High-strength cold-rolled steel sheet with excellent surface quality and little material deviation, and its manufacturing method
A controlled composition and manufacturing process for high-strength cold-rolled steel sheets address surface defects and material deviation, achieving tensile strength and formability suitable for automobile components.
Patent Information
- Application Number
- JP2024518253
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-24
- Filing Date
- 2022-09-20
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-09-20
AI Technical Summary
Conventional high-strength cold-rolled steel sheets face issues with surface defects and material deviation due to the addition of elements like Si, Mn, and high carbon content, which affect weldability and thickness quality, limiting their application to automobile impact-resistant members.
A high-strength cold-rolled steel sheet composition with controlled carbon (C), silicon (Si), manganese (Mn), and other elements, along with specific manufacturing processes including reheating, hot rolling, cooling, winding, and continuous annealing, to minimize surface defects and material deviation.
The solution provides a cold-rolled steel sheet with tensile strength of 780 MPa or more, excellent surface quality, and stable strength-elongation balance, suitable for structural components like automobile fillers.
Smart Images

Figure 2024535899000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-strength cold-rolled steel sheet used for structural components with a large amount of forming, such as fillers, seat rails, and members of an automobile body, and a manufacturing method thereof. More specifically, the present invention relates to a high-strength cold-rolled steel sheet having excellent surface quality and little material deviation, which can be suitably used for automobile parts, and a manufacturing method thereof. [Background technology]
[0002] Recently, as safety and environmental regulations have become more stringent in the automobile industry, the use of high-strength steel with a tensile strength of 780 MPa or more has been increasing in manufacturing vehicle bodies to improve fuel efficiency and protect passengers.
[0003] Conventional high-strength steels used in automobile bodies include dual phase (DP) steel, which is composed of a soft ferrite matrix and hard martensite, transformation induced plasticity (TRIP) steel, which utilizes the transformation-induced plasticity of retained austenite, and complex phase (CP) steel, which is composed of a composite structure of ferrite and hard bainite or martensite.
[0004] However, when high strength steel contains a large amount of Si, Al, Mn, etc., there are problems in that the weldability is deteriorated and surface defects of the steel sheet occur due to in-furnace dents during annealing. In addition, when a large amount of hardening elements such as Mn, Cr, Mo are added, there is a problem in that material deviation occurs in the hot rolled coil, and thickness quality deteriorates during cold rolling. In this case, surface defects caused by in-furnace dents refer to surface defects of the steel sheet that are formed when the metal oxide on the surface of the steel sheet is adsorbed and accumulated on the rolls of the annealing furnace and the steel sheet comes into contact with the rolls during passing.
[0005] The prior art related to the manufacturing technology of high strength cold rolled steel sheet and hot dip galvanized steel sheet for solving the above problems will be briefly described as follows.
[0006] Among the conventional techniques, Patent Document 1 proposes a high-strength cold-rolled steel sheet and its manufacturing method, which comprises a process of cold-rolling a hot-rolled steel sheet containing 60% or more of low-temperature transformation phase by volume at a cold reduction rate of more than 60% and less than 80%, and a process of continuously annealing the cold-rolled steel sheet in the ferrite-austenite two-phase region. However, the cold-rolled steel sheet obtained from Patent Document 1 has a low strength of 370 to 590 MPa, making it difficult to apply to automobile impact-resistant members, and is therefore limited to use only for interior and exterior panel panels.
[0007] In addition, Patent Document 2 discloses a method for producing a cold-rolled steel sheet that has high strength and high ductility at the same time by utilizing a tempered martensite phase and has excellent sheet shape after continuous annealing. However, the technology of Patent Document 2 has problems such as poor weldability due to the high carbon content of the steel of 0.2% or more, and surface defects due to furnace dents caused by the large amount of Si content. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 2004-0066935 [Patent Document 2] JP 2010-090432 A Summary of the Invention [Problem to be solved by the invention]
[0009] According to one aspect of the present invention, there is provided a high-strength cold-rolled steel sheet having excellent surface quality and little material deviation, and a method for manufacturing the same.
[0010] The object of the present invention is not limited to the above-mentioned contents. Anyone having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding further object of the present invention from the entire contents described in the specification of the present invention. [Means for solving the problem]
[0011] One aspect of the present invention is In weight percent, it contains C: 0.05-0.3%, Si: 0.01-2.0%, Mn: 1.5-3.0%, Al: 0.01-0.1%, P: 0.001-0.015%, S: 0.001-0.01%, N: 0.001-0.01%, the balance being Fe and other unavoidable impurities. The value defined by the following relational expression 1 satisfies 0.6 or more and less than 0.9, The microstructure contains, by area%, ferrite: 50% or more, the remainder: bainite and martensite, The average number of surface defects that meet one or more of the following conditions: depth 100μm or more and short side length 1mm or more is 10 defects / m 2 To provide a high strength cold rolled steel sheet having a strength of less than [Equation 1] C+(1.3×Si+Mn) / 6+(Cr+1.2×Mo) / 5+100×B (In the above Relational Formula 1, C, Si, Mn, Cr, Mo and B indicate the average content by weight of each element. In addition, when each of the above elements is not added, 0 is substituted.)
