 0.55 g / (min·hole).
[0132] The spun filaments are cooled and solidified, then pulled and stretched in a rectangular ejector by compressed air at a pressure of 0.10 MPa, collected on a moving collection belt, and spun to a weight of 30 g / m. 2 Thus, a PP fiber web of
[0133] (heat and pressure) The above PP fiber web was heated and pressed in the same manner as for nonwoven fabric A, except that the surface temperature of the embossing roll was set to 130° C., to obtain nonwoven fabric C.
[0134] Nonwoven fabric C was not subjected to the stretching step.
[0135] [Nonwoven fabric D] (cloth making process) (Elastomer layer) The same polypropylene-based elastomer (PP-based EL) as that used for nonwoven fabric A was used to form an elastomer layer by the spunbond method.
[0136] The above PP-based EL was melted in an extruder, and extruded from a rectangular die at a spinning temperature of 230°C and a throughput of 0.55 g / (min·hole) per hole.
[0137] The spun filaments are cooled and solidified, then pulled and stretched in a rectangular ejector by compressed air at a pressure of 0.10 MPa, collected on a moving collection belt, and spun to a weight of 30 g / m. 2 Thus, an elastomeric fiber web of 100 g was obtained.
[0138] (heat and pressure) The above elastomer fiber web was heated and pressed in the same manner as in nonwoven fabric A, except that the surface temperature of the embossing roll was set to 80° C., to obtain nonwoven fabric D.
[0139] Nonwoven fabric D was not subjected to the stretching step.
[0140] [Nonwoven fabric E] (cloth making process) (Crimped fiber web) The same homopolypropylene (PP) and ethylene copolymer polypropylene (coPP) as those used in nonwoven fabric A were used as the first and second components, and the same procedure was followed as for the first crimped fiber web of nonwoven fabric A, except that the moving speed of the collection belt was changed. The basis weight was 30 g / m. 2 Thus, a crimped fiber web of 1000 g was obtained.
[0141] (heat and pressure) The above crimped fiber was heated and pressed in the same manner as for nonwoven fabric A, except that the surface temperature of the embossing roll was set to 120° C., to obtain a nonwoven fabric.
[0142] (Stretching process) The above nonwoven fabric was stretched in the same manner as for nonwoven fabric A to obtain nonwoven fabric E.
[0143] [Table 1]
[0144] The recovery rate at 50% elongation load and 100% elongation was measured for each nonwoven fabric, and the results are shown in Table 1.
[0145] Nonwoven fabrics A, B, and D had favorable elongation recovery rates, whereas nonwoven fabrics C and E had significantly low elongation recovery rates. This indicates that the performance of nonwoven fabrics A, B, and D is achieved by the presence of elastomeric fibers.
[0146] [Example 1] (Laminating process) Nonwoven fabric A was used for the waist portion (ventral waist portion, dorsal waist portion) and leg portion of the backsheet. The sheet was arranged so that the stretch direction in the waist portion was the left-right direction of the diaper, and the stretch direction in the leg portion was the top-bottom direction of the diaper.
[0147] The back sheet was attached in the following manner. The symbols given next to the terms correspond to those in FIG.
[0148] First, nonwoven fabric A was cut into a hexagonal shape for waist part 3-1 so that the stretch direction was the left-right direction of the diaper. In FIG. 3, the side of waist part 3-1 is the upper end side of the diaper. In part 3-1, the length of side 3-1b on the crotch side of the wearer is shorter than the length of side 3-1a.
[0149] Next, the sheet was cut into a rectangular shape to form leg-surrounding part 3-2, with the long side of said part 3-2 being in the up-down direction of the diaper.
[0150] The parts 3-1 and 3-2 cut as described above were stacked so that one short side of the part 3-2 was placed inside the part 3-1, and were bonded with a styrene-based hot melt adhesive. At this time, the area of the part 3-3 where the parts 3-1 and 3-2 overlap was set to 10% of the total area of the part 3-2.
[0151] Next, another part 3-1 was laminated in the same manner to the other short side of part 3-2 on the sheet bonded as described above, and bonded with a styrene-based hot melt adhesive to obtain a back sheet.
[0152] (Lamination process) An absorbent body and a top sheet were laminated in this order on the back sheet prepared in the above process, and each was adhered with a styrene-based hot melt adhesive.
[0153] After bonding, the lateral ends 3-4a of the backsheet in FIG. 3 and 3-4b of the backsheet in FIG. 3 were heat-sealed to each other to obtain a pants-type diaper.
[0154] [Example 2] (Laminating process) Nonwoven fabric A was used in the leg surroundings of the backsheet, and nonwoven fabric C was used in the waist surroundings of the backsheet (ventral waist surroundings and dorsal waist surroundings). In the leg surroundings, the sheet was arranged so that the stretching direction was the vertical direction of the diaper.
