Plasma Etching Technology

JP2024506618A5Active Publication Date: 2024-11-01TOKYO ELECTRON LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023547796
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-02-09
Filing Date
2022-02-02
Publication Date
2024-11-01
Estimated Expiration
2042-02-02

AI Technical Summary

Technical Problem

Conventional etching techniques struggle to selectively etch germanium-containing layers in semiconductor substrates with minimal etching of silicon layers, particularly in 3D vertical structures like nanowires or gate-all-around devices, due to similar chemical reactivity and the presence of native oxide layers, leading to poor selectivity and undesirable etching of silicon.

Method used

A plasma etching process using a mixture of fluorine, hydrogen, and nitrogen agents forms a nitride passivation layer on silicon surfaces, preventing etching while selectively removing germanium-containing layers, even at low germanium concentrations, by generating a plasma from gases like NF3, H2, and noble gases, maintaining low pressure and controlled conditions.

Benefits of technology

The process achieves a selectivity ratio of up to 100:1 in etching germanium to silicon, ensuring sharp etch profiles and reduced surface roughness, suitable for forming nanowires in advanced semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

In one particular embodiment, a method of processing a semiconductor substrate includes receiving a semiconductor substrate including a thin film stack. The thin film stack includes a first silicon layer, a second silicon layer, and a first germanium-containing layer disposed between the first silicon layer and the second silicon layer. The method further includes selectively etching the first germanium-containing layer by exposing the thin film stack to a plasma including a fluorine agent, a nitrogen agent, and a hydrogen agent. The plasma etches the first germanium-containing layer and forms a passivation layer on exposed surfaces of the first silicon layer and the second silicon layer to prevent etching of the first silicon layer and the second silicon layer while the thin film stack is exposed to the plasma.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Patent Application No. 17 / 171,742, filed February 9, 2021, which is incorporated by reference in its entirety.

[0002] The present disclosure relates generally to semiconductor manufacturing and, in a particular embodiment, to plasma etching techniques. [Background technology]

[0003] The integrated circuit (IC) manufacturing industry strives to increase device density to improve speed, performance, and cost. Due to the continuous scaling to smaller node sizes, device architectures have evolved from two-dimensional (2D) planar structures to three-dimensional (3D) vertical structures such as nanowires or vertically oriented transistors. The desire for this change is driven by poor control of the conduction channel by the gate potential. As gate dimensions shrink, short channel effects (SCEs) can become very significant and can increase current conduction when no voltage is applied to the gate (I off ). Changes in device architecture may allow better electrostatic control of the gate, reducing SCE and power losses. Fabricating nanowire devices may present 3D etch challenges where highly selective isotropic etch processes are beneficial. For example, exposed layers of material may need to be etched relative to each other to form recesses in the thin film stack. Summary of the Invention [Means for solving the problem]

[0004] In a particular embodiment, a method of processing a semiconductor substrate includes receiving a semiconductor substrate including a thin film stack. The thin film stack includes a first silicon layer, a second silicon layer, and a first germanium-containing layer disposed between the first silicon layer and the second silicon layer. The method further includes selectively etching the first germanium-containing layer by exposing the thin film stack to a plasma including a fluorine agent, a nitrogen agent, and a hydrogen agent. The plasma etches the first germanium-containing layer and forms a passivation layer on exposed surfaces of the first silicon layer and the second silicon layer to prevent etching of the first silicon layer and the second silicon layer while the thin film stack is exposed to the plasma.

[0005] In a particular embodiment, a method for processing a semiconductor substrate includes placing the semiconductor substrate in a plasma chamber of a plasma tool. The semiconductor substrate includes a thin film stack having silicon and germanium-containing layers, the thin film stack having at least two silicon layers and at least two germanium-containing layers in an alternating stacked arrangement. The method further includes generating a plasma in the plasma chamber of the plasma tool, the plasma including a fluorine agent, a nitrogen agent, and a hydrogen agent. The plasma is generated from a gas including a fluorine-containing gas, a nitrogen-containing gas, a hydrogen-containing gas, and a noble gas. The method further includes exposing the thin film stack to the plasma in the plasma chamber of the plasma tool. The plasma forms a nitride passivation layer on an exposed surface of the silicon layer and selectively etches an opposite exposed edge of the germanium-containing layer to form a recess in the germanium-containing layer relative to the opposite exposed edge of the silicon layer. The nitride passivation layer prevents the plasma from etching the silicon layer.

[0006] In a particular embodiment, a method of processing a semiconductor substrate includes placing the semiconductor substrate in a plasma chamber of a plasma tool. The semiconductor substrate includes a thin film stack having an alternating arrangement of first layers of a first material and second layers of a second material. The first material is a germanium-containing material having a germanium concentration of about 10 to about 50 percent. The method further includes generating a plasma to selectively etch the first layer of the first material. Generating the plasma includes introducing a gas containing fluorine, nitrogen, hydrogen, and a noble gas into the plasma chamber and maintaining a pressure in the plasma chamber below about 50 millitorr. The method further includes exposing the thin film stack to the plasma in the plasma chamber for a period of time. The plasma selectively etches an opposite exposed edge of the first layer of the first material relative to an opposite exposed edge of the second layer of the second material to form a recess in the first layer of the first material.

[0007] For a more complete understanding of the present disclosure and its advantages, reference is made to the following descriptions taken in conjunction with the accompanying drawings, in which: [Brief description of the drawings]

[0008] [Figure 1A] 1A-1D illustrate cross-sectional views of an exemplary semiconductor substrate during an exemplary process for processing the semiconductor substrate in accordance with certain embodiments of the present disclosure. [Figure 1B] 1A-1D illustrate cross-sectional views of an exemplary semiconductor substrate during an exemplary process for processing the semiconductor substrate in accordance with certain embodiments of the present disclosure. [Figure 1C] 1A-1D illustrate cross-sectional views of an exemplary semiconductor substrate during an exemplary process for processing the semiconductor substrate in accordance with certain embodiments of the present disclosure. [Figure 1D] 1A-1D illustrate cross-sectional views of an exemplary semiconductor substrate during an exemplary process for processing the semiconductor substrate in accordance with certain embodiments of the present disclosure. [Diagram 2] 1 illustrates an exemplary method for processing a semiconductor substrate according to certain embodiments of the present disclosure. [Diagram 3] 1 illustrates an exemplary method for processing a semiconductor substrate according to certain embodiments of the present disclosure. [Figure 4] 1 illustrates an exemplary device including a substrate having a concave alternating thin film stack in accordance with certain embodiments of the present disclosure. [Diagram 5] FIG. 1 illustrates a block diagram of an exemplary plasma tool, in accordance with certain embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] There are various techniques for attempting to selectively etch one material relative to another. In some cases, the chemical properties of the two materials are sufficiently different that a plasma that selectively etches one material can be used without concern for etching the other. In other cases, it is more difficult to determine the appropriate etching area for a selective etch because the chemical properties of the materials may be similar or the available etching processes may be limited by other factors. Certain materials, where it is desirable to etch one material with little or no etching of another material, present a difficult challenge in terms of selectivity. Conventional processes for this type of selective etch may not be able to achieve selective etching of one material relative to another or may fall short of process requirements such as selectivity, etch profile (e.g., local uniformity and / or surface roughness), etc.

[0010] Selectivity challenges may arise in forming nanowires or nanosheets that function as channel regions in 3D vertical structures of semiconductor devices such as gate-all-around (GAA) devices. Formation of such nanowires may involve forming a thin film stack on a base layer, the thin film stack including layers of Si and Ge or Si-Ge (SiGe) alloys arranged in alternating stacks. Part of this process may include etching a recess in the thin film stack at the opposite end of the Ge or Ge-containing layer while minimizing etching of the silicon (Si) layer to expose the end of the Si layer for subsequent use as a conductive device. Conventional etching techniques may be unsatisfactory due to various challenges including, in part, native oxide layers (NOLs) and / or other residues (e.g., reactive ion etching (RIE) residues) present on the surface of the thin film stack.