[0012] Another aspect of the present invention is a step of reheating a steel slab containing, by weight percent, C: 0.05-0.3%, Si: 0.01-2.0%, Mn: 1.5-3.0%, Al: 0.01-0.1%, P: 0.001-0.015%, S: 0.001-0.01%, N: 0.001-0.01%, the balance being Fe and other unavoidable impurities, and satisfying a value defined by the following Relation 1 of 0.6 or more and less than 0.9, to 1100-1350°C; hot rolling the reheated steel slab at 850 to 1150°C; cooling the hot-rolled steel sheet to 450 to 700°C at an average cooling rate of 10 to 70°C / s; coiling the cooled steel sheet at 450 to 700°C; cold rolling the coiled steel sheet at a rolling reduction of 40 to 70%; and continuous annealing the cold rolled steel sheet at 740 to 900°C; Including, The coiling step is controlled so that the surface temperature (Te) at both ends in the width direction is 601 to 700°C and the surface temperature (Tc) at the center is 450 to 600°C based on the entire width of the steel sheet. [Equation 1] C+(1.3×Si+Mn) / 6+(Cr+1.2×Mo) / 5+100×B (In the above Relational Formula 1, the above C, Si, Mn, Cr, Mo and B indicate the average content by weight of each element. In this case, when each of the above elements is not added, 0 is substituted.) Effect of the Invention
[0013] According to one aspect of the present invention, it is possible to provide a high-strength cold-rolled steel sheet having excellent surface quality and little material deviation, and a method for manufacturing the same.
[0014] The various yet significant advantages and effects of the present invention are not limited to the above, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]
[0015] [Figure 1] 1 shows photographs of surface defects of each cold-rolled steel sheet obtained from Example 1 of the present invention and Comparative Example 1, taken with a general low-magnification camera. [Diagram 2] 1 shows a photograph of a surface defect defined in the present invention taken with a high-magnification scanning electron microscope (SEM). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, preferred embodiments of the present invention will be described. However, the embodiments of the present invention can be modified into several other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.
[0017] In addition, the terms used in the present specification are intended to describe specific embodiments and are not intended to limit the present invention. For example, the singular form used in the present specification includes the plural form unless the related definition clearly indicates a contrary meaning. In addition, the meaning of "include" used in the specification embodies a configuration and does not exclude the presence or addition of other configurations.
[0018] With conventional technology, there is currently no technology developed that can meet the high-end demand for cold-rolled steel sheets that have high strength (tensile strength (TS) of 780 MPa or more), excellent formability, and can be used in structural components with a large amount of forming, while also having excellent surface quality and little material deviation.
[0019] Therefore, the inventors conducted extensive research to provide a cold-rolled steel sheet that satisfies all of the above-mentioned characteristics while solving the problems of the conventional technology. As a result, they found that the above-mentioned object can be achieved by optimizing the composition and manufacturing conditions of the steel sheet and controlling the characteristics of the microstructure and surface defects, and thus completed the present invention.
[0020] That is, according to the present invention, it is possible to effectively provide a high-strength cold-rolled steel sheet that has a high strength of 780 MPa or more, while also satisfying a product of tensile strength and elongation of 12,000 MPa% or more, and can be suitably applied to structural member parts such as fillers that require a stable balance of strength-elongation and impact absorption properties among parts that constitute an automobile body.
[0021] Hereinafter, a high-strength steel plate having excellent surface quality and little material deviation according to one embodiment of the present invention will be described in detail.
[0022] A high-strength cold-rolled steel sheet according to one embodiment of the present invention contains, by weight, C: 0.05-0.3%, Si: 0.01-2.0%, Mn: 1.5-3.0%, Al: 0.01-0.1%, P: 0.001-0.015%, S: 0.001-0.01%, N: 0.001-0.01%, the balance being Fe and other unavoidable impurities.
[0023] The reasons for adding the elements to the cold-rolled steel sheet according to the present invention and the reasons for limiting the contents thereof will be specifically described below. In this specification, the contents of the elements are expressed in weight percent unless otherwise specified.
[0024] C: 0.05 to 0.3% The carbon (C) is a very important component in securing a martensite structure that is effective in strengthening steel. When the amount of C added increases, the martensite and bainite phase fractions increase, and the tensile strength increases. Therefore, in order to secure high strength, the lower limit of the C content is controlled to 0.05%. However, when the C content increases, the austenite region is expanded during two-phase annealing, so that the martensite and bainite phase fractions, which are hard phases, increase, and the ferrite phase fraction, which is a soft phase, decreases, resulting in deterioration of formability and weldability. Therefore, the upper limit of the C content is controlled to 0.3%. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the C content can be 0.06%, or the upper limit of the C content can be 0.12%.
[0025] Silicon: 0.01 to 2.0% The silicon (Si) is an element advantageous in deoxidizing molten steel, having a solid solution strengthening effect, and delaying the formation of coarse carbides to improve formability. However, if the Si content is less than 0.01%, the above-mentioned effects are small, making it difficult to improve formability. On the other hand, if the Si content exceeds 2.0%, red scale due to Si is severely formed on the steel sheet surface during hot rolling. This causes surface defects, or the surface is concentrated during the annealing process, causing non-plating. Furthermore, there is a problem that the plating adhesion is deteriorated due to the formation of surface oxide, resulting in very poor surface quality. Therefore, in the present invention, the Si content is controlled to 0.01 to 2.0%. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the Si content can be 0.4%, or the upper limit of the Si content can be 1.2%.
[0026] Mn: 1.5-3.0% The manganese (Mn) is an element that is effective in solid-solution strengthening steel, similar to Si, and is an element that greatly increases hardening ability. However, if the Mn content is less than 1.5%, the above-mentioned effect of addition cannot be obtained, and if the Mn content exceeds 3.0%, the strengthening effect increases greatly and ductility decreases. In addition, in the continuous casting process, segregation parts develop significantly at the thickness center during slab casting, and when cooling after hot rolling, the microstructure in the thickness direction becomes non-uniform, and MnS is formed, resulting in poor formability such as stretch flangeability. Therefore, in the present invention, the Mn content is controlled to 1.5 to 3.0%. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the Mn content can be 1.8%, or the upper limit of the Mn content can be 2.6%.
