Methods and apparatus for making carbon nanomaterials and methods using lithium-free electrolytes - Patents.com

By employing lithium-free electrolytes and non-lithium promoting elements, the method addresses the cost and environmental issues of lithium-based CNT production, achieving efficient and high-yield carbon nanomaterial synthesis with improved properties.

JP2024536143AInactive Publication Date: 2024-10-04C2CNT LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024519306
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-29
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing carbon nanotubes (CNTs) using lithium-containing electrolytes are costly due to the high price of lithium, leading to high operating costs and a significant carbon footprint.

Method used

The use of lithium-free electrolytes, such as binary or ternary mixtures of carbonates, in an electrolytic process to produce carbon nanomaterials, including CNTs, by introducing non-lithium promoting elements like transition metal nucleating agents and graphene defect agents to enhance nucleation and conductivity.

Benefits of technology

This approach reduces production costs and carbon footprint while achieving stable and high-yield production of CNTs and other carbon nanomaterials, allowing for the intercalation of larger cations and enhancing properties like electrical conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536143000001_ABST
    Figure 2024536143000001_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure relate to methods and apparatus for producing CNM products that may include carbon nanotubes (CNTs). The methods and apparatus utilize carbon dioxide (CO2) and a lithium-free carbonate electrolyte as reactants in an electrolysis reaction to produce CNTs. In some embodiments of the present disclosure, a graphene defect agent may be introduced into the electrolysis reaction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority from U.S. Provisional Patent Application No. 63 / 250,662, filed September 30, 2021, the entire disclosure of which is incorporated herein by reference.

[0002] Technical Field

[0002] The present disclosure relates generally to the production of carbon nanomaterials. In particular, the present disclosure relates to methods and apparatus for producing carbon nanomaterials using lithium-free electrolytes. [Background technology]

[0003] background Carbon nanotubes (CNTs) have the highest measured tensile strength of any material (strength 93,900 MPa). Multi-walled CNTs consist of concentric layers of cylindrical graphene sheets. Graphene is a nanotube with a thickness of about 0.335 nm, which corresponds to the thickness of one carbon atom. 2 Graphene is a two-dimensional honeycomb-structured material formed by a single layer of hybrid orbital carbon atoms. Graphite, nanotubes and fullerenes can be formed by wrapping and stacking graphene.

[0004]

[0004] CNTs have many useful properties, including high electrical conductivity, high thermal conductivity, flexibility, and they can also be chemically modified. These useful properties have led to a steady expansion of CNTs' applications. For example, low (typically <<1%) concentrations of CNTs in structural materials can increase the strength of a range of structural materials, such as cement, steel, and aluminum. Each of these materials can have a high carbon footprint, so a carbon composite with increased strength that requires less material can dramatically reduce the carbon footprint.

[0005]

[0005] A known process for producing CNTs is chemical vapor deposition (CVD). However, CVD of CNTs is expensive and has a high carbon footprint.

[0006]

[0006] In addition to chemical vapor deposition (CVD), electrolysis using carbon dioxide (CO2) and lithium carbonate electrolyte is also a known fabrication process for CNTs. In this electrolysis, an electrolysis potential of less than 1 volt can be utilized to decompose CO2 in a molten lithium carbonate solution to produce uniform CNT and carbon nanofiber products with high coulombic efficiency. 13 C) CO2 from the atmosphere can be directly converted to CNTs, as confirmed by tracing. Electrolysis in molten lithium carbonate can be carried out as direct carbon capture and conversion from air without CO2 preconcentration, or with exhaust gas CO2, or with concentrated CO2. Summary of the Invention [Problem to be solved by the invention]

[0007]

[0007] These known electrolytic reactions have only been demonstrated using lithium-containing carbonate electrolytes, such as pure molten lithium carbonate (Li2CO3, melting point about 723°C), or electrolytes in which a substantial fraction of Li2CO3 is mixed with other carbonates, such as sodium carbonate (Na2CO3), potassium carbonate (K2CO3), magnesium carbonate (MgCO3), calcium carbonate (CaCO3), barium carbonate (BaCO3), or Li2CO3 is mixed with other salts, including oxides, borates, sulfates, phosphates, or nitrates. It has generally been assumed that lithium cations may be a necessary component for making CNTs using molten carbonates and CO2 in electrolytic reactions. However, the cost of lithium generally results in high operating costs for these electrolytic reactions, so additional methods and systems for producing graphitic carbon nanomaterials are desirable. [Means for solving the problem]

[0008] overview

[0008] Embodiments of the present disclosure relate to electrolytic methods and apparatus for producing carbon nanomaterial (CNM) products, including various nanostructures, including carbon nanotubes (CNTs). The methods and methods utilize CO2 and an electrolyte as reactants in an electrolytic reaction to make CNM products. In some embodiments of the present disclosure, the electrolyte is a binary mixture of two carbonates. In some embodiments of the present disclosure, the electrolyte is a ternary mixture of two carbonates and an oxide. In some embodiments of the present disclosure, the electrolyte is a mixture of more than three components. Embodiments of the present disclosure can be substantially less costly than electrolytic reactions using lithium-containing electrolytes.

[0009] Some embodiments of the present disclosure relate to a method of making a CNM product, the method including heating a lithium-free carbonate electrolyte to obtain a lithium-free molten carbonate electrolyte, positioning the molten carbonate electrolyte between an anode and a cathode of an electrolytic cell, utilizing one or more non-lithium promoting elements, applying a current to the cathode and the anode of the electrolytic cell, and collecting the CNM product from the cathode.

[0010]

[0010] In some embodiments of the present disclosure, the step of utilizing one or more non-lithium promoting elements can mean either adding one or more additional chemical components or modifying one or more reaction or operating conditions to modify the current or both adding additional chemical components or modifying one or more conditions.

[0011] In some embodiments of the present disclosure, the non-lithium promoting element is one or more of: (i) enhancing transition metal nucleation by adding one or more transition metal nucleating agents; (ii) adding one or more defect inducing agents; (iii) reducing or removing electrolyte conductivity inhibiting elements, or any combination thereof. In some embodiments, enhancing transition metal nucleation may be done by adding one or more transition metal nucleating agents. In some embodiments, the addition of defect inducing agents is done by adding tetrahedral sp 3 This may be due to the addition of one or more chemical agents that can induce graphene defects. Inducing defects in the graphene layers of the CNTs as synthesized may provide a mechanism by which larger cations can be used in a stable and high-yield CO2 electrolysis process to make CNTs and other CNM products. In some embodiments, removing electrolyte conductivity inhibitors may mean changing the voltage, current, and / or current density to enhance electrical conductivity.

[0012]

[0012] Some embodiments of the present disclosure relate to methods of selecting one or more structures of a CNM product. For example, some embodiments of the present disclosure relate to methods of producing a CNM product that includes a graphitic structure within the CNM product. For example, the graphitic CNM product includes a structure that includes a CNT, a carbon platelet structure, a graphene structure, a nano-onion structure, a nanosphere structure, a hollow nanosphere structure, or any combination thereof. By using embodiments of the present disclosure, the CNM product can be composed of some, most, substantially all, or all of the selected one or more graphitic structures.

[0013]

[0013] Some embodiments of the present disclosure relate to an apparatus that is an electrolytic cell for making one or more CNM products. The electrolytic cell includes one or more walls that define a plenum and an anode and a cathode positioned within the plenum. The plenum is configured to receive and hold a molten lithium-free carbonate electrolyte between the anode and the cathode. The electrolytic cell can be further configured to receive an electric current that can be applied to the anode and the cathode to initiate an electrolytic reaction to make the graphene defect agent, the nanomaterial select components, and the CNM products.

[0014]

[0014] In some embodiments of the present disclosure, the anode and cathode of the electrolysis cell are generally aligned in a horizontal plane, and they are vertically spaced apart from one another.

[0015]

[0015] Without being bound by any particular theory, it is known that when graphene is fabricated, it may contain various defects, including intrinsic defects and extrinsic defects. Intrinsic defects are non-sp 2 Orbital hybridization of carbon atoms often results in the presence of non-hexagonal rings surrounded by hexagonal rings. Reported intrinsic defects in graphene include Stone-Wales defects, single vacancy defects, multi-vacancy defects, line defects and carbon adatoms. Extrinsic defects can disrupt the crystalline order of graphene by including non-carbon atoms. Reported extrinsic defects in graphene include extrinsic adatoms and substitutional impurities.

