Platinum-supported catalyst with improved hydrogenation / dehydrogenation reversibility and liquid organic hydrogen carrier-based hydrogen storage and release method using the same
A platinum-supported catalyst with monoatomic and cluster forms on alumina, produced via a solid-phase method, addresses the inefficiencies of impregnation methods by enhancing hydrogenation/dehydrogenation activity and stability, facilitating efficient hydrogen storage and release in LOHCs.
Patent Information
- Application Number
- JP2024513081
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-09-29
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2042-09-29
AI Technical Summary
Existing platinum-supported catalysts for hydrogenation/dehydrogenation reactions in liquid organic hydrogen carriers (LOHCs) face challenges with insufficient dehydrogenation activity, limited reversibility, and long-term stability, particularly when produced by time-consuming impregnation methods, limiting their applicability and efficiency in hydrogen storage and release processes.
A platinum-supported catalyst is developed with a combination of monoatomic and cluster forms of platinum on an alumina support, produced through a solid-phase method without solvents, involving a single-step reaction with controlled heat treatment to enhance dispersion and interaction, improving hydrogenation/dehydrogenation activity and stability.
The catalyst achieves enhanced hydrogenation/dehydrogenation efficiency, improved reversibility, and long-term stability, enabling efficient hydrogen storage and release in a wide range of LOHCs, including hydrocarbon-based carriers, while reducing production time and costs compared to conventional methods.
Smart Images

Figure 2024535993000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a platinum-supported catalyst with improved hydrogenation / dehydrogenation reversibility and a liquid organic hydrogen carrier-based hydrogen storage and release method using the same. More specifically, the present disclosure relates to a hydrogenation / dehydrogenation catalyst in which platinum (Pt) metal, which is an active metal and has a mixture of single atom and cluster forms, is supported on an alumina carrier based on a solid phase method, and a technology for reversibly storing and releasing hydrogen with high selective conversion and high efficiency using the same. [Background technology]
[0002] 2. Description of the Related Art As environmental pollution problems, such as dwindling reserves of fossil fuels, pollutants generated during combustion, and global warming caused by carbon dioxide, become more serious, there has been an explosive increase in global interest and demand for the development of alternative energy sources.
[0003] As alternative energy sources, new and renewable energies such as wind power, tidal power, geothermal energy, hydrogen energy, solar energy, etc. are attracting attention, but each of the above listed energy sources has advantages and disadvantages. In relation to this, since it is difficult to smoothly supply and demand new and renewable energies due to the instability of the energy source depending on time and the natural environment, in order to effectively replace conventional fossil fuels, it is necessary to develop a technology to store and supply surplus energy so that energy can be supplied stably.
[0004] From this perspective, hydrogen energy has been attracting particular attention because (i) it has the highest energy efficiency per unit mass, (ii) when burned, only water is produced and no other harmful by-products are produced, (iii) water, the main source of hydrogen, is abundant in nature and is converted into water after use, making it advantageous in terms of reuse, and (iv) it is a distributed power source that uses hydrogen as fuel and is suitable for ensuring the competitiveness of precision and IT industries. Furthermore, hydrogen can be produced using other new and renewable energies such as solar energy and wind power, and can be widely applied not only to various energy sources but also to other industrial sectors (e.g. various petrochemical sectors), and is therefore emerging as a core energy source of the future both in Korea and abroad.
[0005] In general, research and development of hydrogen energy is largely divided into the fields of hydrogen production, transportation, and storage. Hydrogen has excellent energy storage capacity per mass, but low energy storage capacity per volume, so the technology to efficiently store hydrogen is the biggest obstacle to the practical application of hydrogen energy. For example, there are known substances that have a mass storage density of 10% or more by weight at 77K, but the volume storage density of these substances is 40g / L, which is low for practical use as a hydrogen storage material. Therefore, research is being actively conducted into technology to store as much hydrogen as possible in a storage medium that is as light and small in volume as possible.
[0006] In relation to this, countries have invested a lot of money in research and development over the past few years, and the efficient methods of storing hydrogen that have been researched and developed so far include the CGH2 method, which compresses hydrogen using a pressure of 700 bar, and the LH2 method, which stores liquid hydrogen by liquefying it at -253°C. However, these pressurization or liquefaction methods require maintaining low temperatures, and the density of liquid hydrogen is also low at 71.2 kg / m. 3 This is a low level.
[0007] As an alternative to this, materials with hydrogen storage capacity, for example, inorganic-organic frameworks (MOFs), porous organic or inorganic nano materials such as carbon nanotubes, zeolites, activated carbon, metal hydrides, etc., have been attracting attention as materials that can effectively store hydrogen energy (Nature, 427, 523 (2004); J. Am. Chem. Soc., 127, 14904 (2005); JP 2008-95172 A; JP 2011-131120 A, etc.). However, in the case of room temperature gas phase hydrogen storage technology using physical absorption of MOFs and porous nano materials, the energy storage density is relatively low and the energy required for storing and desorbing hydrogen is relatively large, making it difficult to miniaturize and modularize.
[0008] Recently, hydrogen storage technology using reversible catalytic hydrogenation / dehydrogenation reactions using organic matter, specifically liquid organic hydrogen carriers (LOHCs) has been developed (U.S. Patent No. 7,901,491, etc.). LOHC technology has the advantages of being able to store more than 5% by weight of hydrogen, as recommended by the U.S. Department of Energy (DOE), being able to operate in a low pressure range, and being able to easily regenerate the storage material. In addition, due to the advantages of liquid fossil fuels, such as ease of handling and high energy density, it can provide a practical hydrogen storage system that can be efficiently transported and stored using existing liquid fuel transportation and storage infrastructure (Energy Rev., 6 (2002) 141; Energy Environ. Sci., 8 (2015) 1035-1045).
[0009] Although there are known techniques using compounds in the form of π-conjugated substrates as LOHC materials (e.g., U.S. Patent No. 7,351,395, etc.), it is difficult to ensure uniform reactivity due to π-conjugation, and most of them exist as solid phases, so they are used in the form of mixtures. In order to alleviate the above-mentioned difficulties, there are also known techniques using benzyltoluene and dibenzyltoluene as hydrogen storage materials (e.g., Korean Patent Publication No. 2015-97558, etc.). These hydrogen carriers exist as a liquid phase at room temperature and have a boiling point of 280°C or higher, so there are almost no restrictions in terms of utilization, but there are limitations in increasing the efficiency of hydrogenation and dehydrogenation reactions due to limitations in the hydrocarbon structure.
[0010] Meanwhile, in order to commercialize hydrogen storage / release systems using LOHC, various technical factors must be considered in addition to the development of hydrogen storage materials. Among these, for catalysts, the activity and reversibility of hydrogenation / dehydrogenation reactions, catalyst stability (reusability), and applicability of LOHC to commercial processes must be considered.
[0011] In this regard, a LOHC-based hydrogen storage and release process using a platinum-supported catalyst, known to have good hydrogenation activity, can be considered. In the case of platinum-supported catalysts, hydrogen can generally be easily dissociated into hydrogen atoms, so they are effective in reactions in which hydrogen gas is contacted with a reactant, such as hydrogenolysis or hydrogenation. In LOHC systems, such catalysts can also be effective in dehydrogenation, acting as active sites for releasing hydrogen through cyclic compounds.
[0012] However, even when a platinum-supported porous alumina catalyst is used for the hydrogenation / dehydrogenation reaction of LOHC, the degree of dispersion of the active metal is not high, so the dehydrogenation (hydrogen release) activity may still be insufficient. In addition, platinum-supported alumina catalysts are typically manufactured by impregnation, which requires multiple steps to synthesize the alumina support and support the metal, making the catalyst manufacturing time-consuming and disadvantageous in terms of commercialization. In particular, although the inherent properties of alumina can ensure a certain degree of catalyst stability, there is a limit to achieving additional improved performance.
[0013] In addition, existing hydrogenation / dehydrogenation catalysts have shown relatively good hydrogen storage / release performance, mainly in LOHC systems with nitrogen-containing heterocycles, but commercial companies are in high demand for technology that can provide good hydrogen storage / release performance even in LOHCs consisting only of hydrocarbons, such as decalin.
