Apparatus and method for producing doped diamond layers - Patents.com

A plasma-free CVD process using solid precursors and thermal-impact excitation enables safe and uniform doped diamond coating on various substrates, overcoming health risks and substrate damage issues.

JP2024536002AActive Publication Date: 2024-10-04CARBONCOMPETENCE GMBH +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024513905
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-22
Filing Date
2022-10-21
Publication Date
2024-10-04
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

Existing CVD processes for producing doped diamond coatings use gaseous or liquid precursors that pose health and safety risks, and plasma activation can damage the substrate, making homogeneous coating of three-dimensional objects difficult.

Method used

A plasma-free CVD process using a solid precursor other than carbon, activated by thermal and impact excitation, to deposit a uniform doped diamond layer on substrates.

Benefits of technology

This method avoids health and safety hazards while achieving uniform and efficient deposition of high-purity doped diamond layers on both two- and three-dimensional substrates, with high excitation rates and controlled doping concentrations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536002000001_ABST
    Figure 2024536002000001_ABST
Patent Text Reader

Abstract

The invention relates to an apparatus (1) and a process for applying a doped diamond layer to a substrate (2, 2a) by chemical vapor deposition. The apparatus (1) comprises a deposition chamber for holding the substrate (2, 2a), a gas active element (7) in the form of a hollow body with a passage (7b) for a process gas, in particular hydrogen, an outlet opening (16) leading from the passage (7b) to the deposition chamber (3), a heating device (8) for heating the wall (7a) of the gas active element (7) surrounding the passage (7b) and a solid precursor other than carbon in the passage (7b).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an apparatus and method for applying a doped diamond layer to a substrate by chemical vapor deposition. [Background technology]

[0002] Chemical vapor deposition (CVD) processes allow the coating of surfaces of complex three-dimensional shapes, since even the finest recesses and hollow bodies can be coated uniformly inside. Various CVD diamond coating techniques differ mainly in gas activation and gas dissociation methods. The main characteristics are the growth rate, the coating area and the quality of the diamond layer. Usually, high growth rates are limited to very small coating areas. The "hot filament" process (HFCVD process) is established for coating three-dimensional complex substrates, since this process can also be used to coat three-dimensional substrates on larger surfaces. Plasma processes are mainly used for two-dimensional substrates (e.g., Si wafers), since the localized electric field enhancement and the denser plasma arise on the three-dimensional surface, which does not allow the layer to be deposited homogeneously.

[0003] WO 2018 / 064694 A1 describes a CVD apparatus and a CVD process for applying a carbon layer, in particular a diamond layer, to a substrate. A process gas, hydrogen or a mixture of hydrogen and a carbon-containing gas is introduced into the gas inlet and into the flow passage of the gas activation element. The process gas is activated by a combination of thermal and impact excitation and then flows in a locally controlled manner through an outlet opening into a deposition chamber in which the substrate is located. This combination of thermal and impact excitation of the process gas results in a significantly higher excitation rate of atomic hydrogen, a higher growth rate, a uniform deposition of the carbon layer (diamond layer) on the substrate, and a better control of the coating process, which is particularly advantageous for large coating areas and / or substrates with complex shapes.

[0004] Single crystal diamond is highly electrically insulating and -18It has the lowest specific conductivity in S / m of all known substances. Diamond layers can be doped using CVD processes to adjust the electrical, optical and structural properties. By suitable doping (e.g. with elements of the IVth, Vth and VIth main groups; with transition metals; with elements of the IVth, Vth and VIth subgroups), diamond can be made semiconducting (p-type or n-type). Conductive diamond layers are used, for example, as semiconductor materials, electrode materials in electrochemistry, materials for transducers, for example for sensors, or in microsystem technology (MEMS), or as coating layers, for example on printed circuit boards, for wear detection, or for contact drilling.

[0005] Impurity atoms can replace both C atoms in regular lattice sites and therefore have a purely extrinsic character. Impurity atoms such as H, Li, B, N, O, Ne, P, Si, As, Ti, Cr, Ni, Co, Zn, Zr, Ag, W, Xe and Tl are known to form optically active centers in diamond (AM Zaitsev, Optical Properties of Diamond: Data Handbook, 1st ed., Springer, 2001). In polycrystalline diamond layers, grain boundaries play an even more important role in doping. In general, the aim is to "incorporate" the impurity atoms into the diamond lattice. The smaller the deposited diamond crystals, the higher the number of grain boundaries between the crystals associated with a given region. These grain boundaries contain in particular non-diamond-like carbon (e.g., trans-polyacetylene; Frederik Klauser, Doris Steinmuller-Nethl et al.: Raman Studies of Nano- and Ultra-nanocrystalline Diamond Films Grown by Hot-Filament CVD, Chemical Vapour Deposition, Vol. 16, Issue 4-6, pp. 127-135, 2010). Thus, preferably in nanocrystalline diamond films (crystallites in the range of 2-100 nm), boron can be incorporated not only in the diamond lattice but also in the amorphous grain boundaries.