[0016] Some embodiments of the present disclosure relate to exploiting defects in the graphene of the CNT layer to allow larger cations to flow through the graphene to promote CNT growth during CO2 electrolysis. Without being bound by any particular theory, some embodiments of the present disclosure more specifically exploit the induced defects or vacancies in the graphene layer to allow larger cations to flow through the graphene to promote CNT growth during CO2 electrolysis. 3 Regarding graphene defects: Tetrahedral sp 3Graphene defects can be induced by the presence of graphene defect agents such as oxides during the CO2 electrolysis reaction. Graphene sheet "vacancies" are known to enhance the degree of lithium cation intercalation and increase the storage capacity of lithium cation anode batteries. The graphene vacancies and oxide-induced defects in graphene can allow for the intercalation of not only Li cations but also larger cations such as sodium, magnesium, and calcium cations into graphene. Thus, such induced defects in the graphene layers of CNTs during synthesis can provide a mechanism by which cations other than lithium can be used in a stable and high-yield CO2 electrolysis process to make CNTs. In some embodiments, the introduction of high concentrations of oxides can induce larger defects in the growing CNM products.

[0017] Some embodiments of the present disclosure relate to the addition of a transition metal nucleating agent to a lithium-free electrolyte.

[0018] Some embodiments of the present disclosure relate to the use of low current densities to control conductivity during formation of CNM products.

[0019]

[0019] Some embodiments of the present disclosure relate to a system for synthesizing CNM products in a lithium-free environment. The system includes a heater for heating a lithium-free carbonate electrolyte to obtain a molten carbonate electrolyte, an electrolytic cell for receiving or containing the molten carbonate electrolyte between the anode and cathode of the electrolytic cell, one or more non-lithium promoting elements, and a current source for applying a current to the cathode and anode of the electrolytic cell. Without being bound by any particular theory, the system of the present disclosure may utilize the electrolytic cell apparatus described herein. Without being bound by any particular theory, the system of the present disclosure may be configured to perform the method described herein.

[0020]

[0020] By using CO2 from the atmosphere as a reactant in the electrolytic reactions of the present disclosure, embodiments of the present disclosure can reduce the greenhouse gas footprint of processes and systems for making CNTs and other CNM products. By using lithium-free carbonate electrolytes, the cost of making valuable CNM products can be significantly reduced. [Brief description of the drawings]

[0021]

[0021] These and other features of the present disclosure will become more apparent from the following detailed description, in which reference is made to the accompanying drawings.

[0022] [Figure 1] FIG. 1 is a phase diagram for mixtures of sodium carbonate (Na2CO3) and barium carbonate (BaCO3), some of which are for use as lithium-free carbonate electrolyte mixtures in embodiments of the present disclosure. [Figure 2A]

[0023] Two schematic diagrams depicting the proposed carbon nanotube (CNT) growth mechanisms on a cathode in a carbon dioxide (CO2) electrolysis reaction. The tip growth mechanism is shown. [Figure 2B]

[0023] The bottom growth mechanism is shown. [Figure 2C]

[0023] Raman spectra of carbon nanotube products electrolytically grown from electrolytes with (right) and without (left) Li2O. [Figure 3A]

[0024] 1 shows scanning electron microscopy (SEM) and high-resolution SEM images of a carbon nanomaterial (CNM) product part fabricated using lithium carbonate electrolyte. SEM image at first magnification. [Figure 3B]

[0024] Another SEM image at a first magnification. [Figure 3C]

[0024] A second higher magnification SEM image. [Figure 3D]

[0024] Another SEM image at a second magnification. [Figure 3E]

[0024] A high resolution SEM image at a first magnification. [Figure 3F]

[0024] A fourth higher magnification high resolution SEM image. [Figure 3G]

[0024] A fifth higher magnification high resolution SEM image. [Figure 4A]

[0025] 1 shows a photograph of a portion of an electrolytic cell and an SEM image of a CNM product portion produced therein by an electrolytic reaction according to an embodiment of the present disclosure. 2 shows a photograph of a set of vertically spaced anodes and cathodes and a bath forming a part of the electrolytic cell. [Figure 4B]

[0025] Another photograph of the anode and cathode positioned vertically spaced apart from each other. [Figure 4C]

[0025] The inner wall of the cell and the anode and cathode are shown after the electrolytic reaction. [Figure 4D]

[0025] FIG. 2 is an SEM image of a portion of a CNM product at a second magnification. [Figure 4E]

[0025] Another SEM image of a portion of the CNM product at a second magnification. [Figure 5A]

[0026] 1 shows photographs of an anode and cathode and an SEM image of a CNM product made according to an embodiment of the present disclosure. 2 shows a photograph of a vertical arrangement of an anode and cathode before an electrolysis reaction according to an embodiment of the present disclosure. [Figure 5B]

[0026] FIG. 5B is a photograph of the anode and cathode of FIG. 5A after the electrolysis reaction. [Figure 5C]

[0026] Shown is an SEM image of a portion of the CNM product at a sixth magnification. [Figure 5D]

[0026] A SEM image of a portion of carbon nanomaterial at a seventh magnification is shown. [Figure 5E]

[0026] A portion of carbon nanomaterial is shown at an eighth magnification. [Figure 6A]

[0027] 1 shows SEM images of electrolysis products in 1:1 wt % Na2CO3:BaCO3 with an electrolyte current density of 0.05 A / cm2, a planar Nichrome anode and a planar brass cathode at 770° C. SEM images at first magnification. [Figure 6B]

[0027] This is a SEM image at a second magnification. [Figure 6C]

[0027] This is an SEM image at a third magnification. [Figure 6D] Energy dispersive X-ray spectrum of the product showing 92.2% C, 3.6% Ba and 4.2% Ca. [Figure 7A]

[0028] 1 shows an SEM image of a cleaning electrolysis product in a 1:1 wt% Na2CO3 to BaCO3 electrolyte, 0.2 A / cm2, containing 0.08 wt% Fe2O3, with a nichrome anode and a brass cathode at 770° C. This is the first magnification SEM image. [Figure 7B]

[0028] This is an SEM image at a second magnification. [Figure 7C]

[0028] This is an SEM image at a third magnification. [Figure 7D]

[0028] This is an SEM image at a third magnification. [Figure 7E]

[0028] This is an SEM image at a fourth magnification. [Figure 7F]

[0028] This is an SEM image at a fifth magnification. [Figure 8]

[0029] 1 shows SEM images of cleaning electrolysis products at 770° C. in 2.5:1 wt % Na2CO3 to BaCO3 electrolyte, 0.1 A / cm2, containing 0.1 wt % Fe2O3, with a nichrome anode and a brass cathode. [Figure 9A]

[0030] 1 shows an SEM image of a cleaning electrolysis product at 770° C. in a 1:1 wt % Na2CO3:BaCO3 electrolyte at 0.1 A / cm2 with 0.04 wt % Cr2O3 and 0.04 wt % Fe2O3, with a Nichrome anode and a Monel cathode. This is a first magnification SEM image. [Figure 9B]

[0030] This is a SEM image at a second magnification. [Figure 9C]

[0030] This is a SEM image at a second magnification. [Figure 10A]

[0031] 1 shows an SEM image of a cleaning electrolysis product at 770° C. in a 1:1 wt % Na2CO3 to BaCO3 electrolyte at 0.1 A / cm2 with 30 wt % BaO, a Nichrome anode and a Monel cathode. This is the first magnification SEM image. [Figure 10B]

[0031] This is a SEM image at a second magnification. [Figure 10C]

[0031] SEM at third magnification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Detailed Description

[0032] Embodiments of the present disclosure relate to methods and apparatus for producing carbon nanomaterial (CNM) products that include nanoscale graphitic carbon structures such as carbon nanotubes (CNTs). The methods and apparatus utilize carbon dioxide (CO2) as a reactant in an electrolytic reaction to make the CNM products. Embodiments of the present disclosure utilize a lithium-free electrolyte.

[0024]

[0033] Some embodiments of the present disclosure relate to methods that utilize electrolytic reactions to make CNM products. The electrolytic reactions are carried out in the environment of a molten lithium-free electrolyte positioned between an anode and a cathode. Carbon is introduced into the molten electrolyte either as pure CO, concentrated CO, CO entrained in atmospheric air, another carbon-containing gas, or other anthropogenic CO source.

