Block copolymer composition and applications thereof
Metallated sulfonated styrene block copolymers with tailored structures address the limitations of CEMs by improving conductivity and mechanical stability, offering enhanced performance in electrochemical devices.
Patent Information
- Application Number
- JP2024085161
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-06
AI Technical Summary
Existing cation exchange membranes (CEMs) face challenges with low hydroxide conductivity, insufficient long-term chemical and mechanical stability, and low ionic conductivity, particularly in basic environments, limiting their widespread adoption in electrochemical devices.
Development of metallated sulfonated styrene block copolymers with specific structures and functionalization, including triblock, tetrablock, and pentablock configurations, to enhance ion exchange capacity and mechanical strength, featuring ion exchange capacities of 0.5 to 8.0 meq/g and tailored properties for use in energy storage devices.
The metallated sulfonated styrene block copolymers provide improved oxidative stability, high ionic conductivity, and desirable mechanical strength, making them suitable for applications in battery electrolytes and CEMs, enhancing performance and durability.
Smart Images

Figure 2024170322000001 
Figure 2024170322000002 
Figure 2024170322000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to metallized sulfonated styrenic block copolymer compositions, methods of preparation and uses thereof. [Background technology]
[0002] Cation exchange membranes (CEMs) are key components for many electrochemical devices, such as fuel cells and electrolyzers. However, relatively low hydroxide conductivity and poor long-term chemical and mechanical stability are major barriers to the wider adoption of CEM-based technologies. To address these issues, various synthetic approaches have been explored to increase ion exchange capacity and crosslink membrane polymers. However, these approaches typically require multiple synthetic steps to achieve a comprehensive material design with customizable functionality and improved mechanical properties.
[0003] The performance of CEMs depends on the type of material used. Hydrogenated styrene-butadiene block copolymers (SEBS) and non-hydrogenated styrene block copolymers (USBC) have the unique properties of alternating soft and hard blocks and an all-carbon backbone, which gives them high potential for application in phase separation and excellent alkali resistance. USBC has sufficient reactive sites in the form of unsaturation. Functionalized SBCs act as precursor materials that impart excellent membrane processability. However, CEMs based on these polymers suffer from poor stability in basic environments, poor ionic conductivity, and reduced mechanical strength due to water absorption and vulnerability of backbone unsaturation.
[0004] Styrenic block copolymers (SBCs) can be functionalized to modify their properties for use as electrolytes in batteries, which have many similar requirements to CEMs, such as thermal stability, high ionic conductivity, and excellent electrochemical performance. Summary of the Invention [Problem to be solved by the invention]
[0005] There is a need for improved functionalized block copolymers that provide oxidative stability, high ionic conductivity and electrochemical performance, and desirable mechanical strength for a variety of applications such as battery electrolytes, CEMs, etc. [Means for solving the problem]
[0006] Summary of the Invention In one aspect, the present disclosure provides a metallated sulfonated styrenic block copolymer comprising any of a triblock, tetrablock, pentablock, and coupling structure, each of which is selected from the group consisting of ABA, ABA', A'B'A'; ABB'A, ABA'A, ABB'A'; ABA'BA, AA'BA'A, ABABA, AA'BA'A, ABB'A'A, A'B'A'B'A'; (ABA) n X, (AB) n X, (BAB) n X, (ABAB) n X, (ABABA) n X, (A'B') n , (A'B') n (A'), (A'B'A') n , (A'B'A') n X, (A'B') n X, (B'A'B') n X, (A'B'A'B') n X or (A'B'A'B'A') n X, where n is an integer from 2 to 30, and X is a residue of a coupling agent. Prior to hydrogenation, blocks B and B' are the same or different and are independently derived from any of 1,4-isoprene units, 1,2-butadiene units, 1,4-butadiene units, and mixtures thereof. Blocks A and A' are the same or different and are independently derived from any of (i) para-substituted vinyl aromatic monomers or (ii) unsubstituted vinyl aromatic monomers. Each of blocks B and B' is a midblock and is represented by the following formula (I):
[0007] [ka] (M + is Na + , K + , Li + , Cs + , Ag + , Hg + and Cu + and (CH2)y, where y is 3 to 12, is a spacer group. Metal sulfonation (SO3 - M + ) groups. The metallated sulfonated styrene block copolymers have an ion exchange capacity (IEC) of 0.5 to 8.0 meq / g according to ASTM D7131-05.
[0008] In another embodiment, each block B and B' is independently in the range of 30 mol % to 100 mol % of a metalated sulfonated (SO - M + ) degrees.
[0009] In yet another embodiment, the metallated sulfonated styrenic block copolymer is a partially hydrogenated styrenic block copolymer obtained from a styrenic block copolymer precursor. The partially hydrogenated styrenic block copolymer has a residual unsaturation of 0.5 to 15 meq / g.
[0010] In yet another aspect, an energy storage device includes a metallized sulfonated styrenic block copolymer, the metallized sulfonated styrenic block copolymer being applied as either an electrode binder, an electrode, a separator, or an electrolyte.
[0011] In another embodiment, the energy storage device comprises a lithium ion primary battery, a lithium ion secondary battery, a capacitor, a supercapacitor, a fuel cell, a metal-sulfur battery, or a metal-air battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following terms have the following meanings.
[0013] "Consisting essentially of" means that the claimed composition contains primarily the specified material, with the allowance for additional components that do not materially affect the novel properties or function of the claimed invention, and if present, the additional components are in an amount of less than 30%, or less than 20%, or less than 10%.
[0014] "At least one of [groups such as A, B and C]" or "any of [groups such as A, B or C]" means a single member from a group, more than one member from a group, or a combination of members from a group. For example, at least one of A, B and C includes, for example, A only, B only, or C only, as well as any other combination of A and B, A and C, B and C, or A, B and C, or A, B and C.
[0015] The recitation of embodiments presented as "A, B, or C" is to be interpreted as including embodiments of A only, B only, C only, "A or B," "A or C," "B or C," or "A, B, or C."
[0016] "Either A, B, or C" refers to one choice from A, B, or C.
[0017] "Any of A, B, and C" refers to one or more choices from A, B, and C.
[0018] As used herein, a "block" refers to a section of a polymer molecule having a plurality of identical constitutional units (monomers) and possessing at least one structural or compositional feature that is not present in an immediately adjacent section (block).
[0019] "Conjugated diene (CD)" refers to an organic compound containing conjugated carbon-carbon double bonds and a total of 4 to 12 carbon atoms, such as 4 to 8 carbon atoms, which can be any of 1,3-butadiene and substituted butadienes, including but not limited to 1,3 cyclohexadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1-phenyl-1,3-butadiene, 1,3-pentadiene, 3-butyl-1,3-octadiene, chloroprene, and piperylene, or any combination thereof. In an embodiment, the conjugated diene block comprises a mixture of butadiene and isoprene monomers. In an embodiment, 1,3-butadiene alone is used.