[0155] Other than that, the two parts 3-1 and 3-2 were bonded together in the same manner as in Example 1 to form a back sheet body.
[0156] Five elastic threads were attached to the waist area of the above-mentioned backsheet body using a hot melt agent at 3 mm intervals from a position 40 mm below the top end of the diaper in the left-right direction of the diaper while being stretched 100%, and the sheet up to 20 mm from the top end of the diaper was folded back onto the side with the elastic threads attached and attached using a hot melt agent to form a backsheet.
[0157] (Lamination process) Using the above backsheet, a diaper was obtained in the same manner as in Example 1. The waist area of the produced diaper had gathers formed by elastic yarn.
[0158] [Example 3] (Laminating process) Nonwoven fabric C was used in the leg surroundings of the backsheet, and nonwoven fabric A was used in the waist surroundings of the backsheet (ventral waist surroundings and dorsal waist surroundings). In the waist surroundings, the sheet was arranged so that the stretching direction was the left-right direction of the diaper.
[0159] Other than that, the two parts 3-1 and 3-2 were bonded together in the same manner as in Example 1 to form a back sheet body.
[0160] Two elastic threads were attached to the openings around the legs of the above-mentioned backsheet body using a hot melt agent at 3 mm intervals from a position 20 mm from the edge of the opening around the legs of the diaper, while being stretched 100%, along the opening edge.The sheet was then folded back to the side with the elastic threads attached and attached using a hot melt agent to form a backsheet.
[0161] (Lamination process) Using the above backsheet, a diaper was obtained in the same manner as in Example 1. The leg-opening portions of the produced diaper had gathers formed by elastic yarn.
[0162] [Comparative Example 1] (Laminating process) The diaper was produced by using two sheets for the ventral waist and rear waist of the backsheet, with nonwoven fabric A making up 10% of each of the left and right ends of the sheet and nonwoven fabric C making up the rest, and using nonwoven fabric C for the leg parts of the backsheet. The nonwoven fabric A used in the waist parts (ventral waist and rear waist) was positioned so that the stretch direction was the left and right direction of the diaper.
[0163] Other than that, the two parts 3-1 and 3-2 were bonded together in the same manner as in Example 1 to form a back sheet body.
[0164] Two elastic threads were attached to the opening around the legs of the above-mentioned backsheet body using a hot melt agent while being stretched 100% so as to run along the edge of the opening at 3 mm intervals from a position 20 mm from the edge of the opening around the legs of the diaper, and the sheet up to 10 mm from the edge of the opening was folded back onto the side with the elastic threads attached and attached using a hot melt agent to form a backsheet.
[0165] (Lamination process) Using the above backsheet, a diaper was obtained in the same manner as in Example 1. The leg-opening portions of the produced diaper had gathers formed by elastic yarn.
[0166] [Comparative Example 2] A diaper was produced in the same manner as in Example 1, except that nonwoven fabric B was used instead of nonwoven fabric A.
[0167] [Comparative Example 3] (Laminating process) The nonwoven fabric C was used in the leg surroundings of the backsheet, and the nonwoven fabric A was used in the waist surroundings of the backsheet. In the waist surroundings, the sheet was arranged so that the stretching direction was the left-right direction of the diaper.
[0168] Other than that, the two parts 3-1 and 3-2 were bonded together in the same manner as in Example 1 to form a back sheet body.
[0169] Five elastic threads were attached to the waist area of the above-mentioned backsheet body using a hot melt agent at 3 mm intervals from a position 40 mm below the top end of the diaper, stretched 150% in the left-right direction of the diaper, and the sheet was folded back to the side with the elastic threads attached 20 mm from the top end of the diaper and attached using a hot melt agent to form a backsheet.
[0170] (Lamination process) A diaper was produced in the same manner as in Example 1 using the above backsheet.
[0171] [Comparative Example 4] A diaper was produced in the same manner as in Example 1, except that nonwoven fabric D was used instead of nonwoven fabric A.
[0172] [Comparative Example 5] A diaper was produced in the same manner as in Example 1, except that nonwoven fabric E was used instead of nonwoven fabric A.
[0173] [Comparative Example 6] In the lamination process, the sheets were arranged in such a way that the stretch direction of nonwoven fabric A in the leg surroundings was the left-right direction of the diaper. Otherwise, the diaper was produced in the same manner as in Example 1.
[0174] The diapers obtained in Examples 1 to 3 were subjected to a wearing test, and the results are shown in Table 2.
[0175] [Table 2]
[0176] As shown in Table 2, the diapers of Examples 1 to 3 were excellent in terms of surface touch, fit, and movement followability.
