Method for producing nylon 4 fiber

By employing superheated steam or far infrared heating during the stretching process, the method achieves uniform heating of nylon 4 fibers, addressing the non-uniformity issue and enhancing their strength.

JP2024170211AInactive Publication Date: 2024-12-06BRIDGESTONE CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023087243
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for producing nylon 4 fibers face challenges in uniformly heating the fibers during the stretching process, leading to temperature gradients and structural non-uniformity, which hinders the achievement of high strength.

Method used

The method involves using superheated steam heating or far infrared heating during the stretching process to uniformly heat nylon 4 fibers in a short time, with specific temperature and stretching ratio conditions to enhance molecular orientation and avoid fiber breakage.

Benefits of technology

This approach results in high-strength nylon 4 fibers by uniformly heating from the surface to the center, reducing the risk of fiber breakage and void generation, thereby improving mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170211000001_ABST
    Figure 2024170211000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a nylon 4 fiber, capable of producing a high-strength nylon 4 fiber.SOLUTION: The method for producing the nylon 4 fiber comprises: a dissolution step of dissolving a nylon 4 in a solvent to obtain a spinning solution; a spinning step of carrying out dry-spinning using the spinning solution to obtain an undrawn fiber; and a drawing step of drawing the undrawn fiber to obtain the nylon 4 fiber. The method for producing the nylon 4 fiber is characterized in that the drawing step is carried out under superheated steam heating or under far-infrared heating.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing nylon 4 fibers. [Background technology]

[0002] In general, when it is intended to increase the strength of a fiber, the molecular chains are aligned in one direction through the spinning and drawing steps to increase the orientation. The spinning and drawing steps can be carried out continuously, or the fiber obtained in the spinning step can be wound up once and then the drawing step can be carried out.

[0003] Nylon 4, a type of polyamide resin, is a resin that has a high density of amide bonds and is expected to have excellent thermal and mechanical properties. However, since Nylon 4 has strong intermolecular interactions due to hydrogen bonds, it tends to be difficult to stretch and align it as is.

[0004] In this regard, the present inventors have been studying a method for producing high-strength nylon 4 fibers by dry spinning (Patent Document 1). In this method, the fibers are heated in a normal oven to weaken the intermolecular interactions, and then stretched and aligned. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-031790 Summary of the Invention [Problem to be solved by the invention]

[0006] However, subsequent studies confirmed that the heating efficiency during the drawing process was insufficient in the production of nylon 4 fiber described in Patent Document 1. Specifically, it was found that, during drawing, the technology of Patent Document 1 easily heats the surface of the fiber, while the temperature of the center of the fiber is difficult to increase, that is, a temperature gradient is likely to occur in the radial direction of the fiber. In this case, the drawing stress in the center of the fiber increases during drawing, which may easily cause structural non-uniformity such as void generation. Such structural non-uniformity may be an obstacle to further increasing the strength of nylon 4 fiber.

[0007] To address this problem, for example, a method of lengthening the heating time in the oven during drawing in order to heat the center of the fiber sufficiently is considered. However, this method is not preferable because it increases the possibility that the fiber will melt during drawing (called melting breakage) and the effects of thermal degradation become significant. Under these circumstances, it can be said that there is still room for improvement in the prior art in terms of fully avoiding melting and thermal degradation of the fiber and further increasing the strength of nylon 4 fiber.

[0008] Therefore, an object of the present invention is to provide a method for producing nylon 4 fibers that can produce high-strength nylon 4 fibers. [Means for solving the problem]

[0009] In solving the above problems, the present inventors considered that in order to obtain nylon 4 fiber having higher strength, it is essential to heat the fiber uniformly from the surface to the center in a short time. As a result of further investigation, the present inventors found that heating under predetermined conditions during drawing enables heating to be performed uniformly and in a short time, which can contribute to further increasing the strength of nylon 4 fiber, and thus completed the present invention.

[0010] That is, the gist of the present invention for solving the above problems is as follows.

