Crystallized glass and magnetic element core material
The crystallized glass composition addresses the challenges of size reduction and high frequency applications in magnetic elements by enhancing magnetic properties and reducing iron loss, particularly eddy current loss, through optimized component ratios.
Patent Information
- Application Number
- JP2024084470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-06
AI Technical Summary
Magnetic elements in electronic devices face challenges with increased size reduction and high frequency applications, particularly due to deteriorating magnetic properties and high iron loss, especially eddy current loss.
A crystallized glass composition containing specific proportions of FeO+Fe2O3, SiO2, NiO+MnO2, and other components, which enhances magnetic properties and reduces iron loss by increasing relative magnetic permeability and volume resistivity, facilitating the use in high frequency ranges.
The crystallized glass material improves magnetic properties and reduces iron loss, making it suitable for smaller magnetic elements in high frequency applications.
Smart Images

Figure 2024170313000001 
Figure 2024170313000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a crystallized glass and a core material for a magnetic element. [Background technology]
[0002] In recent years, there has been a rapid demand for smaller and more sophisticated electronic devices such as mobile devices and information devices, and similar demands have been placed on the magnetic elements (coils, etc.) used in these devices. However, particularly in the high frequency range (e.g., 1 MHz or higher), issues include a decrease in magnetic properties and an increase in loss (iron loss).
[0003] As a core material suitable for magnetic elements used in high frequency ranges, a material in which a magnetic metal alloy and an oxide coating are formed on the surface thereof have been disclosed (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-166156 A Summary of the Invention [Problem to be solved by the invention]
[0005] To further miniaturize magnetic elements, there is a need to improve magnetic properties and further reduce iron loss. In particular, since eddy current loss, a type of iron loss, increases in proportion to the square of the frequency, there is a need to reduce eddy current loss in high frequency applications.
[0006] In view of the above, an object of the present invention is to provide a crystallized glass and a core material for a magnetic element that can improve magnetic properties and reduce core loss. [Means for solving the problem]
[0007] Various aspects of the crystallized glass and the magnetic element core material that solve the above problems will be described below.
[0008] The crystallized glass of the first aspect contains, in mole percent, 5-80% FeO+Fe2O3, 1-80% SiO2, and 0.5-40% NiO+MnO2, and is characterized in that the relative permeability at a frequency of 100 MHz is 1.3 or more, and the volume resistivity Logρ (Ω·cm) at 25°C is 2 or more. Here, "FeO+Fe2O3" means the total amount of FeO and Fe2O3. "NiO+MnO2" means the total amount of NiO and MnO2. The relative permeability is measured using an impedance analyzer (E4990A manufactured by Keysight) and means the value at a frequency of 100 MHz. The volume resistivity logρ (Ω·cm) means the value measured by a four-terminal method (JIS K7194) using a digital multimeter (R6581 manufactured by ADC Corporation).
[0009] The crystallized glass of the second embodiment is preferably the crystallized glass of the first embodiment, which contains ferrite.
[0010] The crystallized glass of the third embodiment, in the first or second embodiment, preferably contains, in mol %, 0.5 to 40% NiO.
[0011] The crystallized glass of embodiment 4, in any one of embodiments 1 to 3, preferably contains, in mol %, 0.5 to 40% of MnO2.
[0012] The crystallized glass of embodiment 5, in any one of embodiments 1 to 4, preferably contains, in mol %, B2O3 0-80%, P2O50-80%, and Al2O3 0-80%.
[0013] The crystallized glass of embodiment 6, in any one of embodiments 1 to 5, preferably contains, in mol %, 1 to 40% of ZnO.
[0014] The crystallized glass of embodiment 7, in any one of embodiments 1 to 6, preferably contains, in mol %, 0 to 40% Li2O, 0 to 40% Na2O, and 0 to 40% K2O.
[0015] The crystallized glass of embodiment 8, in any one of embodiments 1 to 7, preferably contains, in mol %, 0 to 20% of Bi2O3.