[0011] Etching a Ge-containing layer while minimizing etching of a Si layer can be a challenge, especially when the Ge-containing layer contains a relatively low concentration of Ge, e.g., about 30% Ge or less, and in certain embodiments, about 15% Ge or less. This challenge may be due, at least in part, to the chemical composition of the Ge-containing layer (e.g., a SiGe layer) and to the fact that a Si layer becomes more similar when a Ge-containing layer having a low concentration of Ge is used.

[0012] Prior to performing plasma etching to form recesses in the thin film stack, some prior art techniques remove NOL using wet or dry processes. The thin film stack can be treated using dilute hydrofluoric (HF) acid or using a chemical oxide removal process involving the formation of ammonium silicofluoride. However, removing NOL on the surfaces of both the Si and Ge-containing layers can reduce the selectivity of a subsequent recess plasma etch process (e.g., using a conventional fluorine-based etch process, as described below) to etch the Ge-containing layer with minimal or no etching of the Si layer.

[0013] Some conventional techniques expose the surfaces of both the Si layer and the Ge-containing layer (e.g., along the sidewalls of the thin film stack) to fluorine-containing chemicals (e.g., fluorine (F2), chlorine trifluoride (ClF3), bromine trifluoride (BrF3), or iodine pentafluoride (IF5)) or to fluorine-containing radicals generated by a plasma. Such conventional plasmas can be generated from a gas containing carbon tetrafluoride (CF4) and argon (Ar), or from a gas containing nitrogen trifluoride (NF3) and nitrogen (N2). The fluorine-containing etchant (whether in the fluorine-containing chemical or in the fluorine radicals in the plasma) can react more rapidly with the Ge-containing layer than with the Si layer, thereby achieving a level of selectivity to Si (etching the Ge-containing layer more rapidly than the Si layer). Although the Si layer is less reactive to the fluorine-containing etchants associated with these conventional techniques, an undesirable amount of etching of the Si layer still occurs. For example, if etching of the Si layer occurs at a corner of the Si layer, the etching of the Si layer may result in rounding of the corner. In addition, if the concentration of Ge in the Ge-containing layer is relatively low (e.g., ≦about 30%, and in certain embodiments, ≦about 15%), the difference in reactivity of the Si layer and the Ge-containing layer with respect to a fluorine-containing etchant may be significantly reduced, which may result in poor selectivity (e.g., in certain embodiments, less than about 20:1 (etch rate of Ge-containing layer to etch rate of Si layer) for 15% Ge).

[0014] The embodiments described below provide various techniques for selective etching. For example, embodiments can be used to selectively etch a portion of a thin film stack (e.g., including alternating Si and Ge-containing layers) of a substrate. It may be desirable to selectively etch (or in some cases completely remove) a recess at the edge of the Ge-containing layer to form a contact handle for the Si nanowire layer, and even a low concentration of Ge in the Ge-containing layer (e.g., less than about 50% Ge, less than about 30% Ge, less than about 25% Ge, and in certain embodiments, less than about 15% Ge) can improve selectivity to the Si layer.

[0015] In a particular embodiment, a plasma is used to form recessed regions or recesses in a thin film stack including alternating Si and Ge-containing layers. The plasma may be generated from a gas including a fluorine-containing gas, a hydrogen-containing gas, and a carrier gas (e.g., noble gases such as Ar and He), and the plasma may include a fluorine agent, a hydrogen agent, and a nitrogen agent. The plasma may form a passivation layer (e.g., a nitride passivation layer such as a Si-nitride passivation layer) on the exposed surface of the Si layer, which may act as an etch stop layer on the exposed surface of the Si layer while the etchant (e.g., a fluorine agent) in the plasma etches the Ge-containing layer. Prior to exposing the substrate to the plasma, a barrier layer (e.g., NOL) may be substantially removed from the exposed surface of the thin film stack using a suitable dry or wet etching process.

[0016] 1A-1D show cross-sectional views of an exemplary substrate 102 during an exemplary process 100 for processing the substrate 102, according to an embodiment of the present disclosure. In a particular embodiment, the process 100 includes using a suitable plasma to etch portions of a particular layer (e.g., a Ge-containing layer) of the thin film stack of the substrate 102 while forming a protective passivation layer on exposed portions of other layers (e.g., a Si layer) of the thin film stack, resulting in a substrate 102 having a recessed thin film stack after performing the process 100.

[0017] As shown in FIG. 1A, the substrate 102 is a semiconductor substrate including a thin film stack 104 disposed on a base layer 106. The thin film stack 104 includes Ge-containing layers 108 and Si layers 110 in an alternating stacked configuration. The thin film stack 104 may have any suitable shape and may include any suitable number of layers. By way of example, the vertical thickness of each of the Ge-containing layers 108 and Si layers 110 may be between about 5 nm and about 25 nm, and as a specific example, may be about 10 nm or about 20 nm. In addition, the Ge-containing layers 108 may have the same thickness or may vary in thickness from one another, the Si layers 110 may have the same thickness or may vary in thickness from one another, and the Ge-containing layers 108 and Si layers 110 may have the same thickness or may vary in thickness from one another. In a specific example, the Ge-containing layers 108 and Si layers 110 all have substantially the same thickness.

[0018] For example, the material of the Ge-containing layer 108 may be high purity Ge or a SiGe alloy. As a particular example, the Ge-containing layer 108 may be formed by mixing a SiGe alloy (mixture) in an appropriate ratio (e.g., SiGe alloy) for the desired etching characteristics for a given application, or for the desired performance in the resulting semiconductor device formed in part using the process 100. 0.7 Ge 0.3 , Si 0.85 Ge 0.15 The Ge-containing layer 108 may include any suitable concentration of Ge relative to another material (e.g., Si), including 100% Ge. While the present disclosure contemplates Ge-containing layer 108 including any suitable concentration of Ge relative to another material (e.g., Si), in certain embodiments, the Ge-containing layer 108 includes about 50% Ge or less, about 30% Ge or less, about 25% Ge or less, about 15% Ge or less, or about 10% Ge or less. As just one particular exemplary range, the Ge-containing layer 108 may include about 10% to about 50% Ge relative to one or more other materials (e.g., Si). In certain embodiments, all of the Ge-containing layers 108 include the same material, although the Ge-containing layers 108 may include different materials if desired.

[0019] For example, the material of the Si layers 110 may be high purity Si. In certain embodiments, all of the Si layers 110 include the same material, but the Si layers 110 may include different materials if desired. Although in this particular example, the Si layers 110 are described as being primarily high purity Si, it should be understood that in certain embodiments, the material that is selective when etching a Ge-containing layer (e.g., the Ge-containing layer 108) may include another suitable material, such as Si-nitride (SiN).

[0020] The base layer 106 may be any suitable material, and in one embodiment is or includes Si. In a particular embodiment, the thin film stack 104 is formed by growing alternating heteroepitaxial layers of Ge or SiGe (e.g., Ge-containing layer 108) and Si (e.g., Si layer 110) on the base layer 106.

[0021] An optional hard mask 112 may be included on top of the thin film stack 104. The hard mask 112 may have been used, for example, in a previous etching process to define the structure of the thin film stack 104. In a particular embodiment, the hard mask 112 is SiN (e.g., Si-nitride (Si3N4)), but may comprise any suitable material.

[0022] A barrier layer 114 is formed on the thin film stack 104 (including the hard mask 112) and, in this embodiment, on the base layer 106. The barrier layer 114 may result from a previous fabrication step (e.g., RIE) applied to the substrate 102 or from other handling of the substrate 102 (e.g., exposure to ambient air when transferred between processing tools). As a particular embodiment, the barrier layer 114 may include NOL, RIE residue, or both. The NOL may be a thin layer of SiO2 (or other suitable material), e.g., about 1.0 nm to about 2.0 nm thick, formed on the surface of the substrate 102, such as when the substrate 102 is exposed to ambient air containing O2 and H2O. For example, the surfaces of the base layer 106, the Ge-containing layer 108, the Si layer 110, and the hard mask 112 may interact with the ambient air, resulting in the formation of the barrier layer 114 on those surfaces. As another example, the surfaces of the base layer 106, the Ge-containing layer 108, the Si layer 110, and the hard mask 112 may contain residues from a previous RIE step.