[0014] Therefore, there is a need for a catalyst that not only has better hydrogenation / dehydrogenation reaction activity and reversibility than conventionally known metal-supported catalysts, particularly platinum-supported catalysts, but also provides good performance against various types of LOHC. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] JP 2008-095172 A [Patent Document 2] JP 2011-131120 A [Patent Document 3] U.S. Patent No. 7,901,491 [Patent Document 4] U.S. Patent No. 7,351,395 [Patent Document 5] Korean Patent Publication No. 2015-97558 [Non-patent literature]
[0016] [Non-Patent Document 1] Nature, 427, 523 (2004) [Non-Patent Document 2] J.Am.Chem.Soc.,127,14904(2005) [Non-Patent Document 3] Energy Rev.,6(2002)141 [Non-Patent Document 4] Energy Environ.Sci.,8(2015)1035-1045 Summary of the Invention [Problem to be solved by the invention]
[0017] In one embodiment of the present disclosure, there is provided a catalyst having improved properties in terms of hydrogenation / dehydrogenation reaction efficiency and reversibility for liquid organic hydrogen carriers, long-term stability, and scalability for liquid organic hydrogen carriers, and a method for producing the same.
[0018] According to another embodiment of the present disclosure, there is provided a liquid organic hydrogen carrier-based hydrogen storage / release process using the above-mentioned catalyst. [Means for solving the problem]
[0019] According to a first aspect of the disclosure, A catalyst for hydrogenation / dehydrogenation of a liquid organic hydrogen carrier, comprising: an alumina support; and Platinum, including monoatomic and cluster forms, as the active metal supported on said alumina-containing support; Including, The platinum content (element basis) in the catalyst is 0.01% to 10% by weight. The catalyst is provided in which the supported platinum has a platinum content in the form of clusters ranging from 10% to 55%.
[0020] According to a second aspect of the disclosure, A method for producing a hydrogenation / dehydrogenation catalyst for a liquid organic hydrogen carrier, comprising the steps of: a) carrying out a solid-state reaction in the absence of a solvent while applying external energy to a mixture containing at least one alumina precursor, at least one platinum precursor, and a base component to form a catalyst solid in the form of a gel; and b) heat-treating the catalytic solid in an oxygen-containing atmosphere to support platinum, including platinum in the form of monoatoms and clusters, on the alumina-containing support; Including, The platinum content (element basis) in the catalyst is in the range of 0.01% to 10% by weight. A process is provided in which the content of platinum in cluster form in the supported platinum ranges from 10% to 55%.
[0021] According to the third aspect of this disclosure: A hydrogenation step in which hydrogen is stored in a liquid organic hydrogen carrier in the presence of a catalyst; and a dehydrogenation step of releasing hydrogen from the hydrogenated liquid organic hydrogen carrier in the presence of a catalyst; The catalyst used in at least one of the hydrogenation step and the dehydrogenation step is an alumina support; and Platinum, including monoatomic and cluster forms, as the active metal supported on said alumina-containing support; Including, The platinum content in the catalyst (element basis) is 0.01% by weight to 10% by weight, and the content of platinum in cluster form in the supported platinum is in the range of 10% to 55%. The hydrogenation and dehydrogenation steps are alternated to provide a method for storing and releasing hydrogen. Effect of the Invention
[0022] According to the specific embodiment of the present disclosure, platinum, including platinum in the form of a single atom and platinum in the form of a cluster, is supported as an active metal on the alumina carrier in the catalyst, thereby achieving good hydrogenation (hydrogen storage) / dehydrogenation (hydrogen release) activity not only for nitrogen-containing liquid organic hydrogen carriers but also for all liquid organic hydrogen carriers made of hydrocarbons, and in particular, providing the advantage of improving the reversibility of hydrogenation / dehydrogenation. In addition, in another specific embodiment of the present disclosure, even without the use of a solvent, a single-step reaction is performed by applying simple physical or mechanical external energy such as milling to a raw material mixture containing a platinum precursor and an alumina precursor, and in particular, the unique properties of the platinum-supported alumina catalyst described above can be realized by controlling the heat treatment or calcination conditions to affect the form of platinum present. The catalyst thus prepared can overcome the technical limitations of two-step catalyst preparation methods such as the relatively high catalyst preparation cost and the time-consuming impregnation method, and can provide multiple advantages such as maintaining improved activity for a long period of time during the hydrogenation / dehydrogenation reaction of a liquid organic hydrogen carrier. [Brief description of the drawings]
[0023] [Figure 1] 1 shows XRD patterns of a platinum-supported catalyst (MPtA) according to an embodiment (solid phase method) and a platinum-supported catalyst (Pt / gA) according to a comparative example (impregnation method) each having various platinum contents (1 wt%, 2 wt%, 3 wt%, and 5 wt%) supported thereon. [Diagram 2] 6A and 6B are dark field HAADF-STEM images of a platinum-supported catalyst (MPtA) according to an embodiment (solid phase method) and a platinum-supported catalyst (Pt / gA) according to a comparative example (impregnation method) carrying various platinum contents (1 wt%, 2 wt%, 3 wt%, and 5 wt%), respectively. [Diagram 3]1 shows CO-DRIFT spectrum graphs for platinum-supported catalysts (MPtA) according to an embodiment (solid phase method; Pt loading: 1 wt%, 2 wt%, 3 wt%, and 5 wt%) and platinum-supported catalysts (Pt / gA) according to a comparative example (impregnation method; Pt loading: 1 wt%, 3 wt%, and 5 wt%), each of which has various platinum loadings. [Figure 4] FIG. 1 is a graph showing the H2-TPD results for a platinum-supported catalyst (MPtA) according to an embodiment (solid phase method) and a platinum-supported catalyst (Pt / gA) according to a comparative example (impregnation method) carrying various amounts of platinum (1 wt%, 2 wt%, 3 wt%, and 5 wt%) (the numerical values in the figure are the amount of hydrogen adsorption (unit: mmol gPt-1)). [Diagram 5] Graphs a and b show the results of EXAFS fitting for a platinum-supported catalyst (MPtA) according to an embodiment (solid phase method) and a platinum-supported catalyst (Pt / gA) according to a comparative example (impregnation method) carrying various platinum contents (1 wt%, 3 wt%, and 5 wt%), respectively (reference materials are Pt foil and PtO2). [Figure 6] Graphs a and b compare the hydrogenation and dehydrogenation reaction efficiencies using a platinum-supported catalyst (MPtA) according to an embodiment (solid phase method) and a platinum-supported catalyst (Pt / gA) according to a comparative example (impregnation method) each carrying various amounts of platinum (1 wt%, 2 wt%, 3 wt%, and 5 wt%). [Figure 7] 1 is a graph showing XRD patterns (a, b) and H2-TPD results (c, d) for Pt-supported catalysts (loading amounts: 1 wt % and 3 wt %) under different calcination conditions. [Figure 8] 4 shows HAADF-STEM photographs of Pt-supported catalysts with different calcination conditions (a and b show the loading amount of 3 wt %, and c and d show the loading amount of 1 wt %). [Figure 9] Hydrogen release curves over time of dehydrogenation reaction for Pt-supported catalysts with different calcination conditions (a: 3 wt. % loading, b: 1 wt. % loading). (Reaction conditions: 250°C, 1 bar, 4 h, 0.1% noble metal (mol) / reactant (mol)). [Figure 10] FIG. 1 is a graph showing the results of a dehydrogenation reaction to evaluate the long-term stability of a platinum-supported catalyst (M3PtA) according to an embodiment (solid phase method) and a platinum-supported catalyst (3Pt / gA) according to a comparative example (impregnation method) (reaction conditions: 250° C., 1 bar, 4 h, precious metal (mol) / reactant (mol) 0.1%). [Figure 11] 1 shows XRD patterns (a, b) before and after the reaction of a platinum-supported catalyst (M3PtA) according to an embodiment (solid phase method) and a platinum-supported catalyst (3Pt / gA) according to a comparative example (impregnation method), and HAADF-STEM photographs (c, d) of the catalysts after use. [Figure 12] Graphs a and b show the results of comparing the hydrogen storage and release efficiencies of H0-BT using a platinum-supported catalyst (M3PtA) according to the embodiment (solid phase method) and a platinum-supported catalyst (3Pt / gA) according to the comparative example (impregnation method) (hydrogenation reaction conditions: 150°C, 35 bar H2, 2 h; dehydrogenation reaction conditions: 250°C, 4 h). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention can be achieved by the following description. The following description should be understood as describing a preferred embodiment of the present invention, and the present invention is not necessarily limited thereto. In addition, it should be understood that the attached drawings are for facilitating understanding, and the present invention is not limited thereto.