[0177] The results of a wearing test on the diapers obtained in Comparative Examples 1 to 6 are shown in Table 3. In the Comparative Examples, when neither the waist nor the leg portions met the condition that they were part A, either the leg portions / waist portion or the waist portion / leg portions where the ratio of the vertical elongation loads was less than 1.00 was selected and entered in the F50A / F50B column.
[0178] [Table 3]
[0179] As shown in Table 3, the nonwoven fabric of Comparative Example 1 had poor fit and movement tracking because the area ratio of nonwoven fabric A consisting of crimped fiber and elastomer was low. The diaper of Comparative Example 2 had poor surface touch because the back sheet did not contain crimped fiber. Also, since it did not contain crimped fiber, it had poor elongation and poor fit and movement tracking. The diaper of Comparative Example 3 had excellent surface touch, but since the thickness change rate of the back sheet was high, a space was easily generated between the body and the diaper during movement, and it had poor fit. The diaper of Comparative Example 4 had excellent fit and movement tracking, but due to the rubber touch peculiar to the elastomer, it had a significantly poor surface feel. The diaper of Comparative Example 5 had a good surface touch, but due to the lack of stretchability of the back sheet, it had a significantly poor fit and movement tracking. The diaper of Comparative Example 6 had a good surface touch and fit, but there was no difference in the vertical elongation load between the leg and waist parts, and F50A / F50B did not reach 0.90 or less, so that there were parts of the backsheet that were prone to tension during movement, resulting in poor movement followability. [Explanation of symbols]
[0180] 1-1: Diaper opening around the waist 1-2A, 1-2B: Diaper leg openings X, X': Lower end of the leg opening of the diaper Y, Y': Upper end of the leg opening of the diaper 2-1: Top sheet 2-2: Absorbent 2-3: Liquid-impermeable sheet 2-4: Back seat 2-5: Side gathers 3-1: Torso parts 3-1a: The upper edge of the diaper on the waist part 3-1b: The edge of the waist part near the crotch of the diaper 3-2: Leg parts 3-3: The area where the torso and leg parts overlap 3-4a, 3-4b: Side ends of the waist part
Claims
1. A diaper comprising a top sheet, an absorbent body, and a back sheet, the back sheet being composed of a waist portion and leg portions, at least one of the waist portion and the leg portions being (1) At least 30% of the area of the nonwoven fabric is made of crimped fibers and has an elastomer; and (2) The thickness change rate when elongated by 30% is 20.0% or less compared to the thickness when no load is applied. and when only one of the waist and leg portions satisfies the above (1) and (2), that part is called part A and the other part is called part B; and when both the waist and leg portions satisfy the above (1) and (2), the part which has a lower elongation load when the diaper is elongated 50% in the vertical direction is called part A and the other part is called part B, the elongation load when the diaper is elongated 50% in the vertical direction is 0.90 or less times the elongation load when the diaper is elongated 50% in the vertical direction.
2. The part B is The nonwoven fabric is made of elastomer and has an area ratio of 30% or more composed of crimped fibers; and The thickness change rate when stretched 30% is 20.0% or less compared to the thickness when no load is applied The diaper according to claim 1 , which satisfies the above.
3. A method for producing the diaper according to claim 1 or 2, comprising the steps of: The method for producing the diaper includes the steps of: a back sheet manufacturing process for manufacturing a back sheet; a lamination step of laminating an absorbent body and a top sheet on the back sheet; Including, The back sheet manufacturing process includes: a fabric-making process in which the crimp-producing composite fibers are collected on a collecting belt to form a spunbonded nonwoven fabric layer, and at least one elastomer layer is laminated thereon and then integrated to obtain a laminated nonwoven fabric; A stretching process in which at least a part of the laminated nonwoven fabric obtained in the fabric-making process is stretched in at least one direction by a geared roller; a bonding step of bonding the stretched laminated nonwoven fabric as a sheet of part A so that a portion of the sheet of part A and a portion of the sheet of part B overlap each other; Including, A method for manufacturing diapers.
4. The method for producing a diaper according to claim 3 , wherein the stretched laminated nonwoven fabric is used as a sheet for the waist area so that the stretching direction in the stretching step is the left-right direction of the diaper.
5. The method for producing a diaper according to claim 3, wherein the stretched laminated nonwoven fabric is used as the leg-surrounding sheet so that the stretching direction in the stretching step is the vertical direction of the diaper.
6. The method for producing a diaper according to claim 5, wherein the stretched laminated nonwoven fabric is used as a sheet for the waist area so that the stretching direction in the stretching step is the left-right direction of the diaper.
Citation Information
Patent Citations
Pants-type disposable wearing article
JP2009148607A