[0006] The use of boron-doped diamond layers in particular is widespread because boron atoms have an atomic radius similar to that of carbon atoms, meaning that the lattice distortion in incorporating boron atoms into a carbon lattice is relatively low. Since boron has three outer electrons, one less than carbon, boron acts as an electron acceptor for the carbon lattice, and boron-doped diamond is p-conductive. Boron has a very low ionization energy of 0.37 eV, which means that boron-doped diamond achieves good electrical conductivity even at room temperature.

[0007] As described in US 2013 / 0234165 A1, a solid, liquid or gaseous boron source can be used in the CVD process to deposit a boron-doped diamond layer. The use of liquid or gaseous (usually toxic) boron sources is particularly widespread. In US 10,487,396 B2, CN 108396309 A, CN 111778506 A and CN 111304690 A, a gaseous boron-containing precursor is used, while in CN 108565124 B, trimethyl borate is used as the liquid boron-containing precursor. In CN 104862663 A, for example, acetone is used as the carbon source and trimethyl borate is used as the liquid boron source, which deposits a boron-doped nanodiamond film with a layer thickness of 1 to 10 μm on a single crystal silicon substrate.

[0008] The large-scale use of non-carbon liquid or gaseous precursors in CVD processes is often associated with health risks. For example, boron or boron compounds such as diborane (also called borethane) or trimethylborate are highly toxic and absorption into the human body can lead to chronic intoxication or damage to the central nervous system and skin. Diborane is also highly pyrophoric and explosive, and can cause severe burns, while trimethylborate is highly corrosive, damaging equipment used in CVD processes and shortening its useful life if used for long periods of time.

[0009] The use of solid non-carbon precursors (instead of liquid or gaseous ones) in CVD processes has significant safety and health advantages. Several publications have disclosed methods for producing doped diamond films using solid non-carbon precursors in CVD processes.

[0010] In the methods described in CN 111945131 A and CN 112063996 A, solid boron carbide particles are evenly distributed around the substrate. Hydrogen, argon, and methane are used as process gases. Activation with microwave plasma produces boron and carbon radicals from the boron carbide particles, depositing a boron-doped diamond layer on the substrate surface. In CN 110527973 A, a carbon source (graphite powder) and a boron source (boron powder or boron oxide powder) are mixed and pressed into a bulk material in the formation of a wafer. In the CVD process, several of these wafers are evenly placed around the substrate and a gas is supplied, either hydrogen or a mixture of hydrogen, methane, and an inert gas. The gas is activated by microwave radiation to generate a plasma.

[0011] In summary, CVD processes known in the prior art for producing doped diamond coatings usually use gaseous or liquid precursors other than carbon, which entail health and safety risks. In the few known CVD processes that use solid precursors other than carbon, the process gas is exclusively activated by plasma. However, plasma activation can damage the crystal structure of the substrate material, making homogeneous coating of three-dimensional objects very difficult. Summary of the Invention

[0012] It is therefore an object of the present invention to produce a doped diamond layer in a plasma-free CVD process using a solid precursor other than carbon, thus avoiding the disadvantages of the CVD processes known from the prior art.

[0013] This problem is solved by an apparatus according to claim 1 and a method according to claim 8. Preferred embodiments are set forth in the dependent claims.

[0014] The present invention relates to an apparatus for applying a doped diamond layer to a substrate by chemical deposition, the apparatus comprising a deposition chamber for receiving the substrate, a gas-active element in the form of a hollow body having a flow passage for a process gas, in particular hydrogen, an outlet opening leading from the flow passage to the deposition chamber, a heating device for heating the walls of the gas-active element surrounding the flow passage, and a solid precursor other than carbon in the flow passage.