[0025]

[0034] Some embodiments of the present disclosure relate to an apparatus and a system utilizing the apparatus. The apparatus includes an electrolysis cell including an anode and a cathode. In some embodiments of the present disclosure, the anode and the cathode are vertically spaced apart from one another.

[0026]

[0035] definition

[0027]

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this disclosure belongs.

[0028]

[0037] As used herein, the term "about" refers to approximately a ±10% variation from a given value. Any given value provided herein should always be understood to include such a variation, whether or not specifically referenced.

[0029]

[0038] As used herein, the term "lithium-free" means substantially lithium-free, which contemplates when small amounts of lithium may be present or when there is no detectable amount of lithium at all. In some embodiments of the present disclosure, lithium-free carbonate electrolytes are useful, which may also be referred to as "predominantly non-lithium carbonate electrolytes." For clarity, the terms "lithium-free carbonate electrolyte," "lithium-free electrolyte," "predominantly non-lithium carbonate electrolyte," and "predominantly non-lithium electrolyte" are used herein to refer to electrolytes in which there is no detectable amount of lithium and in which small amounts of lithium are present when the electrolyte is a mixture, and the lithium-containing component forms less than about 5% (wt%) based on the weight of the entire mixture, or less than about 4 wt%, less than about 3 wt%, less than about 2 wt%, less than about 1 wt%, less than about 0.5 wt%, less than about 0.25 wt%, less than about 0.1 wt%, less than about 0.05 wt%, or less than about 0.025 wt%, or less than about 0.01 wt% of the entire mixture.

[0030]

[0039] Embodiments of the present disclosure will now be described, including examples and reference to figures.

[0031]

[0040] Some embodiments of the present disclosure relate to a method for producing a CNM product comprising CNTs. The method includes heating a lithium-free carbonate electrolyte to obtain a lithium-free molten carbonate electrolyte, positioning the molten carbonate electrolyte between an anode and a cathode of an electrolytic cell, applying a current to the cathode and the anode of the electrolytic cell, and collecting the CNM product from the cathode. In some embodiments of the present disclosure, the method further includes utilizing one or more non-lithium promoting elements and / or introducing a graphene defect agent into the lithium-free carbonate electrolyte. In some embodiments of the present disclosure, the CNM product may be doped or magnetic or otherwise.

[0032]

[0041] As the skilled reader will appreciate, the step of heating the lithium-free carbonate electrolyte can be accomplished by a variety of means. For example, a heating device such as an oven or furnace can be used to heat the electrolyte to a temperature sufficient to transition it to a molten liquid state. Thus, any heating device capable of achieving the temperature required to heat the electrolyte to its melting point is contemplated herein.

[0033]

[0042] In some embodiments of the present disclosure, the lithium-free electrolyte may be a binary mixture, a ternary mixture, or a mixture of more than three components. For example, a binary mixture may include two components selected from sodium carbonate, calcium carbonate, and barium carbonate. A ternary mixture may include two lithium-free carbonates and one graphene defect agent.

[0034]

[0043] Without being bound by any particular theory, the reduction of CO2 in a lithium carbonate electrolyte proceeds according to Equation 1 (EQN.1): - It is a process.

[0035]

[0044] Li2CO 3(溶融) +4e - →C (ナノ材料) +O 2(ガス) +LiO (溶解)(EQN.1).

[0036]

[0045] Without being bound by any particular theory, CO2 added to the electrolyte chemically reacts with lithium oxide to renew and reform Li2CO3 according to equation 2 (EQN.2).

[0037]

[0046] CO 2(大気又はスタック) +LiO (溶解) ⇔LiCO 3(溶融) (EQN.2).

[0038]

[0047] Without being bound by any particular theory, combining EQN.1 and EQN.2 gives the net electrolytic reaction according to equation 3 (EQN.3).

[0039]

[0048] CO 2(ガス) +4e - →C (ナノ材料) +O 2(ガス) (EQN.3).

[0040]

[0049] Without being bound by any particular theory, at temperatures above about 800° C., two-electron reduction rather than four-electron reduction may dominate, and up to about 950° C., the electrolysis product is pure carbon monoxide rather than carbon, according to equation 4 (EQN.4).

[0041]

[0050] CO 2(ガス) +2e - →CO (ガス) +1 / 2O 2(ガス) (EQN.4).

[0042]

[0051] Ternary Li, Na and K carbonate eutectic mixtures have melting points below 400°C. The potassium component of the electrolyte has been observed to inhibit carbon nanomaterial formation, and thus under some conditions potassium may not be a desirable component of lithium-free carbonate electrolytes. Below about 600°C, the electrolytic reaction products in ternary carbonate electrolytes are primarily amorphous carbon and 1-2 μm platelets arranged in a "honeycomb-like" morphology. Above about 600°C, the electrolytic carbon products begin to exhibit a mixture of CNM products.

[0043]

[0052] Without being bound by any particular theory, embodiments of the present disclosure relate to an electrolyte that is (i) lithium-free (reducing overall cost) and potassium-free (allowing for the formation of carbon nanomaterials), (ii) stable when melted at about 700° C. to about 800° C., (iii) easily dissolves the oxide, and (iv) inexpensive compared to lithium carbonate. Sodium carbonate has a high melting point of about 851° C. Calcium carbonate can be unstable at such temperatures, where it can decompose into calcium oxide and CO2. Barium carbonate also has a melting point above 810° C. Both sodium carbonate and barium carbonate are an order of magnitude less expensive than lithium carbonate.

[0044]

[0053] Binary mixtures of Na2CO3-BaCO3 have been studied and an example of a phase diagram of Na2CO3-BaCO3 is shown in FIG. 1. As seen in FIG. 1, the eutectic mixture may be composed of approximately 50% BaCO3 by weight, more precisely 34.6 mol% BaCO3. This 50% by weight BaCO3 / Na2CO3 eutectic mixture has a melting point of about 702±2°C. The horizontal x-axis of the phase diagram in FIG. 1 indicates the weight % of BaCO3, which is equal to the weight % of 100%-BaCO3. The vertical y-axis of the phase diagram in FIG. 1 indicates temperature in degrees Celsius (°C). In particular, the top line 116 indicates the melting point of the BaCO3 / Na2CO3 eutectic mixture with various weight % of BaCO3. The bottom line 118 indicates a consistent melting point of about 702±2°C. Region 102 indicates the liquid state of the Na2CO3-BaCO3 mixture. Region 104 represents the liquid state and α-BaCO3. Region 106 represents the liquid state and β-BaCO3. Region 108 represents the liquid state and γ-BaCO3. Region 112 below the melting point of about 702±2° C. represents the solid state of Na2CO3 and γ-BaCO3. Region 110 represents the solid and liquid states with a weight percent of BaCO3 less than 50% and less than about 850° C. Region 114 represents the solid solution state with a weight percent of BaCO3 less than 10%.

[0045]

[0054] The molten electrolyte is then positioned between the anode and cathode of the electrolysis cell. The electrolysis cell can be any type of cell that can maintain its structural integrity against the electrochemical environment encountered during the electrolysis reaction of the present disclosure. The electrolysis cell can be made of any desired material that does not degrade in the environment of the electrolysis reaction or can have one or more walls coated with a desired material. In some embodiments of the present disclosure, the electrolysis cell is made of substantially pure alumina. In some embodiments of the present disclosure, the electrolysis cell is a tubular cell with a closed end.

[0046]

[0055] In some embodiments of the present disclosure, the electrolyte may be melted within the electrolysis cell or melted outside the cell and transferred to it. Since the electrolysis reaction typically occurs over a period of time during which the molten electrolyte may cool, the electrolysis cell may be configured with its own integral heating device, such as an integral heater, or it may be configured to be heated by an external heater that is external to the electrolysis cell such that the electrolyte is maintained in a molten state for a desired period of time.

[0047]

[0056] In some embodiments of the present disclosure, the electrolysis cell can be configured to maintain the electrolyte at at least about 650°C, at least about 675°C, at least about 700°C, at least about 725°C, at least about 750°C, at least about 775°C, at least about 800°C, at least about 825°C, at least about 850°C, at least about 875°C, at least about 900°C, at least about 1000°C, or greater than 1000°C.