[0020] "Butadiene" refers to 1,3-butadiene or 1,4-butadiene.
[0021] "Monovinylarene" or "monoalkenylarenes" or "vinyl aromatics" refer to organic compounds containing a single carbon-carbon double bond, at least one aromatic moiety, and a total of 8 to 18 carbon atoms, e.g., 8 to 12 carbon atoms. Examples include styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, alpha-methylstyrene, vinylnaphthalene, vinyltoluene, vinylxylene, or any mixture thereof. In embodiments, the monoalkenylarenes block comprises substantially pure monoalkenylarenes monomers. In some embodiments, styrene is the major component with a small proportion (less than 10% by weight) of structurally related vinyl aromatic monomers, e.g., o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, a-methylstyrene, vinylnaphthalene, vinyltoluene, vinylxylene, or combinations thereof. In embodiments, styrene alone is used.
[0022] "Vinyl content" refers to the content of conjugated dienes that have been polymerized via 1,2-addition in the case of butadiene or 3,4-addition in the case of isoprene to result in monosubstituted olefins or vinyl groups that are adjacent to the polymer backbone. Vinyl content may be measured by nuclear magnetic resonance (NMR).
[0023] "Coupling efficiency" is expressed as %CE and is calculated using the weight percent of coupled polymer and the weight percent of uncoupled polymer. The weight percent of coupled and uncoupled polymer is determined using the output of a differential refractive index detector. The intensity of the signal at a particular elution volume is proportional to the amount of material of molecular weight equivalent to the polystyrene standard detected in the elution volume.
[0024] "Coupling Agent" or "X" refers to coupling agents commonly used in the preparation of styrenic block copolymer SBC technology, such as silane coupling agents, e.g., isobutyl-trimethoxysilane, methyltrimethoxysilane; polyvinyl compounds, polyvinylarenes, di- or multivinylarene compounds; di- or multiepoxides; di- or multiisocyanates; di- or multialkoxysilanes; di- or multiimines; di- or multialdehydes; di- or multiketones; alkoxytin compounds; di- or multihalides, such as silicon halides and halosilanes; mono-, di- or multianhydrides; di- or multiesters; tin tetrachloride; tetramethylorthosilicate.
[0025] The "polystyrene content" or PSC of a block copolymer refers to the weight percent of vinyl aromatic, e.g., polystyrene, in the block copolymer, which is calculated by dividing the sum of the molecular weights of all vinyl aromatic blocks by the total molecular weight of the block copolymer. PSC may be determined using any suitable methodology, such as proton nuclear magnetic resonance (NMR).
[0026] "Molecular weight" or MW refers to the styrene equivalent molecular weight in kg / mol of a polymer block or block copolymer. MW may be measured by gel permeation chromatography (GPC) using polystyrene calibration standards, such as performed in accordance with ASTM 5296-19. The GPC detector can be an ultraviolet or refractive index detector, or a combination of these. The chromatograph is calibrated using commercially available polystyrene molecular weight standards. The MW of a polymer measured using a GPC so calibrated is the styrene equivalent molecular weight or apparent molecular weight. The MW expressed herein is measured at the peak of the GPC trace, commonly referred to as the styrene equivalent "peak molecular weight", and is the MW of the polymer ... p It is specified as follows.
[0027] "Residual Unsaturation (RU)" refers to the level of unsaturation, i.e., carbon-carbon double bonds, per gram of block copolymer. RU can be measured using proton NMR.
[0028] "pHSBC" is used interchangeably with partially or partially hydrogenated styrenic block copolymer.
[0029] "Mid-block" refers to a block in a multi-block copolymer structure (e.g., SBC) that is located between the terminal blocks (or end blocks). The mid-block may or may not be a central block, e.g., M (mid-block) in the structure of AAMAA or AMAA (where "A" is a terminal or end block).
[0030] "End block" refers to the terminal block in a multi-block copolymer structure (eg, SBC), such as "A" in the example of "AMMA."
[0031] "Crosslinking" refers to the process of chemically linking two or more molecules by covalent bonds. It also refers here to the process in which monomers capable of reacting with functional groups on polymer chains in the presence of a suitable catalyst result in the grafting of multiplying branched chains, some of which react with other chains of the structure. The crosslinking step can be achieved by curing using heat or radiation treatment (UV) or by neutralization. Crosslinking reagents can contain reactive ends for certain functional groups (primary amines, acrylates, sulfides, etc.) on polymers or other molecules.
[0032] "Membrane" refers to a continuous, flexible sheet or layer of material (such as a film or coating) that can act as a selective barrier to allow some things to pass, such as molecules, ions, gases or particles, while stopping others.
[0033] "Cation exchange membrane" or "alkali exchange membrane" or "CEM" refers to a semi-permeable membrane, generally made from an ionomer, designed to conduct anions and repel cations.
[0034] "Cation exchange membrane electrolyzer" (CEMEL) refers to an electrolyzer that has a polymer electrolyte membrane that separates the anode from the cathode. Electrolyzers use electricity to split water (H2O) into hydrogen and oxygen through an electrochemical reaction.
[0035] "Fuel cell" refers to an electrochemical cell that converts the chemical energy of a fuel (eg, hydrogen) and an oxidant (eg, oxygen) into electricity through a set of redox reactions.
[0036] "Ion exchange capacity" or IEC refers to all active sites or functional groups in a polymer that govern ion exchange. Conventional acid-base titration methods can be used to determine IEC, see "Determination of the ion exchange capacity of anion-selective membrane", International Journal of Hydrogen Energy, Vol. 39, No. 10, March 26, 2014, pp. 5054-5062. IEC is the inverse of "equivalent weight" or EW, which is the weight of polymer required to provide one mole of exchangeable protons.
[0037] "Li-ion battery" refers to a lithium-based storage system, although as used herein, the term also refers to batteries containing other metals, such as sodium, potassium, cesium, silver, mercury, copper, etc. (M + ) uses are also included.
[0038] "Charge capacity" refers to the capacity obtained by constant current charging at a current value until a certain battery voltage is reached.
[0039] "Discharge capacity" refers to the discharge of a battery at a current value until the battery voltage reaches a certain value.
[0040] "Metalized sulfonated block copolymer" or "SO3 - M + -Block copolymer" is a metallized sulfonated styrene block copolymer (SO3 - M + The term metallized sulfonated block copolymer may be used interchangeably as SO3Li-SBC or SO3Li-pHSBC. + ) is any of Li, Na, K, Cs, Ag, Hg or Cu.
[0041] The present disclosure relates to a metallized sulfonated styrene block copolymer (SO3 - M + -SBC) composition. - M + -SBC can be obtained by i) hydrogenation of the SBC precursor followed by epoxidation, ii) alcoholysis of the epoxidized SBC, and iii) in situ metallation and sulfonation. The SBC precursor can be prepared by metalation sulfonation (SO - M + -) The block may be a triblock, tetrablock, pentablock, or coupling structure having at least one of the blocks having a functional group. - M + - The SBC is suitable for use as a CEM or CEM water electrolyser.
