Curable resin composition, laminate sheet using the same, prepreg and substrate with cured product and electronic apparatus mounted with the substrate with cured product
A curable resin composition with a specific polyimide resin formulation addresses the limitations of existing polyimides by enhancing adhesive strength and dielectric properties, suitable for high-frequency applications.
Patent Information
- Application Number
- JP2023086915
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
AI Technical Summary
Existing polyimide resins used in electronic materials lack sufficient adhesive strength and dielectric properties, particularly in high-frequency applications, with conventional compositions either compromising flexibility or dielectric performance.
A curable resin composition comprising a polyimide resin with a specific molar ratio of residues derived from maleic anhydride and other acid anhydrides with carbon-carbon unsaturated bonds, combined with a curing aid, to enhance adhesive strength and dielectric properties.
The composition achieves higher adhesive strength and improved dielectric properties, suitable for high-frequency applications, while maintaining flexibility and heat resistance.
Smart Images

Figure 2024170009000001 
Figure 2024170009000002 
Figure 2024170009000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin composition, a laminate sheet, a prepreg, and a substrate with a cured product using the same, and an electronic device equipped with the cured product substrate. [Background technology]
[0002] In recent years, the electronics field has seen remarkable development, particularly in the miniaturization, weight reduction, and high density of electronic devices, and electronic materials such as printed wiring boards are increasingly being required to be thinner, multi-layered, and highly precise. Specific examples of adhesives and coating agents used in the periphery of such electronic materials include the following (1) to (6).
[0003] (1) Interlayer adhesive: Used to bond circuit boards together, it comes into direct contact with copper or silver circuits. It is used between the layers of multilayer boards and is available in liquid and sheet form.
[0004] (2) Adhesives for coverlay films: These are used to bond coverlay films (such as polyimide films used to protect the top surface of circuits) to the underlying circuit board. In most cases, they are used in such a way that a polyimide film and an adhesive layer that are already integrated are bonded to the underlying board.
[0005] (3) Copper-clad film (CCL) adhesives: These are used to bond polyimide films and copper foils, which are often processed by etching or other processes when forming copper circuits.
[0006] (4) Coverlay: Used to protect the top surface of a circuit, it can take the form of a printed ink layer printed on the circuit, a laminated adhesive sheet, etc. In many cases, after laminating the coverlay, there is a process of curing it with light or heat.
[0007] (5) Reinforcing plate adhesive: Used to attach part of a wiring board to a reinforcing plate made of metal, glass epoxy, polyimide, etc., in order to supplement the mechanical strength of the wiring board.
[0008] (6) Electromagnetic shielding adhesive: Attached to flexible printed wiring boards to shield electromagnetic noise generated by electronic circuits. There are two forms: the adhesive itself contains electromagnetic shielding material, and the electromagnetic shielding adhesive is used to attach an electromagnetic shielding coverlay.
[0009] These may be in the form of a liquid (made into an ink for printing) or a sheet (made into a film in advance), and the appropriate form is selected depending on the application.
[0010] In order to meet these high demands for peripheral components for electronic materials, various polyimide resins are being investigated.
[0011] On the other hand, the trend towards higher frequencies requires copper foils with lower roughness, while the demand for higher adhesion due to the increased number of layers has led to a strong demand from the market for further improvements in adhesive strength. In recent years, polyimide resins with high adhesive strength, heat resistance, and good dielectric properties have been developed.
[0012] For example, Patent Document 1 discloses that a terminal maleimide resin containing a dimer diamine skeleton improves dielectric properties. However, even in the invention described in Patent Document 1, the improvement in dielectric properties was insufficient. In addition, because bismaleimide forms a rigid network through thermal radical crosslinking, there was a problem that the flexibility of the resin coating film was reduced and sufficient adhesive strength could not be obtained.
[0013] Moreover, Patent Document 2 discloses a composition that combines citraconimide and an epoxy resin to provide high adhesive strength and good dielectric properties. However, although the invention described in Patent Document 2 has a high adhesive strength, the dielectric properties are deteriorated by the epoxy resin, and therefore the performance is not sufficient for use in electronic substrates. [Prior art documents] [Patent documents]
[0014] [Patent Document 1] JP 2020-196789 A [Patent Document 2] JP 2022-147022 A Summary of the Invention [Problem to be solved by the invention]
[0015] An object of the present invention is to provide a curable resin composition which has higher adhesive strength and heat resistance than conventional ones, and also has good dielectric properties. [Means for solving the problem]
[0016] The present invention comprises a polyimide resin (A) and a curing aid (B), The polyimide resin (A) is a reaction product obtained by imidization reaction between a prepolymer having an amino group at the terminal, which is a reaction product of a tetracarboxylic dianhydride (C) and a dimer diamine, and an acid anhydride (a) having a carbon-carbon unsaturated bond, the polyimide resin (A) contains a residue derived from maleic anhydride (a1) and a residue derived from an acid anhydride (a2) having a carbon-carbon unsaturated bond other than maleic anhydride, The molecular weight of (a2) is 112 to 351, The curable resin composition is characterized in that the molar ratio of the residue derived from (a1) to the residue derived from (a2) in the polyimide resin (A) is 100:10 to 100:500.
[0017] The present invention also relates to the above curable resin composition, wherein (a2) contains at least one selected from the group consisting of citraconic anhydride, itaconic anhydride, allylsuccinic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride.
[0018] The present invention also relates to the above curable resin composition, wherein the tetracarboxylic dianhydride (C) has fluorine or an alicyclic structure.
[0019] The present invention also relates to the above curable resin composition, wherein the polyimide resin (A) has a weight average molecular weight of 5,000 to 150,000.
[0020] The present invention also relates to the above curable resin composition, which further comprises at least one selected from the group consisting of a crosslinking agent, a curing accelerator, and an antioxidant.
[0021] The present invention also relates to the curable resin composition further comprising a filler.
[0022] The present invention also relates to a laminate sheet having a substrate and a resin composition layer, the resin composition layer being formed from the curable resin composition.
[0023] The present invention also relates to a prepreg impregnated with the curable resin composition.
[0024] The present invention also relates to a substrate having a cured product of the curable resin composition on a substrate.
[0025] The present invention also relates to an electronic device equipped with the substrate with the cured product. Effect of the Invention
[0026] The present invention makes it possible to provide a curable resin composition that can achieve both higher adhesive strength and dielectric properties than conventional ones, a laminate sheet, a prepreg, and a substrate with a cured product using the same, and an electronic device equipped with the cured product substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, the curable resin composition of the present invention, a laminate sheet, a prepreg and a substrate with a cured product using the same, and an electronic device equipped with the cured product substrate will be described, but the present invention is not limited thereto. In this specification, the term "(meth)acryloxy group" includes both acryloxy and methacryloxy groups, the term "(meth)acrylamide" includes both acrylamide and methacrylamide, and the term "(meth)acrylate" includes both acrylate and methacrylate. In this specification, a numerical range specified using "to" is intended to include the numerical values before and after "to" as the lower and upper limit values of the range. Unless otherwise noted, the various components appearing in this specification may be used independently as a single type or as a combination of two or more types. The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight determined by gel permeation chromatography (GPC) measurement. The weight average molecular weight can be measured by the method described in the Examples section.
[0028] ≪Curable resin composition≫ The curable resin composition of the present invention contains a polyimide resin (A) and a curing aid (B). The resin composition is molded into a coating film or the like and then heat cured. The thermosetting resin composition may be prepared as a set of an A material containing the polyimide resin (A) and a B material containing the curing aid (B), and these materials are mixed together before use.
[0029] <Polyimide resin (A)> The polyimide resin (A) used in the present invention is a reaction product of an imidization reaction between a prepolymer having an amino group at the terminal and an acid anhydride (a) having a carbon-carbon unsaturated bond, and contains a residue derived from maleic anhydride (a1) and a residue derived from an acid anhydride (a2) having a carbon-carbon unsaturated bond other than maleic anhydride. The prepolymer having an amino group at the terminal is a reaction product of a tetracarboxylic dianhydride (C) and a dimer diamine.
[0030] In the present invention, the molar ratio of the residue derived from (a1) to the residue derived from (a2) in (A) is 100:10 to 100:500, and a range of 100:20 to 100:400 is preferred from the viewpoints of adhesive strength and dielectric properties.
[0031] The molar ratio of the residue derived from (a1) and the residue derived from (a2) in (A) can be calculated based on the amounts of (a1) and (a2) at the time of charging, or calculated from the chemical structure revealed by a nuclear magnetic resonance (NMR) spectrometer. The nuclear magnetic resonance (NMR) spectrometer is used to measure the molecular weight of the compound (RUFUTO's "Pulse NMR Particle Interface Characterization Apparatus Acorn Area"). The molar ratio calculated by either method is sufficient as long as it is within the above range.
[0032] The polyimide resin (A) may be a blend of a resin having (a1) at both ends and a resin having (a2) at both ends, or may be a resin having (a1) and (a2) at both ends. These may also be mixed.
[0033] The weight average molecular weight of the polyimide resin (A) is preferably from 2,000 to 150,000, and more preferably from 5,000 to 100,000. Within the above range, the wettability to the substrate is improved, and high adhesive strength can be achieved.
[0034] The imidization reaction can be carried out by reacting an amine with an acid anhydride at a relatively low temperature, for example, about 10 to 80° C., to form a polyamic acid, and then thermally or chemically imidizing the polyamic acid. Alternatively, the polyamic acid can be obtained by omitting the step of forming the polyamic acid and carrying out a one-step reaction of polymerization and imidization in an organic solvent at a relatively high temperature, for example, about 130 to 250° C.
[0035] Thermal imidization can be carried out at a temperature of, for example, about 140° C. to 200° C., and chemical imidization can be carried out in the presence of, for example, an organic base such as pyridine or triethylamine, and acetic anhydride, etc. The temperature at this time can be selected from any temperature between −20° C. and 200° C.
[0036] <Acid anhydride having carbon-carbon unsaturated bond (a)> The acid anhydride (a) having a carbon-carbon unsaturated bond is classified into maleic anhydride (a1) and acid anhydride (a2) having a carbon-carbon unsaturated bond other than maleic anhydride. The molecular weight of (a2) is 112 to 351, preferably 112 to 200. By being in this range, compatibility with polyimide resins and volatility during reaction are excellent.
