Resin composition, cured coating film, and method for producing the same

A dual-cure resin composition with specific components and ratios addresses the issues of blocking resistance and hardness in curable compositions, resulting in a cured film with enhanced handling and thermoformability.

JP2024179704APending Publication Date: 2024-12-26CHUGOKU MARINE PAINTS

Patent Information

Application Number
JP2023098753
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-15
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Existing curable compositions for plastic film decoration lack sufficient blocking resistance, transparency, and hardness, especially when used as a surface protective layer, and require improved handling properties and moldability during thermoforming.

Method used

A dual-cure type resin composition combining an alkylated melamine resin, trifunctional or higher (meth)acrylate monomer, (meth)acrylate resin with specific molecular weight, and a photopolymerization initiator, with a specific mass ratio, is used to achieve a semi-cured state that is then photocured for enhanced properties.

Benefits of technology

The resin composition forms a cured film with excellent handling properties, transparency, blocking resistance, and heat extensibility, providing improved hardness and suitability for thermoforming applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024179704000001
    Figure 2024179704000001
  • Figure 2024179704000002
    Figure 2024179704000002
Patent Text Reader

Abstract

To provide a resin composition capable of forming a cured coating film excellent in appearance, transparency, blocking resistance, heating extensibility, and hardness.SOLUTION: The resin composition according to the present invention contains (A) an alkylated melamine resin, (B) a tri- or higher functional (meth)acrylate monomer, (C) a (meth)acrylate resin having a weight average molecular weight of 2,000 or more and 20,000 or less, and (D) a photopolymerization initiator having a molecular weight of 250 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition. The present invention also relates to a cured coating formed from the resin composition and a method for producing the same. [Background technology]

[0002] In the field of plastic film decoration, paint films with functionality such as scratch resistance and chemical resistance are integrated with resin through thermoforming to produce resin molded products with functional surfaces. The paint films used in this field must be compatible with thermoformability (heat stretchability) during thermoforming, hard coat properties such as scratch resistance, and chemical resistance. In particular, with the development of molding technology in recent years, more complex molding is now possible, so paint films are also required to have higher moldability.

[0003] Usually, the pre-cure method is the mainstream for thermoforming, which is performed using a fully cured coating film, but when higher formability is required, the after-cure method is effective, in which a coating film in an uncured or semi-cured state is used for thermoforming, and then the coating film is fully cured. However, the after-cure method poses major issues with the handleability of the uncured or semi-cured coating film (how unlikely it is that problems such as scratches on the surface or adhesion of dirt will occur when handling the film) and blocking resistance, and there are also issues with the hard coat properties of the coating film after it has fully cured, so it is necessary to achieve both of these performance properties.

[0004] So far, Patent Document 1 has proposed a hard coat composition containing a specific (meth)acryloyl polymer and specific inorganic oxide nanoparticles, which can produce a hard coat layer having excellent scratch resistance and high hardness when cured and also has excellent moldability during processing. Patent Document 2 has proposed a radiation curable composition for dual cure applications, which contains a hydroxy-functional urethane (meth)acrylate compound (A) that is a reaction product of a specific hydroxy-functional (meth)acrylate compound (A1) with a diisocyanate-functional compound (A3) and an optional compound (A2) that contains two hydroxyl groups and is different from compound (A1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2020 / 031967 [Patent Document 2] Special Publication No. 2021-524523 Summary of the Invention [Problem to be solved by the invention]

[0006] However, there is room for improvement in blocking resistance in the curable compositions described in Patent Documents 1 and 2. Furthermore, when the cured coating is used as a surface protective layer, properties such as transparency and hardness are also required.

[0007] Therefore, an object of the present invention is to provide a resin composition capable of forming a cured coating film that is excellent in handleability, transparency, blocking resistance, heat extensibility, and hardness. [Means for solving the problem]

[0008] In order to solve the above problems, the present inventors have conducted extensive research and found that by using a dual-cure type resin composition that uses a specific thermosetting component and a specific photocuring component in combination, it is possible to achieve both the handleability and blocking resistance of a coating film in a semi-cured state by thermosetting, and the hard coat properties of a coating film in a completely cured state by subsequent photocuring. Specifically, it was found that the above effects can be obtained by blending (A) an alkylated melamine resin, (B) a trifunctional or higher (meth)acrylate monomer, (C) a (meth)acrylate resin having a weight average molecular weight of 2,000 to 20,000, and (D) a photopolymerization initiator having a molecular weight of 250 or more in a resin composition. The present invention has been completed based on these findings.