[0042] Metal sulfonated block copolymer (SO3 - M + -Block copolymer: Metalated sulfonated block copolymer (SO3 - M + -block copolymer) composition is SO3 - M + The process comprises, consists essentially of, or consists of epoxidized, hydrolyzed, and metalated sulfonated styrenic block copolymer (SBC) or partially hydrogenated styrenic block copolymer (p-HSBC) precursors to obtain -SBC. In an embodiment, p-HSBC is prepared from SBC precursors. In an embodiment, SO3 - M + -SBC is either a triblock, tetrablock, pentablock or a coupling structure containing A, A', B and B' blocks, where A, A' and B, B' are the same or different. In all structures, each B or B' block is an intermediate block and has the following formula (I):
[0043] [ka] (In formula (I), M + is Na+ , K + , Li + , Cs + , Ag + , Hg + and Cu + (CH2) y (wherein y is 3 to 12) is an alkyl spacer group. + is Na + , K + Or Li + (It is either Metal sulfonation (SO3 - M + ) moiety.
[0044] In embodiments, the SBC precursor or base polymer is prepared by copolymerizing one or more olefins with at least one conjugated diene, either by themselves or with one or more monoalkenyl arene monomers. The copolymers may or may not be tapered, the individual blocks may be homopolymers or random copolymers, and the polymer molecules may be linear or branched.
[0045] In an embodiment, the SBC precursor is a group of sequential diblock structures such as S-CD, S-CD / CD' or S-CD / S, sequential triblock structures such as S-CD-S, S-CD-CD', S'-CD-S', tetrablock structures such as S-CD-CD'-S, S-CD-S'-S, S-CD-CD'-S', pentablock structures such as S-CD-S'-CD-S, S-CD-S-CD-S, SS'-CD-S'S, S-CD-CD-'S'-S, S'-CD'-S'-CD'-S' or coupled structures such as (S-CD-S) n X, (S-CD) n X, (CD-S-CD) n X, (S-CD-S-CD) n X, (S-CD-S-CD-S) n X, (S'-CD'-S') n X, (S'-CD') nX, (S'-CD'-S'-CD') n X or (S'-CD'-S'-CD'-S') n X and mixtures thereof, where X is the residue of a coupling agent. In embodiments, the S and S' blocks are the same or different and are independently derived from either (i) para-substituted vinyl aromatic monomers and (ii) unsubstituted vinyl aromatic monomers, and each CD and CD' block is the same or different and is independently derived from 1,4-isoprene units, 1,2-butadiene units, 1,4-butadiene units, and mixtures thereof.
[0046] "n" refers to the number of "arms" or "branches" in each of the structures, where n is an integer greater than 1. In embodiments, n ranges from 2 to 30, or from 2 to 20, or from 2 to 10, or from 2 to 7.
[0047] In an embodiment, each block S and S' is independently selected from the group consisting of styrene, alpha-methylstyrene, methylstyrene, para-methylstyrene, ethylstyrene, propylstyrene, butylstyrene, tert-butylstyrene, dimethylstyrene, vinyltoluene, isomers of vinyltoluene, vinylxylene, 1,1-vinylbiphenyl, vinylnaphthalene, vinylanthracene, and mixtures thereof.
[0048] In an embodiment, each block S and S′ independently has a molecular weight (M p In an embodiment, the polymer blocks S and S' comprise up to 50% by weight, or from 5 to 55% by weight, or from 10 to 35% by weight, or from 15 to 25% by weight, or from 5 to 20% by weight, or from 5 to 15% by weight, or from 5 to 20% by weight, based on the total weight of the SBC.
[0049] In an embodiment, each of the polymer blocks CD and CD' independently comprises a polymer or copolymer of a conjugated diene monomer selected from the group consisting of isoprene, 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 1-phenyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 3-butyl-1,3-octadiene, farnesene, piperylene, cyclohexadiene, and mixtures thereof.
[0050] In an embodiment, each of the polymer blocks CD and CD′ independently has a molecular weight (M) of 2 to 350 kg / mol, or 5 to 300 kg / mol, or 7 to 250 kg / mol, or 10 to 200 kg / mol, or 5 to 150 kg / mol, or 3 to 100 kg / mol. p In an embodiment, the polymer blocks CD and CD' constitute up to 100% by weight, or 70-95% by weight, or 75-95% by weight, or 80-95% by weight, or 85-95% by weight, or 75-85% by weight, or 80-90% by weight, or 75% by weight or more, based on the total weight of the SBC.
[0051] Metallized sulfonated styrene block copolymer (SO3 - M + -SBC): In embodiments, the SBC precursor is hydrogenated, epoxidized, then hydrolyzed, and then in situ metallated and sulfonated to form a metallated sulfonated styrenic block copolymer. In embodiments, the metallated sulfonated styrenic block copolymer has either a triblock, tetrablock, pentablock, or coupling structure, each structure being ABA, ABA', A'B'A'; ABB'A, ABA'A, ABB'A'; ABA'BA, ABABA, AA'BA'A, ABB'A'A, A'B'A'B'A'; (ABA) n X, (AB) n X, (BAB) n X, (ABAB) n X, (ABABA) n X, (A'B'A') n X, (A'B') n X, (B'A'B') nX, (A'B'A'B') n X or (A'B'A'B'A') n X, where n is an integer from 2 to 30, and X is the residue of a coupling agent. In embodiments, B and B' are the same or different and are independently derived from any of 1,4-isoprene units, 1,2-butadiene units, 1,4-butadiene units, and mixtures thereof. A and A' are the same or different and are independently derived from either (i) a para-substituted vinyl aromatic monomer or (ii) an unsubstituted vinyl aromatic monomer.
[0052] In an embodiment, SO - M + The functionalized block B or B' is generated from the hydrolyzed SBC in a Grignard reaction, the reactive nucleophile being S N It reacts with epoxides in reactions of type 2. The leaving group is the oxygen atom of the epoxide in the form of an alkoxide, which is converted to an alcohol in acidic workup.
[0053] In an embodiment, the SBC comprises a metal oxide and a C3-C 12 From the mixture with sultone compounds, SO3 - M + The metal oxides for the metallization step include lithium, cesium, sodium, potassium oxides and mixtures thereof. Examples of sultones include those containing a carbon-oxygen-sulfur-carbon bond in the ring, where the hexavalent sulfur atom is further bonded to two additional oxygen atoms. In embodiments, the sultones used for functionalization contain 6 to 12 carbon atoms. These sultones are characterized by minimal foam production. Examples include 1,3-propane sultone, 1,4-butane sultone, 1,3-butane sultone, long chain alkyl sultones (C6-C 12 ), tolylsultone, and mixtures thereof.