[0016] The crystallized glass of embodiment 9, in any one of embodiments 1 to 8, preferably has a saturation magnetization of 10 emu / g or more.
[0017] The crystallized glass of the tenth embodiment is preferably used as a core material of the magnetic element in any one of the first to ninth embodiments.
[0018] In the crystallized glass of embodiment 11, in embodiment 10, the magnetic element is preferably at least one selected from the group consisting of a coil, a transformer, an inductor, a reactor, and a noise filter.
[0019] The magnetic core material of aspect 12 is characterized in that it is made of crystallized glass containing, in mole percent, 5-80% FeO+Fe2O3, 1-80% SiO2, and 0.5-40% NiO+MnO2, and has a relative permeability of 1.3 or more at a frequency of 100 MHz and a volume resistivity Logρ (Ω cm) of 2 or more at 25°C. Effect of the Invention
[0020] According to the present invention, it is possible to provide a crystallized glass and a magnetic element core material capable of improving magnetic properties and reducing core loss. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Preferred embodiments will be described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments.
[0022] <Glass-ceramics> The crystallized glass of the present invention contains, in mole percent, 5-80% FeO+Fe2O3, 1-80% SiO2, and 0.5-40% NiO+MnO2, and is characterized by having a relative permeability of 1.3 or more at a frequency of 100 MHz and a volume resistivity Logρ (Ω·cm) of 2 or more at 25°C. The crystallized glass having the above configuration exhibits high volume resistance because the glass around the precipitated crystals functions as an insulator. The higher the volume resistance, the smaller the eddy current loss, so the crystallized glass of the present invention can reduce eddy current loss and iron loss. In addition, the high relative permeability can improve magnetic properties.
[0023] From the viewpoint of improving magnetic properties, the crystallized glass of the present invention preferably contains ferrite, and more preferably contains ferrite as the main crystal. The ferrite is preferably at least one selected from spinel ferrite, garnet ferrite, and hexagonal ferrite. For example, the spinel ferrite is preferably represented by AFe2O4 (A is at least one selected from the group consisting of Ni, Zn, Cu, Mn, Co, and Mg). The garnet ferrite is preferably represented by RFe5O 12 (R is a rare earth element). Hexagonal ferrite is preferably represented by XFe 12 O 19 (X is at least one selected from the group consisting of Sr, Ba, and Pb). From the viewpoint of increasing the relative magnetic permeability, the ferrite is preferably a spinel ferrite. Specifically, Ni-Zn spinel ferrite or Mn-Zn spinel ferrite is preferable, and MnZnFe2O4 or NiZnFe2O4 is more preferable.
[0024] The crystallized glass of the present invention may contain magnetic crystals other than ferrite to obtain desired magnetic properties. Magnetic crystals refer to crystals having properties such as superferromagnetic, ferromagnetic, paramagnetic, and ferrimagnetic. For example, maghemite (γ-Fe2O3) may be contained.
[0025] The reasons for specifying the preferred glass composition in the crystallized glass of the present invention and the content of each component will be explained below. In the following explanation, "%" means "mol %" unless otherwise specified. In addition, in the present invention, "x+y+z+···" means the total content of each component. Here, each component does not necessarily have to be contained as an essential component, and there may be a component that is not contained (content 0%). In addition, "x+y+z+··· A%~B%" includes, for example, "x=0%, y+z+··· A%~B%" and "x=0%, y=0%, z+··· A%~B%".
[0026] FeO and Fe2O3 are components for precipitating ferrite. The content of FeO+Fe2O3 is 5 to 80%. More specifically, FeO+Fe2O3 (the total content of FeO and Fe2O3) is preferably 5% or more, 6% or more, 7% or more, 8% or more, 10% or more, 12% or more, and particularly preferably 15% or more, and is preferably 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 55% or less, and particularly preferably 50% or less. If the content of FeO+Fe2O3 is too small, ferrite is difficult to precipitate. Even if it precipitates, the amount of precipitation is small, so the magnetic properties are reduced. If the content of FeO+Fe2O3 is too high, vitrification is difficult. The preferred ranges of each component are as follows.