[0009] That is, according to the present invention, the following inventions are provided. [1] A resin composition comprising: (A) an alkylated melamine resin; (B) a tri- or higher functional (meth)acrylate monomer; (C) a (meth)acrylate resin having a weight average molecular weight of 2,000 or more and 20,000 or less; and (D) a photopolymerization initiator having a molecular weight of 250 or more. [2] The resin composition according to [1], wherein the component (B) is a tri- or higher functional (meth)acrylate monomer having a hydroxyl group. [3] The resin composition according to [1] or [2], wherein a mass ratio of the component (A) to the sum of the components (B) and (C) (component (A):(component (B)+component (C))) is 8.0:2.0 to 3.0:7.0 in terms of solid content. [4] The resin composition according to any one of [1] to [3], further comprising (E) a curing accelerator. [5] The resin composition according to any one of [1] to [4], which is a heat-curable or photo-curable coating material. [6] A cured coating formed from the resin composition according to any one of [1] to [5]. [7] A substrate with a cured coating comprising a substrate and the cured coating according to [6] provided on the substrate. [8] A first curing step of thermally curing the resin composition according to any one of [1] to [5] to form a semi-cured coating; a second curing step of photocuring the semi-cured coating to form a completely cured coating; A method for producing a cured coating comprising the steps of: Effect of the Invention

[0010] According to the present invention, it is possible to provide a resin composition capable of forming a cured coating film having excellent handleability, transparency, blocking resistance, thermal elongation property, and hardness. In addition, according to the present invention, it is also possible to provide a cured coating film formed from such a resin composition and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Resin composition> The resin composition according to the present invention contains at least the following components (A), (B), (C), and (D), and may further contain a component (E) and a solvent. The cured coating film formed from the resin composition according to the present invention is excellent in handleability, transparency, blocking resistance, heat elongation, and hardness. The resin composition according to the present invention contains both a thermosetting component and a photocuring component, and therefore can be suitably used as a thermosetting and photocuring coating material.

[0012] In this specification, "(meth)acrylate" refers to acrylate and methacrylate, "(meth)acryloyl group" refers to acryloyl group and methacryloyl group, and "(meth)acrylate resin" refers to acrylate resin and methacrylate resin. "Solid content" refers to the resin composition excluding volatile components such as organic solvent, and indicates the components that constitute the cured coating when cured. Each component that constitutes the resin composition will be described below.

[0013] (Component (A)) Component (A) is an alkylated melamine resin, which is obtained by reacting melamine with formaldehyde to replace some or all of the hydrogen atoms in the amino groups with methylol groups to produce methylol melamine, which is then reacted with an aliphatic alcohol to modify some or all of the methylol groups into alkoxymethyl groups, and then polycondensing the resulting product by heating.

[0014] The alkylated melamine resin is not particularly limited, and conventionally known ones can be used. The number of carbon atoms in the alkyl group of the alkylated melamine resin is preferably 1 to 10, more preferably 1 to 5. The alkyl group may be linear or branched. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a hexyl group, a heptyl group, and an octyl group. The alkylated melamine resin may be used alone or in combination of two or more kinds.

[0015] The content of component (A) is preferably 20% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 75% by mass or less, and even more preferably 35% by mass or more and 75% by mass or less, based on the solid content of the resin composition. If the content of component (A) is within the above range, the handling property and blocking resistance of the coating in a semi-cured state can be improved.

[0016] ((B) component) The component (B) is a tri- or higher functional (meth)acrylate monomer. A tri- or higher functional (meth)acrylate monomer is a monomer having three or more (meth)acryloyl groups as functional groups in the molecule.

[0017] As the trifunctional or higher (meth)acrylate monomer, it is preferable to use a poly(meth)acrylate of a trivalent or higher aliphatic polyol. For example, glycerin tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. may be used. The trifunctional or higher (meth)acrylate monomer may be used alone or in combination of two or more.

