High-strength thick steel plate with excellent hole expandability and ductility and its manufacturing method
A high-strength thick steel plate with a controlled microstructure and thermal processing addresses moldability and crack issues by ensuring high strength and formability, improving crash resistance and suitability for complex automobile parts.
Patent Information
- Application Number
- JP2024518912
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-27
- Filing Date
- 2022-09-21
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-09-21
AI Technical Summary
High-strength steels used in automobile structural members face challenges with decreased elongation rates and formability as strength increases, leading to moldability issues and increased manufacturing costs, along with potential cracks during processing due to low hole expandability, which compromises safety and durability.
A high-strength thick steel plate with a microstructure of 10-30% ferrite, 10-25% recrystallized ferrite bridge, 20-30% bainite, and balance martensite, manufactured through specific alloy composition and thermal processing, including controlled heating, hot rolling, cold rolling, and continuous annealing, to form recrystallized ferrite bridges connecting hard phases and eliminating unidirectionality.
The steel plate achieves high strength, excellent hole expandability, and improved formability, preventing processing defects like cracks and wrinkles, enhancing crash resistance and suitability for complex-shaped structural parts.
Smart Images

Figure 2024535916000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel suitable as a material for automobiles, and more particularly to a high-strength thick steel plate having excellent hole expandability and ductility, and a method for producing the same. [Background technology]
[0002] Recently, in the field of the automobile industry, the use of high-strength steel is required to improve fuel efficiency and durability due to environmental regulations on CO2 emissions and regulations on energy use.
[0003] In particular, as regulations regarding the impact stability of automobiles become more stringent, high-strength steel, which has excellent strength, is being used as a material for structural members such as members, seat rails, pillars, etc. to improve the impact resistance of the vehicle body.
[0004] Such automobile parts have complex shapes according to stability and design, and are mainly manufactured by forming using press dies, so they require a high level of formability as well as high strength.
[0005] However, while the higher the strength of steel, the better it is at absorbing impact energy, there is a problem that, in general, as the strength increases, the elongation decreases, and formability decreases. Furthermore, if the yield strength is excessively high, the flow of the material into the die during forming decreases, resulting in a decrease in formability and an increase in manufacturing costs.
[0006] In addition, since automotive parts have many formed areas that expand after holes are drilled, hole expandability (HER) is required for smooth forming, but high-strength steel has low hole expandability, which causes defects such as cracks during forming. If hole expandability decreases in this way, cracks may occur in the formed parts of the parts in the event of a car collision, making the parts more likely to be destroyed, threatening the safety of passengers. In addition, as standards for passenger safety become higher, the adoption of thicker materials to ensure rigidity is steadily increasing, especially among some automakers.
[0007] On the other hand, typical examples of high-strength steels used in automotive materials include dual phase steel (DP steel), transformation induced plasticity steel (TRIP steel), complex phase steel (CP steel), and ferrite bainite steel (FB steel).
[0008] DP steel, which is an ultra-high tensile steel, has a low yield ratio of about 0.5 to 0.6, making it easy to process, and has the advantage of having the second highest elongation rate after TRIP steel. Therefore, it is mainly used in door outers, seat rails, seat belts, suspensions, arms, wheel discs, etc.
[0009] TRIP steel has a yield ratio in the range of 0.57 to 0.67 and is therefore characterized by excellent formability (high ductility), making it suitable for parts that require high formability, such as members, loops, seat belts, bumper rails, etc.
[0010] CP steel has a low yield ratio as well as high elongation and bending workability, making it suitable for use in side panels and underbody reinforcements, while FB steel has excellent hole expansion properties and is therefore primarily used in suspension lower arms and wheel discs.
[0011] Among them, DP steel is mainly composed of ferrite with excellent ductility and hard phases (martensite phase, bainite phase) with high strength, and may contain a small amount of retained austenite. Such DP steel has low yield strength and high tensile strength, so it has a low yield ratio (YR), high work hardening rate, high ductility, continuous yield behavior, room temperature aging resistance, bake hardenability, etc. In addition, by controlling the fraction, recrystallization degree, and distribution uniformity of each phase, it can be manufactured as a high-strength steel with high hole expandability.
[0012] However, in order to secure ultra-high strength of tensile strength of 980 MPa or more, the fraction of hard phases such as martensite, which is advantageous for improving strength, must be increased. However, in this case, the yield strength increases, which causes defects such as cracks during press forming.
[0013] Generally, DP steel for automobiles is manufactured by producing slabs through the steelmaking and continuous casting processes, and then these slabs are heated, roughly rolled, and finished hot rolled to obtain hot-rolled coils, which are then annealed to produce the final product.
[0014] Here, the annealing process is a process that is mainly carried out during the manufacture of cold-rolled steel sheets. Cold-rolled steel sheets are manufactured by removing surface scale by acid washing a hot-rolled coil, cold-rolling the hot-rolled coil at a certain rolling reduction at room temperature, and then carrying out an annealing process and, if necessary, a further temper rolling process.
[0015] The cold-rolled steel sheet (cold-rolled material) obtained by cold rolling is itself in a very hard state and is unsuitable for manufacturing parts that require workability. Therefore, in a subsequent process, the cold-rolled steel sheet is softened by heat treatment in a continuous annealing furnace to improve its workability.
[0016] For example, the annealing process involves heating a steel sheet (cold-rolled material) to about 650 to 850°C in a heating furnace and maintaining the temperature for a certain period of time, thereby reducing the hardness and improving workability through recrystallization and phase transformation phenomena.
[0017] Steel sheets that have not undergone an annealing process have high hardness, particularly surface hardness, and lack workability, whereas steel sheets that have undergone an annealing process have a recrystallized structure, which reduces hardness, yield point, and tensile strength, thereby improving workability.