[0027] The FeO content is preferably 0% or more, 1% or more, 3% or more, 5% or more, 6% or more, 7% or more, 8% or more, 10% or more, 12% or more, and particularly preferably 15% or more, and is preferably 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 55% or less, and particularly preferably 50% or less.
[0028] The Fe2O3 content is preferably 0% or more, 1% or more, 3% or more, 5% or more, 6% or more, 7% or more, 8% or more, 10% or more, 12% or more, and particularly preferably 15% or more, and is preferably 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 55% or less, and particularly preferably 50% or less.
[0029] The crystallized glass of the present invention may contain at least one of FeO and Fe2O3, and preferably contains Fe2O3. By containing Fe2O3, ferrite is more likely to precipitate.
[0030] In addition, Fe3O4 may be further contained as an Fe component. By containing Fe3O4, saturation magnetization is easily increased. However, if the content is too high, the volume resistivity is easily decreased, so the content of Fe3O4 is preferably 0 to 20%. More specifically, the content of Fe3O4 is preferably 0% or more, more than 0%, 0.5% or more, particularly 1% or more, and is preferably 20% or less, 15% or less, particularly 10% or less. From the viewpoint of particularly increasing the volume resistivity, the content of Fe3O4 is preferably 5% or less, 3% or less, 1% or less, particularly preferably substantially not contained. In this specification, "substantially not contained" means that it is not intentionally contained, and does not exclude the inclusion of impurity levels. Objectively, it refers to the content of each component being less than 0.1%.
[0031] SiO2 is a component for forming glass. The content of SiO2 is 1 to 80%. More specifically, the content of SiO2 is preferably 1% or more, 2% or more, 4% or more, 5% or more, 7% or more, 9% or more, and particularly preferably 10% or more, and is preferably 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 59% or less, and particularly preferably 57% or less. If the content of SiO2 is too low, vitrification becomes difficult. If the content of SiO2 is too high, ferrite becomes difficult to precipitate.
[0032] NiO and MnO2 are components that easily improve the volume resistivity of ferrite. NiO+MnO2 (the total content of NiO and MnO2) is 0.5 to 40%. More specifically, the content of NiO+MnO2 is preferably 0.5% or more, 0.8% or more, and particularly 1% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, and particularly 15% or less. If the content of NiO+MnO2 is too low, it is difficult to obtain the above effects. If the content of NiO+MnO2 is too high, it is difficult to vitrify. In addition, the magnetic properties are easily deteriorated. The preferred ranges of each component are as follows.
[0033] The content of NiO is preferably 0% or more, 0.5% or more, 0.8% or more, particularly preferably 1% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, particularly preferably 15% or less. In particular, by including NiO as an essential component, the volume resistivity can be increased.
[0034] The content of MnO2 is preferably 0% or more, 0.5% or more, 0.8% or more, particularly preferably 1% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, particularly preferably 15% or less. In particular, by including MnO2 as an essential component, the saturation magnetization can be increased.
[0035] The crystallized glass of the present invention may further contain the following components.
[0036] B2O3 is a component that forms a glass skeleton and expands the vitrification range. The content of B2O3 is preferably 0 to 80%. More specifically, the content of B2O3 is preferably 0% or more, 0.5% or more, and particularly preferably 1% or more, and is preferably 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, and particularly preferably 10% or less. If the content of B2O3 is too high, ferrite becomes difficult to precipitate.
[0037] P2O5 is a component that forms a glass skeleton and expands the vitrification range. The content of P2O5 is preferably 0 to 80%. More specifically, the content of P2O5 is preferably 0% or more, 0.5% or more, 1% or more, and particularly preferably 2% or more, and is preferably 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, and particularly preferably 35% or less. If the content of P2O5 is too high, ferrite becomes difficult to precipitate.