[0023] The barrier layer 114 may have different etch characteristics than the layers below the barrier layer 114. Although the barrier layer 114 is shown as having generally uniform coverage over the thin film stack 104 (including the hard mask 112) and the base layer 106, the barrier layer 114 may or may not have uniform coverage.

[0024] Each layer of the thin film stack 104 has a pair of exposed surfaces at opposite ends when viewed from a cross-sectional view as shown: each of the Ge-containing layers 108 has an (opposite) exposed surface 116, and each of the Si layers 110 has an (opposite) exposed surface 118. In addition, in the state shown in FIG. 1A, the substrate 102 includes a barrier layer 114, so that the exposed surface 116 of the Ge-containing layer 108 and the exposed surface 118 of the Si layer 110 include the barrier layer 114.

[0025] As shown in FIG. 1B, the barrier layer 114 is etched to remove some or all of the barrier layer 114 from the exposed surface 116 of the Ge-containing layer 108, from the exposed surface 118 of the Si layer 110, and from the exposed surfaces of the base layer 106 and the hard mask 112. The barrier layer 114 may be removed using any suitable process, including any suitable wet or dry etching process. In a particular embodiment, the substrate 102 is treated to remove some or all of the barrier layer 114 using dilute HF acid or a chemical oxide removal process. The process used to etch the barrier layer 114 may or may not remove some or all of the hard mask 112, but for purposes of this example, the hard mask 112 is shown not to be removed or etched. However, removing the barrier layer 114 from the exposed surface 116 of the Ge-containing layer 108 and from the exposed surface 118 of the Si layer 110 may reduce the selectivity of a subsequent conventional fluorine-based recess plasma etch process to etch the Ge-containing layer 108 with minimal or no etching of the Si layer 110.

[0026] 1C, in a plasma step 120 of the process 100, the substrate 102 is exposed to a plasma 122 to selectively etch the Ge-containing layer 108. For example, the substrate 102 may be exposed to the plasma 122 to selectively etch the exposed surface 116 of the Ge-containing layer 108 with an intermediate state in which an opposite edge of the Ge-containing layer 108 has been removed / etched relative to the adjacent Si layer 110 to form a recess 136 in the thin film stack 104. In certain embodiments, the plasma step 120 is an isotropic etching process.

[0027] The plasma step 120 may be performed in a plasma chamber 123 of a plasma tool. The plasma tool may be any type of suitable plasma tool, including an inductively coupled plasma (ICP) tool, a capacitively coupled plasma (CCP) tool, or a surface wave plasma (SWP) tool. One exemplary plasma tool is described below with reference to FIG.

[0028] While the substrate 102 is exposed to the plasma 122, the plasma 122 may form a passivation layer 124 on the exposed surface 118 of the Si layer 110 to facilitate selective etching of the Ge-containing layer 108. The plasma 122 may form a passivation layer 124 on the exposed surface 118 of the Si layer 110 by removing, replacing or modifying a portion of the Si layer 110 at the exposed surface 118 of the Si layer 110. In certain embodiments, the passivation layer 124 may also be formed on the exposed surface of the base layer 106, such as when the base layer 106 is high purity Si or Si nitride.

[0029] During exposure of the substrate 102 to the plasma 122, the passivation layer 124 on the exposed surface 118 of the Si layer 110 (and, in the illustrated embodiment, on the exposed surface of the base layer 106) prevents etching of the Si layer 110 (and, in the illustrated embodiment, on the base layer 106). In other words, due at least in part to the formation and presence of the passivation layer 124 on the exposed surface 118 of the Si layer 110 (and on the exposed surface of the base layer 106), the plasma 122 selectively etches the Ge-containing layer 108, with the passivation layer 124 acting as an etch stop layer on the exposed surface 118 of the Si layer 110 (and on the exposed surface of the base layer 106). In certain embodiments, the passivation layer 124 that inhibits etching of the Si layer 110 (and, in the illustrated example, of the base layer 106) includes a passivation layer 124 that prevents etching of some or all of the Si layer 110, a passivation layer 124 that reduces etching of some or all of the Si layer 110, a passivation layer 124 that slows etching of some or all of the Si layer 110, etc.

[0030] While the passivation layer 124 may have any suitable thickness, in certain embodiments, the passivation layer 124 is relatively thin, e.g., 2 nm or less. The passivation layer 124 may be, for example, a monolayer. In certain embodiments, the passivation layer 124 is a nitride, e.g., a Si-nitride (e.g., Si3N4).

[0031] As the plasma 122 etches the Ge-containing layer 108, an additional surface 138 of the Si layer 110 is exposed. That is, as a recess 136 or depression is formed in the thin film stack 104 due to the selective etching of the Ge-containing layer 108, an additional surface 138 of the Si layer 110 is exposed. The plasma 122 can continue to form a passivation layer 124 on the additional surface 138. The passivation layer 124 formed on the additional surface 138 may also be a nitride, such as a Si-nitride (e.g., Si3N4). In other words, as the Ge-containing layer 108 is etched above, below, and / or between the Si layers 110, a passivation layer 124 is further formed on the newly exposed surface (e.g., the additional surface 138) of the Si layer 110. The passivation layer 124 on the additional surface 138 prevents etching of the Si layer 110 at the additional surface 138 , while the passivation layer 124 at the exposed surface 118 of the Si layer 110 prevents etching of the Si layer 110 at the exposed surface 118 .

[0032] The plasma 122 may include a fluorine agent 126, a hydrogen agent 128, and a nitrogen agent 130. The fluorine agent 126 may function primarily as an etchant to etch the Ge-containing layer 108 at the exposed surface 116 of the Ge-containing layer 108. The hydrogen agent 128 may function as a reducing agent and, in the presence of the fluorine agent 126, facilitate the etching of the Ge-containing layer 108 at the exposed surface 116 of the Ge-containing layer 108. Furthermore, depending on the gas used to generate the plasma 122, if applicable, the hydrogen agent 128 may further decompose certain compounds of fluorine and nitrogen to form the fluorine agent 126 and the nitrogen agent 130, which may facilitate the formation of a passivation layer 124 (e.g., a nitride such as Si-nitride) on the surface 118 of the Si layer 110 and / or the etching of the Ge-containing layer 108. The nitrogen agent 130 reacts with Si at the exposed surface 118 of the Si layer 110 to form a nitride layer (e.g., a Si nitride layer such as Si3N4) at the exposed surface 118. For example, atomic nitrogen (N) generated in the plasma 122 can react with Si molecules at the exposed surface 118 of the Si layer 110 (and the exposed surface of the base layer 106) to form a passivation layer 124 (e.g., a nitride layer) on the exposed surface 118 of the Si layer 110 (and the exposed surface of the base layer 106).

[0033] While the fluorine agent 126, the hydrogen agent 128, and the nitrogen agent 130 have been primarily shown and described as separate elements, the present disclosure contemplates that the fluorine agent 126, the hydrogen agent 128, and the nitrogen agent 130 are separate, or that some or all of the fluorine agent 126, the hydrogen agent 128, and the nitrogen agent 130 are part of one or more compounds in the plasma 122. For example, the plasma 122 may include one or more of an NH species, an HF species, an NF species, or other suitable species. It will be understood that throughout the present disclosure, references to the fluorine agent 126, the hydrogen agent 128, and the nitrogen agent 130 contemplate both these agents as separate elements and these agents as part of one or more compounds in the plasma 122.

[0034] In certain embodiments, the plasma 122 may be generated from gases including a fluorine-containing gas, a hydrogen-containing gas, a nitrogen-containing gas, and a noble gas. The fluorine-containing gas may function as an etchant, the hydrogen-containing gas may function as a reducing gas, and the noble gas may function as a carrier gas. As some examples, the fluorine-containing gas used to generate the plasma 122 may include NF3, sulfur hexafluoride (SF6), or carbon tetrafluoride (CF4). In certain embodiments, such as some examples where a fluorine-containing gas that does not include nitrogen is used (or even some examples where a fluorine-containing gas that includes nitrogen is used), it may be appropriate to provide the nitrogen gas in another suitable manner, for example, by introducing ammonia (NH3), which may also be used as a hydrogen-containing gas as described below, or nitrogen gas (N2). With respect to the hydrogen-containing gas, as some examples, the hydrogen-containing gas used to generate the plasma 122 may include H2 or ammonia (NH3). As discussed above, the hydrogen gas may facilitate the formation of a passivation layer 124 (eg, a nitride, such as a Si-nitride) on the surface 118 of the Si layer 110 and / or the etching of the Ge-containing layer 108.