[0027] Al: 0.01 to 0.1% The aluminum (Al) is a component added mainly for deoxidation. If the Al content is less than 0.01%, the effect of adding the Al is insufficient. On the other hand, if the Al content exceeds 0.1%, AlN is formed by bonding with nitrogen, which makes it easy for corner cracks to occur in the slab during continuous casting, and defects due to the formation of inclusions are likely to occur. Therefore, in the present invention, the Al content is controlled to 0.01 to 0.1%. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the Al content can be 0.015%, or the upper limit of the Al content can be 0.06%.
[0028] P: 0.001 to 0.015% The phosphorus (P) is an alloy element with a very large solid solution strengthening effect, and has the characteristic that a large strengthening effect can be obtained even with a small content. However, if P is added excessively, brittleness occurs due to grain boundary segregation, fine cracks are likely to occur during molding, and ductility and impact resistance properties are greatly deteriorated. There is also a problem that defects are caused on the surface during plating. Therefore, the upper limit of the P content is controlled to 0.015%. On the other hand, if the P content is less than 0.001%, excessive manufacturing costs are required to meet this, which is not only economically disadvantageous, but also the strength ensured is insufficient, so the lower limit of the P content is controlled to 0.001% or more. Therefore, in the present invention, it is preferable to control the P content to 0.001 to 0.015%. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the P content can be 0.003%, or the upper limit of the P content can be 0.012%.
[0029] S: 0.001 to 0.01% The above-mentioned sulfur (S) is an impurity present in steel, and if the S content exceeds 0.01%, it combines with Mn and the like to form nonmetallic inclusions, which makes it easy for fine cracks to occur during cutting of the steel, and causes a problem that stretch flangeability and impact resistance are significantly deteriorated. In addition, in order to manufacture the steel so that the S content is less than 0.001%, it takes a lot of time during steelmaking operation, and productivity decreases. Therefore, in the present invention, it is preferable to control the S content to 0.001 to 0.01%. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the S content can be 0.002%, or the upper limit of the S content can be 0.007%.
[0030] N: 0.001 to 0.01% The nitrogen (N) is a representative solid solution strengthening element together with C, and contributes to the formation of coarse precipitates together with Ti and Al. In general, the solid solution strengthening effect of N is superior to that of carbon, but there is a problem that the toughness is greatly reduced as the amount of N in steel increases. In addition, in order to manufacture steel so that the N content is less than 0.001%, there is a problem that it takes a lot of time during steelmaking operation and productivity is reduced. Therefore, in the present invention, it is preferable to control the N content to 0.001 to 0.01%. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the N content may be 0.002% and the upper limit of the N content may be 0.006%.
[0031] Meanwhile, according to one aspect of the present invention, although not particularly limited, the cold-rolled steel sheet may selectively further include, by weight percent, one or more selected from Cr: 1.0% or less (including 0%), Mo: 0.2% or less (including 0%), and B: 0.005% or less (including 0%). Hereinafter, the reasons for adding the selectively added elements and the reasons for limiting the contents thereof will be described.
[0032] Cr: 1.0% or less (including 0%) Chromium (Cr) is a component added to improve the hardenability of steel and ensure high strength, and is an element that plays a very important role in martensite formation. It is advantageous for manufacturing a dual-phase steel having high ductility by minimizing the decrease in elongation with respect to the increase in strength. Therefore, Cr can be selectively added for the above-mentioned effects. However, if the Cr content exceeds 1.0%, not only the above-mentioned effects are saturated, but also there is a problem that the cold rolling property is deteriorated due to an excessive increase in hot rolling strength. In addition, there is a problem that the martensite fraction after annealing increases significantly, resulting in a decrease in elongation, so the upper limit of the Cr content is controlled to 1.0% or less. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the Cr content can be 0.01%, or the upper limit of the Cr content can be 0.8%.
[0033] Mo: 0.2% or less (including 0%) Molybdenum (Mo) is an element that suppresses pearlite formation and increases hardenability. Therefore, in order to ensure the above-mentioned effects, Mo can be selectively added in the present invention. However, if the Mo content exceeds 0.2%, the effect of improving strength does not increase significantly, while ductility deteriorates, which may be economically disadvantageous. Therefore, it is preferable to control the Mo content to 0.2% or less. On the other hand, from the viewpoint of further improving the above-mentioned effects, more preferably, the lower limit of the Mo content can be 0.01%, or the upper limit of the Mo content can be 0.1%.
[0034] B: 0.005% or less (including 0%) Boron (B) has the effect of stabilizing grain boundaries and improving the brittleness of steel at low temperatures when present in a solid solution state in steel, and greatly increases the hardenability of steel. Therefore, B can be selectively added for the above-mentioned effect. However, if the upper limit of B exceeds 0.005%, recrystallization is delayed during annealing, and oxides are formed on the surface, resulting in deterioration of platability. Therefore, it is preferable to control the content of B to 0.005% or less. On the other hand, from the viewpoint of further improving the above-mentioned effect, more preferably, the lower limit of the B content can be 0.0003%, or the upper limit of the B content can be 0.0025%.
[0035] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, unintended impurities are inevitably mixed in due to raw materials and surrounding environmental variables, and it is not possible to exclude them. These impurities are known to any engineer of normal steel manufacturing processes, so the contents of all of them will not be mentioned in this specification.
[0036] According to one aspect of the present invention, the high strength cold rolled steel sheet may have a value defined by the following Relational Expression 1 of 0.6 or more and less than 0.9. By satisfying this, it is possible to minimize the material deviation of the cold rolled steel sheet and suppress the occurrence of surface defects, thereby ensuring the desired material properties. [Equation 1] C+(1.3×Si+Mn) / 6+(Cr+1.2×Mo) / 5+100×B (In the above Relational Formula 1, the above C, Si, Mn, Cr, Mo and B indicate the average content by weight of each element. In this case, when each of the above elements is not added, 0 is substituted.)