[0038] Al2O3 is a component that forms a glass skeleton and expands the vitrification range. The content of Al2O3 is preferably 0 to 80%. More specifically, the content of Al2O3 is preferably 0% or more, 0.5% or more, 1% or more, particularly 2% or more, and is preferably 80% or less, 75% or less, 70% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 10% or less, 9% or less, 5% or less, 3% or less, 2% or less, 1% or less, particularly preferably substantially none. If the content of Al2O3 is too high, ferrite is less likely to precipitate.
[0039] ZnO is a component that easily improves the volume resistivity of ferrite. The ZnO content is preferably 0 to 40%, and particularly preferably 1 to 40%. More specifically, the ZnO content is preferably 0% or more, 0.5% or more, 1% or more, and particularly preferably 2% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 13% or less, and particularly preferably 11% or less. If the ZnO content is too high, ferrite becomes difficult to precipitate.
[0040] The crystallized glass of the present invention preferably contains both NiO and ZnO, particularly from the viewpoint of increasing the volume resistivity. More specifically, NiO+ZnO (the total content of NiO and ZnO) is preferably 1.5% or more, 2% or more, particularly 3% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, particularly 22% or less. By crystallizing the raw glass containing these components, Ni and Zn are incorporated into ferrite, which makes it easier to increase the volume resistivity.
[0041] The crystallized glass of the present invention preferably contains both MnO2 and ZnO, particularly from the viewpoint of increasing saturation magnetization. More specifically, MnO2+ZnO (the total content of MnO2 and ZnO) is preferably 1.5% or more, 2% or more, particularly 3% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, particularly 22% or less. By crystallizing the raw glass containing these components, Mn and Zn are incorporated into the ferrite, which makes it easier to increase saturation magnetization.
[0042] Li2O is a component that reduces the viscosity of glass and improves the melting and moldability of glass. The content of Li2O is preferably 0 to 40%. More specifically, the content of Li2O is preferably 0% or more, 0.5% or more, 1% or more, particularly 2% or more, and is preferably 40% or less, 30% or less, 20% or less, 15% or less, particularly 10% or less. If the content of Li2O is too high, the amount of evaporation of Li2O during melting increases, which increases the environmental load, and the chemical durability of the crystallized glass is likely to decrease. From the viewpoint of reducing the cost of glass, the content of Li2O is preferably 5% or less, 1% or less, particularly preferably substantially absent.
[0043] Na2O is a component that reduces the viscosity of glass and improves the meltability and moldability of glass. The Na2O content is preferably 0 to 40%. More specifically, the Na2O content is preferably 0% or more, 0.5% or more, 1% or more, and particularly preferably 2% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, and particularly preferably 20% or less. If the Na2O content is too high, the amount of evaporation of Na2O during melting increases, which increases the environmental load, and the chemical durability of the crystallized glass is likely to decrease.
[0044] K2O is a component that reduces the viscosity of glass and improves the melting and moldability of glass. The content of K2O is preferably 0 to 40%. More specifically, the content of K2O is preferably 0% or more, 0.5% or more, 1% or more, particularly 2% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 10% or less, particularly 5% or less. If the content of K2O is too high, the amount of evaporation of K2O during melting increases, which increases the environmental load, and the chemical durability of the crystallized glass is likely to decrease.
[0045] CaO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. The CaO content is preferably 0 to 40%. More specifically, the CaO content is preferably 0% or more, 0.5% or more, 1% or more, particularly 2% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, particularly 20% or less. If the CaO content is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, and the crystallized glass or the original glass before crystallization is likely to be damaged.
[0046] SrO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. The SrO content is preferably 0 to 40%. More specifically, the CaO content is preferably 0% or more, 0.5% or more, 1% or more, particularly 2% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, particularly 20% or less. If the SrO content is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, and the crystallized glass or the original glass before crystallization is likely to be damaged.
[0047] BaO is a component that reduces the viscosity of glass and improves the meltability and formability of glass. The content of BaO is preferably 0 to 40%. More specifically, the content of BaO is preferably 0% or more, 0.5% or more, 1% or more, particularly preferably 2% or more, and is preferably 40% or less, 35% or less, 30% or less, 25% or less, particularly preferably 20% or less. If the content of BaO is too high, unintended crystals (devitrification particles) are likely to precipitate during melting and forming, and the crystallized glass or the original glass before crystallization is likely to be damaged.