[0011] [1] A dissolving step of dissolving nylon 4 in a solvent to obtain a spinning solution; a spinning step of dry spinning the spinning solution to obtain an undrawn fiber; and a drawing step of drawing the undrawn fiber to obtain a nylon 4 fiber, 1. A method for producing nylon 4 fiber, wherein the drawing step is carried out under heating with superheated steam or under heating with far infrared rays. According to this method for producing nylon 4 fiber, it is possible to produce high strength nylon 4 fiber.

[0012] [2] The method for producing nylon 4 fiber according to [1], wherein the atmospheric temperature in the drawing step is 260°C or higher and 270°C or lower. In this case, the hydrogen bonds of nylon 4 are weakened, molecular orientation is promoted, and defects such as fiber breakage can be sufficiently avoided.

[0013] [3] The method for producing nylon 4 fiber according to [1] or [2], wherein the stretching ratio in the stretching step is 5.5 times or more. In this case, the effect of improving the fiber strength can be more significantly achieved.

[0014] [4] The method for producing a nylon 4 fiber according to any one of [1] to [3], wherein the solvent contains formic acid. In this case, it is advantageous in terms of availability and high solubility in nylon 4. Effect of the Invention

[0015] According to the present invention, a method for producing nylon 4 fiber, which is capable of producing high-strength nylon 4 fiber, can be provided. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic diagram of an example of a dry spinning apparatus that can be used in the method for producing nylon 4 fiber of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of an example of a drawing device that can be used in the method for producing nylon 4 fiber of the present invention. [Diagram 3]1 is a SEM image of the interior of a nylon 4 fiber of a comparative example. [Figure 4] 1 is a SEM image of the inside of a nylon 4 fiber of an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in detail below with reference to the embodiments. The compounds described in this specification may be derived partially or entirely from fossil resources, from biological resources such as plant resources, or from recycled resources such as used tires, or may be derived from a mixture of two or more of fossil resources, biological resources, and recycled resources.

[0018] (Nylon 4 fiber manufacturing method) A method for producing nylon 4 fiber according to one embodiment of the present invention (hereinafter, sometimes referred to as "the method for producing the present embodiment") includes at least a step of dissolving nylon 4 resin in a solvent to obtain a spinning solution (dissolving step), a step of dry spinning the spinning solution to obtain an undrawn fiber (spinning step), and a step of drawing the undrawn fiber to obtain a nylon 4 fiber (drawing step), and may further include other steps, such as a step of drying the undrawn fiber before the drawing step (drying step), as necessary. A feature of the method for producing the present embodiment is that the drawing step is performed under superheated steam heating or far-infrared heating.

[0019] Superheated steam is a medium that condenses when it comes into contact with a low-temperature substance and can provide heat to the substance. In other words, superheated steam has the inherent property of steam of raising the product temperature and the property of heating a substance like heated air. It has been found that superheated steam having such properties has a significant effect on heating fibers obtained from nylon 4 by dry spinning. Therefore, according to the manufacturing method of this embodiment, by using superheated steam heating during the drawing step, it is possible to uniformly heat the undrawn nylon 4 fibers in a short time, and as a result, it is possible to obtain nylon 4 fibers with even higher strength.

[0020] Furthermore, when far-infrared rays strike a substance, the light energy resonates with the molecules of the substance and is absorbed, inducing molecular-level motion. This molecular-level motion is effectively brought to the inside of the substance, and heat is generated by friction throughout the substance. It has been found that far-infrared rays, which have such an effect, have a significant effect on heating fibers obtained from nylon 4 by dry spinning. Therefore, according to the manufacturing method of this embodiment, by using far-infrared heating during the drawing process, undrawn nylon 4 fibers can be heated uniformly in a short time, making it possible to obtain nylon 4 fibers with even higher strength.

[0021] In addition, the manufacturing method of the present embodiment has the advantage that the undrawn nylon 4 fiber can be uniformly heated in a short time as described above, and therefore the fiber can be drawn without breakage even at a draw ratio that would cause breakage in the conventional technology.

[0022] In this specification, the term "nylon 4 fiber" refers to a fiber made of a linear polymer containing nylon 4. In addition, in this specification, "dry spinning" means dissolving a raw material in a solvent and discharging it from a spinneret (nozzle), and evaporating the solvent in a hot atmosphere to form fibers. In addition, in this specification, the term "superheated steam" refers to steam heated to a temperature above the boiling point, i.e., steam heated to a temperature above 100°C under atmospheric pressure. In addition, in this specification, "far infrared rays" refers to light (electromagnetic waves) with a wavelength of 3 μm to 1000 μm.