[0037] In the present invention, the above-mentioned Relational Formula 1 is an equation showing the hardenability of the steel material according to the composition of the present invention, and the coefficient before each element quantitatively expresses the scale of the contribution of the element to the hardenability. If the hardenability of the steel material is high, it is advantageous for securing hard low-temperature transformation phases such as bainite and martensite phases, and contributes to improving strength, while the lower the hardenability, the more the ferrite transformation is promoted, which is disadvantageous for securing strength.
[0038] In particular, in order to secure a high strength of tensile strength (TS) of 780 MPa or more, which is the target in the present invention, the value defined by the above-mentioned relational expression 1 must satisfy 0.6 or more. On the other hand, if the value defined by the above-mentioned relational expression 1 is 0.9 or more, the strength becomes too high, and there is a problem that the elongation rate deteriorates. Furthermore, if the value defined by the above-mentioned relational expression 1 is 0.9 or more, the phase transformation of ferrite is significantly delayed in the stage of cooling the hot-rolled steel sheet to 450 to 700 ° C. at an average cooling rate of 10 to 70 ° C. / s immediately after hot rolling. As a result, in the subsequent coiling stage, the lower bainite phase and martensite phase, which have high hardness, are formed excessively in the bainite phase in the hot-rolled steel sheet, and the material deviation due to the position in the width direction becomes severe, and the shape is deteriorated. Therefore, in the present invention, it is preferable to control the value defined by the above-mentioned relational expression 1 so that it satisfies 0.6 or more and less than 0.9. On the other hand, from the viewpoint of further maximizing the above-mentioned effect, the lower limit of the value defined by the above-mentioned relational expression 1 can be 0.62, or the upper limit of the value defined by the above-mentioned relational expression 1 can be 0.84.
[0039] Meanwhile, according to one aspect of the present invention, the high-strength cold-rolled steel sheet contains, in terms of area percent, ferrite: 50% or more, and the remainder: bainite and martensite as a microstructure. If the ferrite in the microstructure is less than 50%, there is a problem that the elongation is insufficient and the formability is deteriorated. In addition, the remainder may be 50% or less as bainite and martensite. If the sum of the bainite and martensite exceeds 50%, there is a problem that the strength is too high and the elongation is insufficient.
[0040] Alternatively, according to one embodiment of the present invention, although not particularly limited thereto, from the viewpoint of improving elongation and formability, the microstructure of the high-strength cold-rolled steel sheet may contain, by area%, ferrite: 50 to 85% and the total of bainite and martensite: 15 to 50%.
[0041] If the ferrite content in the high-strength cold-rolled steel sheet exceeds 85%, a problem of not achieving a target strength may occur, and if the total content of the bainite and martensite is less than 15%, a problem of not achieving a target strength may occur. On the other hand, from the viewpoint of further improving the above-mentioned effects, the microstructure of the high-strength cold-rolled steel sheet more preferably contains, by area %, 66 to 75% ferrite.
[0042] According to one embodiment of the present invention, the microstructure of the high-strength cold-rolled steel sheet may contain, in area percent, 3 to 7% bainite and / or 19 to 31% martensite. If the bainite content in the high-strength cold-rolled steel sheet is less than 3%, a problem of not achieving a target strength may occur, and if it exceeds 7%, a problem of high strength but low elongation may occur. Alternatively, if the martensite content in the high-strength cold-rolled steel sheet is less than 19%, a problem of not achieving a target strength may occur, and if it exceeds 31%, a problem of high strength but low elongation may occur.
[0043] According to one aspect of the present invention, the high-strength cold-rolled steel sheet has an average number of surface defects that satisfy at least one of the conditions of a depth of 100 μm or more and a short side length of 1 mm or more of 10 defects / m 2 Less than (0 pieces / m 2 In measuring the average number of surface defects, the conditions of "depth of 100 μm or more" and "short side length of 1 mm or more" are merely criteria that are sufficient to measure the average number of surface defects. Therefore, in this specification, there are no particular limitations on the upper limits of the depth and short side length described above.
[0044] In the present invention, the surface defect means a defect having a groove shape, specifically, a defect that can be confirmed when the steel sheet surface is visually observed as a concave defect in the thickness direction. The depth of the surface defect may mean the "maximum depth" of the groove-shaped defect in the thickness direction based on the cross section in the thickness direction of the cold-rolled steel sheet (i.e., the direction perpendicular to the rolling direction based on the cross section). The short side length of the surface defect may mean the shortest length passing through the point of the maximum depth based on the surface of the cold-rolled steel sheet. Meanwhile, in order to observe the groove-shaped surface defects present on the surface of the above-mentioned steel sheet and confirm the depth and short side length of each surface defect, a photograph taken using a high-magnification scanning electron microscope (SEM) is shown in FIG. 2.
[0045] The present inventors have conducted extensive research in order to solve the problems of the conventional technology and provide a cold-rolled steel sheet that can minimize surface defects and material deviations while ensuring a desired level of strength and formability.
[0046] As a result, the average number of surface defects that satisfy one or more of the above conditions of a depth of 100 μm or more and a short side length of 1 mm or more was 10 defects / m 2 In other words, in the present invention, it has been found that the above-mentioned effects can be ensured by controlling the average number of the surface defects to be less than 10 / m. 2 If the average number of surface defects is more than 8 / m, a problem of surface dents may occur.2 It can be the following:
[0047] Meanwhile, according to one aspect of the present invention, the present inventors have conducted further research in order to provide a cold-rolled steel sheet that can simultaneously secure a desired level of strength and formability without affecting material deviation, etc., even if surface defects are present on the surface of the steel sheet. As a result, in the present invention, additional surface defect characteristics that do not affect material deviation, etc., even if surface defects are present, have been discovered. Specifically, although not particularly limited in the present invention, the maximum depth of the surface defects may satisfy 500 μm or less. In this case, the maximum depth of the surface defects may mean the maximum value of the depth of each surface defect present on the surface of the steel sheet.
