Non-aqueous electrolyte secondary battery

The non-aqueous electrolyte secondary battery with a specified negative electrode current collector surface characteristics addresses the issue of lithium metal detachment by promoting dense growth, thereby maintaining capacity retention.

JP2024170248AInactive Publication Date: 2024-12-06TOYOTA JIDOSHA KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023087308
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium secondary batteries face a decrease in capacity retention due to lithium metal deposition on the negative electrode current collector, which grows long and thin, leading to detachment and separation during charging and discharging.

Method used

A non-aqueous electrolyte secondary battery with a negative electrode current collector having a specific arithmetic mean roughness (Ra) of 1.25 μm to 3.50 μm and surface area of 1.20 cm² to 1.75 cm², which increases the number of lithium metal precipitation starting points, promoting dense growth and reducing detachment.

Benefits of technology

The solution effectively suppresses the decrease in capacity retention rate by ensuring lithium metal grows densely, minimizing detachment and maintaining battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170248000001
    Figure 2024170248000001
Patent Text Reader

Abstract

To provide a non-aqueous electrolyte secondary battery in which the decrease in capacity retention rate is suppressed.SOLUTION: A non-aqueous electrolyte secondary battery includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, the negative electrode includes a negative electrode current collector including a main surface on which lithium metal is deposited during charging, the main surface has an arithmetic mean roughness (Ra) of 1.25 μm to 3.50 μm and a surface area per 1 cm2 of the main surface is 1.20 cm2 to 1.75 cm2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery. [Background technology]

[0002] 2. Description of the Related Art Non-aqueous electrolyte secondary batteries, including lithium secondary batteries, are used in information and communication technologies (for example, personal computers and smartphones), hybrid cars, electric cars, storage batteries, and the like.

[0003] In a lithium secondary battery, lithium metal is deposited on the surface of the negative electrode current collector during charging. The deposited lithium metal may grow long and dendritic on the surface of the negative electrode current collector. The lithium metal deposited in the dendritic form dissolves during discharging of the lithium secondary battery. There is no problem if the lithium metal dissolves from the branch of the lithium metal deposited in the dendritic form, but the deposit that has grown long may shrink and be cut off and fall off, or the deposit may dissolve from the base of the branch and detach from the negative electrode current collector. The fallen or detached lithium metal cannot contribute to the battery reaction. As a result, the capacity retention rate of the lithium secondary battery may decrease.

[0004] In view of this, Patent Document 1 describes a lithium secondary battery capable of suppressing lithium metal deposition, which includes at least a positive electrode, a negative electrode, and an electrolyte solution interposed between the positive electrode and the negative electrode, wherein the negative electrode contains lithium metal, the electrolyte solution contains an ionic liquid containing a cation and its counter anion, and a lithium salt, the cation having one or more ether groups in its structure, and the counter anion being inactive against lithium metal. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2012 / 017520 Summary of the Invention [Problem to be solved by the invention]

[0006] Although the lithium secondary battery of Patent Document 1 has a certain effect in suppressing the deposition of lithium metal, the deposited lithium metal tends to grow elongated, and therefore, during charging and discharging, a part of the lithium metal deposited on the surface of the negative electrode current collector may fall off or break away, resulting in a decrease in the capacity retention rate.

[0007] An object of one embodiment of the present disclosure is to provide a nonaqueous electrolyte secondary battery in which a decrease in capacity retention rate is suppressed. [Means for solving the problem]

[0008] Means for solving the above problems include the following aspects. <1> The battery comprises a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte. The negative electrode comprises a negative electrode current collector including a main surface on which lithium metal is deposited during charging. The arithmetic mean roughness (Ra) of the main surface is 1.25 μm to 3.50 μm, and the main surface has an arithmetic mean roughness (Ra) of 1 cm 2 The surface area per unit is 1.20 cm 2 ~1.75cm 2 This is a non-aqueous electrolyte secondary battery. Effect of the Invention

[0009] According to one embodiment of the present disclosure, a nonaqueous electrolyte secondary battery in which a decrease in capacity retention rate is suppressed is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In the present disclosure, a numerical range indicated using "~" indicates a range including the numerical values ​​described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, the amount of each component in the composition means the total amount of the corresponding multiple substances present in the composition, unless otherwise specified, when multiple substances corresponding to each component are present in the composition. In the present disclosure, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the intended effect of the process is achieved.