[0054] In an embodiment, SO - M + -SBC is represented by the following formula (II)
[0055] [ka] where R1 is H, CH3 or a t-butyl group, m and n are >1, A is an endblock comprising polymerized para-substituted vinyl aromatic monomers, and the midblock B before functionalization consists of ethylene and butylene or propylene units. It is a triblock having a structure according to the formula:
[0056] In an embodiment, the polymer block B comprises more than 95% of the functionalized units. - M + -SBC has a weight ratio of polymer block A to polymer block B of 15:5 to 19:1 or 16:4 to 18:2. - M + The degree of SBC functionalization is in the range of 30 mol% to 95 mol%, or 15 to 80 mol%, or 20 to 70 mol%, or 25 to 60 mol%, or is greater than 20 mol%, or greater than 50 mol%, based on the total number of monomer units.
[0057] In an embodiment, SO - M + -SBC is a tetrablock with the general structure of ABB'A, ABA'A and mixtures thereof.
[0058] In an embodiment, SO - M + -SBC is a pentablock having the general structure ABA'BA, AA'BA'A, ABABA, AA'BA'A and mixtures thereof.
[0059] In an embodiment, polymer blocks B and B' are midblocks, are the same or different, and are independently derived from 1,4-isoprene units, 1,2-butadiene units, 1,4-butadiene units, or mixtures thereof. Blocks A and A' can be midblocks or endblocks, are the same or different, and are independently derived from either i) para-substituted vinyl aromatic monomers or ii) unsubstituted vinyl aromatic monomers.
[0060] Partially hydrogenated metal sulfonated styrene block copolymer (SO3 - M + -pHSBC): In an embodiment, the SBC precursor is converted to SO - M + -SO3 before conversion to pHSBC - M + -Partially hydrogenated styrene block copolymers (pHSBC) are selected from the group consisting of styrene-ethylene / butylene-styrene (SE / BS), styrene-ethylene / butylene-styrene-ethylene / butylene-styrene block copolymers (S-EB-S-EB-S), styrene-ethylene / butylene / styrene-styrene (S-EB / SS), styrene-styrene / ethylene / butylene-styrene (SS / EB-S), styrene-ethylene / butylene-styrene-ethylene / propylene-styrene block copolymers (S-EB-S-EP-S), styrene-ethylene / propylene-styrene-ethylene / propylene-styrene block copolymers (S-EP-S-EP-S) and mixtures thereof.
[0061] The SBC precursor is partially hydrogenated, meaning that the hydrogenated conjugated diene has a hydrogenation level of 20-90%, or 25-85%, or more than 20%, or more than 40%, or less than 70%, or less than 80%, or less than 85%, or 50-85%, or 55-80%, or 60-75%. The hydrogenation level refers to the percentage of the original unsaturated bonds that become saturated upon hydrogenation. The hydrogenation level in the hydrogenated vinyl aromatic polymer can be determined using UV-VIS spectrophotometry and / or proton NMR. The hydrogenation level in the hydrogenated diene polymer can be determined using proton NMR.
[0062] In an embodiment, the partially hydrogenated block copolymer initially contains residual aliphatic double bonds in the polymer. The residual aliphatic double bonds provide excellent sites for reaction with functional groups. In an embodiment, the partially hydrogenated conjugated diene has a residual unsaturation or RU of less than 20 meq / g, or less than 15 meq / g, or less than 10 meq / g, or less than 8 meq / g, or greater than 3 meq / g, or less than 5 meq / g, or between 2 and 15 meq / g, or greater than 0.5 meq / g.
[0063] In an embodiment, the polymer blocks B and / or B' in the pHSBC have, after hydrogenation (derived from polymerized butadiene or isoprene monomers), an RU of less than 20 meq / g, or less than 15 meq / g, or less than 10 meq / g, or less than 8 meq / g, or greater than 3 meq / g, or less than 5 meq / g, or between 2 and 15 meq / g, or greater than 0.5 meq / g.
[0064] In embodiments, the pHSBC has an average 1,2-vinyl or 3,4-vinyl content of 5-75% by weight, or 15-45% by weight, or 20-40% by weight, or 25-35% by weight, or greater than 35% by weight or less than 50% by weight. The vinyl content may be measured via proton NMR before or after hydrogenation.
[0065] In an embodiment, each of polymer blocks B and B′ has polymerized 1,2 and 1,3-butadiene units in an amount of 40 to 70 wt.%, or 45 to 65 wt.%, or 50 to 60 wt.%, or greater than 45 wt.%, or less than 65 wt.%, based on the total 1,3-butadiene units in polymer block B.
[0066] In embodiments, each of polymer blocks B and B' has polymerized 3,4 isoprene units in an amount of 5 to 15% by weight, or 6 to 12% by weight, or 5 to 10% by weight, based on the total isoprene units in polymer block B.
[0067] In an embodiment, the pHSBC prior to hydrogenation has a polystyrene content of from 0 to 40% by weight, or from 15 to 35% by weight, or from 8 to 30% by weight, or less than 45% by weight, or less than 40% by weight.
[0068] In an embodiment, the pHSBC before hydrogenation has a molecular weight (M p ).
[0069] In an embodiment, SO - M + The -pHSBC copolymer has a triblock structure, with block B or B' consisting of polymerized ethylene, butylene or propylene units or mixtures thereof, and containing up to 20% non-hydrogenated units that are not functionalized. In an embodiment, the triblock SO3 - M + -pHSBC has a weight ratio of block A (and A') to block B (or B') in the range of 5:15 to 1:19 or 4:16 to 2:18.
[0070] Optional Additives: In an embodiment, SO - M +The -SBC composition further comprises optional additives selected from the group consisting of activators, curing agents, crosslinkers other than diamines, stabilizers, neutralizing agents, thickeners, coalescing agents, leveling agents, mold release agents, antiozonants, color changing pH indicators, plasticizers, tackifiers, film-forming additives, dyes, pigments, UV stabilizers, UV absorbers, other resins, redox couples, flame retardants, viscosity modifiers, wetting agents, degassing agents, colorants, heat stabilizers, light stabilizers, lubricants, flow improvers, anti-drip agents, anti-blocking agents, antistatic agents, processing aids, stress relief additives, binders, and mixtures thereof.
[0071] In embodiments, the optional additives further include low aspect ratio fillers to enhance toughness and overall strength or to achieve controlled porosity in the membrane, while high aspect ratio fillers are used to increase toughness and tensile strength in membranes that do not have a supporting structure.
[0072] In embodiments, the low aspect ratio fillers have an aspect ratio of less than 5, or less than 4, or less than 3, or less than 2, or less than 1.5, or greater than 1. The low aspect ratio fillers are selected from the group consisting of alkali metal and alkaline earth metal carbonates, sulfates and phosphates, and mixtures thereof. Examples include calcium carbonate, sodium carbonate, barium sulfate, calcium sulfate, sodium sulfate, sodium phosphate, potassium phosphate, calcium phosphate, and mixtures thereof. In embodiments, the high aspect ratio fillers have an aspect ratio of 50-1500, or 200-1400, or 350-1350, or 400-1250, or 500-1100. Examples include silicates, alumina, carbon, and mixtures thereof.