[0037] Examples of (a2) include, but are not limited to, citraconic anhydride, itaconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, allylsuccinic anhydride, bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride, 2-buten-1-ylsuccinic anhydride, 1-cyclohexene-1,2-dicarboxylic anhydride, 7-oxabicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic anhydride, 3-methyl-4-cyclohexene-1,2-dicarboxylic anhydride, (2-methyl-2-propenyl)succinic anhydride, 4,9-decadiene-1,2-dicarboxylic anhydride, and 2,3-dimethylmaleic anhydride. Among these, citraconic anhydride, itaconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, and allylsuccinic anhydride are preferred from the viewpoint of improving adhesive strength, and citraconic anhydride, itaconic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride are more preferred. (a2) may be used alone or in combination of two or more kinds.
[0038] <Prepolymer with amino groups at the terminals> The prepolymer having an amino group at the end is a reaction product of a tetracarboxylic dianhydride (C) and a dimer diamine.
[0039] [Tetracarboxylic acid dianhydride (C)] The tetracarboxylic dianhydride (C) used in the present invention includes 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, 4,4'-[propane-2,2-diylbis(1,4-phenyleneoxy)]diphthalic acid, Dianhydrides, 2,2-bis(3,3',4,4'-tetracarboxyphenyl)tetrafluoropropane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2'-bis(3,4-dicarboxyphenoxyphenyl)sulfone dianhydride, 2,2',3,3'-biphenyltetracarboxylic acid dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, pyromellitic dianhydride, 1,2,3,4-benzenetetracarboxylic acid anhydride, 1,4,5 ,8-Naphthalenetetracarboxylic anhydride, 2,3,6,7-Naphthalenetetracarboxylic anhydride, 9,9'-Bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride, 9,9'-Bis(3,4-dicarboxyphenoxy)fluorene dianhydride, 1',2'-dianhydride; 4,4'-[4,4'-(propane-2,2-diyl)diphenoxy]diphthalic dianhydride, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene Phthalene-1,2-dicarboxylic anhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, bicyclo[2.2.2] Octane-2,3,5,6-tetracarboxylic acid 2,3:5,6-dianhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic acid dianhydride, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic acid anhydride, 7-methyl-4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydride, 7-tertiary butyl-4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydride, 7-tertiary butyl-4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydride, and the like are exemplified. The tetracarboxylic dianhydride (C) is not limited to the above, and may be used alone or in combination of two or more kinds.
[0040] The tetracarboxylic dianhydride (C) preferably contains fluorine or an alicyclic structure, since it has excellent compatibility with the curing assistant (B), adhesion, and dielectric properties. Specifically, 2,2-bis(3,3',4,4'-tetracarboxyphenyl)tetrafluoropropane dianhydride, 9,9-bis(trifluoromethyl)-9H-xanthene-2,3,6,7-tetracarboxylic acid 2,3:6,7-dianhydride, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride, and 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride are preferred. , 7-methyl-4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydride, 7-tert-butyl-4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydride, 7-tert-butyl-4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydride, and the like. Among these, 2,2-bis(3,3',4,4'-tetracarboxyphenyl)tetrafluoropropane dianhydride, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride, and 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride are more preferable in terms of improving adhesive strength and dielectric properties.
[0041] [Dimer diamine] Dimer diamine can be obtained, for example, by converting the carboxy group of a dimer acid into an amino group.
[0042] Dimer acid refers to the dimer of unsaturated aliphatic carboxylic acid or its hydrogenation product. For example, dimer acid can be obtained by dimerizing natural fatty acids such as soybean oil fatty acid, tall oil fatty acid, rapeseed oil fatty acid, or unsaturated fatty acids such as linoleic acid, linoleic acid, oleic acid, erucic acid, myristoleic acid, palmitoleic acid, sapienic acid, elaidic acid, stearolic acid, vaccenic acid, gadoleic acid, eicosenoic acid, brassidic acid, nervonic acid, eicosadienoic acid, docosadienoic acid, pinolenic acid, eleostearic acid, mead acid, dihomo-γ-linolenic acid, eicosatrienoic acid, stearidonic acid, arachidonic acid, eicosatetraenoic acid, cetoleic acid, adrenic acid, bosseopentaenoic acid, osbondo acid, sardine acid, tetracosapentaenoic acid, eicosapentaenoic acid, docosahexaenoic acid, and herring acid. The unsaturated bonds may be hydrogenated as necessary to reduce the degree of unsaturation. Dimer diamines and dimer diisocyanates with reduced degrees of unsaturation are suitable in terms of oxidation resistance (particularly coloring at high temperatures) and suppression of gelation during synthesis.
[0043] The dimer acid is preferably a compound having 20 to 60 carbon atoms, more preferably a compound having 24 to 56 carbon atoms, even more preferably a compound having 28 to 48 carbon atoms, and even more preferably a compound having 36 to 44 carbon atoms. A dicarboxylic acid compound having a branched structure obtained by Diels-Alder reaction of a fatty acid is preferable. The branched structure is preferably an aliphatic chain and a ring structure, more preferably a ring structure. The ring structure is preferably one or more aromatic rings and / or alicyclic structures, more preferably an alicyclic structure. When there are two ring structures, the two rings may be independent or continuous. One or more types of compounds can be used as the dimer diamine. The alicyclic structure may have one or more double bonds in the ring, or may have no double bonds. The method of converting the carboxy group of the dimer acid to an amino group includes, for example, a method of amidating the carboxylic acid, converting it to an amine by Hofmann rearrangement, and further distilling and purifying it. The carboxy group of the dimer acid can be converted to a diisocyanate group, for example, by converting a carboxylic acid into an isocyanate group through Curtius rearrangement.
[0044] The amino group in the dimer diamine may be directly bonded to the ring structure, but from the viewpoint of improving solubility and flexibility, it is preferable that the amino group is bonded to the ring structure via an aliphatic chain. The number of carbon atoms between the amino group and the ring structure is preferably 2 to 25. A suitable example of the aliphatic chain is a chain-like hydrocarbon group such as an alkylene group. A suitable example is a compound in which the two amino groups are bonded to the ring structure via an alkylene group.
[0045] Specific examples of dimer acids (polybasic acids) for obtaining dimer diamine include the following chemical formulas (d1) to (d4). These are only examples, and the dimer acid is not limited to the following structures.
[0046] [ka]
[0047] The dimer diamine is preferably a compound having 20 to 60 carbon atoms, more preferably a compound having 24 to 56 carbon atoms, even more preferably a compound having 28 to 48 carbon atoms, and still more preferably a compound having 36 to 44 carbon atoms. Such carbon numbers are preferred from the viewpoint of availability.
[0048] Commercially available dimer diamine products include, for example, "Priamine 1071", "Priamine 1073", "Priamine 1074", and "Priamine 1075" manufactured by Croda Japan Ltd., and "Versamin 551" manufactured by BASF Japan Ltd.
[0049] (Method of manufacturing prepolymer having amino group at the end) The reaction between the tetracarboxylic dianhydride (C) and the diamine can be carried out in an aprotic polar solvent by a known method. Examples of the aprotic polar solvent include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), methyldiglyme, cyclohexanone, and 1,4-dioxane. Only one type of aprotic polar solvent may be used, or two or more types may be mixed and used. In this case, there is no problem in mixing the above aprotic polar solvent with a nonpolar solvent that is compatible with it, and aromatic hydrocarbons such as toluene, xylene, mesitylene, and solvent naphtha are often used. The ratio of the nonpolar solvent in the mixed solvent is preferably 30% by mass or less. This is because if the nonpolar solvent is 30% by mass or more, the dissolving power of the solvent is improved and the polyamic acid is less likely to precipitate. The reaction between the tetracarboxylic dianhydride and the diamine component is preferably carried out by dissolving the well-dried diamine component in the above-mentioned reaction solvent which has been dehydrated and purified, and then adding the well-dried tetracarboxylic dianhydride thereto.
[0050] The reaction between the tetracarboxylic dianhydride (C) and the diamine may be either a random reaction or a block reaction. The reactants may be, for example, homogeneous reactants obtained by separately reacting each diamine component, mixed together, or the reactants may be further subjected to a recombination reaction in some cases. For example, an oligomer having an acid group at its terminal, which has been prepared in advance with an excess of tetracarboxylic dianhydride, and an oligomer having an amino group at its terminal, which has been prepared with an excess of diamine, may be mixed and further reacted.
[0051] <Other polyimide resins> Other polyimide resins using diamine compounds other than dimer diamine may also be included. The other polyimide resin can be obtained in the same manner as the polyimide resin (A) except that the dimer diamine is replaced with a diamine compound. By including the other polyimide resin, the heat resistance is improved.
[0052] (Diamine compounds) The diamine compound other than the dimer diamine may be used in combination with an aliphatic diamine, an aromatic diamine, an alicyclic diamine, etc., as exemplified below. In particular, from the viewpoint of heat resistance, an aromatic diamine or a diamine containing a phenol skeleton is preferred.
[0053] [ka]
[0054] [ka] (l is an integer from 1 to 3)
[0055] [ka]
[0056] [ka] The diamines that can be used in combination are not limited to those mentioned above, and two or more of them may be used in combination.
[0057] <Curing aid (B)> The curing auxiliary (B) is a compound that generates radicals, and an example of such a compound is a radical polymerization initiator.
[0058] The radical polymerization initiator may be a known compound. For example, peroxides such as benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di-t-butyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, di-t-butylperoxyisophthalate, t-butylperoxybenzoate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, trimethylsilyltriphenylsilylperoxide, and diisopropylbenzene hydroperoxide may be mentioned. In addition, 2,3-dimethyl-2,3-diphenylbutane is also suitable as a radical polymerization initiator.
[0059] The amount of the curing aid is in the range of 0.01 to 10 parts by mass, preferably 0.1 to 8 parts by mass, per 100 parts by mass of the polyimide resin (A). Within this range, the reaction proceeds smoothly and high adhesive strength can be achieved.
[0060] The curable resin composition of the present invention preferably contains, in addition to the polyimide resin (A) and the curing aid (B), at least one selected from the group consisting of a crosslinking agent, a curing accelerator, and an antioxidant.