[0015] The invention also relates to a method for applying a doped diamond layer to a substrate by chemical vapour deposition, comprising the steps of: (a) providing a deposition chamber with a substrate and a gas-active element in the form of a hollow body having a flow passage; (b) providing a solid-state precursor other than carbon in the flow channel; (c) heating a wall surrounding the flow passage of the gas active element with a heating device; (d) introducing a process gas, in particular hydrogen, into the flow passage of the gas-active element; (e) activating the process gas by impact excitation and thermal excitation, and activating the precursor by thermal excitation; (f) introducing active process gases and active precursors into the deposition chamber through the exit ports of the gas active element; (g) Depositing a doped diamond layer onto the substrate.

[0016] The invention also relates to the use of an apparatus for thermal and impingement excitation of process gases and for thermal excitation of solid precursors other than carbon to deposit doped diamond layers on a substrate by chemical vapour deposition.

[0017] Surprisingly, it has been found that by providing a solid, non-carbon precursor in the flow path of the gas-active element of the CVD apparatus according to the invention, it is possible to deposit a uniform, doped diamond layer on the substrate. By using a solid, non-carbon precursor for doping, it is possible to completely avoid the negative effects on health and / or process safety that occur with liquid or gaseous, non-carbon precursors. Using a combined activation by thermal activation and impact excitation, it is possible to deposit a uniform doped diamond layer even on three-dimensional substrates.

[0018] A process gas, preferably hydrogen or a mixture of hydrogen and another gas, such as a carbon-containing gas, is supplied to the gas-active element, which is preferably arranged perpendicularly thereto, via a gas supply element. The gas-active element is a hollow body formation with lateral surfaces, which has a flow passage for the process gas and a wall surrounding the flow passage, which is heated by a heating device. The process gas is preferably introduced into the flow passage of the gas-active element via two gas supply elements arranged in the two end regions of the side surfaces of the gas-active element. This ensures a uniform distribution of the process gas in the flow passage of the gas-active element.

[0019] The wall of the gas-active element is preferably heated over its entire length by a heating device in order to ensure a uniform temperature distribution. For this purpose, the wall of the gas-active element is connected to a heating device which heats the wall of the gas-active element. The wall of the gas-active element is preferably heated by a resistive heater. This allows a simple and precise control of the heating process.

[0020] The process gas and the solid precursors other than carbon, which are arranged in the flow passage of the gas-active element, are preferably heated to at least 2000° C., preferably at least 2200° C., particularly preferably at least 2400° C., to achieve good thermal excitation of the process gas. The process gas, particularly preferably hydrogen, is activated by impact excitation and thermal excitation, whereas the solid precursors other than carbon are activated by thermal excitation. The activated process gas and the activated solid precursors are then transported through at least one outlet opening of the gas-active element to the substrate arranged in the deposition chamber.

[0021] The cross-sectional area of ​​the flow path is 0.1 to 50 mm 2 The range is preferably 5 to 30 mm. 2A range of is particularly preferred. This increases the impact excitation with the wall surface. The flow passage of the gas active element is preferably closed at both ends, for example by end bodies, so that the gas active element has no other openings apart from the inlet and outlet openings. The ratio between the area of ​​exactly one outlet opening and the cross-sectional area of ​​the gas active element is preferably 1:5 to 1:20, in particular 1:10, which further increases the excitation rate of the process gas. Due to the small number of openings and the flow passages closed at both ends, the partial pressure in the flow passage of the gas active element is significantly increased, which is many times higher than the pressure of the deposition chamber. In addition to the thermal excitation, this high partial pressure also allows the impact excitation (i.e. collision induced dissociation) of the process gas, which is preferably hydrogen, resulting in a very high yield of atomic hydrogen. This combined activity consisting of thermal and impact excitation can achieve an excitation rate of atomic hydrogen of more than 80%, whereas thermal excitation alone results in an excitation rate of up to 30%. This high excitation rate, combining thermal and impact excitation, allows an accelerated growth of high purity doped diamond layers and an energy-efficient deposition of high growth rates.

[0022] The mean free path length of the hydrogen radicals can be increased to several centimeters due to the high excitation rate by a combination of thermal and impact excitation, which allows the distance between the gas active element and the substrate to be increased, significantly improving the homogeneity of the deposited doped diamond layer.

[0023] In a preferred embodiment of the present invention, the solid precursor other than carbon is preferably selected from the group comprising boron, silicon, lithium, sodium, phosphorus, nitrogen, sulfur, arsenic or combinations thereof. These elements are particularly suitable for doping diamond layer, for example for incorporation into diamond lattice, and allow the diamond layer to be endowed with specific properties, such as electrical conductivity. The solid precursor can be provided in various forms, for example in the form of particles (e.g., flakes, powder) or in the form of wire. Since boron-doped diamond layer has very good electrical conductivity, the solid precursor other than carbon is preferably a boron-containing precursor. Due to the ease of handling, boron-containing particles, boron-containing wire or combinations thereof are particularly preferred or preferred as solid precursor.