[0023] The raw materials used in the production method of this embodiment will be specifically described below.

[0024] <Nylon 4> As described above, in the manufacturing method of this embodiment, nylon 4 is used as a raw material. The method for preparing nylon 4 used in this embodiment is not particularly limited. For example, nylon 4 can be prepared by the ring-opening polymerization method of 2-pyrrolidinone described in Polymer, 46, pp. 9987-9993 (2005). Furthermore, high molecular weight nylon 4 can be prepared from 2-pyrrolidinone as a monomer by referring to the manufacturing method described in JP-A-5-0201.

[0025] As the raw material 2-pyrrolidinone, for example, one produced from petroleum, one produced from biological resources such as γ-aminobutyric acid using a microbial enzyme, etc. can be used.

[0026] <Other polyamide resins> In the manufacturing method of this embodiment, other polyamide resins may be used as raw materials together with nylon 4. Examples of other polyamide resins include aliphatic polyamides other than nylon 4 (nylon 6, nylon 66, etc.), wholly aromatic polyamides (aramid, etc.), and semi-aromatic polyamides (nylon 6T / 66, nylon 6T / 6I, etc.). However, in order to reliably obtain the desired effects and from the viewpoint of environmental considerations, it is preferable not to use the other polyamide resins in the manufacturing method of this embodiment.

[0027] Next, each step included in the manufacturing method of this embodiment will be specifically described.

[0028] <Dissolution process> The dissolving step is a step of dissolving the nylon 4 in a solvent to obtain a spinning solution. The concentration of nylon 4 in the spinning solution obtained in this dissolving step is not particularly limited, but is preferably 15% by mass or more. If the concentration of nylon 4 in the obtained spinning solution is 15% by mass or more, the amount of solvent to be evaporated becomes appropriate, and efficient dry spinning can be achieved while suppressing the generation of voids in the obtained fiber. From the same viewpoint, the concentration of nylon 4 in the spinning solution is more preferably 18% by mass or more.

[0029] On the other hand, the solubility of nylon 4, although it depends on the molecular weight of the nylon 4 and the solvent used, is generally up to about 30% by mass at 25° C. From the viewpoint of optimization, the concentration of nylon 4 in the spinning solution is preferably 22% by mass or less.

[0030] The solvent is not particularly limited, but from the viewpoint of availability and high solubility in nylon 4, it is preferable to use formic acid. In other words, the solvent used in the dissolving step preferably contains formic acid. In addition to formic acid, examples of the solvent include hexafluoroisopropanol (HFIP) and trifluoroacetic acid (TFA), which can be used in combination with formic acid. In other words, the solvent used in the dissolving step can further contain, in addition to formic acid, one or more selected from hexafluoroisopropanol and trifluoroacetic acid.

[0031] <Spinning process> The spinning step is a step of obtaining an undrawn fiber by dry spinning using the spinning solution obtained in the dissolving step. The dry spinning operation is not particularly limited, and dry spinning can be performed using a conventional dry spinning device.

[0032] As an example, FIG. 1 shows a schematic diagram of a dry spinning apparatus that can be used in the manufacturing method of this embodiment. In the dry spinning apparatus 100 shown in FIG. 1, first, a spinning solution is filled into a syringe 11. A heater 117 is provided in the syringe 11, and the spinning solution can be appropriately heated. The spinning solution filled in the syringe 11 is discharged in a filamentous form into the air from a nozzle 116 attached to the lower end of the syringe 11 by applying pressure from above with a plunger 115. In addition, a heater 12 is provided immediately below the nozzle 116, and a thermal atmosphere that can be adjusted to a predetermined temperature is formed. Then, fibers are formed from the solution after discharge, and the evaporation of the solvent from the fibers is promoted by the thermal atmosphere. Thereafter, the fibers are sequentially sent through one or more feed rollers including a feed roller 13 provided vertically below the nozzle, and the fibers (undrawn fibers) are wound up by a take-up roller 15.