[0018] Among the trifunctional or higher polyfunctional (meth)acrylate monomers, it is preferable to use trifunctional or higher (meth)acrylate monomers having hydroxyl groups, such as pentaerythritol tri(meth)acrylate and dipentaerythritol penta(meth)acrylate. By using a trifunctional or higher (meth)acrylate monomer having hydroxyl groups, the hydroxyl groups in component (B) react with the melamine resin in component (A) by heating and cure, so that the hardness of the coating in the completely cured state can be further improved.

[0019] ((C) component) The component (C) is a (meth)acrylate resin having a specific weight average molecular weight. The weight average molecular weight of the (meth)acrylate resin is 2,000 or more and 20,000 or less, preferably 3,000 or more and 19,000 or less, more preferably 5,000 or more and 17,000 or less, and even more preferably 7,000 or more and 15,000 or less. If the weight average molecular weight of the (meth)acrylate resin is within the above numerical range, the blocking resistance of the coating film in a semi-cured state can be improved, and the hardness of the coating film in a completely cured state can be improved. In the present invention, the weight average molecular weight of the (meth)acrylate resin can be measured by a conventionally known gel permeation chromatography (GPC) method.

[0020] The (meth)acrylate resin is not particularly limited as long as it has the above weight average molecular weight. The (meth)acrylate resin is a homopolymer of a (meth)acrylate monomer, or a copolymer of a (meth)acrylate monomer and a monomer copolymerizable therewith. Examples of the (meth)acrylate resin include urethane (meth)acrylate resin, acrylic (meth)acrylate resin, polyester (meth)acrylate resin, polyether (meth)acrylate resin, and epoxy (meth)acrylate resin. Among these, urethane (meth)acrylate resin and acrylic (meth)acrylate resin are preferred from the viewpoint of being tack-free in a semi-cured state and being more likely to obtain blocking resistance of the coating.

[0021] The urethane (meth)acrylate resin is a resin having a urethane bond (-NHCOO-) in the molecule and a (meth)acryloyl group as a functional group in the molecule. The urethane (meth)acrylate resin is not particularly limited, but can be obtained, for example, by a urethane reaction between a polyisocyanate, a hydroxyl group-containing (meth)acrylate, and an optionally used polyol. In this reaction, an isocyanate group-containing urethane prepolymer may be synthesized from the polyisocyanate and the polyol, and a hydroxyl group-containing (meth)acrylate may be added thereto. Also, instead of or together with the polyisocyanate, an isocyanate group-containing (meth)acrylate, such as 2-(meth)acryloyloxyethyl isocyanate, may be used. Furthermore, any other copolymerizable (meth)acrylate, such as an alkyl (meth)acrylate such as methyl (meth)acrylate, may be used.

[0022] Examples of polyisocyanates include aliphatic or alicyclic polyisocyanates. Specific examples of the polyisocyanate include aliphatic diisocyanates such as hexamethylene diisocyanate and pentamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate, norbornane diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylylene diisocyanate, 1,3-bis(isocyanatomethyl)-cyclohexane and dicyclohexylmethane-4,4'-diisocyanate; biuret, isocyanurate or allophanate forms of these compounds; and compounds in which a portion of the isocyanate groups of these compounds are modified with alcohols such as trimethylolpropane, tricyclodecane dimethanol, 1,4-cyclohexane dimethanol, amides such as δ-lactams, imides such as phthalimide, carbodiimide, epoxides, etc.

[0023] Examples of hydroxy group-containing (meth)acrylates include hydroxyalkyl group-containing monofunctional (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 1,4-cyclohexanedimethanol mono(meth)acrylate; hydroxy group-containing polyfunctional (meth)acrylates such as glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate; and alkylene oxide modified or caprolactone modified versions of these.

[0024] Examples of polyols include aliphatic or alicyclic polyols such as 1,4-butanediol, 1,6-hexanediol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, glycerin, and hydrogenated bisphenol A.

[0025] The acrylic (meth)acrylate resin is a (meth)acrylic resin containing an acryloyl group. The acrylic (meth)acrylate resin is not particularly limited, but examples thereof include a resin obtained by adding acrylic acid to a (meth)acrylic resin copolymerized with glycidyl (meth)acrylate, a resin obtained by adding 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, pentaerythritol triacrylate, or the like to an acrylic resin copolymerized with 2-acryloyloxyethyl isocyanate, and a resin obtained by adding 2-acryloyloxyethyl isocyanate to a (meth)acrylic resin copolymerized with a hydroxyl group-containing monomer.

[0026] The polyester (meth)acrylate resin has an acryloyl group in the molecule, and examples thereof include a dehydration condensation product of a polyester polyol and (meth)acrylic acid. The polyether (meth)acrylate resin has an acryloyl group in the molecule, and examples thereof include a dehydration condensation product of a polyether polyol and (meth)acrylic acid. The epoxy (meth)acrylate resin has an acryloyl group in the molecule, and examples thereof include compounds in which (meth)acrylic acid is substituted for the epoxy group of an epoxy group-containing compound such as polyglycidyl ether.

[0027] The mass ratio of component (A) to the sum of components (B) and (C) (component (A):(component (B)+component (C))) is, calculated as solid content, preferably 8.0:2.0-3.0:7.0, more preferably 7.5:2.5-3.5:6.5, and even more preferably 7.0:3.0-4.0:6.0. When the mass ratio of component (A) to the sum of components (B) and (C) is within the above range, the handleability, blocking resistance, and heat extensibility of the coating in a semi-cured state can be improved, and the hardness of the coating in a completely cured state can be improved.

[0028] ((D) component) Component (D) is a photopolymerization initiator having a molecular weight of 250 or more. The lower limit of the molecular weight of the photopolymerization initiator is preferably 255 or more, more preferably 260 or more, and more preferably 270 or more, and the upper limit may be 500 or less, 450 or less, or 400 or less. If the molecular weight of the photopolymerization initiator is 250 or more, the photopolymerization initiator is less likely to volatilize even when heated (for example, at 130° C. or more) in the thermal curing step, and the hardness of the coating in a completely cured state can be improved.

[0029] As the photopolymerization initiator, a conventionally known photopolymerization initiator for UV curing can be used as long as it has the above-mentioned molecular weight. Examples of the photopolymerization initiator include an alkylphenone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, a thioxanthone-based polymerization initiator, and an oxime ester-based polymerization initiator.

[0030] Examples of the alkylphenone photopolymerization initiator include 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one (molecular weight: 340.4), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (molecular weight: 279.4), 2,2-dimethoxy-2-phenylacetophenone (molecular weight: 256.3), 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (molecular weight: 366.5), and 2-(dimethylamino)-2-(4-methylbenzyl)-1-[4-(morpholin-4-yl)phenyl]butan-1-one (molecular weight: 380.5). Examples of the acylphosphine oxide photopolymerization initiator include 2,4,6-trimethylbenzoyldiphenylphosphine oxide (molecular weight: 348.4) and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (molecular weight: 418.5). An example of the thioxanthone-based photopolymerization initiator is isopropylthioxanthone (molecular weight: 254.4). Examples of the oxime ester photopolymerization initiator include 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyloxime) (molecular weight: 445.6) and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone O-acetyloxime (molecular weight: 412.5).

[0031] The content of the (D) component is preferably 0.1% by mass or more and 15.0% by mass or less, more preferably 0.5% by mass or more and 10.0% by mass or less, and even more preferably 1.0% by mass or more and 7.0% by mass or less, based on the solid content of the resin composition. If the content of the (D) component is within the above numerical range, the curability of the resin composition is good.

[0032] ((E) component) The component (E) is a curing accelerator. The curing accelerator is not particularly limited, and may be any conventionally known acid catalyst used in thermal curing. For example, organic sulfonic acid compounds such as p-toluenesulfonic acid, dodecylbenzenesulfonic acid, camphorsulfonic acid, and the like, as well as amine neutralized products thereof, phosphoric acid compounds, and the like, may be used as the curing accelerator.

[0033] The content of the (E) component is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.2% by mass or more and 5.0% by mass or less, and even more preferably 0.3% by mass or more and 3.0% by mass or less, based on the solid content of the resin composition. If the content of the (E) component is within the above numerical range, the curability of the resin composition is good.

[0034] (Other Ingredients) The resin composition according to the present invention may contain other components in addition to the above components (A) to (E) within the scope of the present invention. As other components, antistatic agents, polymerization inhibitors, non-reactive diluents, matting agents, defoaming agents, dispersants, anti-settling agents, leveling agents, water and oil repellents, heat stabilizers, light stabilizers, adhesion improvers, photosensitizers, antibacterial agents, antifungal agents, antiviral agents, silane coupling agents, anti-scratch agents, etc. may be blended as necessary.