[0048] Meanwhile, according to one aspect of the present invention, the difference in yield strength (YS) between both ends and the center in the width direction of the cold rolled steel sheet may be 100 MPa or less. By satisfying the requirement that the difference in yield strength between both ends and the center be 100 MPa or less, a steel sheet with reduced material deviation in the width direction can be provided, and the effect of uniform material in the width direction is achieved. In this case, the "both ends" refers to 30% sections (corresponding to a total of 60%) from both ends based on the entire width (referred to as 100%) of the cold rolled steel sheet in the width direction, and the "center" refers to the remaining 40% section excluding the both ends based on the entire width of the cold rolled steel sheet in the width direction.
[0049] Meanwhile, according to one aspect of the present invention, the cold-rolled steel sheet may have a tensile strength (TS) of 780 MPa or more, preferably 780 MPa or more and less than 1180 MPa, and more preferably 800 MPa or more and 1100 MPa or less. If the tensile strength of the cold-rolled steel sheet is less than 780 MPa, a problem may occur in which the target strength required for the applied part is not satisfied, and if it exceeds 1100 MPa, a problem may occur in which cracks are generated during part molding or the impact absorption resistance of the part is significantly reduced.
[0050] According to one embodiment of the present invention, the cold-rolled steel sheet may have a yield strength (YS) of 380 MPa or more, more preferably 390 MPa or more and 650 MPa or less. If the yield strength of the cold-rolled steel sheet is less than 380 MPa, a problem of deterioration in crash resistance of the part may occur, and if it exceeds 650 MPa, a problem of deterioration in formability may occur.
[0051] According to one embodiment of the present invention, the cold-rolled steel sheet may have a product of tensile strength and elongation of 12,000 MPa% or more (more preferably, 12,000 MPa% or more and 16,500 MPa% or less, and most preferably, 12,000 MPa% or more and 16,200 MPa% or less). By satisfying the above-mentioned physical properties, it is possible to ensure an effect that can be suitably applied to structural member parts such as fillers, which require a stable balance of strength-elongation and impact absorption properties among parts constituting an automobile body.
[0052] Although not particularly limited, the cold-rolled steel sheet may selectively further include a plating layer formed on the surface. In this case, the plating layer may be formed by a plating process described later. In addition, the composition of the plating layer may be differently applied depending on the purpose, and is not particularly limited in the present specification. An example of the plating layer is a zinc-based plating layer.
[0053] Hereinafter, a method for producing a high-strength cold-rolled steel sheet according to one embodiment of the present invention will be described in detail. However, it does not necessarily mean that the cold-rolled steel sheet according to the present invention needs to be produced by the following production method.
[0054] Steel slab reheating stage The steel slab satisfying the above-mentioned composition is reheated to 1100 to 1350°C. The composition of the steel slab is the same as that of the above-mentioned cold-rolled steel sheet, and the reasons for adding each component and limiting the content in the steel slab are the same as those for the above-mentioned cold-rolled steel sheet. On the other hand, if the reheating temperature of the steel slab is less than 1100°C, the segregated alloy elements in the center of the slab remain, and the starting temperature of hot rolling is too low, resulting in a problem of heavy rolling load. On the other hand, if the reheating temperature of the steel slab exceeds 1350°C, a problem of strength reduction due to coarsening of austenite grains occurs. Therefore, in the present invention, it is preferable to control the reheating temperature of the steel slab to 1100 to 1350°C.
[0055] Hot rolling stage The reheated steel slab is hot rolled at 850 to 1150°C. If the hot rolling temperature exceeds 1150°C, the temperature of the hot rolled steel sheet increases, the grain size becomes coarse, and the surface quality of the hot rolled steel sheet deteriorates. If the hot rolling temperature is less than 850°C, the load during rolling increases due to the development of elongated grains caused by excessive recrystallization delay, the temperature at both ends decreases significantly, and a non-uniform microstructure is formed during cooling, which increases material deviation and deteriorates formability.
[0056] Cooling stage after hot rolling The hot-rolled steel sheet is cooled to 450-700°C at an average cooling rate of 10-70°C / s (more preferably 20-50°C / s). If the cooling temperature of the hot-rolled steel sheet is less than 450°C, the problem of material deviation worsens, and if it exceeds 700°C, not only material deviation occurs but also internal oxidation occurs during hot rolling, resulting in surface defects. If the average cooling rate is less than 10°C / s, the crystal grains of the matrix structure become coarse, resulting in a problem of non-uniform microstructure. If the average cooling rate exceeds 70°C / s, the bainite phase and martensite phase are easily formed, resulting in a problem of increased load during cold rolling.
[0057] Winding stage The cooled steel sheet is wound at 450 to 700°C. If the steel sheet is cooled to a winding temperature of less than 450°C, the bainite and martensite phases in the steel are unnecessarily formed, resulting in an uneven shape and a large increase in rolling load during cold rolling. If the steel sheet is wound at a temperature exceeding 700°C, the ferrite grains become large, a coarse pearlite phase is easily formed, and an uneven microstructure is formed during annealing, resulting in a problem of deterioration in formability of the steel. Furthermore, the hot-rolled oxide increases and is adsorbed to the roll during annealing, leading to the oxide accumulation on the roll, which causes a problem of inducing surface defects such as dent defects on the surface of the steel sheet due to friction between the steel sheet and the roll during passing the steel sheet. In addition, if the hot-rolled oxide remains on the steel sheet, it causes deterioration in plating quality and plating adhesion during plating of the steel sheet.