[0024] When a boron-containing wire is used as a solid precursor in the present invention, its diameter is preferably in the range of 0.05-2.2 mm, particularly preferably in the range of 0.1-0.5 mm. This makes it possible to vary and very precisely adjust the degree of doping in order to customize the properties of the deposited doped diamond layer. Furthermore, this range of diameters ensures that the reservoir of solid precursor in the flow channel is available for a long time, allowing the production of doped diamond layers with greater layer thicknesses.

[0025] In a preferred embodiment, the boron-containing wire is arranged essentially along the entire length of the flow passage of the gas active element. This results in a particularly uniform and homogeneous doping of the entire diamond layer. Furthermore, several, preferably two or three, boron-containing wires are preferably provided as solid precursors in the flow passage of the gas active element. This not only ensures very good process control, but also the deposited doped diamond layer is very homogeneous.

[0026] The structure or chemical composition of the solid precursor can be changed to adjust the doping concentration accordingly. For example, in the case of a boron-containing wire, the core of the wire can be composed of a chemical element or compound other than boron, such as tungsten or tantalum. This not only ensures stable process control, but also achieves the best results in terms of homogeneity and electrical conductivity of the boron-doped diamond layer.

[0027] According to the desired doping concentration, a corresponding amount of solid precursor is provided in the flow passage and can be evaporated in a controlled manner using process parameters. The doping concentration in the diamond layer can be influenced in a controlled manner by various parameters. On the one hand, the doping concentration can be controlled by process parameters, such as the flow rate, temperature and pressure of process gas, both in the flow passage and in the deposition chamber. On the other hand, the doping concentration can be influenced by the geometry of the device according to the invention, such as the number and / or geometry of the outlet openings, and the distance of the substrate from the gas active element, as well as the amount of solid precursor.

[0028] Due to the preferably horizontal arrangement of the gas active elements of the deposition chamber, the solid precursors can be arranged in the flow channels such that they rest at the bottom on the inside of the outer / lateral surfaces of the gas active elements. If the ends of the flow channels are closed, for example by end bodies, the solid precursors can alternatively also be attached to these closed ends and thus arranged in any possible position of the flow channels.

[0029] In a preferred embodiment of the invention, the gas inlet element for introducing an additional process gas, in particular a carbon-containing process gas, is arranged in the deposition chamber in such a way that the additional process gas flows over the heated wall of the gas-active element. The other, preferably carbon-containing process gas is preferably methane, but the use of other carbon-containing process gases such as ethylene or acetylene is also possible. This additional process gas is thermally activated by flowing over the heated wall of the gas inlet element, so that carbon-containing radicals, such as methyl radicals, are formed by homolytic fission. The effectiveness of the excitation is further increased by collisions of the activated hydrogen with the carbon-containing process gas. The highest possible excitation rate of hydrogen, which is achieved in the device according to the invention by combining thermal and impact excitation, is very important for achieving high excitation rates of the carbon-containing process gas. The formed carbon-containing radicals are sp 3 -Hybridized carbon (diamond) forms as well as spanned and / or sp 2 However, activated hydrogen atoms can be deposited on the substrate surface as sp -hybridized carbon. 2 Prevents or eliminates hybridization formation, so sp 3 Hybridization and thus the formation of pure doped diamond structures is promoted. The higher the amount of active hydrogen, the more effective the suppression or elimination of undesired hybridization. This allows the deposition of high-purity doped diamond crystals in the micrometer and / or nanometer range on the substrate.

[0030] The activated process gas, preferably hydrogen, and the activated precursor are introduced from the gas active element into the deposition chamber through outlet openings, which are preferably located on the outer / lateral surface of the gas active element. The outlet openings are preferably oriented sideways and not vertically downwards, in order to prevent the precursor from escaping in the molten state. Also, several outlet openings can be provided at a defined (regular or irregular) distance from each other, which are preferably arranged alternately at an angle to each other, to cover a larger volume range for coating. This is particularly advantageous when coating three-dimensional substrates. The shape and arrangement of the outlet openings depends on the required activity and flow rate. By having a large number of (preferably small) outlet openings, the process gas is distributed homogeneously in the deposition chamber, so that the deposited doped diamond layer has a very uniform thickness and a very high homogeneity. The advantageous arrangement and geometry of the outlet openings can be determined for the respective CVD apparatus by flow simulations. By arranging several outlet openings accordingly, the process gas can be introduced into the deposition chamber in a spatially evenly distributed manner, so that a homogeneous deposition is guaranteed over the entire substrate surface. The flow of the process gas together with the precursor through the outlet opening is not impeded due to the small particle size.Depending on the position of the substrate, the gas active element can be located above or to the side of the substrate.