[0018] A representative method for reducing the yield strength of DP steel is to completely recrystallize ferrite in the heating process during continuous annealing to produce an equiaxed crystal form, so that the austenite is generated and grown in the subsequent process in an equiaxed crystal form, thereby forming a uniform austenite phase with a small grain size.
[0019] In addition, in the case of thick materials, the hot-rolled thickness must be relatively thick to ensure a certain rolling reduction, which causes a large load during the subsequent cold rolling, resulting in a problem of reduced operability. If the rolling reduction is low when manufacturing thick materials, the degree of non-uniformity of the structure increases due to non-recrystallization of ferrite during annealing, resulting in high yield strength, and the directionality of the cold rolling is maintained in a fine structure, resulting in a problem of reduced workability. Therefore, in the case of thick materials, the material variation in the thickness direction is inevitably large due to the dimensional characteristics, so a technology for homogenizing the material as much as possible is required to improve workability and usable physical properties.
[0020] On the other hand, Patent Document 1 discloses that hole expandability and elongation can be ensured by forming fine precipitates using Ti, Mo, etc. and configuring a microstructure from ferrite, bainite, and martensite phases.
[0021] However, this document has problems with weldability and liquid metal embrittlement (LME) due to the excessive addition of carbon for forming fine precipitates and silicon for introducing bainite. In addition, problems still remain due to the difference in hardness between the soft and hard phases, and the bainite phase is formed in an excessive fraction for high hole expandability, resulting in high yield strength, difficulty in processing, and poor elongation.
[0022] In view of the above-mentioned conventional techniques, in order to simultaneously improve formability such as elongation and hole expandability of thick high-strength steel, it is necessary to develop a method that can form a uniform structure within the steel while lowering the yield strength and improving the workability. [Prior art documents] [Patent documents]
[0023] [Patent Document 1] Korean Patent Publication No. 10-2021-0095156 Summary of the Invention [Problem to be solved by the invention]
[0024] One aspect of the present invention is to provide a high-strength thick steel plate having a low yield ratio, high strength, and excellent formability such as hole expandability due to improved ductility as a material suitable for automobile structural members, etc., and a method for producing the same.
[0025] The object of the present invention is not limited to the above. The object of the present invention can be understood from the entire contents of this specification, and a person having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding further object of the present invention. [Means for solving the problem]
[0026] One embodiment of the present invention contains, by weight percent, carbon (C): 0.05 to 0.12%, manganese (Mn): 2.0 to 3.0%, silicon (Si): 0.5% or less (excluding 0%), chromium (Cr): 1.0% or less (excluding 0%), niobium (Nb): 0.1% or less (excluding 0%), titanium (Ti): 0.1% or less (excluding 0%), boron (B): 0.003% or less (excluding 0%), aluminum (sol.Al): 0.02 to 0.05%, phosphorus (P): 0.05% or less (excluding 0%), sulfur (S): 0.01% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), iron (Fe) and other inevitable impurities, The present invention provides a high-strength thick steel plate having excellent hole expandability and ductility, the microstructure of which includes 10-30% area fraction of ferrite, 10-25% area fraction of recrystallized ferrite bridges, 20-30% area fraction of bainite, and the remainder martensite.
[0027] Another aspect of the present invention includes the steps of preparing a steel slab, heating the steel slab in a temperature range of 1100 to 1300 ° C., hot rolling the heated steel slab to produce a hot-rolled steel sheet, coiling the hot-rolled steel sheet in a temperature range of 400 to 700 ° C., and cooling the hot-rolled steel sheet to room temperature after the coiling, cold rolling the cooled hot-rolled steel sheet at a cold reduction of 55 to 80% to produce a cold-rolled steel sheet, subjecting the cold-rolled steel sheet to continuous annealing, performing primary cooling at an average cooling rate of 1 to 10 ° C. / s to a temperature range of 650 to 700 ° C. after the continuous annealing, and performing secondary cooling at an average cooling rate of 5 to 50 ° C. / s to a temperature range of 450 to 500 ° C. after the primary cooling, The continuous annealing is carried out in equipment equipped with a heating zone, a soaking zone, and a cooling zone, and the cold-rolled steel sheet passes through a recrystallization zone in which the temperature is maintained at 600 to 700°C for 1 to 3 minutes when the cold-rolled steel sheet is raised to the heating zone. This is a method for producing a high-strength thick steel sheet having excellent hole expandability and ductility. Effect of the Invention
[0028] According to the present invention, it is possible to provide a thick steel plate having excellent hole expansibility, formability, and impact resistance despite having high strength.
[0029] The steel sheet of the present invention, which has improved formability, can prevent processing defects such as cracks or wrinkles during press forming, and is therefore suitable for use in structural parts that require processing into complex shapes. Furthermore, it is also effective in producing materials with improved crash resistance so that defects such as cracks are less likely to occur when an automobile using such parts inevitably crashes. [Brief description of the drawings]
[0030] [Figure 1]1 shows the thermal history and phase transformation history during continuous annealing according to one embodiment of the present invention. In Fig. 1, the dashed line shows the thermal history during conventional continuous annealing, and the solid line shows the thermal history during continuous annealing according to the present invention. [Diagram 2] 1A shows the mechanism of void formation within the structure, and FIG. 1B shows the mechanism of interface reinforcement within the structure in an example of the invention according to one embodiment of the present invention. [Diagram 3] 1 shows a microstructure photograph of a comparative example according to an embodiment of the present invention. [Figure 4] 4 shows a microstructure photograph of an example of the present invention according to one embodiment of the present invention (the arrows in FIG. 4 represent recrystallized ferrite bridge structures). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The inventors of the present invention have conducted extensive research in order to develop a material having a level of formability suitable for use in automotive components that require processing into complex shapes.
