Heat-storage silicone composition and cured product thereof

The heat storage silicone composition addresses the issues of microcapsule damage and agglomeration by using silicone rubber or resin powder as a co-filler, ensuring stable and efficient heat storage without leakage or contamination, suitable for electronic component cooling.

JP2024169849APending Publication Date: 2024-12-06SHIN ETSU CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023086658
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing heat storage materials, such as acrylic resin compositions, suffer from poor heat resistance, cold resistance, and weather resistance, leading to polymer deterioration, and the use of thermally conductive particles can damage microcapsules, causing leakage and agglomeration issues, which reduce heat storage efficiency and contaminate surrounding areas.

Method used

A heat storage silicone composition is formulated using microcapsules encapsulating a heat storage material and silicone rubber or resin powder as a co-filler, combined with specific additives to maintain the integrity of the microcapsules and enhance heat storage properties, preventing leakage and ensuring uniform dispersion.

Benefits of technology

The composition provides a stable, high heat storage effect with maintained cohesion of microcapsules, preventing contamination and applying minimal stress to heat-generating components, while offering flexibility and compressibility for efficient heat dissipation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169849000001
    Figure 2024169849000001
  • Figure 2024169849000002
    Figure 2024169849000002
  • Figure 2024169849000003
    Figure 2024169849000003
Patent Text Reader

Abstract

To provide a heat-storage silicone composition that contains microcapsules with heat-storage functionality without damaging their outer shells or breaking their aggregation, exhibits superior heat-storage performance, and ensures no contamination to a surrounding environment, and a cured product thereof.SOLUTION: A heat-storage silicone composition contains (A) an organopolysiloxane with two or more alkenyl groups in one molecule, (B) an organohydrogenpolysiloxane with two or more hydrosilyl groups in one molecule, (C) microcapsules, serving as a heat-storage filler, with an outer shell made of organic resin, encapsulating a heat-storage material, (D) silicone rubber powder and / or silicone resin powder, (E) a platinum group metal-based curing catalyst, (F) an addition reaction control agent, and (G) a surface treatment agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat-storing silicone composition and a cured product thereof. [Background technology]

[0002] As electronic devices become smaller and more highly integrated, the effects of heat generated from electronic components such as power semiconductors and memory are becoming more serious than ever. When heat accumulates in an electronic component, the temperature of the electronic component rises, which may cause malfunction or failure. Many heat dissipation methods and heat dissipation members used therefor have been proposed to efficiently dissipate the heat generated from the electronic component to a cooling member such as a heat sink.

[0003] In recent years, in order to miniaturize electronic devices, heat dissipation designs that do not use heat sinks have been considered, and in such designs, heat storage materials are sometimes used. Heat storage materials are materials that can store heat by utilizing changes in the state of matter, and by contacting this heat storage material with a heat generating body, a cooling effect can be obtained. Here, microcapsules in which a phase change material having latent heat such as paraffin is encapsulated in capsules of melamine resin or the like are well known as a heat storage filler in which the heat storage material is granulated to facilitate dispersion in a matrix. A molded body obtained by curing a composition containing such microcapsules is used as a heat storage molded body. Specifically, a heat storage acrylic resin sheet formed using microcapsules encapsulating paraffin has been disclosed (Patent Document 1). Also, a heat storage sheet obtained by molding and curing a heat storage acrylic resin composition containing a predetermined amount of microcapsules encapsulating paraffin into a sheet shape has been disclosed (Patent Document 2). However, such acrylic resin compositions have the problem that they are poor in heat resistance, cold resistance and weather resistance, and the polymer deteriorates with long-term use.

[0004] In addition, in order to increase the filling efficiency, the heat storage filler may use particles that have been enlarged by agglomerating the primary particles of the microcapsules using spray drying or the like. However, if only large particles are filled, there is a problem that the composition loses its smoothness, and its fluidity and moldability decrease. To solve these problems, a material has been disclosed in which thermally conductive particles and microcapsules encapsulating paraffin or the like are blended with organopolysiloxane (Patent Document 3). However, when the microcapsules and the thermally conductive particles are dispersed in the organopolysiloxane, the outer shell of the microcapsule may be damaged by the load during mixing, causing the internal heat storage material to leak out. In this case, problems may arise such as contamination of the surroundings by the leaked heat storage material and failure to obtain the desired heat storage effect. Furthermore, the impact load of the thermally conductive particles causes the aggregation of the microcapsules to break down, making it impossible to achieve a high packing density of the microcapsules, and as a result, there has been a problem in that the desired heat storage effect cannot be obtained. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-29985 A [Patent Document 2] JP 2007-31610 A [Patent Document 3] JP 2014-208728 A Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, an object of the present invention is to provide a heat storage silicone composition which can be incorporated without destroying the outer shells or aggregates of heat storage microcapsules, has excellent heat storage properties, and does not contaminate the surrounding area, as well as a cured product thereof. [Means for solving the problem]