[0025] The terms used herein may be defined as follows:
[0026] A "heterogeneous catalyst" may refer to a catalyst that exists in a different phase from the reactants during a catalytic reaction, for example, a catalyst that is not dissolved in the reaction medium. In the case of a heterogeneous catalyst, at least one reactant must diffuse and adsorb onto the surface of the heterogeneous catalyst in order for a reaction to occur, and after the reaction, the product must desorb from the surface of the heterogeneous catalyst.
[0027] "Support" may mean a material (typically a solid phase material) with a high specific surface area to which catalytically active components are attached.
[0028] "Active metal in single atom form" may be understood as the active metal attached or fixed to the support being present in an isolated or individualized state in the form of an atom.
[0029] An "active metal in the form of a cluster" may be understood as, for example, an active metal having a size of about 5 nm or less, specifically a size of about 3 nm or less, and more specifically a size of about 2 nm or less (i.e., a collection of at least two active metal atoms) attached or fixed to a support.
[0030] "Hydrogenation" may refer to a reaction in which the hydrogen content in a compound is increased by contacting the compound with a catalyst in the presence of a supply of hydrogen to chemically add hydrogen to at least a portion of the compound.
[0031] "Dehydrogenation" may refer to a reaction in which hydrogen is removed from a compound and then the removed hydrogen is released from the compound.
[0032] The term "impregnation" refers to a method of preparing a catalyst by impregnating a solution in which a catalyst precursor is dissolved into a separately synthesized support, and then optionally drying and / or calcining (or reducing) the support.
[0033] "Salt" may refer generally to a compound in which a metal cation is combined with an inorganic anion or an organic anionic species.
[0034] [Overall disclosure content] One specific example of the present disclosure can overcome all of the technical limitations of platinum-supported alumina catalysts, which are known as conventional catalysts for hydrogenation / dehydrogenation reactions, when they are applied to hydrogen storage and release (i.e., hydrogenation and dehydrogenation) processes using liquid organic hydrogen carriers, such as difficulty in ensuring good reversibility of hydrogenation / dehydrogenation reactions, difficulty in repeatedly operating hydrogen storage and release systems due to reduced long-term stability of the catalyst, and applicability to hydrogen storage and release using limited types of liquid organic hydrogen carriers.
[0035] In general, the size of the metal (especially nanometer-level metal particles) as the active metal in the catalyst acts as a factor that has a significant effect on the reaction activity. That is, when the same amount of active metal is supported on a support having the same surface area, the number of metal active sites supported on the same support increases as the size of the metal is minimized. Therefore, by increasing the dispersion of the active metal and increasing the ratio of coordinated surface atoms, the catalytic activity per metal atom can be promoted.
[0036] In this regard, single atom catalysts (SACs) bound to a support in atomic units (monoatomic form) are effective in increasing the active sites of the catalyst, but have a tendency to increase in particle size due to their large surface energy, which induces aggregation at high temperatures. On the other hand, catalysts supported in cluster form have excellent catalyst stability because multiple metal atoms and ligands are bound to each other and have an organized structure similar to other metal oxides. The platinum-supported catalyst according to this embodiment can disperse metals uniformly over a wide surface area and increase activity compared to catalysts synthesized by conventional impregnation methods, and in particular, it supports platinum in a form in which monoatoms and clusters are combined (mixed), and can provide effects that exceed the extent expected from the form of monoatoms and clusters by simultaneously realizing the respective advantages of monoatoms and clusters. In particular, when prepared by the impregnation method, the catalyst is supported in the form of particles larger than clusters, which is an element that clearly differentiates the catalyst according to this embodiment from platinum-supported catalysts according to the prior art.
[0037] Thus, in the case of the platinum-supported catalyst according to this embodiment, platinum is supported in a form including a combination of single atoms and clusters through the catalyst synthesis method, and it not only exhibits excellent catalytic activity for both gas-phase or liquid-phase hydrogenation and dehydrogenation reactions even in a single reactor, but also exhibits good reversibility and can provide improved properties in terms of long-term stability of the catalyst. Of particular note is that when the ratio of platinum in cluster (or single atom) form in the supported active metal (platinum) is appropriately adjusted within a predetermined range, it is possible to effectively increase the hydrogen release efficiency of platinum-based catalysts, which is more difficult to improve than the hydrogen storage efficiency, in hydrogen storage / release reactions using liquid organic hydrogen carriers.
[0038] [Hydrogenation / Dehydrogenation Catalyst] According to one embodiment of the present disclosure, a catalyst (i.e., a heterogeneous catalyst) is provided that is suitable for storing / releasing hydrogen through hydrogenation / dehydrogenation reactions, particularly for a wide range of liquid organic hydrogen carriers, particularly not only liquid organic hydrogen carriers having nitrogen-containing heterocycles, but also all liquid organic hydrogen carriers consisting only of hydrocarbons.
[0039] In this regard, the hydrogenation / dehydrogenation catalyst is broadly a supported catalyst containing platinum as an active metal on a porous alumina-containing support, and in particular, platinum may be dispersed and supported on the support in a mixed form of single atoms and clusters, or may be in the form of crystallites. In this case, the platinum crystals may mainly contain the (111) plane. In addition, platinum in the catalyst may be in an oxidized state and / or a reduced state (or an elemental state or a partially reduced state), and more specifically, in a reduced state. In this case, the reduced state may be realized by reducing the catalyst in an oxidized state (calcined state).
[0040] In an exemplary embodiment, the platinum content (loading) in the catalyst can range, for example, from about 0.01% to 10% by weight, specifically from about 0.1% to 5% by weight, and more specifically from about 0.5% to 3% by weight, on an elemental basis.
[0041] According to an exemplary embodiment, the platinum in the catalyst may be in the form of a combination of single atoms and clusters having a size of about 5 nm or less, specifically about 3 nm or less, more specifically about 0.1 nm to 2 nm. If the size of the platinum exceeds a certain level, the reaction efficiency decreases due to the decrease in the dispersion of the metal supported on the support, so it may be advantageous to adjust it within the above range, but it may be somewhat changed within the above range depending on the reaction conditions, etc.
[0042] Meanwhile, in this embodiment, the support of the hydrogenation / dehydrogenation catalyst can be an alumina-containing support. Such alumina can be a mesoporous alumina, typically exhibiting ink-bottle or channel-type pore connectivity, and thus exhibiting relatively high surface area, high packing density, thermal stability, physical strength, and regeneration ability in the hydrogenation / dehydrogenation reaction.
[0043] According to an exemplary embodiment, the BET specific surface area of the support in the catalyst is, for example, at least about 300 m 2 / g, specifically about 320m 2 / g~400m 2 / g, more specifically, about 350m 2 / g~380m 2 This specific surface area is significantly higher than that of γ-alumina supports used in various conventional chemical reactions, and is therefore suitable for effectively dispersing platinum, which is an active metal.
[0044] According to an exemplary embodiment, the pore volume of the support in the catalyst is, for example, about 0.4 cm 3 / g~0.55cm 3 / g, specifically, about 0.42 cm 3 / g~0.5cm 3 / g, more specifically, about 0.45 cm 3 / g~0.49cm 3 The pore size of the support in the catalyst can range, for example, from about 3 nm to 4.5 nm, specifically from about 3.5 nm to 4.3 nm, and more specifically from about 3.8 nm to 4.1 nm.
[0045] According to an exemplary embodiment, the shape of the catalyst is not particularly limited, but considering the stability and efficiency of the catalyst, structures such as ball shape, tablet shape, granule shape, pellet shape, etc. can be applied. In this case, the size (or diameter) of the catalyst can be, for example, in the range of about 0.1 mm to 10 mm, specifically about 0.5 mm to 5 mm, more specifically about 1 mm to 3 mm, but this can be understood as an exemplary purpose.
[0046] The platinum-supported alumina catalyst according to this embodiment can enhance the hydrogenation / dehydrogenation reaction activity for a wide range of liquid organic hydrogen carriers, and in particular can improve the reversibility of the hydrogenation / dehydrogenation reaction. Furthermore, due to the improved interaction between the metal components constituting the catalyst, the catalyst can maintain good catalytic activity (i.e., long-term stability) even under continuous repeated operation of the hydrogenation / dehydrogenation reaction, which distinguishes it from conventional platinum-supported catalysts (typically manufactured by impregnation methods).