[0048]

[0057] Anodes can be made of a variety of metals or alloys. Some anodes can be made of materials that include nickel. Some non-limiting examples of materials suitable for the anodes of the present disclosure include substantially pure nickel, alloys that are substantially composed mostly of nickel, and alloys that are composed of some nickel. For example, Inconel 718 or other Inconels, including but not limited to Inconel 600 and Inconel 625, Nichrome A (composed of about 80% nickel and about 20% chromium), Nichrome C (composed of nickel, iron, and chromium), Incoloy alloys (e.g., Incoloy 800, composed of about 40% iron, about 30-35% nickel, and about 19-23% chromium).

[0049]

[0058] The anode may be planar in shape and may be made in a variety of dimensions. In some embodiments of the present disclosure, the anode may be made of wire rolled into a substantially flat coil having an upper surface and a lower surface. The upper and lower surfaces of the coiled anode may have substantially equal areas suitable for mounting in an electrolysis cell. In some embodiments, the coiled anode surface may be approximately 1 cm2. 2 ~about 20cm 2 , about 2 cm 2 ~10cm 2 Or about 3 cm 2 ~about 5cm 2 A person skilled in the art will appreciate that the size of the electrolytic cell may dictate the size of the coiled anode. The coiled anode may be positioned so that it is generally aligned in a horizontal plane.

[0050]

[0059] The cathode may be made of a variety of metals or alloys. Some cathodes may be made of materials including steel, galvanized steel, copper, or any combination thereof. Some further non-limiting examples of materials suitable for the anodes of the present disclosure include Monel and brass.

[0051]

[0060] The cathode may be planar in shape and may be made in a variety of dimensions. In some embodiments of the present disclosure, the cathode may be made of wire rolled into a flat coil having an upper surface and a lower surface. The upper and lower surfaces of the coiled cathode may have substantially equal areas suitable for mounting in an electrolysis cell. In some embodiments, the coiled cathode surface may be approximately 1 cm2. 2 ~about 20cm 2 , about 2 cm 2 ~10cm 2 Or about 3 cm 2 ~about 5cm 2 One skilled in the art will appreciate that the size of the electrolytic cell may dictate the size of the coiled cathode. The coiled cathode may be positioned so as to be generally aligned in a horizontal plane.

[0052]

[0061] In some embodiments of the present disclosure, the size and orientation of the cathode may be selected to substantially mirror the size and orientation of the anode. In some embodiments of the present disclosure, the anode and cathode may be generally aligned in a horizontal plane and vertically spaced apart from each other. As will be appreciated by those skilled in the art, the distance between the electrodes must allow sufficient current to pass between them, but the amperage of the current and the size of the electrolysis cell may also affect how far apart the electrodes are vertically spaced. In some embodiments of the present disclosure, the electrodes may be vertically spaced apart from each other by about 0.25 cm, about 0.5 cm, about 0.75 cm, about 1 cm, about 1.25 cm, about 1.5 cm, about 1.75 cm, about 2 cm, about 3 cm, about 4 cm, about 5 cm, about 7.5 cm, about 10 cm, or even more.

[0053]

[0062] To initiate and maintain the electrolysis reaction in the electrolysis cell, a current is applied and passed between the anode and the cathode through the molten electrolyte therebetween. In some embodiments of the present disclosure, the current can be alternating or direct current. In some embodiments of the present disclosure, the current can be from about 0.01 amperes (A) to about 5 amperes. In some embodiments of the present disclosure, the current can be from about 0.025 A to about 4 A, from about 0.05 A to about 3 A, from about 0.075 A to about 2 A, from about 0.1 A to about 1 A. In some embodiments of the present disclosure, the current is about 0.5 A.

[0054]

[0063] In some embodiments of the present disclosure, the current is applied at a substantially constant current density. For example, the current density of the applied current is about 0.01 A / cm 2 ~About 1A / cm 2 In some embodiments, the current density of the applied current may be about 0.025 A / cm 2 ~about 0.75A / cm 2 , about 0.05A / cm 2 ~about 0.5A / cm 2 , about 0.075A / cm 2 ~about 0.25A / cm 2 or about 0.01A / cm 2 ~about 0.1A / cm 2In some embodiments of the present disclosure, the current density can be about 0.1 A / cm 2 In some embodiments, low current densities are used to control conductivity during formation of the CNM products.

[0055]

[0064] In some embodiments of the present disclosure, the method further includes utilizing one or more non-lithium promoting elements. In some embodiments of the present disclosure, the one or more non-lithium promoting elements may include (i) enhancing transition metal nucleation, ii) adding one or more defect inducers, (iii) reducing or removing electrolyte conductivity inhibiting elements, and (iv) any combination thereof.

[0056]

[0065] In some embodiments of the present disclosure, the step of enhancing transition metal nucleation may include adding a transition metal nucleating agent to the lithium-free electrolyte either before, during, or after the heating step. In some embodiments, the transition metal oxide may be iron oxide (Fe2O3), chromium oxide (Cr2O3), or a combination thereof. In a particular embodiment, the transition metal nucleating agent is Fe2O3. In some embodiments, the transition metal nucleating agent may be one or more transition metal salts of iron salts, chromium salts, nickel salts, copper salts, manganese salts, titanium salts, zirconium salts, molybdenum salts, tantalum salts, tungsten salts, silver salts, cadmium salts, tin salts, ruthenium salts, vanadium salts, or cobalt salts. In some embodiments, the transition metal nucleating agent may be a transition metal oxide.

[0057]

[0066] In some embodiments of the present disclosure, the step of adding one or more defect-inducing agents includes introducing a graphene defect agent into the lithium-free carbonate electrolyte either before, during, or after the heating step. This adding step can be accomplished by various techniques depending on the nature of the graphene defect agent. For example, the graphene defect agent can be a chemical, mechanical, optical, physical, or any combination thereof that induces graphene defects and / or graphene vacancies in the graphitic structure of the CNM product. This step of introducing a graphene defect agent into the lithium-free carbonate electrolyte can be performed before, during, or after heating the lithium-free carbonate electrolyte to the molten state.

[0058]

[0067] In some embodiments of the present disclosure, the graphene defects are localized within the graphene component of the graphitic structure in the CNM product, and the defects are intrinsic, extrinsic, or any combination thereof.

[0059]

[0068] Examples of intrinsic graphene defects are Stone-Wales defects, single vacancy defects, multi-vacancy defects, line defects, incorporation of carbon adatoms or any combination thereof.

[0060]

[0069] Examples of extrinsic graphene defects are the incorporation of foreign adatoms or substitutional impurities.

[0061]

[0070] In adatom defects, oxygen can attach to the surface of CNTs or other carbon nanomaterials and break bonds or replace carbon in the structure itself.

[0062]

[0071] In some embodiments of the present disclosure, the graphene defect agent is an oxide, which may be introduced into the lithium-free carbonate electrolyte by adding a chemical oxide, by a chemical reaction due to a temperature change in the molten carbonate electrolyte, by degradation of the electrode, by oxidation of the anode, or any combination thereof.

[0063]

[0072] Suitable examples of chemical oxides that may be added to the lithium-free carbonate electrolyte include, but are not limited to, alkali oxides, alkaline earth oxides, metal oxides, non-metal oxides, or any combination thereof. In some embodiments of the present disclosure, sodium oxide (Na2O), barium oxide (BaO), calcium oxide (CaO), aluminum oxide (Al2O3), or any combination thereof are added to the lithium-free carbonate electrolyte. The combination may also be added as a reorganized oxide salt, such as, but not limited to, sodium aluminate or barium aluminate. In some embodiments of the present disclosure, the oxide is one or more of barium oxide, sodium oxide, or calcium oxide. In some embodiments of the present disclosure, the oxide is iron oxide or cobalt oxide. In some embodiments of the present disclosure, the oxide is lithium oxide at a concentration of 5 percent or less.