[0032] In particular, the inventors have derived a microstructural structure capable of increasing the crack resistance between hard phases in thick steel plates for automobiles, which necessitate a relatively low cold rolling reduction ratio, and have confirmed that the target conditions can be achieved by refining the hard phases and controlling the crystal grain shape, which are advantageous in preventing the generation and propagation of voids, and have thus completed the present invention.
[0033] In particular, the present invention has a technical significance in that a recrystallized ferrite bridge having a structure that connects the hard phases to each other so as to eliminate the unidirectionality of the hard phases is introduced, and in forming such a structure, the alloy composition and manufacturing conditions are optimized.
[0034] The present invention will be described in detail below.
[0035] A high-strength thick steel plate having excellent hole expandability and ductility according to one embodiment of the present invention can contain, by weight percent, carbon (C): 0.05 to 0.12%, manganese (Mn): 2.0 to 3.0%, silicon (Si): 0.5% or less (excluding 0%), chromium (Cr): 1.0% or less (excluding 0%), niobium (Nb): 0.1% or less (excluding 0%), titanium (Ti): 0.1% or less (excluding 0%), boron (B): 0.003% or less (excluding 0%), aluminum (sol.Al): 0.02 to 0.05%, phosphorus (P): 0.05% or less (excluding 0%), sulfur (S): 0.01% or less (excluding 0%), and nitrogen (N): 0.01% or less (excluding 0%).
[0036] The reasons for restricting the alloy composition of the high strength thick steel plate provided by the present invention as described above will be described in detail below.
[0037] Meanwhile, unless otherwise specified in the present invention, the content of each element is based on weight, and the proportion of the structure is based on area.
[0038] Carbon (C): 0.05~0.12% Carbon (C) is an important element that is added for solid solution strengthening. Such C combines with precipitated elements to form fine precipitates, thereby contributing to improving the strength of steel.
[0039] If the C content exceeds 0.12%, the hardening ability increases, and when manufacturing the steel, martensite is formed during cooling, which causes an excessive increase in strength, but also a decrease in elongation. In addition, the weldability is poor, and there is a risk of welding defects occurring during processing into parts. On the other hand, if the C content is less than 0.05%, it becomes difficult to ensure the target level of strength.
[0040] Therefore, the C content can be 0.05 to 0.12%, more preferably 0.06% or more and 0.10% or less.
[0041] Manganese (Mn): 2.0-3.0% Manganese (Mn) is an element that precipitates sulfur (S) in steel as MnS, prevents hot embrittlement due to the formation of FeS, and is advantageous for solid solution strengthening of steel.
[0042] If the Mn content is less than 2.0%, not only are the above-mentioned effects not obtained, but it is also difficult to ensure the target level of strength. On the other hand, if the Mn content exceeds 3.0%, there is a high possibility that problems with weldability, hot rolling, etc. will occur, and martensite will be formed more easily due to the increased hardenability, which may result in a decrease in ductility. In addition, there is a problem that Mn-Bands (Mn oxide bands) are excessively formed in the structure, increasing the risk of defects such as processing cracks. And there is a problem that Mn oxides dissolve onto the surface during annealing, greatly impairing platability.
[0043] Therefore, the Mn content can be 2.0 to 3.0%, and more advantageously, 2.2% or more and 2.8% or less.
[0044] Silicon (Si): 0.5% or less (excluding 0%) Silicon (Si) is a ferrite stabilizing element, which is advantageous in promoting ferrite transformation and ensuring a target level of ferrite fraction. It also has good solid solution strengthening ability, is effective in increasing the strength of ferrite, and is a useful element in ensuring strength without reducing the ductility of steel.
[0045] If the Si content exceeds 0.5%, the solid solution strengthening effect becomes excessive, and the ductility decreases, and surface scale defects are induced, adversely affecting the surface quality of the plating. In addition, there is a problem that the chemical conversion treatability is impaired.
[0046] Therefore, the Si content may be 0.5% or less, 0% may be excluded, and more preferably 0.1% or more.
[0047] Chromium (Cr): 1.0% or less (excluding 0%) Chromium (Cr) is an element that exerts a hardening effect during cooling, facilitating the formation of the bainite phase and suppressing the formation of the martensite phase during annealing heat treatment, while forming fine carbides, contributing to improving strength.
[0048] In addition, in the present invention, the Cr content is adjusted to an appropriate level, so that the Cr content acts as a ferrite stabilizing element during heating to delay the austenite phase transformation reaction, while the phase transformation starts at a higher temperature, so that the steel remains in the region (Trex to A1) where only recrystallization occurs during heating for a long time, thereby ensuring a recrystallized ferrite bridge structure.
[0049] If the Cr content exceeds 1.0%, the intended recrystallized ferrite bridge is not formed, the ductility and hole expandability of the steel are reduced, and if carbides are formed at the grain boundaries, the strength and elongation may be deteriorated. In addition, there is a problem that the manufacturing cost increases.
[0050] Therefore, the Cr content may be 1.0% or less, 0% may be excluded, and more preferably, 0.01% or more.
[0051] Niobium (Nb): 0.1% or less (excluding 0%) Niobium (Nb) is an element that segregates at the austenite grain boundaries, suppresses the coarsening of austenite crystal grains during annealing heat treatment, and forms fine carbides, thereby contributing to improving strength.
[0052] If the Nb content exceeds 0.1%, coarse carbides precipitate, and the carbon content in the steel is reduced, which may result in poor strength and elongation, and increases the production costs.
[0053] Therefore, the Nb content can be 0.1% or less, and 0% can be excluded.