[0033] In addition, the fibers may be enclosed by a tube 16 (e.g., a polycarbonate tube) provided with a solvent trap 17 from the heater 12 to the feed roller 13 vertically below, as shown in Fig. 1. Also, as shown in Fig. 1, an outer diameter measuring device 18 may be provided between the rollers (e.g., between the feed roller 13 and the feed roller 14, or between the feed roller 14 and the take-up roller 15) so that the diameter of the fibers obtained by dry spinning can be measured periodically. Furthermore, as shown in Fig. 1, a series of spinning steps may be performed in a dry spinning apparatus 100 covered with a protective cover 19.

[0034] <Drying process> In the manufacturing method of the present embodiment, after the above-mentioned spinning step and before the drawing step described below, a drying step may be performed to dry the undrawn fibers obtained in the spinning step. The drying method is not particularly limited, and examples thereof include a method in which the fibers are left in a chamber adjusted to a predetermined temperature and humidity.

[0035] <Stretching process> The drawing step is a step of drawing the undrawn fiber after the spinning step or drying step to obtain a nylon 4 fiber. In the manufacturing method of the present embodiment, this drawing step is performed under superheated steam heating or far infrared heating. This allows a high-strength nylon 4 fiber to be finally obtained.

[0036] As an example, the drawing process is performed under superheated steam heating, and FIG. 2 shows a schematic diagram of a drawing device that can be used in the manufacturing method of this embodiment. In the drawing device 200 shown in FIG. 2, the fiber passes through a cylindrical superheated steam heating chamber (hereinafter, sometimes simply referred to as a "heating chamber") 22 that can be adjusted to a predetermined atmospheric temperature while being sent in sequence by a send-off roller 21, yarn guides 23, 26, and a take-up roller 25, and is drawn by making the take-up speed of the take-up roller 25 faster than the send-off speed of the send-off roller 21. The heating chamber 22 is also connected to a superheated steam generator 27 via an introduction pipe 28. In the drawing process, the superheated steam that has been generated by the superheated steam generator 27 and adjusted to a predetermined temperature is filled into the heating chamber 22 via the introduction pipe 28, and the fiber is drawn by passing through the chamber.

[0037] 2, a protective tube 29 is preferably provided to surround the fibers near the connection point of the inlet pipe 28 in the heating chamber 22. This makes it possible to prevent the superheated steam supplied from the inlet pipe 28 from directly hitting the fibers.

[0038] The connection point of the introduction pipe 28 in the heating chamber 22 may be located anywhere from upstream to downstream in the stretching direction (traveling direction) of the fiber in the cylindrical heating chamber 22. However, from the viewpoint of uniformly and efficiently filling the heating chamber with superheated steam, the connection point is preferably located near the center of the heating chamber 22 in the longitudinal direction, as shown in FIG.

[0039] The number of connection points of the introduction pipe 28 in the heating chamber 22 is one in FIG. 2, but is not limited to this and may be two or more.

[0040] A tension meter (not shown) may be provided upstream of the take-up roller 25 so as to continuously measure the tension of the drawn fiber. If necessary, a preliminary drying oven (not shown, for example, 125° C.×1 m) may be provided upstream of the heating chamber 22.

[0041] On the other hand, when the stretching step is performed under far-infrared heating, the stretching device that can be used is not particularly limited as long as it has both a stretching function and a far-infrared heating function. In addition, such a stretching device can have a configuration equivalent to the configurations of the above-mentioned feed roller 21, heating chamber 22, yarn guide 23, winding roller 25, and yarn guide 26.

[0042] The atmospheric temperature in the stretching step (also referred to as the temperature inside the heating chamber 22) is preferably 260°C or higher and 270°C or lower. If the atmospheric temperature is 260°C or higher, the hydrogen bonds of nylon 4 can be weakened and molecular orientation can be promoted. If the atmospheric temperature is 270°C or lower, defects such as fiber breakage can be sufficiently avoided. The atmospheric temperature can be adjusted by the temperature of the superheated steam filled in the heating chamber 22 or the temperature of far infrared rays. It should be noted that the above-mentioned atmospheric temperature does not necessarily coincide with the actual temperature of the fiber itself during drawing.