[0064]

[0073] In the process of CO2 molten carbonate electrolysis reaction, small transition metal "seeds" were observed at the edge of the CNT product, indicating that the mechanism of molten carbonate CNT growth can be activated by both tip and bottom transition metal nucleation processes. Without being bound by any theory, the mechanistic concept that graphene defects or vacancies can promote CNT growth in lithium-free molten carbonate electrolyte can be seen in FIG. 2. In FIG. 2A, the catalyst tip can move along with the CNT growth. In FIG. 2B, the catalyst is at the stationary bottom or base where the CNTs grow. SEM evidence of both tip and bottom grown CNTs is observed. FIG. 2 shows two schematic diagrams representing the proposed carbon nanotube (CNT) growth mechanism on a cathode during carbon dioxide (CO2) electrolysis reaction, FIG. 2A shows the CO2 → CNT + O2 electrolysis tip growth mechanism, and FIG. 2B shows the CO2 → CNT + O2 bottom growth mechanism. The top arrow 202 in FIG. 2A indicates the mechanism of the CO2 → CNT + O2 electrolysis tip growth mechanism. 2(ガス) +M2O (溶解) →2M + (溶融) +CO3 2- (溶融) Arrow 204 represents the CO dissolution reaction in molten carbonate represented by the formula: 2M + +CO32- +4e - →C+M2O+2O2. Arrow 206 represents the net cathodic reaction represented by the equation: 2- →O2+4e - In both Figures 2A and 2B, the net anodic reaction is represented by sp 3 There are oxide-induced graphene defects, where low M=Li + and high M=Li + Or Na + In FIG. 2A, the metal catalyst 210 on top of the layered graphene 218 is at the tip of the CNT cylindrical graphene layer 208 of the carbon nanotube 210. In FIG. 2B, the metal catalyst 210 is at the bottom of the CNT cylindrical graphene layer 208 of the carbon nanotube 210, closer to the cathode 216. In both FIG. 2A and FIG. 2B, the growth direction is represented by the arrow 214, and the double arrow 218 pointing upwards is 4e - Represents.

[0065]

[0074] Without being bound by any particular theory, carbonate species arising from continuous CO2 renewal of the carbonate electrolyte provide the ongoing carbon building blocks of the CNT layer, and carbonate reduction to carbon takes place at the metal-catalyzed interface with the growing CNT cylindrical graphene layer. However, the carbonate must have easy access to the interface with the CNT inner layer as well as the outer CNT layer. Carbonate migration to the inside of the growing carbon nanotube can be inhibited by charge accumulation. This charge accumulation can be reduced if the cation has easy access to the inner layer. Lithium cations are small cations and require relatively few defects or vacancies in the growing cylindrical carbon nanotube layer to access the inner region of the CNT. However, a larger number of defects is required to allow ions larger than lithium cations to easily migrate through the CNT layer. A larger number of defects can be achieved through the addition of graphene defect agents. This is at least part of the basis behind the development of embodiments of the present disclosure to grow CNM products by CO2 electrolysis in lithium-free carbonate electrolyte.

[0066]

[0075] In some embodiments of the present disclosure, the CNM product produced according to the methods, devices, and systems described herein above may result in a doped CNM product. Without being bound by any particular theory, when a doping component, also referred to as a dopant, is introduced into the present methods, devices, or systems, the atoms of the dopant may be directly incorporated into some of the graphitic structures of the CNM product. When the atoms of the doping component are directly introduced into the CNM product, as constructed in situ on the cathode, the resulting doped CNM product has desirable chemical and physical properties that differ from a CNM product that does not contain the atoms of the doping component (an undoped CNM product). Without being bound by any particular theory, the doping component may include at least one material having a Group IIIA element, a non-carbon Group IVA element, a Group VA element, a Group VIA chalcogenide element, or at least one material having gold, platinum, iridium, iron, or other period 4, 5, or 6 metal. In some embodiments of the present disclosure, the doping component includes chemical species having oxygen atoms, halide atoms, one or more of the following: nitrates, phosphates, thiophosphates, silicates, thionyl chloride, sulfur chloride, silicon chloride, thiophosphates, thionyl nitrate, silicon nitrate, silicon nitrite, sulfur oxide, and nitrous oxide gas. Without being bound by any particular theory, the desired chemical properties of the doped CNM product may include greater electrical conductivity (compared to the undoped CNM product), enhanced charge storage (compared to the undoped CNM product), heterogeneous catalysis, homogeneous catalysis, fuel cell catalysis, aerobic oxidation catalysis, enhanced reaction activity, and any combination thereof. The desired physical and chemical properties of the doped CNM products made according to embodiments of the present disclosure may have a wide variety of applications, such as catalysis, heavy metal removal, energy storage, sorption applications, batteries, ultrasensitive sensors, and combinations thereof.

[0067]

[0076] In some embodiments of the present disclosure, the CNM product produced according to the methods, devices, and systems described herein above may result in a magnetic CNM product. For clarity, the magnetic CNM product is one that is physically movable by a magnetic field. Without being bound by any particular theory, when the magnetic additive component is introduced into the present method, device, or system, some carbide-driven growth of graphite-like structures in the magnetic CNM product occurs. In some embodiments of the present disclosure, the magnetic additive component includes at least one of a magnetic material additive component, a carbide growth component, and any combination thereof. In some embodiments of the present disclosure, the magnetic material additive component is one or more of iron, nickel, cobalt, gadolinium, samarium, neodymium, steel, and alloys, where the magnetic material additive component constitutes one or more magnetic materials having ferromagnetic, paramagnetic, diamagnetic, and any combination thereof. In some embodiments of the present disclosure, the iron-based additive is one or more of cast iron powder, iron metal, steel, stainless steel, iron-containing metal alloy, iron oxide, FeO, Fe2O3, Fe3O4, or iron-containing salts. Within the magnetic CNM product, the magnetic additive component is incorporated or formed on the magnetic CNM product as one or more nodules that may be covered with one or more layers of graphitic carbon. In some embodiments of the present disclosure, the carbide growth component may be a metal carbide, such as iron carbide, nickel carbide, cobalt carbide, zirconium carbide, chromium carbide, tantalum carbide, hafnium carbide, and any combination thereof. In some embodiments of the present disclosure, the carbide growth component may be a non-metal carbide, such as silicon carbide, germanium carbide, and any combination thereof. The magnetic additive component may be added to the methods, apparatus, and systems of the present disclosure as a chemical additive or it may originate from one or more walls of the electrolytic cell, the anode, the cathode, the electrolyte medium, and any combination thereof. EXAMPLES

[0068]

[0077] Working Example

[0069]

[0078] The components of the molten electrolyte mixture described herein are commercially available: barium carbonate (BaCO, Alfa Aesar, about 99.5% pure), lithium carbonate (LiCO, Alfa Aesar, about 99% pure), sodium carbonate (NaCO, Alfa Aesar, about 99% pure), lithium oxide (LiO, Alfa Aesar, about 99.5% pure), and barium oxide (BaO, Alfa Aesar, about 97% pure).

[0070]

[0079] CNM products made according to the following examples were washed to remove excess electrolytes (either with deionized water or up to 6M HCl), separated from the wash solutions, and analyzed on a PHENOM Pro-X scanning electron microscope (SEM) with a PHENOM Pro-X energy dispersive spectroscopy, a high resolution FEI Tenco LV SEM, and / or a FEI Talos F200X transmission electron microscope (TEM).

[0071]

[0080] A 0.6 cm Raman microscope (LabRAM HR800, HORIBA) was used. -1 Raman spectroscopy was performed with a high resolution of 532.14 wavelength laser light.

[0072]

[0081] Example 1

[0073]

[0082] To produce the CNM product, the electrolysis reaction was carried out in an electrolysis cell that contained a tubular vessel, an anode, and a cathode. The tubular vessel was made of pure alumina (approximately 99.6% pure alumina commercially available from AdValue) and was provided with a closed end.

[0074]

[0083] The anode was configured to generate oxygen during an electrolytic reaction. The anode was made of nichrome and was configured as a substantially flat coil.

[0075]

[0084] The cathode was made of brass and was also configured as a substantially flat coil.

[0076]

[0085] In this Example 1, the electrolyte was lithium carbonate (Li2CO3) containing 2% (by weight, %) lithium oxide (Li2O). The electrolyte was heated to about 770° C. and positioned between the anode and cathode of a tubular chamber of an electrolysis cell.

[0077]

[0086] The electrolytic reaction is about 0.14 A / cm 2 The test was initiated by applying a current of about 0.5 amperes (A) at a substantially constant current density of 100 .mu.m.