[0054] Titanium (Ti): 0.1% or less (excluding 0%) Titanium (Ti) is an element that forms fine carbides and contributes to ensuring yield strength and tensile strength. In addition, Ti precipitates N in steel as TiN and inhibits the formation of AlN from Al that is inevitably present in steel, thereby reducing the possibility of cracks occurring during continuous casting.
[0055] If the Ti content exceeds 0.1%, coarse carbides are precipitated, and the strength and elongation may decrease due to the reduction in the carbon content in the steel. In addition, nozzle clogging may occur during continuous casting, resulting in an increase in production costs.
[0056] Therefore, the Ti content can be 0.1% or less, and 0% can be excluded.
[0057] Boron (B): 0.003% or less (excluding 0%) Boron (B) is an element that delays the transformation of austenite into pearlite during the cooling process after annealing heat treatment. However, if the B content exceeds 0.003%, B will be excessively concentrated on the surface, which may lead to a deterioration of plating adhesion.
[0058] Therefore, the above B can be contained in an amount of 0.003% or less, and 0% can be excluded in consideration of the level of unavoidable addition.
[0059] Aluminum (sol.Al): 0.02~0.05% Aluminum (sol.Al) is an element added to steel for grain refinement and deoxidation, and if its content is less than 0.02%, aluminum-killed steel cannot be manufactured in a stable state. On the other hand, if its content exceeds 0.05%, the grains are refined and strength is improved, but excessive formation of inclusions during continuous casting of steel increases the risk of surface defects on plated steel sheets.
[0060] Therefore, the sol. Al content can be 0.02 to 0.05%.
[0061] Phosphorus (P): 0.05% or less (excluding 0%) Phosphorus (P) is a substitutional element with the greatest solid solution strengthening effect, and is an advantageous element for improving in-plane anisotropy and ensuring strength without significantly reducing formability. However, when P is added in excess, there are problems in that the possibility of brittle fracture increases significantly, the possibility of slab breakage during hot rolling increases, and the coating surface properties are impaired.
[0062] Therefore, in the present invention, the P content can be controlled to 0.05% or less, and 0% can be excluded in consideration of the unavoidable added level.
[0063] Sulfur (S): 0.01% or less (excluding 0%) Sulfur (S) is an element that is inevitably added as an impurity element in steel, and since it impairs ductility, it is preferable to control its content as low as possible. In particular, since S has the problem of increasing the possibility of generating red shortness, it is preferable to control its content to 0.01% or less. However, 0% can be excluded in consideration of the level of S that is inevitably added during the manufacturing process.
[0064] Nitrogen (N): 0.01% or less (excluding 0%) Nitrogen (N) is a solid solution strengthening element. If its content exceeds 0.01%, there is a high risk of embrittlement and it bonds with Al in the steel to precipitate excessive AlN, which may impair the quality of continuous casting.
[0065] Therefore, the above N can be contained at 0.01% or less, and 0% can be excluded taking into consideration the level of unavoidable addition.
[0066] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, there is a possibility that unintended impurities are inevitably mixed in from the raw materials or the surrounding environment, and this cannot be excluded. Since these impurities are known to any technician in a normal manufacturing process, the entire contents of them will not be mentioned in this specification.
[0067] The steel sheet of the present invention having the above-mentioned alloy composition may have a microstructure including ferrite, which is a soft phase, and bainite and martensite, which are hard phases, as well as a recrystallized ferrite bridge structure formed by connecting the hard phases.
[0068] In the present invention, the most significant change in the microstructure due to the formation of recrystallized ferrite bridges is the disappearance of the rolling direction of existing ferrite and the degree of connection around the hard phase is large. In addition, due to the formation of recrystallized ferrite bridges during heating, the number of positions where reverse transformed austenite is formed is reduced, the formation of austenite at high temperatures is delayed, and a smaller size secondary phase can be formed after cooling. The unrecrystallized ferrite region is an elongated structure with rolling directionality and remains as an irregular rough interface, while the recrystallized ferrite bridge grain boundary has a smooth polygonal interface. The method of determining the recrystallized ferrite bridges can be, for example, classified by EBSD crystal orientation (electron backscatter diffraction orientation), or optically classified by etching with a hydrogen peroxide solution (e.g., 140 ml of distilled water, 100 ml of hydrogen peroxide, 4 g of oxalic acid, 2 ml of sulfuric acid, and 1.5 ml of hydrofluoric acid).
[0069] Specifically, the steel sheet of the present invention contains a ferrite phase at an area fraction of 10 to 30%, a recrystallized ferrite bridge phase at an area fraction of 10 to 25%, and a hard phase of bainite at 20 to 30% and a residual martensite phase, and may further contain a small amount of retained austenite phase.
[0070] In the present invention, the recrystallized ferrite bridge phase is a structure that is advantageous in suppressing the propagation of voids that occur along the grain boundaries of the hard phase by eliminating the unidirectionality of the hard phase, and is a structure that is distinct from existing polygonal ferrite.
[0071] The recrystallized ferrite bridge is a structure distinct from general recrystallized ferrite, and is relatively coarse, preferably having an average size of 1 to 6 μm based on the equivalent circular diameter. If the size of the recrystallized ferrite bridge phase is less than 1 μm, it is difficult to eliminate the orientation of the hard phase, and the intended effect cannot be obtained. On the other hand, if the size exceeds 6 μm, the structure becomes excessively coarse, and physical properties such as strength may be impaired.
[0072] As shown in Figure 2, when the hard phase is formed to have directionality (a), voids formed along the grain boundaries are easily connected, which favors the propagation of cracks. On the other hand, when the structure intended in the present invention (b), particularly the recrystallized ferrite bridge phase, is formed as a structure that connects the hard phases to each other while removing the unidirectionality of the hard phase, voids are less likely to coalesce along the grain boundaries, which results in an effect of greatly suppressing the occurrence and propagation of cracks.