[0007] As a result of extensive research into the above-mentioned problems, the inventors have discovered that by using microcapsules containing a heat storage material as a heat storage filler, and silicone rubber powder and / or silicone resin powder as a co-filler, it is possible to obtain a heat storage silicone composition and a heat storage silicone cured product (heat storage silicone sheet) obtained by curing said composition, without destroying the outer shells or aggregates of the microcapsules, and have completed the present invention. That is, the present invention provides the following heat-storing silicone composition and cured product thereof.

[0008] [1] (A) an organopolysiloxane having two or more alkenyl groups per molecule: 100 parts by mass, (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the number of moles of hydrosilyl groups is 0.1 to 5.0 times the number of moles of alkenyl groups derived from component (A); (C) as a heat storage filler, microcapsules having an organic resin outer shell and encapsulating a heat storage material: 100 to 400 parts by mass, (D) silicone rubber powder and / or silicone resin powder: 10 to 200 parts by mass, (E) Platinum group metal curing catalyst: 0.1 to 2,000 ppm by mass of platinum group element relative to component (A); (F) Addition reaction inhibitor: 0.01 to 4.0 parts by mass per 100 parts by mass of component (A), (G) (G-1) and (G-2) below; (G-1) The following formula (1) R 1 a R 2 b Si(OR 3 ) 4-a-b (1) (In formula (1), R 1 are independently alkyl groups having 6 to 18 carbon atoms, R 2 are independently selected from an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 12 carbon atoms; R 3are independently an alkyl group having 1 to 6 carbon atoms, a is a number from 1 to 3, and b is a number from 0 to 2, with the proviso that a+b is a number from 1 to 3. An alkoxysilane compound represented by the formula: (G-2) The following formula (2) [ka] (In formula (2), R 4 are independently an alkyl group having 1 to 6 carbon atoms, and c is a number from 5 to 100. a dimethylpolysiloxane having one molecular chain end blocked with a trialkoxysilyl group, represented by the formula: one or more surface treatment agents selected from the following: 10 to 200 parts by mass per 100 parts by mass of the (A) component; A heat storage silicone composition comprising: [2] Furthermore, as the component (H), [ka] (In formula (3), R 5 are independently selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 12 carbon atoms, and d is a number from 5 to 1,500. The kinetic viscosity at 23°C is 5 to 100,000 mm 2 / s organopolysiloxane: 0.1 to 100 parts by mass per 100 parts by mass of component (A) The heat storage silicone composition according to [1], [3] The heat storage silicone composition according to [1] or [2], wherein the heat storage material of component (C) is paraffin having a melting point of 0°C or higher. [4] (C) The heat storage silicone composition according to any one of [1] to [3], wherein the outer shell of the heat storage filler is made of a melamine resin. [5] (C) The heat storage silicone composition according to any one of [1] to [4], wherein the heat storage filler is an aggregate of particles having an average particle size of 20 to 80 μm. [6] (C) The heat storage silicone composition according to any one of [1] to [5], wherein the heat storage filler is primary particles having an average particle size of 1 to 10 μm. [7] A cured product of the heat storage silicone composition according to any one of [1] to [6]. [8] An electric or electronic part comprising a cured product of the heat storage silicone composition according to [7]. Effect of the Invention

[0009] The heat storage silicone composition of the present invention is made by blending microcapsules having an organic resin outer shell and encapsulating a heat storage material as a heat storage filler with silicone rubber powder and / or silicone resin powder as a co-filler in a specific composition and ratio, which makes it possible to easily provide a composition that has high heat storage and is uniform and stable. In addition, the heat storage silicone cured product (heat storage silicone sheet) obtained from the silicone composition of the present invention has a high heat storage effect because the aggregation of the microcapsules is maintained, and there is no need to worry about the surrounding area being contaminated by the bleeding of the heat storage material. Furthermore, since it has a low hardness, it does not apply stress to the heat generating member, and has flexibility and compressibility that can follow the fine unevenness of the heat generating member and the cooling member. Therefore, the present invention is useful as a cooling member for efficiently dissipating heat generated from electronic components. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below, but the present invention is not limited thereto.

[0011] [(A) Alkenyl-containing organopolysiloxane] The alkenyl-containing organopolysiloxane of component (A) is an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in one molecule, and is the main component of the heat-storing silicone composition of the present invention. Usually, the main chain portion is basically composed of a repetition of diorganosiloxane units, but this may include a branched structure as part of the molecular structure, or may be a cyclic body, but from the viewpoint of physical properties such as the mechanical strength of the cured product of the composition, linear diorganopolysiloxanes are preferred.