[0078]

[0087] Carbon dioxide from the air was directly captured by the molten electrolyte during the electrolysis reaction.

[0079]

[0088] After about 4 hours, the electrolysis reaction was stopped by turning off the current, the cathode was removed from the tubular cell, allowed to cool, and the solid CNM product was removed from the cathode.

[0080]

[0089] FIG. 3 shows a scanning electron microscope (SEM) image of the CNM product, which includes carbon nanotubes (CNTs). FIG. 3B shows CNTs collected from the side of the cathode that does not face the anode, also referred to as the back surface. In particular, the piece of multilayer graphene sheet that initially formed on the cathode and from which the CNTs grew is clearly visible, consistent with the tip-growth mechanism of FIG. 2A. The CNTs grew consistent with the tip-growth mechanism. The CNM product was approximately 98% uniform CNTs as determined by visual inspection of multiple SEM images.

[0081]

[0090] The scale bars in Figures 3A, 3B, 3C, and 3D are 200 μm, 200 μm, 10 μm, and 10 μm, respectively, and the scale bars in Figures 3E, 3F, and 3G are 200 μm, 3 μm, and 1 μm, respectively.

[0082]

[0091] A useful gauge of the number of defects in a graphite-like structure is 1575 cm -1 The high frequency E 2g ) peak intensity at 1350 cm -1 Intensity of the D (disorder-induced band) peak located at ID The ratio of the photon density of the nuclei to the photon density of the nuclei is given by Raman spectroscopy.

[0083]

[0092] The concentration of oxides in molten carbonates can be determined by equilibrium with the partial pressure of CO2, as exemplified by CO2 in air versus molten Li2CO3. For example, at 750°C, molten Li2CO3 has an equilibrium concentration of 0.3m oxide (m = moles / kg Li2CO3) under air at 750°C. Increasing the oxide concentration can be achieved by changing the temperature or pressure of the system.

[0084]

[0093] CNTs grown in pure molten Li2CO3 with an internal equilibrium induced oxide concentration of 0.2 m were D / I G = 0.4, whereas that grown in 4m Li2O in Li2CO3 (10.6 wt% Li2O) exhibits a D / I G It has been previously shown that the Raman spectrum of 2 wt% LiO grown exhibits I D / I G = 0.7, and the CNTs are generally straighter and less entangled than those grown in 10.6 wt% lithium carbonate electrolyte. Presumably, the structure and organization of these CNTs is different from that of conventional graphitic sp 2 Lower concentration of out-of-plane sp compared to carbon bonds 3 The ratio of 0.70 corresponds to that of commercially available CNTs.

[0085]

[0094] In the left and right parts of Figure 2C, the D and G Raman peaks of CNTs are clearly visible for CNTs grown electrolytically in electrolytes with (right) or without (left) lithium oxide added to the lithium carbonate electrolyte. The lithium carbonate electrolysis product used in the right Raman spectrum is generated at an electrolyte lithium oxide concentration of 4mLi2O (4mLi2O = 12 wt% Li2O per weight of Li2CO3). The larger relative height of the D peak is indicative of a larger number of defects in carbon nanotubes grown in the presence of added oxide. The I peaks due to oxide addition during electrolytic growth of CNTs are clearly visible for CNTs grown electrolytically in electrolytes with (right) or without (left) lithium oxide added to the lithium carbonate electrolyte. The I peaks due to oxide addition during electrolytic growth of CNTs are clearly visible for CNTs grown electrolytically in electrolytes with (right) or without ...left) or without lithium oxide added to the lithium carbonate electrolyte. D / IG This increase in the ratio is consistent with larger defects and improved reversible intercalation of Li ions into the CNTs when used as anodes in battery applications.

[0086]

[0095] Example 2

[0087]

[0096] This example used many of the same steps as Example 1, with one exception being the use of a lithium-free electrolyte.

[0088]

[0097] The electrolysis cell included a tubular vessel made of essentially pure alumina with an internal volume of about 100 ml. The anode was a horizontally aligned coil (approximately 5 cm) of nickel wire spaced vertically about 1 centimeter (cm) above a cathode made of galvanized steel wire. 2 The cathode was also a horizontally aligned coil of wire (approximately 5 cm2 as shown in Figures 4A and 4B). 2 (having an area of ​​1.5m).

[0089]

[0098] The electrolyte in this Example 2 is a ternary mixture of 1:1 wt% Na2CO3 to BaCO3, having a low melting point according to Figure 1 and containing 2m (23 wt%) barium oxide (BaO). The electrolyte was heated to about 750°C and positioned between the anode and cathode of a tubular cell. Carbon dioxide from the air was captured directly by the molten electrolyte during the electrolysis reaction.

[0090]

[0099] Approximately 0.1A / cm 2 A current of about 0.5 A was applied to the anode and cathode at a substantially constant current density of 1000 mA to initiate the electrolysis reaction.

[0091]

[0100] After approximately 4 hours of electrolysis, the current was stopped and the cathode was removed from the tubular cell and allowed to cool. The CNM product was removed from the cathode and washed to remove excess electrolyte. The CNM product was washed with either deionized water (DI water) or up to 6 molar hydrochloric acid. Both types of washing gave similar CNM products, but it was observed that the acid washing accelerated the washing. The washed CNM product was then separated from the washing solution by either paper filtration or centrifugation. It was observed that both separation techniques gave similar CNM products, but the centrifuge accelerated the separation step.

[0092]

[0101] To characterize the structural morphology of the CNM products, the products were imaged using SEM imaging. Figures 4D and 4E show SEM images of the CNM products containing discernible but minor CNT products, including approximately 5% curled CNTs. The remainder of the CNM products were a mixture of carbon nanoonions and nanoplatelets. Scale bars in Figures 4D and 4E are both 10 μm.

[0093]

[0102] After completing the electrolysis reaction, the washed nickel electrode appeared unchanged. However, as seen in FIG. 4C, the electrolyte appeared green in both tubular cells and solidified on the removed cathode, which may be evidence of nickel oxidation and electrolyte buildup. To avoid this corrosion, a nickel-chromium alloy anode may be useful.

[0094]

[0103] Example 3

[0095]

[0104] This example used many of the same steps as Example 2, including the use of a lithium-free electrolyte. The main difference from Example 3 was the materials used in the anode and cathode.

[0096]

[0105] The electrode material has a substantial effect on the yield and morphology of CNTs grown by molten carbonate electrolysis. With lithium carbonate electrolyte, Monel cathodes and Nichrome anodes are known to produce the longest CNTs to date by CO2 electrolysis. The CNTs are uniform and produced in high yields. Without being bound by any particular theory, it has been proposed that both nickel and chromium may act as effective nucleating agents for CNT growth, with nickel promoting CNT growth and chromium promoting healing to allow for continued CNT growth.

[0097]

[0106] The electrolysis cell contained a tubular vessel made of essentially pure alumina with an internal volume of about 100 mL. The anode was a horizontally aligned coil (approximately 5 cm long) of nichrome wire spaced vertically 1 cm above a cathode made of Monel wire. 2 The cathode was also a horizontally aligned coil of wire (approximately 5 cm in area) (see FIG. 5A). 2 (having an area of ​​1.2 m).

[0098]

[0107] The electrolyte in this Example 3 was a mixture of 1:1 wt% Na2CO3:BaCO3 with no added BaO. The electrolyte was heated to about 770° C. and positioned in a tubular cell. Carbon dioxide from the air was captured directly by the molten electrolyte during the electrolysis reaction.

[0099]

[0108] Approximately 0.1A / cm 2 The electrolysis reaction was initiated by applying a current of about 0.5 A to the anode and cathode at a constant current density of 1000 .mu.m.

[0100]

[0109] After about 4 hours of electrolysis, the current was turned off and the cathode was removed from the tubular cell and allowed to cool. Figure 5B shows the electrode after the electrolysis reaction had stopped. Although solidified electrolyte (a clear white material) was present, there was little or no evidence that the anode had corroded. The CNM product was then removed from the cathode and washed to remove excess electrolyte.

[0101]

[0110] As shown in the SEM images in Figures 5C, 5D, and 5E, the CNM product contained approximately 10% identifiable short, curled CNTs (scale bars in Figures 5C, 5D, and 5E are 80 μm, 30 μm, and 20 μm, respectively).