[0061] <Crosslinking agent> The curable resin composition of the present invention may further contain a crosslinking agent in order to improve heat resistance and adhesion by forming crosslinks with the polyimide (A) or a phase separation structure. Examples of the crosslinking agent include epoxy compounds, cyanate compounds, maleimide compounds, allyl group-containing compounds, vinyl group-containing compounds, (meth)acryloyl group-containing compounds, metal chelate compounds, carbodiimide compounds, etc. In particular, from the viewpoint of adhesive strength, epoxy compounds, metal chelate compounds, and carbodiimide compounds are preferred, and the blending amount is 0.01 to 80 parts by mass, preferably 0.1 to 30 parts by mass, per 100 parts by mass of the polyimide resin (A). Within this range, high adhesive strength can be expressed.
[0062] (Epoxy compounds) The epoxy compound refers to a curable compound having an epoxy group. It is preferable to use the epoxy compound in combination with an active ester compound. The active ester compound refers to a compound that has one or more ester groups in one molecule that react with an epoxy group and cures an epoxy resin. Examples of commercially available active ester compounds include "HPC-8000-65T", "EXB9416-70BK" and "EXB8100-65T" manufactured by DIC Corporation.
[0063] By using an active ester compound, an ester group is generated by the reaction between the epoxy compound and the active ester compound. Therefore, the polarity can be lowered compared to the case where a phenol-based curing agent is used. As a result, the compatibility between the dimer structure of the polyimide resin (A) and the epoxy compound can be effectively increased.
[0064] Specific examples of epoxy compounds include glycidyl ether type epoxy resins; glycidyl amine type epoxy resins such as tetraglycidyl diaminodiphenylmethane, triglycidyl para-aminophenol, triglycidyl meta-aminophenol, tetraglycidyl meta-xylylenediamine, and sorbitol polyglycidyl ether; glycidyl ester type epoxy resins such as diglycidyl phthalate, diglycidyl hexahydrophthalate, and diglycidyl tetrahydrophthalate; cyclic aliphatic (alicyclic) epoxy resins such as epoxycyclohexylmethyl-epoxycyclohexanecarboxylate and bis(epoxycyclohexyl)adipate; bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, and bisphenol AD type epoxy resins. Other examples include cresol novolac type epoxy resins, phenol novolac type epoxy resins, α-naphthol novolac type epoxy resins, bisphenol A type novolac type epoxy resins, dicyclopentadiene type epoxy resins, tetrabromobisphenol A type epoxy resins, and brominated phenol novolac type epoxy resins.
[0065] (Cyanate compounds) The cyanate compound refers to a curable resin having a cyanate group. Examples of cyanate compounds include bisphenol A type cyanate ester resins, bisphenol A type cyanate esters, bisphenol F type cyanate ester resins, bisphenol E type cyanate ester resins, bisphenol S type cyanate ester resins, bisphenol sulfide type cyanate ester resins, phenylene ether type cyanate ester resins, naphthylene ether type cyanate ester resins, biphenyl type cyanate ester resins, tetramethylbiphenyl type cyanate ester resins, polyhydroxynaphthalene type cyanate ester resins, phenol novolac type cyanate ester resins, cresol novolac type cyanate ester resins, and tetramethylbiphenyl type cyanate ester resins. Examples of the cyanate ester resin include triphenylmethane type cyanate ester resin, tetraphenylethane type cyanate ester resin, dicyclopentadiene-phenol addition reaction type cyanate ester resin, phenol aralkyl type cyanate ester resin, naphthol novolac type cyanate ester resin, naphthol aralkyl type cyanate ester resin, naphthol-phenol co-condensed novolac type cyanate ester resin, naphthol-cresol co-condensed novolac type cyanate ester resin, aromatic hydrocarbon formaldehyde resin modified phenol resin type cyanate ester resin, biphenyl modified novolac type cyanate ester resin, and anthracene type cyanate ester resin.
[0066] Commercially available cyanate compounds, such as phenol novolac type cyanate ester resins ("PT-30" and "PT-60" manufactured by Lonza Japan), and prepolymers obtained by trimerizing bisphenol type cyanate ester resins ("BA-230S", "BA-3000S", "BTP-1000S", and "BTP-6020S" manufactured by Lonza Japan), may also be used.
[0067] (Maleimide compounds) A maleimide compound refers to a curable resin having a maleimide group. The type of maleimide compound is not particularly limited. From the viewpoint of long-term heat resistance, the average number of maleimide groups is preferably 1.5 to 4, and more preferably 2 or more.
[0068] The weight average molecular weight (Mw) of the maleimide compound is not particularly limited, but from the viewpoint of suppressing volatilization during drying, it is preferably 100 or more, and more preferably 150 or more. The upper limit of Mw is not particularly limited, but in consideration of availability, it is 8000 or less, more preferably 5000 or less.
[0069] The maleimide compound may be a polyfunctional maleimide obtained by reacting a polyfunctional amine with maleic anhydride. Examples of polyfunctional amines include isophorone diamine, dicyclohexylmethane-4,4'-diamine, and Huntsman Corporation's Jeffamine D-230, HK-511, D-400, XTJ-582, D-2000, XTJ-578, XTJ-509, XTJ-510, T-403, and T-5000 having an aminated polypropylene glycol backbone, and XTJ-500, XTJ-501, XTJ-502, XTJ-504, XTJ-511, XTJ-512, and XTJ-590 having an aminated polytetramethylene glycol backbone, and XTJ-542, XTJ-533, XTJ-536, XTJ-548, and XTJ-559 having an aminated polytetramethylene glycol backbone.
[0070] Maleimide compounds include 4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, bis-(3-ethyl-5-methyl-4-maleimidophenyl)methane, 4-methyl-1,3-phenylene bismaleimide, N,N'-ethylene dimaleimide, N,N'-hexamethylene dimaleimide, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3'-dimethyl-5, Resins with two maleimide groups in the molecule, such as 5'-diethyl-4,4'-diphenylmethane bismaleimide, bisphenol A diphenyl ether bismaleimide, biphenyl aralkyl type maleimide, polyphenylmethane maleimide (CAS NO: 67784-74-1, reaction product of a polymer of formaldehyde and aniline with maleic anhydride), N,N'-(toluene-2,6-diyl) bismaleimide, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis (3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, N,N'-ethylene bismaleimide, N,N'-trimethylene bismaleimide, N,N'-propylene bismaleimide, N,N'-tetramethylene bismaleimide, N,N'-pentamethylene bismaleimide, N,N'-(1,3-pentanediyl)bis(maleimide), N,N'-hexamethylene bismaleimide, N,N'-(1,7-heptanediyl)bismaleimide, N,N'-(1,8-octanediyl)bismaleimide dodecane, N,N'-(1,9-notanediyl)bismaleimide, N,N'-(1,10-decanediyl)bismaleimide, N,N'-(1,11-undecanediyl)bismaleimide, N,N'-(1,12-dodecanediyl)bismaleimide, N,N'-[(1,4-phenylene)bismethylene]bismaleimide, N,N'-[(1,2-phenylene)bismethylene]bismaleimide, N,N'-[(1,3-phenylene)bismethylene]bismaleimide, 1,6'-bismaleimido-(2,2,4-trimethyl)hexane, N,N'-[(methylimino)bis(4,1-phenylene)]bismaleimide, N,N'-(2-hydroxypropane-1,3-diylbisiminobiscarbonylbisethylene)bismaleimide, N,N'-(dithiobisethylene)bismaleimide, N,N'-[hexamethylenebis(iminocarbonylmethylene)]bismaleimide, N,N'-carbonylbis(1,4-phenylene)bismaleimide, N,N',N''-[nitrilotris(ethylene)]trismaleimide, N,N',N''-[nitrilotris(4,1-phenylene)]trismaleimide, N,N'-[p-phenylenebis(oxy-p-phenylene)]bismaleimide, N,N' -[Methylenebis(oxy)bis(2-methyl-1,4-phenylene)]bismaleimide, N,N'-[methylenebis(oxy-p-phenylene)]bis(maleimide) N,N'-[dimethylsilylenebis[(4,1-phenylene)(1,3,4,-oxadiazole-5,2-diyl)(4,1-phenylene)]]bismaleimide, N,N'-[(1,3-phenylene)bisoxybis(3,1 -phenylene)]bismaleimide, 1,1'-[3'-oxospiro[9H-xanthene-9,1'(3'H)-isobenzofuran]-3,6-diyl]bis(1H-pyrrole-2,5-dione), N,N'-(3,3'-dichlorobiphenyl-4,4'-diyl)bismaleimide, N,N'-(3,3'-dimethylbiphenyl-4,4'-diyl)bismaleimide, N,N'-(3,3'-dimethoxy Biphenyl-4,4'-diyl)bismaleimide, N,N'-[methylenebis(2-ethyl-4,1-phenylene)]bismaleimide, N,N'-[methylenebis(2,6-diethyl-4,1-phenylene)]bismaleimide, N,N'-[methylenebis(2-bromo-6-ethyl-4,1-phenylene)]bismaleimide, N,N'-[methylenebis(2-methyl-4,1-phenylene)]bismaleimide Imide, N,N'-[ethylenebis(oxyethylene)]bismaleimide, N,N'-[sulfonylbis(4,1-phenylene)bis(oxy)bis(4,1-phenylene)]bismaleimide, N,N'-[naphthalene-2,7-diylbis(oxy)bis(4,1-phenylene)]bismaleimide, N,N'-[p-phenylenebis(oxy-p-phenylene)]bismaleimide, N,N'-[(1,3-phenylene)bisoxybis(3,1-phenylene)]bismaleimide, N,N'-(3,6,9-trioxaundecane-1,11-diyl)bismaleimide, N,N'-[isopropylidenebis[p-phenyleneoxycarbonyl(m-phenylene)]]bismaleimide, N,N'-[isopropylidenebis[p-phenyleneoxycarbonyl(p-phenylene)]]bismaleimide, N,N'-[isopropylidenebis[(2,6-dichlorobenzene-4,1-diyl)oxycarbonyl(p-phenylene)]]bismaleimide, N, N'-[(phenylimino)bis(4,1-phenylene)]bismaleimide, N,N'-[azobis(4,1-phenylene)]bismaleimide, N,N'-[1,3,4-oxadiazole-2,5-diylbis(4,1-phenylene)]bismaleimide, 2,6-bis[4-(maleimido-N-yl)phenoxy]benzonitrile, N,N'-[1,3,4-oxadiazole-2,5-diylbis(3,1-phenylene)]bismaleimide, N,N'-[bis[9-oxo-9H-9-phospha(V)-10-oxaphenanthrene-9- N,N'-[hexafluoroisopropylidenebis[p-phenyleneoxycarbonyl(m-phenylene)]]bismaleimide, N,N'-[carbonylbis[(4,1-phenylene)thio(4,1-phenylene)]]bismaleimide, N,N'-carbonylbis(p-phenyleneoxy-p-phenylene)bismaleimide, N,N'-[5-tert-butyl-1,3-phenylenebis[(1,3,4-oxadiazole-5,2-diyl)(4,1-phenylene)]]bismaleimide , N,N'-[cyclohexylidenebis(4,1-phenylene)]bismaleimide, N,N'-[methylenebis(oxy)bis(2-methyl-1,4-phenylene)]bismaleimide, N,N'-[5-[2-[5-(dimethylamino)-1-naphthylsulfonylamino]ethylcarbamoyl]-1,3-phenylene]bismaleimide, N,N'-(oxybisethylene)bismaleimide, N,N'-[dithiobis(m-phenylene)]bismaleimide, N,N'-(3,6,9-trioxaundecane-1,11-diyl)bismaleimide, N,Examples of polyfunctional maleimides include N'-(ethylenebis-p-phenylene)bismaleimide, BMI-689, BMI-1500, BMI-1700, BMI-3000, BMI-5000, and BMI-9000 manufactured by Designer Molecules, and ODA-BMI and BAFBMI manufactured by JFE Chemical Corporation.