[0035] <Method for preparing resin composition> The resin composition according to the present invention can be obtained by mixing and stirring the above-mentioned components using a conventionally known device such as a mixer, disperser, stirrer, etc. Examples of such devices include a mixing and dispersion mill, a homodisper, a mortar mixer, a roll, a paint shaker, a homogenizer, etc.

[0036] In the present invention, the resin composition can be diluted with a solvent as necessary, for example, to adjust the viscosity of the resin composition to a level suitable for application. The solvent is not particularly limited as long as it dissolves the resin content in the resin composition. Specific examples include aromatic hydrocarbons (e.g., toluene, xylene, and ethylbenzene), esters or ether esters (e.g., ethyl acetate, butyl acetate, and methoxybutyl acetate), ethers (e.g., diethyl ether, tetrahydrofuran, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, monomethyl ether of propylene glycol, and monoethyl ether of diethylene glycol), ketones (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, di-n-butyl ketone, and cyclohexanone), alcohols (e.g., methanol, ethanol, n- or i-propanol, n-, i-, sec-, or t-butanol, 2-ethylhexyl alcohol, and benzyl alcohol), amides (e.g., dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc.), and sulfoxides (e.g., dimethyl sulfoxide). These solvents may be used alone or in combination of two or more.

[0037] <Cured film> When the cured coating formed from the resin composition according to the present invention has a thickness of 3.0 to 3.5 μm, the haze measured according to JIS K 7136:2000 is preferably 2% or less, more preferably 1.5% or less. When the cured coating has a thickness of 3.0 to 3.5 μm or less, the total light transmittance measured according to JIS K 7361-1:1997 is preferably 90% or more. When the haze and total light transmittance are within the above ranges, the cured coating has excellent transparency.

[0038] The cured coating formed from the resin composition according to the present invention preferably has an extensibility (elongation rate) of 30% or more, more preferably 40% or more, measured at a temperature of 150° C. in the case of a strip-shaped test piece having a thickness of 3.0 to 3.5 μm and a size of 15 mm×150 mm. If the numerical value of the elongation rate is within the above range, the cured coating has excellent extensibility when heated and can be suitably used as a coating film for thermoforming, particularly as a coating film for in-mold molding. The method for measuring the extensibility is the method described in the Examples below.

[0039] <Coated substrate> The coated substrate according to the present invention is provided with the above-mentioned cured coating on the substrate. The substrate is not particularly limited, and any conventionally known substrate can be used. For example, when the coated substrate is a coating film for in-mold molding, the substrate can be a thermoplastic resin film such as a polyester film, a polyolefin film, a nylon film, a polycarbonate film, or a polymethyl methacrylate film.

[0040] The coated substrate according to the present invention may further comprise other layers in applications requiring multiple layers. For example, the coated substrate according to the present invention may comprise other layers between the substrate and the cured coating, or may comprise other layers on the cured coating. Examples of other layers in the coated substrate according to the present invention include an intermediate layer, a primer layer, a protective layer, and the like. These other layers may be composed of only one layer, or may be composed of multiple layers.

[0041] The substrate with the coating according to the present invention can be produced by applying the above-mentioned resin composition onto the substrate and then curing the coating by the method (first step, second step) described in detail below. For application, for example, a coater such as a bar coater, a gravure coater, a roll coater (such as a natural roll coater or a reverse roll coater), an air knife coater, a spin coater, or a blade coater can be used. Among these, the application method using a gravure coater is preferred from the viewpoint of workability and productivity.

[0042] <Production method of cured film> The method for producing a cured coating according to the present invention includes a method for curing the above-mentioned resin composition in two steps: a first curing step (thermal curing step) and a second curing step (photocuring step). Each step will be described in detail below.

[0043] (First curing step) The first curing step is a step of thermally curing the resin composition to form a semi-cured coating. Examples of the thermal curing method include heat drying such as hot air drying (with a dryer, etc.). The heating temperature is preferably 100 to 200°C, more preferably 110 to 150°C. If the heating temperature is within the above numerical range, a sufficient thermosetting reaction can be obtained. The heating time is not particularly limited and can be appropriately adjusted depending on the thermosetting temperature, but is, for example, 3 to 5 minutes at 130°C and 1 to 2 minutes at 150°C.