[0102]

[0111] Example 4

[0103]

[0112] Without being bound by any particular theory, the failure of attempts to synthesize CNTs in high yields in non-lithiated electrolytes may be due to (i) the inherently higher resistivity of lithium-free molten electrolytes, resulting in lower mobility and restricted growth; and (ii) the Li + This may be correlated with insufficient defect size in the growing CNT layer to facilitate the easy exchange of larger ions than Li2CO3 (3 Siemens cm2). Specifically, molten Li2CO3 not only requires lower thermodynamic electrolysis energy, but also has a higher electrolysis energy near its melting point than Na2CO3 (3 Siemens cm2). -1 ) or K2CO3 (2 siemens cm -1 ) with a higher conductivity (6 Siemens cm -1 ). Higher conductivity is desirable because it can result in lower electrolytic ohmic losses, increase reactant mobility, and prevent constraints on mass diffusion. Furthermore, lithium mobility within carbon nanotube growth sites appears to contribute to the high carbon nanotube growth rates observed in lithium-containing media.

[0104]

[0113] In this example, the current density is half, 0.05 A / cm 2The electrolysis product grown in 1:1 Na2CO3:BaCO3 electrolyte (without BaO addition) demonstrates the higher yield synthesis of CNTs in lithium-free electrolytes. The electrolysis used a planar rather than coiled and brass rather than Monel cathode, and it was observed that neither the change in shape nor the choice of alloy substantially affected the lithium-free CNT growth. As can be seen from the representative SEM images in Figures 9A-9C, the product contains 80-90% CNTs that appear granular and not smooth. The scale bars in Figures 6A, 9B and 9C are 80 μm, 50 μm and 20 μm, respectively. Figure 6D shows the energy dispersive X-ray spectroscopy results from the product obtained in this example, showing 92.2% C, 3.6% Ba and 4.2% Na. The unavailable element O is present as residual sodium and barium carbonates.

[0105]

[0114] Example 5

[0106]

[0115] In this example, an additional concentration of transition metal nucleating agent was used for carbon nanotube synthesis in a lithium-free electrolyte. 2 Although electrolysis was performed at a high current density of 1000 nm, very high quality carbon nanotube products were obtained via the direct addition of 0.08 wt% Fe2O3 to the 1:1 Na2CO3:BaCO3 electrolyte. As seen in Figure 7, the carbon nanotube products are smooth, have 80-90% CNT purity, and have high CNT length-to-diameter aspect ratios. TEM (not shown) of the products from non-lithiated electrolyte exhibits the regular CNT morphology of hollow-cored structures with layers made up of discernible concentric cylindrical graphene layers observed above for CNTs formed from CO2 electrolysis in lithiated carbonate electrolyte. The separation between graphene layers in graphite is approximately 0.335 nm and may vary near this value for multi-walled CNTs. Scale bars for SEM images shown in Figures 7A-7F are 200 μm, 30 μm, 20 μm, 20 μm, 10 μm, and 8 μm, respectively. In this example, a brass cathode was used, however other cathodes such as Monel steel, galvanized steel, copper, nickel alloys, etc. may also be effective.

[0107]

[0116] The high CNT yields shown in FIG. 7 are observed over a range of current densities, a range of Fe2O3 concentrations, various cathodes, and a range of relative weight ratios of Na2CO3 and BaCO3 in the electrolyte. For example, 2 Electrolysis at lower current densities, 770 °C electrolytes in the range of 2.5:1 to 1:2.5 wt% Na2CO3 to BaCO3, and 0.1 wt% Fe2O3 content was also observed to produce products with 80-90% CNT purity. However, as seen in the high-resolution, high-magnification SEM images in Figure 8 (scale bar 2 μm), the products in such sodium carbonate-rich electrolytes deviate significantly from the conventional smooth cylindrical CNT morphology seen in Figure 9, with bead-like nodules and platelets clearly visible along with the tubular morphology.

[0108]

[0117] Example 6

[0109]

[0118] In this example, the effect of transition metal nucleating agents on the quality of carbon nanomaterial products was demonstrated. The electrolysis conditions used were similar to those described in Example 6, but instead of 0.08 wt% Fe2O3 additive, Fe2O3 and Cr2O3 (0.04 wt% each) additives were used in the lithium-free electrolysis. Chromium has been used as an effective CNT growth nucleating agent. However, when used as an additive in the lithium-free electrolysis, the reaction product was not as good as that obtained with Fe2O3 alone, since it consisted of approximately 60% CNTs (see FIG. 9, scale bars in FIGS. 9A, 9B, and 9C are 20 μm, 10 μm, and 10 μm, respectively).

[0110]

[0119] Example 7

[0111]

[0120] In this example, 30 wt. % BaO was added to a 1:1 Na2CO3:BaCO3 electrolyte and a current of 0.1 A / cm was obtained using a NiCr anode and Monel cathode. 2 As shown in Figure 10, the carbon nanotube layer was 2The addition of oxides to induce defects was also found to improve the quality of carbon nanotubes synthesized in lithium-free electrolytes. Scale bars in Figures 10A, 10B, and 10C are 200 μm, 30 μm, and 20 μm.

[0112]

[0121] Example 8

[0113]

[0122] 0.05A / cm 2 At a lower current density of 1:1 wt% Na2CO3:BaCO3 electrolyte containing both 30 wt% BaO and 0.04 wt% Fe2O3 and 0.04 wt% Cr2O3 at 770 °C, electrolysis between a NiCr anode and a brass cathode is observed to have a fairly low yield (<20%) of CNTs as product. This suggests that the beneficial effects of (i) the addition of a higher amount of specific transition metal nucleating agent, (ii) the introduction of oxides, and (iii) the application of a lower current density to increase the product yield in a lithium-free electrolyte may not work in combination.

[0114]

[0123] Without being bound by any particular theory, the embodiments and examples described herein provide a high-yield approach to directly produce CNTs from atmospheric CO2 via an electrolytic reaction utilizing a lithium-free electrolyte. This lithium-free approach can be enhanced by the addition of one or more graphene defect agents to the electrolyte, suggesting that sufficiently large defects and vacancies in the CNT layer, introduced by graphene defect agents such as oxides, may be required to allow intercalation of ions larger than lithium cations through the layer of the growing CNT.

[0115]

[0124] The introduction of oxides (e.g., BaO) and additional transition metal nucleating agents (e.g., Fe2O3) may provide a more energetically favorable route for the formation of CNM products, as they may remove electrolyte conductivity inhibition (e.g., to allow higher conductivity), and may affect the stability of certain species formed in lithium-free electrolysis. Without modification of the lithium-free electrolyte electrolysis conditions, CNM products may still be observed, but in low yields. However, using lithium-free sodium carbonate / barium carbonate electrolyte under either of the following conditions: (i) the addition of a larger amount of specific transition metal nucleating agents, e.g., Fe2O3; (ii) the introduction of a high concentration of oxides, e.g., BaO, to induce larger defects in the growing CNTs; or (iii) low current density to overcome the conductivity challenge, CNTs with a yield of over 80% may be observed. Although high yield growth of carbon nanotubes is exemplified herein, systematic variation of the melt electrochemical configurations disclosed herein may provide a route to alternative growth of other carbon nanomaterials, such as carbon nanofibers, carbon nano-onions, hollow carbon nanospheres, carbon nanoplatelets or graphene, in lithium-free electrolytes.

[0116]

[0125] Example 9

[0117]

[0126] Lithium salts are exemplified by, but are not limited to, lithium carbonate, lithium oxide, lithium silicate, lithium nitrate, lithium sulfate, lithium phosphate, lithium borate, lithium halides, or combinations thereof. Examples of lithium halides include, but are not limited to, lithium chloride, lithium bromide, lithium iodide, or combinations thereof. Low concentrations of lithium salts may add improved properties without adding substantial lithium cost to the electrolyte. Examples of improved properties are exemplified by, but are not limited to, increased electrolyte conductivity and / or improved purity or selectivity of the carbon nanomaterial product. The ability to increase electrolyte conductivity through the addition of lithium salts is clearly seen in the relative conductivity magnitudes of pure alkali carbonates of 6, 3, and 2 S / cm for lithium carbonate, sodium carbonate, and potassium carbonate, respectively. Like barium oxide and unlike calcium oxide, lithium oxide is also highly soluble in carbonate electrolytes. CNM products are also clearly seen with the addition of either 1% or 5% lithium carbonate or lithium borate to the electrolytes of Examples 4, 5, and 7. By including lithium borate in the electrolyte, boron-doped carbon nanotubes can be formed.