[0073] In an embodiment, the additive is SO3 - M + - used in an amount of up to 10 wt.%, or 0.1-10 wt.%, or 0.5-5 wt.%, or 1-10 wt.%, or 1-5 wt.%, based on the total weight of the SBC composition.
[0074] In an embodiment, SO- M + The SBC further comprises at least a plasticizer, high dielectric constant solvent, or liquid electrolyte to facilitate increased ionic conductivity. Examples of plasticizers include bis(2-ethylhexyl) phthalate (BEHP), dibutyl phthalate (DBP), diisobutyl phthalate (DIBP), or mixtures thereof. In embodiments, the high dielectric constant solvent is selected from propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), or mixtures thereof. In embodiments, the liquid electrolyte comprises an electrolyte such as LiPF6, LiBF4, LiClO4, LiTFSI, or SO3 - M + - Formed by dissolving in a solvent with a high dielectric constant prior to addition to the SBC (i.e. lithium salt).
[0075] Optional Polymer Component: In an embodiment, SO3 - M + The SBC composition is further blended with another polymer selected from the group consisting of polytetrafluoroethylene (PTFE), polyolefin, polyimide, polyamide, polyester, polystyrene, polysulfone, polyketone, poly(2,6 dimethyl 1,4 phenylene) ether, poly(p-phenylene oxide) (PPO), polyphenylene ether, polyisoprene, polybutadiene, polyvinylidene fluoride, polycarbonate, polyetherimide, ethylene-vinyl alcohol copolymer, polyvinylidene chloride, polyacrylate, polytertbutylstyrene, and mixtures thereof.
[0076] The molecular weight of the optional polymer component is - M +- can be adjusted to obtain miscibility between the SBC and the second (optional) polymer. In an embodiment, the optional polymer component is selected from PPOs having a molecular weight in the range of 1-15 kg / mol, or 2-12 kg / mol, 7-9 kg / mol, or 10-12 kg / mol. In an embodiment, the ratio of the MW of the second (optional) polymer to the MW of the A block is in the range of 5:1-1:2, or 4:1-3:1, or 2:1-1:1.
[0077] In an embodiment, SO - M + -The second polymer for blending with SBC is SO3 - M + - present in an amount of 0.1-50% by weight, or 1-35% by weight, or 5-30% by weight, or more than 15% by weight, or less than 25% by weight, or 15-25% by weight, relative to the weight of the polystyrene block of the SBC.
[0078] Acidifier: In an embodiment, SO - M + The SBC is further acidified with a strong acid solution selected from the group consisting of hydrochloric acid (HCL), hydrobromic acid (HBr), nitric acid (HNO3), hydroiodic acid (HI), hydrochloric acid (HCLO3), sulfuric acid (H2SO4) and mixtures thereof to obtain SO3H functionalization in the SBC. In embodiments, the degree of sulfonation in the block copolymer ranges from 30 mol% to 95 mol%, or 15 to 80 mol%, or 20 to 70 mol%, or 25 to 60 mol%, or greater than 20 mol%, or greater than 50 mol%, based on the total number of monomer units.
[0079] SO3 - M + -Method of forming block copolymer: SO3 - M +The functionalized block copolymer may be formed in a series of reaction steps. In embodiments, a precursor SBC is provided or prepared by known methods. The precursor may be prepared by sequential (or consecutive) polymerization of monomers in solution (in a solvent) in the presence of an initiator, with stepwise addition of monomers and initiator, followed by hydrogenation (or partial hydrogenation). The precursor may be prepared by coupling the resulting block copolymer with a coupling agent prior to the hydrogenation step.
[0080] In an embodiment, an epoxidized SBC is applied or an SBC precursor (applied or prepared) is epoxidized by known methods (e-SBC). In an embodiment, epoxidation of the SBC is carried out using a peracid exemplified by peracetic acid, hydrogen peroxide in the presence of acetic acid and sulfuric acid, or hydrogen peroxide in the presence of a low molecular weight fatty acid such as formic acid. Relatively low temperatures are utilized, for example 25-40° C., and reaction times of 0.5-4 hours are usually sufficient to achieve the high degree of epoxidation desired in the conjugated diene polymer block.
[0081] In embodiments, the e-SBC has a degree of epoxidation of 1-90%, or 1-99%, or 3-95%, or 5-90%, or 10-85%, or 10-80%, or 10-75%, or 10-60%, or 15-50%, or more than 15%, or more than 20%, relative to the polymer block susceptible to functionalization, i.e., block B. The amount of epoxy in the e-SBC can be determined by titration, FTIR or 1 It can be measured by HNMR.
[0082] The amount of functionalizing / epoxidizing agent added to the base block copolymer (hydrogenated SBC) varies based on the desired level of functionalization. In embodiments, the epoxidizing agent is added in an amount ranging from 0.1 to 20% by weight, or 0.5 to 15% by weight, or 1 to 12% by weight, or 2 to 10% by weight, based on the total weight of the base block copolymer.
[0083] In an embodiment, the epoxidized base polymer (e-SBC) has a degree of epoxidation of up to 100%, or 1-99%, or 5-90%, or 10-80%, or 20-70%, or 30-90%, or 40-80%, or greater than 40%, or greater than 50%, relative to the polymer block amenable to functionalization.
[0084] In embodiments, alcoholysis of e-SBC is carried out by reacting e-SBC with a Grignard reagent, for example, R-MgBr with S N Hydroxyl-SBC copolymers are then prepared by reacting in situ with a mixture of metal oxides and sultones in a ratio of 10:90 or 20:80 or 30:70 or 40:60 or 50:50 in an organic solvent or mixtures thereof to produce hydroxyl-SBC copolymers. - M + -SBC block copolymer. Examples of solvents include n-hexane, cyclohexane, methylene chloride, ethylene chloride, isopropyl alcohol, acetone, N,N-dimethylacetamide, 1-methyl-2-pyrrolidinone, 1,3-dioxolane, 2-methoxyethanol, dimethylformamide, benzyl alcohol, and mixtures thereof.
[0085] SO3 - M + The -SBC is further acidified using a strong acid solution to obtain SO3H functionalization.
[0086] In an embodiment, SO - M + -SBC can be used as flakes or in solution (solvent) or as pellets to prepare the final application. In an embodiment, SO3 in solution - M + The SBCs can also be fabricated into films or membranes for subsequent use in end applications.
[0087] SO3 - M +-Membrane or film containing SBC: In an embodiment, the SO3 formed - M + The SBC is dissolved in a solvent and then used to fabricate into a membrane or film. Examples of solvents include n-hexane, cyclohexane, methylene chloride, ethylene chloride, isopropyl alcohol, acetone, N,N-dimethylacetamide, 1-methyl-2-pyrrolidinone, 1,3-dioxolane, 2-methoxyethanol, dimethylformamide, benzyl alcohol, toluene, xylene, dimethylsulfoxide, and mixtures thereof.