[0011] <Nonaqueous electrolyte secondary battery> The non-aqueous electrolyte secondary battery of the present disclosure includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte. The negative electrode includes a negative electrode current collector including a main surface on which lithium metal is deposited during charging, and the arithmetic mean roughness (Ra) of the main surface is 1.25 μm to 3.50 μm and the surface roughness is within 1 cm2 of the main surface. 2 The surface area per unit is 1.20 cm 2 ~1.75cm 2 It is.

[0012] The term "negative electrode current collector" refers to a conductive sheet-like material (e.g., foil, film) excluding lithium metal and lithium alloys. The term "main surface" refers to the surface having the largest area. The negative electrode current collector has two main surfaces. The term "main surface on which lithium metal is deposited during charging" refers to at least one of the two main surfaces of the negative electrode current collector.

[0013] The nonaqueous electrolyte secondary battery of the present disclosure has the above-mentioned configuration, and thus the decrease in the capacity retention rate is suppressed. This effect is presumably due to, but not limited to, the following reasons. 2When the surface area per unit area is a predetermined value, the number of lithium metal precipitation starting points increases. This reduces the current density of the lithium metal precipitated from each precipitation starting point, and the lithium metal grows to a high density. In other words, the lithium metal precipitated from each precipitation starting point is less likely to grow elongated, and is less likely to fall off. As a result, it is presumed that the capacity retention rate of the nonaqueous electrolyte secondary battery of the present disclosure is less likely to decrease.

[0014] <Negative electrode> The negative electrode has a negative electrode current collector. The negative electrode current collector includes a main surface on which lithium metal is deposited during charging. The negative electrode current collector is not limited as long as it is a conductive material. Examples of conductive materials that can be used for the negative electrode current collector include copper (Cu), nickel (Ni) and iron (Fe). Examples of alloys include copper alloys and stainless steel (SUS). Among them, copper is preferable because it has high conductivity and does not form an intermetallic compound with lithium (Li).

[0015] The negative electrode current collector is preferably a copper foil having a thickness of 10 μm to 13 μm, and more preferably a copper foil having a thickness of 12 μm to 13 μm. The method for measuring the thickness of the negative electrode current collector is the same as that described in the Examples.

[0016] The arithmetic mean roughness (Ra) of the main surface is 1.25 μm to 3.50 μm, and from the viewpoint of suppressing a decrease in the capacity retention rate, it is preferably 1.3 μm to 3.3 μm, more preferably 2.3 μm to 3.3 μm, and even more preferably 2.7 μm to 3.2 μm. If the Ra of the main surface is less than 1.25 μm, the surface area of ​​the main surface is reduced, and the number of precipitation starting points is reduced. Furthermore, lithium metal is precipitated in elongated strips, and the capacity retention rate is reduced. If the Ra of the main surface is more than 3.50 μm, the roots of the recesses in the surface irregularities of the main surface cannot be the starting points for precipitation of lithium metal, and the capacity retention rate is reduced.

[0017] The arithmetic mean roughness (Ra) refers to the "arithmetic mean roughness (Ra)" defined in JIS B 0601: 2013. The method for measuring the arithmetic mean roughness (Ra) of the main surface is the same as the method described in the examples.

[0018] Main surface 1cm2 The surface area per square meter is 1.20 cm 2 ~1.75cm 2 From the viewpoint of suppressing the decrease in capacity retention rate, 2 ~1.75cm 2 is preferred, 1.35 cm 2 ~1.75cm 2 is preferred, 1.50 cm 2 ~1.68cm 2 is more preferable. 2 Surface area per unit is 1.20 cm 2 If the thickness is less than 1 cm, the number of lithium metal precipitation initiation sites will decrease, resulting in a decrease in the capacity retention rate. 2 Surface area per unit is 1.75cm 2 If the thickness is larger than this, the concave portions of the main surface irregularities become too deep, and as a result, the bases of the concave portions cannot become starting points for the deposition of lithium metal, resulting in a decrease in the capacity retention rate. Main surface 1cm 2 The method for measuring the surface area per unit area is the same as that described in the Examples.