[0044] (Second curing step) The second curing step is a step of photocuring the semi-cured coating obtained in the first curing step to form a completely cured coating. Examples of photocuring methods include irradiating the semi-cured coating with ultraviolet light using a high-pressure mercury lamp, metal halide lamp, xenon lamp, chemical lamp, UV-LED, or the like that emits light in the wavelength range of 200 to 500 nm. The amount of ultraviolet light irradiation is preferably 100 to 3,000 mJ / cm from the viewpoints of the curability of the resin composition and the flexibility of the cured product. 2 and more preferably 200 to 1,000 mJ / cm2 It is. EXAMPLES

[0045] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0046] <Preparation of Resin Composition> For the preparation of the resin composition, the following raw materials were prepared. Alkylated melamine resin 1: Methylated / butylated melamine resin, manufactured by Allnex Japan Co., Ltd., product name: Cymel 202 Alkylated melamine resin 2: Methylated melamine resin, manufactured by Allnex Japan Co., Ltd., product name: Cymel 701 Acrylic resin: DIC Corporation, product name: Acrydic WNL-379 Trifunctional or higher (meth)acrylate monomer 1: Dipentaerythritol penta / hexaacrylate (5 / 6 functional), manufactured by Toagosei Co., Ltd., product name: ARONIX M400 Trifunctional or higher (meth)acrylate monomer 2: Pentaerythritol triacrylate (trifunctional), manufactured by Daicel Allnex Corporation, product name: PETIA Bifunctional (meth)acrylate monomer: Tripropylene glycol diacrylate (bifunctional), manufactured by Miwon Co., Ltd., product name: MIRAMER M220 (Meth)acrylate resin 1: Urethane acrylate (Mw: 8,000), manufactured by Negami Chemical Industries, Ltd., product name: Art Resin UN-952 (Meth)acrylate resin 2: Acrylic acrylate (Mw: 13,000), manufactured by Daicel Allnex Corporation, product name: IRR742 Radical curing acrylic polymer: Radical curing acrylic polymer (Mw: 22,000), manufactured by Daicel Allnex Corporation, product name: Cyclomer P (ACA) Z250 Photopolymerization initiator 1: alkylphenone-based photopolymerization initiator, molecular weight: 340.4, manufactured by IGM Resins, product name: Omnirad 127 Photopolymerization initiator 2: alkylphenone-based photopolymerization initiator, molecular weight: 279.4, manufactured by IGM Resins, product name: Omnirad 907 Photopolymerization initiator 3: alkylphenone-based photopolymerization initiator, molecular weight: 164.2, manufactured by IGM Resins, product name: Omnirad 1173 Hardening accelerator: Phosphate compound, manufactured by Allnex Japan Co., Ltd., Cycat 296-9 Solvent: Propylene glycol monomethyl ether (PGM)

[0047] [Example 1] A resin composition was prepared according to the formulation shown in Table 1. Specifically, 34.3 parts by mass of alkylated melamine resin 1 as component (A), 5.1 parts by mass of trifunctional or higher (meth)acrylate monomer 1 as component (B), 9.4 parts by mass of (meth)acrylate resin 1 as component (C), 1.0 part by mass of photopolymerization initiator 1 as component (D), and 1.1 parts by mass of curing accelerator as component (E) were added to 49.1 parts by mass of solvent, stirred, and dissolved to obtain a resin composition with a solid content of 40%.

[0048] [Examples 2 to 10, Comparative Examples 1 to 7] A resin composition was obtained in the same manner as in Example 1, except that the composition was changed according to the formulations shown in Tables 1 and 2.

[0049] <Preparation of Semi-cured Film-Coated Substrate> The resin composition prepared above was applied once to a PET film (manufactured by Toyobo Co., Ltd., product name: Cosmoshine A4360, thickness 100 μm) using a bar coater so that the dry film thickness was approximately 3 μm, and then dried for 3 minutes in a hot air dryer at 130°C to obtain a substrate with a semi-cured coating.

[0050] <Preparation of substrate with fully cured coating> The substrate with the semi-cured coating obtained above was further irradiated with ultraviolet light from a high-pressure mercury lamp (irradiation dose: 300 mJ / cm 2 ) to obtain a substrate with a completely cured coating.

