Production method of carbon nanotube dispersion paste and production method of mixed material paste for lithium ion secondary battery

A method using a resin with specific polar functional groups, N-methyl-2-pyrrolidone, and controlled water content addresses high viscosity and concentration issues in carbon nanotube dispersions, enhancing dispersibility, stability, and recyclability for improved battery electrode performance and sustainability.

JP2024170340APending Publication Date: 2024-12-06KANSAI PAINT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024165359
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-09-24
Publication Date
2024-12-06

Smart Images

  • Figure 2024170340000001
    Figure 2024170340000001
  • Figure 2024170340000002
    Figure 2024170340000002
  • Figure 2024170340000003
    Figure 2024170340000003
Patent Text Reader

Abstract

To provide a production method of a carbon nanotube dispersion paste excellent in solvent recyclability, pigment dispersibility, and storage stability, a production method of a mixed material paste, and an electrode layer for a lithium ion secondary battery excellent in performances (a finishing property, a battery performance, etc.).SOLUTION: A production method of a carbon nanotube dispersion paste includes mixing and dispersing components including a pigment dispersion resin (A), a carbon nanotube (B), N-methyl-2-pyrrolidone (C), and an amine compound (D) to obtain the paste. The pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphonic acid group, a silanol group, a cyano group, a pyrrolidone group, and an amino group. The pigment dispersion resin (A) has a polar functional group concentration of 0.3 mmol / g or more and 23 mmol / g or less. A formula (Xc)-10>(Xd) is shown where the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a carbon nanotube dispersion paste (also referred to as a conductive pigment paste in the present invention) having excellent solvent recyclability, pigment dispersibility, and storage stability, a method for producing a composite paste (for lithium ion secondary batteries), and a method for producing a battery electrode layer having excellent battery performance. [Background technology]

[0002] Conventionally, paste-like pigment dispersions in which a pigment is dispersed in a mixture of a pigment dispersing resin and a solvent have been widely used in the fields of paints, battery electrodes, coating materials, coating materials, electromagnetic shields, display panels, touch screen panels, colored films, colored sheets, decorative materials, protective materials, magnet modifiers, printing inks, device members, electronic device members, printed wiring boards, solar cells, functional rubber members, resin molded films, etc. Furthermore, conductive pigments, conductive polymers, etc. are contained in these materials to impart functions such as electrostatic paintability, conductivity, electromagnetic shielding properties, and antistatic properties.

[0003] In these fields, there is an increasing demand for improvements in performance such as pigment dispersibility, storage stability, electrical conductivity, coatability, and finish. For this reason, pigment dispersing resins and pigment pastes that have excellent pigment dispersing ability and excellent pigment dispersion stability that prevents re-aggregation of pigment particles in the formed pigment dispersion are being developed.

[0004] In designing a pigment paste, it is important to prepare a pigment paste with a high concentration and uniform dispersion using as small an amount of solvent and pigment dispersion resin as possible, so that the pigment dispersion resin does not adversely affect the conductive properties of the final product itself, such as the coating film, or from the viewpoint of reducing the amount of solvent and pigment dispersion resin used and reducing the energy used during drying. In addition, there is a demand for the recycling suitability of waste generated during the manufacturing process in order to reduce waste, be environmentally friendly, and reduce costs.

[0005] For example, Patent Document 1 discloses a method for producing an electrode slurry for a lithium secondary battery, which is characterized by dispersing a solvent containing fibrous carbon with a media (hereinafter sometimes written as "media") type disperser to obtain a slurry, kneading the slurry with an electrode active material, and applying the resulting mixture to a current collector to obtain a slurry. However, in the case of a paste with a high pigment concentration and / or high viscosity, uniform dispersion may not be achieved, and storage stability may be poor. In particular, when the slurry contains a large amount of water, high viscosity or gelation may occur. Furthermore, there is no particular disclosure regarding waste recycling. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-182892 A Summary of the Invention [Problem to be solved by the invention]

[0007] The object of the present invention is to provide a method for producing a carbon nanotube-dispersed paste and a method for producing a composite paste that are excellent in pigment dispersibility, storage stability, and solvent recyclability even in pastes with high pigment concentrations and / or high viscosity, and further to provide a method for producing a coating film (electrode layer for batteries) that is excellent in finish properties, etc. [Means for solving the problem]

[0008] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by a method for producing a carbon nanotube dispersion paste obtained by mixing and dispersing components containing a pigment dispersion resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), in which the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, and the polar functional group concentration of the pigment dispersion resin (A) is 0.3 mmol / g or more and 23 mmol / g or less, and when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc) ° C. and the boiling point of the amine compound (D) is (Xd) ° C., (Xc)-10>(Xd). This has led to the completion of the present invention.

[0009] That is, the present invention provides the following method for producing a carbon nanotube dispersion paste, a method for producing a composite paste, and a method for producing an electrode layer for a lithium ion secondary battery. Item 1. A method for producing a carbon nanotube dispersion paste obtained by mixing and dispersing components including a pigment dispersion resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), the pigment dispersing resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, and the concentration of the polar functional group in the pigment dispersing resin (A) is 0.3 mmol / g or more and 23 mmol / g or less; A method for producing a carbon nanotube dispersion paste, wherein, when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, (Xc)-10>(Xd). Item 2. A method for producing a carbon nanotube dispersion paste according to Item 1, wherein the N-methyl-2-pyrrolidone (C) is a recycled product, the moisture content in the N-methyl-2-pyrrolidone (C) is controlled to 10,000 ppm or less, and the content of an amine compound in the N-methyl-2-pyrrolidone (C) is controlled to 10,000 ppm or less. Item 3. The method for producing a carbon nanotube-dispersed paste according to Item 1 or 2, wherein the carbon nanotube-dispersed paste has a water content of 10,000 ppm or less. Item 4. The method for producing a carbon nanotube-dispersed paste according to any one of Items 1 to 3, wherein the content of the carbon nanotubes (B) is 0.1 mass % or more and less than 15 mass % based on 100 mass % of the total amount of the carbon nanotube-dispersed paste. Item 5. The method for producing a carbon nanotube-dispersed paste according to any one of Items 1 to 4, wherein the carbon nanotube-dispersed paste further contains polyvinylidene fluoride (E). Item 6. A method for producing a composite paste for a lithium ion secondary battery, comprising a step of mixing an electrode active material (G) with a carbon nanotube dispersion paste obtained by the method for producing a carbon nanotube dispersion paste according to any one of items 1 to 5. Item 7. A method for producing an electrode layer for a lithium ion secondary battery, comprising coating a lithium ion secondary battery composite paste obtained by the method for producing a lithium ion secondary battery composite paste according to item 6 on a current collector. Item 8. A step of coating a lithium ion secondary battery composite paste obtained by the method for producing a lithium ion secondary battery composite paste according to item 6 on a current collector and drying it by heating; A step of recovering a vapor containing N-methyl-2-pyrrolidone (C) and an amine compound (D) to produce a mixed solution; a step of separating the amine compound (D) from the mixed solution to produce a regenerated product of N-methyl-2-pyrrolidone (C); A method for producing an electrode layer for a lithium ion secondary battery containing N-methyl-2-pyrrolidone (C) and a method for producing a recycled product of N-methyl-2-pyrrolidone (C). Effect of the Invention

[0010] The method for producing a carbon nanotube-dispersed paste of the present invention is excellent in recyclability, pigment dispersibility, and storage stability (suppression of thickening) even at a high pigment concentration and / or high viscosity, and can sufficiently reduce the viscosity of the paste with a relatively small amount of dispersion resin. In addition, the coating film (battery electrode layer) is excellent in finish and battery performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail.

[0012] It should be understood that the present invention is not limited to the following embodiments, but includes various modified examples that are implemented within the scope that does not deviate from the gist of the present invention. In the present invention, the paste containing carbon nanotubes is called a "carbon nanotube dispersion paste", but it can also be called an "conductive pigment paste". The carbon nanotubes can also be abbreviated as "CNT." The paste prepared by further mixing at least one electrode active material and, optionally, other various components in order to coat the carbon nanotube dispersion paste is called a "composite paste." The composite paste that is coated on a substrate and dried is called a "coating film" or a "composite layer." It can be said that the carbon nanotube dispersion paste is a paste that does not substantially contain an electrode active material. When the coating film is used as an electrode for a battery, it can also be called an "electrode layer."

[0013] In the present invention, the carbon nanotube dispersion paste contains a specific pigment dispersion resin (A) and an amine compound (D), so that the pigment dispersibility is good and the increase in viscosity and gelation during storage can be suppressed. Furthermore, by making the water content of the carbon nanotube dispersion paste 10,000 ppm or less [and the water content of N-methyl-2-pyrrolidone (C) 10,000 ppm or less], the increase in viscosity and gelation during storage can be suppressed.

[0014] The mechanism by which the carbon nanotube dispersion paste and the composite paste become viscous and gel is not clear, but the following mechanism is presumed.

[0015] For example, in carbon nanotube dispersion paste and composite paste containing polyvinylidene fluoride, the acidity of the proton adjacent to the fluorine group in polyvinylidene fluoride is very high due to the electron-attracting property of the fluorine group, so that this proton desorption proceeds easily, especially under basic conditions. It is speculated that such proton desorption is particularly likely to proceed when moisture is present in the carbon nanotube dispersion paste and composite paste. After proton desorption, anions are generated on the carbon, which promotes the desorption of the fluorine group, and double bonds are generated in the main chain of the polyvinylidene fluoride molecule. It is speculated that the multiple polyvinylidene fluoride molecules that have double bonds are polymerized and further polymerized, leading to an increase in viscosity and gelation. In particular, since the electrode active material in the composite paste may contain lithium hydroxide, which is a relatively strong base, the increase in viscosity and gelation are remarkable in the composite paste.

[0016] In the present invention, it is believed that by using raw materials with a specified moisture content and by specifying the moisture content of the carbon nanotube dispersion paste and composite paste, polymerization of the polymer component (polyvinylidene fluoride) is suppressed, and the increase in viscosity and gelation of the carbon nanotube dispersion paste or composite paste can be suppressed. Furthermore, since the moisture is brought in from various raw materials (particularly solvents) and mixed in from water vapor contained in the air during the manufacturing process, it is practically impossible to reduce the moisture to zero. Therefore, the water content (lower limit) of the carbon nanotube dispersion paste that can be used in the present invention is preferably 100 ppm or more, more preferably 200 ppm or more, and even more preferably 500 ppm or more. The water content (lower limit) of N-methyl-2-pyrrolidone (C) is preferably 100 ppm or more, more preferably 200 ppm or more, and even more preferably 500 ppm or more. If the moisture content is within the above lower limit, the product can be produced without excessive moisture content control of the raw materials (reduction of moisture content) or excessive moisture content control in the production process (reduction of moisture contamination).

[0017] In the present invention, the recyclability of the solvent (mainly N-methyl-2-pyrrolidone) discharged during the production of an electrode layer for a lithium ion secondary battery is particularly important in terms of reducing waste and the environment, and when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, (Xc)-10>(Xd).

[0018] [Method of manufacturing carbon nanotube dispersion paste] The present invention relates to a method for producing a carbon nanotube dispersion paste obtained by mixing and dispersing components including a pigment dispersion resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), wherein the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, the concentration of the polar functional group in the pigment dispersion resin (A) is 0.3 mmol / g or more and 23 mmol / g or less, and when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, (Xc)-10>(Xd).

[0019] The water content (upper limit) of the carbon nanotube dispersion paste is usually 10000 ppm or less, preferably 7500 ppm or less, more preferably 5000 ppm or less, further preferably 2500 ppm or less, and particularly preferably 1000 ppm or less. The carbon nanotube dispersion paste used in the present invention can be said to be a substantially non-aqueous paste.

[0020] In the present invention, the water content can be measured by Karl Fischer coulometric titration. Specifically, the water content can be measured by using a Karl Fischer moisture meter (manufactured by Kyoto Electronics Manufacturing Co., Ltd., product name "MKC-610") and setting the temperature of a moisture vaporizer (manufactured by Kyoto Electronics Co., Ltd., product name "ADP-611") provided in the device at 130°C.

[0021] Pigment dispersing resin (A) The pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of amide, imide, hydroxyl, carboxyl, sulfonic acid, phosphoric acid, silanol, cyano, pyrrolidone, and amino groups, and the concentration of the polar functional group in the pigment dispersion resin (A) is 0.3 mmol / g or more and 23 mmol / g or less. The acid group may be in the form of a salt. Among them, as the polar functional group, it is preferable to use at least an amide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphoric acid group, and an amino group, and it is more preferable to use at least a hydroxyl group, a carboxyl group, and an amino group. The pigment dispersion resin (A) preferably has an alkyl group having 12 or more carbon atoms. Any known alkyl group (hydrocarbon group) can be used as the alkyl group having 12 or more carbon atoms without any particular limitation, and is preferably a linear or branched alkyl group, more preferably a linear alkyl group. The alkyl group having 12 or more carbon atoms is preferably an alkyl group having 12 or more and less than 30 carbon atoms, more preferably an alkyl group having 15 or more and less than 26 carbon atoms, and even more preferably an alkyl group having 19 or more and less than 24 carbon atoms. The alkyl group having 12 or more carbon atoms can be introduced into the resin, for example, by (co)polymerizing a polymerizable monomer containing an alkyl group having 12 or more carbon atoms. Examples of polymerizable monomers containing an alkyl group having 12 or more carbon atoms include lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, lauryl (meth)acrylamide, stearyl (meth)acrylamide, behenyl (meth)acrylamide, etc. These may be used alone or in combination of two or more. It is believed that when the pigment dispersing resin (A) has a relatively bulky side chain of an alkyl group having 12 or more carbon atoms, the pigment dispersibility and storage stability are improved due to steric repulsion.

[0022] The type of resin is not particularly limited as long as it is a resin other than polyvinylidene fluoride (E) described later. For example, acrylic resin, polyester resin, epoxy resin, polyether resin, alkyd resin, urethane resin, polyvinyl alcohol, polyvinyl acetal, polyvinylpyrrolidone, polyvinyl acetate, silicone resin, polycarbonate resin, chlorine-based resin, and composite resins thereof can be mentioned. These resins can be used alone or in combination of two or more. Among these, from the viewpoints of pigment dispersibility, storage stability, finish quality, and the like, it is preferable for the pigment dispersing resin (A) to contain a vinyl (co)polymer (A1) obtained by polymerizing or copolymerizing a monomer containing a polymerizable unsaturated group-containing monomer of the following formula (1), and in particular, an acrylic resin (co)polymerized with at least one polymerizable unsaturated group-containing monomer that contains a (meth)acryloyl group is preferred. Incidentally, the "(co)polymer" of the present invention includes both a polymer obtained by polymerizing one type of monomer and a copolymer obtained by copolymerizing two or more types of monomers.

[0023] C(-R)2=C(-R)2...Equation (1) [In the above formula, R may be the same or different and is a hydrogen atom or an organic group.] Examples of the vinyl (co)polymer (A1) include hydroxyl group-containing vinyl (co)polymer, carboxyl group-containing vinyl (co)polymer, amide group-containing vinyl (co)polymer, sulfonic acid group-containing vinyl (co)polymer, phosphoric acid group-containing vinyl (co)polymer, pyrrolidone group-containing vinyl (co)polymer, amino group-containing (co)polymer, etc. These (co)polymers may be used alone or in combination of two or more.

[0024] Examples of hydroxyl group-containing vinyl (co)polymers include polyhydroxyethyl (meth)acrylate, polyvinyl alcohol, vinyl alcohol-fatty acid vinyl copolymer, vinyl alcohol-ethylene copolymer, vinyl alcohol-(N-vinylformamide) copolymer, copolymers of hydroxyethyl (meth)acrylate and other polymerizable unsaturated monomers, etc. The vinyl alcohol units in the (co)polymer may be obtained by (co)polymerizing fatty acid vinyl units and then hydrolyzing them.

[0025] Examples of the carboxyl group-containing vinyl (co)polymer include a polymer of (meth)acrylic acid, and a copolymer of poly(meth)acrylic acid and other polymerizable unsaturated monomers.

[0026] Examples of the amide group-containing vinyl (co)polymer include a polymer of (meth)acrylamide, and a copolymer of (meth)acrylamide and other polymerizable unsaturated monomers.

[0027] Examples of the sulfonic acid group-containing vinyl (co)polymer include polymers of allylsulfonic acid or styrenesulfonic acid, and copolymers of allylsulfonic acid and / or styrenesulfonic acid with other polymerizable unsaturated monomers.

[0028] Examples of the phosphoric acid group-containing vinyl (co)polymer include a polymer of (meth)acryloyloxyalkyl acid phosphate, and a copolymer of (meth)acryloyloxyalkyl acid phosphate with other polymerizable unsaturated monomers.

[0029] Examples of the amino group-containing vinyl (co)polymer include copolymers of N,N-dimethylaminoethyl (meth)acrylate and N,N-diethylaminoethyl (meth)acrylate with other polymerizable unsaturated monomers.

[0030] Examples of other copolymerizable unsaturated monomers include vinyl carboxylate ester monomers such as vinyl formate, vinyl acetate, vinyl propionate, isopropenyl acetate, vinyl valerate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl versatate, and vinyl pivalate; olefins such as ethylene, propylene, and butylene; aromatic vinyls such as styrene and α-methylstyrene; methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; Examples of the monomers include ethylenically unsaturated carboxylic acid alkyl ester monomers such as dimethyl fumarate, dimethyl maleate, diethyl maleate, and diisopropyl itaconate; vinyl ether monomers such as methyl vinyl ether, n-propyl vinyl ether, isobutyl vinyl ether, and dodecyl vinyl ether; halogenated vinyl monomers or vinylidene monomers such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; and quaternary ammonium group-containing monomers such as 3-(meth)acrylamidopropyltrimethylammonium chloride. These monomers can be used alone or in combination of two or more.

[0031] From the viewpoints of pigment dispersibility, storage stability, and compatibility with the solvent, the polar functional group concentration of the pigment dispersing resin (A) is preferably 0.3 mmol / g to 23 mmol / g, more preferably 0.3 mmol / g to 15.0 mmol / g, further preferably 0.3 mmol / g to 8.5 mmol / g, and particularly preferably 0.3 mmol / g to 5.0 mmol / g. The acid group and amino group may be in the form of a salt.

[0032] The vinyl (co)polymer (A1) can be produced by a polymerization method known per se, for example, solution polymerization is preferably used, but is not limited thereto, and may be bulk polymerization, emulsion polymerization, suspension polymerization, etc. When solution polymerization is carried out, it may be continuous polymerization or batch polymerization, and the monomers may be charged all at once or in portions, or may be added continuously or intermittently.

[0033] The polymerization initiator used in the solution polymerization is not particularly limited, but specific examples thereof include azo compounds such as azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), azobis-2,4-dimethylparabennitrile, and azobis(4-methoxy-2,4-dimethylparabennitrile); acetyl peroxide, benzoyl peroxide, lauroyl peroxide, acetylcyclohexylsulfonyl peroxide, 2,4,4-trimethylpentyl-2,4-dimethylparabennitrile; peroxides such as .-peroxyphenoxyacetate; percarbonate compounds such as diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and diethoxyethyl peroxydicarbonate; perester compounds such as t-butyl peroxyneodecanate, α-cumyl peroxyneodecanate, and t-butyl peroxyneodecanate; and known radical polymerization initiators such as azobisdimethylvaleronitrile and azobismethoxyvaleronitrile can be used.

[0034] The polymerization reaction temperature is not particularly limited, but can usually be set within the range of about 30°C or higher and 200°C or lower.

[0035] The vinyl (co)polymer (A1) obtainable as described above has a degree of polymerization of, for example, 100 or more, preferably 150 or more, and for example, 4,000 or less, preferably 3,000 or less, more preferably 700 or less.

[0036] The weight average molecular weight is, for example, 1,000 or more, preferably 2,000 or more, more preferably 7,000 or more, and for example, 2,000,000 or less, preferably 1,000,000 or less, more preferably 500,000 or less.

[0037] In addition, unless otherwise specified, the weight average molecular weight in this specification is a value obtained by converting the retention time (retention volume) measured using a gel permeation chromatograph (GPC) into the molecular weight of polystyrene using the retention time (retention volume) of a standard polystyrene with a known molecular weight measured under the same conditions. Specifically, the measurement can be performed using a gel permeation chromatograph "HLC8120GPC" (manufactured by Tosoh Corporation, product name) and four columns "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL" and "TSKgel G-2000HXL" (all manufactured by Tosoh Corporation, product names) under the conditions of a mobile phase of tetrahydrofuran, a measurement temperature of 40°C, a flow rate of 1 mL / min, and a detector RI.

[0038] After completion of the synthesis, the vinyl (co)polymer (A1) can be converted into a solid or into a resin solution in which any solvent has been replaced by removing the solvent and / or replacing the solvent.

[0039] The method for removing the solvent may be performed by heating at normal pressure or under reduced pressure. The method for replacing the solvent may be performed by adding a replacement solvent at any stage before, during, or after the removal of the solvent.

[0040] In addition, the content of alkyl groups having 12 or more carbon atoms in the dispersing resin (A), in the case of a vinyl (co)polymer (A1), is preferably 1 to 100 mass%, more preferably 10 to 90 mass%, even more preferably 20 to 80 mass%, and particularly preferably 30 to 60 mass%, expressed as the mass ratio of the monomer when all monomers are taken as 100 mass%. In addition, when a compound having a reactive alkyl group having 12 or more carbon atoms is added to the resin later, the content of the alkyl group having 12 or more carbon atoms is calculated based on the mass proportion of the compound.

[0041] When the pigment dispersion resin (A) is converted from a solid state into a resin solution, it is preferable, from the viewpoint of solubility in the solvent, to first mix and dissolve the resin in a solvent having a liquid temperature of 60° C. or higher (preferably 80° C. or higher) (upper limit is 200° C. or lower, preferably 100° C. or lower) to convert it into a resin solution, and then mix it with other components [components (B), (C), (D), etc.]. The "liquid temperature" refers to the temperature of the solvent or resin solution at the time of dissolution. The solid pigment dispersion resin (A) may be mixed and dissolved in a solvent at 60° C. or higher in advance, or the solid pigment dispersion resin (A) may be mixed with a solvent and then heated to a temperature of 60° C. or higher. Furthermore, the ink may contain components other than the pigment dispersing resin (A) and the solvent. The solvent may be used alone or in combination of two or more kinds, and the types of solvents that can be suitably used are those exemplified below as solvents.

[0042] The solid content of the pigment dispersion resin (A) is, based on 100% by mass of the total solid content of the carbon nanotube dispersion paste, for example, 0.1% by mass or more, preferably 1% by mass or more, and more preferably 3% by mass or more, and for example, 40% by mass or less, preferably 30% by mass or less, and more preferably 20% by mass or less. In addition, the solid content of the pigment dispersion resin (A) is, based on 100% by mass of the total amount of the carbon nanotube dispersion paste, for example, 0.1% by mass or more, preferably 0.4% by mass or more, and more preferably 0.7% by mass or more, and for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 2% by mass or less.

[0043] In addition, the solid content of the pigment dispersion resin (A) is, based on the content of the carbon nanotubes (B) being 100% by mass, for example, 0.1% by mass or more, preferably 1% by mass or more, and more preferably 5% by mass or more, and for example, 150% by mass or less, preferably 120% by mass or less, and more preferably 80% by mass or less.

[0044] Carbon nanotubes (B) As the carbon nanotubes (B), single-walled carbon nanotubes or multi-walled carbon nanotubes can be used alone or in combination. In particular, in terms of viscosity, electrical conductivity, and cost, it is preferable to use multi-walled carbon nanotubes.

[0045] The content of the carbon nanotubes (B) is 0.1% by mass or more, for example, 0.2% by mass or more, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and even more preferably 2% by mass or more, and less than 15% by mass, for example, less than 13% by mass, preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 6% by mass or less, based on the total amount of the carbon nanotube dispersion paste (100% by mass). For example, it can be 0.1% by mass or more and less than 15% by mass, 0.2% by mass or more and less than 13% by mass, 0.3% by mass or more and less than 10% by mass, or 0.5% by mass or more and less than 7% by mass. Furthermore, based on 100% by mass of the total solid content of the carbon nanotube dispersion paste, it is, for example, 5% by mass or more, preferably 10% by mass or more, and more preferably 20% by mass or more, and for example, 90% by mass or less, preferably 70% by mass or less, and more preferably 50% by mass or less.

[0046] The average outer diameter of the carbon nanotubes (B) is, for example, 1 nm or more, preferably 3 nm or more, more preferably 5 nm or more, and for example, 30 nm or less, preferably 28 nm or less, more preferably 25 nm or less.

[0047] The average length of the carbon nanotubes (B) is, for example, 0.1 μm or more, preferably 1 μm or more, more preferably 5 μm or more, and for example, 100 μm or less, preferably 80 μm or less, more preferably 60 μm or less.

[0048] The BET specific surface area of ​​carbon nanotubes (B) is usually set at 100 m due to the relationship between viscosity and electrical conductivity. 2 / g or more, preferably 130m 2 / g or more, more preferably 160m 2 / g or more, usually 800m 2 / g or less, preferably 600m 2 / g or less, more preferably 400m 2 / g or less.

[0049] The BET specific surface area of ​​the present invention can be calculated by the BET method using nitrogen adsorption measurement. Specifically, for example, the BET specific surface area (m 2 / g) can be measured.

[0050] The amount of acidic groups in the carbon nanotubes (B) is usually 0.01 mmol / g or more, preferably 0.01 mmol / g or more, and usually 1.0 mmol / g or less, preferably 0.5 mmol / g or less, more preferably 0.2 mmol / g or less, and further preferably 0.1 mmol / g or less, from the viewpoints of dispersibility and storage property. If the amount of acidic groups is 0.01 mmol / g or more, the dispersibility is good, and if it is 1.0 mmol / g or less, the storage property is good.

[0051] The acidic groups can be imparted to the carbon nanotubes by the acid treatment described below.

[0052] (Acid treatment method) The acid treatment method is not particularly limited as long as the carbon nanotube can be brought into contact with the acid, but a method of immersing the carbon nanotube in an acid treatment liquid (aqueous solution of acid) is preferred. The acid contained in the acid treatment liquid is not particularly limited, but examples thereof include nitric acid, sulfuric acid, and hydrochloric acid. These can be used alone or in combination of two or more. Among these, nitric acid and sulfuric acid are preferred. The amount of acidic groups in the carbon nanotubes can be adjusted by the concentration of the acid treatment solution, the temperature, the treatment time, and the like.

[0053] After the acid treatment, the excess acid component adhering to the surface is removed by a washing method described below, whereby acid-treated carbon nanotubes can be obtained. The method for washing the acid-treated carbon nanotubes is not particularly limited, but washing with water is preferred. For example, the carbon nanotubes are collected from the acid-treated carbon nanotubes by a known method such as filtration, and then washed with water. After the washing, if necessary, the water adhering to the surface can be removed by drying, etc., to obtain the acid-treated carbon nanotubes.

[0054] The volumetric median diameter (D50) of the carbon nanotubes (B) is usually 10 μm or more, preferably 15 μm or more, more preferably 20 μm or more, and usually 250 μm or less, preferably 200 μm or less, more preferably 150 μm or less, when measured by the method described in the examples below. Here, the median diameter (D50) can be obtained by irradiating a carbon nanotube particle with a laser beam and converting the diameter of the carbon nanotube into a sphere from the scattered light. The larger the median diameter (D50), the more carbon nanotube aggregates there are, which means that the dispersibility is poor. If the median diameter (D50) is larger than 250 μm, there is a high possibility that carbon nanotube aggregates exist in the electrode, and the conductivity of the entire electrode becomes non-uniform. On the other hand, if the median diameter (D50) is smaller than 10 μm, the fiber length is short, so the conductive path is insufficient, and the conductivity decreases. When the median diameter (D50) is within the range of 10 μm or more and 250 μm or less, the carbon nanotubes can be uniformly dispersed in the electrode while maintaining their electrical conductivity.

[0055] In the Raman spectrum of the carbon nanotube (B), -1 More than 1600cm -1 The maximum peak intensity within the following range is G, 1310cm -1 More than 1350cm -1 The G / D ratio, when the maximum peak intensity within the following range is D, is usually 0.1 or more, preferably 0.4 or more, more preferably 0.6 or more, and is usually 5.0 or less, preferably 3.0 or less, more preferably 1.0 or less.

[0056] Here, it is preferable for the G / D ratio to be within the range of 0.1 to 5.0, since there are few defects and crystal interfaces on the carbon surface and the electrical conductivity is likely to be high.

[0057] Unlike acetylene black, carbon nanotubes (B) have a fibrous shape and become viscous, so that if the content is 15% by mass or more, the viscosity becomes high and handling becomes difficult.

[0058] (Dry dispersion of carbon nanotubes) The carbon nanotubes (B) can be previously dry-dispersed in a media-type grinder before producing the carbon nanotube dispersion paste. The "dry dispersion" of the present invention refers to pulverization (including disintegration) by a pulverizer at a solid content concentration in the pulverized component of 80 mass% or more (preferably 90 mass% or more, more preferably 95 mass% or more, and even more preferably 98 mass% or more). Although it is possible to pulverize together with components other than the carbon nanotubes (B), it is suitable that the content of the carbon nanotubes (B) contained in the solid content of the pulverized component is usually 80 mass% or more, preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 98 mass% or more, and particularly preferably only the carbon nanotubes (B). As the components other than the carbon nanotubes (B) in the ground component, solvents, resins, pigments other than the carbon nanotubes (B), etc. can be suitably used, but it is preferable that the ground component contains substantially only the carbon nanotubes (B). The above "solid content concentration" refers to the proportion of solid content (mass %) when 1 g of a sample is dried by heating at 130° C. for 3 hours.

[0059] The dry dispersion method is to grind the pigment without substantially containing any liquid components, and since energy can be applied directly to the pigment, it is possible to perform highly efficient and powerful grinding (disintegration). In addition, since the grinding surface is activated and interacts with the surrounding substances, good dispersibility and storage stability can be obtained in the paste dispersion process described below, and the coating film can have excellent conductivity and finish. In the dry dispersion, the material is pulverized using a pulverizer incorporating pulverizing media such as glass beads, zirconia beads, steel balls, etc. The pulverization is carried out by utilizing the pulverizing or destructive force caused by the collision of the pulverizing media with each other and / or the collision of the pulverizer with the pulverizing media. Known pulverizing devices such as high-speed rotation impact mills, jet mills, roll mills, attritors, ball mills, vibration mills, and bead mills can be used as the pulverizing device.

[0060] In addition, various steam or gases can be blown into the mill during pulverization to further activate the surface of the carbon nanotubes (B) or adjust the activity. As the steam, an acidic or basic compound is preferable, and as the gas, oxygen, nitrogen, etc. are preferable.

[0061] The outer diameter of the grinding media is preferably 0.1 mm to 5 mm, and more preferably 0.5 mm to 3 mm. Within the above range, a desired grinding force can be obtained, and the pigment can be efficiently ground and disintegrated without excessively destroying the fiber shape of the carbon nanotubes.

[0062] Other conductive pigments (B1) The carbon nanotube dispersion paste used in the present invention can also contain other conductive pigments (B1) other than the carbon nanotubes (B). Examples of other conductive pigments (B1) include at least one conductive carbon selected from the group consisting of acetylene black, ketjen black, furnace black, thermal black, graphene, and graphite. Preferably, it is at least one selected from the group consisting of acetylene black, ketjen black, furnace black, and thermal black, more preferably at least one selected from the group consisting of acetylene black and ketjen black, and even more preferably acetylene black.

[0063] The average primary particle diameter of the other conductive pigment (B1) is, for example, 10 nm or more, preferably 20 nm or more, and more preferably, for example, 80 nm or less, preferably 70 nm or less. Here, the average primary particle diameter refers to the average particle diameter of the primary particles obtained by observing the conductive pigment (B1) with an electron microscope, calculating the projected area of ​​each of 100 particles, calculating the diameter of a circle equivalent to the area, and simply averaging the diameters of the 100 particles. Note that, if the pigment is in an aggregated state, the calculation is performed using the primary particles that make up the aggregated particles.

[0064] The BET specific surface area of ​​the other conductive pigment (B1) is not particularly limited. 2 / g or more, preferably 10m 2 / g or more, more preferably 20m 2 / g or more, for example, 500m 2 / g or less, preferably 250m 2 / g or less, more preferably 200m 2 / g or less.

[0065] The dibutyl phthalate (DBP) oil absorption of the other conductive pigment (B1) is not particularly limited, and is, for example, 60 ml / 100 g or more, preferably 150 ml / 100 g or more, and for example, 1,000 ml / 100 g or less, preferably 800 ml / 100 g or less, in relation to pigment dispersibility and conductivity.

[0066] N-Methyl-2-pyrrolidone (C) The N-methyl-2-pyrrolidone (C) preferably has a moisture content of 10,000 ppm or less, and is preferably controlled and adjusted before use so that the moisture content is below a certain level. In addition, from the viewpoints of reducing waste, environmental friendliness, and cost reduction, it is preferable to use a regenerated product (recycled product).

[0067] The water content (upper limit) of N-methyl-2-pyrrolidone (C) is preferably 10000 ppm or less, more preferably 7500 ppm or less, even more preferably 5000 ppm or less, particularly preferably 2500 ppm or less, and even more particularly preferably 1000 ppm or less. The water content (lower limit) is preferably 100 ppm or more, more preferably 200 ppm or more, and even more preferably 500 ppm or more.

[0068] N-methyl-2-pyrrolidone may contain amine components as impurities generated during production or as unreacted raw materials, and in the carbon nanotube dispersion paste of the present invention, the viscosity or tendency to thicken may vary from lot to lot due to the amine components as impurities. In addition, there is a problem of odor (work environment), so it is necessary to control it as a raw material to a certain amount or less.

[0069] In addition, when the carbon nanotube dispersion paste of the present invention is applied to an electrode layer by the method described below, the solvent and the like volatilize and do not remain, but it is preferable to recover and reuse the volatilized solvent in order to reduce waste, be environmentally friendly, and / or reduce raw material costs. That is, it is preferable to use a recycled product as N-methyl-2-pyrrolidone (C). This recycled solvent (recycled product) also contains the amine compound originally contained therein, and similarly, the viscosity or thickening tendency of the paste varies from lot to lot. In addition, amine compounds often have a strong odor.

[0070] Therefore, in this case, it is preferable to control and adjust the amine compound content in the recycled product, N-methyl-2-pyrrolidone (C), so that it is a certain amount or less. The amine compound content is preferably 10,000 ppm or less, more preferably 7,500 ppm or less, even more preferably 5,000 ppm or less, particularly preferably 2,500 ppm or less, and even particularly preferably 1,000 ppm or less. Since the above-mentioned recycled product contains a minimum amount of amine compounds, the lower limit is 1 ppm or more, 5 ppm or more, or 10 ppm or more. The content of amine compounds can be quantified by common analyses such as ion chromatography-mass spectrometry (IC-MS). The content can be quantified by creating a calibration curve in advance for the peaks of amine species that are expected to be mixed in.

[0071] The above-mentioned "use of recycled products" means that the N-methyl-2-pyrrolidone (C) used in the present invention contains recycled products at a content of 5% by mass or more (preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more).

[0072] As the above-mentioned recycled product, it is preferable to use a recycled solvent recovered in the process of producing an electrode layer by heating and drying a composite paste, which will be described later.

[0073] From the viewpoint of recyclability, when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, it is preferable that (Xc)-10>(Xd) from the viewpoint of distillation (separation of the amine compound (D)), and it is more preferable that (Xc)-15>(Xd).

[0074] The content of N-methyl-2-pyrrolidone (C) in the carbon nanotube dispersion paste is, based on 100% by mass of the total amount of the carbon nanotube dispersion paste, for example, 40% by mass or more, preferably 60% by mass or more, and more preferably 80% by mass or more, and for example, 99% by mass or less, preferably 98% by mass or less, and more preferably 97% by mass or less. The solid content of the carbon nanotube dispersion paste is typically 0.1% by mass or more, for example 1% by mass or more, preferably 2% by mass or more, and more preferably 3% by mass or more, based on 100% by mass of the total amount of the carbon nanotube dispersion paste, and is typically less than 80% by mass, for example 60% by mass or less, preferably 40% by mass or less, and more preferably 20% by mass or less.

[0075] The carbon nanotube dispersion paste may contain a solvent other than N-methyl-2-pyrrolidone (C). Specific examples of the solvent include hydrocarbon solvents such as n-butane, n-hexane, n-heptane, n-octane, cyclopentane, cyclohexane, and cyclobutane; aromatic solvents such as toluene and xylene; ketone solvents such as methyl isobutyl ketone; ether solvents such as n-butyl ether, dioxane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, and diethylene glycol; ester solvents such as ethyl acetate, n-butyl acetate, isobutyl acetate, ethylene glycol monomethyl ether acetate, and butyl carbitol acetate; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone; alcohol solvents such as ethanol, isopropanol, n-butanol, sec-butanol, and isobutanol; and amide solvents such as equamide (an amide solvent, product name, manufactured by Idemitsu Kosan Co., Ltd.), N,N-dimethylformamide, N,N-dimethylacetamide, N-methylformamide, N-methylacetamide, and N-methylpropionamide. These can be used alone or in combination of two or more.

[0076] Amine Compounds (D) Examples of the amine compound (D) include ammonia, primary amines, secondary amines, and tertiary amines. The amine compound (D) of the present invention also includes the amine compounds present as impurities in the above-mentioned N-methyl-2-pyrrolidone (C) and the amine compounds contained in the recycled product of N-methyl-2-pyrrolidone (C). Examples of common amine compounds include the following amine compounds:

[0077] Examples of primary amines include ethylamine, n-propylamine, sec-propylamine, n-butylamine, sec-butylamine, i-butylamine, tert-butylamine, pentylamine, hexylamine, heptylamine, octylamine, decylamine, laurylamine, myristyrylamine, 1,2-dimethylhexylamine, 3-pentylamine, 2-ethylhexylamine, allylamine, aminoethanol, 1-aminopropanol, 2-aminopropanol, aminobutanol, aminopentanol, aminohexanol, 3-ethoxypropylamine, 3-propoxypropylamine, 3-isopropoxypropylamine, 3-butoxypropylamine, 3-isobutoxypropylamine, 3-(2-ethylhexyloxy)propylamine, aminocyclopentane, aminocyclohexane, aminonorbornene, aminomethylcyclohexane, aminobenzene, benzylamine, phenethylamine, α-phenylethylamine, naphthylamine, Primary monoamines such as furfurylamine; ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,2-diaminobutane, 1,3-diaminobutane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, dimethylaminopropylamine, diethylaminopropylamine, bis-(3-aminopropyl)ether, 1,2-bis-(3-aminopropoxy)ethane, 1,3-bis -(3-aminopropoxy)-2,2'-dimethylpropane, aminoethylethanolamine, 1,2-bisaminocyclohexane, 1,3-bisaminocyclohexane, 1,4-bisaminocyclohexane, 1,3-bisaminomethylcyclohexane, 1,4-bisaminomethylcyclohexane, 1,3-bisaminoethylcyclohexane, 1,4-bisaminoethylcyclohexane, 1,3-bisaminopropylcyclohexane, 1,4-bisaminopropylcyclohexane, hydrogenated 4,4'-Diaminodiphenylmethane, 2-aminopiperidine, 4-aminopiperidine, 2-aminomethylpiperidine, 4-aminomethylpiperidine, 2-aminoethylpiperidine, 4-aminoethylpiperidine, N-aminoethylpiperidine, N-aminopropylpiperidine, N-aminoethylmorpholine, N-aminopropylmorpholine, isophoronediamine, menthanediamine, 1,4-bisaminopropylpiperazine, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 2,4-tolylenediamine, 2,6-tolylenediamine, 2,4-toluenediamine, m-aminobenzylamine, 4-chloro-o-phenylenediamine, tetrachloro-p-xylylenediamine, 4-methoxy-6-methyl-m-phenylenediamine, m-xylylenediamine, p-xylylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, benzidine, 4,4'-bis( o-toluidine), dianisidine, 4,4'-diaminodiphenylmethane, 2,2-(4,4'-diaminodiphenyl)propane, 4,4'-diaminodiphenyl ether, 4,4'-thiodianiline, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminoditolyl sulfone, methylenebis(o-chloroaniline), 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro[5,5]undecane, diethylenetriamine, Examples of primary polyamines include iminobispropylamine, methyliminobispropylamine, bis(hexamethylene)triamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, N-aminoethylpiperazine, N-aminopropylpiperazine, 1,4-bis(aminoethylpiperazine), 1,4-bis(aminopropylpiperazine), 2,6-diaminopyridine, and bis(3,4-diaminophenyl)sulfone.

[0078] Examples of secondary amines include secondary monoamines such as diethylamine, dipropylamine, di-n-butylamine, di-sec-butylamine, diisobutylamine, di-n-pentylamine, di-3-pentylamine, dihexylamine, dioctylamine, di(2-ethylhexyl)amine, methylhexylamine, diallylamine, pyrrolidine, piperidine, 2,4-lupetidine, 2,6-lupetidine, 3,5-lupetidine, diphenylamine, N-methylaniline, N-ethylaniline, dibenzylamine, methylbenzylamine, dinaphthylamine, pyrrole, indoline, indole, and morpholine; N,N'-dimethylethylenediamine, N,N'-dimethyl-1,2-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N,N'-dimethyl-1,2-diaminobutane, N,N'-dimethyl-1,3-diaminobutane, N,N' -Dimethyl-1,4-diaminobutane, N,N'-Dimethyl-1,5-diaminopentane, N,N'-Dimethyl-1,6-diaminohexane, N,N'-Dimethyl-1,7-diaminoheptane, N,N'-Diethylethylenediamine, N,N'-Diethyl-1,2-diaminopropane, N,N'-Diethyl-1,3-diaminopropane, N,N'-Diethyl-1,2-diaminobutane, N,N'-Diethyl-1,3-diaminobutane Examples of secondary polyamines include secondary polyamines such as 1,1-di-(4-piperidyl)methane, 1,2-di-(4-piperidyl)ethane, 1,3-di-(4-piperidyl)propane, and 1,4-di-(4-piperidyl)butane.

[0079] Examples of tertiary amines include trimethylamine, triethylamine, tri-n-propylamine, tri-iso-propylamine, tri-1,2-dimethylpropylamine, tri-3-methoxypropylamine, tri-n-butylamine, tri-iso-butylamine, tri-sec-butylamine, tri-pentylamine, tri-3-pentylamine, tri-n-hexylamine, tri-n-octylamine, tri-2-ethylhexylamine, tri-dodecylamine, tri-laurylamine, dicyclohexylethylamine, cyclohexyldiethylamine, tri-cyclohexylamine, N,N-dimethylhexylamine, N-methyldihexylamine, N,N-dimethylcyclohexylamine, N-methyldicyclohexylamine, N,N-diethylethanolamine, N,N-dimethylethanolamine, N-ethyldiethanolamine, triethanolamine, tribenzylamine, N,N-dimethylbenzylamine, diethylbenzylamine, Tertiary monoamines such as diphenylamine, triphenylamine, N,N-dimethylamino-p-cresol, N,N-dimethylaminomethylphenol, 2-(N,N-dimethylaminomethyl)phenol, N,N-dimethylaniline, N,N-diethylaniline, pyridine, quinoline, N-methylmorpholine, N-methylpiperidine, 2-(2-dimethylaminoethoxy)-4-methyl-1,3,2-dioxabornane, and 2-, 3-, and 4-picoline; tetramethylethylenediamine , tertiary polyamines such as pyrazine, N,N'-dimethylpiperazine, N,N'-bis((2-hydroxy)propyl)piperazine, hexamethylenetetramine, N,N,N',N'-tetramethyl-1,3-butanamine, 2-dimethylamino-2-hydroxypropane, diethylaminoethanol, N,N,N-tris(3-dimethylaminopropyl)amine, 2,4,6-tris(N,N-dimethylaminomethyl)phenol, and heptamethylisobiguanide.

[0080] These may be used alone or in combination of two or more. Here, the amine compound (D) that can be used at least in the present invention is an amine compound within the range of (Xc)-10>(Xd), where the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of amine compound (D) is (Xd)°C. However, an amine compound outside this range can also be used together with amine compound (D).

[0081] Of these, primary amine compounds are preferred, and monovalent amine compounds (monoamines) are more preferred.

[0082] The amine compound (D) includes alkanolamines, aliphatic amines, alicyclic amines, aromatic amines, etc., and any of them can be suitably used, with aromatic amines being preferred.

[0083] Since it is preferable that no amine compound (D) remains in the electrode layer after drying, the weight average molecular weight of the amine compound (D) is preferably less than 1,000, more preferably 800 or less, even more preferably 500 or less, particularly preferably 350 or less, and even more particularly preferably 250 or less. Furthermore, if the boiling point is low, there is a possibility that the liquid will volatilize during production or storage, and furthermore, from the viewpoint of odor, the lower limit of the boiling point is preferably 50° C. or higher, and more preferably 100° C. or higher.

[0084] The amine value of the amine compound (D) is usually 5 mgKOH / g or more, preferably 50 mgKOH / g or more, more preferably 105 mgKOH / g or more, and is usually within the range of 1,000 mgKOH / g or less.

[0085] By including amine compound (D), pigment dispersibility and storage stability are improved, but many of them have a strong odor, which may worsen the working environment during mixing or drying. In addition, they are generally expensive, which may increase costs. Furthermore, for the sake of recycling suitability, which will be described later, the content must be kept to the minimum necessary.

[0086] The content of the amine compound (D) is, based on 100% by mass of the total amount of the carbon nanotube dispersion paste, for example, 0.01% by mass or more, preferably 0.05% by mass or more, and more preferably 0.1% by mass or more, and is, for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 1% by mass or less.

[0087] Based on 100% by mass of the solid content of the carbon nanotubes (B), the lower limit is, for example, 1% by mass or more, preferably 2% by mass or more, and more preferably 5% by mass or more, and the upper limit is, for example, 500% by mass or less, preferably 50% by mass or less, and more preferably 15% by mass or less. Furthermore, based on 100% by mass of the solid content of the carbon nanotube dispersion paste, it is, for example, 1% by mass or more, preferably 1.5% by mass or more, more preferably 2% by mass or more, and for example, 600% by mass or less, preferably 300% by mass or less, more preferably 50% by mass or less.

[0088] Polyvinylidene fluoride (E) The carbon nanotube dispersion paste that can be used in the present invention preferably contains polyvinylidene fluoride (E), which is an essential component of the composite paste described below.

[0089] Polyvinylidene fluoride (E) is a resin intended for forming a film of an electrode layer, and may be modified in various ways. From the viewpoint of adhesion to a substrate, it preferably has a polar functional group.

[0090] The weight average molecular weight of polyvinylidene fluoride (E) is, from the viewpoints of adhesion to the substrate, reinforcement of the film properties, and solvent resistance, for example, 100,000 or more, preferably 500,000 or more, and more preferably 650,000 or more, and is, for example, 3 million or less, preferably 2 million or less.

[0091] The content of polyvinylidene fluoride (E) is, for example, 10.0 mass% or more, preferably 30.0 mass% or more, more preferably 40.0 mass% or more, and for example, 99.0 mass% or less, preferably 80.0 mass% or less, more preferably 60.0 mass% or less, based on 100 mass% of the solid content of the carbon nanotube dispersion paste. Also, for example, 0.1 mass% or more, preferably 0.5 mass% or more, more preferably 1 mass% or more, and for example, 10 mass% or less, preferably 7 mass% or less, more preferably 5 mass% or less, based on 100 mass% of the total amount of the carbon nanotube dispersion paste.

[0092] When the polyvinylidene fluoride (E) is converted from a solid state into a resin solution, it is preferable to convert it into a resin solution by mixing and dissolving it in a solvent having a liquid temperature of 40° C. or higher (preferably 60° C. or higher, and more preferably 80° C. or higher) (upper limit is 200° C. or lower, and preferably 100° C. or lower) in advance from the viewpoint of solubility in the solvent, and it is preferable to mix it with other components [components (A), (B), (C), etc.] after conversion into a resin solution. The "liquid temperature" refers to the temperature of the solvent or resin solution at the time of dissolution. The solid polyvinylidene fluoride (E) may be mixed in advance with a solvent at 40° C. or higher and dissolved therein, or the solid polyvinylidene fluoride (E) may be mixed with a solvent and then heated to a temperature of 40° C. or higher. In addition, the composition may contain components other than the polyvinylidene fluoride (E) and the solvent. The solvent may be used alone or in combination of two or more kinds. Any solvent that dissolves polyvinylidene fluoride (E) may be suitably used, with N-methyl-2-pyrrolidone (C) being preferred. In addition, it is preferable to cool the resin solution that has been hot-dissolved as described above to a predetermined temperature of 10° C. or more and less than 40° C., and the cooling step is carried out by reacting the resin solution with the resin solution at a temperature of 10° C. or more and less than 40° C. ... Cooling rate = (solution temperature at the start of cooling - solution temperature at the end of cooling) / cooling time From the viewpoint of preventing precipitation, it is preferable that the cooling rate defined by is 0.5° C. / min or more (preferably 1° C. / min or more).

[0093] Mixing and Dispersion In the manufacturing method of the present invention, the mixing and dispersing step is a step of mixing and further dispersing components containing at least a pigment dispersion resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), thereby obtaining a liquid carbon nanotube dispersion paste.

[0094] The upper limit of the solid content of the carbon nanotube dispersion paste is usually less than 80% by mass, preferably less than 50% by mass, more preferably less than 20% by mass, and even more preferably less than 10% by mass. The lower limit is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more.

[0095] In the above mixing and dispersing step, each component can be uniformly mixed and dispersed using a conventionally known dispersing machine such as a paint shaker, a sand mill, a ball mill, a pebble mill, an LMZ mill, a DCP pearl mill, a planetary ball mill, a homogenizer, a twin-screw kneader, a thin film rotary high-speed mixer (manufactured by Filmix, product name "Clearmix", etc.), etc. The order in which each component is mixed is not particularly limited. The mixing and dispersing step further comprises: Step 1: Adding a component containing carbon nanotubes (B) in an amount of 70% by mass or less (preferably 50% by mass or less) based on 100% by mass of the total amount of carbon nanotubes (B) contained in the carbon nanotube dispersion paste obtained after dispersion to a dispersing machine, and performing a dispersion treatment; Step 2: adding carbon nanotubes (B) to a disperser until the desired concentration is reached, and performing a dispersion treatment; It is preferable that the method includes the steps of sequentially carrying out the steps. The dispersion treatment time in step 1 is preferably at least 30 seconds or more (preferably 1 minute or more). By carrying out the above-mentioned mixing and dispersion, the aggregation of the carbon nanotubes (B) is alleviated, and a homogeneous paste with good dispersibility is obtained even in a high-concentration paste, and the resulting battery electrode layer (coating film) has excellent finish, conductivity, battery performance, etc.

[0096] Other Ingredients The carbon nanotube dispersion paste may further contain other components in addition to the above-mentioned components (A), (B), (C), and (D) and the component (E) which may be contained as necessary.

[0097] Examples of other components include resins other than the pigment dispersion resin (A) and polyvinylidene fluoride (E), neutralizing agents, defoamers, preservatives, rust inhibitors, plasticizers, pigments other than the carbon nanotubes (B), and dehydrating agents (F).

[0098] Examples of pigments other than carbon nanotubes (B) include the other conductive pigments (B1) described above; white pigments such as titanium white and zinc oxide; blue pigments such as cyanine blue and indanthrene blue; green pigments such as cyanine green and verdigris; organic red pigments such as azo and quinacridone, red pigments such as red iron oxide; organic yellow pigments such as benzimidazolone, isoindolinone, isoindoline and quinophthalone, yellow pigments such as titanium yellow and yellow lead, etc. These pigments can be used alone or in combination of two or more. Pigments other than these carbon nanotubes (B) can be used for purposes such as color adjustment and reinforcement of the physical properties of the film, as long as they do not significantly impair the electrical conductivity. They may be dispersed simultaneously with the pigment dispersion resin (A) and the carbon nanotubes (B), or they may be mixed as a pigment or pigment paste after dispersing the pigment dispersion resin (A) and the carbon nanotubes (B) to prepare a paste.

[0099] The content of pigments other than the carbon nanotubes (B) is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably 1 mass% or less, based on 100 mass% of all pigments in the carbon nanotube dispersion paste, and it is particularly preferable that they are substantially not contained.

[0100] The viscosity of the carbon nanotube dispersion paste is determined from the viewpoints of pigment dispersibility and storage stability by setting the shear rate at 2s -1 The viscosity at 200° C. is, for example, less than 5,000 mPa·s, preferably less than 2,500 mPa·s, more preferably less than 1,000 mPa·s, and is, for example, 10 mPa·s or more, preferably 50 mPa·s or more, more preferably 100 mPa·s or more. The viscosity can be measured, for example, using a cone and plate viscometer (manufactured by HAAKE, product name "Mars2", diameter 35 mm, 2° inclined cone and plate).

[0101] The dehydrating agent (F) may be any known agent having a dehydrating effect, without any particular limitation. It may be a solid dehydrating agent that is not dissolved in the solvent of the paste, or may be a dehydrating agent that is dissolved in the solvent. Specific examples of the dehydrating agent include solid dehydrating agents such as zeolite, silica gel, calcium oxide, molecular sieves, activated alumina, barium oxide, calcium hydride, and sodium sulfate; phosphoric acid esters such as trimethyl phosphate, tri-2-propyl phosphate, tributyl phosphate, and tetraisopropyl ethylene phosphonate; phosphine oxides such as tributyl phosphine oxide, trioctyl phosphine oxide, and triphenyl phosphine oxide; orthoformic acid methyl ester, orthoformic acid ethyl ester, and the like. orthoesters such as oxalic anhydride, methyl orthoacetate, ethyl orthoacetate, and ethyl orthobenzoate; and acid anhydrides such as oxalic anhydride, acetic anhydride, propionic anhydride, butyric anhydride, benzoic anhydride, trifluoroacetic anhydride, disulfuric acid, dinitrogen pentoxide, diphosphoric acid, diphosphorus pentoxide, diphosphorus trioxide, diarsenic pentoxide, diarsenic trioxide, methanesulfonic anhydride, trifluoromethanesulfonic anhydride, and sulfobenzoic anhydride, and these may be used alone or in combination of two or more.

[0102] [Method of manufacturing composite paste (for lithium-ion secondary batteries)] In the manufacturing method of the present invention, first, a carbon nanotube dispersion paste having carbon nanotubes (B) is prepared by the above-mentioned method. The carbon nanotube dispersion paste and at least one electrode active material (G) are mixed to produce a composite paste (for lithium ion secondary batteries).

[0103] The solid content of the electrode active material (G) is usually 10% by mass or more, preferably 20% by mass or more, based on 100% by mass of the total amount of the composite paste, and is usually 99% by mass or less, preferably 95% by mass or less, which is suitable in terms of battery performance. In addition, polyvinylidene fluoride (E), which was an optional component in the carbon nanotube dispersion paste, is an essential component in the composite paste and is always contained. The solid content of polyvinylidene fluoride (E) is usually 0.05 mass% or more, preferably 0.1 mass% or more, based on 100 mass% of the total amount of the composite paste, and is usually 10 mass% or less, preferably 2 mass% or less, which is suitable in terms of battery performance, paste viscosity, etc.

[0104] In the above-mentioned step of mixing the electrode active material (G), the composite paste can be mixed uniformly using a conventionally known mixer and disperser.

[0105] The solid content of the pigment dispersion resin (A) in the solid content of the composite paste is usually 0.01% by mass or more, preferably 0.05% by mass or more, based on 100% by mass of the total amount of the composite paste, and is usually 10% by mass or less, preferably 1% by mass or less, which is suitable in terms of battery performance, paste viscosity, etc.

[0106] In the composite paste of the present invention, from the viewpoint of storage stability (suppression of thickening) in the composite paste, it is preferable to include a sequence of first mixing the carbon nanotubes (B) with the amine compound (D) by bringing the amine compound (D) into contact with (wetting) the carbon nanotubes (B) and then mixing the electrode active material (G), in order to reduce aggregation between the carbon nanotubes (B) and the electrode active material (G).

[0107] The solid content of carbon nanotubes (B) in the composite paste solid content of the present invention is usually 0.01% by mass or more, preferably 0.05% by mass or more, more preferably 0.1% by mass or more, based on 100% by mass of the total amount of the composite paste, and is usually 30% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, which is preferable from the viewpoint of battery performance. In addition, the content of N-methyl-2-pyrrolidone (C) in the composite paste of the present invention is usually 1% by mass or more, preferably 4% by mass or more, more preferably 7% by mass or more, based on 100% by mass of the total amount of the composite paste, and is usually 90% by mass or less, preferably 70% by mass or less, more preferably 50% by mass or less, which is preferable from the viewpoint of electrode drying efficiency and paste viscosity.

[0108] The composite paste is suitable for use in the positive or negative electrode applications of lithium ion secondary batteries, and is preferably used for the positive electrode application.

[0109] In addition, the moisture content of the composite paste is usually 10,000 ppm or less, preferably 7,500 ppm or less, more preferably 5,000 ppm or less, even more preferably 2,500 ppm or less, and particularly preferably 1,000 ppm or less, from the viewpoint of suppressing the viscosity increase or gelation of the composite paste described above. The composite paste used in the present invention can be said to be a substantially non-aqueous composite paste. Furthermore, for the reasons mentioned above (moisture carried over from raw materials and moisture mixed in during the manufacturing process), the moisture content of the composite paste is preferably 100 ppm or more, more preferably 200 ppm or more, and even more preferably 500 ppm or more.

[0110] Electrode active material (G) Examples of the electrode active material (G) include lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), lithium cobalt oxide (LiCoO2), LiNi 1 / 3 Co 1 / 3 Mn 1 / 3Examples of the electrode active material (G) include lithium composite oxides such as O2, lithium iron phosphate (LiFePO4), sodium composite oxides, and potassium composite oxides. These electrode active materials (G) can be used alone or in combination of two or more. The electrode active material containing lithium iron phosphate is inexpensive and has relatively good cycle characteristics and energy density, and can therefore be used preferably.

[0111] The particle size of the electrode active material is usually 0.5 μm or more, preferably 10.5 μm or more, and usually 30 μm or less, preferably 20 μm or less.

[0112] The solid content of the electrode active material (G) in 100% by mass of the solid content of the composite paste for lithium ion secondary battery electrodes of the present invention is usually 50% by mass or more, preferably 60% by mass or more, and is preferably less than 100% by mass in terms of battery capacity, battery resistance, etc.

[0113] When the electrode active material (G) is contained in the composite paste, the paste may thicken due to storage. The reason for this is that the electrode active material (G) has alkali metal hydroxides (e.g., LiOH, KOH, NaOH, etc.) derived from the raw materials on the particle surface, and is thought to aggregate (thicken) due to the conductive pigment having an acidic surface. Therefore, by containing a certain amount or more of the amine compound (D), the thickening of the composite paste due to storage can be suppressed.

[0114] In addition, the water content of the electrode active material (G) is usually 10,000 ppm or less, preferably 7,500 ppm or less, more preferably 5,000 ppm or less, even more preferably 2,500 ppm or less, and particularly preferably 1,000 ppm or less, from the viewpoint of suppressing an increase in viscosity or gelation of the composite paste described above.

[0115] As the electrode active material (G) of the present invention, an electrode active material composite (G-1) having at least a part of its surface covered with carbon nanotubes can be suitably used. The above composite (G-1) can be obtained by previously mixing the electrode active material (G), the carbon nanotubes, and, if necessary, other components (e.g., a solvent or a dispersion resin). If necessary, a drying step can be carried out after mixing, so that the carbon nanotubes can be more uniformly adsorbed and / or fixed to the electrode active material (G). Furthermore, the electrode active material composite (G-1) produced as described above can form a uniform conductive network around the electrode active material by adsorbing and / or fixing the carbon nanotubes to the surface of the electrode active material. As the carbon nanotubes that can be used in the electrode active material composite (G-1), any known carbon nanotubes can be used without any particular limitation, but the carbon nanotubes listed as the carbon nanotubes (B) can be preferably used.

[0116] Method for manufacturing electrode layers for lithium-ion secondary batteries As described above, an electrode layer for a lithium ion secondary battery (also referred to as an electrode composite layer or composite layer) can be produced by applying a composite paste for a lithium ion secondary battery to the surface of a core material (current collector) of a positive electrode or a negative electrode and drying the applied paste, and is particularly preferably used for a positive electrode.

[0117] In addition, the carbon nanotube dispersion paste obtained by the manufacturing method of the present invention can be used not only as a paste for a composite layer (electrode layer), but also as a primer layer (also called a functional layer or adhesive layer) between the electrode core material and the composite layer (electrode layer). The method of applying the composite paste for lithium ion secondary batteries can be carried out by a method known per se using a die coater or the like. The amount of application of the composite paste for lithium ion secondary batteries is not particularly limited, but can be set so that the thickness of the composite layer after drying is, for example, 0.04 mm or more, preferably 0.06 mm or more, and, for example, 0.30 mm or less, preferably 0.24 mm or less. The temperature of the drying step can be appropriately set, for example, 80° C. or more, preferably 100° C. or more, and, for example, 250° C. or less, preferably 200° C. or less. The time of the drying step can be appropriately set, for example, 5 seconds or more, and, for example, 120 minutes or less, preferably 60 minutes or less.

[0118] In the drying step, all or a part of N-methyl-2-pyrrolidone (C) and amine compound (D) volatilize. As described above, in order to reduce waste, to be environmentally friendly, and / or to reduce costs, it is preferable to recover and reuse the volatilized components (C) and (D).

[0119] In addition, in lithium ion secondary batteries, there is a problem that the cycle life is reduced when impurities such as moisture are present in the electrode layer. That is, if the carbon nanotube dispersion paste or the composite paste contains more than a specified amount of moisture, or if the electrode layer is not dried sufficiently in the manufacturing process, moisture remains in the electrode layer, which causes deterioration of the cycle characteristics of the battery. The moisture content in the electrode layer is usually less than 1000 ppm, preferably less than 750 ppm, more preferably less than 500 ppm, even more preferably less than 250 ppm, and particularly preferably less than 100 ppm.

[0120] As described above, when the composite paste is applied onto a current collector and dried by heating, it is preferable to produce a mixed solution by recovering vapor containing N-methyl-2-pyrrolidone (C), the amine compound (D), etc., and then to remove and separate impurities other than N-methyl-2-pyrrolidone (C) as much as possible by distillation, thereby producing a recycled product of N-methyl-2-pyrrolidone (C). The water content and the amount of amine compounds in the N-methyl-2-pyrrolidone (C) recycled product are as described above, and are preferably controlled and adjusted to a certain amount or less. It is also desirable that the content of components other than water and amine compounds is as small as possible, and in that sense, the purity is at least 99.0% or more, preferably 99.9% or more, and more preferably 99.95% or more.

[0121] The method for removing and separating impurities to produce the above-mentioned regenerated product can be carried out by a method known per se, such as the method disclosed in JP-A-10-310795 (specifically, filtration, distillation, contact with an acidic substance, etc.). These methods can be carried out alone or in combination of two or more, and can be repeated multiple times. EXAMPLES

[0122] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these specific embodiments. In each example, "parts" indicates parts by mass and "%" indicates % by mass.

[0123] [Manufacturing of dispersion resin] Manufacturing Example 1 A reaction vessel equipped with a thermometer, thermostat, stirrer, reflux condenser and water separator was charged with 75 parts of N-methyl-2-pyrrolidone (note 1) and heated to 120°C in a nitrogen stream. When the temperature reached 120°C, a mixture of the monomer species (total 100 parts) shown in Table 1 below and 2 parts of 2,2'-azobis(2-methylbutyronitrile) was added dropwise over 3 hours. After the addition was completed, the mixture was aged at 120°C for 30 minutes, and a mixture of 1 part of 2,2'-azobis(2-methylbutyronitrile) and 20 parts of N-methyl-2-pyrrolidone (note 1) was added dropwise over 1 hour. After further aging at 120°C for 1 hour, the mixture was cooled and N-methyl-2-pyrrolidone (note 1) was added to obtain an acrylic resin (A1) with a solid content of 50%. The polar functional group concentration was 1.3 (mmol / g). (Note 1) N-methyl-2-pyrrolidone: A solvent for the recycled product, made by mixing new material with the recycled product produced in Application Example 1C in a 1:1 ratio. The water content is 500 ppm (Note 2) and the amine content is 500 ppm (Note 2). (Note 2) The moisture content and amine content were measured using a Karl Fischer moisture meter (Kyoto Electronics Manufacturing, product name "MKC-610") and ion chromatography (Shimadzu Corporation, product name "Prominence HIC-NS").

[0124] Manufacturing Example 2 An acrylic resin (A2) having a solid content of 50% was obtained in the same manner as in Production Example 1, except that the monomer types shown in Table 1 below were used. The weight average molecular weight values ​​of the obtained resins are shown in the following Table 1. In the table, "resin A1" means acrylic resin (A1), and "resin A2" means acrylic resin (A2).

[0125] [Table 1]

[0126] The abbreviations for the monomer types in Table 1 above are as follows. · iBA: i-Butyl acrylate (has a hydrocarbon group with 4 carbon atoms) BEMA: Behenyl methacrylate (has a hydrocarbon group with 22 carbon atoms) St: styrene ·DMAEMA: N,N-Dimethylaminoethyl methacrylate.

[0127] [Production of carbon nanotube dispersion paste and composite paste] Example 1A Using a continuous dry bead mill "Drystar SDA1" (manufactured by Ashizawa Finetech Co., Ltd.), carbon nanotubes (CNT1 (Table 2)) were pulverized at a feed rate of 0.5 kg / hr using zirconia beads (diameter 3.0 mm), a filling rate of 70%, and a mill peripheral speed of 5.0 m / s. Next, 5000 parts of N-methyl-2-pyrrolidone (note 1), 200 parts of the above-mentioned crushed carbon nanotubes, 80 parts of polyvinylpyrrolidone (40 parts solids) (note 3) as a dispersion resin, 1800 parts of KF polymer W#7300 (manufactured by Kureha Corporation, product name, polyvinylidene fluoride, weight average molecular weight 1 million) resin solution (180 parts solids) (note 4), and 25 parts of benzylamine as an amine were mixed while stirring, and finally N-methyl-2-pyrrolidone (note 1) was used to adjust the total mass to 10000 parts. Then, the mixture was dispersed in a ball mill for 4 hours to produce a carbon nanotube dispersion paste (A-1). The water content of the carbon nanotube dispersion paste (A-1) was 800 ppm (note 2). (Note 3) Polyvinylpyrrolidone: Heterocyclic resin, weight average molecular weight (Mw) 12,000, functional group concentration 9 (mmol / g) (Note 4) The polyvinylidene fluoride resin solution was prepared by mixing and dissolving polyvinylidene fluoride and N-methyl-2-pyrrolidone (Note 1) at a temperature of 80°C. The solution was then cooled to 30°C at a rate of about 1°C / min.

[0128] [Table 2]

[0129] The carbon nanotubes are multi-walled carbon nanotubes. The median diameter (D50), G / D ratio, specific surface area (BET specific surface area), and amount of acidic groups in Table 2 above were measured by the methods described below.

[0130] Examples 2A to 5A, Comparative Examples 1A to 4A Carbon nanotube dispersion pastes (A-2) to (A-9) were obtained in the same manner as in Example 1A, except that the dispersion resin, carbon nanotubes (CNTs), amine, and N-methyl-2-pyrrolidone were those shown in Table 3 below and the compositions shown in Table 3 were used. In Example 3A (carbon nanotube dispersion paste (A-3)), carbon nanotubes (CNT1) that were not crushed (dry dispersed) were used. Comparative Example 3A (carbon nanotube dispersion paste (A-8)) uses only new N-methyl-2-pyrrolidone (water content 100 ppm or less, amine content 100 ppm or less) that is not recycled. In addition, the water content of the carbon nanotube dispersion paste (Note 2) and the results of the evaluation test described below are shown in Table 3 below.

[0131] [Table 3]

[0132] The blending amount of the dispersing resin in Table 3 above is the value on solid content. The composition of the dispersing resin (polymethyl methacrylate) in Table 3 above is as follows. Polymethyl methacrylate: Weight average molecular weight 20,000, homopolymer of methyl methacrylate, polar functional group concentration 0 (mmol / g) The boiling points and molecular weights of the solvents and amine compounds in Table 3 above are as follows. N-Methyl-2-pyrrolidone: 202℃, molecular weight 99 Benzylamine: boiling point 185℃, molecular weight 107 Aminomethylpropanol: boiling point 166℃, molecular weight 89 Phenylethylamine: 195℃, molecular weight 121 ·Diethanolamine: 217°C, molecular weight 105.

[0133] Examples 6A to 9A Water was added to the carbon nanotube dispersion paste (A-2) (moisture content 800 ppm) obtained in Example 2A so as to obtain the moisture content shown below (Note 2), and the mixture was thoroughly stirred to obtain the following carbon nanotube dispersion pastes (A-10) to (A-13). The results of the evaluation of the dispersibility of the carbon nanotube dispersion paste are shown in Table 5, which will be described later. Example 6A: Carbon nanotube dispersion paste (A-10), water content 2000 ppm Example 7A: Carbon nanotube dispersion paste (A-11), water content 4000 ppm Example 8A: Carbon nanotube dispersion paste (A-12), water content 8000 ppm Example 9A: Carbon nanotube dispersion paste (A-13), water content 12000ppm.

[0134] Example 1B For 100 parts of the carbon nanotube dispersion paste (A-1), electrode active material particles (composition formula LiNi 0.5 Mn 1.5 Lithium nickel manganese oxide particles with a spinel structure represented by O4, average particle size 6 μm, BET specific surface area 0.7 m 2 900 parts of cellulose acetate (100 ppm / g) and water content 100 ppm were mixed in a disperser to prepare a composite paste (B-1). The moisture content of the composite paste (B-1) was 800 ppm (Note 2).

[0135] Examples 2B to 5B, Comparative Examples 1B to 4B Composite pastes (B-2) to (B-9) were obtained in the same manner as in Example 1B, except that the compositions were as shown in Table 4 below. The results of the evaluation test of the composite paste, which will be described later, are shown in Table 3 above.

[0136] [Table 4]

[0137] Examples 6B to 9B Composite pastes (B-10) to (B-13) were obtained in the same manner as in Example 1B, except that the compositions were as shown in Table 5 below. The results of evaluation of the storage stability of the composite paste are shown in Table 5 below.

[0138] [Table 5]

[0139] <Median diameter (D50)> The median diameter (D50) was measured using a laser diffraction / scattering type particle size distribution analyzer "LA-960" (trade name, manufactured by HORIBA Corporation) according to the following procedure.