[0012] Examples of the alkenyl group include those having 2 to 8 carbon atoms, such as vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, and cyclohexenyl groups, among which lower alkenyl groups such as vinyl and allyl are preferred, and vinyl is particularly preferred. The alkenyl group is characterized by the presence of two or more alkenyl groups in one molecule, preferably 2 to 6, and more preferably 2 to 3. In order to improve the flexibility of the resulting cured product, it is most preferred that the alkenyl group is present only bonded to the silicon atom at the molecular chain end.

[0013] Examples of functional groups other than alkenyl groups bonded to silicon atoms include monovalent hydrocarbon groups having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms. Examples include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenylyl; and aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl. Among these, methyl, ethyl, propyl, and phenyl groups are preferred. In addition, all of the functional groups other than alkenyl groups bonded to silicon atoms may be the same or different.

[0014] The kinematic viscosity of this organopolysiloxane at 23°C is 10 to 100,000 mm 2 / s range is preferable, and 100 to 50,000 mm 2 The kinematic viscosity is particularly preferably in the range of 10 mm / s. 2 If the viscosity is less than 100,000 mm / s, the storage stability of the resulting composition will be poor. 2 If the viscosity exceeds 1 / s, the extensibility of the resulting composition may be poor. In this specification, the kinematic viscosity is a value measured at 23°C using a Cannon-Fenske viscometer according to the method described in JIS Z 8803:2011. The organopolysiloxane of component (A) may use either a single type alone, or a combination of two or more types having different kinetic viscosities.

[0015] [(B) Organohydrogenpolysiloxane] The organohydrogenpolysiloxane of component (B) is an organohydrogenpolysiloxane having two or more, preferably 2 to 100, hydrosilyl groups (hydrogen atoms directly bonded to silicon atoms) in one molecule. It is a component that acts as a crosslinking agent for component (A). That is, the hydrosilyl groups in component (B) and the alkenyl groups in component (A) are added by a hydrosilylation reaction promoted by the platinum group metal curing catalyst of component (E) described below, to give a three-dimensional network structure having a crosslinked structure. Note that when the number of hydrosilyl groups in one molecule of the organohydrogenpolysiloxane is less than two, the organohydrogenpolysiloxane does not cure.

[0016] Examples of the organohydrogenpolysiloxane of component (B) include, but are not limited to, those represented by the following formula (4): The organohydrogenpolysiloxane of component (B) may be used alone or in combination of two or more different types. [ka] (In formula (4), R 6are independently a hydrogen atom or a monovalent hydrocarbon group selected from an alkyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 12 carbon atoms. However, there are two or more, preferably two to ten, R 6 is a hydrogen atom. Also, e is a number of 1 or more, preferably a number of 10 to 200.

[0017] In formula (4), R 6 Examples of the monovalent hydrocarbon group other than hydrogen atom include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl, cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl, aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenylyl, and aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl. Among these monovalent hydrocarbon groups, groups having 1 to 10 carbon atoms, particularly preferably 1 to 6 carbon atoms, are preferred, and alkyl groups having 1 to 3 carbon atoms, such as methyl, ethyl, and propyl, and phenyl groups are particularly preferred.

[0018] The amount of the (B) component is characterized in that the hydrosilyl group derived from the (B) component is 0.1 to 5.0 mol per 1 mol of the alkenyl group derived from the (A) component. The amount is preferably 0.3 to 2.0 mol, more preferably 0.5 to 1.5 mol. If the amount of the hydrosilyl group derived from the (B) component is less than 0.1 mol per 1 mol of the alkenyl group derived from the (A) component, the composition may not cure, or the strength of the cured product may be insufficient to maintain the shape of the molded product and make it difficult to handle. If the amount exceeds 5.0 mol, the cured product may lose flexibility and become brittle.