[0058] Generally, after coiling, both ends in the width direction of the coiled steel sheet (coil) are exposed to the surrounding atmosphere and cooled quickly, while the center in the width direction is cooled slowly. As a result, a cooling deviation occurs in the width direction of the steel sheet from the coiling stage, which causes a difference in the microstructure depending on the position of the coiled steel sheet, and ultimately causes a material deviation in the hot-rolled steel sheet. In the case of a hot-rolled steel sheet having a large material deviation, not only does the material deviation deepen during cold rolling, but also groove-like surface defects that were not visually observed in the hot-rolled steel sheet deepen after cold rolling, resulting in a problem of significant surface defects. In other words, a hot-rolled steel sheet having a large material deviation not only has a poor shape during cold rolling, but also induces material deviation depending on the position in the width direction even in the final annealed material. As a result of intensive research to solve the above problem, the present inventors have devised a manufacturing method in which the temperatures of both ends and the center are controlled differently during the coiling stage.
[0059] Specifically, in the present invention, as a method for reducing the material deviation in the width direction of the steel sheet and suppressing surface defects, the surface temperature (Te) of both ends in the width direction is controlled to be 601 to 700°C and the surface temperature (Tc) of the central portion is controlled to be 450 to 600°C based on the entire width of the steel sheet during the coiling. In this case, the "width direction of the steel sheet" means a direction perpendicular to the transport direction of the steel sheet based on the surface of the steel sheet. The above explanation is similarly applied to both ends and the central portion.
[0060] If the Te is less than 601° C., there is a problem that the material deviation due to overcooling at both ends becomes severe, and if the Te exceeds 700° C., there is a problem that the material deviation and surface defects due to deterioration at the center become severe. Also, if the Tc is less than 450° C., there is a problem that the temperature difference between the center and both ends becomes large, and the material deviation becomes worse, and if the Tc exceeds 600° C., there is a problem that the temperature at the center is too high, causing material deviation and surface defects.
[0061] In this manner, in the above-mentioned coiling step, various methods can be applied to control the surface temperature of both ends and the surface temperature of the center of the steel sheet in the width direction to be different, and the method is not particularly limited. For example, in order to control the temperatures of both ends and the center of the steel sheet to be different during the coiling, the cooling water injected at both ends in the cooling step before coiling can be stopped before it reaches the steel sheet, the amount of cooling water injected can be controlled to be different, or the two methods can be used in parallel. As an example, according to one aspect of the present invention, in the cooling step before coiling, the amount of cooling water injected at the center excluding both ends can be controlled to be larger than the main amount of cooling water injected at both ends in the width direction based on the entire width of the steel sheet.
[0062] In addition, according to one aspect of the present invention, from the viewpoint of further reducing the material deviation and further improving the effect of suppressing surface defects, the winding step may be performed with a difference (Te-Tc) between the surface temperature at both ends and the surface temperature at the center being 150°C or less, although this is not particularly limited. In this case, if the value of Te-Tc exceeds 150°C, a problem may occur in that the material deviation in the width direction worsens. However, since the temperature deviation calculated from Te-Tc is preferably as small as possible, the lower limit may not be separately limited, and may be preferably 0°C. Meanwhile, more preferably, the lower limit of the value of Te-Tc may be 50°C, and the upper limit of the value of Te-Tc may be 90°C.
[0063] Heat retention cover maintenance stage After the above-mentioned coiling step, the steel sheet may be selectively moved into a heat-retaining cover and maintained at a temperature range of 400 to 500°C for 6 hours or more. By maintaining the steel sheet in the heat-retaining cover for a long time after the coiling step, the temperatures of both ends and the center of the steel sheet in the width direction are maintained at temperatures in the ranges of 601 to 700°C and 450 to 600°C, respectively, and a large amount of bainite structure is uniformly formed at both ends and the center over the entire length of the coil, so that a cold-rolled steel sheet having excellent shape quality, low rolling load during cold rolling, and uniform thickness can be produced.
[0064] During the stage of maintaining inside the heat-retaining cover, the surface temperature of the steel sheet can be adjusted to 400 to 500° C. If the surface temperature of the steel sheet is less than 400° C. during the stage of maintaining inside the heat-retaining cover, the above-mentioned effects cannot be ensured, and if it exceeds 500° C., coarse carbides are locally formed and hot-rolled oxides are increased, which may deteriorate the formability and surface quality of the steel.
[0065] Furthermore, if the maintenance time inside the heat-retaining cover is less than 6 hours, a problem of material deviation may occur. There is no upper limit to the maintenance time inside the heat-retaining cover, but it may be, for example, 8 hours or less.
[0066] Furthermore, in order to further improve the above-mentioned effects, the coiled steel sheet can be stored in the heat-insulating cover within 90 minutes immediately after coiling, and if the time before being stored in the heat-insulating cover exceeds 90 minutes, excessive air-cooling may occur in the central portion in the width direction, and the temperature may not satisfy the range of 450 to 600° C. Alternatively, after the step of maintaining inside the heat-insulating cover, air-cooling or water-cooling may be further performed to room temperature.
[0067] Cold rolling stage The coiled steel sheet is cold-rolled at a cold reduction of 40 to 70%. If the cold reduction is less than 40%, it is difficult to ensure the target thickness and also difficult to correct the shape of the steel sheet, whereas if it exceeds 70%, there is a high possibility that cracks will occur at the edge of the steel sheet, resulting in a load during cold rolling. Therefore, in the present invention, it is preferable to limit the cold reduction to 40 to 70%.
[0068] Annealing stage The cold-rolled steel sheet is continuously annealed at 740 to 900° C. If the annealing temperature is less than 740° C., the steel sheet may become non-recrystallized, resulting in a problem of not achieving the target strength and elongation, whereas if the annealing temperature exceeds 900° C., a problem of surface oxide generation may occur. On the other hand, from the viewpoint of further improving the above-mentioned effects, the annealing temperature is more preferably set to 750 to 850° C.