[0071] When the maleimide compound is crosslinked by radicals, a radical polymerization initiator can be added. Specific examples include azo compounds and organic peroxides. The polymerization initiators are used alone or in combination of two or more. Examples of azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane]. Examples of organic peroxides include benzoyl peroxide, t-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, t-butyl peroxy 2-ethylhexanoate, t-butyl peroxy neodecanoate, t-butyl peroxypivalate, (3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide.
[0072] (Allyl group-containing compounds) The allyl group-containing compound may be either monofunctional or polyfunctional. An example of a monofunctional allyl compound is (meth)allyl alcohol. An example of a polyfunctional allyl compound is triallyl isocyanurate, trimethylolpropane diallyl ether, trimethylolpropane triallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether, tetraallyloxyethane, polyallyl saccharose, di(meth)allyl phthalate, tri(meth)allyl isocyanurate, and tri(meth)allyl cyanurate. In addition, the following compounds may be mentioned. [ka]
[0073] (vinyl group-containing compound) The vinyl group-containing compound may be monofunctional or polyfunctional. Examples of monofunctional vinyl compounds include styrene, vinyltoluene, N-vinylpyrrolidone, N-vinylcaprolactam, vinylimidazole, and vinylpyridine. Examples of polyfunctional vinyl compounds include vinyl ethers such as hexanediol dinorbornene carboxylate, vinylbenzyl-modified polyphenylene ether, pentaerythritol tetranorbornene carboxylate, triethylene glycol divinyl ether, cyclohexane dimethanol divinyl ether, and cyclohexane diol divinyl ether, and divinylbenzene. Among these, vinyl group-containing polyphenylene ether is particularly preferred.
[0074] ((Meth)acryloxy group-containing compound) The (meth)acryloxy group-containing compound may be monofunctional or polyfunctional, and examples thereof include monofunctional (meth)acrylamide compounds, polyfunctional (meth)acrylamide compounds, monofunctional (meth)acrylate compounds, and polyfunctional (meth)acrylate compounds.
[0075] Examples of monofunctional (meth)acrylamide compounds include diacetone (meth)acrylamide, isobutoxymethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, t-octyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylamide, (meth)acryloylmorpholine, acrylamido-2-methylpropanesulfonic acid, and N-isopropyl (meth)acrylamide. Examples of polyfunctional (meth)acrylamide compounds include N,N'-diacryloyl-4,7,10-trioxa-1,13-tridecanediamine, N,N',N''-triacryloyldiethylenetriamine, N,N',N'',N'''-tetraacryloyltriethylenetetramine, and N,N'-{[2-acrylamido-2-[(3-acrylamidopropoxy)methyl]propane-1,3-diyl)bis(oxy)]bis(propane-1,3-diyl)}diacrylamide.
[0076] Monofunctional (meth)acrylate compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, cyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, (meth)acrylate of phenol alkylene oxide adduct, and p-cumyl phenol alkylene oxide adduct. (meth)acrylate of o-phenylphenol alkylene oxide adduct (meth)acrylate, nonylphenol alkylene oxide adduct (meth)acrylate, 2-methoxyethyl (meth)acrylate, ethoxyethoxyethyl (meth)acrylate, 2-ethylhexyl alcohol alkylene oxide adduct (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, caprolactone-modified tetrahydrofurfuryl (meth)acrylate, (2-ethyl-2-methyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (2-isobutyl-2-methyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (1,4-dioxaspiro[4,5]decan-2-yl)methyl (meth)acrylate, glycidyl (meth)acrylate, 3,Examples of the acrylate include 4-epoxycyclohexylmethyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, 2-(meth)acryloyloxyethyl isocyanate, allyl (meth)acrylate, N-(meth)acryloyloxyethyl hexahydrophthalimide, N-(meth)acryloyloxyethyl tetrahydrophthalimide, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl succinic acid, ω-carboxy-polycaprolactone mono(meth)acrylate, 2-(meth)acryloyloxyethyl acid phosphate, 3-(meth)acryloyloxypropyl trimethoxysilane, 3-(meth)acryloyloxypropyl dimethoxymethylsilane, 3-(meth)acryloyloxypropyl triethoxysilane, and 2-(meth)acryloyloxyethyl acid phosphate. In the alkylene oxide adduct, examples of the alkylene oxide include ethylene oxide and propylene oxide.
[0077] Polyfunctional (meth)acrylate compounds include methacrylate group-containing polyphenylene ethers, di(meth)acrylates of aliphatic diols such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 2-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, and 1,9-nonanediol di(meth)acrylate; Di(meth)acrylates of alicyclic diols such as cyclohexanedimethylol di(meth)acrylate and tricyclodecanedimethylol di(meth)acrylate; Alkylene glycol di(meth)acrylates such as diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; Esterification reaction product of neopentyl glycol, hydroxypivalic acid, and (meth)acrylic acid (hereinafter referred to as "hydroxypivalic acid neopentyl glycol di(meth)acrylate"), caprolactone-modified hydroxypivalic acid neopentyl glycol di(meth)acrylate; Di(meth)acrylates of alkylene oxide adducts of bisphenol compounds, such as di(meth)acrylates of alkylene oxide adducts of bisphenol A; Di(meth)acrylates of hydrogenated bisphenol compounds, such as di(meth)acrylate of hydrogenated bisphenol A; poly(meth)acrylates of isocyanuric acid alkylene oxide adducts, such as di(meth)acrylates of isocyanuric acid alkylene oxide adducts, tri(meth)acrylates of isocyanuric acid alkylene oxide adducts, di(meth)acrylates of caprolactone-modified isocyanuric acid alkylene oxide adducts, and tri(meth)acrylates of caprolactone-modified isocyanuric acid alkylene oxide adducts; Polyol poly(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri- or tetra(meth)acrylate, dipentaerythritol penta- or hexa(meth)acrylate; Poly(meth)acrylates of polyol alkylene oxide adducts such as tri(meth)acrylate of trimethylolpropane alkylene oxide adduct, tetra(meth)acrylate of ditrimethylolpropane alkylene oxide adduct, tri- or tetra(meth)acrylate of pentaerythritol alkylene oxide adduct, penta- or hexa(meth)acrylate of dipentaerythritol alkylene oxide adduct: Urethane (meth)acrylates; epoxy (meth)acrylates; and An example is polyester (meth)acrylate. In the alkylene oxide adduct, examples of the alkylene oxide include ethylene oxide and propylene oxide.
[0078] (Metal chelate compounds) The metal chelate compound is an organometallic compound consisting of a metal and an organic substance, which reacts with the reactive functional group of the polyimide resin (A) to form a crosslink. The type of organometallic compound is not particularly limited, and examples thereof include organoaluminum compounds, organotitanium compounds, and organozirconium compounds. The bond between the metal and the organic substance may be a metal-oxygen bond, and is not limited to a metal-carbon bond. In addition, the bond between the metal and the organic substance may be any of a chemical bond, a coordinate bond, and an ionic bond. Furthermore, it is preferable that the compound has three or more functional groups from the viewpoint of heat resistance.
[0079] The organic aluminum compound is preferably an aluminum metal chelate compound.Examples of the aluminum metal chelate compound include ethyl acetoacetate aluminum diisopropylate, aluminum tris(ethyl acetoacetate), alkyl acetoacetate aluminum diisopropylate, aluminum monoacetylacetonate bis(ethyl acetoacetate), aluminum tris(acetylacetate), aluminum monoacetylacetate bis(ethyl acetoacetate), aluminum di-n-butoxide monomethyl acetoacetate, aluminum diisobutoxide monomethyl acetoacetate, aluminum di-sec-butoxide monomethyl acetoacetate, aluminum isopropylate, monosec-butoxy aluminum diisopropylate, aluminum sec-butyrate, aluminum ethylate, etc.
[0080] The organic titanium compound is preferably a titanium metal chelate compound.Titanium metal chelate compounds include, for example, titanium acetylacetonate, titanium tetraacetylacetonate, titanium ethylacetoacetate, titanium octylene glycolate, titanium ethylacetoacetate, titanium-1.3-propanedioxybis(ethylacetoacetate), polytitanium acetylacetonate, tetraisopropyl titanate, tetranormalbutyl titanate, butyl titanate dimer, tetraoctyl titanate, dashalyamyl titanate, tetratertiarybutyl titanate, tetrastearyl titanate, titanium isostearate, tri-n-butoxy titanium monostearate, di-i-propoxy titanium distearate, titanium stearate, di-i-propoxy titanium diisostearate, (2-n-butoxycarbonylbenzoyloxy)tributoxy titanium, etc. The organic zirconium compound is preferably a zirconium metal chelate compound. Examples of the zirconium metal chelate compound include zirconium tetraacetylacetonate, zirconium tributoxy acetylacetonate, zirconium monobutoxy acetylacetonate bis(ethylacetoacetate), zirconium dibutoxy bis(ethylacetoacetate), zirconium tetraacetylacetonate, normal propyl zirconate, normal butyl zirconate, zirconium stearate, zirconium octylate, etc. Among these, organic titanium compounds and organic zirconium compounds are preferred from the viewpoint of thermosetting reactivity.