[0035] Although shown separately, the nitrogen-containing gas may be provided separately (e.g., as nitrogen gas (N2)) and / or as part of a compound with one or more of the other gases used to generate the plasma 122 (e.g., as part of a compound with a fluorine-containing gas and / or as part of a compound with a hydrogen-containing gas). For example, a nitrogen carrier gas (N2) may be added and / or the nitrogen agent 130 for forming the passivation layer 124 (e.g., in embodiments where the passivation layer 124 is a nitride layer) may be provided from other gases, such as a nitrogen-containing compound for a fluorine-containing gas or a nitrogen-containing compound for a hydrogen-containing gas. In other words, the source of the nitrogenous agent 130 in the plasma 122 may be a nitrogen-containing etchant gas (e.g., a fluorine-containing gas) (e.g., NF3), a nitrogen-containing reducing gas (e.g., a hydrogen-containing gas) (e.g., NH3), a nitrogen-containing carrier gas (e.g., an N2 carrier gas), or another suitable nitrogen-containing source gas, and the nitrogenous agent 130 may be atomic nitrogen dissociated from the source gas.

[0036] As a particular example, the gases used to generate the plasma 122 may include a suitable combination of NF3, Ar, and H2. In particular embodiments, Ar may be replaced with other noble gases, such as helium (He) or krypton (Kr). As a particular example, the gas combinations used to generate the plasma 122 may include NF3 / NH3 / Ar, NF3 / NH3 / N2 / Ar, NF3 / H2 / Ar, or NF3 / H2 / Ar / N2.

[0037] Various process parameters for the plasma step 120 can be optimized to promote the formation of fluorine agent 126 for effective etching of Ge-containing layer 108 while generating sufficient hydrogen agent 128 and nitrogen agent 130 to form passivation layer 124 (e.g., a nitride passivation layer such as Si-nitride) at exposed surface 118 and additional surface 138 of Si layer 110. In one embodiment where the gas used to generate plasma 122 includes NF3 and H2, it may be appropriate to consider the ratio of NF3 to H2. The ratio of one gas to another may be measured in terms of the respective flow rates, e.g., standard cubic centimeters per minute (sccm). In certain embodiments, the plasma 122 includes more fluorine agent 126 than hydrogen agent 128 to ensure that the Ge-containing layer 108 is still etched and that a passivation layer similar to passivation layer 124 may not form on the exposed surface 116 of the Ge-containing layer 108 (especially if the Ge concentration in the Ge-containing layer 108 is low), but includes sufficient nitrogen agent 130 and hydrogen agent 128 to promote the formation of the passivation layer 124 quickly enough to reduce or eliminate etching of the Si layer 110 by the generally more reactive fluorine agent 126.

[0038] The appropriate ratio (or range of ratios) may depend on various factors, including other process parameters and the concentration of Ge in the Si layer 110. Hydrogen gas (H2) may help support reactions occurring in the plasma chamber 123, including etching the Ge-containing layer 108 and forming a passivation layer 124 on the exposed surface 118 and additional surface 138 of the Si layer 110. Exemplary ranges for the ratio of NF3 to H2 may include NF3:H2=about 4:about 1 to NF3:H2=about 10:about 1, and in certain embodiments, NF3:H2=about 5:about 1. In certain embodiments, when H2low is greater than about 30 sccm and the concentration of Ge in the Ge-containing layer 108 is about 15% or less, the etching rate of the Ge-containing layer 108 by the fluorine agent 126 may be reduced. It should be understood that this may or may not be applicable for a particular implementation, as the specific etching rate may depend on various factors. For noble gases, exemplary ranges for the ratio of NF3 to Ar can include NF3:Ar=about 1:about 2.5 to NF3:Ar=about 1:about 10.

[0039] Other process parameters for generating the plasma 122 include gas flow rates, pressure, plasma source power, plasma bias power, time, and temperature. The gases for forming the plasma 122 may be provided at any suitable flow rates. In certain embodiments, the etchant source gas flow rates are: fluorine-containing gas (e.g., NF3)=20-80 sccm (and in certain embodiments, 50 sccm), H2=5-15 sccm (and in certain embodiments, 10 sccm), and Ar=500-1500 sccm (and in certain embodiments, 1000 sccm). In these embodiments, the flow rate of the fluorine-containing gas is relatively moderate, the flow rate of the hydrogen-containing gas is relatively low, and the flow rate of the noble gas is relatively high.

[0040] In certain embodiments, the plasma step 120 may be performed at a relatively low pressure (e.g., less than about 100 mTorr, less than about 50 mTorr, and in one example, about 15 mTorr to about 25 mTorr) and at a relatively low source power (e.g., less than about 400 W, less than about 100 W, and in one example, about 100 W RF source power and about 0 W low frequency bias power). The exposure time for the plasma step 120 may be any suitable time. In certain embodiments, the exposure time may be only about 5 seconds or less, 15 seconds or less, 25 seconds or less, 30 seconds or less, or 45 seconds or less. The appropriate exposure time may depend on other parameters, such that an optimal combination of parameters is determined to achieve a desired level of selectivity (or other suitable goal). In certain embodiments, the plasma step 120 is performed at a temperature of about -40°C to about 20°C, and in one example, about 0°C.

[0041] One example recipe for the plasma step 120 includes: a pressure of about 15 to about 25 mTorr, a source power of 100 W (inductively coupled plasma), a bias power of 0 W, a wafer process temperature of 0° C., and NF3, H2, and Ar flow rates of 50 sccm, 10 sccm, and 1000 sccm, respectively.

[0042] For all parameters described herein, it should be understood that specific values ​​and ranges are provided for illustrative purposes only.

[0043] In certain embodiments, the plasma step 120 is an oxygen-free plasma etch step that etches a portion of a particular layer of a thin film stack of the substrate 102, resulting in a substrate 102 having a recessed or concave thin film stack after performing the process 100. It should be understood that oxygen-free does not necessarily mean that all oxygen is excluded from the plasma step 120, but instead reflects that an oxygen-containing gas was not intentionally introduced as part of the plasma step 120. It may be difficult or impossible to remove all oxygen from the plasma chamber 123, so some oxygen may still be present in the plasma chamber 123 during the plasma step 120.

[0044] 1D shows the substrate 102 after the plasma step 120. In the state shown in FIG. 1D, the thin film stack 104 includes depressions 136 (two examples of which are labeled). Furthermore, due to the formation of the depressions 136, exposed edges 141 of the Si layer 110 may be formed (one example of which is labeled).

[0045] FIG. 1D illustrates certain measurements of the resulting substrate 102, such as exposed edge separation width 142 and etched width 144. For example, exposed edge separation width 142 indicates the remaining width of the Ge-containing layer 108 (for this cross-section) by measuring each Ge-containing layer 108 from a first exposed surface 116 on a first side of the thin film stack 104 to an opposing second exposed surface 116 on a second side of the thin film stack 104. The exposed edge separation width 142 may be less than about 20 nm in certain embodiments, and in one embodiment, may be between about 2 nm and about 20 nm. The exposed edge separation width may also refer to the separation width of the exposed edges before etching. The etched width 144 may measure how much of a particular Ge-containing layer 108 has been removed from a particular edge of the particular Ge-containing layer 108. In other words, the etched width 144 may measure the amount of recession 136 in the Ge-containing layer 108. In particular embodiments, the etched width 144 is between about 5 nm and about 50 nm, however, the exposed end separation width 142 and the etched width 144 can be outside of these ranges depending on a given application.

[0046] Subsequent processing may then be performed on the substrate 102. For example, the plasma step 120 may be incorporated into a process to form the Si layer 110 into corresponding nanowires for a channel region of a semiconductor device, such as a GAA or other 3D device. In such a device, subsequent processing may include filling the recess 136 with an insulator, removing remaining portions of the Ge-containing layer 108, providing a gate oxide around the Si layer 110, and other associated steps, all of which are provided for illustrative purposes. In such a device, the exposed end 141 of the Si layer 110 may serve as a conductive contact to a channel region formed in an area of ​​the thin film stack 104.