[0043] The draw ratio in the drawing step is not particularly limited and can be, for example, 4.5 times or more. However, in the manufacturing method of the present embodiment, when the draw ratio is 5.5 times or more, the effect of improving the fiber strength can be more significantly achieved compared to the conventional technique when the same draw ratio is adopted. Moreover, from the viewpoint of more sufficiently increasing the strength of the obtained nylon 4 fiber, the draw ratio is more preferably 5.8 times or more, and even more preferably 6.0 times or more. In the stretching device 200 shown in FIG. 2, the stretching ratio can be adjusted by changing the winding speed of the winding roller 25 and the delivery speed of the delivery roller 21, respectively.

[0044] The residence time in the drawing step (residence time of the fiber in the heating chamber 22) is not particularly limited, but a long residence time may cause deterioration of the fiber, so a short residence time is preferable, for example, 45 seconds or less. The residence time can be adjusted by changing the delivery speed of the delivery roller 21, the take-up speed of the take-up roller 25, and the longitudinal length of the heating chamber 22.

[0045] The nylon 4 fiber obtained in this manner has high strength and can be used in a wide range of applications, including tire cords, clothing, ropes, airbags, seat belts, and parachutes. EXAMPLES

[0046] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples and can be modified as appropriate without departing from the gist of the present invention.

[0047] (Preparation of Nylon 4) Nylon 4 was prepared according to the procedure given below.

[0048] <Nylon 4 purification> 4.0 g of sulfuric acid was added to 600 g of 2-pyrrolidinone (Kanto Chemical Co., Ltd., purity: 98.0%) and stirred in an argon stream in an oil bath at 100°C. Next, distillation was performed under reduced pressure at an external bath temperature of 150°C and 1 mmHg, and after collecting about 10 mL of initial distillate, about 570 g of main distillate was obtained. In this way, 2-pyrrolidinone was purified in advance as a monomer.

[0049] Next, a 1L separable 4-neck flask was equipped with a stirring blade, a septum cap, a three-way cock equipped with a balloon and an argon bubbler, and a distillation device, and 500 g of the above-mentioned purified 2-pyrrolidinone was added. Decompression and argon replacement were performed three times, and after an argon atmosphere was created, an argon stream was used, and the flask was immersed in an oil bath at 40°C and stirred at 100 rpm. Next, 70.4 g of potassium hydroxide was added as a catalyst, the pressure was reduced to 1 mmHg, and after decompression and stirring were performed for 30 minutes, the water bath temperature was raised to 135°C at a rate of 10°C per 10 minutes, and the pyrrolidone that was azeotroped with the reaction was removed. During the temperature increase, the entire flask was covered with aluminum foil and kept warm. Subsequently, argon replacement was performed, and after an argon stream was used, the oil bath temperature was set to 40°C, and the distillation device was removed. A PFA cannula was inserted through the septum cap, and carbon dioxide gas as an initiator was bubbled at 60 mL / min (nitrogen gas equivalent: 75 mL / min) for 93 minutes while stirring. When carbon dioxide gas was blown in for 93 minutes at a flow rate of 60 mL / min, the substance amount n corresponds to 0.228 moles according to the ideal gas state equation (pV=nRT) (p=1(atm); V=60×93 / 1000(L); R=0.082; T=298(K)). In this case, the mass of carbon dioxide gas is calculated to be 0.228×44.01≒10.0g, since the molar mass is 44.01g / mol. After bubbling the carbon dioxide gas, the stirring blade was raised from the liquid surface, and the mixture was left in an argon stream with an oil bath temperature of 40°C for about 40 hours to perform ring-opening polymerization. In this way, a solid was obtained.