[0088] In an embodiment, SO - M + In addition to the -SBC polymer, optional components including crosslinkers, additives, alkyl halide substituted non-SBC polymers, etc. may also be used / added to the solvent to form the membrane / film.
[0089] In embodiments, the membrane (film) is formed by known methods such as casting, electrospinning, extrusion, compression, coating such as dipping, flow coating, roll coating, bar coating, spray coating, curtain, rotogravure, brushing, wire wound rod coating, pan-fed reverse roll coating, electroless nickel coating, spraying, knife coating, spin coating, dip coating, slot die coating, ultrasonic spray coating, printing, film transfer, and the like. The film may be dried at 20° C.-210° C., or 30-180° C., or 35-150° C., or 40-100° C., with or without vacuum, in a continuous or batch process. In embodiments, the film is a stand-alone film or is supported by an ion-permeable substrate such as glass, carbon or other woven or nonwoven mats, polymers or filled polymers, plastic films, ceramics, porcelain porous rigid substrates, and the like.
[0090] In another embodiment, the membrane (film) is formed directly on the electrode of the energy storage device using methods such as casting, electrospinning, extrusion, compression, coating, such as dipping, flow coating, roll coating, bar coating, spray coating, curtain, rotogravure printing, brushing, wire-wound rod coating, pan-fed reverse roll coating, electroless nickel coating, spraying, knife coating, spin coating, dip coating, slot die coating, ultrasonic spray coating, printing, film transfer, etc. In the case of lithium-ion batteries, the membrane (film) can be formed directly on the cathode or anode. Suitable electrodes are cathodes made of materials such as lithium nickel manganese cobalt oxide (NMC) or lithium iron phosphate, and anodes made of materials such as graphite, silicon-containing graphite, and lithium metal.
[0091] In an embodiment, SO - The H-SBC membrane has a thickness of 0.1 to 500 μm, or 1 to 200 μm, or 50 to 300 μm, or 3 to 100 μm, or 1 to 50 μm, or 5 to 45 μm, or 5 to 40 μm, or 20 to 150 μm, or 12 to 25 μm, or more than 0.1 μm or less than 50 μm.
[0092] SO3 - Further processing of H-SBC membrane or film: In an embodiment, SO - The H-SBC is cross-linked with a cross-linking agent, such as glycol, polyethylene glycol (PEG), etc. - The amount of H-SBC to crosslinker is in a ratio of 98:2 to 95:5 mol %, or 90:10 to 80:20 mol %, or 75:25 to 70:30 mol %, or 60:40 to 55:35 mol %. - The H-SBC is dissolved in a binary mixture of toluene / isopropanol and the crosslinker is dissolved separately in a toluene solution. The two solvent systems are mixed together and cast onto a substrate to form a film or membrane.
[0093] Properties: SO3 - H-SBC or SO3 - M + From SBC or polyethylene glycol (PEG) cross-linked SO3 - The films / membranes obtained from H-SBC are elastic and have low swelling properties. The films are highly dimensionally stable and have high ion transport properties, methanol resistance, barrier properties, hardness, thermal / oxidative stability and anti-fouling properties.
[0094] In an embodiment, SO - M + The SBC film has an ion exchange capacity (IEC) of 0.5 to 3.5 meq / g, or 1.2 to 3.0 meq / g, or 1.5 to 3 meq / g, or more than 1 meq / g, or less than 2 meq / g, or less than 3 meq / g, or more than 0.5 meq / g.
[0095] In an embodiment, SO - The crosslinked film of H-SBC and PEG has an ion exchange capacity (IEC) of 1.0 to 3 meq / g, or 1.2 to 3.0 meq / g, or 1.5 to 3 meq / g, or more than 1 meq / g, or less than 2 meq / g, or less than 3 meq / g, or more than 0.5 meq / g.
[0096] In an embodiment, SO - M + The SBC film has a Young's modulus of 100 to 2000 MPa, or 500 to 1000 MPa, or 600 to 800 MPa.
[0097] In an embodiment, SO - The crosslinked film of H-SBC and PEG has a Young's modulus of 100 to 2000 MPa, or 500 to 1000 MPa, or 600 to 800 MPa.
[0098] In an embodiment, SO - M + The SBC film has a tensile strength of 2 to 30 MPa, or 7 to 25 MPa, or 10 to 20 MPa, or 5 to 20 MPa, or 7 to 18 MPa, or 10 to 25 MPa.
[0099] In an embodiment, SO - The crosslinked film of H-SBC and PEG has a tensile strength of 2 to 30 MPa, or 7 to 25 MPa, or 10 to 20 MPa, or 5 to 20 MPa, or 7 to 18 MPa, or 10 to 25 MPa.
[0100] In an embodiment, SO - M + -SBC film is 1~8MJ / m 3 Or 1.5 to 6 MJ / m 3 Or 1 to 5 MJ / m 3 It has toughness of .
[0101] In an embodiment, SO - The crosslinked film of H-SBC and PEG has a thermal conductivity of 1-8MJ / m 3 Or 1.5 to 6 MJ / m 3 Or 1 to 5 MJ / m 3 It has toughness of .
[0102] In an embodiment, SO - M + The SBC film has an elongation at break of 10-150%, or more than 100%, or less than 150%, or more than 20%, or more than 35%, or 15-50%, or 25-75%, or 35-90%.
[0103] In an embodiment, SO - The crosslinked film of H-SBC and PEG has an elongation at break of 10 to 150%, or more than 100%, or less than 150%, or more than 20%, or more than 35%, or 15 to 50%, or 25 to 75%, or 35 to 90%.
[0104] In an embodiment, SO - M + The SBC film has a water absorption capacity (or swelling degree) after 24 hours (weight gain in deionized water at 80°C) of 5 to 100% by weight, or 10 to 90% by weight, or 20 to 80% by weight, or 30 to 60% by weight, or 10 to 50% by weight, or 30 to 80% by weight, based on the total initial weight of the film (before immersing the film in water).
[0105] In an embodiment, SO - The crosslinked film of H-SBC and PEG has a water supplying ability (after 24 hours) of 5 to 100% by weight, 10 to 90% by weight, 20 to 80% by weight, 30 to 60% by weight, 10 to 50% by weight, or 30 to 80% by weight, based on the total initial weight of the film.
[0106] In an embodiment, SO - M + The SBC films have a swelling degree after 1 week in 80° C. deionized water of less than 70%, or less than 90%, or less than 100%, or less than 120%, or less than 150%, or less than 200%, or less than 250%, or 40-300%, or 50-250%, or 60-220%, or 70-200%, or 80-180%, or 100-160%, based on the total initial weight of the film.