[0047] The process 100 may provide one or more technical advantages. Some conventional techniques that attempt to selectively etch the Ge-containing layer 108 relative to the Si layer 110 expose the surfaces of both the Si layer 110 (e.g., the exposed surface 118 and the additional surface 138) and the Ge-containing layer 108 (e.g., the exposed surface 116) (e.g., along the sidewalls of the thin film stack 104) to a fluorine-containing chemical (e.g., F2, ClF3, BrF3, or IF5) or fluorine-containing radicals generated by a plasma. Such conventional plasmas may be generated, for example, from a gas containing CF4 and Ar or from a gas containing NF3 and N2. The fluorine-containing etchant (whether in the fluorine-containing chemical or in the fluorine radicals in the plasma) may react more rapidly with the Ge-containing layer 108 than the Si layer 110, thereby achieving a level of selectivity to Si (etching the Ge-containing layer 108 more rapidly than the Si layer 110). However, an undesirable amount of etching of the Si layer 110 still occurs.

[0048] For example, if etching of the Si layer 110 occurs at a corner of the Si layer 110, etching of the Si layer 110 may result in rounding of the corner. Additionally, as the exposed surface 116 of the Ge-containing layer 108 etches inwardly to form the recess 136, the vertical thickness of the Si layer 110 may decrease an undesirable amount, especially toward the exposed surface 118 that is exposed to the etchant for the longest time. Furthermore, if the concentration of Ge in the Ge-containing layer 108 is relatively low (e.g., ≦about 30%, and in certain embodiments ≦about 15%), the difference in reactivity of the Si layer 110 and the Ge-containing layer 108 with respect to the fluorine-containing etchant may be significantly reduced, which may result in poor selectivity (less than about 20:1 (etch rate of the Ge-containing layer to the etch rate of the Si layer)).

[0049] In addition, conventional fluorine-based plasmas may etch other materials on the semiconductor substrate, such as Si-oxide (SiO2), Si-nitride (Si3N4), oxides, and low-k dielectric materials, which may be undesirable. In other words, such conventional fluorine-based plasmas do not have selectivity to SiO2, Si3N4, oxides, and low-k dielectric materials (e.g., Si-oxycarbonitride (SiOCN), Si-boron carbonitride (SiBCN), etc.).

[0050] According to an embodiment of the process 100, the plasma step 120 may include forming a passivation layer 124 (e.g., a nitride such as Si-nitride) on the Si layer 110. The passivation layer 124 prevents etching of the Si layer 110 (e.g., exposed surface 118 and additional surface 138) while an etchant (e.g., fluorine agent 126) of the plasma 122 etches the Ge-containing layer 108 to form a recess 136 in the thin film stack 104. In certain embodiments, despite a potentially low concentration of Ge in the Ge-containing layer 108 (e.g., in certain embodiments, less than about 50%, less than about 30%, less than about 25%, and less than about 15%), and depending in part on the concentration of Ge in the Ge-containing layer 108, the selectivity ratio (as measured by the respective etch rates) of the Ge-containing layer 108 to the Si layer 110 is equal to or greater than about 50:about 1, equal to or greater than about 70:about 1, or equal to or greater than about 100:about 1. It should be understood that the respective etch rates may be determined in any suitable manner.

[0051] In addition, the thin film stack 104 may have an improved etch profile due at least in part to the high selectivity of the plasma 122 to the Si layer 110, which may be due at least in part to the rapid formation of the passivation layer 124 on the exposed surface 118 and the additional surface 138 of the Si layer 110. The improved etch profile may include reduced surface roughness along the surface 116 of the Ge-containing layer 108 (to the extent that the Ge-containing layer 108 has not been completely removed), and particularly along the exposed surface 118 and the remaining surface 138 of the Si layer 110, after the plasma step 120. Additionally or alternatively, the improved etch profile may include improved sharp edges and a relatively square profile of the exposed end 141 of the Si layer 110 after the plasma step 120, as compared to the extent possible with the prior art. In certain embodiments, the plasma step 120, which includes the use of the plasma 122, provides a relatively straight etch front along the surface 116 of the Ge-containing layer 108 (to the extent that the Ge-containing layer 108 is not completely removed) and good local uniformity with respect to the amount of material removed from each Ge-containing layer 108 of the thin film stack 104.

[0052] The nitride (e.g., Si-nitride) passivation layer 124 may be water insoluble, allowing the passivation layer 124 to act as an O2 and H2O diffusion barrier, thereby improving the stability of nanowires formed from the Si layer 110. In addition to being selective to Ge and SiGe, the plasma 122 (e.g., a fluorine-, hydrogen-, and nitrogen-containing plasma) may also be selective to SiO2, Si3N4, oxides, and low-k dielectric materials (e.g., SiOCN, SiBCN, etc.), due to the lack of oxygen in the chemistry that is typically present in certain embodiments to remove carbon and nitrogen bonds in these compounds (e.g., SiO2, Si3N4, oxides, and low-k dielectric materials (e.g., SiOCN, SiBCN, etc.).

[0053] Furthermore, certain embodiments may provide improved structures that may be used in 3D devices, such as may be suitable for GAA devices, 3D NAND or other memory devices, logic devices, or any other suitable type of semiconductor device.

[0054] 2 illustrates an exemplary method 200 for processing a substrate 102 according to certain embodiments of the present disclosure. The method 200 begins at step 202. In step 204, the substrate 102 is received. The substrate 102 has a thin film stack 104 including an alternating Ge-containing layer 108 and a Si layer 110. That is, the thin film stack 104 may include alternating Ge-containing layers 108 and Si layers 110 (e.g., as illustrated in FIG. 1A). A barrier layer 114 (e.g., NOL) may be present on a surface of the thin film stack 104, for example, on an exposed surface 116 of the Ge-containing layer 108, an exposed surface 118 of the Si layer 110, and exposed surfaces of the base layer 106 and the hard mask 112.

[0055] In step 206, the barrier layer 114 on the surface of the thin film stack 104 is etched to remove the barrier layer 114, for example, from the exposed surface 116 of the Ge-containing layer 108, from the exposed surface 118 of the Si layer 110, and from the exposed surfaces of the base layer 106 and the hard mask 112. The barrier layer 114 may be removed using any suitable process, such as a wet or dry etching process.

[0056] In step 208, the Ge-containing layer 108 is selectively etched by exposing the substrate 102 (including the thin film stack 104) to a plasma 122. The plasma 122 may include a fluorine agent 126, a hydrogen agent 128, and a nitrogen agent 130. The plasma 122 etches the Ge-containing layer 108 and forms a passivation layer 124 on the exposed surface 118 of the Si layer 110 to prevent etching of the Si layer 110 while the semiconductor device 102 (including the thin film stack 104) is exposed to the plasma 122. In a particular embodiment, step 208 is an isotropic etching process.

[0057] In a particular embodiment, the plasma 122 is generated from a gas including NF3 gas, and the fluorine agent 126 includes fluorine dissociated from NF3 gas. In one example, the nitrogen agent 130 includes nitrogen dissociated from NF3 gas. In a particular embodiment, the plasma 122 is generated from a gas including H2 gas, and the hydrogen agent 128 includes hydrogen. In a particular embodiment, the plasma 122 is generated from a gas including at least one noble gas, such as Ar, He, or Kr. As a particular example, the plasma 122 may be generated from a combination of gases including NF3, NH3, and Ar; NF3, NH3, N2, and Ar; NF3, H2, and Ar; or NF3, H2, Ar, and N2. In a particular embodiment, the passivation layer 124 formed on the exposed surface 118 of the Si layer 110 includes Si nitride (e.g., Si3N4).

[0058] Selectively etching the Ge-containing layer 108 may include selectively etching edges of the Ge-containing layer 108 to form recesses 136 in the thin film stack 104 above, below, or between the Si layers 110. As the Ge-containing layer 108 is selectively etched, additional surfaces 138 of the Si layers 110 are exposed and the plasma 122 forms a passivation layer 124 on the additional surfaces 138. In certain embodiments, selectively etching the Ge-containing layer 108 includes selectively removing substantially all of the Ge-containing layer 108 such that the Si layer 110 is open.