[0118]

[0127] Electrolytes made as mixtures of sodium carbonate and barium carbonate are an order of magnitude less expensive than comparable lithium carbonate-based electrolytes. The use of binary (e.g., sodium carbonate / barium carbonate) and / or ternary (e.g., Na / Ba carbonate+barium oxide) electrolytes can provide electrolyte melting points within the optimal range of CO2 for carbon nanomaterial growth of about 700°C to about 800°C. Lithium-free electrolysis can be performed with planar rather than coiled and brass rather than Monel cathodes without substantial impact on lithium-free CNT growth.

Claims

1. 1. A method for producing a CNM product, comprising: (a) heating a lithium-free carbonate electrolyte to obtain a molten carbonate electrolyte; (b) positioning the molten carbonate electrolyte between an anode and a cathode of an electrolytic cell; (c) applying a current to the cathode and the anode of the electrolysis cell; (d) collecting a carbon nanomaterial (CNM) product from the cathode; and The method includes:

2. The method of claim 1 further comprising utilizing one or more non-lithium promoter elements.

3. 3. The method of claim 2, wherein the one or more non-lithium promoting factors are: (i) enhancing transition metal nucleation by adding one or more transition metal nucleating agents; (ii) adding one or more defect inducing agents; (iii) reducing electrolyte conductivity inhibiting factors; and (iv) any combination thereof.

4. 4. The method of claim 3, wherein the step of adding one or more defect inducers comprises introducing one or more oxides into the lithium-free carbonate electrolyte.

5. 5. The method of claim 4, wherein the one or more oxides are one or more of barium oxide, sodium oxide, calcium oxide, iron oxide, cobalt oxide, lithium oxide, or any combination thereof.

6. The method of claim 3 , wherein the one or more transition metal nucleating agents comprise a transition metal salt in the electrolyte.

7. 4. The method of claim 3, wherein the removing the electrolyte conductivity inhibition step comprises inducing one or more graphene defects in the CNM product.

8. 8. The method of claim 7, wherein the step of inducing graphene defects comprises adding one or more foreign adatoms, one or more substitutional impurities, or any combination thereof.

9. The method of claim 2 , wherein the step of removing the electrolytic conductivity obstruction comprises reducing a current density of the current.

10. 6. The method of claim 5, wherein the transition metal salt is one or more of a salt comprising iron, chromium, nickel, copper, manganese, titanium, zirconium, molybdenum, tantalum, tungsten, silver, cadmium, tin, ruthenium, vanadium, cobalt, or any combination thereof.

11. The method of claim 1 further comprising the step of adding an oxidizing agent to induce structural defects in the CNM product.

12. The method of claim 4 , wherein the one or more oxides are alkali oxides, alkaline earth oxides, and any combination thereof.

13. The method of claim 4 , wherein the one or more oxides comprise a metal oxide, a non-metal oxide, or any combination thereof.

14. The method of claim 4 , wherein the one or more oxides include sodium oxide, barium oxide, calcium oxide, or any combination thereof.

15. 5. The method of claim 4, wherein the one or more oxides are introduced into the molten carbonate electrolyte in a further step of increasing or decreasing the temperature of the lithium-free carbonate electrolyte.

16. The method of claim 4 , wherein the one or more oxides are introduced into the molten carbonate electrolyte by oxidizing the anode.

17. The method of claim 1 further comprising the step of introducing a nanomaterial selection component into the electrolytic cell.

18. The method of claim 1 further comprising the step of adding a doping component into the electrolytic cell.

19. 20. The method of claim 17, wherein the nanomaterial selection component selects the CNM product to include a carbon nanotube (CNT) product.

20. The method of claim 17 , wherein the nanomaterial selection component selects the CNM product to include a carbon nanofiber product.

21. 20. The method of claim 17, wherein the nanomaterial selection component selects the CNM product to include a carbon platelet product.

22. 20. The method of claim 17, wherein the nanomaterial selection component selects the CNM product to include a graphene product.

23. 20. The method of claim 17, wherein the nanomaterial selection component selects the CNM product to include a carbon nano-onion product.

24. 20. The method of claim 17, wherein the nanomaterial selection component selects the CNM product to include a hollow carbon nanosphere product.

25. 10. The method of claim 1, wherein the lithium-free carbonate electrolyte comprises a non-lithium alkali carbonate, an alkaline earth carbonate, and any combination thereof.

26. 10. The method of claim 1, wherein the lithium-free carbonate electrolyte is one of a binary mixture, a ternary mixture, or a mixture of more than three components.

27. 27. The method of claim 26, wherein the lithium-free carbonate electrolyte comprises sodium carbonate, calcium carbonate, barium carbonate, and any combination thereof.

28. The method of claim 1 further comprising the step of introducing a doping component to produce a doped CNM product.

29. The method of claim 1 further comprising the step of introducing a magnetic additive component to produce a magnetic CNM product.

30. 10. The method of claim 1, wherein the lithium-free carbonate electrolyte comprises lithium in an amount based on the weight of the total mixture, less than about 5% (wt%), or less than about 4% by weight of the total mixture, less than about 3% by weight of the total mixture, or less than about 2% by weight of the total mixture.

31. 31. The method of claim 30, wherein the lithium is present as lithium carbonate, lithium oxide, lithium chloride, lithium bromide, lithium iodide, lithium silicate, lithium nitrate, lithium sulfate, lithium phosphate, lithium borate, or any combination thereof.

32. 1. An electrolysis cell for making a CNM product, comprising: one or more walls defining a plenum; an anode and a cathode positioned within the plenum, the plenum configured to receive a lithium-free molten carbonate electrolyte between the anode and the cathode; The cell is further configured to receive an electric current applicable to the anode and the cathode to initiate an electrolytic reaction to produce a graphene defect agent, a nanomaterial select component, and a CNM product in the plenum.

33. 33. The electrolysis cell of claim 32, wherein the anode and the cathode are vertically spaced apart from one another.

34. 33. The electrolysis cell of claim 32, wherein the anode is made of nickel or a nickel alloy.

35. 33. The electrolytic cell of claim 32, wherein the anode is a coiled wire aligned in a horizontal plane.

36. 33. The electrolysis cell of claim 32, wherein the cathode is made of brass, steel, galvanized steel, copper, Monel, nickel alloy and any combination thereof.

37. 33. The electrolytic cell of claim 32, wherein the cathode is a coiled wire aligned in a horizontal plane.

38. 33. The electrolysis cell of claim 32, further comprising a heating device for melting the lithium free carbonate electrolyte and / or maintaining the lithium free carbonate electrolyte in a molten state.

39. 33. The electrolysis cell of claim 32, wherein the graphene defect agent is a chemical entity, a mechanical entity, an optical entity, a physical entity, or any combination thereof that induces graphene defects and / or graphene vacancies in the graphitic structure of the CNM product.

40. 33. The electrolytic cell of claim 32, wherein the lithium-free molten carbonate electrolyte is one of a binary mixture, a ternary mixture, or a mixture of more than three components.

41. 33. The electrolytic cell of claim 32, wherein the lithium-free molten carbonate electrolyte comprises sodium carbonate, calcium carbonate, barium carbonate, and any combination thereof.

42. 1. A system for synthesizing a CNM product, comprising: (a) a heater for heating a lithium-free carbonate electrolyte to obtain a molten carbonate electrolyte; (b) an electrolytic cell for receiving or containing said molten carbonate electrolyte between an anode and a cathode of the electrolytic cell; (c) one or more non-lithium promoters; (d) a current source for applying a current to the cathode and the anode of the electrolysis cell; A system including:

43. 43. The method of claim 42, wherein the lithium-free carbonate electrolyte comprises lithium in an amount less than about 0.1%, less than about 0.05%, or less than about 0.025%, or less than about 0.01% by weight of the total mixture.

Citation Information

Patent Citations

  • Methods and systems for carbon nanofiber production

    JP2018513911A

  • Method and system for producing long carbon nanofibers

    JP2019535906A

  • Method and system for producing doped carbon nanomaterials

    JP2020514542A