[0107] In an embodiment, SO - The crosslinked copolymer film of H-SBC and PEG has a swelling degree after 1 week in 80° C. deionized water of less than 70%, or less than 90%, or less than 100%, or less than 120%, or less than 150%, or less than 200%, or less than 250%, or 40-300%, or 50-250%, or 60-220%, or 70-200%, or 80-180%, or 100-160%, based on the total initial weight of the film. (SO3 - M + Properties of Li-ion batteries containing SBC films: SO3 - M + SBC (in the formula, M + =Li + Films of the composition are expected to exhibit excellent discharge capabilities when used in batteries / cells.
[0108] In an embodiment, SO - M +- The Li-ion battery containing the SBC film has electrochemical stability of 1-12V or 2-10V or 2.5-8V or 3-6V or 3.5-5.5V or 4-7V or greater than 4V or less than 10V. Electrochemical stability refers to the control of the open circuit voltage of the polymer electrolyte.
[0109] In an embodiment, the Li-ion battery has a retention capacity of greater than 80%, or greater than 85%, or greater than 90%, or greater than 95%, or greater than 97%, or less than 99.5% of the first cycle after at least 1000 charge / discharge cycles at room temperature. The retention capacity of a Li-ion battery refers to the battery's ability to fully charge or discharge after it has been used for a period of time or when it has been left unused for an extended period of time.
[0110] Application: Acidified-sulfonated block copolymer composition (SO3 - H-SBCs) can be used in applications including electrochemical, e.g. submersible electrolysers, cation exchange membranes for fuel cells, membrane electrode assemblies, acid batteries (electrolyte separators), supercapacitors (electrolytes); separation cells for metal recovery processes (electrolyte barriers); sensors (especially for sensing humidity); energy storage solutions such as in vanadium or iron redox flow battery membranes.
[0111] In an embodiment, SO - The H-SBC compositions are for use in energy storage devices, including flow batteries, hydrogen generation, CEMs for water electrolysis, water splitting, and the like.
[0112] In an embodiment, SO - M + The SBC composition is for use as a component of an energy storage device, for example, in either a current collector, electrode, or separator (as a binder). - M + -SBC is coated or deposited on the porous separator. - M +In yet another embodiment, the -SBC layer is coated on at least one side of the separator. - M + -Coated with an SBC composition. EXAMPLES
[0113] The following examples are non-limiting.
[0114] The following tests were carried out:
[0115] The epoxide ring-opening reaction and subsequent quaternization reaction were characterized by FT-IR (Nicolet-iS-50 FTIR spectrometer equipped with an attenuated total reflectance (ATR) attachment). The film was placed directly on the ATR diamond and the spectrum was recorded at room temperature.
[0116] The epoxide ring-opening reaction was further characterized by differential scanning calorimetry (DSC) from −75° C. to 250° C. using a TA Instruments Q2000.
[0117] Mechanical properties including toughness, Young's modulus, tensile strength and elongation at break were measured according to ASTM D412.
[0118] The components used in the examples include the following:
[0119] The precursor USBCs are for use in making partially hydrogenated styrenic block copolymer (p-HSBC) precursors. USBC, p-HSBC-1, p-HSBC-2, at different PSC content (polystyrene), residual unsaturation (RU) levels and MFR are as provided in Table 1 of the SBCs used in the examples.
[0120] [Table 1]
[0121] Example 1 -Epoxidation of SBC: The SBC in Table 1 was dissolved in cyclohexane at a temperature of 40°C. The formic acid level was varied to adjust the level of epoxidation. A 1.0:0.5 molar solution of formic acid and hydrogen peroxide was first reacted to form performic acid. The solution was added to the SBC in cyclohexane and stirred for 1 hour. The reaction was carried out in a batch reactor operating at 60°C for a reaction time of 3-4 hours. All reactants were immediately neutralized with sodium bicarbonate to avoid secondary reactions. The reaction mixture was washed twice with 10% aqueous sodium bicarbonate. The polymer was precipitated in isopropyl alcohol (IPA), washed, and 1 The epoxy content was determined by HNMR analysis.
[0122] Each of the resulting products (from the epoxidation of the SBCs in Table 1) is referred to as epoxidized e-SBC.
[0123] Example 2 -Hydroxy-SBC: 6 g of e-SBC (three epoxidized e-SBC products from Example 1) was dissolved in 250 ml of THF. The reaction mixture was then cooled to 10° C. under N2. 0.67 g of CuCl2 was added to the cooled reaction mixture and stirred well for 10 minutes. 2.2 ml of CH3MgBr2 was added slowly to the stirred reaction mixture (raising the temperature to 25-30° C.). Stirring was continued for 3 hours and then the reaction mixture was quenched with 100 ml of 10% AlCl3. The solution was acidified with 1.5 N HCl and extracted with dichloromethane followed by washing to obtain the crude product, which was precipitated in methanol and dried well to obtain hydroxy-SBC.
[0124] Example 3 Lithiation and Sulfonation of -Hydroxy-SBC: For the three products of Example 2, 3 g of hydroxy SBC was dissolved in 200 ml of THF followed by stirring for 30 minutes. 6 ml of lithium tert-butoxide was added to the stirred solution and stirring was continued for 1 hour at 60-70°C. After stirring overnight, 1.05 ml of 1,3 propane sultone was added at 60-70°C. The reaction mixture was cooled to room temperature. The solvent was evaporated to give SO3 - Li + -SBC was obtained and then dissolved in a methanol solution, and the solution was then cast onto a substrate to form a film or membrane.
[0125] Example 4 -SO3 - Li + -SO3 from SBC - H-SBC: The reaction product SO3 in THF obtained in Example 3 - Li + Each of the -SBCs was mixed with 1.5N HCl and stirred for 3-4 hours. The THF was distilled off under vacuum and the viscous product was precipitated in methanol, dried under vacuum and dehydrated with SO3 - The H-SBC product was then dissolved in a methanol solution and cast onto a substrate to form a film or membrane.
[0126] Example 5 -SO3 - Crosslinking of H-SBC with PEG1000: SO3 - The solution of H-SBC is mixed with a suitable amount of SO - H-SBC is prepared by dissolving in toluene / isopropanol solvent. A suitable amount of crosslinker PEG1000 is separately dissolved in the toluene solution. The two solvent systems are mixed together with stirring for a sufficient time (30 minutes). The solution is cast onto a substrate to form a film or membrane.
[0127] Example 6 - SO3 - M + -PPO blending with SBC, i.e. PPO and SO3 - M +-SBC blends were performed with PPO samples and SO3 - M + The e-SBC samples are separately prepared by dissolving them in chloroform solution in a suitable ratio (wt% of PPO to wt% of polystyrene (PS) component of e-SBC). A solution of PPO in chloroform is first prepared and thoroughly stirred to ensure complete dissolution. This solution is diluted with SO3 - M + -Add to a premixed chloroform solution of the SBC sample. The solution is further stirred to further ensure complete dissolution. The premixed chloroform solution is cast onto a substrate, followed by evaporation of the solvent to form a film.