[0050] About 500 g of the solid obtained above was finely ground in liquid nitrogen, stirred in 3 L of pure water at room temperature for 30 minutes, and then filtered. Stirring and filtration were repeated until the pH of the filtrate became neutral. Next, the solid was immersed in 1 L of pure water and stirred for 10 hours. After confirming that the pH of the filtrate was neutral, the solid obtained was washed with acetone and dried under reduced pressure at 80°C and 1 mmHg for 48 hours. The solid was then ground using a benchtop grinder (manufactured by LabNext Co., Ltd., "Mini Speed ​​Mill MS-05") and classified through a 100 mesh sieve. About 100 g of the classified solid obtained was placed in 1 L of ion-exchanged water, boiled for about 5 minutes, left to cool, and then subjected to suction filtration. The above process was repeated once more, and washing was performed twice each time. The lumps after suction filtration were roughly loosened, moderately spread, and dried in a vacuum oven at 120°C for 20 minutes. In this way, nylon 4 was obtained. The obtained nylon 4 was placed in a container and stored in a desiccator ("MacDry MCU-201" manufactured by Eclar-Cie Co., Ltd.) at a relative humidity of about 1% or less.

[0051] The weight average molecular weight (Mw) of the obtained nylon 4 was measured under the following conditions. Measurement device: HLC-8320GPC (using RI detector) (manufactured by Tosoh Corporation) Column: TSKgel Super AWM-H × 2 (Tosoh Corporation) Solvent: Hexafluoroisopropanol (manufactured by Central Glass Co., Ltd.) Concentration: 2mg / 5mL Eluent: Trifluoroethanol (Tokyo Chemical Industry Co., Ltd.) Additive: Sodium trifluoroacetate (Fujifilm Wako Pure Chemical Industries, Ltd.) (10 mmol / L in the eluent) Pretreatment: Filtration with a membrane filter (Myshoridisk H-25-5, Tosoh Corporation) Injection volume: 20μL Flow rate: 0.3mL / min Column temperature: 40℃ Standard sample 1: SIGMA-ALDRICH, poly(methyl methacrylate) set 81506-1EA Standard sample 2: PSS Polymer Standards Service, Poly(methyl methacrylate) PSS-mm3m

[0052] The weight average molecular weight (Mw) of nylon 4 measured under the above conditions was 695,297 g / mol.

[0053] The obtained nylon 4 was weighed and stirred and mixed with formic acid (99% formic acid (special grade), manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a solvent to obtain a spinning solution. The above weighing was performed so that the concentration of nylon 4 in the spinning solution was 20 mass %. Furthermore, in order to prevent moisture absorption or weight loss due to scattering of formic acid, the above stirring was performed using a ceiling mixer UZU (manufactured by Nakamura Scientific Instruments Industry Co., Ltd.) at an external bath temperature of 50°C and at 2 rpm for 18 hours until the nylon 4 was completely dissolved in the solvent.

[0054] The obtained spinning solution was left in a sealed container in an oven at 40°C for about 1 hour to remove bubbles in the solution. Next, the solution was transferred to a syringe of a spinning device while being careful not to introduce bubbles into the solution. As the spinning device, a small spinning device manufactured by AIKI Riotech Co., Ltd. was used, and dry spinning was performed using this spinning device. The outline of this spinning device is as shown in the dry spinning device 100 in FIG. 1. Specifically, the spinning solution was kept at 40°C, pressure was applied from above to the spinning solution filled in the syringe 11 by a plunger 115, and the solution was discharged from a nozzle 116 (single-hole nozzle, length: 13 mm, inner diameter: 0.26 mm) attached to the lower end of the syringe 11 at about 0.05 mL / min. In order to dry and solidify the fluid surface on the spinning line to an extent that it would have enough strength to withstand spinning, a heater 12 (a transparent glass heater with a heating length of 10 cm) was installed directly under the nozzle 116 and the atmosphere was heated at 70° C. The distance from the nozzle 116 to the first feed roller 13 was 75 cm, and the yarn was fed at approximately the speed of free fall so as to minimize orientation of the molecular chains, and the yarn (undrawn fiber) was wound up by the downstream winding roller 15.