[0019] The negative electrode may have a negative electrode active material layer supported on a portion of a main surface of the negative electrode current collector. The negative electrode active material layer contains a negative electrode active material (e.g., graphite, etc.) and may further contain a binder (e.g., styrene-butadiene copolymer, etc.) as known in the art.

[0020] <Positive electrode> The positive electrode has, for example, a positive electrode current collector (e.g., aluminum foil, etc.) and a positive electrode active material layer supported by the positive electrode current collector. The positive electrode active material layer is made of a known positive electrode active material (e.g., LiNiO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM), etc.), and may further contain a known conductive material (for example, carbon black, etc.) and a known binder (for example, polyvinylidene fluoride, etc.).

[0021] <separator> The separator separates the positive electrode from the negative electrode, and provides a path for lithium ions to move between the positive electrode active material layer and the negative electrode active material layer. Examples of the separator include a microporous resin sheet made of a resin such as polyethylene (PE). The separator may have a single-layer structure or a multi-layer structure.

[0022] <Non-aqueous electrolyte> The non-aqueous electrolyte may be a non-aqueous solvent (e.g., propylene carbonate (PC), fluoroethylene carbonate (FEC), ethyl carbonate (EC)) in which a supporting salt (e.g., lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), etc.) is dissolved or dispersed. The non-aqueous electrolyte may contain various additives (e.g., lithium bis(oxalato)borate, etc.).

[0023] <Case> A non-aqueous electrolyte secondary battery usually has a case that contains a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte. The case is not particularly limited, and examples thereof include a laminate film (e.g., an aluminum sheet, etc.) and a battery can (e.g., a cylindrical, rectangular, coin-shaped, etc.). EXAMPLES

[0024] The present disclosure will be described in more detail below with reference to examples, but the invention of the present disclosure is not limited to these examples.

[0025] [Example 1] <Preparation of positive electrode> The following samples were used to prepare the positive electrode. ·Cathode active material: LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM) 95.7 parts by mass Conductive additive: Li-400 (manufactured by Denka Co., Ltd., material: acetylene black) 2.0 parts by weight Binder: Polyvinylidene fluoride (PVdF) 2.3 parts by weight Solvent: n-methylpyrrolidone (NMP) The conductive assistant and the binder were mixed by hand for 1 minute, mixed for 5 minutes using a mixer (Thinky Corporation, "Awatori Rentaro"), and the positive electrode active material was added to obtain a first mixture. The first mixture was mixed 4 times to prevent the first mixture from becoming hot, and a second mixture was obtained. The mixing operation refers to the operation of mixing the first mixture with the mixer at 2,000 rpm for 1 minute, mixing the first mixture by hand, and removing heat from the first mixture. A solvent was added to the second mixture, and the mixture was mixed with the mixer at 2,000 rpm for 5 minutes, and the solvent was further added and mixed with the mixer at 2,000 rpm for 2 minutes to obtain a slurry. The solid content concentration of the slurry was 58.89%.

[0026] An aluminum foil (thickness: 12 μm to 15 μm) was used as the positive electrode current collector. The slurry was applied to one side of the positive electrode current collector using a doctor blade, and the coating was dried. The coating was rolled using a roller, and then cut into a size with a diameter of 14 mm to prepare a positive electrode. The positive electrode had a positive electrode current collector and a positive electrode active material layer supported on one side of the positive electrode current collector. The basis weight of the positive electrode active material layer was 23 mg / cm. 2 ~30mg / cm 2 The density of the electrode active material layer was 2.4 g / cc to 2.9 g / cc.

[0027] <Preparation of negative electrode> An electrolytic copper foil (manufactured by Nippon Denkai Co., Ltd., arithmetic mean roughness (Ra) of the main surface: 1.31 μm, thickness: 10 μm) was used as the negative electrode current collector. The negative electrode current collector was cut to a size of 16 mm in diameter to prepare a negative electrode. Note that the slurry containing the negative electrode active material was not applied onto the electrode current collector.