[0031] Hydrogen and carbon-containing process gases can be introduced separately into the deposition chamber. Hydrogen is fed into the deposition chamber via a gas-active element and carbon-containing process gas is fed into the deposition chamber via a gas inlet element via a hot gas-active element. This provides greater flexibility with regard to the process parameters. For example, the separate introduction allows for spatially and / or temporally separated gas inlets. As a result, the temperature, the gas inlet rate into the deposition chamber, the time sequence and / or the concentration of these components of the process gas can be adjusted individually. These parameters can be optimized for coating processes with different requirements and can be adapted, for example, to the thickness of the doped diamond layer, its purity, grain size, concentration of doping, duration of the coating process, substrate material and / or substrate geometry.

[0032] Alternatively, the carbon-containing process gas can also be introduced into the deposition chamber together with the hydrogen through a gas activation element and activated by thermal excitation, which simplifies process control and equipment design since no gas inlet element is required to introduce the carbon-containing process gas into the deposition chamber.

[0033] The weight ratio of hydrogen to carbon-containing process gas is preferably in the range of 95:5 to 99.99:0.01, depending on the desired morphology. Additional process gases, such as nitrogen, oxygen and / or argon, can be used as needed to accelerate diamond growth, which can be provided by one or more gas injection / injection elements.

[0034] In order to favor the formation of the diamond layer on the surface of the substrate, the deposition chamber is preferably operated under reduced pressure. This ensures a high degree of purity and homogeneity of the deposited doped diamond layer. For this purpose, the deposition chamber is evacuated before and during the deposition process. For this purpose, a vacuum pump is preferably arranged outside the apparatus, which creates the vacuum necessary for the deposition process in the deposition chamber. The pressure in the deposition chamber is preferably in the range of 0.5-50 mbar, in particular 1-10 mbar. The partial pressure in the flow passages of the gas-active elements is therefore preferably a multiple of the pressure in the deposition chamber.

[0035] In known HFCVD processes, due to the low excitation speed of the process gases, a small distance between the gas active elements and the substrate must be selected (usually in the range of 5-10 mm), which leads to a highly non-uniform temperature distribution on the substrate surface, high temperatures, the occurrence of local concentrations of atomic hydrogen and, as a result, non-uniform coating. In the process according to the invention, the relatively high excitation speed of the process gases makes it possible to provide a larger distance between the gas active elements and the substrate surface, which is preferably in the range of 20-100 mm, particularly preferably in the range of 40-60 mm. In the process according to the invention, this larger distance between the gas active elements and the substrate ensures a uniform temperature distribution on the substrate surface.

[0036] Usable substrate materials include hard metals, silicon wafers, titanium implants, electrode materials (e.g., silicon, titanium, tantalum, tungsten, molybdenum, copper, niobium), graphite, sapphire, high melting point glasses and / or quartz. To further improve adhesion of the coating, the surface of the substrate material can also be pretreated, if necessary, for example to increase roughness and thus mechanical anchoring / adhesion.

[0037] The substrate temperature ranges from 500 to 950 °C depending on the substrate and coating parameters. Preferably, substrate temperatures in the range of 750 to 850 °C are used, which allows the deposition of a very homogeneous and doped diamond layer. It should be noted that at lower temperatures (lower than the preferred temperature range, e.g. below 600 °C), the growth rate is correspondingly lower. This may require adjustment of the process parameters. The substrate to be coated can be placed inside the deposition chamber in a substrate holder, which is preferably located below or to the side of the gas active elements in the operating conditions of the deposition chamber. Depending on the temperature resistance / stability of the substrate, the substrate holder can be connected to a cooling device. Due to the possibility of cooling the substrate and the relatively large distance between the substrate and the gas active elements, more temperature-sensitive substrates such as glass can also be coated, whereby the substrate temperature for more temperature-sensitive substrates is preferably in the range of 500 to 700 °C. This allows the deposition of a homogeneously doped diamond layer, thereby simultaneously avoiding damage to the more temperature-sensitive substrates.

[0038] The orientation of the gas-active elements can preferably be adapted to the shape of the substrate. The gas-active elements are preferably arranged horizontally in the deposition chamber and thus parallel to the substrate surface. This ensures a uniform distance between the gas-active elements and the substrate, so that the doped diamond layer has a uniform thickness over the entire substrate surface, especially in the case of two-dimensional substrates. The gas-active elements can also be arranged inside the hollow substrate to be coated (e.g. inside the forming tool or drawing die) or on the side of a complex 3D substrate. By arranging several outlet openings on the corresponding side of the gas-active elements, then a uniform coating of the inside of the hollow substrate or 3D structure is possible.

[0039] In a preferred embodiment of the invention, the deposition chamber is provided with several gas-active elements. This is advantageous, for example, for the coating of large-area substrates, such as silicon wafers, or for the coating of three-dimensional substrates. It is also possible to coat several substrates simultaneously. The heating device can be designed in such a way that the gas-active elements can be heated separately, together or in several groups. Also, the various gas-active elements can be connected to separate gas supply lines, and different process gases can be supplied to the deposition chambers of the individual gas-active elements. In this way, the properties of the coating can be adjusted locally, for example the doping concentration in the doped diamond layer, and the resulting properties, such as electrical conductivity.

[0040] The shape and arrangement of the gas-active elements or gas-active elements can be of any design and are preferably oriented to the shape of the substrate to be coated. If several gas-active elements are used, they are preferably arranged parallel to each other. This allows a uniform coating of the entire substrate surface. When coating a two-dimensional substrate, all gas-active elements are preferably arranged parallel and at the same distance from the substrate. By selecting the respective distances accordingly, a uniform temperature distribution and therefore a uniform coating of the substrate is ensured.

[0041] The substrate, which is located on a substrate holder under the gas active system, is preferably moved in a horizontal plane. The substrate, which is arranged on the side of the gas active element, can be moved by rotation. Naturally, the speed at which the substrate is moved is adapted to the process parameters.

[0042] All embodiments of the present invention are interrelated and any disclosed embodiments and / or features may be combined with each other, or any combination of two or more embodiments and / or features may be provided.

[0043] For purposes of this disclosure, the designations "top," "apex," "bottom," "bottom," "upper," "upper," "lower," "lower" and the like refer to the intended operating condition of the CVD apparatus.

[0044] In this application, the term "process gas" refers to both a single gas (such as hydrogen) and a gas mixture (composed of hydrogen and another gas, such as a carbon-containing gas), unless expressly disclosed otherwise.

[0045] The invention is further explained below with reference to preferred embodiments in the drawings and description, but is not limited thereto. [Brief description of the drawings]

[0046] [Figure 1] FIG. 1 shows an apparatus according to the invention for applying a doped diamond layer to a substrate by chemical deposition. [Figure 2a] FIG. 2a shows gas active elements with different numbers of wires provided as solid precursors other than carbon. [Figure 2b] FIG. 2b shows gas active elements with different numbers of wires provided as solid precursors other than carbon. [Figure 3a] FIG. 3a shows gas active elements with different numbers of wires provided as solid precursors other than carbon. [Figure 3b] FIG. 3b shows gas active elements with different numbers of wires provided as solid precursors other than carbon. [Figure 4a] FIG. 4a shows gas active elements with different numbers of wires provided as solid precursors other than carbon. [Figure 4b] FIG. 4b shows gas active elements with different numbers of wires provided as solid precursors other than carbon. [Figure 5a] Figure 5a shows an SEM image of a boron doped diamond layer. [Figure 5b] Figure 5b shows an SEM image of the boron doped diamond layer. [Figure 5c]Figure 5c shows an SEM image of the boron doped diamond layer. [Figure 5d] Figure 5d shows an SEM image of the boron doped diamond layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0047] Figure 1 shows an apparatus 1 for applying a doped diamond layer to a substrate 2, 2a. In the design shown, the doped diamond layer is deposited on the one hand on the outside of the substrate 2 and on the other hand on the inside of the substrate 2a. The apparatus 1 comprises a deposition chamber 3 for holding the substrate 2, 2a. Also provided is a gas and electricity supply element 4. The gas and electricity supply element 4 comprises an inner element 5a for supplying a process gas (preferably hydrogen) and an outer element 5b made of a conductive material for supplying an electric current.

[0048] As can also be seen from Fig. 1, the gas and electricity supply element 4 inside the deposition chamber 3 is connected via a clamp screw connection 6 to a gas active element 7 arranged horizontally in the arrangement shown so that process gases can be supplied to the gas active element 7 via an inner element 5a of the gas and electricity supply element 4. Inside the gas active element there is a solid precursor other than carbon, which is provided in the form of a wire 11. Furthermore, a heating device 8 is shown (only diagrammatically), by means of which the wall 7a of the gas active element 7 is heated.

[0049] In the embodiment shown in FIG. 1, the heating device 8 has a power supply 8a (only symbolically shown) and is able to conduct an electric current to the gas active element 7 via the outer element 5b of the gas and electricity supply element 4. The electric current is converted into heat by the resistance of the material of the gas active element 7, which heats up the gas active element 7. The wall 7a of the gas active element 7 is heated such that the flow passage 7b of the gas active element is heated to at least 2000° C. As a result, the process gas is activated by thermal and impact excitation and the solid precursor is activated by thermal excitation. For this purpose, the wall 7a of the gas active element 7 consists of a high-temperature resistant material. An electric insulator 9, for example of a ceramic material, is also provided between the outer element 5b of the gas and current supply element 4 and the housing of the deposition chamber 3.

[0050] FIG. 1 also shows a gas inlet element 10, which in the version shown in the figure is arranged vertically at the top of the deposition chamber 3, through which a carbon-containing process gas (preferably methane) can be introduced into the deposition chamber 3. The carbon-containing process gas is thermally excited by flowing through the heated wall 7a of the gas active element 7, which results in the generation of carbon-containing radicals (e.g. methyl radicals). Alternatively, the carbon-containing process gas can be introduced into the deposition chamber 3 together with hydrogen in a defined mixture ratio via the heated gas active element 7 and thereby activated. Other process gases, for example nitrogen, oxygen or argon, can also be supplied via other gas inlet elements (not shown). A substrate holder 13, on which the substrate 2, 2a is arranged, is arranged inside the deposition chamber 3 and below the gas active element 7. The substrate holder 13 can be heated or cooled via a temperature control element 14 (schematically shown).

[0051] Figures 2a, 3a and 4a show an embodiment of a gas-active element 7, the flow passage 7b of which is provided longitudinally with a solid precursor other than carbon in the form of a wire 11. Figures 2b, 3b and 4b each show a section through the gas-active element 7. It can be seen that Figures 2-4 differ in the number of wires 11 provided in the flow passage 7b. In Figure 2, one wire 11 is provided in the flow passage 7b, in Figure 3, two wires 11 are provided and in Figure 4, three wires 11 are provided.

[0052] As further shown in Figures 2a-4b, the gas active element 7 has inlet openings 15 in each of the two end regions, through which the process gas (preferably hydrogen) is fed into the flow channels 7b of the gas active element 7. In addition, the gas active element 7 has a number of outlet openings 16 arranged in the longitudinal direction of the gas active element 7, laterally on its lateral surfaces. The activated process gas and the activated precursors are channeled through these outlet openings 16 in the direction of the substrates 2 and 2a, the direction of flow being indicated by the arrows 17. Furthermore, end bodies 18 for closing the flow channels 7b at the ends of the gas active element 7 are diagrammatically visible.

[0053] Figure 5a-d show SEM images of a boron-doped, microcrystalline diamond layer on a tungsten carbide-cobalt hard metal tool (WC-Co hard metal tool) with a layer thickness of 10 μm. A boron wire type B 005915 from Goodfellow Cambridge Ltd., UK was used in the flow passage of the gas activation element. Hydrogen and methane were used as process gases in a weight ratio of 99.8:0.2. The pressure in the deposition chamber was 1 mbar and the substrate temperature was 850 °C. In Figure 5a, a boron wire was used as a solid precursor (type B 005915, Goodfellow Cambridge Ltd., UK). Figure 5b-d show the doped diamond layer, for the production of which two boron wires (type B 005915) were used as solid precursors, at different magnifications.

[0054] (Example) The following examples are intended to further illustrate the invention as described in this application without limiting the scope of the invention.

[0055] WC-Co hard metal tools were coated with diamond coatings of different boron concentrations. One to three boron-containing wires (type B 005915, Goodfellow Cambridge Ltd., UK) were used as solid precursors in the flow passages of the gas-active elements. These were continuous monofilaments with a tungsten core (core diameter 5 μm), wire diameter 0.2 mm and wire length 140 mm. The process parameters were kept constant for all coatings. Hydrogen and methane were used as process gases in a weight ratio of 99.8:0.2. The pressure in the deposition chamber was 1 mbar and the substrate temperature was 850 °C.