[0055] The undrawn fibers were then drawn using a drawing device. The drawing device used in Examples 1 to 3 (superheated steam heating) is as shown in FIG. 2, which shows a drawing device 200. Specifically, a "SH-ROBO" manufactured by Nippon Dentsu Co., Ltd. was used as the superheated steam generator 27, and a cylindrical heating chamber 22 (length: 70 cm, material: stainless steel) was attached to the outlet of the superheated steam generator 27 via an inlet pipe 28. A thermocouple was provided in the heating chamber 22 to check the temperature inside. Furthermore, a protective tube 29 was provided in the heating chamber 22 near the connection point of the inlet pipe 28 so as to surround the fiber. Then, the superheated steam generated by the superheated steam generator 27 was filled into the heating chamber 22, and after the temperature inside the heating chamber 22 became constant at a predetermined temperature (ambient temperature), the fiber was passed through the heating chamber 22 and drawn to obtain a drawn fiber (nylon 4 fiber). The stretching ratio at this time was determined by keeping the rotation speed (feeding speed) of the feed roller 21 constant and the ratio of the rotation speed of the feed roller 21 to the take-up roller 25. Table 1 shows the conditions of the atmospheric temperature and the stretching ratio in each example.

[0056] On the other hand, the stretching apparatus used in Comparative Examples 1 to 3 (normal heating) generally corresponds to the stretching apparatus 200 shown in FIG. 2, which does not have a mechanism for supplying superheated steam to the heating chamber. Specifically, a ceramic electric tubular furnace "AFR3-500-30KC" having a length of 30 cm and a temperature controller "AMF-10P-III" (both manufactured by Asahi Rika Seisakusho) were used as the heating chamber 22. Then, the inside of the heating chamber 22 was adjusted to a predetermined temperature (ambient temperature), and the fibers were stretched by passing through the heating chamber 22 to obtain stretched fibers (nylon 4 fibers). The stretching ratio at this time was determined from the rotation speed ratio of the feed roller 21 and the take-up roller 25, with the rotation speed (feeding speed) of the feed roller 21 kept constant. The conditions of the ambient temperature and the stretching ratio in each example are shown in Table 1.

[0057] The drawn fibers (nylon 4 fibers) obtained in each example were evaluated as follows.

[0058] <Measurement of fineness> The drawn fibers were left overnight in a constant temperature and humidity chamber adjusted to a temperature of 20° C. and a relative humidity of 65%, and then the fineness (dtex) was measured using a fineness measuring device "DENICON DC-21" manufactured by Search Co., Ltd. The measurement results are shown in Table 1.

[0059] <Measurement of tensile strength and elongation at break> First, the density of the drawn fibers was measured. Specifically, the density of the drawn fibers was measured by the density gradient tube method using a specific gravity measuring device Type A (direct reading type) manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd., in accordance with JIS K 7112 D method. At this time, carbon tetrachloride / toluene was used as the density liquid, and 1.230, 1.249, 1.270, and 1.290 (all units are g / cm) were used as the standard density spheres. 3 The water bath temperature was measured three times at 20±0.1℃, and the average value was calculated. On the other hand, the drawn fibers were left in a constant temperature and humidity room, and then tensile tests were performed using a small benchtop testing machine "EZTest EZ-SX" manufactured by Shimadzu Corporation under conditions of a sample chuck length of 20 mm and a tensile speed of 20 mm / min, and the breaking strength (cN) in this tensile test was determined. Next, the strength (unit: cN / dtex) calculated using this breaking strength and the fineness measured above was converted to Pa using the density of the drawn fiber measured above to determine the tensile strength (MPa). In addition, the breaking elongation (%) was determined by a similar tensile test. The measurement results of the tensile strength and breaking elongation are shown in Table 1 together with the density. The higher the values ​​of the tensile strength and breaking elongation, the higher the strength of the fiber.

[0060] <Measurement of knot strength> Using a tensile tester "Small tabletop tester EZTest EZ-SX" manufactured by Shimadzu Corporation, the stretched fiber was left to stand for 18 hours or more in a constant temperature and humidity environment of 20°C and 65% humidity, and then the knot strength was measured under the following conditions: load cell: 50N, initial sample length: 20mm, tensile speed: 20mm / min. The values ​​were also normalized by fineness. The measurement results are shown in Table 1. The higher the knot strength value, the higher the strength of the fiber. In particular, high knot strength of a fiber may have a positive effect on fatigue properties when used as a fiber with complex movements such as tire cord.