[0048] TiO2 and ZrO2 are components that act as nucleus forming agents. However, if the content is too high, the amount of heterogeneous crystals increases, making it difficult for ferrite to precipitate. Also, it becomes difficult to vitrify. The contents of TiO2 and ZrO2 are preferably 0% or more, particularly 0.1% or more, and are preferably 10% or less, 8% or less, 7% or less, 5% or less, 4% or less, 3% or less, 2% or less, 1% or less, less than 1%, particularly 0.5% or less.
[0049] Bi2O3 is a component that facilitates vitrification. On the other hand, since it is also a component with a strong diamagnetic effect, the magnetic properties deteriorate when the content is high. Therefore, it is preferable that the content of Bi2O3 is 20% or less, 15% or less, 10% or less, 5% or less, 1% or less, and in particular, substantially none is contained.
[0050] PbO is a component that facilitates vitrification. On the other hand, because PbO has a strong diamagnetic effect, the magnetic properties deteriorate when the content is high. Therefore, it is preferable that the PbO content is 1% or less, 0.8% or less, 0.1% or less, and in particular, substantially none is contained.
[0051] CoO, CuO, MgO and CdO are components that contribute to magnetic properties. CoO+CuO+MgO+CdO (the total content of CoO, CuO, MgO and CdO) is preferably 0 to 30%. More specifically, the content of CoO+CuO+MgO+CdO is preferably 0% or more, 0.5% or more, 1% or more, particularly 2% or more, and is preferably 30% or less, 25% or less, particularly 20% or less. If the content of CoO+CuO+MgO+CdO is too high, vitrification becomes difficult. The content of each of CoO, CuO, MgO and CdO is preferably 0% or more, 0.5% or more, 1% or more, particularly 2% or more, and is preferably 30% or less, 25% or less, particularly 20% or less.
[0052] Pt is a component that promotes crystallization, but when its content is high, the volume resistivity is likely to decrease. Therefore, the Pt content is preferably 2000 ppm or less by weight. More specifically, the Pt content is preferably 0 ppm or more, 0.1 ppm or more, 0.5 ppm or more, 0.8 ppm or more, and particularly preferably 1 ppm or more, and is preferably 2000 ppm or less, 1000 ppm or less, 500 ppm or less, 300 ppm or less, and particularly preferably 100 ppm or less.
[0053] The crystallized glass of the present invention has a relative magnetic permeability of 1.3 or more at a frequency of 100 MHz, and is preferably 1.5 or more, 2 or more, 2.5 or more, 2.8 or more, and particularly 3 or more. By satisfying the above-mentioned value of relative magnetic permeability, it can have particularly high magnetic properties. The upper limit is not particularly limited, but it may be, for example, 50 or less, particularly 30 or less.
[0054] The crystallized glass of the present invention has a volume resistivity logρ (Ω·cm) at 25°C of 2 or more, preferably 2.5 or more, 3 or more, 3.5 or more, 4 or more, and particularly 4.3 or more. When the volume resistivity at 25°C satisfies the above values, it is possible to reduce eddy current loss and iron loss in particular. The upper limit is not particularly limited, but may be, for example, 14 or less, particularly 12 or less.
[0055] The crystallized glass of the present invention preferably has a saturation magnetization of 10 to 100 emu / g. More specifically, the saturation magnetization is preferably 10 emu / g or more, 11 emu / g or more, 12 emu / g or more, and particularly preferably 14 emu / g or more. If the saturation magnetization is too small, magnetic saturation is likely to occur, leading to a decrease in magnetic permeability. The upper limit is not particularly limited, but may be, for example, 100 emu / g or less, 90 emu / g or less, 80 emu / g or less, 70 emu / g or less, 60 emu / g or less, 52 emu / g or less, and particularly 50 emu / g.