[0056] The concentration of boron atoms in the boron-doped diamond layer produced according to the present invention was determined using secondary ion mass spectrometry (SIMS). 20 ~10 21 / cm 3 The boron concentration was measured and it varied depending on the penetration depth (up to 1.5 μm). As shown in Table 1, the sheet resistance and resistivity of the boron doped diamond layer significantly decreased with increasing number of boron-containing wires (used in the production of the boron doped diamond layer according to the invention) and correspondingly with increasing boron concentration, resulting in a significant increase in electrical conductivity.

[0057] Table 1 shows the resistance measurements (two-point method, length 10 mm) of diamond coatings produced with different numbers of boron wires (microcrystalline diamond coating, coating thickness 10 μm, substrate: WC-Co hard metal). [Table 1]

Claims

1. An apparatus (1) for applying a doped diamond layer by chemical vapor deposition to a substrate (2, 2a), comprising: a deposition chamber containing said substrate (2, 2a); a gas-active element (7) in the form of a hollow body having a flow passage (7b) for a process gas, in particular hydrogen, an outlet opening (16) leading from said flow passage (7b) to the deposition chamber (3); a heating device (8) for heating the wall (7a) of the gas active element (7) surrounding the flow passage (7b); a solid, non-carbon precursor within said channel (7b); An apparatus (1) comprising:

2. 2. The apparatus (1) according to claim 1, characterized in that the solid precursor is selected from the group comprising boron, silicon, lithium, sodium, phosphorus, nitrogen, sulfur, arsenic, and combinations thereof.

3. 3. The apparatus (1) according to claim 2, characterized in that at least one of boron-containing particles, boron-containing wires and combinations thereof is provided as the solid precursor, preferably a boron-containing wire.

4. 4. The device (1) according to claim 3, characterized in that the boron-containing wire is arranged longitudinally of the flow channel (7b), preferably along substantially the entire length of the flow channel (7b).

5. The device (1) according to claim 3 or 4, characterized in that the boron-containing wire has a diameter in the range of 0.05 to 2.2 mm, preferably in the range of 0.1 to 1 mm.

6. 6. Apparatus (1) according to any one of claims 3 to 5, characterized in that several, preferably two or three, of the boron-containing wires are provided as the solid precursor.

7. Apparatus (1) according to any one of the preceding claims, characterized in that the deposition chamber (3) is provided with a plurality of said gas-active elements (7).

8. A method for applying a doped diamond layer to a substrate (2, 2a) by chemical vapour deposition, comprising the steps of: (a) providing a deposition chamber (3) with said substrate (2, 2a) and with a gas-active element (7) in the form of a hollow body having a flow passage (7b), (b) providing a solid, non-carbon precursor inside the flow channel (7b); (c) heating the wall (7a) of the gas active element (7) surrounding the flow path (7b) with a heating device (8); (d) introducing a process gas, in particular hydrogen, into the flow passage (7b) of the gas-active element (7); (e) activating a process gas by impulse excitation and thermal excitation, and activating the precursor by thermal excitation; (f) introducing the activated process gas and the activated precursor into the deposition chamber (3) through an outlet opening (16) of the gas-activating element (7); (g) depositing said doped diamond layer onto said substrate (2, 2a). The method includes:

9. 9. The method of claim 8, wherein the solid precursor is selected from the group including boron, silicon, lithium, sodium, phosphorus, nitrogen, sulfur, arsenic, and combinations thereof.

10. 10. The method of claim 8 or 9, wherein at least one of boron-containing particles, boron-containing wires, and combinations thereof is provided as the solid precursor, preferably a boron-containing wire.

11. 11. The process according to any one of claims 8 to 10, characterized in that a gas inlet element (10) for introducing a further process gas, in particular a carbon-containing process gas, is arranged in the deposition chamber (3) such that said further process gas flows through a heated wall (7a) of the gas-active element (7).

12. 8. Application of the device (1) according to any one of claims 1 to 7 for the thermal excitation of a solid precursor other than carbon, for the application of a doped diamond layer on a substrate (2, 2a) by thermal excitation, impingement excitation and chemical vapour deposition of process gases.

Citation Information

Patent Citations

  • Formation of thin diamond film

    JP1994345592A

  • Manufacture of field emitter array

    JP1995272618A

  • Diamond film for lithography and manufacture thereof

    JP2001077016A

  • Microwave plasma CVD system and method for producing diamond film

    JP2005298293A

  • Diamond semiconductor and method for producing the same