[0128] Although the terms "comprising" and "including" are used herein to describe various embodiments, the terms "consisting essentially of" and "consisting of" can be used in place of "comprising" and "including" to provide more specific embodiments of the present disclosure and are disclosed.
Claims
1. A metallated sulfonated styrene block copolymer comprising any of a triblock, tetrablock, pentablock, and coupling structure, each structure being: ABA, ABA', A'B'A'; ABB'A, ABA'A, ABB'A'; ABA'BA, AA'BA'A, ABABA, AA'BA'A, ABB'A'A, A'B'A'B'A'; (ABA) n X, (AB) n X, (BAB) n X, (ABAB) n X, (ABABA) n X, (A'B') n , (A'B') n (A'), (A'B'A') n , (A'B'A') n X, (A'B') n X, (B'A'B') n X, (A'B'A'B') n X or (A'B'A'B'A') n X (In the formula, n is an integer from 2 to 30; X is a residue of a coupling agent; Prior to hydrogenation, B and B' are the same or different and are independently derived from 1,4-isoprene units, 1,2-butadiene units, 1,4-butadiene units, and mixtures thereof; blocks A and A′ are the same or different and are independently derived from either (i) para-substituted vinyl aromatic monomers or (ii) unsubstituted vinyl aromatic monomers; Each of blocks B and B′ is an intermediate block and has the following formula (I): 【Chemistry 1】 (M + is Na + , K + , Li + , Cs + , Ag + , Hg + and Cu + is selected from the group consisting of (CH 2 ) y (wherein y is 3 to 12) is a spacer group. Metalated sulfonated (SO 3 - M + ) groups) The general structure of the present invention is as follows: having an ion exchange capacity (IEC) of 0.5 to 8.0 meq / g as measured in accordance with ASTM D7131-05; Metallated sulfonated styrene block copolymers.
2. Blocks B and B' each independently comprise 30 to 100 mol % of a metal sulfonated (SO 3 - M + 2. The metallized sulfonated styrenic block copolymer of claim 1 having a degree of .
3. The following formula (II) 【Chemistry 2】 (In the formula, R 1 is H, CH 3 or a t-butyl group, m and n are >1; Block A is an endblock comprising polymerized para-substituted vinyl aromatic monomers; The intermediate block B before functionalization consists of ethylene units and butylene units or propylene units. is a triblock having a structure according to 3. The metallated sulfonated styrene block copolymer of claim 1 or 2.
4. ABB'A, ABA'A, ABB'A' where blocks A and A' are the same or different polymer midblocks or endblocks, and are independently derived from either (i) para-substituted vinyl aromatic monomers or (ii) unsubstituted vinyl aromatic monomers. and mixtures thereof.
3. The metallated sulfonated styrene block copolymer of claim 1 or 2.
5. ABA'BA, AA'BA'A, ABABA, AA'BA'A, ABB'A'A, A'B'A'B'A' where blocks A and A' are midblocks or endblocks, are the same or different, and are independently derived from either (i) para-substituted vinyl aromatic monomers or (ii) unsubstituted vinyl aromatic monomers. and mixtures thereof.
3. The metallated sulfonated styrene block copolymer of claim 1 or 2.
6. S-CD-S, S-CD-CD', S'-CD-S'; S-CD-CD'-S, S-CD-S'-S, S-CD-CD'-S'; S - CD - S' - CD - S, S - CD - S - CD - S, SS' - CD - S'S, S - CD - CD' - S' - S, S' - CD' - S' - CD' - S', (S - CD - S) n X, (S - CD) n X, (CD - S - CD) n X, (S - CD - S - CD) n X, (S - CD - S - CD - S) n X, (S' - CD' - S') n X, (S' - CD') n X, (S' - CD' - S'CD') n X or (S' - CD' - S' - CD' - S') n X (In the formula, n is an integer from 2 to 30, X is a residue of a coupling agent; CD and CD' are the same or different and are independently derived from 1,4-isoprene units, 1,2-butadiene units, 1,4-butadiene units, or a mixture thereof; S and S' are the same or different and are independently derived from either (i) a para-substituted vinyl aromatic monomer or (ii) an unsubstituted vinyl aromatic monomer. by sulfonating and metallating a styrene block copolymer precursor having the general structure 3. The metallated sulfonated styrene block copolymer of claim 1 or 2.
7. M + Li + 7. The metallized sulfonated styrenic block copolymer of claim 6, obtained by sulfonation and lithiation of said styrenic block copolymer precursor.
8. 7. The metallized sulfonated styrenic block copolymer of claim 6, wherein the styrenic block copolymer precursor is a partially hydrogenated styrenic block copolymer, the partially hydrogenated styrenic block copolymer having a residual unsaturation level of 0.5 to 15 meq / g.
9. C 3 ~C 12 The CH 2 The spacer group is 1,3-propane sultone, 1,4-butane sultone, 1,3-butane sultone, C 6 ~C 12 3. The metallated sulfonated styrenic block copolymer of claim 1 or 2, which is derived from a sultone selected from the group consisting of alkyl sultones, tolylsultones, and mixtures thereof.
10. 3. An energy storage device comprising the metallized sulfonated styrenic block copolymer of claim 1 or 2, wherein the metallized sulfonated styrenic block copolymer is applied as any of an electrode binder, an electrode, a separator, and an electrolyte.
11. 11. The energy storage device of claim 10, which is any one of a lithium ion primary battery, a lithium ion secondary battery, a capacitor, a supercapacitor, a fuel cell, a metal-sulfur battery, a sodium-ion battery, and a metal-air battery.
12. A film comprising the metallized sulfonated styrenic block copolymer of claim 1 or 2.
13. 13. The film of claim 12 applied over a microporous membrane comprising a polyolefin selected from the group consisting of modified polyolefins, polyethylene, polypropylene, polymethylpentene, and mixtures thereof.
14. The metallated sulfonated styrene block copolymer is dissolved in a liquid electrolyte, the liquid electrolyte comprising a lithium salt dissolved in a solvent selected from the group consisting of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, or mixtures thereof, the lithium salt being LiPF 6 , LiBF 4 , LiClO 4 3. The metallated sulfonated styrenic block copolymer of claim 1 or 2, comprising LiTFSI, LiTFSI, and mixtures thereof.
15. 1. A method for preparing a membrane for use in an electrochemical application, comprising the steps of: acidifying the metallated sulfonated styrenic block copolymer of claim 1 or 2 with an acid solution selected from the group consisting of hydrochloric acid, hydrobromic acid, nitric acid, hydroiodic acid, chloric acid, sulfuric acid, and mixtures thereof to form a sulfonated styrenic block copolymer; crosslinking the sulfonated styrene block copolymer with polyethylene glycol; and Casting the crosslinked sulfonated styrenic block copolymer to form a film, the film having a swelling degree in water of less than 250% based on the total initial weight of the film after one week. A method comprising: