Method for producing conductive polymer dispersion, method for producing coating composition and method for producing conductive laminate

By polymerizing thiophene compounds in a carbon dioxide atmosphere with controlled agent addition and using polyanions, the method addresses viscosity increase issues, producing a conductive polymer dispersion with stable conductivity for capacitors and laminates.

JP2024173262APending Publication Date: 2024-12-12SHIN ETSU POLYMER CO LTD

Patent Information

Application Number
JP2023091576
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Conductive polymer dispersions used in capacitor production and conductive laminates face issues with increased viscosity during storage, affecting their conductivity and manufacturing stability.

Method used

The polymerization of thiophene compounds is conducted in a carbon dioxide atmosphere with controlled addition of oxidizing agents and catalysts, using a polyanion to form a conductive polymer dispersion with low viscosity and high conductivity, and further processing with ion exchange resins to stabilize the dispersion.

Benefits of technology

The method results in a conductive polymer dispersion with stable viscosity and excellent conductivity, enabling the production of high-quality capacitors and laminates with consistent performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024173262000002
    Figure 2024173262000002
  • Figure 2024173262000001
    Figure 2024173262000001
Patent Text Reader

Abstract

To provide a method for producing a conductive polymer dispersion which has reduced increase in viscosity during storage and has good conductivity after drying and curing, a method for producing a coating composition and a method for producing a conductive laminate.SOLUTION: There is provided a method for producing a conductive polymer dispersion in which conductive polymer dispersion liquid containing a polythiophene-based conductive polymer, the polyanion and water is produced by polymerizing the thiophene-based compound in reaction liquid containing an aqueous solvent, a thiophene-based compound and a polyanion, wherein the polymerization is carried out under a carbon dioxide atmosphere.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a conductive polymer dispersion containing a π-conjugated conductive polymer, a method for producing a coating composition, and a method for producing a conductive laminate. [Background technology]

[0002] A π-conjugated conductive polymer, the main chain of which is composed of a π-conjugated system, forms a conductive complex by being doped with a polyanion having an anionic group, and becomes dispersible in water. A method for manufacturing a capacitor has been disclosed in which a paint made of a conductive polymer dispersion liquid containing a conductive complex is applied to a dielectric layer provided on the surface of an anode made of a valve metal, the paint is dried to form a solid electrolyte layer, and a cathode is placed opposite the solid electrolyte layer (for example, Patent Document 1). According to this disclosure, the performance of the capacitor is improved by adding a specific unsaturated aliphatic alcohol compound to the paint. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2022-071400 Summary of the Invention [Problem to be solved by the invention]

[0004] The conductive polymer dispersion liquid used in the manufacture of the capacitor is required to have low viscosity so that it can permeate the porous structure of the dielectric layer, and the solid electrolyte layer formed by drying the permeated conductive polymer dispersion is also required to have high conductivity. However, there is a problem in that the viscosity of conventional conductive polymer dispersions increases during storage. The increase in viscosity can be a problem not only in the production of capacitors, but also in the production of conductive laminates in which a conductive polymer dispersion is applied to a substrate to form a conductive layer.

[0005] The present invention provides a method for producing a conductive polymer dispersion which reduces an increase in viscosity during storage and has good conductivity after drying and curing, a method for producing a coating composition, and a method for producing a conductive laminate. [Means for solving the problem]

[0006] [1] A method for producing a conductive polymer dispersion containing a polythiophene-based conductive polymer, the polyanion, and water, by polymerizing a thiophene-based compound in a reaction liquid containing an aqueous solvent, the thiophene-based compound, and a polyanion, wherein the polymerization is carried out in a carbon dioxide atmosphere. [2] The method for producing a conductive polymer dispersion according to [1], wherein the water solvent is brought into contact with carbon dioxide gas before the start of the polymerization. [3] The method for producing a conductive polymer dispersion according to [1] or [2], further comprising adding dry ice to the aqueous solvent. [4] The method for producing a conductive polymer dispersion according to any one of [1] to [3], comprising preparing an aqueous polyanion solution containing the polyanion and having a pH of 2 to 4 separately from the aqueous solvent, and mixing the aqueous polyanion solution with the aqueous solvent to obtain the reaction liquid. [5] The method for producing a conductive polymer dispersion according to any one of [1] to [4], wherein the polythiophene-based conductive polymer is poly(3,4-ethylenedioxythiophene). [6] The method for producing a conductive polymer dispersion according to any one of [1] to [5], wherein the polyanion is polystyrene sulfonic acid. [7] The method for producing a conductive polymer dispersion according to any one of [1] to [6], further comprising contacting the conductive polymer dispersion obtained after the polymerization with at least one of a cation exchange resin and an anion exchange resin to perform ion exchange. [8] A method for producing a coating composition, comprising the steps of obtaining a conductive polymer dispersion by the production method according to any one of [1] to [7], and blending a water-soluble organic solvent with the conductive polymer dispersion to obtain a coating composition. [9] A method for producing a conductive laminate, comprising: obtaining a conductive polymer dispersion by the production method according to any one of [1] to [7]; and applying the conductive polymer dispersion to at least a partial surface of a substrate.

[10] A method for producing a conductive laminate, comprising the steps of obtaining a coating composition by the method described in [8], and applying the coating composition to at least a portion of a surface of a substrate. Effect of the Invention

[0007] According to the method for producing a conductive polymer dispersion of the present invention, a conductive polymer dispersion in which an increase in viscosity during storage is suppressed can be obtained. In addition, the conductive polymer dispersion has good electrical conductivity in a cured product. In addition, the coating composition obtained by the method for producing a coating composition of the present invention has good electrical conductivity in a cured product. According to the method for producing a conductive laminate of the present invention, a conductive polymer dispersion in which an increase in viscosity during storage is suppressed is used, so that a conductive laminate with stable quality can be easily produced.

[0008] This invention is believed to contribute to SDGs Goal 12, "Responsible Consumption and Production."

[0009] In this specification and claims, the lower limit and upper limit of a numerical range indicated with "to" are included in the numerical range. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a cross-sectional view illustrating one embodiment of a capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Method for producing conductive polymer dispersion> A first aspect of the present invention is a method for producing a conductive polymer dispersion containing a polythiophene-based conductive polymer, the polyanion, and water, by polymerizing a thiophene-based compound in a reaction liquid containing an aqueous solvent, the thiophene-based compound, and a polyanion, and the polymerization is carried out in a carbon dioxide atmosphere.

[0012] The solvent of the reaction solution is not particularly limited as long as it can dissolve the thiophene compound and the polyanion and does not inhibit the polymerization of the thiophene compound, and is preferably water. In addition to water, a water-soluble organic solvent that is miscible with water may be included. The content of water relative to the total mass of the solvent is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and may be 100% by mass.

[0013] A first embodiment is illustrated. Carbon dioxide gas is blown into a mixed liquid containing water, a polyanion, and a catalyst, and the mixture is bubbled to increase the carbon dioxide concentration and reduce the oxygen concentration. A thiophene-based compound, which is a monomer, is added to this mixed liquid, and an oxidizing agent aqueous solution containing an oxidizing agent is gradually added dropwise or stepwise to obtain a reaction liquid. In the reaction liquid containing the catalyst and the oxidizing agent, radicals are generated as the oxidizing agent decomposes, and the polymerization of the thiophene-based compound proceeds. By slowly adding the oxidizing agent aqueous solution, a sudden increase in the oxidizing agent concentration in the reaction liquid can be suppressed, and the thiophene-based compound can be gently oxidized and polymerized, and a polythiophene-based conductive polymer can be gently formed.

[0014] A second embodiment is illustrated. Carbon dioxide gas is blown into a mixed liquid containing water, a polyanion, and an oxidizing agent, and the mixture is bubbled to increase the carbon dioxide concentration and reduce the oxygen concentration. A thiophene-based compound, which is a monomer, is added to this mixed liquid, and an aqueous catalyst solution containing a catalyst is gradually added dropwise or stepwise to obtain a reaction liquid. In the reaction liquid containing the catalyst and the oxidizing agent, radicals are generated as the oxidizing agent decomposes, and the polymerization of the thiophene-based compound proceeds. By slowly adding the aqueous catalyst solution, a sudden increase in catalyst concentration in the reaction liquid can be suppressed, and the thiophene-based compound can be gently oxidized and polymerized, and a polythiophene-based conductive polymer can be gently formed.

[0015] A third embodiment is illustrated. Dry ice is added little by little to a mixed liquid containing water, a polyanion, and a catalyst, carbon dioxide gas is generated in the mixed liquid, and the mixed liquid is bubbled to increase the carbon dioxide concentration and reduce the oxygen concentration. A thiophene-based compound, which is a monomer, is added to this mixed liquid, and an oxidizing agent aqueous solution containing an oxidizing agent is gradually added dropwise or stepwise to obtain a reaction liquid. In the reaction liquid containing the catalyst and the oxidizing agent, radicals are generated as the oxidizing agent decomposes, and the polymerization of the thiophene-based compound proceeds. It is preferable that dry ice is added little by little to the reaction liquid during the polymerization reaction, so that dry ice is always present in the reaction liquid. This allows the carbon dioxide concentration in the reaction liquid to be constantly increased. The method of adding dry ice does not require equipment for blowing carbon dioxide gas into the reaction liquid, and the carbon dioxide concentration can be easily increased.

[0016] In any of the above-mentioned embodiments, the polythiophene-based conductive polymer formed in the reaction solution is naturally doped with the polyanion, and a conductive complex consisting of the polythiophene-based conductive polymer and the polyanion is formed.

[0017] Since the polymerization can be stably progressed and a conductive polymer dispersion liquid having excellent conductivity and low viscosity can be reliably obtained, it is preferable to contact the aqueous solvent constituting the reaction liquid with carbon dioxide gas before the start of polymerization of the thiophene compound. The polymerization is initiated by the coexistence of an oxidizing agent and a catalyst in the presence of a thiophene compound as a monomer. It is preferable to mix either an oxidizing agent or a catalyst into the aqueous solvent, and to mix the other after the aqueous solvent and carbon dioxide gas are brought into contact with each other. It is preferable to mix a polyanion into the aqueous solvent in advance. It is also preferable to add the thiophene compound to the reaction system after the aqueous solvent and carbon dioxide gas are brought into contact with each other. It is preferable to slowly add the other of the oxidizing agent and the catalyst gradually or stepwise to the reaction system to which the thiophene compound has been added. By the above-mentioned suitable method, the polymerization can be gently progressed and a conductive polymer dispersion liquid having high conductivity, low viscosity, and high storage stability can be easily obtained.

[0018] The dissolved oxygen concentration in the reaction solution into which carbon dioxide has been bubbled is preferably 5.0 mg / L or less, more preferably 2.0 mg / L or less, and even more preferably 0.5 mg / L or less. Since oxygen in the reaction solution can inhibit polymerization, the polymerization proceeds stably when the oxygen concentration is low. The dissolved oxygen concentration in the reaction solution can be easily measured using a commercially available dissolved oxygen concentration meter. In the examples described below, the sampled reaction solution was measured in a glove box using an optical dissolved oxygen meter manufactured by Mettler Toledo (product name: Seven2GoPro).

[0019] When preparing the reaction liquid of this embodiment, it is preferable to prepare an aqueous polyanion solution containing the polyanion and having a pH of 2 to 4 separately from the aqueous solvent, and mix the aqueous polyanion solution with the aqueous solvent to obtain the reaction liquid. The reaction liquid obtained by this method also tends to have a pH in the range of 2 to 4. By carrying out polymerization in a reaction liquid having a pH of about 2 to 4, preferably 2 to 3, into which carbon dioxide has been blown, rather than by carrying out a reaction at a pH of less than 1, a conductive polymer dispersion having a lower viscosity and high storage stability can be obtained.

[0020] It is preferable to add a known catalyst and oxidizing agent to the reaction solution to promote the chemical oxidation of the thiophene compound. Examples of the catalyst include transition metal compounds such as ferric chloride, ferric sulfate, ferric nitrate, and cupric chloride. Examples of the oxidizing agent include persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate.

[0021] The amount of the catalyst to be mixed relative to the total mass of the reaction liquid is, for example, preferably from 0.01% by mass to 0.50% by mass, and more preferably from 0.01% by mass to 0.30% by mass.

[0022] The amount of the oxidizing agent relative to the total mass of the reaction liquid is, for example, preferably 0.10% by mass or more and 5.00% by mass or less, more preferably 0.30% by mass or more and 3.00% by mass or less, and even more preferably 0.50% by mass or more and 2.50% by mass or less.

[0023] The amount of the thiophene compound relative to the total mass of the reaction liquid is, for example, preferably from 0.1% by mass to 3.0% by mass, more preferably from 0.3% by mass to 2.0% by mass, and even more preferably from 0.5% by mass to 1.5% by mass. When the content is within the above preferred range, it becomes easy to polymerize almost all of the thiophene-based compound contained in the reaction liquid, and it becomes easy to obtain a conductive polymer dispersion liquid having low viscosity and excellent storage stability.

[0024] The amount of the polyanion relative to the total mass of the reaction solution is, for example, preferably 0.1% by mass to 5.0% by mass, more preferably 1.0% by mass to 4.0% by mass, and even more preferably 1.5% by mass to 3.0% by mass. When the content is within the above preferred range, the polythiophene-based conductive polymer formed by the polymerization reaction is sufficiently doped with the polyanion, and a conductive polymer dispersion having excellent water dispersibility, low viscosity, and excellent storage stability can be easily obtained.

[0025] The combined amount of the thiophene compound and the polyanion relative to the total mass of the reaction liquid is preferably 1.0 to 10.0 mass %, more preferably 1.5 to 6.0 mass %, and even more preferably 2.0 to 4.0 mass %. When the content is equal to or greater than the lower limit, the production efficiency of the conductive composite is improved, and when the content is equal to or less than the upper limit, a conductive polymer dispersion having superior storage stability can be obtained.

[0026] Since a conductive composite having excellent water dispersibility is easily obtained, the ratio of the thiophene-based compound and the polyanion to be mixed in the reaction solution is preferably 1 part by mass or more and 1,000 parts by mass or less, more preferably 10 parts by mass or more and 700 parts by mass or less, and even more preferably 100 parts by mass or more and 500 parts by mass or less, relative to 100 parts by mass of the thiophene-based compound.

[0027] (Thiophene compounds) Thiophene compounds are monomers that polymerize to form polythiophene conductive polymers, the main chain of which constitutes a π-conjugated system. Polythiophene-based conductive polymers include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), and poly(3-iodothiophene). thiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), oxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-di dodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), and poly(3-methyl-4-carboxybutylthiophene). Among these polythiophene-based conductive polymers, poly(3,4-ethylenedioxythiophene) is particularly preferred because of its excellent conductivity, transparency, and heat resistance. The thiophene-based compound to be added to the reaction solution may be one type or two or more types.

[0028] (Polyanion) The polyanion to be added to the reaction solution is a polymer having two or more monomer units each having an anionic group in the molecule. The anionic group of this polyanion functions as a dopant for the polythiophene-based conductive polymer, improving the conductivity of the polythiophene-based conductive polymer. The anion group of the polyanion is preferably a sulfo group or a carboxy group. Specific examples of such polyanions include polymers having a sulfo group, such as polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic acid esters having a sulfo group, polymethacrylic acid esters having a sulfo group (for example, poly(4-sulfobutyl methacrylate, polysulfoethyl methacrylate, polymethacryloyloxybenzenesulfonic acid), poly(2-acrylamido-2-methylpropanesulfonic acid), and polyisoprene sulfonic acid; and polymers having a carboxy group, such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), and polyisoprene carboxylic acid. The polyanion may be a homopolymer in which a single monomer is polymerized, or a copolymer in which two or more monomers are polymerized. Among these polyanions, polymers having a sulfo group are preferred, and polystyrene sulfonic acid is more preferred, since they can provide higher electrical conductivity. The polyanion to be added to the reaction solution may be one type or two or more types.

[0029] The weight average molecular weight Mw of the polyanion is preferably from 20,000 to 1,000,000, and more preferably from 50,000 to 800,000. When the weight average molecular weight Mw is within the above preferred range, the storage stability of the conductive polymer dispersion of this embodiment is further improved. The weight average molecular weight Mw is an average molecular weight based on mass measured by gel filtration chromatography and calculated as pullulan.

[0030] In the polyanion doped into the polythiophene conductive polymer, some of the anion groups are not doped into the polythiophene conductive polymer, and there are excess anion groups that are not involved in the doping. Since these excess anion groups are hydrophilic groups, the conductive complex has high water dispersibility and low organic solvent dispersibility. When the number of all anionic groups in the polyanion is taken as 100 mol %, the excess anionic groups are preferably from 30 mol % to 90 mol %, more preferably from 45 mol % to 75 mol %.

[0031] The temperature of the reaction solution during the polymerization reaction, i.e., the reaction temperature, can be, for example, 10 to 30° C. At the reaction temperature, the polymerization reaction is usually completed within about 4 to 12 hours. The completion of the polymerization reaction can be determined by measuring the amount of unreacted thiophene-based compound in the reaction solution by gas chromatography or the like.

[0032] The content ratio (by mass) of polythiophene-based conductive polymer:polyanion in the conductive complex in the reaction solution after the reaction is completed is approximately the same as the ratio of the thiophene-based compound and polyanion blended in the reaction solution. In other words, the content ratio of the monomer and polyanion blended in the reaction solution is reflected in the content ratio of the polythiophene-based conductive polymer and polyanion in the conductive complex contained in the conductive polymer dispersion.

[0033] [Conductive composite] Since the reaction solution contains polyanions in advance, the polyanions naturally dope with the polythiophene-based conductive polymer formed by the polymerization reaction to form a conductive complex having electrical conductivity. In the manufacturing method of this embodiment, a conductive polymer dispersion is obtained in which the conductive complex is dispersed in water as a solvent. In this specification and claims, the dispersed state and the dissolved state are not distinguished unless otherwise specified.

[0034] The content of the polyanion in the conductive complex is preferably in the range of 1 part by mass to 1000 parts by mass, more preferably 10 parts by mass to 700 parts by mass, and even more preferably 100 parts by mass to 500 parts by mass, per 100 parts by mass of the polythiophene-based conductive polymer. If the content of the polyanion is equal to or greater than the lower limit, the doping effect on the polythiophene-based conductive polymer tends to be stronger, and the conductivity becomes higher. On the other hand, if the content of the polyanion is equal to or less than the upper limit, the relative proportion of the polythiophene-based conductive polymer can be increased, so that the conductivity can be ensured.

[0035] Since the conductive polymer dispersion (reaction liquid) after the polymerization reaction contains residual decomposition products of the added catalyst and oxidizing agent, it may be preferable to remove these before using the conductive polymer dispersion. Examples of the removal method include a method of contacting the conductive polymer dispersion with an ion exchange resin to adsorb the catalyst and oxidizing agent to the ion exchange resin, and a method of ultrafiltrating the conductive polymer dispersion to remove them together with replacement of the dispersion medium. Among these, the method of using an ion exchange resin is preferable because it is simple. It is preferable to use a cation exchange resin and an anion exchange resin in combination as the ion exchange resin.

[0036] The conductive polymer dispersion may be subjected to a dispersion treatment by a conventional method such as using a high-pressure homogenizer.

[0037] The content of the conductive complex relative to the total mass of the conductive polymer dispersion is preferably from 0.01 to 5.0 mass%, more preferably from 1.0 to 4.0 mass%, and even more preferably from 1.5 to 3.0 mass%. When the content is at least as large as the lower limit of the above range, the conductivity of the conductive layer formed by curing the conductive polymer dispersion can be further improved. When the content is equal to or less than the upper limit of the above range, the dispersibility of the conductive composite in the conductive polymer dispersion can be improved, and the storage stability can be further improved.

[0038] The initial viscosity of the conductive polymer dispersion at 23°C (viscosity immediately after production to within one day) is preferably 60 mPa·s or less, more preferably 50 mPa·s or less, even more preferably 40 mPa·s or less, and particularly preferably 30 mPa·s or less, when the concentration of the conductive complex relative to the total mass of the conductive polymer dispersion is adjusted to 1.6 mass%. There is no particular restriction on the lower limit of the viscosity, and a guideline is 1 mPa·s or more. The storage viscosity of a conductive polymer dispersion having the above viscosity after being left to stand and stored at 20 to 25° C. for 30 days is preferably 70 mPa·s or less, more preferably 60 mPa·s or less, even more preferably 50 mPa·s or less, and particularly preferably 40 mPa·s or less. There is no particular restriction on the lower limit of the viscosity, and a guideline is 1 mPa·s or more. When the composition has a viscosity within the above preferred range, when used in the manufacture of a capacitor, the production of a solid electrolyte layer becomes easy, and the capacitor performance can be improved. In measuring the viscosity, the conductive polymer dispersion preferably contains only ion-exchanged water as a dispersion medium, and preferably does not contain any additives other than the conductive complex. The viscosity was measured at 23° C. using a tuning fork vibration viscometer in accordance with JIS Z8803:2011 (viscosity measurement method using a vibration viscometer).

[0039] <Action and effect> The conductive polymer dispersion produced by this embodiment can be stably stored while maintaining high conductivity and low viscosity, which is a marked improvement over the conductive polymer dispersion obtained by a conventional polymerization method (see Comparative Example described below). Although the details of the mechanism are not yet clear, it is believed that this is due to the fact that polymerization in the reaction solution under a carbon dioxide atmosphere is milder and / or more stable than in the past.

[0040] <Coating composition (paint)> In order to enhance the wettability of the conductive polymer dispersion to the substrate, a water-soluble organic solvent may be added to the conductive polymer dispersion. The conductive polymer dispersion to which the water-soluble organic solvent has been added is sometimes called a coating composition (paint). The coating composition contains water, a conductive complex, and a water-soluble organic solvent. A mixed medium of water and a water-soluble organic solvent is sometimes called an aqueous dispersion medium.

[0041] A second aspect of the present invention is a method for producing a coating composition, comprising the steps of obtaining a conductive polymer dispersion by the production method of the first aspect, and blending a water-soluble organic solvent with the conductive polymer dispersion to obtain a coating composition.

[0042] A water-soluble organic solvent is an organic solvent that dissolves in an amount of 1 g or more in 100 g of water at 20°C. Examples of the water-soluble organic solvent include alcohol-based solvents, ether-based solvents, ketone-based solvents, nitrogen atom-containing solvents, and ester-based solvents. Examples of alcohol-based solvents include methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 2-methyl-2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, allyl alcohol, ethylene glycol, propylene glycol, propylene glycol monomethyl ether, and ethylene glycol monomethyl ether. Examples of the ether solvent include diethyl ether, dimethyl ether, propylene glycol dialkyl ether, and diethylene glycol diethyl ether. Examples of the ketone solvent include diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl amyl ketone, diisopropyl ketone, methyl ethyl ketone, acetone, and diacetone alcohol. Examples of the nitrogen atom-containing solvent include N-methylpyrrolidone, dimethylacetamide, and dimethylformamide. The water-soluble organic solvent may be contained alone or in combination of two or more kinds. As the water-soluble organic solvent, an alcohol-based solvent or a ketone-based solvent is preferred, and an alcohol-based solvent is more preferred, since this improves the applicability of the coating composition to the substrate.

[0043] The content of the water-soluble organic solvent relative to the total mass of the aqueous dispersion medium is preferably 30 to 70 mass %, more preferably 40 to 60 mass % or more, and the content of water relative to the total mass of the aqueous dispersion medium is preferably 70 to 30 mass %, more preferably 60 to 40 mass % or less. When the content is within the above suitable range, it is possible to improve the wettability of the conductive composite to the substrate while suppressing deterioration over time of the dispersion stability of the conductive composite in the coating composition.

[0044] The content of the conductive complex relative to the total mass of the coating composition is, for example, preferably 0.1 to 2.5 mass%, more preferably 0.3 to 2.0 mass%, and even more preferably 0.5 to 1.5 mass%. Within the above range, it is possible to suppress the deterioration of the dispersion stability of the conductive complex in the coating composition over time, and it is possible to form a conductive layer or the like with good conductivity.

[0045] (Polyol Compound) The coating composition may further contain one or more polyol compounds. Here, the polyol compound refers to a compound having two or more hydroxyl groups. By containing the polyol compound, the conductivity of the conductive layer formed by curing the conductive polymer dispersion can be increased, and the equivalent series resistance in the solid electrolyte layer of the capacitor can be reduced.

[0046] Examples of the polyol compound include one or more selected from ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, glycerin, pentaerythritol, trimethylolpropane, and trimethylolethane.

[0047] The content of the polyol compound in the coating composition is, for example, preferably 100 parts by mass or more and 10,000 parts by mass or less, more preferably 200 parts by mass or more and 2,000 parts by mass or less, and even more preferably 300 parts by mass or more and 1,000 parts by mass or less, relative to 100 parts by mass of the conductive composite. When the content is within the above range, the above-mentioned effects can be more effectively obtained.

[0048] The content of the polyol compound relative to the total mass of the coating composition is, for example, preferably from 1 to 20 mass%, more preferably from 2 to 10 mass%, and further preferably from 3 to 8 mass%. When the content is within the above range, the coatability of the coating composition is improved, and the above-mentioned effects are more effectively obtained.

[0049] (Other additives) The coating composition and the conductive polymer dispersion may contain other known additives. Examples of the additives that can be used include surfactants, inorganic conductive agents, antifoaming agents, coupling agents, antioxidants, and ultraviolet absorbing agents. The surfactant may be a nonionic, anionic or cationic surfactant, with the nonionic surfactant being preferred from the standpoint of storage stability. A polymer surfactant such as polyvinylpyrrolidone may also be added. Examples of the inorganic conductive agent include metal ions, conductive carbon, etc. Metal ions can be generated by dissolving a metal salt in water. The antifoaming agent includes silicone resin, polydimethylsiloxane, silicone oil, and the like. The coupling agent may be a silane coupling agent having a vinyl group or an amino group. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, oxanilide-based ultraviolet absorbers, hindered amine-based ultraviolet absorbers, and benzoate-based ultraviolet absorbers. When the above-mentioned additives are contained, the content ratio is appropriately determined depending on the type of additive, but can be, for example, in the range of 0.001 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the conductive composite.

[0050] <Method for manufacturing conductive laminate> A third aspect of the present invention is a method for producing a conductive laminate, the method comprising the steps of obtaining a conductive polymer dispersion by the production method of the first aspect, and applying the conductive polymer dispersion to at least a partial surface of a substrate to form a conductive layer. A fourth aspect of the present invention is a method for producing a conductive laminate, comprising the steps of obtaining a coating composition by the production method of the second aspect, and applying the coating composition to at least a part of a surface of a substrate to form a conductive layer.

[0051] Examples of a method for applying (coating) the conductive polymer dispersion or coating composition to any surface of a substrate include a method using a coater such as a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, or a screen coater; a method using a sprayer such as an air spray, an airless spray, or a rotor dampening; and an immersion method such as dipping.

[0052] The amount of the conductive polymer dispersion or coating composition applied to the substrate is not particularly limited, but may be, for example, 0.01 to 10.0 g / m as a non-volatile component. 2 The range is preferably:

[0053] A conductive layer can be formed by drying a coating film made of a conductive polymer dispersion or a coating composition applied onto a substrate to remove at least a portion of the dispersion medium and curing the coating film. Methods for drying the coating film include heat drying, vacuum drying, etc. Examples of heat drying that can be used include hot air heating and infrared heating. When applying heat drying, the heating temperature is appropriately set depending on the dispersion medium used, but is usually within the range of 50° C. to 200° C. Here, the heating temperature is the set temperature of the drying device. A suitable drying time within the above heating temperature range is preferably 0.5 minutes to 30 minutes, more preferably 1 minute to 15 minutes.

[0054] <Conductive laminate> The conductive laminate obtained by the manufacturing methods of the third and fourth aspects comprises a substrate and a conductive layer formed on at least a portion of the surface of the substrate, the conductive layer being made of the conductive polymer dispersion obtained in the first aspect or the cured product of the coating composition obtained in the second aspect.

[0055] [Conductive layer] The conductive layer may be formed over the entire surface of any surface of the substrate, or over a portion of the entire surface. In the conductive film, it is preferable that a conductive layer of substantially uniform thickness is formed over substantially the entire surface of one surface or the other surface of the film substrate. When a conductive layer is formed only over a portion of the surface of the substrate, the conductive layer may be, for example, a fine conductive pattern such as a circuit or an electrode, or the conductive layer may be provided on the same surface and the conductive layer may be not provided on the same surface and may be roughly divided.

[0056] The average thickness of the conductive layer is, for example, preferably 10 nm or more and 100 μm or less, more preferably 20 nm or more and 50 μm or less, and even more preferably 30 nm or more and 30 μm or less. When the average thickness of the conductive layer is equal to or greater than the lower limit, high conductivity can be exhibited, and when the average thickness is equal to or less than the upper limit, the adhesion of the conductive layer to the substrate is further improved.

[0057] [Base material] The substrate may be a substrate made of an insulating material or a substrate made of a conductive material. The shape of the substrate is not particularly limited, and examples thereof include a shape mainly having a flat surface, such as a film or a substrate. Examples of insulating materials include glass, synthetic resin, and ceramics. The conductive material may be a metal, a conductive metal oxide, carbon, or the like.

[0058] (Film substrate) When a film substrate is used as the substrate, the conductive laminate becomes a conductive film. The film substrate may be, for example, a plastic film made of a synthetic resin, such as ethylene-methyl methacrylate copolymer resin, ethylene-vinyl acetate copolymer resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyvinylidene fluoride, polyarylate, styrene-based elastomer, polyester-based elastomer, polyethersulfone, polyetherimide, polyetheretherketone, polyphenylene sulfide, polyimide, cellulose triacetate, cellulose acetate propionate, etc. From the viewpoint of improving the adhesion between the film substrate and the conductive layer, the synthetic resin for the film substrate is preferably a polyester resin, and among these, polyethylene terephthalate is preferable.

[0059] The synthetic resin for the film substrate may be either amorphous or crystalline. The film substrate may be either unstretched or stretched. The film substrate may be subjected to a surface treatment such as a corona discharge treatment, a plasma treatment, or a flame treatment in order to further improve the adhesion of the conductive layer.

[0060] The average thickness of the film substrate is preferably 5 μm to 500 μm, more preferably 20 μm to 200 μm. If the average thickness of the film substrate is equal to or more than the lower limit, the film is less likely to break, and if the average thickness is equal to or less than the upper limit, the film can have sufficient flexibility. The average thickness of the film substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.

[0061] (Glass substrate) Examples of the glass substrate include an alkali-free glass substrate, a soda-lime glass substrate, a borosilicate glass substrate, and a quartz glass substrate. If the substrate contains an alkali component, the conductivity of the conductive layer tends to decrease, so among the above glass substrates, an alkali-free glass is preferred. Here, the alkali-free glass refers to a glass composition in which the content of the alkali component is 0.1 mass% or less with respect to the total mass of the glass composition.

[0062] The average thickness of the glass substrate is preferably from 100 μm to 3000 μm, more preferably from 100 μm to 1000 μm. If the average thickness of the glass substrate is equal to or more than the lower limit, the substrate is less likely to break, and if the average thickness is equal to or less than the upper limit, the substrate can contribute to a thinner conductive laminate. The average thickness of the glass substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.

[0063] <Capacitor manufacturing method> A fifth aspect of the present invention is a method for producing a capacitor, comprising the steps of obtaining a conductive polymer dispersion or a coating composition by the production method according to the third or fourth aspect, and applying the conductive polymer dispersion or the coating composition to a surface of a dielectric layer formed on a surface of an anode made of a porous body of a valve metal, and drying the conductive polymer dispersion or the coating composition to form a solid electrolyte layer.

[0064] The method for manufacturing a capacitor of this embodiment preferably includes a step of oxidizing the surface of an anode made of a porous valve metal to form a dielectric layer (dielectric forming step), a step of arranging a cathode in a position facing the dielectric layer (cathode forming step), and a step of forming a solid electrolyte layer on at least a part of the surface of the dielectric layer (film forming step). Each step will be described below with reference to FIG.

[0065] [Dielectric formation process] In this step, the surface of anode 11 made of a porous valve metal is oxidized to form dielectric layer 12. The method for forming dielectric layer 12 is not particularly limited, and examples thereof include a method in which the surface of anode 11 is anodized in an electrolyte for chemical conversion treatment, such as an aqueous solution of ammonium adipate, an aqueous solution of ammonium borate, or an aqueous solution of ammonium phosphate.

[0066] [Cathode formation process] In this step, the cathode 13 is disposed at a position facing the dielectric layer 12. The method for disposing the cathode 13 is not particularly limited, and examples thereof include a method of forming the cathode 13 using a conductive paste such as a carbon paste or a silver paste, and a method of disposing a metal foil such as an aluminum foil facing the dielectric layer 12.

[0067] [Film forming process] In this step, the aforementioned conductive polymer dispersion or coating composition is applied to at least a portion of the surface of the dielectric layer 12 and then dried to form the solid electrolyte layer 14.

[0068] Examples of the method for applying the conductive polymer dispersion or coating composition include immersion (dip coating), comma coating, reverse coating, lip coating, and microgravure coating. Of these, a method in which the anode 11 is immersed in the conductive polymer dispersion or coating composition under reduced pressure is preferred. The immersion method allows the conductive polymer dispersion or coating composition to be sufficiently applied even to the inside of the porous structure on the surface of the dielectric layer 12. After immersion, the anode is removed and subjected to the next drying treatment.

[0069] Examples of the drying method include room temperature drying, hot air drying, far infrared drying, etc. Among these, hot air drying is preferred. The drying temperature is, for example, preferably 100 to 180° C., and more preferably 120 to 150° C. The drying time is, for example, preferably 0.2 to 1 hour. After drying, the capacitor can be assembled in the usual manner.

[0070] <Capacitor> A sixth aspect of the present invention comprises an anode made of a porous body of a valve metal, a dielectric layer made of an oxide of the valve metal, a cathode made of a conductive material provided on the dielectric layer opposite to the anode, and a solid electrolyte layer formed between the dielectric layer and the cathode, the solid electrolyte layer containing a cured product of the conductive polymer dispersion or coating composition obtained by the manufacturing method of the first to second aspects. The capacitor of the sixth aspect can be manufactured by the manufacturing method of the fifth aspect.

[0071] An example of an embodiment of the sixth aspect will be described with reference to Fig. 1. A capacitor 10 shown in Fig. 1 includes an anode 11 made of a porous body of a valve metal, a dielectric layer 12 made of an oxide of the valve metal, a solid electrolyte layer 14 formed on the surface of the dielectric layer 12, and a cathode 13 provided on the outermost side. The cathode 13 is provided on the opposite side to the anode 11, with the dielectric layer 12 and the solid electrolyte layer 14 sandwiched therebetween.

[0072] Examples of valve metals constituting the anode 11 include aluminum, tantalum, niobium, titanium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony. Among these, aluminum, tantalum, and niobium are preferable. Specific examples of the anode 11 include an aluminum foil that has been etched to increase its surface area and then oxidized, and a tantalum or niobium particle sintered body that has been oxidized and pelletized. Such a processed body is a porous body with irregularities on the surface.

[0073] The dielectric layer 12 in this embodiment is a layer formed by oxidizing the surface of the anode 11, for example, by anodizing the surface of the metallic anode 11 in an electrolyte such as an aqueous solution of ammonium adipate. Similar to the anode 11, the dielectric layer 12 also has projections and recesses.

[0074] The cathode 13 in this embodiment may be a conductive layer formed from a conductive paste or a metal layer made of a conductive material such as aluminum foil.

[0075] The solid electrolyte layer 14 in this embodiment is formed on the surface of the dielectric layer 12. The solid electrolyte layer 14 covers at least a portion of the surface of the dielectric layer 12, and may cover the entire surface of the dielectric layer 12. The thickness of the solid electrolyte layer 14 may be constant or may not be constant, and may be, for example, between 1 μm and 100 μm.

[0076] [Electrolyte] The capacitor of this embodiment may have an electrolyte that impregnates the solid electrolyte layer. Examples of the solvent constituting the electrolytic solution include alcohol-based solvents such as ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, and glycerin; lactone-based solvents such as γ-butyrolactone, γ-valerolactone, and δ-valerolactone; sulfur-based solvents such as sulfolane, dimethyl sulfoxide, and dimethyl sulfone; amide-based solvents such as N-methylformamide, N,N-dimethylformamide, N-methylacetamide, and N-methylpyrrolidinone; nitrile-based solvents such as acetonitrile and 3-methoxypropionitrile; and water. Examples of the electrolyte constituting the electrolytic solution include organic acids such as adipic acid, glutaric acid, succinic acid, benzoic acid, isophthalic acid, phthalic acid, terephthalic acid, maleic acid, toluic acid, enanthic acid, malonic acid, formic acid, decanedicarboxylic acids such as 1,6-decanedicarboxylic acid and 5,6-decanedicarboxylic acid, octanedicarboxylic acids such as 1,7-octanedicarboxylic acid, azelaic acid, and sebacic acid; or boric acid, a polyhydric alcohol complex compound of boric acid obtained from boric acid and a polyhydric alcohol; inorganic acids such as phosphoric acid, carbonic acid, and silicic acid as anion components, and primary amines (methylamine, ethylamine, propylamine, butylamine, ethylenediamine, etc.), secondary amines (dimethylamine, diethylamine, dipropylamine, methylethylamine, diphenylamine, etc.), tertiary amines (trimethylamine, triethylamine, tripropylamine, triphenylamine, 1,8-diazabicyclo(5,4,0)-undecene-7, etc.), tetraalkylammonium (tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, methyltriethylammonium, dimethyldiethylammonium, etc.), etc., as a cationic component.

[0077] The capacitor of this embodiment is not limited to the above configuration, and a separator may be provided between the dielectric layer and the cathode. An example of a capacitor having a separator provided between the dielectric layer and the cathode is a wound type capacitor. Examples of the separator include sheets (including nonwoven fabrics) made of cellulose, polyvinyl alcohol, polyester, polyethylene, polystyrene, polypropylene, polyimide, polyamide, polyvinylidene fluoride, etc., and nonwoven fabrics of glass fibers. The density of the separator is, for example, 0.1 g / cm 3 More than 1.0g / cm 3 The following are included: When a separator is provided, a method of forming a cathode by impregnating the separator with carbon paste or silver paste can also be applied. EXAMPLES

[0078] [Preparation of polyanions] As a raw material, an aqueous solution (concentration 30%) of poly(sodium 4-styrenesulfonate) having a weight average molecular weight of 200,000 manufactured by Sigma-Aldrich was used. First, ion-exchanged water was added to an aqueous solution of poly(sodium 4-styrenesulfonate) to adjust it to a uniform aqueous solution with a solid concentration of 15 wt%, and cation-exchange resin was added until the pH became less than 1. After that, the cation-exchange resin was filtered off using a stainless steel mesh filter, and the solid concentration was adjusted to 10 wt% with ion-exchanged water to obtain an aqueous solution of polystyrenesulfonic acid (PSS aqueous solution).

[0079] [Preparation of thiophene compounds] Commercially available 3,4-ethylenedioxythiophene (Tokyo Chemical Industry Co., Ltd.) was purchased and purified by vacuum distillation before use in the reaction.

[0080] [Example 1] 91g of PSS aqueous solution, 400g of ion-exchanged water, and 0.50g of ferric sulfate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 1000ml three-neck flask, and carbon dioxide was bubbled at a flow rate of 1L / min for 10 minutes, and the mixture was stirred under a carbon dioxide atmosphere and kept at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution and stirred for another hour. 70.9g of a 10wt% aqueous solution of sodium peroxodisulfate (manufactured by Junsei Chemical Industries, Ltd.) was added to this solution using a metering pump over a period of 2 hours. The mixture was then stirred at 25°C for 3 hours to react, synthesizing the conductive polymer PEDOT-PSS. 100g of ion-exchanged water, 100g of cation exchange resin (Duolite C255LFH, exchange capacity 2.0eq. / L, manufactured by Sumika Chemtex Co., Ltd.), and 100g of anion exchange resin (Duolite A368MS, exchange capacity 1.7eq. / L, manufactured by Sumika Chemtex Co., Ltd.) were added to this reaction solution and stirred for 30 minutes. The ion-exchange resin was filtered off using a stainless steel mesh filter, and a dispersion treatment was carried out using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 1.9wt%. Ion-exchanged water was added to this conductive polymer dispersion to adjust the solid concentration to 1.6wt%.

[0081] [Example 2] 91g of PSS aqueous solution, 200g of ion-exchanged water, and 7.09g of sodium peroxodisulfate were added to a 1000ml three-neck flask, and the mixture was bubbled with carbon dioxide at a flow rate of 1L / min for 10 minutes, stirred under a carbon dioxide atmosphere, and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution, and the mixture was stirred for another hour. 29.9g of 1wt% aqueous solution of iron(III) nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to this solution using a metering pump over 15 minutes. The mixture was then stirred at 25°C for 3 hours to react, synthesizing the conductive polymer PEDOT-PSS. In this reaction, the sum of the solid concentration of the thiophene compound and the polyanion was 3.8wt%. 100g of ion-exchanged water, 100g of cation-exchanged resin, and 100g of anion-exchanged resin were added to this reaction solution and stirred for 30 minutes. The ion-exchanged resin was filtered out using a stainless steel mesh filter, and a dispersion treatment was carried out using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 2.5wt%. Ion-exchanged water was added to this conductive polymer dispersion to adjust the solid concentration to 1.6wt%.

[0082] [Example 3] 91g of PSS aqueous solution, 400g of ion-exchanged water, and 0.50g of ferric sulfate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to a 1000ml three-neck flask and stirred for 1 hour, and then dry ice was added little by little until the dissolved oxygen was 1.0mg / L or less. 3.5g of 3,4-ethylenedioxythiophene purified by distillation was added to this solution and stirred for another 1 hour. The temperature of the solution at this time was 12°C. 1.0g of sodium peroxodisulfate was added to this solution at 30 minute intervals for a total of 7 times, and the solution was stirred for 6 hours to react, synthesizing PEDOT-PSS, a conductive polymer. Dry ice was added from time to time so that dry ice was always present in the reaction vessel. The temperature of the reaction solution was 10-15°C. To this reaction solution, 100 g of ion-exchanged water, 100 g of cation exchange resin (Duolite C255LFH, exchange capacity 2.0 eq. / L, manufactured by Sumika Chemtex Corp.), and 100 g of anion exchange resin (Duolite A368MS, exchange capacity 1.7 eq. / L, manufactured by Sumika Chemtex Corp.) were added and stirred for 30 minutes. The ion exchange resin was filtered off using a stainless steel mesh filter, and a dispersion treatment was carried out using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a solid concentration of 1.6 wt%.

[0083] [Example 4] A PSS aqueous solution having a solid content of 10 wt% and a pH of 3 was obtained in the same manner as described in the section on preparation of polyanion, except that the amount of cation exchange resin added was adjusted to pH 3. Using this PSS aqueous solution, PEDOT-PSS was synthesized in the same manner as in Example 1, and a conductive polymer dispersion having a solid content of 1.6 wt% was obtained.

[0084] [Comparative Example 1] PEDOT-PSS was synthesized in the same manner as in Example 1, except that dry air was used instead of carbon dioxide, to obtain a conductive polymer dispersion liquid with a solid content concentration adjusted to 1.6 wt %.

[0085] [Comparative Example 2] PEDOT-PSS was synthesized in the same manner as in Example 1, except that nitrogen was used instead of carbon dioxide, to obtain a conductive polymer dispersion liquid with a solid content concentration adjusted to 1.6 wt %.

[0086] The conductive polymer dispersions obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were evaluated by the following method.

[0087] <Evaluation of Viscosity> The viscosity of the conductive polymer dispersion having a solid content concentration of 1.6 wt % obtained in each example was measured at 23° C. using a vibration type viscometer. The measurement results of the initial viscosity are shown in Table 1. The above viscosity is a value measured at 23° C. using a tuning fork vibration viscometer in accordance with JIS Z8803:2011 (viscosity measurement method using a vibration viscometer).

[0088] <Evaluation of storage stability> The conductive polymer dispersion obtained in each example was stored at 24°C for 30 days, after which the viscosity was measured. The measurement results of the viscosity after storage and the calculated increase rate (%) based on the ratio to the initial viscosity are shown in Table 1. Note that a lower increase rate indicates less viscosity change and better storage stability.

[0089] <Evaluation of electrical conductivity> To 50 g of the conductive polymer dispersion obtained in each example, 0.01 g of an acetylene surfactant (Dinol 604, manufactured by Nissin Chemical Industry Co., Ltd.), 45 g of methanol, and 5 g of ethylene glycol were added and thoroughly mixed to prepare a coating composition. This coating material was applied to a polyethylene terephthalate film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater with a wet film thickness of 8 μm, and a conductive film was obtained by heating and drying at a drying temperature of 100° C. for 1 minute. The surface resistance value of the obtained conductive film was measured using a resistivity meter (Loresta, manufactured by Nitto Seiko Analytech Co., Ltd.) under the condition of an applied voltage of 10 V. The results are shown in Table 1. The lower the surface resistance value, the higher and better the conductivity.

[0090] [Table 1]

[0091] From the above, it is clear that the manufacturing methods of Examples 1 to 4 according to the present invention are capable of forming a conductive layer exhibiting excellent conductivity, and are capable of obtaining a conductive polymer dispersion having high storage stability in which a low viscosity is maintained even during storage. [Explanation of symbols]

[0092] 10 Capacitor 11 Anode 12 Dielectric layer 13 Cathode 14 Solid electrolyte layer

Claims

1. A method for producing a conductive polymer dispersion containing a polythiophene-based conductive polymer, the polyanion, and water, by polymerizing a thiophene-based compound in a reaction liquid containing an aqueous solvent, the thiophene-based compound, and a polyanion, the method comprising the steps of: The method for producing a conductive polymer dispersion, wherein the polymerization is carried out in a carbon dioxide atmosphere.

2. The method for producing a conductive polymer dispersion according to claim 1 , wherein the water solvent is contacted with carbon dioxide gas before the start of the polymerization.

3. The method for producing a conductive polymer dispersion according to claim 2 , further comprising the step of adding dry ice to the aqueous solvent.

4. 2. The method for producing a conductive polymer dispersion according to claim 1, further comprising the steps of: preparing an aqueous polyanion solution containing the polyanion and having a pH of 2 to 4 separately from the aqueous solvent; and mixing the aqueous polyanion solution with the aqueous solvent to obtain the reaction liquid.

5. 2. The method for producing a conductive polymer dispersion according to claim 1, wherein the polythiophene-based conductive polymer is poly(3,4-ethylenedioxythiophene).

6. The method for producing a conductive polymer dispersion according to claim 1 , wherein the polyanion is polystyrene sulfonic acid.

7. The method for producing a conductive polymer dispersion according to claim 1 , further comprising contacting the conductive polymer dispersion obtained after the polymerization with at least one of a cation exchange resin and an anion exchange resin to carry out ion exchange.

8. A method for producing a coating composition, comprising: obtaining a conductive polymer dispersion by the production method according to any one of claims 1 to 7; and blending a water-soluble organic solvent with the conductive polymer dispersion to obtain a coating composition.

9. A method for producing a conductive laminate, comprising: obtaining a conductive polymer dispersion by the production method according to any one of claims 1 to 7; and applying the conductive polymer dispersion to at least a partial surface of a substrate.

10. A method for producing a conductive laminate, comprising the steps of obtaining a coating composition by the production method according to claim 8 and applying the coating composition to at least a portion of a surface of a substrate.

Citation Information

Patent Citations

  • Carbon dioxide sensitive material and carbon dioxide sensor

    JP2004361336A

  • Method for improving conductivity of conductive polymer

    JP2009215422A

  • Electroconductive NANO sized polymer particles and method for producing the conductive NANO sized polymer particles

    JP2009215424A

  • Biologically integrated electrode device

    JP2009506836A

  • Process to produce functionalized polythiophenes

    JP2018507268A

Cited By

  • Liquid dispersion, separator for electrolytic capacitor, electrolytic capacitor, and method for producing electrolytic capacitor

    WO2026182214A1