[0073] If the fraction of such recrystallized ferrite bridge phase is too high, the fraction of the hard phase will be relatively low, and the target level of strength will not be ensured. In consideration of this, the recrystallized ferrite bridge phase can be contained at 25% or less. On the other hand, if the fraction is less than 10%, the above-mentioned effects (elimination of the unidirectionality of the hard phase and suppression of void propagation, etc.) cannot be sufficiently obtained, and the hole expandability will be poor.
[0074] That is, the present invention has a technical significance in that a recrystallized ferrite bridge phase is introduced in addition to the soft ferrite phase and the hard bainite and martensite phases, and the shape and distribution of the recrystallized ferrite bridge phase are controlled to further improve formability.
[0075] If the proportion of the ferrite phase is less than 10%, it is disadvantageous in ensuring the ductility of the steel. On the other hand, if the proportion exceeds 30%, the proportion of the hard phase becomes relatively low, making it difficult to ensure the target level of strength.
[0076] If the bainite phase fraction is less than 20%, not only is it difficult to ensure strength, but there is also a problem that the difference in hardness between the soft phase and the martensite phase becomes large, whereas if the fraction exceeds 30%, the fraction of the soft phase becomes low, making it difficult to ensure ductility.
[0077] The martensite phase, which is one of the structures excluding the ferrite phase, recrystallized ferrite bridge phase, and bainite phase, is not specifically limited in its fraction, but may contain an area fraction of 15% or more in order to ensure ultra-high strength of tensile strength of 980 MPa or more. However, if the fraction of the martensite phase exceeds 60%, the ductility decreases, making it difficult to ensure the desired level of formability.
[0078] On the other hand, it is clear that it is advantageous for the fraction of the above-mentioned retained austenite phase not to exceed 3%, and that even if it is 0%, it is not difficult to ensure the intended physical properties.
[0079] The high-strength thick steel plate of the present invention having the above-mentioned microstructure has a tensile strength of 980 MPa or more, a yield strength of 550 to 700 MPa, and an elongation (total elongation) of 14% or more, and can have high strength as well as high ductility properties.
[0080] Furthermore, the above steel sheet has a hole expansion ratio (HER) of 30% or more, and thus has the effect of being excellent in resistance to cracks that may occur during processing and in resistance to impact fracture.
[0081] The high strength thick steel plate of the present invention may have a thickness of 1 to 3 mm, and more preferably a thickness of 1.5 to 2.5 mm.
[0082] Hereinafter, a method for producing a high-strength thick steel plate having excellent hole expandability and ductility according to another aspect of the present invention will be described in detail.
[0083] In short, the present invention can produce the desired steel sheet through the steps of [steel slab heating - hot rolling - coiling - cold rolling - continuous annealing], and each step will be described in detail below.
[0084] [Steel slab heating] First, a steel slab satisfying the above-mentioned alloy composition can be prepared and then heated.
[0085] This process is carried out in order to smoothly carry out the subsequent hot rolling process and to sufficiently obtain the target physical properties of the steel sheet. In the present invention, the conditions of such a heating process are not particularly limited, and normal conditions may be used. As an example, the heating process can be carried out in a temperature range of 1100 to 1300°C.
[0086] [Hot rolling] The steel slab heated as described above can be hot rolled to produce a hot rolled steel sheet, and at this time, finish hot rolling can be performed at an outlet side temperature of Ar3 or more and 1000°C or less.
[0087] If the exit temperature during the finish hot rolling is less than Ar3, the hot deformation resistance increases rapidly, the top, tail and edges of the hot rolled coil become single-phase regions, and the in-plane anisotropy increases, which may deteriorate the formability. On the other hand, if the temperature exceeds 1000°C, the rolling load decreases relatively, which is advantageous for productivity, but there is a risk of thick oxide scale being generated.
[0088] More specifically, the finish hot rolling can be carried out in the temperature range of 760 to 940°C.
[0089] [Winding] The hot-rolled steel sheet produced as described above can be wound into a coil.
[0090] The coiling can be performed at a temperature range of 400 to 700°C. If the coiling temperature is less than 400°C, martensite or recrystallized ferrite bridge phase is excessively formed, which leads to an excessive increase in strength of the hot-rolled steel sheet, and problems such as defective shape due to load during subsequent cold rolling may occur. On the other hand, if the coiling temperature exceeds 700°C, there is a problem that surface scale increases and pickling properties deteriorate.
[0091] [cooling] It is preferable that the coiled hot-rolled steel sheet is cooled to room temperature at an average cooling rate of 0.1° C. / s or less (excluding 0° C. / s). In this case, the coiled hot-rolled steel sheet may be cooled after undergoing processes such as transportation and stacking, but it is clear that the process before cooling is not limited thereto.
[0092] In this manner, by cooling the coiled hot-rolled steel sheet at a constant speed, it is possible to obtain a hot-rolled steel sheet in which carbides that serve as austenite nucleation sites are finely dispersed.
[0093] [Cold rolling] The coiled hot-rolled steel sheet can be cold-rolled to produce a cold-rolled steel sheet, and the cold rolling in the present invention can be performed at a cold reduction rate of 55 to 80%.
[0094] The present invention can further promote the recrystallization of ferrite in the heating section of the subsequent continuous annealing process while applying an appropriate cold reduction rate during cold rolling, thereby inducing the formation of fine ferrite and allowing the austenite formed at the ferrite grain boundaries to be small and uniform.
[0095] If the reduction rate during the cold rolling is less than 55%, ferrite recrystallization is delayed, making it difficult to obtain a fine and uniform austenite phase. On the other hand, if it exceeds 80%, excessive recrystallization reduces the yield strength too much, making it impossible to ensure the target level of strength. More preferably, the reduction rate can be 78% or less.