[0059] In particular embodiments, one or more of the Ge-containing layers 108 is a SiGe layer containing about 50 percent Ge or less. In even more particular embodiments, one or more of the Ge-containing layers 108 contains about 15 percent Ge or less, and the selectivity (as measured by respective etch rates) between the one or more 15 percent Ge-containing layers 108 and the Si layer 110 is equal to or greater than about 70:1.

[0060] In step 210, additional fabrication steps are performed. The discussion of possible additional processing steps discussed above with reference to Figure 1D is incorporated by reference. For example, in certain embodiments, step 208 is incorporated into a process for forming Si layer 110 into corresponding nanowires for a channel region of a semiconductor device, such as a GAA device. In step 212, the method ends.

[0061] 3 illustrates an exemplary method 300 for processing a substrate 102 in accordance with certain embodiments of the present disclosure. The method 300 begins at step 302. At step 304, the substrate 102 is placed in a plasma chamber 123 of a plasma tool. The substrate 102 has a thin film stack 104 including alternating Ge-containing layers 108 and Si layers 110 (e.g., as shown in FIG. 1A ).

[0062] In step 306, a plasma 122 is generated in a plasma chamber 123 of the plasma tool. The plasma 122 includes a fluorine agent 126, a hydrogen agent 128, and a nitrogen agent 130. The plasma 122 may be generated from a gas including a fluorine-containing gas, such as NF3, SF6, or CF4. The fluorine agent 126 may include fluorine dissociated from a fluorine-containing gas. In certain embodiments, the nitrogen agent 130 includes nitrogen dissociated from NF3 or another suitable nitrogen-containing gas that may or may not be part of a compound used to introduce the etchant (e.g., fluorine). In certain embodiments, the plasma 122 is generated from a gas including a hydrogen-containing gas (e.g., H2 or NH3), and the hydrogen agent 128 includes hydrogen dissociated from a hydrogen-containing gas.

[0063] In a particular embodiment, the plasma 122 is generated from gases including at least one noble gas, such as Ar, He, or Kr. As a particular example, the plasma 122 may be generated from a combination of gases including NF3, NH3, and Ar; NF3, NH3, N2, and Ar; NF3, H2, and Ar; or NF3, H2, Ar, and N2. In a particular embodiment, the passivation layer 124 formed on the exposed surface 118 of the Si layer 110 includes Si nitride (e.g., Si3N4).

[0064] In step 308, the substrate 102 (including the thin film stack 104) is exposed to a plasma 122 in a plasma chamber 123. The plasma 122 forms a passivation layer 124, which may be a nitride layer, on the exposed surface 118 and the additional surface 138 of the Si layer 110. In a particular embodiment, the passivation layer 124 includes Si nitride (Si3N4). The plasma 122 also selectively etches the exposed surface 116 (e.g., the opposite exposed end) of the Ge-containing layer 108 to form a recess 136 in the Ge-containing layer 108 relative to the exposed surface 118 (e.g., the opposite exposed end) of the Si layer 110. The passivation layer 124 prevents the etching of the Si layer 110 by the plasma 122. In a particular embodiment, step 308 is an isotropic etching process.

[0065] Additional fabrication steps are performed in step 310. The discussion of possible additional processing steps discussed above with reference to step 210 of Figure 2 is incorporated by reference. In step 312, the method ends.

[0066] 4 illustrates an exemplary device 400 including a substrate having a concave alternating thin film stack in accordance with certain embodiments of the present disclosure, at least a portion of which may be formed using any of the processes and methods described herein.

[0067] The device 400 includes a substrate 402 that includes a channel material 404 (e.g., Si or SiGe) and a gate material 406 (e.g., Ge or SiGe). The channel material 404 may correspond to the Si layer 110 of the substrate 102 at some point after the process 100. The device 400 may be a GAA device as shown here, or any other device, such as a Fin Field Effect Transistor (FinFET). The device 400 may also include an isolation region 408. In a particular embodiment, the isolation region 408 is a shallow trench isolation (STI).

[0068] Device 400 may be fabricated by first forming a recessed alternating thin film stack 410 (which may correspond to thin film stack 104 after process 100, possibly with additional subsequent processes), and then depositing additional gate material 406 onto recessed alternating thin film stack 410. In particular, device 400 may be formed by heteroepitaxially growing alternating Si and Ge or SiGe layers, followed by patterning to form vertical recesses and laterally expose the Si layers.

[0069] Applications of the embodiments described herein may advantageously be optimal solutions for the 5 nm node, 3 nm node, or below. For example, the GAA device architecture may be suitable for scaling beyond the 7 nm node. The GAA device architecture can address the short channel effect seen in some FinFET architectures by wrapping the gate around the entire channel, not just on three sides. The GAA device architecture can reduce or eliminate current leakage under the gate of the FinFET, thus reducing power loss during inactivity.

[0070] 5 illustrates a block diagram of an exemplary plasma tool 500 in accordance with certain embodiments of the present disclosure. Although a particular plasma tool 500 is shown and described, any suitable type of plasma tool may be used. The plasma tool 500 may be used to perform the plasma step 120 described with reference to FIGS. 1A-1D and 2-4.

[0071] The plasma tool 500 includes a plasma chamber 123 in which a semiconductor substrate (e.g., substrate 102) is processed using a plasma (e.g., plasma 122). The plasma chamber 123 includes a substrate table 502 configured to support the substrate 102 during processing. In a particular embodiment, to perform the plasma step 120 with the plasma 122, the substrate 102 is placed on the substrate table 502 in the state shown in FIG. 1B, for example following removal of the barrier layer 114. Material of the Ge-containing layer 108 (e.g., as described above with reference to FIGS. 1A-1D) of the thin film stack 104 of the substrate 102 is selectively etched in the plasma chamber 123 by injecting a plasma (e.g., plasma 122) through a showerhead 504 of the plasma tool 500. The showerhead 504 may include a single mixing reaction cavity filled with a precursor gas, a mixed gas, and a carrier gas that mix to form the plasma 122, and a set of exit holes for distributing the plasma 122 towards the substrate 102.

[0072] The plasma chamber 123, in certain embodiments, includes and / or is coupled to a vacuum pump 506 coupled to a vacuum line 508 for purging residual precursor gas from the plasma chamber 123, and may further include and / or be coupled to a pressure system for maintaining a target pressure. The plasma chamber 123 may further include mechanical tools, such as a heater 510 and a temperature sensor 512, used to heat the substrate 102 and control the temperature within the plasma chamber 123 and / or of the substrate 102.

[0073] The plasma tool 500 includes a precursor gas line 514, a mixture gas line 516, and a carrier gas line 518 coupled to a showerhead 504. In certain embodiments, the precursor gas supplied through the precursor gas line 514 may include a fluorine-based precursor, such as NF3 and / or SF6, the mixture gas supplied through the mixture gas line 516 may include hydrogen (e.g., H2 or NH3), and the carrier gas supplied through the carrier gas line 518 may include a noble gas, such as Ar, He, or Kr.

[0074] In certain embodiments, the plasma tool 500 may include a system of mass flow controllers and sensors for control of gas flows (e.g., mass flow rates). Thus, the plasma tool 500 may include a first flow controller 520, a second flow controller 522, a third flow controller 524, a vacuum pump 506, a heater 510, a temperature sensor 512, a voltage and current (VI) sensor 526, and substrate sensors 528, 530, 532, and 534 (528-534). The precursor gas line 514, the mixture gas line 516, and the carrier gas line 518 are coupled to and controlled by the first flow controller 520, the second flow controller 522, and the third flow controller 524, respectively.

[0075] The plasma tool 500 may include a controller 536 for controlling aspects of the plasma step 120. The controller 536 may be implemented in any suitable manner. For example, the controller 536 may be a computer. As another example, the controller 536 may include one or more programmable ICs programmed to provide the functionality described herein. In certain examples, one or more processors (e.g., microprocessors, microcontrollers, central processing units, etc.), programmable logic devices (e.g., complex programmable logic devices), field programmable gate arrays, etc.), and / or other programmable ICs are programmed with software or other programming instructions to provide the functionality described herein for the controller 536. The software or other programming instructions may be stored on one or more non-transitory computer-readable media (e.g., memory storage devices, flash memory, dynamic random access memory, reprogrammable storage devices, hard drives, floppy disks, DVDs, CD-ROMs, etc.), which, when executed by the programmable ICs, cause the programmable ICs to perform the operations described herein.