[0051] <Performance evaluation> (Condition of hardened coating) The appearance of the substrate with the semi-cured coating obtained above was evaluated visually and by touch according to the following criteria. The evaluation results are shown in Tables 1 and 2. If it was rated as "good," the handleability was evaluated as excellent. (Evaluation Criteria) ◯: The surface of the cured coating was sticky and free of dirt adhesion or other abnormalities. ×: The surface of the cured coating was sticky and had dirt adhering thereto, and other abnormalities were observed.

[0052] (transparency) For the substrate with the semi-cured coating produced above, the haze was measured in accordance with JIS K7136:2000 using a haze meter (NDH4000, manufactured by Nippon Denshoku Industries Co., Ltd.), and the total light transmittance was measured in accordance with JIS K7361-1:1997. The measurement results are shown in Tables 1 and 2. If the haze was 2.0% or less and the total light transmittance was 90.0% or more, the transparency was evaluated to be excellent.

[0053] (Blocking resistance) Two test pieces measuring 10 cm x 10 cm were prepared from the semi-cured coated substrate prepared above. The coated surfaces of the test pieces were then attached together and placed in a hot air dryer at 50°C for 24 hours under a load of 10 kg. The test pieces were then removed and peeled off to check their condition, and evaluated according to the following criteria. The evaluation results are shown in Tables 1 and 2. If the evaluation result was "◎" or "◯", the blocking resistance was evaluated as excellent. (Evaluation Criteria) ◎: There was absolutely no trace of the painted surfaces sticking to each other. ◯: Traces of adhesion between the painted surfaces were less than 10% of the area of ​​the bonded surfaces. ×: Traces of adhesion between the painted surfaces were 10% or more of the area of ​​the adhesion.

[0054] (Heating extensibility) A rectangular test piece measuring 15 mm x 150 mm was prepared from the semi-cured coated substrate prepared above. The test piece was then pulled using a thermostatic tensile tester (Shimadzu Corporation, AG-X plus) at a temperature of 150°C, a chuck distance of 100 mm, and a pulling speed of 10 mm / min, and the elongation rate (%) until the coating cracked was measured visually. The measurement results are shown in Tables 1 and 2. A test piece with an elongation rate of 30% or more was evaluated as having excellent heat elongation.

[0055] (Pencil hardness) The hardness of the substrate with the fully cured coating prepared above was measured using a pencil scratch tester (Yasuda Manufacturing Co., Ltd., No. 553-M) in accordance with JIS K5600-5-4:1999. Specifically, a pencil was set on the coating at a 45 degree angle, and a load of 750g was applied to scratch the coating for 5 cm, and the hardness of the pencil that did not leave a scratch was used for evaluation. The evaluation results are shown in Tables 1 and 2. If the pencil hardness was F or higher (F, H, 2H, etc.), the hardness was evaluated as excellent.

[0056] [Table 1]

[0057] [Table 2]

Claims

1. A resin composition comprising: (A) an alkylated melamine resin; (B) a tri- or higher functional (meth)acrylate monomer; (C) a (meth)acrylate resin having a weight average molecular weight of 2,000 or more and 20,000 or less; and (D) a photopolymerization initiator having a molecular weight of 250 or more.

2. The resin composition according to claim 1 , wherein the component (B) is a tri- or higher functional (meth)acrylate monomer having a hydroxyl group.

3. The resin composition according to claim 1, wherein the mass ratio of the component (A) to the total of the components (B) and (C) (component (A):(component (B)+component (C))) is 8.0:2.0 to 3.0:7.0 in terms of solid content.

4. The resin composition according to claim 1 , further comprising (E) a curing accelerator.

5. The resin composition according to claim 1, which is a heat-curable and photo-curable coating material.

6. A cured coating formed from the resin composition according to any one of claims 1 to 5.

7. A substrate with a cured coating comprising a substrate and the cured coating according to claim 6 provided on the substrate.

8. A first curing step of thermally curing the resin composition according to any one of claims 1 to 5 to form a semi-cured coating; a second curing step of photocuring the semi-cured coating to form a completely cured coating; A method for producing a cured coating comprising the steps of:

Citation Information

Patent Citations

  • Radiation-hardening components

    JP2021524523A

  • Hard-coat composition, laminate film, and curable film

    WO2020031967A1

Cited By

  • Magnetic film, magnetoresistive effect element, and method for manufacturing magnetic film

    US12433173B2