[0081] (Carbodiimide group-containing compound) The carbodiimide group-containing compound is not particularly limited as long as it has a carbodiimide group in the molecule. Examples of the carbodiimide group-containing compound include Carbodilite V-01, V-03, V-05, V-07, and V-09 (Nisshinbo Chemical Inc.), and cyclic carbodiimide (Teijin Ltd.). From the viewpoint of heat resistance, it is preferable to have an average of three or more carbodiimide groups in one molecule.
[0082] The crosslinking agent is not limited to the above, and other than these, phenol resins and compounds containing an isocyanate group may also be used, and two or more of them may be used in combination.
[0083] The content of the crosslinking agent is preferably 0.1 to 20% by mass relative to 100% by mass of the non-volatile content of the polyimide resin (A), which further improves the adhesive strength and heat resistance.
[0084] <Antioxidants> The curable resin composition of the present invention may contain an antioxidant. The antioxidant can prevent yellowing due to oxidation during thermal curing and suppress deterioration of the dielectric properties of the coating.
[0085] The antioxidant is a compound having a radical scavenging function or a peroxide decomposition function. Examples of the antioxidant include hindered phenol compounds, hindered amine compounds, phosphorus compounds, sulfur compounds, and hydroxylamine compounds. The antioxidant is preferably a compound that does not contain a halogen atom.
[0086] Examples of the hindered phenol compounds include 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,1,3-tris-(2'-methyl-4'-hydroxy-5'-t-butylphenyl)-butane, 4,4'-butylidene-bis-(2-t-butyl-5-methylphenol), 3-(3,5-di-t-butyl-4-hydroxyphenyl)stearyl propionate, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 3,9-bis[2-[3-(3-t-butyl-4-hydroxy-5 -methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3,5-tris(3,5-di-t-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene, 1,3,5-tris(3-hydroxy-4-t-butyl-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,2'-methylenebis(6-t-butyl-4-ethylphenol), 2,2'-thiodiethylbis-(3,5-di-t-butyl-4-hydroxyphenylmethyl)- bis(3-(3-methyl-4-hydroxy-5-t-butylphenyl)propionate, N,N-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), i-octyl 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,6-bis(dodecylthiomethyl)-o-cresol, calcium salt of 3,5-di-t-butyl-4-hydroxybenzylphosphonic acid monoethyl ester, 4,6-bis(octylthiomethyl)-o-cresol, bis[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propionic acid]ethylenebisoxybisethylene, 1,6-Hexanediol bis[3-(3,5-di-t-butyl-4-hydroxyphenyl propionate, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3 ,5-di-t-butylanilino)-1,3,5-triazine, 2,2'-thio-bis-(6-t-butyl-4-methylphenol), 2,5-di-t-amyl-hydroquinone, 2,6-di-t-butyl-4-nonylphenol, 2,2'-isobutylidene-bis-(4,6-dimethyl-phenol), 2,2'-methylene-bis-(6-(1-methyl-cyclohexyl)-p-cresol), 2,4-dimethyl-6-(1-methyl-cyclohexyl)-phenol, and the like.
[0087] Commercially available products include ADK STAB AO-20, AO-30, AO-40, AO-50, AO-60, AO-80, and AO-330 manufactured by ADEKA CORPORATION; KEMINOX 101, 179, 76, and 9425 manufactured by Chemipro Corporation; IRGANOX 1010, 1035, 1076, 1098, 1135, 1330, 1726, 1425WL, 1520L, 245, 259, 3114, 5057, and 565 manufactured by BASF Corporation; and Cyanox CY-1790 and CY-2777 manufactured by Sun Chemical Corporation.
[0088] Examples of the hindered amine compound include tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)1,2,3,4-butane tetracarboxylate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)1,2,3,4-butane tetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, 1,2,2,6,6-pentamethoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, and 1,2,2,6,6-pentamethoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate. 2,2,6,6-tetramethyl-4-piperidyl methacrylate, polycondensation product of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine, poly[[6-[(1,1,3,3-tetramethylbutyl)amino]-s-triazine-2,4-diyl]-[(2,2,6,6-tetramethyl-4-piperidyl)imino]-hexamethylene-[(2,2,6,6-tetramethyl-4-piperidyl)imino]], 4-hydroxy-2,2,6,6-tetramethyl-1-pi Ester of peridineethanol with 3,5,5-trimethylhexanoic acid, N,N'-4,7-tetrakis[4,6-bis{N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino}-1,3,5-triazin-2-yl]-4,7-diazadecane-1,10-diamine, decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl)ester, reaction products of 1,1-dimethylethyl hydroperoxide with octane, bis(1,2,2,6,6-pentamethyl-4-pyridyl)[[3,5-bi 1,2,2,6,6-pentamethyl-4-pyridyl sebacate, poly[[6-morpholino-s-triazine-2,4-diyl]-[(2,2,6,6-tetramethyl-4-piperidyl)imino]-hexamethylene-[(2,2,6,6-tetramethyl-4-piperidyl)imino]], 2,2,6,6-tetramethyl-4-piperidyl-C12-21 and C18 unsaturated fatty acid esters, N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl)-1,6-Hexamethylenediamine, 2-methyl-2-(2,2,6,6-tetramethyl-4-piperidyl)amino-N-(2,2,6,6-tetramethyl-4-piperidyl)propionamide, etc.
[0089] Commercially available products include ADKA STAB LA-52, LA-57, LA-63P, LA-68, LA-72, LA-77Y, LA-77G, LA-81, LA-82, LA-87, LA-402F, and LA-502XP manufactured by ADEKA Corporation; KAMISTAB 29, 62, 77, and 94 manufactured by Chemipro Chemicals; Tinuvin 249, TINUVIN 111FDL, 123, 144, 292, and 5100 manufactured by BASF; and Cyasorb UV-3346, UV-3529, and UV-3853 manufactured by Sun Chemical.
[0090] Examples of phosphorus compounds include di(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, 2,2'-methylenebis(4,6-di-t-butylphenyl)2-ethylhexyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, tris(nonylphenyl)phosphite, tetra(C12-C15 alkyl)-4,4'-isopropylidenediphenyl diphosphite, diphenyl mono(2- ethylhexyl) phosphite, diphenyl isodecyl phosphite, tris(isodecyl) phosphite, triphenyl phosphite, tetrakis(2,4-di-t-butylphenyl)-4,4-biphenyl diphosphonate, tris(tridecyl) phosphite, phenyl isooctyl phosphite, phenyl isodecyl phosphite, phenyl di(tridecyl) phosphite, diphenyl isooctyl phosphite, diphenyl tridecyl phosphite, 4,4'-isopropylidene Diphenol alkyl phosphite, trisnonylphenyl phosphite, trisdinonylphenyl phosphite, tris(biphenyl) phosphite, di(2,4-di-t-butylphenyl)pentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, tetratridecyl 4,4'-butylidenebis(3-methyl-6-t-butylphenol) diphosphite, hexatridecyl Examples of such phosphite include 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane triphosphite, 3,5-di-t-butyl-4-hydroxybenzyl phosphite diethyl ester, sodium bis(4-t-butylphenyl)phosphite, sodium-2,2-methylene-bis(4,6-di-t-butylphenyl)-phosphite, 1,3-bis(diphenoxyphosphonyloxy)-benzene, and ethyl bis(2,4-ditert-butyl-6-methylphenyl)phosphite.
[0091] Commercially available products include Adeka STAB PEP-36, PEP-8, HP-10, 2112, 1178, 1500, C, 135A, 3010, and TPP manufactured by ADEKA Corporation, IRGAFOS168 manufactured by BASF, and HostanoxP-EPQ manufactured by Clariant Chemicals.
[0092] Examples of sulfur-based compounds include 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diylbis[3-(dodecylthio)propionate], ditridecyl 3,3'-thiobispropionate, 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,4-bis[(octylthio)methyl]-o-cresol, and 2,4-bis[(laurylthio)methyl]-o-cresol.
[0093] Commercially available products include Adeka STAB AO-412S and AO-503 manufactured by ADEKA Corporation, and KEMINOXPLS manufactured by Chemipro Chemicals.
[0094] The antioxidants can be used alone or in combination of two or more.
[0095] The content of the antioxidant is preferably 0.1 to 1 mass % relative to 100 mass % of the nonvolatile content of the polyimide resin (A), which further improves the adhesive strength, dielectric constant, and dielectric loss tangent.
[0096] <Curing accelerator> The curable resin composition of the present invention may contain a curing accelerator for the purpose of efficiently promoting the curing process. The addition of the curing accelerator lowers the curing temperature and prevents the resin from being oxidized and deteriorated, thereby improving the dielectric properties. Suitable examples of the curing accelerator include imidazole-based catalysts, amine-based catalysts, and phosphorus-based catalysts.
[0097] The curing accelerator is preferably an amine catalyst. For example, dimethylcyclohexylamine, N-methyldicyclohexylamine, triethylamine, tripropylamine, tributylamine, N-methylmorpholine, N-ethylmorpholine, N-dimethylbenzylamine, and other non-reactive monoamines, triethylenediamine, tetramethylhexamethylenediamine, bisdimethylaminoethylether, tetramethylpropanediamine, dimethylaminoethylmorpholine, tetramethylethylenediamine, diazabicycloundecene, 2-methyl-1,4-diazo[2.2.2]bicyclooctane, and other non-reactive diamines, pentamethyldiethylenetriamine, pentamethyldipropylenetriamine, and other non-reactive triamines, dimethylethanolamine, N-trioxyethylene-N,N-dimethylamine, N,N-dimethyl-N-hexanolamine, and other reactive amines, may be mentioned. These compounds may be used alone or in combination of two or more.