[0019] [(C) Microcapsules containing heat storage material] The heat storage filler of component (C) is a microcapsule having an organic resin outer shell and encapsulating a heat storage material. The heat storage filler of component (C) may be used alone or in combination of two or more kinds. Examples of organic resins that form the outer shell of microcapsules include polystyrene, polyamide, ethyl cellulose, polyurethane, acrylic resin, aminoplast resin, urea resin, and melamine resin. Among these, melamine resin and acrylic resin are preferred from the viewpoint of strength and flexibility. These organic resins can be used alone or in combination to form the film that becomes the outer shell. As the heat storage material to be encapsulated in the microcapsules, paraffin, organic acid, alcohol, etc. are preferable because they have a large heat storage amount per unit volume, are safe and resistant to corrosion, and can stably dissipate and store heat even when melted and solidified repeatedly, and are inexpensive. Among them, paraffin is particularly preferable from the viewpoint of exhibiting excellent heat storage properties. As the paraffin, those containing linear aliphatic hydrocarbons having a melting point of 0°C or higher are preferable, and those containing linear aliphatic hydrocarbons having a melting point of 0°C or higher and having 14 or more carbon atoms are more preferable. As the linear aliphatic hydrocarbons having a melting point of 0°C or higher, saturated aliphatic hydrocarbons such as n-tetradecane, n-hexadecane, n-eicosane, n-docosane, n-pentacosane, n-hexacosane, and n-triacontane can be mentioned. The number of carbon atoms of the saturated aliphatic hydrocarbon is preferably 16 to 40.

[0020] The melting point of the heat storage material may be selected according to the type of heat generating element, the heat generating temperature of the heat generating element, the temperature after cooling or the temperature to be maintained, and the purpose of cooling, etc. By appropriately selecting the melting point, for example, the temperature of the heat generating element can be stably maintained at an appropriate temperature that is not too cold. Such a heat storage material can be appropriately selected according to the purpose of use, and for example, one type of heat storage material having a melting point in the target temperature range can be selected and used, or two or more types of heat storage materials can be mixed and used. There is no particular limitation on the method for microencapsulating the heat storage material, and a known method can be appropriately adopted. In addition, as the microcapsules containing such a heat storage material, commercially available microcapsules containing a heat storage material (heat storage filler) may be appropriately used.

[0021] The heat storage filler (microcapsules containing a heat storage material) preferably has an average particle size of 20 to 80 μm, more preferably 40 to 80 μm, of the aggregated particles. The average particle size of the primary particles of the heat storage filler is preferably 1 to 10 μm, more preferably 2 to 8 μm. If the aggregated particles and primary particles are within this range, high loading into silicone becomes easy, and the aggregates are less likely to break down, resulting in a stable composition. If the agglomerated particles are too small, when they are mixed into silicone, the viscosity of the composition tends to become too high, reducing processability. Conversely, if the agglomerated particles are too large, they are difficult to mix uniformly, making it difficult to disperse them uniformly in the sheet. If the primary particles are too small, the proportion of the heat storage material in the heat storage filler will be small, and the heat storage effect will tend to decrease. If the primary particles are too large, the aggregated particles will tend to crumble, and when mixed with silicone, the viscosity of the composition will tend to become too high, and processability will tend to decrease. The primary particle diameter of the primary particles is the average particle diameter of the microcapsules uniformly dispersed in the slurry-like material before aggregation. The average particle diameter of the aggregated particles is the average particle diameter of the microcapsules uniformly dispersed in the slurry-like material when they aggregate. Furthermore, the above average particle diameters of the primary particles and aggregated particles are the cumulative 50% particle diameters on a volume basis (D 50 ) value.

[0022] The amount of the heat storage filler in the present invention is 100 to 400 parts by mass, and preferably 150 to 350 parts by mass, per 100 parts by mass of component (A). If the amount of the heat storage filler is less than 100 parts by mass, the resulting composition and cured product will not have sufficient heat storage properties, whereas if it exceeds 400 parts by mass, the viscosity of the composition after blending may increase, decreasing processability.

[0023] [(D) Silicone rubber powder and silicone resin powder] The silicone rubber powder and silicone resin powder of component (D) improve the uniformity and fluidity of the heat storage silicone composition of the present invention. Because the silicone rubber powder and silicone resin powder have excellent lubricity and impact absorption properties, even when used in combination with the heat storage filler (C), destruction of the aggregates and destruction of the outer shell of the heat storage filler are suppressed.

[0024] The silicone rubber powder is preferably a spherical powder of silicone rubber having a structure in which linear dimethylpolysiloxane is crosslinked. The silicone resin powder is preferably (CH3SiO 3 / 2 ) n It is preferable that the spherical powder of polymethylsilsesquioxane has a three-dimensional network-like crosslinked structure represented by the formula: The average particle size is preferably 0.1 to 20 μm. The average particle size is a value measured by an electrical resistance method particle size distribution measuring device (Multisizer 3: manufactured by Beckman Coulter, Inc.). If the particle size is too small, the viscosity of the composition may become too high when mixed with silicone, resulting in poor processability, while if the particle size is too large, it may be difficult to mix uniformly and therefore difficult to disperse uniformly in the sheet. Silicone composite powders in which the surface of spherical silicone rubber powder is coated with silicone resin may also be used. Examples of such rubber powders, resin powders, and composite powders include the KMP series manufactured by Shin-Etsu Chemical Co., Ltd. The silicone rubber powder of component (D) may be used alone or in combination of two or more kinds. The silicone resin powder of component (D) may be used alone or in combination of two or more kinds. Note that component (D) may be used in combination of a silicone rubber powder and a silicone resin powder.