[0061] <SEM Observation of Fiber Interior (Comparative Example 2 and Example 2)> The surface of the drawn fiber was coated with Pt, embedded in resin, and a cross section was prepared using a cryo-ultramicrotome without thermal deformation or deterioration. The prepared cross section was then subjected to plasma etching using a Fischione 1020 plasma cleaner. The etching conditions were 25% oxygen and 75% argon gas, and the treatment time was 10 minutes. The cross section was then subjected to Pt sputtering treatment of several nm, and then observed using a Zeiss Merlin field emission scanning electron microscope (FE-SEM) at an acceleration voltage of 0.8 kV. An SEM image of the inside of the drawn fiber of Comparative Example 2 is shown in FIG. 3, and an SEM image of the inside of the drawn fiber of Example 2 is shown in FIG. 4.

[0062] In Table 1 below, it is important to compare the properties of drawn fibers with the same draw ratio, because the properties of the resulting drawn fiber can change significantly when the draw ratio is changed.

[0063] [Table 1]

[0064] From Table 1, it is clear that in a comparison between Comparative Example 1 and Example 1 (both of which had a stretch ratio of 5.0), Example 1 was higher in all of the tensile strength, elongation at break, and knot strength.

[0065] Furthermore, from Table 1, in a comparison between Comparative Example 2 and Example 2 (both of which had a draw ratio of 5.5 times), it can be seen that Example 2 was higher in all of the tensile strength, elongation at break, and knot strength. In particular, in terms of the improvement rate of the Example relative to the Comparative Example with the same draw ratio, Example 2 was greater than Example 1. In other words, it is suggested that the higher the draw ratio, the more remarkable the effect of improving the fiber strength is, in comparison with the prior art when the same draw ratio is adopted.

[0066] Furthermore, in Comparative Example 3, in which normal heating and a draw ratio of 6.0 were used, the fibers were broken during drawing, and therefore could not be drawn. On the other hand, in Example 3, in which superheated steam heating was used at the same draw ratio, a nylon 4 fiber with sufficiently high strength was obtained. This also suggests that the higher the draw ratio, the more remarkable the effect of improving the fiber strength, compared to the prior art when the same draw ratio is used.

[0067] As can be seen from Fig. 3, voids were observed inside the nylon 4 fiber of Comparative Example 2. It is believed that such voids are an obstacle to increasing the strength of the nylon 4 fiber. In contrast, as can be seen from Fig. 4, no voids were visible inside the nylon 4 fiber of Example 2 from the SEM image. That is, in the example, the fiber was able to be heated uniformly from the surface to the center during drawing in a short time, which is believed to have contributed to further increasing the strength of the nylon 4 fiber. [Industrial Applicability]

[0068] According to the present invention, a method for producing nylon 4 fiber, which is capable of producing high-strength nylon 4 fiber, can be provided. [Explanation of symbols]

[0069] 100: dry spinning apparatus, 11: syringe, 115: plunger, 116: nozzle, 117: heater, 12: heater, 13, 14: feed rollers, 15: take-up roller, 16: cylinder, 17: solvent trap, 18: outer diameter measuring device, 19: protective cover, 200: drawing device, 21: delivery roller, 22: superheated steam heating chamber, 23: yarn guide, 25: winding roller, 26: yarn guide, 27: superheated steam generator, 28: introduction pipe, 29: protection pipe

Claims

1. A dissolving step of dissolving nylon 4 in a solvent to obtain a spinning solution; a spinning step of dry spinning the spinning solution to obtain an undrawn fiber; and a drawing step of drawing the undrawn fiber to obtain a nylon 4 fiber, 13. A method for producing nylon 4 fiber, wherein the drawing step is carried out under heating with superheated steam or under heating with far infrared rays.

2. The method for producing nylon 4 fiber according to claim 1, wherein the atmospheric temperature in the drawing step is 260° C. or higher and 270° C. or lower.

3. The method for producing nylon 4 fiber according to claim 1, wherein the drawing ratio in the drawing step is 5.5 times or more.

4. 2. The method of claim 1, wherein the solvent comprises formic acid.

Citation Information

Patent Citations

  • Method for producing nylon 4 fiber and nylon 4 fiber