[0028] (Measurement of thickness of negative electrode current collector) The thickness (film thickness) of the negative electrode current collector was measured using a film thickness meter (PG-02J, manufactured by Techclock Corporation). The results are shown in Table 1.

[0029] (Method of measuring arithmetic mean roughness (Ra)) The arithmetic mean roughness (Ra) of the main surface of the negative electrode current collector was measured in accordance with JIS B 0651 and JIS B 0601. The results are shown in Table 1.

[0030] (Method of measuring surface area) 1cm of the main surface of the negative electrode current collector 2 A laser microscope (Keyence Corporation, VK-X3000) was used to measure the surface area per 1 cm of the main surface. 2 The surface area per unit area was calculated by calculating the area of ​​the irregular surface on the main surface from an image obtained by a laser microscope. The results are shown in Table 1.

[0031] Using the obtained positive and negative electrodes, a coin cell (diameter: about 1.5 mm) was fabricated as a non-aqueous electrolyte secondary battery. The coin cell includes a positive electrode, a negative electrode, a separator disposed between the positive and negative electrodes, an electrolyte, and a coin-shaped battery can that houses these. A porous separator made of a composite material of polyethylene and polypropylene was used as the separator. A solution prepared by dissolving lithium bis(fluorosulfonyl)imide to a concentration of 1 M (mol / l) in a mixed solvent containing 70 volume % propylene carbonate and 30 volume % fluoroethylene carbonate was used as the non-aqueous electrolyte.

[0032] [Examples 2 to 6 and Comparative Examples 1 to 5] A coin cell was produced in the same manner as in Example 1, except that the negative electrode current collector was changed to an electrolytic copper foil (film thickness 8 μm to 30 μm) shown in Table 1. The electrolytic copper foil of Comparative Example 2 is a product that has been conventionally used as a negative electrode current collector for nonaqueous electrolyte secondary batteries.

[0033] (Evaluation of capacity retention rate) In a 25°C environment, the coin cells of Examples 1 to 6 and Comparative Examples 1 to 5 were subjected to the following first CCCV charge, first rest, first CC discharge and second rest in this order. Then, 40 charge-discharge cycles were repeated. The charge-discharge cycle indicates that the following second CCCV charge, third rest and second CC discharge were performed in this order. "CC" indicates a constant current method. "CV" indicates a constant voltage method. "CCCV" indicates a constant current-constant voltage method. The current rate unit "C" indicates the current rate at which the rated capacity of the battery is fully discharged in one hour.

[0034] 1st CCCV charging: CC current = 0.1C, CV voltage = 4.3V, final current = 0.01C 1st pause: 5 minutes First CC discharge: CC current = 0.1C, final voltage = 3.0V 2nd break: 5 minutes 2nd CCCV charging: CC current = 1C, CV voltage = 4.3V, final current = 0.01C 3rd break: 5 minutes Second CC discharge: CC current = 0.1C, final voltage = 3.0V

[0035] The capacity retention rate was calculated from the discharge capacity of the charge-discharge cycle. The capacity retention rate is the percentage of the discharge capacity after 40 charge-discharge cycles to the discharge capacity after one charge-discharge cycle. The calculation results are shown in Table 1.

[0036] [Table 1]

[0037] As shown in the results in Table 1, in Examples 1 to 6, the decrease in the capacity retention rate was suppressed to 64.2% to 66.5%. On the other hand, in Comparative Examples 1 to 5, the capacity retention rate was decreased to 54.2% to 61.3% compared to the Examples. From the above results, the arithmetic mean roughness (Ra) of the main surface of the negative electrode current collector and the roughness per cm 2 It was shown that the decrease in capacity retention rate can be suppressed by setting the surface area per unit area to a predetermined value.

Claims

[Claim 1] A positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte; the negative electrode has a negative electrode current collector including a main surface on which lithium metal is deposited during charging; The arithmetic average roughness (Ra) of the main surface is 1.25 μm to 3.50 μm, The main surface 1 cm 2 The surface area per 2 ~1.75cm 2 A non-aqueous electrolyte secondary battery.