[0025] The amount of silicone rubber powder and / or silicone resin powder blended in the present invention is 10 to 200 parts by mass, preferably 20 to 150 parts by mass, and more preferably 50 to 120 parts by mass, per 100 parts by mass of component (A).

[0026] [(E) Platinum group metal curing catalyst] The platinum group metal curing catalyst of component (E) is a catalyst for promoting the addition reaction between the alkenyl group derived from component (A) and the hydrosilyl group derived from component (B), and may be any of the well-known catalysts used in hydrosilylation reactions. Specific examples of platinum group metal curing catalysts include platinum (including platinum black), rhodium, palladium, and other platinum group metal elements, H2PtCl4·nH2O, H2PtCl6·nH2O, NaHPtCl6·nH2O, KaHPtCl6·nH2O, Na2PtCl6·nH2O, K2PtCl4·nH2O, PtCl4·nH2O, PtCl2, Na2HPtCl4·nH2O (wherein n is a number from 0 to 6, preferably 0 or 6), platinum chlorides such as chloroplatinic acid and chloroplatinic acid salts, and alcohol-modified chloroplatinic acid (U.S. Pat. No. 3,220,933). No. 72), complexes of chloroplatinic acid and olefins (see U.S. Pat. Nos. 3,159,601, 3,159,662, and 3,775,452), platinum black, platinum group metals such as palladium supported on supports such as alumina, silica, and carbon, rhodium-olefin complexes, chlorotris(triphenylphosphine)rhodium (Wilkinson's catalyst), complexes of platinum chloride, chloroplatinic acid, or chloroplatinate with vinyl group-containing siloxanes, particularly vinyl group-containing cyclic siloxanes. The blend amount of component (E) is 0.1 to 2,000 ppm, and preferably 50 to 1,000 ppm, calculated as the mass of platinum group metal element relative to component (A). The platinum group metal curing catalyst of the component (E) may use either a single type alone, or a combination of two or more types.

[0027] [(F) Addition reaction regulator] The addition reaction inhibitor of component (F) is not particularly limited as long as it is a known addition reaction inhibitor used in normal addition reaction curing silicone compositions. For example, acetylene compounds such as 1-ethynyl-1-cyclohexanol, 3-butyn-1-ol, 2-methyl-3-butyn-2-ol, and 3-methyl-1-tridecyne-3-ol, various nitrogen compounds, organic phosphorus compounds, oxime compounds, organic chloro compounds, and vinyl group-containing siloxanes such as 1,3-divinyl-1,1,3,3-tetramethyldisiloxane and 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane can be mentioned. The blend amount of component (F) is 0.01 to 4.0 parts by mass, and preferably about 0.1 to 2.5 parts by mass, per 100 parts by mass of component (A). If the blend amount is too large, the curing reaction will not proceed well, and molding efficiency may be impaired. The addition reaction inhibitor of the component (F) may use either a single type alone, or a combination of two or more types.

[0028] [(G) Surface treatment agent] The surface treatment agent of component (G) hydrophobizes component (C) during the preparation of the composition, improves the wettability with component (A), and disperses component (C) uniformly in the matrix derived from component (A). Component (G) is at least one selected from components (G-1) and (G-2) shown below. The (G-1) component may be used alone or in combination of two or more kinds. The (G-2) component may be used alone or in combination of two or more kinds.

[0029] (G-1) Component The component (G-1) is an alkoxysilane compound represented by the following formula (1). R 1 a R 2 b Si(OR 3 ) 4-a-b (1) (In formula (1), R 1 are independently alkyl groups having 6 to 18 carbon atoms, R 2 are independently selected from an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 12 carbon atoms; R 3 are independently an alkyl group having 1 to 6 carbon atoms, a is a number from 1 to 3, and b is a number from 0 to 2, with the proviso that a+b is a number from 1 to 3.

[0030] In the above formula (1), R 1 Examples of the alkyl group having 6 to 18 carbon atoms represented by the formula (I) include a hexyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, a tetradecyl group, and a hexadecyl group. 1 When the alkyl group represented by the formula (I) has 6 to 18 carbon atoms, the wettability of the component (A) is sufficiently improved, the handleability is good, and the low-temperature properties of the composition are excellent. R 2 Examples of the alkyl group having 1 to 5 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, and a neopentyl group. Examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and a biphenylyl group. Examples of the aralkyl group having 7 to 12 carbon atoms include a benzyl group, a phenylethyl group, a phenylpropyl group, and a methylbenzyl group. Among these, R 2 As the alkyl group, an alkyl group having 1 to 3 carbon atoms, such as a methyl group, an ethyl group, or a propyl group, and a phenyl group are preferable. R 3 Examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, and a hexyl group.