[0047] [Preparation of catalyst] According to another embodiment of the present disclosure, there is provided a method for preparing a hydrogenation / dehydrogenation catalyst for liquid organic hydrogen carriers, in which platinum, an active metal, is supported on an alumina support in the form of a combination of single atoms and clusters.
[0048] In this regard, when a platinum / alumina supported catalyst is prepared by the impregnation method commonly used in the prior art, platinum is present in the form of particles on the alumina support, and a relatively high content of platinum must be supported in order to exhibit a desired activity. However, in the catalyst preparation method according to this embodiment, a solvent is not used, which is required for preparing a metal precursor solution in the impregnation method (a method of preparing a liquid metal precursor solution, contacting it with a porous inorganic oxide support (specifically, alumina), and fixing or attaching the metal precursor to the pores of the support), and platinum having a mixture of monoatomic and cluster forms is selectively and uniformly dispersed on the alumina-containing support through a simple method of reacting platinum precursor and alumina precursor in a single step and subsequently performing heat treatment (specifically, heat treatment under an oxygen-containing atmosphere), thereby improving the activity and reversibility of hydrogenation / dehydrogenation reactions, and further, a catalyst having excellent hydrogenation / dehydrogenation activity during liquid or gas phase reactions can be prepared not only for liquid organic hydrogen carriers having nitrogen-containing heterocycles, but also for liquid organic hydrogen carriers consisting of only hydrocarbons.
[0049] Furthermore, in order to improve the long-term stability of the catalyst, a strong interaction between the active metal and the support is required, and it is preferable to disperse and support the active metal as uniformly as possible on the support. As a metal oxide-based support, an alumina support is basically strongly bonded to the precursor of the active metal, and is therefore known to be effective in terms of catalyst stability. However, in the case of γ-alumina, which is widely used as an alumina support by the impregnation method, it is difficult to provide properties (particularly the specific surface area) for uniformly dispersing the active metal in fine sizes such as single atoms and clusters. In addition, even when platinum is supported by the impregnation method using alumina having a relatively high specific surface area as a support, there is a limit to dramatically increasing the specific surface area of the final catalyst due to the characteristics of the manufacturing method, and it is still difficult to reduce the platinum size to the single atom level.
[0050] According to one embodiment, first, a precursor mixture is prepared that includes at least one alumina precursor, at least one platinum precursor, and a base component.
[0051] For example, the precursor mixture may be prepared by mixing the three components simultaneously. Alternatively, the precursor mixture may be prepared by mixing two of the three components first and then adding the remaining components. For example, the alumina precursor and the base component may be mixed first, and then the platinum precursor may be added and mixed.
[0052] According to an exemplary embodiment, the platinum precursor may be an organic or inorganic salt of platinum, a complex, or a combination thereof. Examples of such platinum precursors include PtF6, PtF4, [PtF5]4, PtCl3, PtCl4, Pt6Cl, etc. 12, PtBr3, PtBr4, PtI2, PtI3, PtI4, PtO, PtO2, PtO, PtS, PtS2, Pt(CO)4, [PtCl2(NH3)2], [PtCl 2(NH3)2], K2[PtCl6], K2[Pt(CN)4], PtCl4·5H2O, K[PtCl3(NH3)], Na2[PtBr6]·6H2O, (NH4) At least one of the platinum precursors may be used, but is not limited to, 2[PtBr6], K2[PtI6], (NH4)2[PtCl6], K2[Pt(CN)6], (NH4)2[PtCl4], K2[Pt(NO2)4], K[PtCl3(C2H4)]·H2O, [Pt(NH3)4](NO3)2, H2PtCl6, etc. According to a particular embodiment, the platinum precursor may be [Pt(NH3)4](NO3)2.
[0053] The alumina precursor may be an organic or inorganic salt of aluminum, an alkoxide, a complex, or a combination thereof, and a representative example thereof may be at least one selected from the group consisting of aluminum acetate, aluminum acetylacetonate, aluminum bromide, aluminum t-butoxide, aluminum sec-butoxide, aluminum pentoxide, aluminum ethoxide, aluminum isopropoxide, aluminum tributoxide, aluminum chloride, aluminum iodide, aluminum sulfate, aluminum nitrate, and hydrates thereof. More specifically, aluminum nitrate and / or its hydrate may be used as the alumina precursor.
[0054] According to an exemplary embodiment, the base component may be at least one selected from the group consisting of ammonium carbonate, ammonium bicarbonate, ammonium chloride, ammonium oxalate, ammonium sulfate, ammonium hydroxide, ammonium nitrate, lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide, and magnesium hydroxide, and more specifically, ammonium bicarbonate may be used. The reason for using a base in this manner is that, in forming a metal oxide from an acidic metal precursor, a neutralization reaction occurs in which a metal salt and water are formed as the base component is added and precipitated.
[0055] According to an exemplary embodiment, the molar ratio of platinum precursor / base component in the precursor mixture may be, for example, in the range of about 0.0001 to 0.1, specifically about 0.002 to 0.05, more specifically about 0.008 to 0.02. However, if the amount of base used is too small or too large, the time required for gel formation, which is the final stage of synthesis, will be shorter or longer, making it difficult to form a metal oxide having a desired crystal phase, and it may be advantageous to appropriately adjust the amount within the above range to the extent that it may affect the properties of the catalyst, such as the specific surface area, the degree of dispersion of the metal, and the size of the particles. However, the range may be changed depending on the type of precursor and base. In addition, the mixing ratio between the platinum precursor and the alumina precursor in the precursor mixture may be determined by the respective contents of the alumina support and platinum in the above catalyst.
[0056] According to one embodiment, the reaction can be carried out while adding external energy during the process of preparing the precursor mixture or after forming the physical mixture, and unlike the impregnation method, the reaction between the precursors in solid phase form is carried out without using a solvent. In this way, by inducing stronger interactions between the metal precursors (platinum precursor and inorganic oxide (alumina) precursor) through the solid phase method, when the calcination or heat treatment conditions are adjusted after the solid phase reaction as described below, the clumping (or agglomeration) phenomenon of platinum can be significantly reduced, and in particular, platinum can be supported on the alumina support in the form of a combination of single atoms and clusters.
[0057] According to one embodiment, the external energy applied to carry out the solid-state reaction between the above-mentioned three components may typically be physical or mechanical energy, for example, in the form of frictional energy such as milling, grinding, or crushing, specifically, frictional energy by ball milling, but this is merely exemplary, and any external energy may be utilized without particular limitation as long as it can induce a reaction between the platinum precursor and the alumina precursor under a solvent-free condition.
[0058] According to an illustrative embodiment, the solid-phase reaction under the application of the external energy may be carried out for, for example, about 5 minutes to 40 minutes, specifically about 10 minutes to 30 minutes, and more specifically about 13 minutes to 25 minutes, but this can be understood as an illustrative example, and the reaction time can be changed depending on the reaction scale, etc.
[0059] At this time, a solid-phase reaction between the precursors may proceed, forming a gel-type solid catalyst. Specifically, during the solid-phase reaction process or during mixing under the application of external energy (e.g., frictional energy), the base component is partially or completely decomposed, and when the metal precursor is in the form of a metal salt, an anion or anion species bound to the metal cation may be replaced with a hydroxide group. During this process, gas derived from the precursor and the base may be released. For example, when ammonium bicarbonate is used as the base, a large amount of carbon dioxide may be generated. As the reaction proceeds under this gas release, each precursor forms a gel, and then undergoes a process of increasing hardness due to solidification and then forming a gel again, resulting in a gel-type solid catalyst.
[0060] Next, the catalyst solid formed from the solid-state reaction may be heat-treated, i.e., calcined, in an oxygen-containing atmosphere (specifically, air atmosphere) to convert the gel-type catalyst solid into an oxide. Through this heat treatment, platinum may be uniformly dispersed in the pores of the alumina support. It should be noted that platinum monoatoms and clusters may be supported on the alumina support in an appropriate ratio by controlling the heat treatment conditions to affect the crystallinity of platinum. In this regard, when the heat treatment time is shortened or the heating rate is decreased, the ratio of platinum in monoatomic form tends to increase.