[0056] The crystallized glass of the present invention has the above-mentioned configuration, and thus it is possible to improve the magnetic properties and reduce the iron loss. Therefore, the crystallized glass of the present invention can be suitably used as a core material of a magnetic element. That is, the core material of the magnetic element of the present invention is made of crystallized glass containing, in mol%, FeO+Fe2O3 5-80%, SiO2 1-80%, and NiO+MnO2 0.5-40%, and has a relative permeability of 1.3 or more at a frequency of 100 MHz and a volume resistivity Logρ (Ω·cm) of 2 or more at 25°C. The magnetic element is preferably at least one selected from a coil, a transformer, an inductor, a reactor, and a noise filter. However, the crystallized glass of the present invention is not limited to the above-mentioned magnetic element. For example, the crystallized glass of the present invention may be used in electromagnetic devices such as a motor, an actuator, an induction heater (IH), and a speaker. In particular, it can be suitably used in a high frequency range where the iron loss is likely to be large. For example, it can be suitably used in a high frequency range of 1 MHz or more, 10 MHz or more, 50 MHz or more, and particularly 100 MHz or more.
[0057] <Method of manufacturing crystallized glass> The crystallized glass of the present invention can be produced, for example, as follows.
[0058] First, raw material powders are mixed to obtain a raw material batch so as to obtain glass of a desired composition. Next, the raw material batch is put into a glass melting furnace and melted at 1200 to 1750°C. Next, the molten glass is molded to obtain crystallizable glass (crystallizable raw glass). Alternatively, crystals may be precipitated while the molten glass is cooled and solidified, and crystallized glass may be obtained without going through the crystallizable glass process. The raw material batch may be melted using a crucible, or may be melted by laser irradiation in a floating state.
[0059] The molten glass may be formed by a known forming method such as a float method, an overflow method, a down-draw method, a roll-out method, or a mold press method. The molten glass may be quenched using a twin roller. If necessary, the molten glass may be subjected to a bending process or other process. The obtained crystallizable glass may be pulverized in a ball mill to obtain a crystallizable glass powder.
[0060] Next, the obtained crystallizable glass is crystallized by heat treatment. First, nucleation is performed at 500 to 800°C for 1 to 10 hours, and then crystal growth is performed at 650 to 1100°C for 1 to 10 hours. In this way, crystallized glass in which ferrite is precipitated as the main crystal can be obtained. The heat treatment may be performed only at a certain temperature, or may be performed stepwise by holding at two or more levels of temperature, or may be heated while applying a temperature gradient.
[0061] Crystallization may be promoted by applying or irradiating sound waves or electromagnetic waves to the crystallizable glass. When cooling the high-temperature crystallized glass, it may be cooled with a specific temperature gradient, or with two or more levels of temperature gradient. If sufficient thermal shock resistance is desired, it is preferable to control the cooling rate to sufficiently relax the structure of the remaining glass phase. The cooling rate of the surface can be estimated by a contact thermometer or a radiation thermometer, and the internal temperature can be estimated by placing the high-temperature crystallized glass in a cooling medium, measuring the heat quantity and heat quantity change rate of the cooling medium, and using the numerical data and the specific heat and thermal conductivity of the crystallized glass and the cooling medium. EXAMPLES
[0062] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.
[0063] Tables 1 and 2 show Examples 1 to 18 of the present invention.
[0064] [Table 1]
[0065] [Table 2]
[0066] (Example) The samples were prepared as follows. First, the raw material powders were prepared to have the glass compositions shown in Tables 1 and 2, and then mixed and melted at 1200 to 1750°C for 1 hour. Then, the mixture was quenched using a twin roller to obtain crystallizable glass. The obtained glass was pulverized in a ball mill to obtain crystallizable glass powder.
[0067] The obtained crystallizable glass powder was subjected to a heat treatment in a nitrogen atmosphere at 500 to 1000°C to crystallize the powder, thereby obtaining a crystallized glass. The crystallized glass obtained was measured for saturation magnetization, volume resistivity at 25°C, and relative permeability at a frequency of 100 MHz. In addition, the precipitated crystals were measured using XRD.