[0031] (G-2) Component The component (G-2) is a dimethylpolysiloxane having one molecular chain end blocked with a trialkoxysilyl group, as represented by the following formula (2). [ka] (In formula (2), R 4 are independently alkyl groups having 1 to 6 carbon atoms, and specifically, 3 Examples of the alkyl group include the same alkyl groups as those exemplified in the above. c is a number from 5 to 100, preferably from 5 to 70, and particularly preferably from 10 to 50.

[0032] As the surface treatment agent for the component (G), either the component (G-1) or the component (G-2) may be used, or the components (G-1) and (G-2) may be used in combination. The blending amount of component (G) is 10 to 200 parts by mass, and preferably 20 to 150 parts by mass, per 100 parts by mass of component (A). If it exceeds 200 parts by mass, there is a risk of inducing oil separation.

[0033] [(H) Organopolysiloxane] The heat-storage silicone composition of the present invention contains, as component (H), a silicone oil having a kinetic viscosity at 23° C. of 5 to 100,000 mm, which is represented by the following formula (3), for the purpose of adjusting the viscosity of the heat-storage silicone composition. 2 The component (H) may be used alone or in combination of two or more different organopolysiloxanes. [ka] (In formula (3), R 5 are independently selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 12 carbon atoms, and d is a number from 5 to 1,500.

[0034] In the above formula (3), R 5R is independently a group selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 12 carbon atoms. 5 Specific examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, and pentyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenylyl groups; and aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl groups. Among these, alkyl groups having 1 to 3 carbon atoms such as methyl, ethyl, and propyl groups, and phenyl groups are preferred, with methyl and phenyl groups being particularly preferred.

[0035] From the viewpoint of the required viscosity, the above d is preferably a number from 5 to 1,500, and particularly preferably a number from 10 to 1,000.

[0036] The kinetic viscosity of component (H) at 23°C is 5 to 100,000 mm 2 / s, and particularly 100 to 10,000 mm 2 It is preferable that the kinematic viscosity is 5 mm / s. 2 If the kinematic viscosity is lower than 100,000 mm / s, the resulting cured product of the composition may be prone to oil bleeding. 2 If it is greater than / s, the flexibility of the resulting composition may be poor.

[0037] When component (H) is blended into the heat storage silicone composition of the present invention, its blending amount is not particularly limited as long as the desired effect is obtained, but it is preferably 0.1 to 100 parts by mass, and more preferably 1 to 50 parts by mass, per 100 parts by mass of component (A). If the blending amount is within this range, it is easy to maintain good fluidity and workability in the heat storage silicone composition before curing, and it is also easy to fill the microcapsules of component (C) into the composition.

[0038] [Other ingredients] The heat-storing silicone composition of the present invention may further contain other components as long as the purpose and effects of the present invention are not impaired. For example, optional components such as a heat resistance improver, a viscosity modifier other than component (H), a colorant, and a release agent (component (I)) may be added. Examples of the release agent (component (I)) include methylphenyl silicone oil, fluorosilicone oil, zinc stearate, etc. The component (I) may be used alone or in combination of two or more types. When component (I) is used, the amount of component (I) is 0.01 to 50 parts by mass, and preferably 0.1 to 25 parts by mass, per 100 parts by mass of component (A).

[0039] [Preparation of heat storage silicone composition] The heat-storage silicone composition of the present invention can be prepared by uniformly mixing the above-mentioned components in accordance with a conventional method. The method for producing the silicone composition is not particularly limited, but it can be obtained, for example, by kneading a predetermined amount of the above-mentioned components with a known kneading machine such as a planetary mixer. In addition, heat treatment (kneading under heat) may be performed as necessary.

[0040] [Method of manufacturing heat-storing silicone cured product] The curing conditions for molding the heat storage silicone composition may be the same as those for known addition reaction curing type silicone rubber compositions. For example, the composition will cure sufficiently at room temperature, but may be heated and pressurized as necessary. Addition curing is preferably performed at 100 to 120°C for 5 to 20 minutes. The cured product of the heat storage silicone composition of the present invention thus produced has excellent heat storage properties. If the cured product is in sheet form, it will be easier to handle during transportation and packaging.