[0061] However, as mentioned above, when only platinum in the form of a single atom is supported, the activity resulting from the single atom catalyst is improved, but platinum aggregates under the heating conditions accompanying the hydrogenation / dehydrogenation reaction of the liquid organic hydrogen carrier, which is undesirable in terms of long-term stability. Therefore, in this embodiment, by adjusting the heat treatment time and / or heating rate during the catalyst preparation process by the solid phase method, platinum is supported in a form in which a single atom and a cluster are combined, so that the catalytic activity and reversibility of the hydrogenation / dehydrogenation reaction can be maintained at a good level, and long-term stability can be ensured even in repeated operations of storing / releasing hydrogen. This corresponds to an unexpected effect at the level of knowledge regarding existing catalysts.
[0062] According to an exemplary embodiment, the content of cluster forms in platinum supported in the catalyst can be determined, for example, through observation by HAADF-STEM (specifically, dark-field HAADF-STEM). In this regard, the number of monatoms and clusters in platinum supported in the catalyst (most of the supported platinum exists as monatoms and clusters, but nanoparticles having a size larger than the cluster (e.g., about 2 nm to 8 nm, specifically about 2.5 nm to 6 nm, more specifically about 3 nm to 5 nm) may also be included, in which case the number of monatoms, clusters, and nanoparticles) can be measured to calculate the relative ratio (content) of the cluster form. In this case, the content of nanoparticles having a size larger than the cluster in platinum can be, for example, about 20% or less, specifically about 10% or less, more specifically about 5% or less.
[0063] According to one embodiment, the content of cluster form in platinum supported on an alumina carrier may be adjusted, for example, in the range of about 10% to 55%, specifically about 12% to 50%, more specifically about 15% to 40%. According to a specific embodiment, the content of cluster form in platinum, which is an active metal, may be adjusted in the range of about 20% to 35%, specifically about 22% to 30%. In this regard, if the content of cluster form in platinum deviates from a certain range (i.e., if the content of single atoms is too high or too low), the dehydrogenation reaction activity decreases and it is difficult to improve the reversibility of the hydrogenation / dehydrogenation reaction, so it may be advantageous to set the heat treatment conditions so that the content of cluster form is adjusted within the above-mentioned range.
[0064] According to an exemplary embodiment, the heat treatment may be performed under a temperature condition of, for example, about 300° C. to 800° C., specifically about 400° C. to 750° C., more specifically about 500° C. to 700° C. In this case, it may be advantageous to appropriately adjust the heating rate, for example, about 1° C. / min to 15° C. / min (specifically, about 1.5° C. / min to 12° C. / min, more specifically, about 2° C. / min to 10° C. / min), and the heat treatment time, for example, within a range of about 3 hours to 60 hours (specifically, about 5 hours to 50 hours, more specifically, about 10 hours to 40 hours) in consideration of the desired ratio of single atoms and clusters.
[0065] On the other hand, after the heat treatment under oxygen atmosphere, a reduction treatment can be additionally performed to activate the catalyst for the final use of hydrogenation / dehydrogenation reaction. According to an exemplary embodiment, hydrogen, carbon monoxide, methane, or a combination thereof can be used as the reduction gas, and the reduction treatment can be more typically performed under a hydrogen atmosphere.
[0066] For example, the reduction temperature may be in the range of about 300°C to 600°C (specifically, about 350°C to 550°C, more specifically, about 400°C to 500°C). At this time, the heating rate may be in the range of about 1°C / min to 10°C / min, specifically, about 4°C / min to 6°C / min. The reduction time may be set in the range of about 1 hour to 10 hours, specifically, about 2 hours to 5 hours. In addition, the pressure during the reduction (partial pressure of the reducing gas) is not particularly limited, but may be in the range of about 1 bar to 5 bar, specifically, about 1.5 bar to 4 bar, more specifically, about 2 bar to 3 bar. The above-mentioned reduction conditions can be understood as examples, and are not necessarily limited thereto. Through the above-mentioned reduction treatment, a catalyst in which platinum, which is an active metal, is supported on the alumina support in, for example, a fully reduced (i.e., elemental) state or a partially reduced (or oxidized) state, specifically, in a fully reduced state, can be produced.
[0067] [Hydrogenation / dehydrogenation reactions using liquid organic hydrogen carrier compounds (storage and release of hydrogen)] According to an embodiment of the present disclosure, a liquid organic hydrogen carrier (LOHC) can be used as a hydrogen storage material, and such a liquid organic hydrogen carrier system is composed of hydrogen-lean and hydrogen-rich organic compounds, and can store and release hydrogen through repeated liquid or gas phase catalytic hydrogenation and dehydrogenation cycles. In particular, by handling hydrogen in the form of a liquid organic hydrogen carrier, existing fuel equipment can be utilized, and unlike hydrogen storage by hydrogenation of gas (e.g., carbon dioxide or nitrogen), when hydrogen is released from a liquid organic hydrogen carrier, pure hydrogen can be produced after condensation of a carrier compound having a relatively high boiling point.
[0068] According to this embodiment, a catalyst in which platinum is supported on an alumina support in the form of a combination of single atoms and clusters can be used to carry out reversible hydrogenation / dehydrogenation reactions of liquid organic hydrogen carriers (LOHCs).
[0069] According to an exemplary embodiment, the above-mentioned platinum-supported catalyst can be effectively applied to a wide range of liquid organic hydrogen carriers, including nitrogen-containing heterocyclic liquid organic hydrogen carriers and liquid organic hydrogen carriers made of hydrocarbons (specifically, aromatic hydrocarbon-based liquid organic hydrogen carriers such as dibenzyltoluene). Such compounds typically have at least one conjugated bond in the molecule.
[0070] According to one embodiment, the liquid organic hydrogen carrier may be at least one compound (hydrogen-lean form) selected from the compounds represented by the following general formulas 1 to 9:
[0071] [ka]
[0072] [ka]
[0073] [ka]
[0074] [ka]
[0075] [ka]
[0076] [ka]
[0077] [ka]
[0078] [ka]
[0079] [ka]
[0080] In the above formula, R, R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 and R 18 Each of is hydrogen or a C1 to C6 alkyl group, and X is -(CHR 19 ) n - (n is an integer from 1 to 3, R 19 is H, OH, or a C1 to C6 alkyl group; and Y is CH or N.
[0081] The liquid organic hydrogen carrier compounds exemplified above may have a melting point of, for example, about 100° C. or less, specifically about 0° C. to 80° C., more specifically about 10° C. to 60° C., and therefore may maintain a liquid phase at room temperature, and a boiling point may be about 380° C. or less, specifically about 130° C. to 350° C., more specifically about 180° C. to 300° C. Due to such melting and boiling point characteristics, the hydrogen storage and release system using the liquid organic hydrogen carrier has an advantage in that it is possible to omit the use of a separate solvent and / or additive for improving reactivity.
[0082] As described above, a catalyst in which platinum as an active metal is supported on an alumina carrier in a mixed form of single atoms and clusters is suitable for storing and releasing hydrogen by repeating the hydrogenation / dehydrogenation cycle of a liquid organic hydrogen carrier.
[0083] The hydrogen storage and release method according to the exemplary embodiment may involve contacting an organic compound (specifically, in a liquid phase form) that is a liquid organic hydrogen carrier with the platinum-supported alumina catalyst described above in a reaction system. For example, the ratio (M / R) of active metal (Pt) / LOHC in the catalyst may be determined, for example, in the range of about 0.05 mol% to 0.4 mol%, specifically about 0.07 mol% to 0.35 mol%, more specifically about 0.1 mol% to 0.3 mol%. In this case, the M / R ratio may be distinguished between hydrogenation and dehydrogenation reactions, and may be set relatively high in the hydrogenation reaction, while being set relatively low in the dehydrogenation reaction. In this regard, if the M / R ratio is too low, there is a limit to lowering the activation energy of the reaction, and therefore insufficient reaction activity may be exhibited. On the other hand, if the M / R ratio is too high, the solid-phase catalyst increases considerably in volume compared to the liquid-phase reactants, forming an excessively slurried state, which not only makes stirring during the reaction difficult, but also causes diffusion limitations, which can lead to insufficient utilization of the active sites of the catalyst. Therefore, it may be advantageous to appropriately adjust the M / R ratio within the above range. However, the ratio may vary depending on the type of hydrogen storage compound used.