[0098] The content of the curing accelerator is preferably 0.1 to 5% by mass, particularly preferably 0.1 to 1% by mass, relative to 100% by mass of the nonvolatile content of the polyimide resin (A). When the content is within the above range, the dielectric properties and adhesive strength are most improved.
[0099] <Filler> The curable resin composition of the present invention preferably further contains a filler. By containing the filler, the dielectric properties can be improved. The filler may be either an inorganic filler or an organic filler, and an inorganic filler is more preferable.
[0100] The content of the filler may be appropriately adjusted depending on the application, and is usually 5 to 95% by mass relative to 100% by mass of the non-volatile content of the curable resin composition. The shape of the filler is not particularly limited. For example, spherical, powdery, fibrous, needle-like, scaly, etc. may be mentioned. By using multiple types of fillers with different particle sizes and shapes, it may be possible to highly fill the filler. The filler may be used alone or in combination of two or more types.
[0101] Specific examples of inorganic fillers include alumina, aluminum hydroxide, zirconium hydroxide, barium hydroxide, calcium hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, zinc carbonate, barium carbonate, magnesium sulfate, titanium oxide, tin oxide, aluminum oxide, magnesium oxide, zirconium oxide, calcium oxide, magnesium oxide, zinc oxide, molybdenum oxide, antimony oxide, nickel oxide, calcium silicate, beryllia, calcium titanate, silicon carbide, silicon nitride, aluminum nitride, boron nitride, and titanium white. Examples of fillers include metal compounds such as zinc borate and aluminum borate; talc; clay; mica; metal oxides and metal nitrides such as glass fiber, kaolin, hydrotalcite, wollastonite, xonotlite, calcium hydrogen phosphate, calcium phosphate, glass flakes, hydrated glass, and sepiolite; hydrated metal compounds; silica-based fillers such as fused crushed silica, fused spherical silica, crystalline silica, non-crystalline silica, secondary agglomerated silica, fine silica, hollow silica, and porous silica; and nitride-based and carbon-based fillers such as silicon carbide, silicon nitride, titanium carbide, and diamond. Among these, alumina, aluminum oxide, aluminum nitride, and boron nitride are more preferable, and among these, boron nitride is particularly preferable from the viewpoint of effectively improving the dielectric properties.
[0102] In addition, fillers in which the surface of the inorganic fillers listed above is coated with a resin or a dispersant may be used. In the present invention, the surface-coated inorganic fillers are classified as inorganic fillers. As a method for coating the surface of the inorganic filler with a resin or a dispersant, a known method can be applied. The surface of the inorganic filler can be surface-treated with, for example, a silane-based, titanate-based, or aluminate-based coupling agent. The surface treatment can increase the dispersibility of the inorganic filler in the binder component, and can efficiently improve the dielectric properties. In addition, the interfacial adhesive strength between the binder component and the filler can also be increased.
[0103] Specific examples of organic fillers include fluorine fillers: polytetrafluoroethylene powder and modified products thereof, tetrafluoroethylene-perfluoroalkyl vinyl ether powder, tetrafluoroethylene-ethylene powder, tetrafluoroethylene-hexafluoropropylene powder, tetrafluoroethylene-vinylidene fluoride powder, tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether powder, polychlorotrifluoroethylene powder, chlorotrifluoroethylene-ethylene powder, chlorotrifluoroethylene-vinylidene fluoride powder, polyvinylidene fluoride powder, and polyvinyl fluoride powder. In addition to polyethylene powder, polyacrylic ester powder, epoxy resin powder, polyamide powder, polyimide powder, polyurethane powder, liquid crystal polymer beads, polysiloxane powder, etc., polymer fillers such as multi-layered core-shell structures using silicone, acrylic, styrene-butadiene rubber, butadiene rubber, etc.; (poly)phosphate compounds such as melamine phosphate, melamine polyphosphate, guanidine phosphate, guanidine polyphosphate, ammonium phosphate, ammonium polyphosphate, ammonium amide phosphate, ammonium polyphosphate, carbamate phosphate, carbamate polyphosphate, organic phosphate compounds, phosphazenes, etc. phosphorus-based fillers such as compounds, phosphonic acid compounds, phosphinic acid compounds such as aluminum diethylphosphinate, aluminum methylethylphosphinate, aluminum diphenylphosphinate, aluminum ethylbutylphosphinate, aluminum methylbutylphosphinate, and polyethylene aluminum phosphinate, phosphine oxide compounds, phosphorane compounds, and phosphoramide compounds; and nitrogen-based fillers such as benzoguanamine, melamine, melam, melem, melon, melamine cyanurate, cyanuric acid compounds, isocyanuric acid compounds, triazole compounds, tetrazole compounds, diazo compounds, and urea.
[0104] Examples of silane coupling agents include aminosilanes such as γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane; epoxysilanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercaptosilanes such as 3-mercaptopropyltrimethoxysilane; and vinylsilanes such as p-styryltrimethoxysilane, vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane.
[0105] Examples of titanate coupling agents include isopropyl triisostearoyl titanate, isopropyl tri(N-aminoethyl aminoethyl) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, diisopropyl bis(dioctyl phosphate) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, and tetraoctyl bis(ditridecyl phosphite) titanate.
[0106] Also, a preferred embodiment is one in which the surface of the inorganic filler is coated with a fluorine-based resin.
[0107] The method of adding the filler is not particularly limited, and a conventionally known method can be used. Suitable examples include a method of adding the filler to a polymerization reaction solution before or during polymerization of the polyimide resin (A), a method of kneading the filler into the polyimide resin (A) using a three-roll mill, and a method of preparing a dispersion containing the filler and mixing it into the polyimide resin (A). In addition, in order to disperse the filler well and stabilize the dispersion state, a dispersant, a thickener, etc. can also be used within a range that does not affect the physical properties of the resin composition.
[0108] <Other additives> The curable resin composition of the present invention may further contain additives such as an ultraviolet absorber, a hydrolysis inhibitor, an antifungal agent, a thickener, a plasticizer, a pigment, a photoinitiator, etc. as necessary. In addition, the curable resin composition may be solvent-free or may contain a solvent.
[0109] Examples of the solvent include toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-pyrrolidone, acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, n-hexane, cyclohexane, cyclohexanone, and mixtures thereof.
[0110] <Laminated sheets and prepregs> The laminate sheet of the present invention has a substrate and a resin composition layer formed from the curable resin composition of the present invention. The resin composition layer exhibits excellent adhesiveness after curing treatment, and is therefore suitable for use in bonding various materials (resin layers, metal layers, inorganic layers such as ITO, composite layers, etc.) For example, it is suitable as an adhesive sheet for copper clad laminates (CCL), and as a bonding material between components such as electronic circuit boards and electronic components.
[0111] Examples of the substrate include resin materials such as polyimide film, polyethylene film, polycarbonate, polyethylene, liquid crystal polymer, phenolic resin, and aramid resin; metal materials such as copper, aluminum, and stainless steel; inorganic materials such as ITO, glass, silicon, and silicon carbide, and composite materials in which any of these materials are combined. In addition, the substrate may be a peelable substrate in which the surface of the resin material is treated for easy peeling. By using the polyimide resin (A) of the present curable resin composition, the adhesive strength to various substrates, the dielectric properties, and the heat resistance are excellent.
[0112] The method for producing the laminated sheet is not particularly limited, but for example, the laminated sheet can be obtained by applying a coating liquid (varnish) of the present curable resin composition containing an organic solvent to one side of a release substrate, and removing and drying the liquid medium such as the organic solvent by heating. By laminating another release substrate on the surface of the obtained adhesive sheet, a laminated sheet that is an adhesive sheet with double-sided release substrates can be obtained. By laminating both sides with release substrates, surface contamination of the adhesive sheet can be prevented. The adhesive sheet can be isolated by peeling off the release substrate. The two release substrates can be either the same or different. By using release substrates with different release properties, the peeling force can be made stronger or weaker, making it easier to peel them off in order. In addition, a laminated sheet having an adhesive sheet (resin composition layer) may be obtained by applying a coating liquid to a substrate other than the release substrate.
[0113] The coating method may be selected from known methods such as comma coating, knife coating, die coating, lip coating, roll coating, curtain coating, bar coating, gravure printing, flexographic printing, screen printing, dip coating, spray coating, spin coating, etc. In order to ensure sufficient adhesiveness and from the standpoint of ease of handling, the thickness of the adhesive sheet after drying is preferably 5 to 500 μm, more preferably 10 to 100 μm.
[0114] The present curable resin composition can also be suitably used for forming a prepreg obtained by impregnating a substrate with the present curable resin composition. The prepreg can be produced, for example, by impregnating a fiber substrate with the present curable resin composition, and then heating and drying the resin composition to semi-cure (B-stage). The solid content of the resin composition attached to the fiber substrate is preferably 20 to 90 mass% in terms of the content of the resin composition after drying relative to the prepreg. More preferably, it is 30 to 80 mass%, and even more preferably, it is 40 to 70 mass%. For example, the present curable resin composition can be impregnated or coated on a fiber substrate so that the solid content of the resin composition in the prepreg is 20 to 90 mass%, and then the prepreg can be semi-cured (B-staged) by, for example, heating and drying at a temperature of 40 to 250°C for 1 to 30 minutes.
[0115] As the fiber substrate, known materials can be used without limitation, and examples thereof include organic fibers, inorganic fibers, and glass fibers. Examples of organic fibers include polyimide, polyester, tetrafluoroethylene, and fully aromatic polyamide. Examples of inorganic fibers include carbon fibers. Examples of glass fibers include E-glass cloth, D-glass cloth, S-glass cloth, Q-glass cloth, NE-glass cloth, L-glass cloth, T-glass cloth, spherical glass cloth, and low dielectric glass cloth. Among these, from the viewpoint of low thermal expansion coefficient, E-glass cloth, T-glass cloth, S-glass cloth, Q-glass cloth, and organic fibers are suitable. The fiber substrate may be used alone or in combination of two or more types.
[0116] The shape of the fiber substrate can be appropriately selected depending on the intended use and performance. Specific examples include woven fabric, nonwoven fabric, roving, chopped strand mat, and surfacing mat. Examples of the weaving method of the woven fabric include plain weave, sash weave, and twill weave. It can be arbitrarily selected and designed depending on the desired characteristics. The thickness of the fiber substrate can be, for example, in the range of about 0.01 to 1.0 mm. From the viewpoint of thinning, it is preferably 500 μm or less, more preferably 300 μm or less.