[0096] In the present invention, the cold rolling reduction can be achieved not only from a hot-rolled thick material having a certain thickness with a high rolling capacity (e.g., 5000KN / mm level) of ZRM equipment, but also includes a process of achieving a target rolling reduction by repeated rolling using a reversing mill. As a non-limiting example, the hot-rolled thick material may have a thickness of 4 to 8 mm, and it is clear that a cold rolling process using a reversing mill can be performed when the thickness of the hot-rolled thick material is 6 mm or more.
[0097] A reversing rolling mill is a type of rolling mill generally used for rolling thin materials, and refers to a rolling mill that rolls the material by moving it back and forth between a pair of rolls, and one way of the material's reciprocation can be set as one pass.
[0098] The present invention reveals that the hot-rolled steel sheet can be pickled before the cold rolling, and the pickling process can be carried out in a conventional manner.
[0099] [Continuous annealing] It is preferable to subject the cold rolled steel sheet produced as described above to a continuous annealing process. As an example, the continuous annealing process can be performed in a continuous annealing furnace (CAL).
[0100] Typically, a continuous annealing furnace (CAL) can be composed of a heating zone, a soaking zone, a cooling zone (slow cooling zone and quenching zone), and (if necessary, an overaging zone). After a cold-rolled steel sheet is charged into such a continuous annealing furnace, it is heated to a specific temperature in the heating zone, and after the target temperature is reached, it is maintained for a certain period of time in the soaking zone.
[0101] In the present invention, the temperatures of the heating zone and the soaking zone during the continuous annealing can be controlled to be the same, which means that the end temperature of the heating zone and the start temperature of the soaking zone are controlled to be the same (FIG. 1).
[0102] Specifically, the temperatures of the heating zone and the soaking zone can be controlled to 790 to 850°C.
[0103] If the temperature of the heating zone is less than 790°C, sufficient heat input for recrystallization cannot be applied, while if the temperature exceeds 850°C, the productivity decreases, the austenite phase is excessively formed, and the fraction of the hard phase increases significantly after the subsequent cooling, which may result in poor ductility of the steel.
[0104] If the temperature of the soaking zone is less than 790°C, excessive cooling is required at the end of the heating zone, which is economically disadvantageous and may result in insufficient heat for recrystallization, whereas if the temperature exceeds 850°C, the austenite fraction becomes excessive, and the hard phase increases during cooling, which may result in reduced formability.
[0105] Increasing the temperature of the soaking zone within the above-mentioned temperature range increases the fraction of the hard phase in the final structure, thereby increasing the yield strength, and also reduces the hardness difference between the phases by introducing bainite, thereby improving the hole expansion ratio.
[0106] On the other hand, the present invention is characterized in that sufficient recrystallization occurs during the annealing process, thereby inducing the formation of recrystallized ferrite bridges.
[0107] Specifically, in the present invention, when the above-mentioned cold-rolled steel sheet is heated to the temperature region of the heating zone, a recrystallization zone can be introduced in which the intermediate temperature is maintained for a certain period of time, and more preferably, a process of maintaining the temperature in the range of 600 to 700°C for 1 to 3 minutes is preferably performed (dashed line graph in Figure 2).
[0108] If the temperature of the recrystallization zone is less than 600°C or the holding time is less than 1 minute, the recrystallization of ferrite is insufficient and the recrystallized ferrite bridge phase cannot be formed at the target fraction. On the other hand, if the temperature exceeds 700°C or the holding time exceeds 3 minutes, the recrystallization becomes excessive, which may result in a decrease in strength and a decrease in physical properties due to the coarsening of crystal grains.
[0109] The present invention provides an effect of improving processability by introducing a recrystallized ferrite bridge phase together with an appropriate fraction of a hard phase and a soft phase as a final microstructure through the recrystallization zone process, thereby improving crack toughness, in other words, crack resistance, while maintaining strength.
[0110] [Stepwise cooling] As described above, a target structure can be formed by cooling the cold-rolled steel sheet that has been subjected to the above-described continuous annealing treatment, and at this time, it is preferable to perform the cooling stepwise.
[0111] In the present invention, the stepwise cooling may include primary cooling and secondary cooling. Specifically, after the continuous annealing, primary cooling may be performed at an average cooling rate of 1 to 10°C / s to a temperature range of 650 to 700°C, and then secondary cooling may be performed at an average cooling rate of 5 to 50°C / s to a temperature range of 450 to 500°C.
[0112] At this time, by carrying out the primary cooling slower than the secondary cooling, it is possible to suppress defects in the sheet shape that would otherwise occur due to a sudden drop in temperature during the secondary cooling, which is a relatively rapid cooling period.
[0113] If the end temperature of the first cooling is less than 650°C, the carbon diffusion activity is low due to the low temperature, and the carbon concentration in the ferrite increases, while the carbon concentration in the austenite decreases, causing the hard phase fraction to become excessive, increasing the yield ratio and increasing the tendency for cracks to occur during processing. In addition, the cooling rate between the soaking zone and the cooling zone (slow cooling zone) becomes too high, causing the plate shape to become non-uniform. If the end temperature exceeds 700°C, there is a disadvantage that an excessively high cooling rate is required for the subsequent cooling (secondary cooling).
[0114] Furthermore, if the average cooling rate during the primary cooling exceeds 10° C. / s, carbon diffusion will not occur sufficiently. On the other hand, in consideration of productivity, the primary cooling can be performed at an average cooling rate of 1° C. / s or more.
[0115] As described above, after the primary cooling is completed, rapid cooling (secondary cooling) can be performed at a certain cooling rate or higher. If the secondary cooling end temperature is less than 450°C, cooling variations occur in the width and length directions of the steel sheet, which may cause deterioration of the sheet shape. On the other hand, if the temperature exceeds 500°C, the hard phase cannot be sufficiently secured, which may result in a decrease in strength.
[0116] If the average cooling rate during the secondary cooling is less than 5° C. / s, the proportion of the soft phase may be excessive, whereas if it exceeds 50° C. / s, the proportion of the hard phase may be insufficient.
[0117] If necessary, overaging treatment can be carried out after the stepwise cooling is completed.
[0118] The overaging treatment is a process of maintaining the temperature for a certain period of time after the end of the secondary cooling, and has the effect of improving the shape quality by performing a uniform heat treatment in the width direction and length direction of the coil. For this purpose, the overaging treatment can be performed for 200 to 800 seconds.
[0119] Since the overaging treatment can be performed immediately after the completion of the secondary cooling, the temperature can be the same as the secondary cooling end temperature, or can be within the secondary cooling end temperature range, or can be performed at a lower temperature than the secondary cooling end temperature. More preferably, it can be performed at a temperature range of 300 to 450°C.
[0120] The high strength thick steel plate of the present invention manufactured as described above has a microstructure composed of a hard phase and a soft phase, and by maximizing ferrite recrystallization through an optimized cold rolling and annealing process, the final recrystallized ferrite matrix has a structure in which a martensite phase, which is a hard phase, is uniformly distributed. Furthermore, by introducing a relatively coarse recrystallized ferrite bridge phase to connect the hard phase, it has an effect of increasing crack resistance during processing.
[0121] For this reason, the thick steel plate of the present invention can ensure excellent formability such as excellent hole expandability by ensuring a low yield ratio and high ductility, despite having a high strength of tensile strength of 980 MPa or more. EXAMPLES
[0122] The present invention will be described in more detail below with reference to examples. However, the description of such examples is for illustrating the implementation of the present invention, and the present invention is not limited by the description of such examples. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0123] (Example) Steel slabs having the alloy composition shown in Table 1 below were prepared, and then each steel slab was heated at 1200°C for 1 hour, and then finish hot-rolled at a finish rolling temperature of 880 to 920°C to produce hot-rolled steel sheets. Then, each hot-rolled steel sheet was coiled at 650°C, and cooled to room temperature at a cooling rate of 0.1°C / s. Then, the coiled hot-rolled steel sheet was cold-rolled and continuously annealed under the conditions shown in Table 2 below, and then stepwise cooled (1st-2nd), and then overaged at 360°C for 520 seconds to produce a final steel sheet with a thickness of 1.8 mm.
[0124] In this stepwise cooling, the first cooling was performed at an average cooling rate of 3°C / s, and the second cooling was performed at an average cooling rate of 20°C / s.
[0125] The microstructure of each of the steel sheets manufactured as described above was observed, and the tensile and processing properties, hole expansion ratio, and other processing property indexes were evaluated. The results are shown in Table 3 below.
[0126] At this time, the tensile test for each test piece was carried out by taking a JIS No. 5 size tensile test piece in the direction perpendicular to the rolling direction and then carrying out the tensile test at a strain rate of 0.01 / s.
[0127] Meanwhile, the hole expansion ratio (HER,%) measurement test was conducted according to the ISO16630 standard. Specifically, after punching a circular hole in the test piece, it was expanded using a conical punch. The hole expansion amount until the crack generated at the edge of the hole penetrates through the thickness direction was expressed as a percentage of the initial hole. At this time, the dimensions of the test piece were 120mm x 120mm, the clearance was 12%, the punching hole diameter was 10mm, the punching holding load was 20 tons, and the test speed was 12mm / min.
[0128] Among the structural phases, the bainite phase, which corresponds to a hard phase, was etched with picral, and the martensite phase was etched with nital, and then observed through a SEM at 2000 and 5000 magnifications.
[0129] In addition, the fractions of the ferrite phase and the recrystallized ferrite bridge phase were measured using an SEM and an image analyzer program after nital etching.
[0130] [Table 1]
[0131] [Table 2]
[0132] [Table 3]
[0133] As shown in Tables 1 to 3 above, in Examples 1 to 6, in which the alloy composition and manufacturing conditions of the steel, particularly the cold rolling and continuous annealing processes, all meet the conditions proposed in the present invention, the hard phase was formed by being connected by the recrystallized ferrite bridge phase due to sufficient recrystallization of ferrite during the annealing process after cold rolling. As a result, while having high strength, it had a yield strength suitable for plate processing and excellent elongation. In addition, it can be confirmed that the homogeneous distribution of the hard phase provides excellent hole expandability and ensures the target level of formability.
[0134] On the other hand, in Comparative Examples 1 to 4 and 6 to 9, which did not pass through the recrystallization zone during the heating process of continuous annealing during the manufacturing process of the steel sheet, recrystallization did not occur sufficiently, and the recrystallized ferrite bridge phase was insufficient. Among these, Comparative Examples 1 to 4, in which the continuous annealing temperature was relatively low, were inferior in at least one of the physical properties of elongation and hole expandability, and Comparative Examples 6 to 9, in which the continuous annealing temperature was relatively high, were excessively formed with bainite phase, and thus had excessively high yield strength and poor elongation.
[0135] Comparative Examples 5 and 10 had the annealing temperature required to drive recrystallization and sufficient austenite stability to ensure strength, but recrystallization did not occur sufficiently due to an insufficient rolling reduction, and a uniform structure could not be formed, resulting in poor elongation and relatively high yield strength.
[0136] Moreover, in Comparative Examples 11 to 14 in which the secondary cooling temperature was very low, the yield strength was excessively high, so there was a high risk of cracks occurring during processing, and the elongation was poor due to the absence of a recrystallized ferrite bridge phase.
[0137] FIG. 3 shows microstructure photographs of Comparative Examples 1, 4-5 and 9, and FIG.
[0138] As shown in Fig. 3, in Comparative Examples 1, 4, and 9, the recrystallization zone process was not introduced during the temperature rise process during continuous annealing, so the connection structure of the hard phases due to the recrystallized ferrite bridges was hardly observed. Also, in Comparative Example 5, the fraction of the recrystallized zone was low due to an insufficient rolling reduction rate, and the recrystallization was insufficient due to a low driving force, so the hard phases were formed into a structure where they gathered together, forming a structure with low crack propagation resistance.
[0139] On the other hand, as shown in FIG. 4, in the example of the present invention, a relatively coarse recrystallized ferrite bridge phase was observed due to the recrystallization zone process, and it can be seen that the unidirectionality of the hard phase was eliminated by this phase.
Claims
1. In weight percent, carbon (C): 0.05 to 0.12%, manganese (Mn): 2.0 to 3.0%, silicon (Si): 0.5% or less (excluding 0%), chromium (Cr): 1.0% or less (excluding 0%), niobium (Nb): 0.1% or less (excluding 0%), titanium (Ti): 0.1% or less (excluding 0%), boron (B): 0.003% or less (excluding 0%), aluminum (sol.Al): 0.02 to 0.05%, phosphorus (P): 0.05% or less (excluding 0%), sulfur (S): 0.01% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), iron (Fe) and other unavoidable impurities. A high-strength thick steel plate having excellent hole expandability and ductility, the microstructure of which includes 10 to 30% ferrite in area fraction, 10 to 25% recrystallized ferrite bridges, 20 to 30% bainite, and the remainder martensite.
2. The high-strength thick steel plate having excellent hole expandability and ductility according to claim 1, wherein the recrystallized ferrite bridge has an average circle equivalent diameter of 1 to 6 μm.
3. The high-strength thick steel plate having excellent hole expandability and ductility according to claim 1, wherein the steel plate contains a martensite phase at an area fraction of 15% or more.
4. The high-strength thick steel plate having excellent hole expandability and ductility according to claim 1, wherein the steel plate further contains a retained austenite phase at an area fraction of 3% or less (including 0%).
5. The high-strength thick steel plate having excellent hole expandability and ductility according to claim 1, wherein the steel plate has a tensile strength of 980 MPa or more, a yield strength of 550 to 700 MPa, and a total elongation of 14% or more.
6. The high-strength thick steel plate having excellent hole expandability and ductility according to claim 1, wherein the steel plate has a hole expansion ratio (HER) of 30% or more.
7. The high-strength thick steel plate having excellent hole expandability and ductility according to claim 1, wherein the steel plate has a thickness of 1 to 3 mm.
8. preparing a steel slab containing, by weight percent, 0.05-0.12% carbon (C), 2.0-3.0% manganese (Mn), 0.5% or less (except 0%) silicon (Si), 1.0% or less (except 0%) chromium (Cr), 0.1% or less (except 0%) niobium (Nb), 0.1% or less (except 0%) titanium (Ti), 0.003% or less (except 0%) boron (B), 0.02-0.05% aluminum (sol. Al), 0.05% or less (except 0%) phosphorus (P), 0.01% or less (except 0%) sulfur (S), 0.01% or less (except 0%) nitrogen (N), iron (Fe) and other inevitable impurities; heating the steel slab to a temperature range of 1100 to 1300°C; hot rolling the heated steel slab to produce a hot rolled steel sheet; coiling the hot-rolled steel sheet at a temperature in the range of 400 to 700°C; After the coiling, cooling the hot-rolled steel sheet to room temperature; cold rolling the cooled hot-rolled steel sheet at a cold reduction of 55 to 80% to produce a cold-rolled steel sheet; subjecting the cold rolled steel sheet to a continuous annealing treatment; After the continuous annealing, a primary cooling step is performed to a temperature range of 650 to 700 ° C. at an average cooling rate of 1 to 10 ° C. / s. After the primary cooling, secondary cooling is performed at an average cooling rate of 5 to 50 ° C. / s to a temperature range of 450 to 500 ° C., The continuous annealing is performed in a facility equipped with a heating zone, a soaking zone, and a cooling zone, and when the cold-rolled steel sheet is heated to the heating zone, the cold-rolled steel sheet passes through a recrystallization zone maintained at 600 to 700 ° C. for 1 to 3 minutes. A method for producing a high-strength thick steel sheet having excellent hole expandability and ductility.
9. The method for producing a high-strength thick steel plate having excellent hole expandability and ductility according to claim 8, wherein the hot rolling is finish hot rolling at an outlet side temperature of Ar3 to 1000 ° C.
10. The manufacturing method of a high-strength thick steel plate having excellent hole expandability and ductility according to claim 8, wherein the cooling after the coiling is performed at a cooling rate of 0.1 ° C. / s or less (excluding 0 ° C. / s).
11. The manufacturing method of high-strength thick steel plate having excellent hole expandability and ductility according to claim 8, wherein the heating zone and the soaking zone are controlled in a temperature range of 790 to 850 ° C.
12. The method further includes a step of performing an overaging treatment after the secondary cooling, The method for producing a high-strength thick steel plate having excellent hole expandability according to claim 8, wherein the overaging treatment is performed for 200 to 800 seconds.
Citation Information
Patent Citations
High-strength cold rolled steel sheet excellent in ductility and stretch-flanging property and manufacturing method for the same
JP2005213640A
Cold-rolled steel sheet
WO2020071522A1
Cold-rolled steel sheet of 980 MPa grade having a high hole expansion ratio and relatively high elongation and its manufacturing method