[0084] As an example, the M / R ratio in the hydrogenation reaction (hydrogen storage) can be adjusted, for example, in the range of about 0.1 mol% to 0.4 mol% (specifically, about 0.15 mol% to 0.35 mol%, more specifically, about 0.2 mol% to 0.3 mol%), while the M / R ratio in the dehydrogenation reaction (hydrogen release) can be adjusted, for example, in the range of about 0.05 mol% to 0.15 mol% (specifically, about 0.07 mol% to 0.13 mol%, more specifically, about 0.09 mol% to 0.12 mol%).
[0085] In this regard, a hydrogenation reaction can be performed to store hydrogen in a hydrogen storage material (liquid organic hydrogen carrier), and the hydrogenation reaction temperature can be, for example, about 50° C. to 250° C., specifically about 80° C. to 220° C., and more specifically about 100° C. to 190° C. The hydrogenation reaction pressure can be, for example, about 5 bar to 100 bar, specifically about 20 bar to 80 bar, more specifically about 25 bar to 70 bar, and particularly about 30 bar to 50 bar. In addition, the hydrogenation reaction time is not particularly limited, and can be, for example, about 0.5 hours to 24 hours, specifically about 1 hour to 12 hours, and more specifically about 1.5 hours to 6 hours.
[0086] According to an illustrative embodiment, by using the above-described platinum / alumina supported catalyst, the hydrogenation reaction efficiency (defined as the number of moles of hydrogen stored by the actual hydrogenation reaction relative to the number of moles of hydrogen that can be theoretically stored in one mole of dehydrogenation reactant) can be, for example, at least about 62%, specifically at least about 90%, more specifically at least about 96%, while the selectivity to the hydrogenation product corresponding to the hydrogen storage compound can be, for example, at least about 58%, specifically at least about 90%, more specifically at least about 99%.
[0087] Meanwhile, a dehydrogenation reaction may be performed to release hydrogen from a hydrogen storage material (liquid organic hydrogen carrier). Since the dehydrogenation reaction is an endothermic reaction, it may be performed at a higher reaction temperature (for example, a temperature range that is about 50° C. to 150° C., specifically about 60° C. to 120° C., and more specifically about 80° C. to 100° C. higher than the hydrogenation reaction temperature) compared to a hydrogenation reaction (exothermic reaction) of the same hydrogen storage material. According to an exemplary embodiment, the dehydrogenation reaction temperature may be, for example, about 100° C. to 350° C., specifically about 150° C. to 320° C., and more specifically about 180° C. to 290° C. In addition, unlike the reaction temperature, the dehydrogenation reaction pressure may be at a lower level compared to the pressure conditions of the hydrogenation reaction, for example, about 1 bar to 10 bar, specifically about 1 bar to 5 bar, and more specifically, may be at normal pressure. The dehydrogenation reaction time is not particularly limited, but may be set, for example, in the range of about 0.5 hours to 24 hours, specifically about 2 hours to 12 hours, and more specifically about 3 hours to 8 hours.
[0088] According to illustrative embodiments, by using the above-described catalysts, the dehydrogenation reaction efficiency (defined as the number of moles of hydrogen produced by the actual dehydrogenation reaction relative to the number of moles of hydrogen that can be theoretically released by one mole of hydrogenation reactant) can be, for example, at least about 50%, specifically at least about 60%, and more specifically at least about 86%.
[0089] Meanwhile, according to one embodiment, the hydrogenation / dehydrogenation reaction may be carried out using any reactor known in the art, such as a batch reactor, a continuous reactor, a semi-continuous reactor, etc. In particular, in the case of liquid organic hydrogen carriers, especially liquid organic hydrogen carrier compounds having a relatively high boiling point, the reactor may be equipped with an agitator since the hydrogenation and dehydrogenation reactions may occur in the liquid phase. According to an exemplary embodiment, the reaction may be carried out in a fixed bed reactor using a particulate catalyst.
[0090] The present invention can be more clearly understood by the following examples, which are merely for illustrative purposes of the present invention and are not intended to limit the scope of the invention. EXAMPLES
[0091] In the examples and comparative examples, the catalysts prepared were analyzed by the following methods.
[0092] [Transmission electron microscope (TEM, HAADF-STEM) analysis] Using a transmission electron microscope (TEM, HAADF-STEM, JEOL, TEM2100F), a sample dispersed in methanol was dropped onto a Cu grid test piece, which was then dried in a vacuum oven at 60°C for more than 20 hours, and the size of the metal particles supported on the carrier was measured.
[0093] [Crystalline state analysis of Pt metal (CO-DRIFT)] For CO-DRIFT (chemisorbed diffuse reflectance infrared Fourier transform) spectroscopy, a Nicolet 6700 FT-IR (equipped with a Harrick Praying Mantis high temperature reaction chamber) was used. Prior to the measurement, 30 mg of sample was heated at 500 °C for 1 h in 5% H2 / Ar (100 cm 3 min -1 After reduction, the temperature was lowered to 50°C and the gas was replaced with Ar gas to remove the substances physically adsorbed on the surface of the sample. 3 min -1 The sample was exposed to a flow of CO for 30 minutes, and then the sample was subjected to evacuation for 30 minutes to desorb the adsorbed CO, followed by IR analysis.
[0094] [Example] [Production of platinum / alumina catalyst by solid phase method] First, 21.84g of Al precursor (Al(NO3)3·9H2O), 13.88g of ammonium bicarbonate (NH4HCO3), and 20.182g of Pt metal precursor [Pt(NH3)4](NO3) were added to a mortar without a solvent and then physically mixed. The physical mixture was then stirred for 20 minutes to apply frictional heat, during which the solid precursors were mixed a total of three times, generating a large amount of CO2 and forming a gel. 10 minutes after mixing, the mixture hardened as it solidified again in the form of a gel, and 6 minutes later it softened and formed a gel again.
[0095] Next, the gel solids mixed for 20 minutes were placed in a crucible and calcined at a heat treatment temperature of 600°C for 5 hours (heating rate: 2°C / min). After calcination, reduction treatment was performed using hydrogen (500°C, 5°C / min, 3 hours), and reaction activity in the presence of the reduced catalyst was compared (the platinum / alumina catalyst prepared according to the embodiment was represented as M3PtA x_y (x: calcination temperature, y: calcination time)) (platinum loading: 3 wt%). In addition, platinum / alumina catalysts with various platinum loadings (1 wt%, 2 wt%, and 5 wt%) were prepared by the same procedure and their activity was evaluated.
[0096] Comparative Example [Production of platinum / alumina catalyst by impregnation method] 3g of commercial γ-Al2O3(gA) was mixed uniformly with 0.182g of 3wt% Pt metal precursor solution ([Pt(NH3)4](NO3)2) and 2ml of distilled water.) was physically supported through impregnation method, dried in an oven at 100℃, and then placed in a crucible and fired for 5 hours (600℃, 2℃ / min). Then, hydrogen reduction treatment (500℃, 3 hours, heating rate 5℃ / min) was performed, and finally, 3Pt / gA x_y (x: firing temperature, y: firing time) catalyst was obtained (platinum loading 3wt%). In addition, platinum / alumina catalysts with various platinum loadings (1wt%, 2wt%, and 5wt%) were prepared by the same procedure and their activity was evaluated.
[0097] [A. Analysis of catalyst properties and reaction activity by synthesis method] [Catalyst physical property analysis] FIG. 1 shows XRD patterns of the platinum-supported catalyst (MPtA) according to the embodiment (solid phase method) and the platinum-supported catalyst (Pt / gA) according to the comparative example (impregnation method) with various platinum contents (1 wt%, 2 wt%, 3 wt%, and 5 wt%).
[0098] According to the figure, even with the same platinum content, the size of platinum crystals differed depending on the synthesis method. In the case of the catalyst prepared by the impregnation method (Comparative Example), the crystal sizes of Pt(111), (200), and (220) were large even with a low platinum content of 1 wt%. On the other hand, in the case of the catalyst prepared by the solid phase method (Example), only Pt(111) crystals were formed even when 5 wt% platinum was supported, which indicates that platinum is more uniformly distributed in the catalyst according to the Example compared to the Comparative Example.
[0099] Meanwhile, dark-field HAADF-STEM photographs of the platinum-supported catalyst (MPtA) according to the embodiment (solid phase method) and the platinum-supported catalyst (Pt / gA) according to the comparative example (impregnation method), which have various platinum contents (1 wt%, 2 wt%, 3 wt%, and 5 wt%), are shown in Figures 2a and 2b, respectively.