[0140] (Preparation of aqueous dispersion medium) 0.10 g of F10MC (trade name, carboxymethylcellulose sodium (hereinafter also referred to as CMCNa) manufactured by Nippon Paper Industries Co., Ltd.) was added to 100 mL of distilled water and dissolved by stirring at room temperature for 24 hours or more to prepare an aqueous dispersion medium containing 0.1% by mass of CMCNa.

[0141] (Preparation of CMCNa aqueous solution) 2.0 g of F10MC (trade name, sodium carboxymethylcellulose, manufactured by Nippon Paper Industries Co., Ltd.) was added to 100 mL of distilled water and dissolved by stirring at room temperature for 24 hours or more to prepare an aqueous solution of 2.0 mass % CMCNa.

[0142] (Pre-measurement processing) 6.0 mg of carbon nanotubes were weighed into a vial, and 6.0 g of the aqueous dispersion medium was added. An ultrasonic homogenizer (Microtech Nithion, "SmurtNR-50") was used for pre-measurement treatment. The tip was checked for deterioration and adjusted so that it was immersed at least 10 mm below the surface of the sample. The time set (irradiation time) was 40 seconds, the power set was 50%, the start power was 50% (output 50%), and the output power was set to a constant, and the carbon nanotube aqueous dispersion was homogenized by ultrasonic irradiation using auto power operation.

[0143] [measurement] <Proportion of dispersed carbon nanotube particles of 1 μm or less and median diameter (D50)> Using the carbon nanotube aqueous dispersion, the proportion of dispersed carbon nanotube particles having a size of 1 μm or less and the median diameter (D50) were measured according to the following methods. The optical model of the LS 13 320 universal liquid module is set to the refractive index of carbon nanotubes at 1.520 and water at 1.333, and after the module is cleaned, it is filled with approximately 1.0 mL of CMCNa aqueous solution. After performing offset measurement, optical axis adjustment, and background measurement under the condition of 50% pump speed, the prepared carbon nanotube water dispersion was added to the particle size distribution meter so that the relative concentration, which indicates the percentage of light scattered outside the beam by the particles, was 8-12%, or the PIDS was 40-55%, and ultrasonic irradiation was performed for 2 minutes at 78 W using the particle size distribution meter attachment (measurement pretreatment), and after circulating for 30 seconds to remove air bubbles, the particle size distribution was measured. A graph of particle size (particle diameter) vs. volume % was obtained, and the presence ratio of dispersed particles of 1 μm or less and the median diameter (D50) were calculated. For each carbon nanotube sample, three measurement samples were taken from different locations and particle size distribution was measured. The proportion of dispersed particles of 1 μm or less and the median diameter (D50) were calculated as the average value.

[0144] <G / D ratio of carbon nanotubes> The Raman spectrum of the carbon nanotube was measured by placing the carbon nanotube in a Raman microscope (manufactured by Horiba, Ltd., product name "XploRA") and using a laser wavelength of 532 nm. -1 More than ~1600cm -1 The maximum peak intensity within the following range is G, 1310cm -1 More than ~1350cm -1 The G / D ratio when the maximum peak intensity within the following range is taken as D is the G / D ratio of the carbon nanotube.

[0145] <Specific surface area (BET specific surface area)> The BET specific surface area of ​​carbon nanotubes was measured in accordance with JIS Z8830:2013 using a specific surface area measuring device (BERSORP-MAX (Microtrack BEL Co., Ltd.)). 2 / g) was measured.

[0146] <Amount of acidic groups in carbon nanotubes (CNTs)> 2 g of CNT was weighed out, immersed in 50 ml of 0.01 M benzylamine / n-methylpyrrolidone solution, and dispersed for 1 hour using an ultrasonic irradiator. The mixture was then centrifuged and the supernatant was filtered. The benzylamine remaining in the filtrate was quantitatively analyzed by potentiometric titration with 0.1 M hydrochloric acid, and the amount of acidic groups (mmol / g) per 1 g of the obtained CNT was identified.

[0147] Evaluation Test The carbon nanotube dispersion pastes and composite pastes obtained in the above Examples and Comparative Examples were subjected to evaluation tests. If even one evaluation result was unacceptable, the evaluation was deemed to be unacceptable.

[0148] <Dispersibility> The obtained carbon nanotube dispersion paste was evaluated for dispersibility using a grain gauge according to the dispersibility test of JIS K-5600-2-5, based on the following criteria: E is failure. A: The pigment is dispersed at less than 10 μm. The dispersibility is very good. B: The pigment is dispersed at a size of 10 μm or more and less than 20 μm. The dispersibility is somewhat good. C: The pigment is dispersed at 20 μm or more, but no aggregates can be visually confirmed. Dispersibility is normal. D: A small amount of aggregates was visually observed. Dispersibility was slightly poor. E: Many large aggregates are visually observed. Dispersibility is very poor.

[0149] <Storage stability> The obtained composite paste was stored at a temperature of 50°C for two weeks, and the initial viscosity and viscosity after storage were compared. The viscosity was measured using a cone and plate viscometer (manufactured by HAAKE, product name "Mars2", diameter 35 mm, cone and plate with a 2° inclination) at a shear rate of 2.0 s -1 The viscosity increase rate was calculated using the following formula, and the storage stability was evaluated according to the following criteria. D is unsatisfactory. Viscosity increase rate (%) = viscosity after storage (mPa·s) / initial viscosity (mPa·s) × 100-100 A: The viscosity increase rate (%) after storage is less than 20%. B: The viscosity increase rate (%) after storage is 20% or more and less than 100%. C: The viscosity increase rate (%) after storage is 100% or more and less than 300%. D: The viscosity increase rate (%) after storage is 300% or more (or gelation makes it impossible to measure).

[0150] <Recyclability> A solution was prepared by removing the resin components (dispersion resin and polyvinylidene fluoride) and pigment components (CNT and active material) from the composite paste compositions of the Examples and Comparative Examples. Next, 100 g of the above solution was placed in an open container equipped with a thermometer, thermostat, and stirrer, and heated to 200±2°C while stirring the inside of the container, and distilled off until the solution was 95 g, producing a recycled N-methyl-2-pyrrolidone product. The amine content (Note 2) was measured, and the recyclability of the solvent was evaluated according to the following criteria. B and C are failures. A: The amine content in the solution is 1000 ppm or less. B: The amine content in the solution is greater than 1000 ppm and less than 2500 ppm. C: The amine content in the solution is greater than 2500 ppm.

[0151] [Manufacturing of electrode layers for batteries] Application examples 1C~5C The composite pastes obtained in Examples 1B to 5B were applied to both sides of a long aluminum foil (positive electrode current collector) having an average thickness of 15 μm, with a basis weight of 10 mg / cm per side. 2 (based on solid content) and dried (drying temperature 200°C, 30 minutes) to form a positive electrode layer. The positive electrode active material layer (positive electrode layer) supported on the positive electrode current collector was rolled with a roll press machine to adjust the properties. The resulting electrode layer had a residual solvent amount of less than 1% and was an electrode layer with good finish.

[0152] Moreover, the vapor evaporated during the heating and drying in the above step was collected to obtain a collected solution (mixed solution). The mixed solution was then placed in a flask equipped with a condenser, and the flask was heated to 185°C or higher to distill off the amine. This was continued until the amine content reached 1000 ppm (note 2), producing a regenerated N-methyl-2-pyrrolidone. The water content of the regenerated N-methyl-2-pyrrolidone was also 1000 ppm (note 2).

Claims

1. A method for producing a carbon nanotube-dispersed paste obtained by mixing and dispersing components including a pigment dispersion resin (A), carbon nanotubes (B), N-methyl-2-pyrrolidone (C), and an amine compound (D), comprising: the pigment dispersion resin (A) has at least one polar functional group selected from the group consisting of an amide group, an imide group, a hydroxyl group, a carboxyl group, a sulfonic acid group, a phosphate group, a silanol group, a cyano group, a pyrrolidone group, and an amino group, and the concentration of the polar functional group in the pigment dispersion resin (A) is 0.3 mmol / g or more and 23 mmol / g or less; A method for producing a carbon nanotube dispersion paste, wherein, when the boiling point of N-methyl-2-pyrrolidone (C) is (Xc)°C and the boiling point of the amine compound (D) is (Xd)°C, (Xc)-10>(Xd).

2. The method for producing a carbon nanotube dispersion paste according to claim 1, wherein the N-methyl-2-pyrrolidone (C) is a recycled product, the moisture content in the N-methyl-2-pyrrolidone (C) is controlled to 10,000 ppm or less, and the content of an amine compound in the N-methyl-2-pyrrolidone (C) is controlled to 10,000 ppm or less.

3. 2. The method for producing a paste dispersed with carbon nanotubes according to claim 1, wherein the paste dispersed with carbon nanotubes has a moisture content of 10,000 ppm or less.

4. 2. The method for producing a carbon nanotube-dispersed paste according to claim 1, wherein the content of the carbon nanotubes (B) is 0.1 mass % or more and less than 15 mass % based on 100 mass % of the total amount of the carbon nanotube-dispersed paste.

5. 2. The method for producing a paste dispersed with carbon nanotubes according to claim 1, wherein the paste dispersed with carbon nanotubes further contains polyvinylidene fluoride (E).

6. A method for producing a composite paste for a lithium ion secondary battery, comprising the step of mixing an electrode active material (G) with the carbon nanotube dispersion paste obtained by the method for producing a carbon nanotube dispersion paste according to any one of claims 1 to 5.

7. A method for producing an electrode layer for a lithium ion secondary battery, comprising coating a composite paste for a lithium ion secondary battery obtained by the method for producing a composite paste for a lithium ion secondary battery according to claim 6 on a current collector.

8. A step of applying the lithium ion secondary battery composite paste obtained by the method for producing a lithium ion secondary battery composite paste according to claim 6 onto a current collector and drying the same by heating; A step of recovering a vapor containing N-methyl-2-pyrrolidone (C) and an amine compound (D) to produce a mixed solution; a step of separating the amine compound (D) from the mixed solution to produce a recycled product of N-methyl-2-pyrrolidone (C); A method for producing an electrode layer for a lithium ion secondary battery containing N-methyl-2-pyrrolidone (C) and a method for producing a recycled product of N-methyl-2-pyrrolidone (C).

Citation Information

Patent Citations

  • Method for manufacturing slurry for lithium secondary battery electrode use, and slurry for electrode use