[0076] Mechanical components, such as the heater 510 and temperature sensor 512 in the plasma chamber 123, as well as flow controllers 520, 522 and 524, vacuum pump 506, and other components external to the plasma chamber 123, are coupled to and controlled by a controller 536.

[0077] Equipment sensors measure and provide signals for equipment parameters such as substrate table 502 temperature, heater current, vacuum pump speed, and temperature to ensure that the equipment is operating properly. Various process sensors measure and provide signals for process parameters such as process temperature, process pressure, plasma density, gas flow rate, and gas composition to ensure that the process is operating properly. Data from the equipment and process sensors provides feedback to the controller 536 continuously throughout the plasma step 120. The controller 536 can make adjustments in real time to keep the equipment and process close to the center of specification.

[0078] The controller 536 receives data from the sensors and controls process parameters of the plasma chamber 123 based on the sensor data. The controller 536 can analyze the data collected by the sensors and determine when to modify or terminate one or more of the plasma steps 120 and provide feedback to control process parameters of the components of the plasma chamber 123.

[0079] The controller 536 can be connected to the VI sensor 526 and the substrate sensors 528-534 to monitor the plasma 122 as the substrate 102 is exposed to the plasma 122 and provide real-time status, and optionally compositional and thickness data, of the plasma 122. This feedback data can be used by the controller 536 to continuously adjust the plasma step 120 as the substrate 102 is selectively etched with the plasma 122, for example, to turn off the plasma step 120 when a target recess (e.g., etched width 144) is reached.

[0080] Specifically, measurement data from the substrate sensors 528-534 and the temperature sensor 512 may be received by the controller 536, while the controller 536 generates control signals that are sent to the first flow controller 520, the second flow controller 522, the third flow controller 524, the vacuum pump 506, and the heater 510.

[0081] The controller 536 may receive measurement or metrology data from the substrate sensors 528-534 taken at multiple points across the substrate 102 to measure in situ and in real time the process non-uniformity and thickness and composition of the passivation layer 124 (formed by exposing the substrate 102 to the plasma 122), the exposed edge separation width 142, and / or the target thickness (e.g., etch width 144). For example, multiple sensors across the substrate in a multi-substrate plasma tool can be used to monitor and adjust the thickness and composition of the passivation layer 124 (formed by exposing the substrate 102 to the plasma 122), the exposed edge separation width 142, and / or the target recess (e.g., etch width 144) from the top to the bottom of the substrate 102. Multiple sensors across the substrate in a single substrate plasma tool can be used to monitor and adjust the thickness and composition of the passivation layer 124 (formed by exposing the substrate 102 to the plasma 122), the exposed edge separation width 142, and / or the target recess (e.g., etch width 144) from the center of the substrate 102 to the edge of the substrate 102.

[0082] Substrate sensors 528-534 may be coupled to and / or located within the plasma chamber 123 to monitor various parameters of the substrate 102, the plasma tool 500, and / or the plasma step 120. The substrate sensors 528-534 may include various types of sensors, including, but not limited to, optical sensors (e.g., cameras, lasers, light, reflectometers, spectrometers, etc., ellipsometers, etc.), capacitive sensors, ultrasonic sensors, gas sensors, or other sensors capable of monitoring conditions of the substrate 102, the plasma 122, and / or the plasma tool 500. In certain embodiments, one or more optical sensors may be used to measure in real time (during the plasma step 120) the thickness and refractive index of material at the surface 118 of the Si layer 110 and the surface of the base layer 106 (e.g., where the passivation layer 124 is formed), the exposed edge separation width 142, and / or the etched width 144a (or other suitable measurements). As another example, a spectrometer may be used to measure in real time (during plasma step 120) the thickness of material at surface 118 of Si layer 110 and at the surface of base layer 106 (e.g., where passivation layer 124 is formed), exposed edge separation width 142, and / or etched width 144a (or other suitable measurements). In yet another embodiment, a residual gas analyzer (RGA) may be used to detect precursor destruction in real time (during plasma step 120) for real time chemical reaction completion detection.

[0083] The controller 536 may receive user-input process parameters including, for example, etch rate (e.g., of the passivation layer 124), conformality, profile, and deposition rate based on standard plasma etch parameters such as chamber pressure, chamber temperature, RF source power, RF bias power, RF waveform (e.g., continuous wave RF, pulsed RF, square pulse, sawtooth pulse, etc.), etch time, and various process and carrier gas compositions and flow rates. Advantageously, the user can tune the plasma 122 to meet a target local critical dimension uniformity (LCDU).

[0084] Based on the data from the substrate sensors 528-534 and user-entered process parameters, the controller 536 generates and sends control signals to the temperature sensor 512 and the heater 510 to regulate the heating in the plasma chamber 123. While the heater 510 heats the plasma chamber 123, the controller 536 periodically or periodically monitors the temperature sensor 512 to track the temperature of the plasma chamber 123 and sends control signals to the heater 510 to maintain the temperature in the plasma chamber 123.

[0085] When the controller 536 determines that the target temperature of the plasma chamber 123 has been reached based on the data provided by the temperature sensor 512, the controller 536 generates control and data signals to activate the first flow controller 520, the second flow controller 522, and the third flow controller 524, and provides a target flow rate of the precursor gas to the first flow controller 520, a target flow rate of the mixture gas to the second flow controller 522, and a target flow rate of the carrier gas to the third flow controller 524 based on the process parameters entered by the user. When the controller 536 determines that the corresponding flow rates have been established, the controller 536 provides power to the plasma chamber 123 through the bias and source electrodes to power the plasma 122. The power provided to the bias and source electrodes may be adjusted based on measurements from the VI sensor 526. The first flow controller 520, the second flow controller 522, and the third flow controller 524 may each be a closed loop control system connected to a flow sensor and an adjustable proportional valve, which allows each flow controller to periodically or cyclically monitor and internally maintain a target flow rate for each gas via the flow sensor and adjustable proportional valve.

[0086] In certain embodiments, when the controller 536 determines, based on user-inputted data, that the etch process time has been met, the controller 536 generates control signals to shut down the first flow controller 520, the second flow controller 522, and the third flow controller 524. The controllers may be shut down simultaneously or at different times, as appropriate.

[0087] The controller 536 may use or analyze the substrate sensor data to determine when to terminate the plasma step 120. For example, the controller 536 may receive data from a residual gas analyzer to detect the end point of the plasma step 120. In another example, the controller 536 may use spectroscopic ellipsometry to detect the average thickness of the passivation layer 124, the exposed edge 141 of the Si layer 110, and / or the exposed edge separation width 142 during the plasma step 120 to indicate changes during the plasma step 120. In another example, the controller 536 may use spectroscopic ellipsometry to detect the refractive index of the material at the surface 118 of the Si layer 110 (e.g., on which the passivation layer 124 is formed) and the surface of the base layer 106 during the plasma step 120 to indicate film composition changes during the plasma step 120. The controller 536 may automatically terminate the plasma step 120 when the objectives of the exposed edge separation width 142 and / or the etched width 144a (or other suitable measurements) are achieved. In certain embodiments, the controller 536 may automatically adjust one or more parameters during the plasma step 120, such as, for example, the ratio of NF3 to H2 (or NH3) and / or the ratio of NF3 to Ar, to achieve a desired etch profile of the thin film stack 104. Data from the controller 536 and the substrate sensors 528-534 may also be used to achieve a desired semiconductor substrate throughput goal. Additionally, data from the controller 536 and the substrate sensors 528-534 may be used to achieve, or alternatively target a combination of, a desired etch profile and composition of the thin film stack 104 along with the desired semiconductor substrate throughput.