[0117] If necessary, the fiber substrate may be surface-treated with a silane coupling agent or mechanically opened to bring out desired properties. Corona treatment or plasma treatment may also be performed. Surface treatments using silane coupling agents include aminosilane coupling treatment, vinylsilane coupling treatment, cationic silane coupling treatment, and epoxysilane coupling treatment.
[0118] The method of impregnating the fiber substrate with the resin composition is not particularly limited, but examples include a method of preparing a varnish of the resin composition using an organic solvent such as alcohols, ethers, acetals, ketones, esters, alcohol esters, ketone alcohols, ether alcohols, ketone ethers, ketone esters, or ester ethers, and immersing the fiber substrate in the varnish, a method of coating or spraying the varnish onto the fiber substrate, or a method of laminating both sides of the fiber substrate with a film made of the resin composition.
[0119] Furthermore, a resin composition layer formed from the present curable resin composition, a cured product layer thereof, etc. are suitable for use as an insulating layer for a semiconductor chip package, an underfill material, an adhesive material, etc. They are also suitable as a composition for a copper-clad laminate, a bonding sheet for forming a wiring board, and a cover coat for a flexible substrate.
[0120] (Method of producing the cured product) A cured product is obtained by curing the curable resin composition. When a thermosetting compound is contained, the composition is usually cured by a heat curing process, and when a photocurable compound is contained, the composition is usually cured by a light irradiation process. For example, the resin composition is molded into a desired shape such as a sheet and cured. A molded product such as a sheet of the resin composition can be easily obtained by applying a resin composition containing a solvent and drying it. Then, the molded product is cured to form a cured product. The timing of the molding and the curing may be simultaneous. The sheet-shaped cured product is also called a cured layer.
[0121] The temperature for the thermal curing treatment may be appropriately selected depending on the type of crosslinking agent. For example, a method of heat treatment at a temperature of 150 to 300°C for 30 to 180 minutes may be exemplified. In the photocuring treatment, active light may be irradiated at an intensity sufficient for curing. During curing, pressure may be applied (for example, 5 MPa) for thermocompression bonding as necessary. A crosslinked structure is formed in the curable resin composition by the curing treatment, and a three-dimensionally crosslinked cured product is obtained.
[0122] <Substrate with cured product and electronic device> The substrate with a cured product of the present invention is a substrate having a cured product of a curable resin composition. Specific examples thereof include a metal-clad laminate and a printed wiring board having a cured product of a curable resin composition. The cured product of the present curable resin composition is preferable because it has excellent heat resistance, adhesive strength and dielectric properties.
[0123] The metal-clad laminate can be obtained, for example, by forming an insulating layer using the present curable resin composition, and laminating the insulating layer and a metal layer. For example, a metal layer and a prepreg formed using the present curable resin composition are laminated, and then a curing process is performed by hot pressing to obtain a metal-clad laminate. The hot pressing process can be performed by a known method. For example, the hot pressing process is performed by hot pressing at a temperature of 120 to 250°C and a pressure of 0.5 to 10 MPa for 0.5 to 5 hours.
[0124] Examples of the laminated structure of the metal-clad laminate include a two-layer laminate of a metal layer / cured layer, a laminate consisting of multiple layers of a metal layer / cured layer / metal layer, or a metal-clad laminate having a multi-layer structure in which metal layer / cured layer / metal layer / cured layer / metal layer are alternately laminated. In addition, an insulating layer other than the cured layer formed from the present curable resin composition may be included in the laminate, and multiple sheets of prepreg or the like may be stacked and cured to adjust the thickness of the cured layer. In addition, a conductive layer other than the metal layer may be laminated.
[0125] For example, a metal-clad laminate having a layer structure of metal layer / hardened layer / metal layer can be obtained by forming a circuit pattern on the metal layer formed on both main surfaces of the hardened layer to obtain a circuit board having a circuit pattern layer. A through hole or via may be formed in the hardened layer by a laser or the like. A core board may be laminated with an insulating hardened layer by a build-up process to form a via and to form a multi-layer structure. The circuit board can be obtained, for example, by forming the metal layer of the metal-clad laminate into a desired circuit pattern by a subtractive method, or by forming a desired circuit pattern on one or both sides of the insulating layer by an additive method.
[0126] Copper foil or the like is used as the metal layer. In the case of a copper-clad laminate, a step is performed in which electrolytic copper plating is performed on the copper foil surface, and then etching is performed with an alkaline or other plating solution after removing the resist layer. The present curable resin composition has excellent substrate processing suitability such as plating solution resistance, and is therefore suitable for use in copper-clad laminates. Furthermore, the present cured product has excellent crack resistance and heat resistance after a heat cycle test of the cured product, and therefore a substrate with the cured product, including the cured product formed by curing the present curable resin composition, can be used for a wide range of applications under various environments.
[0127] The printed wiring board can be manufactured, for example, by processing the copper foil in a copper-clad laminate by etching or the like, forming a signal circuit or the like, bonding the substrate and cover film via an adhesive sheet, and carrying out a curing process or the like. In addition, for example, a flexible printed wiring board can be manufactured by forming a conductor pattern on an insulating flexible film, forming a protective film thereon via the adhesive sheet, and carrying out a process of thermocompression bonding or the like. Examples of the flexible film include polyester, polyimide, liquid crystal polymer, and PTFE film. Examples of the conductor pattern include a method of forming the conductor pattern by printing technology, and a method of sputtering and plating.
[0128] The cured layer of the present curable resin composition formed on one or both sides of the printed wiring board may be provided with an opening by drilling or laser processing, and filled with a conductive agent to form a via. A circuit layer may also be formed on the cured layer of the present curable resin composition. The cured product of the present curable resin composition has excellent plating solution resistance, and is therefore suitable for the manufacture of multi-layer printed wiring boards. The printed wiring board formed using the present curable resin composition has excellent processability, and is excellent in heat resistance and crack resistance after a heat cycle test, and is therefore suitable for various electronic devices such as smartphones and tablet terminals.
[0129] The polyimide resin (A) of the present curable resin composition has excellent dielectric properties, and therefore can provide a cured product with excellent insulation. For example, it is preferably used as an insulating layer forming material on a circuit board (including a coverlay layer of a printed wiring board, an interlayer insulating layer of a built-up board, a bonding sheet, etc.). In addition, by using a conductive material in a filler such as a thermally conductive filler, it can also be used as a conductive member of an electronic component. Examples of electronic components include power modules such as power semiconductor devices, LEDs, and inverter devices.
[0130] Furthermore, by blending a thermally conductive filler with the cured product of the present curable resin composition, it can be applied to all applications requiring heat dissipation. For example, by utilizing the moldability of the resin composition, it can be suitably used as a heat dissipation part of a desired shape. In particular, it is useful as a heat dissipation adhesive or heat dissipation sheet for electronic devices (smartphones, tablet terminals, etc.) that cannot be equipped with a fan or heat sink due to the need for light, thin, short, and small size, and for battery exterior materials, because of the need for heat dissipation adhesive or heat dissipation sheet for battery exterior materials. In addition, the cured product of the present curable resin composition is suitable as an adhesive layer between a heating element and a heat sink, or as a heat spreader. In addition, it can be applied as a heat dissipation layer that covers one or more electronic components mounted on a substrate. EXAMPLES
[0131] The present invention will be described in more detail below with reference to examples and comparative examples. In the examples and comparative examples, parts and % mean parts by mass and % by mass unless otherwise specified.
[0132] <Method of measuring mass average molecular weight (Mw)> The Mw was measured using a GPC (gel permeation chromatography) "HPC-8020" manufactured by Tosoh Corporation. GPC is a liquid chromatography that separates and quantifies substances dissolved in a solvent (THF; tetrahydrofuran) based on the difference in their molecular size. The measurement in the present invention was performed using two "LF-604" columns (manufactured by Showa Denko K.K.: GPC column for rapid analysis: 6 mm ID x 150 mm size) connected in series, at a flow rate of 0.6 ml / min and a column temperature of 40°C, and the mass average molecular weight (Mw) was determined in polystyrene equivalent.
[0133] (Synthesis Example 1) Production of polyimide resin (1) In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank and a nitrogen gas inlet tube, 224 parts of xylene and 88.8 parts of 2,2-bis(3,3',4,4'-tetracarboxyphenyl)tetrafluoropropane dianhydride (6FDA) were charged, and the temperature was raised to 100°C while stirring under a nitrogen stream. 135.4 parts of Priamine 1075 (DA) were dropped over 1 hour, and then the mixture was stirred at 60°C for 2 hours. 4.2 parts of methanesulfonic acid were added, and the mixture was heated to 150°C and refluxed for 1 hour to carry out the reaction. The mixture was cooled to 40°C, and 5.6 parts of citraconic anhydride and 4.9 parts of maleic anhydride (a1) were added as (a2) over 1 hour, and the mixture was stirred for 2 hours. The mixture was heated to 150°C and refluxed for 14 hours to carry out the dehydration reaction. The resulting solution was washed three times with water, and then heated at 150°C to remove xylene and water from the system, after which 214 parts of toluene were added to obtain polyimide resin (A-1) having a number average molecular weight of about 6000 and a weight average molecular weight of about 15,000. The resin solid content was 50%.
[0134] (Synthesis Examples 2 to 27) A polyimide resin was obtained by synthesis in the same manner as in Synthesis Example 1, according to the composition and parts by weight of ingredients in Tables 1 and 2. The properties of the resin are shown in Tables 1 and 2.
[0135] [Table 1]
[0136] [Table 2]
[0137] The abbreviations in Tables 1 and 2 are shown below. DA1: Priamine 1075; a dimer diamine having 36 carbon atoms and a ring structure having 6 carbon atoms (dimer structure ratio: 95% or more, manufactured by Croda Japan) DA2: Versamine 551; a dimer diamine having 36 carbon atoms and a ring structure having 6 carbon atoms (manufactured by BASF Japan) NA: bis(aminomethyl)norbornane (Tokyo Chemical Industry Co., Ltd.) 6FDA: 2,2-bis(3,3',4,4'-tetracarboxyphenyl)tetrafluoropropane dianhydride BIS-DA: 4,4'-[propane-2,2-diylbis(1,4-phenyleneoxy)]diphthalic dianhydride (SABIC, BISDA-1000) MCTC: 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride (Tokyo Chemical Industry Co., Ltd.) TDA-100: 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride
[0138] [Example 1] (Preparation of Curable Resin Composition) According to Table 3, 30 parts of polyimide resin (A-1) and 0.3 parts of Percumyl D (B-1) as a curing aid (B) were charged, a solvent (toluene:MEK=9:1 (mass ratio)) was added so that the non-volatile content concentration became 60%, and the mixture was stirred with a disperser for 10 minutes to obtain a curable resin composition according to Example 1.