[0041] [Heat storage effect of heat storage silicone cured material] The heat storage effect of the heat storage silicone cured product can be confirmed by the fusion enthalpy observed in the temperature range of 10 to 60°C by differential scanning calorimetry, and the fusion enthalpy is preferably 30 J / g or more. If the fusion enthalpy observed in the temperature range of 10 to 60°C is 30 J / g or more, effective heat storage can be expected.

[0042] [Hardness of heat storage silicone cured product] The hardness of the heat storage silicone cured product of the present invention is preferably 10 or more and 60 or less, more preferably 10 or more and 40 or less, measured at 23°C using an Asker C hardness tester. If the hardness exceeds 60, the product may deform to fit the shape of the adherend, making it difficult to exhibit good heat storage properties without applying stress to the heat dissipation target. If the hardness is 10 or less, the tack may increase, resulting in poor handling. If the hardness is 10 or less, the cured product may deform or break. Such hardness can be adjusted by changing the ratio of the (A) component and the (B) component to adjust the crosslink density. EXAMPLES

[0043] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to these.

[0044] [Preparation of Composition] The components (A) to (I) used in the following examples and comparative examples are shown below.

[0045] Component (A) The kinetic viscosity at 23°C, as shown in the following formula (5), is 600 mm 2 / s organopolysiloxane [ka]

[0046] (B) Component Organohydrogenpolysiloxane represented by the following formula (6): [ka] (In formula (6), the bonding order of these siloxane units may be block or random.)

[0047] (C) Component (C-1) Paraffin-encapsulated melamine capsules consisting of aggregated particles with an average particle size of 72 μm Primary particle size: 7μm, paraffin melting point: 44℃ (C-2) Paraffin-encapsulated melamine capsules consisting of aggregated particles with an average particle size of 20 μm Primary particle size: 2μm, paraffin melting point: 44℃

[0048] (D) Component (D-1) Silicone resin powder manufactured by Shin-Etsu Chemical Co., Ltd.: KMP-706, average particle size: 2 μm (D-2) Silicone rubber powder manufactured by Shin-Etsu Chemical Co., Ltd.: KMP-597, average particle size: 5 μm (D-3) Irregular aluminum hydroxide with an average particle size of 1.5 μm (for comparison)

[0049] (E) Component 5% by weight solution of chloroplatinic acid in 2-ethylhexanol

[0050] Ingredient (F) 3-Methyl-1-tridecyl-3-ol

[0051] (G) Component (G-1) An alkoxysilane compound represented by the following formula (7): CH3(CH2) 15 Si(OCH3)3(7) (G-2) Dimethylpolysiloxane with an average degree of polymerization of 30 and one end capped with a trimethoxysilyl group [ka]

[0052] (H) Component As a plasticizer, dimethylpolysiloxane represented by the following formula (9) (kinematic viscosity at 23°C is 100 mm 2 / s) [ka]

[0053] Component (I) Methylphenyl silicone oil (KF-54: Shin-Etsu Chemical Co., Ltd.)

[0054] [Examples 1 to 5, Comparative Examples 1 to 3] In Examples 1 to 5 and Comparative Examples 1 to 3, compositions were prepared as described below using the above components (A) to (I) in the amounts shown in Table 1 below, molded and cured, and the hardness, enthalpy of fusion, and flow of the heat storage material of the cured products were measured and confirmed according to the methods described below. The results are shown in Table 1.

[0055] [Preparation of Composition] Components (A), (C), (D), (G), and (H) were added in the amounts shown in Examples 1 to 5 and Comparative Examples 1 to 3 in Table 1 below, and kneaded for 60 minutes with a planetary mixer. Component (E) was then added in the amount shown in Examples 1 to 5 and Comparative Examples 1 to 3 in Table 1 below, and further component (I) was added as an internal release agent to promote release from the separator, and kneaded for 30 minutes. Further, premixed components (B) and (F) were added thereto in the prescribed amounts shown in Examples 1 to 5 and Comparative Examples 1 to 3 in Table 1 below, and kneaded for 30 minutes to obtain compositions.

[0056] [Forming method] The compositions obtained in Examples 1 to 5 and Comparative Examples 1 to 3 were poured into a mold 60 mm long x 60 mm wide x 6 mm thick, and molded using a press molding machine at 120°C for 10 minutes to obtain cured products.

[0057] [Evaluation method] Hardness of the cured product The compositions obtained in Examples 1 to 5 and Comparative Examples 1 to 3 were cured under the above conditions using a press molding machine to prepare two 6 mm-thick sheets, which were then measured for hardness using an Asker C hardness tester. The results are shown in Table 1.