[0069] Furthermore, although not particularly limited, according to one embodiment of the present invention, the continuous annealing step may be followed by a primary cooling step to 650-700°C at a cooling rate of 1-10°C / sec; and the primary cooling step may be followed by a secondary cooling step to Ms-100°C to Ms+100°C at a cooling rate of 11-20°C / sec. In addition, the secondary cooling step may be followed by an overaging step while maintaining a constant temperature. By satisfying the conditions of the primary cooling step, the secondary cooling step, and the overaging step, the strength and elongation can be further improved. Here, Ms means the start temperature at which martensite is generated during cooling of the steel sheet after annealing, and can be calculated from the following Relation 2. [Equation 2] Ms=539-423×C-30.4×Mn-12.1×Cr-17.7×Ni-7.5×Mo (In the above Relational Formula 2, C, Mn, Cr, Ni, and Mo indicate the average content by weight of each element. In addition, when each of the above elements is not added, 0 is substituted.)
[0070] According to one embodiment of the present invention, the method may further include a step of selectively plating (preferably hot-dip galvanizing) the cold-rolled steel sheet, and a plated steel sheet can be obtained by carrying out the plating. EXAMPLES
[0071] The present invention will be described in more detail below with reference to examples. However, it should be noted that the following examples are merely for the purpose of illustrating the present invention, and are not intended to limit the scope of the present invention, since the scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred from the claims.
[0072] (Example) A steel slab satisfying the composition in Table 1 below was reheated at 1200°C, hot-rolled at 900°C, cooled to 450-700°C at a cooling rate of 20-50°C / s, and then coiled. At this time, the main amount of cooling water injected onto the center excluding both ends was controlled to be larger than the amount of cooling water injected onto both ends in the width direction of the steel sheet, so that the steel sheet surface temperature (Te) of both ends in the 30% section from both ends and the steel sheet surface temperature (Tc) of the remaining 40% in the center satisfy the hot rolling conditions listed in Table 2 below, based on the entire width of the steel sheet in the width direction. In addition, the coiled hot-rolled steel sheet was moved into a heat-retaining cover, and the average temperature and maintenance time before and after charging into the cover were controlled to satisfy the heat-retaining cover conditions listed in Table 2 below. Next, the hot-rolled steel sheet was cold rolled at a cold reduction rate of 50% and subjected to continuous annealing at 800°C. After that, it was primarily cooled to 670°C at an average cooling rate of 8°C / s, and then secondarily cooled to Ms+100°C at an average cooling rate of 12°C / s to obtain a cold-rolled steel sheet.
[0073] For each of the cold-rolled steel sheets thus obtained, the microstructure, mechanical properties, and average number of surface defects per unit area (number / m2) observed on the surface of the inventive and comparative examples were measured. 2 ) were measured and shown in Tables 3 to 5 below. Here, YS, TS, and El mean 0.2% off-set yield strength, tensile strength, and fracture elongation, respectively, and show the results of testing JIS No. 5 standard test pieces taken at the center and both ends in the direction perpendicular to the rolling direction. The above-mentioned microstructure was measured by area % in a photograph observed at 3,000 to 5,000 magnifications using a scanning electron microscope (FE-SEM). The average number of surface defects was measured by visually observing the surface of the manufactured steel sheet and measuring the average number of surface defects that satisfied one or more of the conditions of a depth of 100 μm or more and a short side length of 1 mm or more. In particular, the maximum depth for the above surface defects was measured in the same manner as described in this specification. The yield strength was measured in the same manner as described above for test pieces taken at the center and both ends in the width direction of the cold-rolled steel sheet, and the material deviation in the width direction for these was measured and shown in Tables 4 and 5 below.
[0074] [Table 1]
[0075] [Table 2]
[0076] [Table 3]
[0077] [Table 4]
[0078] [Table 5]
[0079] As can be seen from the experimental results in Tables 1 to 5, in the case of Examples 1 to 6 which satisfy the composition and manufacturing conditions of the present invention, a cold-rolled steel sheet was obtained in which the material deviation and surface defects were suppressed while a tensile strength (TS) of 780 MPa or more was ensured. At this time, it was confirmed that the maximum depth of the surface defects measured in the cold-rolled steel sheets obtained from Examples 1 to 6 of the present application satisfied 500 μm or less.
[0080] On the other hand, in the case of Comparative Examples 1 to 16 which do not satisfy one or more of the composition and manufacturing conditions of the present invention, the material deviation deteriorated, surface defects occurred, and / or it was difficult to secure the physical properties targeted by the present invention.
[0081] In particular, the amount of Si added in Comparative Steel 1 exceeded 2.0%, and thus the relational formula 1 was not satisfied. Therefore, in the case of Comparative Examples 13 and 14 using Comparative Steel 1, although the manufacturing conditions proposed by the present invention were satisfied and the material deviation was good, there was a problem that the accumulation of Si oxides in the annealing furnace caused dent problems and the average number of defects on the product surface exceeded the target value.
[0082] In addition, Comparative Steel 2 had a small amount of alloy added and therefore did not satisfy Relation 1. Therefore, in the case of Comparative Examples 15 and 16 using Comparative Steel 2, even though the manufacturing conditions proposed by the present invention were met and the surface defects and material deviation were good, the tensile strength was less than 780 MPa and the target material properties were not satisfied.
[0083] In addition, Comparative Examples 1, 5, and 9 are examples in which the temperatures at both ends and the center in the width direction were higher than the temperature proposed in the present invention, and Comparative Examples 4, 8, and 12 are examples in which the temperature of the heat retention cover exceeded the reference temperature. As a result, in the comparative examples, hot rolling oxides were generated in an excessive amount, and the oxides caused a large number of surface defects in the final steel sheet.
[0084] In addition, Comparative Examples 2, 6, and 10 show examples in which the temperatures at both ends and the center in the width direction were lower than the temperatures proposed in the present invention, and the difference (Te-Tc) between the surface temperatures at both ends and the center exceeded 150°C, and Comparative Examples 3, 7, and 11 show examples in which a heat-retaining cover was not applied. As a result, the above comparative examples were able to ensure the target material properties of the annealed steel sheet, and the average number of surface defects was good, but there was a problem in that the deviation in the yield strength in the width direction of the annealed steel sheet exceeded the target value of 100 MPa.
Claims
1. In weight percent, C: 0.05-0.3%, Si: 0.01-2.0%, Mn: 1.5-3.0%, Al: 0.01-0.1%, P: 0.001-0.015%, S: 0.001-0.01%, N: 0.001-0.01%, the balance being Fe and other unavoidable impurities, The value defined by the following relational expression 1 satisfies 0.6 or more and less than 0.9, The microstructure contains, in terms of area percentage, ferrite: 50% or more, and the remainder: bainite and martensite, The average number of surface defects that satisfy one or more of the following conditions: depth 100 μm or more and short side length 1 mm or more is 10 / m 2 Less than 100% high strength cold rolled steel. [Relationship 1] C+(1.3×Si+Mn) / 6+(Cr+1.2×Mo) / 5+100×B (In the above Relational Formula 1, C, Si, Mn, Cr, Mo and B indicate the weight percent average content of each element. In addition, when each element is not added, 0 is substituted.)
2. The high-strength cold-rolled steel sheet according to claim 1, wherein the microstructure contains, in area percentage, ferrite: 50 to 85% and a total of bainite and martensite: 15 to 50%.
3. The high-strength cold-rolled steel sheet according to claim 1, wherein the microstructure contains, in terms of area percentage, ferrite: 66 to 75%.
4. The high-strength cold-rolled steel sheet according to claim 3, wherein the microstructure contains, in area%, bainite: 3 to 7%.
5. The high-strength cold-rolled steel sheet according to claim 3, wherein the microstructure contains, by area%, 19 to 31% martensite.
6. The high strength cold rolled steel sheet according to claim 1, further comprising at least one selected from the group consisting of Cr: 1.0% or less (including 0%), Mo: 0.2% or less (including 0%), and B: 0.005% or less (including 0%), by weight%.
7. The high strength cold rolled steel sheet according to claim 1, having a tensile strength of 780 MPa or more and a yield strength of 380 MPa or more.
8. The high strength cold rolled steel sheet according to claim 1, wherein the product of tensile strength and elongation is 12,000 MPa% or more.
9. The high-strength cold-rolled steel sheet according to claim 1, wherein a difference in yield strength between both ends and a center portion in a width direction of the cold-rolled steel sheet is 100 MPa or less.
10. a step of reheating a steel slab containing, in weight percent, C: 0.05-0.3%, Si: 0.01-2.0%, Mn: 1.5-3.0%, Al: 0.01-0.1%, P: 0.001-0.015%, S: 0.001-0.01%, N: 0.001-0.01%, the balance being Fe and other inevitable impurities, and satisfying a value defined by the following Relational Formula 1 of 0.6 or more and less than 0.9, to 1100-1350°C; hot rolling the reheated steel slab at 850-1150°C; cooling the hot-rolled steel sheet to 450 to 700° C. at an average cooling rate of 10 to 70° C. / s; coiling the cooled steel sheet at 450 to 700°C; cold rolling the coiled steel sheet at a rolling reduction of 40 to 70%; and The cold-rolled steel sheet is continuously annealed at 740 to 900°C; The coiling step is performed by controlling the surface temperature (Te) of both ends in the width direction to be 601 to 700°C and the surface temperature (Tc) of the center portion to be 450 to 600°C based on the entire width of the steel sheet. [Relationship 1] C+(1.3×Si+Mn) / 6+(Cr+1.2×Mo) / 5+100×B (In the above Relational Formula 1, C, Si, Mn, Cr, Mo and B indicate the weight percent average content of each element. In addition, when each element is not added, 0 is substituted.)
11. The method for producing a high strength cold rolled steel sheet according to claim 10, further comprising the steps of: moving the wound steel sheet into a heat retention cover and maintaining the steel sheet at a temperature in the range of 400 to 500° C. for 6 hours or more after the winding step.
12. The method for producing a high strength cold rolled steel sheet according to claim 10, wherein the coiling step is controlled so that a difference (Te-Tc) between the surface temperature of both ends and the surface temperature of the center portion is 150°C or less.
13. 11. The method for manufacturing a high strength cold rolled steel sheet according to claim 10, wherein the cooling step is controlled so that an amount of cooling water injected into a center portion excluding both ends in a width direction based on an entire width of the steel sheet is greater than an amount of cooling water injected into both ends in the width direction.
Citation Information
Patent Citations
High-strength galvannealed steel sheet excellent in workability and fatigue resistance, and method of producing the same
JP2011001579A
Cold rolled steel sheet and method for producing the same
JP2013221198A
High-strength cold-rolled steel plate with minimized dispersion of mechanical characteristics, and method for manufacturing the same
JP2013249501A
HIGH STRENGTH STEEL SHEET, HIGH STRENGTH HOT-DIP GALVANIZED STEEL SHEET, AND HIGH STRENGTH HOT-DIP GALVANNEALED STEEL SHEET EACH HAVING MAXIMUM TENSILE STRENGTH OF 780 MPa AND EXCELLENT IN COLLISION CHARACTERISTIC, AND PRODUCTION METHODS OF THEM
JP2015175061A
High strength steel sheet excellent in formability and production method therefor
JP2016216808A
Cited By
Batch annealing method for steel sheet coil, and cold-rolled steel sheet
WO2026078986A1