[0139] (Preparation of cured product) The curable resin composition was applied to a 50 μm-thick heavy release film (a polyethylene terephthalate (PET) film coated with a heavy release agent) using a blade coater so that the thickness after drying would be 50 μm. The composition was then heated at 120°C for 20 minutes and then heated in a vacuum oven at 190°C for 2 hours. The heavy release film was then removed to obtain a cured product.
[0140] (Preparation of laminated sheets) The obtained curable resin composition was applied to a polyimide film: Kapton® H type (manufactured by DuPont-Toray Co., Ltd.) using a blade coater so that the thickness after drying would be 50 μm, and the coating was heated at 120° C. for 20 minutes to obtain a laminate sheet.
[0141] (Preparation of substrate with cured material) The treated side of an 18 μm-thick electrolytic copper foil (product name "F2-WS", manufactured by Furukawa Circuit Foil Co., Ltd.) was placed on the adhesive surface of the obtained laminate sheet, and the resulting laminate was laminated at a pressure of 10 MPa for 1 minute, and then heated in a vacuum oven at 190°C for 2 hours to produce a laminate.
[0142] [Examples 2 to 32, Comparative Examples 1 to 9] Curable resin compositions according to Examples 2 to 32 and Comparative Examples 1 to 9 were obtained in the same manner as in Example 1, except that the ingredients and amounts were changed to those shown in Tables 3 and 4. Subsequently, cured products, laminate sheets, and laminates were produced using each of the curable resin compositions.
[0143] The materials used in the examples and comparative examples are shown below. <Curing aid (B)> (B-1): Parkmill D, manufactured by NOF Corp. (B-2): Perloil L, manufactured by NOF Corporation
[0144] <Inorganic filler (C)> (C-1): SC2050-MB (silica, average particle size D 50 0.5μm) manufactured by Admatechs (C-2): SP-2 (boron nitride, average particle size D 50; 4.0 μm) manufactured by Denka (C-3): E101-S (liquid crystal polymer, average particle size D 50 ;17.5μm) Sumitomo Chemical Co., Ltd. (C-4): Exolit OP935 (aluminum phosphinate, average particle size D 50 ;2.5μm) Clariant
[0145] <Crosslinking agent (D)> (D-1): YX-8800 (glycidyl ether type epoxy resin, functional group equivalent weight 180g / eq, bifunctional) manufactured by Mitsubishi Chemical Corporation (D-2): Orgatix ZC-150 (organic zirconia compound, functional group equivalent weight 122g / eq, 4 functional groups) manufactured by Matsumoto Fine Chemical Co., Ltd. (D-3): Carbodilite V-05 (carbodiimide group-containing compound, functional group equivalent: 262 g / eq, multifunctional) manufactured by Nisshinbo Chemical Co., Ltd.
[0146] <Curing accelerator> E: Diazobicycloundecene, manufactured by San-Apro Co., Ltd.
[0147] <Antioxidants> F: Adeka STAB AO-40 manufactured by Adeka Corporation
[0148] The cured products of the curable resin compositions of the Examples and Comparative Examples were evaluated for adhesion, heat resistance, dielectric constant, and dielectric loss tangent. The measurement methods and evaluation criteria were as follows:
[0149] (Evaluation of mechanical properties) The obtained laminated sheet was peeled off in the vertical direction at a width of 15 mm at room temperature using a tensile tester (manufactured by Shimadzu Corporation, product name: EZ-TEST), at a pulling speed of 50 mm / min, and the load was measured and evaluated according to the following criteria. ◎: Tensile strength 15.0N / 15mm or more (very good) ○: Tensile strength 8.0N / 15mm or more and less than 15.0N / 15mm (good) △: Tensile strength 5.0N / 15mm or more and less than 8.0N / 15mm (usable) ×: Tensile strength less than 5.0N / 15mm (unusable)
[0150] (Heat resistance) The substrate with the cured product prepared in each example was cut into a test piece with a width of 15 mm and a length of 65 mm. The test pieces were stored under various conditions, and then the copper foil surface was brought into contact with molten solder at various temperatures and allowed to float for 1 minute. The appearance of the test pieces was then visually observed, and the presence or absence of adhesive abnormalities such as foaming, lifting, and peeling of the adhesive layer after curing was evaluated according to the following criteria. ◎: Test piece stored for 24 hours in an atmosphere of 40℃ and 90% humidity showed no change in appearance when floated in molten solder at 280℃ (Very good) Good: When a test piece stored for 24 hours in an atmosphere of 23°C and 50% humidity was floated in molten solder at 280°C, there was no change in appearance. When a test piece stored for 24 hours in an atmosphere of 40°C and 90% humidity was floated in molten solder at 280°C, bubbles were observed. (Good) △: When a test piece stored for 24 hours in an atmosphere of 23°C and 90% humidity is floated on molten solder at 260°C, there is no change in appearance. When a test piece stored for 24 hours in an atmosphere of 23°C and 50% humidity is floated on molten solder at 280°C, bubbles are observed. (Usable) ×: When a test piece stored for 24 hours in an atmosphere of 23°C and 50% humidity was floated in molten solder at 260°C, bubbles were observed. (Not for use)
[0151] (Evaluation of relative dielectric constant) Three test pieces, each 3 mm wide and 80 mm long, were cut from the cured material prepared in each example and placed in an ADMS01Oc dielectric constant measuring device manufactured by AET. The dielectric constant was measured at a measurement temperature of 23°C and a measurement frequency of 10 GHz using the cavity resonator method. The rate was calculated and evaluated according to the following criteria. ◎: Dielectric constant less than 2.5 (very good) ○: Dielectric constant 2.5 or more and less than 2.7 (good) △: Dielectric constant 2.7 or more and less than 2.8 (usable) ×: Dielectric constant 2.8 or more (unusable)
[0152] (Evaluation of dielectric tangent) Three test pieces, each 3 mm wide and 80 mm long, were cut from the cured material prepared in each example and placed in an ADMS01Oc dielectric constant measuring device manufactured by AET. The dielectric constant was measured at a measurement temperature of 23°C and a measurement frequency of 10 GHz using the cavity resonator method. The contact was measured and evaluated according to the following criteria. ◎: Dielectric tangent less than 0.002 (very good) ○: Dielectric tangent 0.002 or more and less than 0.0024 (good) △: Dielectric tangent 0.0024 or more and less than 0.003 (usable) ×: Dielectric tangent 0.003 or more (not suitable for use)
[0153] [Table 3]
[0154] [Table 4]
[0155] As shown in Tables 3 and 4, Examples 1 to 32, which use cured compositions in which the molecular weight of (a2) in acid anhydride (a) having a carbon-carbon unsaturated bond is in the range of 112 to 351 and the molar ratio of the residues derived from (a1) to the residues derived from (a2) in (A) is in the range of 100:10 to 100:500, have good adhesive strength and are also excellent in dielectric properties and heat resistance, as compared with Comparative Examples 1 and 3 which contain only (a1), Comparative Examples 2 and 4 which contain only (a2), and Comparative Examples 5 to 9 which fall outside the above range.
[0156] (Prepreg manufacturing) Next, the varnish obtained in Example 1 was impregnated into a glass cloth (Nitto Boseki Co., Ltd., #2116 type, WEA116E, E glass) so that the mass ratio of glass cloth to resin composition of non-volatile components was 2:3, and then the prepreg of Example 1 was obtained by heating and drying at 140°C for about 5 minutes.
[0157] (Printed circuit board manufacturing) A glass cloth-based epoxy resin copper-clad laminate on which two types of circuit patterns, L / S=25μm / 25μm and copper thicknesses of 25μm and 50μm, were formed was prepared as an inner layer circuit board. The prepreg according to Example 1 was hot-pressed on both sides under vacuum reduced pressure at 190°C, 3.0MPa, and 120 minutes, and then copper foil was placed on the outermost layers on both sides to create a printed wiring board. It was also confirmed that printed wiring boards could be created in the same manner for the other examples.
Claims
1. A curing agent (B) comprising a polyimide resin (A), The polyimide resin (A) is a reaction product obtained by an imidization reaction between a prepolymer having an amino group at a terminal, which is a reaction product of a tetracarboxylic dianhydride (C) and a dimer diamine, and an acid anhydride (a) having a carbon-carbon unsaturated bond, the polyimide resin (A) contains a residue derived from maleic anhydride (a1) and a residue derived from an acid anhydride (a2) having a carbon-carbon unsaturated bond other than maleic anhydride, The molecular weight of (a2) is 112 to 351, A curable resin composition, characterized in that in the polyimide resin (A), a molar ratio of a residue derived from (a1) to a residue derived from (a2) is 100:10 to 100:
500.
2. The curable resin composition according to claim 1, wherein the (a2) contains at least one selected from the group consisting of citraconic anhydride, itaconic anhydride, allylsuccinic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride.
3. The curable resin composition according to claim 1 , wherein the tetracarboxylic dianhydride (C) has a fluorine atom or an alicyclic structure.
4. 2. The curable resin composition according to claim 1, wherein the weight average molecular weight of the polyimide resin (A) is 5,000 to 150,000.
5. The curable resin composition according to claim 1, further comprising at least one selected from the group consisting of a crosslinking agent, a curing accelerator and an antioxidant.
6. The curable resin composition according to claim 1, further comprising a filler.
7. A laminate sheet having a substrate and a resin composition layer, the resin composition layer being formed from the curable resin composition according to any one of claims 1 to 6.
8. A prepreg impregnated with the curable resin composition according to any one of claims 1 to 6.
9. A substrate having a cured product of the curable resin composition according to any one of claims 1 to 6 on a substrate.
10. An electronic device equipped with the substrate with the cured product according to claim 9.
Citation Information