[0058] Fusion enthalpy of hardened material The melting enthalpy observed within a temperature range of 10 to 60°C of the cured products obtained in Examples 1 to 5 and Comparative Examples 1 to 3 was measured by differential scanning calorimetry (DSC). A DSC7000X manufactured by Hitachi High-Tech Science Corporation was used for the measurement. The measurement results are shown in Table 1.

[0059] Heat cycle test The cured products obtained in Examples 1 to 5 and Comparative Examples 1 to 3 were placed on a glass plate and subjected to a heat cycle test (50 cycles) from -20°C to 100°C. The fusion enthalpy observed within the temperature range of 10 to 60°C after the heat cycle was measured by differential scanning calorimetry (DSC) and compared with the initial value before aging (heat cycle test). The results are shown in Table 1. In addition, the glass plate was visually inspected for traces of flowing out of the heat storage material. The results are shown in Table 1. [Table 1]

[0060] In Examples 1 to 5, the flexibility and moldability of the composition, and the hardness and heat storage properties of the cured product were all good. In addition, the heat storage properties were maintained even after the heat cycle test, and the heat storage material did not flow out and contaminate the surrounding area. In Comparative Example 1, the amount of heat storage filler blended was too large, and a composition could not be obtained. In Comparative Example 2, the amount of the heat storage filler was too small, so that the heat storage capacity could not be improved. In Comparative Example 3, when ceramic powder such as aluminum hydroxide was used in combination with component (C), the outer wall of the heat storage filler was destroyed, decreasing the initial heat storage capacity, and the heat cycle test significantly decreased the heat storage capacity. Furthermore, contamination thought to be caused by the outflow of the heat storage material was visually confirmed.

Claims

1. (A) organopolysiloxane having two or more alkenyl groups in one molecule: 100 parts by mass, (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the number of moles of hydrosilyl groups is 0.1 to 5.0 times the number of moles of alkenyl groups derived from component (A); (C) as a heat storage filler, microcapsules having an organic resin outer shell and encapsulating a heat storage material: 100 to 400 parts by mass, (D) silicone rubber powder and / or silicone resin powder: 10 to 200 parts by mass, (E) Platinum group metal curing catalyst: 0.1 to 2,000 ppm by mass of platinum group element relative to component (A) (F) Addition reaction inhibitor: 0.01 to 4.0 parts by mass per 100 parts by mass of component (A), (G) The following (G-1) and (G-2); (G-1) Formula (1) below R 1 a R 2 b Si(OR 3 ) 4-a-b (1) (In formula (1), R 1 are independently alkyl groups having 6 to 18 carbon atoms; R 2 are independently selected from an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 12 carbon atoms; R 3 are independently an alkyl group having 1 to 6 carbon atoms, a is a number from 1 to 3, and b is a number from 0 to 2, with the proviso that a+b is a number from 1 to 3. An alkoxysilane compound represented by the formula: (G-2) Formula (2) below [Case 1] (In formula (2), R 4 are independently an alkyl group having 1 to 6 carbon atoms, and c is a number from 5 to 100. a dimethylpolysiloxane having one molecular chain end blocked with a trialkoxysilyl group, represented by the formula: one or more surface treatment agents selected from the following: 10 to 200 parts by mass per 100 parts by mass of component (A); A heat storage silicone composition comprising:

2. Furthermore, as the component (H), [Case 2] (In formula (3), R 5 are independently selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 12 carbon atoms, and d is a number from 5 to 1,500. The kinetic viscosity at 23°C represented by 2 / s organopolysiloxane: 0.1 to 100 parts by mass per 100 parts by mass of component (A) The heat storage silicone composition according to claim 1 , which contains

3. 2. The heat storage silicone composition according to claim 1, wherein the heat storage material of component (C) is paraffin having a melting point of 0° C. or higher.

4. 2. The heat storage silicone composition according to claim 1, wherein the outer shell of the heat storage filler (C) is a melamine resin.

5. The heat storage silicone composition according to claim 1, wherein the heat storage filler (C) is an aggregate of particles having an average particle size of 20 to 80 μm.

6. 2. The heat storage silicone composition according to claim 1, wherein the heat storage filler (C) is in the form of primary particles having an average particle size of 1 to 10 μm.

7. A cured product of the heat storage silicone composition according to claim 1.

8. An electric or electronic part comprising a cured product of the heat storage silicone composition according to claim 7.

Citation Information

Patent Citations

  • Epoxy resin composition and semiconductor device using the same

    JP1998189832A

  • Heat storage composition

    JP2008088376A

  • Heat storage elastomer molded body

    JP2010155932A

  • Curable silicone resin composition, cured product thereof, and optical semiconductor device

    JP2013216849A

  • Heat storable silicone material and method for producing the same

    JP2014208728A