[0100] As can be seen in the figure, platinum single atoms and clusters are relatively non-uniformly distributed in the catalyst of the example, while in the catalyst of the comparative example, platinum had a particulate form even when supported at a low content of 1 wt %.
[0101] FIG. 3 shows CO-DRIFT spectrum graphs for the platinum-supported catalyst (MPtA) according to the embodiment (solid phase method) and the platinum-supported catalyst (Pt / gA) according to the comparative example (impregnation method) with various platinum contents.
[0102] According to the figure, in the case of the catalyst according to the embodiment, 2090 cm -1 , 2070cm -1 and 2040cm-1 On the other hand, the catalyst according to the comparative example had a peak at 2070 cm -1 2060cm corresponding to the peak -1 The peak at 2090 cm corresponding to a single atom was relatively larger. -1 The peak was hardly observed even when 1 wt % of platinum was supported.
[0103] FIG. 4 is a graph showing the H2-TPD results for the platinum-supported catalyst (MPtA) according to the embodiment (solid phase method) and the platinum-supported catalyst (Pt / gA) according to the comparative example (impregnation method) with various platinum contents (1 wt%, 2 wt%, 3 wt%, and 5 wt%) supported thereon.
[0104] Referring to the drawing, the degree of hydrogen desorption according to the platinum content was compared by H2-TPD. As a result, in the catalyst of the embodiment, the hydrogen desorption peak tended to shift from 500°C to around 200°C as the platinum content increased, whereas in the catalyst of the comparative example, almost no change was observed in the desorption section.
[0105] In order to more accurately analyze the form of platinum, EXAFS analysis was performed, and the results are shown in Table 1 below and FIG.
[0106] According to the tables and figures, when compared with the fitting results of the reference materials Pt foil and PtO2, the catalysts according to the examples showed patterns almost similar to PtO2 even when the platinum content was increased, while the catalysts according to the comparative examples showed patterns similar to Pt foil.
[0107] [Table 1]
[0108] According to the table, many Pt-Pt bonds were observed in the catalysts according to the comparative examples, whereas many Pt-O, Pt-O-Pt and Pt-O-Al bonds were present in the catalysts according to the examples at low platinum contents, and a tendency was observed that the number of Pt-Pt bonds increased as the platinum content increased.
[0109] [Reaction activity analysis] The efficiency of hydrogenation (reaction conditions: M / R 0.22 mol%, 35 bar, 150°C, and 2 hours) and dehydrogenation (reaction conditions: M / R 0.1 mol%, 250°C, and 4 hours) reactions for the catalysts prepared in the Examples and Comparative Examples are compared in Tables 2 and 3 below, and FIG. 6 shows the results.
[0110] [Table 2]
[0111] a : Calculation results through GC analysis. b Hydrogen storage efficiency = (full hydrogenation product [mol] x 6H2 + single-ring hydrogenation product [mol] x 3H2) / (reactant [mol] x 6H2) x 100%
[0112] [Table 3]
[0113] a : Calculation results through GC analysis. b Hydrogen release efficiency = (full dehydrogenation product [mol] x 6H2 + single-ring dehydrogenation product [mol] x 3H2) / (reactant [mol] x 6H2) x 100%
[0114] Referring to the above results, in the case of the catalysts according to the examples, the catalyst carrying 3 wt% platinum showed the best activity in both hydrogenation and dehydrogenation reactions. On the other hand, in the catalysts according to the comparative examples, the catalyst carrying 1 wt% platinum showed the best activity, which is believed to be due to the increase in platinum size as the amount of platinum carried increases. In particular, it is believed that such a difference in activity is caused by the difference in the size of platinum particles carried on the alumina carrier depending on the catalyst manufacturing method.
[0115] [B. Analysis of catalyst properties and reaction activity according to calcination conditions] [Catalyst physical property analysis] The calcination conditions were changed from 600°C, 5h (heating rate 2°C / min) to 5h (heating rate 10°C / min), 20h (heating rate 2°C / min), and 40h (heating rate 2°C / min), and the size change of the platinum catalyst supported at 1wt% and 3wt% was observed. XRD patterns, H2-TPD results, and HAADF-STEM images of the Pt-supported catalysts (supporting amounts: 1wt% and 3wt%) under different calcination conditions are shown in Figures 7 and 8, respectively.
[0116] In the figure, the results of XRD analysis showed that when the calcination temperature (600°C) and calcination time (5h) were fixed and the heating rate was changed from 2°C / min to 10°C / min, the Pt(111) peak increased in all platinum catalysts loaded with 1wt% and 3wt%. In addition, when the calcination temperature (600°C) and the heating rate (2°C / min) were fixed and the calcination time was changed from 5h to 20h and 40h, respectively, the Pt(111) peak increased relatively in all platinum catalysts loaded with 1wt% and 3wt%, although the increase was smaller than the change in the heating rate. In addition, the H2-TPD analysis showed that the hydrogen desorption peak shifted to a lower temperature as the platinum size increased.
[0117] On the other hand, as confirmed by the HAADF-STEM results in Figure 8, in the case of the M1PtA (same as M1PtA c6005 h_2) catalyst in Figure 2, platinum single atoms were mainly observed, while when the calcination time was increased to 40 h and the heating rate to 10 °C / min, the ratio of clusters increased and particle morphology was also observed. Considering the above results, it is suggested that the calcination conditions affect the crystallinity of the metal, which corresponds to the main variable that can adjust the size of platinum.
[0118] [Reaction activity analysis] The hydrogenation and dehydrogenation reaction activities of the Pt-supported catalysts were measured according to the calcination conditions, and the results are shown in Table 4 (hydrogenation reaction conditions: M / R 0.22 mol%, 35 bar, 150°C, 2 hours) and Table 5 (dehydrogenation reaction conditions: M / R 0.1 mol%, 250°C, 4 hours) below, and in FIG. 9.
[0119] [Table 4]
[0120] a : Calculation results through GC analysis. b Hydrogen storage efficiency = (full hydrogenation product [mol] x 6H2 + single-ring hydrogenation product [mol] x 3H2) / (reactant [mol] x 6H2) x 100%
[0121] [Table 5]
[0122] a : Calculation results through GC analysis. bHydrogen release efficiency = (full dehydrogenation product [mol] x 6H2 + single-ring dehydrogenation product [mol] x 3H2) / (reactant [mol] x 6H2) x 100%
[0123] Referring to the table and the figure, the catalyst M1PtA c600 5h_2, which has a high ratio of platinum single atoms, showed a storage efficiency of 62.5% and a release efficiency of 33.7% in hydrogenation and dehydrogenation reactions, respectively. On the other hand, the catalyst M1PtA c600 40h_2, which had an increased calcination time during catalyst production, showed an improved storage efficiency of 75.2% and a release efficiency of 83.5%.
[0124] [C. Analysis of catalyst stability using synthetic methods] [Evaluation of dehydrogenation reaction activity and changes in the physical properties of catalysts after use] In order to evaluate the long-term stability of the catalyst, the activity of the dehydrogenation reaction was evaluated. The results of the dehydrogenation reaction to evaluate the long-term stability of the catalyst for each of the platinum-supported catalyst (M3PtA) according to the embodiment (solid phase method) and the platinum-supported catalyst (3Pt / gA) according to the comparative example (impregnation method) are shown in Figure 10. In addition, the XRD patterns before and after the reaction of each of the platinum-supported catalyst (M3PtA) according to the embodiment and the platinum-supported catalyst (3Pt / gA) according to the comparative example, and the HAADF-STEM photographs of the catalyst after use are shown in Figure 11.
[0125] Referring to the figure, the catalyst (3Pt / gA) according to the comparative example rapidly decreased in catalytic activity when reused five times. In addition, after the reaction, the state of the metal particles of the catalyst was observed by XRD and HAADF-STEM. As a result, the XRD patterns of the catalyst (M3PtA) according to the embodiment before and after use were almost the same, and the STEM analysis showed that platinum single atoms and clusters were still relatively non-uniformly distributed. This is believed to be due to the strong interaction between platinum and the alumina support in the catalyst (M3PtA) according to the embodiment. Meanwhile, in the case of the 3Pt / gA catalyst, the initial hydrogen release efficiency (55.7%) decreased by about two times to 27.4% after reuse five times. This is believed to be due to the weakening of the interaction between platinum and the alumina support and the increase in particle size due to platinum sintering.
[0126] [Evaluation of reversibility of hydrogenation / dehydrogenation reactions] Platinum is active in both hydrogenation and dehydrogenation reactions, so hydrogen storage and release efficiency can be achieved even when the same type of catalyst is used in a single reactor. Since the interaction between the active metal and the support differs depending on the synthesis method, it was determined that this would also affect the continuous reversible reaction, so hydrogenation and dehydrogenation reactions were continuously repeated three times. In this regard, the hydrogen storage and release efficiency of H0-BT for the catalyst according to the embodiment (M3PtA) and the catalyst according to the comparative example (3Pt / gA) was measured and compared, and the results are shown in Figure 12.
[0127] Referring to the figure, under the same hydrogenation and dehydrogenation reaction conditions, the catalyst according to the embodiment (M3PtA) consistently maintained the initial hydrogen storage and release efficiency, whereas the catalyst according to the comparative example (3Pt / gA) showed a consistent decrease in hydrogen storage and release efficiency.
[0128] [D. Evaluation of dehydrogenation reaction activity by type of liquid organic hydrogen carrier] Dehydrogenation reactions were carried out using various types of pyridine- and bipyridine-based liquid organic hydrogen carriers, and the results are shown in Table 6 below.
[0129] [Table 6]
[0130] As can be seen from the table, the catalyst according to the embodiment (M3PtA 600 5h) showed improved reaction efficiency compared to the catalyst according to the comparative example (3Pt / gA 600 5h), regardless of the liquid organic hydrogen carrier.
[0131] [E. Evaluation of dehydrogenation reaction activity based on the cluster content (ratio) of platinum in the catalyst] Platinum-supported catalysts were prepared by the solid-phase method while changing the heat treatment conditions (heat treatment temperature, time, and heating rate) (platinum loading: 1 wt%, 3 wt%, and 5 wt%). The number of single atoms and clusters (additionally nanoparticles larger than clusters) was measured from dark-field HAADF-STEM images, and the content of clusters in the supported platinum was calculated. The results are shown in Table 7 below (reaction conditions: 250°C, 1 bar, 4 hours, precious metal (mol) / reactant (mol) 0.1%).
[0132] [Table 7]
[0133] In the above table, the firing conditions corresponding to a are 600°C, 5 hours (heating rate: 2°C / min), the firing conditions corresponding to b1 are 600°C, 40 hours (heating rate: 2°C / min), and the firing conditions corresponding to b2 are 600°C, 5 hours (heating rate: 10°C / min).
[0134] According to the above table, when the cluster content in the supported platinum is too low (M1PtA a : 4.8%) or when the cluster content is excessively high (M5PtA b2The hydrogen desorption efficiencies of M3PtA and M4PtA were low at 36.2% and 35.2%, respectively. On the other hand, when the cluster content was adjusted to an appropriate range, good hydrogen desorption efficiencies could be obtained, especially for M3PtA b1 The catalyst (cluster content: 22.6%) achieved a high hydrogen release efficiency of 86.9%.
[0135] Simple variations and modifications of the present invention are readily accessible to those of ordinary skill in the art, and all such variations and modifications are to be considered as falling within the scope of the present invention.
Claims
1. A catalyst for hydrogenation / dehydrogenation of a liquid organic hydrogen carrier, comprising: an alumina support; and Platinum, including monoatomic and cluster forms, as the active metal supported on said alumina-containing support; Including, The platinum content (element basis) in the catalyst is 0.01% to 10% by weight, A catalyst in which the content of platinum in cluster form in the supported platinum ranges from 10% to 55%.
2. The catalyst of claim 1, wherein the platinum in the catalyst has a size of 5 nm or less.
3. The alumina support in the catalyst is at least 300 mm 2 BET specific surface area of 0.4 cm 3 / g~0.55cm 3 2. The catalyst according to claim 1, characterized in that it has a pore volume of 1000 nm / g and a pore size of 3 nm to 4.5 nm.
4. 2. The catalyst according to claim 1, wherein the content of platinum in cluster form in the supported platinum ranges from 22% to 30%.
5. 10. The catalyst of claim 1, wherein the catalyst contains platinum crystals having (111) faces and is in a reduced state.
6. A method for producing a hydrogenation / dehydrogenation catalyst for a liquid organic hydrogen carrier, comprising the steps of: a) carrying out a solid-state reaction in the absence of a solvent while applying external energy to a mixture containing at least one alumina precursor, at least one platinum precursor, and a base component to form a catalytic solid in the form of a gel; and b) heat treating the catalytic solid in an oxygen-containing atmosphere to deposit platinum, including both monoatomic and cluster forms, on the alumina-containing support; Including, The platinum content in the catalyst (on an elemental basis) is in the range of 0.01% to 10% by weight, The method according to claim 1, wherein the content of platinum in the cluster form in the supported platinum ranges from 10% to 55%.
7. 7. The method according to claim 6, wherein the heat treatment temperature in the heat treatment step of step b) is adjusted in the range of 300° C. to 800° C., the heating rate is adjusted in the range of 1° C. / min to 15° C. / min, and the heat treatment time is adjusted in the range of 3 hours to 60 hours.
8. c) further comprising a step of reducing the heat-treated catalytic solid to convert platinum to a fully reduced state or a partially reduced state; The method according to claim 6, wherein the reduction temperature is adjusted in the range of 300° C. to 600° C., the heating rate is adjusted in the range of 1° C. / min to 10° C. / min, and the reduction time is adjusted in the range of 1 hour to 10 hours.
9. 7. The method of claim 6, wherein the platinum precursor / base component molar ratio in step a) is in the range of 0.0001 to 0.
1.
10. A hydrogenation step in which hydrogen is stored in a liquid organic hydrogen carrier in the presence of a catalyst; and a dehydrogenation step of releasing hydrogen from the hydrogenated liquid organic hydrogen carrier in the presence of a catalyst; The catalyst used in at least one of the hydrogenation step and the dehydrogenation step is an alumina support; and Platinum, including monoatomic and cluster forms, as the active metal supported on said alumina-containing support; Including, A catalyst in which the platinum content (element basis) in the catalyst is 0.01% by weight to 10% by weight, and the content of platinum in cluster form in the supported platinum is in the range of 10% to 55%, The hydrogenation step and the dehydrogenation step are alternately performed to store and release hydrogen.
11. The method according to claim 10, wherein the liquid organic hydrogen carrier is at least one selected from the compounds represented by the following general formulas 1 to 9: [Formula 1] [Case 2] [C3] [C4] [C5] [C6] [C7] [C8] [C9] In the above formula, R, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 and R 18 Each of 1 ~C 6 and X is an alkyl group represented by -(CHR 19 ) n - (n is an integer from 1 to 3, R 19 is H, OH, or C 1 ~C 6 and Y is CH or N.
12. 12. The method of claim 11, wherein the liquid organic hydrogen carrier has a melting point of 100°C or less and a boiling point of 380°C or less.
13. The method according to claim 10, wherein the ratio (M / R) of active metal (Pt) to liquid organic hydrogen carrier in the catalyst is adjusted in the range of 0.05 mol % to 0.4 mol %.
14. 14. The process according to claim 13, characterized in that the ratio M / R in the hydrogenation step is adjusted in the range of 0.1 mol% to 0.4 mol%, while the ratio M / R in the dehydrogenation step is adjusted in the range of 0.05 mol% to 0.15 mol%.
15. The hydrogenation step is carried out at a temperature of 50° C. to 250° C. and a pressure of 5 bar to 100 bar; 15. The method according to claim 14, characterized in that the dehydrogenation step is carried out at a temperature of 100°C to 350°C and a pressure of 1 bar to 10 bar.
16. 11. The method of claim 10, wherein the hydrogenation step has a hydrogenation reaction efficiency of at least 62% and the dehydrogenation step has a dehydrogenation reaction efficiency of at least 50%.
Citation Information
Patent Citations
Catalyst containing metal clusters in structurally collapsed zeolite and use thereof
JP2016520419A
Hydrogen storage material and manufacturing method therefor
JP2008095172A
Hydrogen occlusion material
JP2011131120A
KR2015-97558
KR20200117354A