[0068] The saturation magnetization was measured using a vibrating sample magnetometer VSM (VSM-P7, manufactured by Toei Industry Co., Ltd.).
[0069] The volume resistivity at 25° C. was measured by the four-terminal method (JIS K7194) using a digital multimeter (R6581 manufactured by ADC Corporation).
[0070] The relative permeability was measured using an impedance analyzer (E4990A manufactured by Keysight) to determine the value at a frequency of 100 MHz.
[0071] As shown in Table 1, in Examples 1 to 9, NiZnFe2O4 precipitated as the main crystal, and the volume resistivity at 25°C was 4.9 to 8.2 Ω·cm, the saturation magnetization was 12 to 50 emu / g, and the relative permeability at a frequency of 100 MHz was 3.3 to 5.2.
[0072] As shown in Table 2, in Examples 10 to 18, MnZnFe2O4 precipitated as the main crystal, and the volume resistivity at 25°C was 4.3 to 7.9 Ω·cm, the saturation magnetization was 14 to 52 emu / g, and the relative permeability at a frequency of 100 MHz was 1.9 to 4.8.
[0073] Comparative Example 1 As in the example, the volume resistivity and saturation magnetization of iron oxide (Fe3O4) at 25°C were measured. The saturation magnetization of Fe3O4 was high at 90 emu / g. On the other hand, the volume resistivity logρ (Ω cm) at 25°C was low at 1.4.
[0074] Comparative Example 2 As in the examples, the volume resistivity and saturation magnetization of soda-lime glass at 25°C were measured. The volume resistivity logρ (Ω cm) of soda-lime glass at 25°C was high at 7.5. However, since it is a non-magnetic material, it did not exhibit magnetic properties. [Industrial Applicability]
[0075] The crystallized glass of the present invention is suitable as a magnetic core for electromagnetic devices such as coils, transformers, inductors, reactors, noise filters, motors, actuators, induction heaters (IH), speakers, etc. In particular, it is suitable as a core material for high frequency applications where iron loss is likely to be large.
Claims
1. In mole percent, FeO + Fe 2 O 3 5-80%, SiO 2 1-80%, NiO+MnO 2 The crystallized glass contains 0.5 to 40% of ZnO, has a relative permeability of 1.3 or more at a frequency of 100 MHz, and has a volume resistivity Log ρ (Ω·cm) of 2 or more at 25° C.
2. The crystallized glass of claim 1 , wherein the crystallized glass comprises ferrite.
3. 3. The crystallized glass according to claim 1, containing, in mol %, 0.5 to 40% NiO.
4. In mole percent, MnO 2 The crystallized glass according to claim 1 or 2, containing 0.5 to 40%.
5. In mole percent, B 2 O 3 0-80%, P 2 O 5 0-80%, Al 2 O 3 The crystallized glass according to claim 1 or 2, containing 0 to 80%.
6. 3. The crystallized glass according to claim 1, containing, in mole percent, 1 to 40% of ZnO.
7. In mole percent, Li 2 O 0-40%, Na 2 O 0-40%, K 2 3. The crystallized glass according to claim 1, containing 0 to 40% O.
8. In mole percent, Bi 2 O 3 The crystallized glass according to claim 1 or 2, containing 0 to 20%.
9. 3. The crystallized glass according to claim 1, having a saturation magnetization of 10 emu / g or more.
10. The crystallized glass according to claim 1 or 2, which is used as a core material for a magnetic element.
11. 11. The crystallized glass according to claim 10, wherein the magnetic element is at least one selected from the group consisting of a coil, a transformer, an inductor, a reactor, and a noise filter.
12. In mole percent, FeO + Fe 2 O 3 5-80%, SiO 2 1-80%, NiO+MnO 2 The magnetic element core material is made of crystallized glass containing 0.5 to 40% of Cr, and having a relative magnetic permeability of 1.3 or more at a frequency of 100 MHz and a volume resistivity Log ρ (Ω·cm) of 2 or more at 25° C.
Citation Information
Patent Citations