[0088] Although described in terms of a specific application of forming nanowires / nanosheets for GAA devices, the present disclosure can be used in any type of isotropic etching of Si that is selective to a Ge-containing layer. Furthermore, although the etching performed is described as primarily removing a portion of the opposing end of the Ge-containing layer 108 to form a recess in the thin film stack 104, the processes 100 and 400 may be used to remove substantially all of the Ge-containing layer 108, which may be referred to as opening up the Si layer 110.

[0089] Although the present disclosure describes certain process / method steps occurring in a particular order, the present disclosure contemplates that the process steps may occur in any suitable order. Although the present disclosure has been described with reference to exemplary embodiments, this description is not intended to be construed in a limiting sense. Various modifications and combinations of the exemplary embodiments, as well as other embodiments of the present disclosure, will be apparent to those skilled in the art upon reference to this specification. Accordingly, it is intended that the appended claims cover any such modifications or embodiments.

Claims

1. 1. A method for processing a semiconductor substrate, the method comprising: receiving a semiconductor substrate including a thin film stack, the thin film stack including a first silicon layer, a second silicon layer, and a first germanium-containing layer disposed between the first silicon layer and the second silicon layer; selectively etching the first germanium-containing layer by exposing the thin film stack to a plasma comprising a fluorine agent, a nitrogen agent, and a hydrogen agent, the plasma etching the first germanium-containing layer and simultaneously forming a passivation layer on exposed surfaces of the first silicon layer and the second silicon layer to inhibit etching of the first silicon layer and the second silicon layer while the thin film stack is exposed to the plasma, the passivation layer comprising nitride; The method comprising:

2. The method of claim 1 , wherein the plasma is generated from a gas that includes a noble gas.

3. The plasma is nitrogen trifluoride (NF 3 ) gases, including The fluorine agent is the NF 3 The method of claim 1 comprising dissociating fluorine from the gas.

4. The plasma is H 2 2. The method of claim 1, wherein the hydrogen agent is generated from a gas containing gas, and the hydrogen agent is hydrogen.

5. The plasma is Nitrogen trifluoride (NF 3 ), ammonia (NH 3 ) and argon (Ar); N.F. 3 , N.H. 3 , nitrogen (N 2 ) and Ar; N.F. 3 , hydrogen (H 2 ) and Ar; or N.F. 3 , H 2 , Ar and N 2 ; The method of claim 1 , wherein the gas is generated from a combination of gases including

6. 2. The method of claim 1, wherein the passivation layer formed on the exposed surfaces of the first and second silicon layers comprises silicon nitride.

7. 2. The method of claim 1, wherein the first germanium-containing layer is a silicon-germanium (SiGe) layer containing about 50 percent germanium or less.

8. the first germanium-containing layer comprises about 15 percent or less germanium; 8. The method of claim 7, wherein a selectivity of the first germanium-containing layer to the first silicon layer and the second silicon layer is about 70:1 or greater.

9. 2. The method of claim 1 , wherein selectively etching the first germanium-containing layer comprises selectively etching an edge of the first germanium-containing layer to form an indent in the thin film stack between the first silicon layer and the second silicon layer.

10. 2. The method of claim 1 , wherein as the first germanium-containing layer is selectively etched, additional surfaces of the first silicon layer and the second silicon layer are exposed, and the plasma forms the passivation layer on the additional surfaces.

11. 2. The method of claim 1 , wherein selectively etching the first germanium-containing layer comprises selectively removing substantially all of the first germanium-containing layer between the first silicon layer and the second silicon layer.

12. Prior to the step of selectively etching the first germanium-containing layer, a native oxide layer is present on a surface of the thin film stack; The method of claim 1 , further comprising the step of etching the native oxide layer.

13. the thin film stack further comprising a second germanium-containing layer and a third silicon layer, the second germanium-containing layer being disposed between the second silicon layer and the third silicon layer; The method includes selectively etching the second germanium-containing layer by exposing the thin film stack to the plasma; 2. The method of claim 1, wherein the plasma forms a passivation layer on exposed surfaces of the third silicon layer to inhibit etching of the third silicon layer while the thin film stack is exposed to the plasma.

14. 1. A method for processing a semiconductor substrate, the method comprising: placing a semiconductor substrate in a plasma chamber of a plasma tool, the semiconductor substrate having a thin film stack, the thin film stack having alternating silicon and germanium-containing layers, the thin film stack having at least two silicon layers and at least two germanium-containing layers; generating a plasma in the plasma chamber of the plasma tool, the plasma comprising a fluorine agent, a nitrogen agent, and a hydrogen agent, the plasma being generated from gases including a fluorine-containing gas, a nitrogen-containing gas, a hydrogen-containing gas, and a noble gas; exposing the thin film stack to the plasma in the plasma chamber of the plasma tool, the plasma forming a nitride passivation layer on exposed surfaces of the silicon layer and selectively etching opposing exposed ends of the germanium-containing layer relative to opposing exposed ends of the silicon layer to form recesses in the germanium-containing layer, the nitride passivation layer inhibiting etching of the silicon layer by the plasma; The method comprising:

15. The fluorine-containing gas is nitrogen trifluoride (NF 3 ), sulfur hexafluoride (SF 6 ), or carbon tetrafluoride (CF 4 ), The method of claim 14 , wherein the fluorine agent comprises fluorine dissociated from the fluorine-containing gas.

16. The hydrogen-containing gas is H 2 or ammonia (NH 3 ), The method of claim 14 , wherein the hydrogen agent comprises hydrogen dissociated from the hydrogen-containing gas.

17. The nitrogen-containing gas is N 2 , nitrogen trifluoride (NF 3 ) or ammonia (NH 3 ), The method of claim 14 , wherein the nitrogen agent comprises nitrogen dissociated from the nitrogen-containing gas.

18. the nitrogen-containing gas and the fluorine-containing gas are part of the same gas compound; or The method of claim 14 , wherein the nitrogen-containing gas and the hydrogen-containing gas are part of the same gas compound.

19. a flow rate of the noble gas is greater than a flow rate of the fluorine-containing gas; The method of claim 14 , wherein the flow rate of the fluorine-containing gas is greater than the flow rate of the hydrogen-containing gas.

20. The method of claim 14 , wherein the noble gas is argon (Ar).

21. The gas in which the plasma is generated is Nitrogen trifluoride (NF 3 ), ammonia (NH 3 ) and argon (Ar); N.F. 3 , N.H. 3 , nitrogen (N 2 ) and Ar; N.F. 3 , hydrogen (H 2 ) and Ar; or N.F. 3 , H 2 , Ar and N 2 ; 15. The method of claim 14, comprising:

22. 15. The method of claim 14, wherein the nitride passivation layer formed on the exposed surfaces of both the silicon layers comprises silicon nitride.

23. 1. A method for processing a semiconductor substrate, the method comprising: placing a semiconductor substrate in a plasma chamber of a plasma tool, the semiconductor substrate having a thin film stack including a first layer of a first material and a second layer of a second material in an alternating layer-by-layer arrangement, the first material being a germanium-containing material including a germanium concentration of about 10 to about 50 percent; generating a plasma for selectively etching the first layer of the first material, the generating the plasma comprising introducing a gas including fluorine, nitrogen, hydrogen and a noble gas into the plasma chamber and maintaining a pressure in the plasma chamber below about 50 millitorr; exposing the thin film stack to the plasma in the plasma chamber for a period of time, the plasma forming a nitride passivation layer on the exposed surface of the second layer of the second material and selectively etching opposing exposed ends of the first layer of the first material relative to opposing exposed ends of the second layer of the second material to form a recess in the first layer of the first material; The method comprising:

24. A method for processing a semiconductor substrate, the method comprising: receiving a semiconductor substrate having a thin film stack, the thin film stack including a first silicon layer, a second silicon layer, and a first germanium-containing layer disposed between the first silicon layer and the second silicon layer; selectively etching the first germanium-containing layer by exposing the thin film stack to a plasma comprising a fluorine agent, a nitrogen agent, and a hydrogen agent, the plasma etching the first germanium-containing layer while simultaneously forming a passivation layer on exposed surfaces of the first silicon layer and the second silicon layer to inhibit etching of the first silicon layer and the second silicon layer while the thin film stack is exposed to the plasma, and a gas generating the plasma is oxygen-free; The method comprising: