Nonaqueous electrolyte for lithium secondary battery and lithium secondary battery containing same

The non-aqueous electrolyte with an isocyanate or isothiocyanate compound forms a stable film to address thermal decomposition issues in lithium-ion batteries, enhancing high-temperature safety and performance by scavenging Lewis acids and suppressing transition metal ion elution.

JP2024536177AActive Publication Date: 2024-10-04LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024519399
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-22
Filing Date
2022-10-18
Publication Date
2024-10-04
Estimated Expiration
2042-10-18

AI Technical Summary

Technical Problem

Lithium-ion batteries are prone to thermal decomposition of lithium salts, leading to the generation of Lewis acids that corrode electrode surfaces, causing transition metal ion elution, increased resistance, and reduced battery performance, especially at high temperatures.

Method used

A non-aqueous electrolyte for lithium secondary batteries containing a compound with an isocyanate or isothiocyanate terminal group is used to form a stable film on electrode surfaces, effectively scavenging Lewis acids and suppressing transition metal ion elution.

Benefits of technology

The solution enhances high-temperature storage safety and performance by reducing gas generation and resistance, improving capacity retention and cycle characteristics of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536177000001
    Figure 2024536177000001
  • Figure 2024536177000002
    Figure 2024536177000002
  • Figure 2024536177000003
    Figure 2024536177000003
Patent Text Reader

Abstract

The present invention relates to a non-aqueous electrolyte for a lithium secondary battery that can form a stable coating on the surface of an electrode, and a lithium secondary battery containing the same. Specifically, the non-aqueous electrolyte for a lithium secondary battery of the present invention may contain a lithium salt, a non-aqueous organic solvent, and a compound represented by Chemical Formula 1.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0142019, filed on October 22, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a nonaqueous electrolyte solution for a lithium secondary battery, which contains an additive capable of forming a stable coating on the surfaces of a positive electrode and a negative electrode, and a lithium secondary battery containing the same, which has improved high-temperature storage safety. [Background technology]

[0003] In recent years, the development of the information society has led to the development of personal IT devices and computer networks, which has increased society's overall dependence on electrical energy. This has led to a demand for the development of battery technology that can efficiently store and utilize electrical energy.

[0004] In particular, with growing interest in solving environmental problems and realizing a sustainable recycling-based society, extensive research is being conducted on lithium-ion batteries, which are attracting attention as a clean energy source with low carbon dioxide emissions.

[0005] Lithium-ion batteries can be miniaturized to the extent that they can be used in personal IT devices, and because they have high energy density and operating voltage, they are used not only as power sources for laptop computers and mobile phones, but also for power storage and electric vehicles.

[0006] The lithium-ion secondary battery comprises a positive electrode whose main component is a lithium-containing transition metal oxide, a negative electrode made of a lithium alloy or a carbonaceous material such as graphite, a separator interposed between the positive electrode and the negative electrode, and a nonaqueous electrolyte that serves as a medium for Li ions to move in. The nonaqueous electrolyte is typically one in which an electrolyte such as lithium hexafluorophosphate (LiPF6) is dissolved in an organic solvent with a high dielectric constant such as ethylene carbonate or dimethyl carbonate.

[0007] On the other hand, electrolytes such as lithium hexafluorophosphate (LiPF6) are sensitive to heat and moisture and can react with moisture present inside the cell or undergo thermal decomposition to generate Lewis acids such as PF5. These Lewis acids can erode the passivation film formed at the electrode-electrolyte interface, potentially causing transition metal ions to leach from the positive electrode. These leachable transition metal ions can accelerate gas generation by promoting the decomposition of the electrolyte solvent, or they can be redeposited on the positive electrode, increasing the resistance of the positive electrode. They can also migrate to the negative electrode via the electrolyte and be electrodeposited on the negative electrode, causing self-discharge of the negative electrode, breakdown and regeneration of the solid electrolyte interphase (SEI), resulting in additional lithium ion consumption and increased resistance.

[0008] Therefore, there is a need for a non-aqueous electrolyte composition that can remove by-products (such as HF and PF5) generated by the thermal decomposition of lithium salts, and that can form a stable coating on the surface of the electrode to suppress the elution of transition metals, or that can suppress the electrodeposition of eluted transition metal ions onto the negative electrode, thereby improving not only safety but also battery performance such as high-rate charge / discharge characteristics. Summary of the Invention [Problem to be solved by the invention]

[0009] In order to solve the above problems, an object of the present invention is to provide a nonaqueous electrolyte solution for a lithium secondary battery that forms a stable ion-conductive coating on the surface of an electrode and contains an additive that can effectively remove decomposition products of lithium salts.

[0010] Another object of the present invention is to provide a lithium secondary battery that contains the nonaqueous electrolyte solution for lithium secondary batteries and thereby has improved high-temperature storage safety. [Means for solving the problem]

[0011] According to one embodiment, the present invention comprises: A lithium salt, a non-aqueous organic solvent; and a compound represented by the following Chemical Formula 1:

[0012] [ka]

[0013] In the above Chemical Formula 1, R is an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 1 to 6 carbon atoms, or an alkynyl group having 1 to 6 carbon atoms; R1 is an alkylene group having 1 to 3 carbon atoms, X is O or S.

[0014] In addition, one embodiment of the present invention provides a lithium secondary battery including a negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and the nonaqueous electrolyte solution for a lithium secondary battery of the present invention. [Effects of the Invention]

[0015] The nonaqueous electrolyte solution of the present invention contains, as an additive, a compound having an isocyanate (-NCO) or isothiocyanate (-NCS) terminal group, which effectively scavenges Lewis acids generated as decomposition products of the electrolyte salt, forms stable coatings on the surfaces of the positive and negative electrodes, and reduces deterioration of the SEI coating.

[0016] Therefore, by using the nonaqueous electrolyte of the present invention, it is possible to realize a lithium secondary battery that is prevented from leaching out of the positive electrode and has improved high-temperature storage safety. DETAILED DESCRIPTION OF THE INVENTION

[0017] The present invention will now be described in more detail.

[0018] The terms and words used in this specification and claims should not be interpreted in a limited way to their ordinary or dictionary meanings, but should be interpreted in a way that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best explain their inventions.

[0019] On the other hand, in this specification, the terms "comprise," "include," "comprise," or "have" are intended to specify the presence of implemented features, numbers, steps, components, or combinations thereof, and should be understood not to preclude the presence or possibility of addition of one or more other features, numbers, steps, components, or combinations thereof.

[0020] Furthermore, prior to describing the present invention, in the description of "number of carbon atoms a to b" in the specification, "a" and "b" refer to the number of carbon atoms contained in a specific functional group. That is, the functional group can contain "a" to "b" carbon atoms. For example, "an alkyl group having 1 to 5 carbon atoms" refers to an alkyl group containing 1 to 5 carbon atoms, i.e., -CH3, -CH2CH3, -CH2CH2CH3, -CH2(CH3)CH3, -CH(CH3)CH3, and -CH(CH3)CH2CH3.

[0021] In addition, in this specification, unless otherwise defined, the term "substituted" means that at least one hydrogen atom bonded to a carbon atom is substituted with an element other than hydrogen, for example, with an alkyl group having 1 to 4 carbon atoms or a fluorine atom.

[0022] Also, in this specification, "%" means % by weight unless expressly indicated otherwise.

[0023] During operation of a secondary battery, structural changes in the positive electrode due to repeated charge and discharge cycles can easily cause transition metal ions to leach from the positive electrode into the electrolyte, reducing the amount of available lithium ions in the battery and resulting in battery capacity degradation. In particular, Lewis acids generated by thermal decomposition of the electrolyte salt can degrade passivation films such as the solid electrolyte interphase (SEI), accelerating the leaching of transition metal ions. These leached transition metal ions can be re-deposited on the positive electrode, increasing its resistance, or electrodeposited on the surface of the negative electrode, destroying the SEI film and potentially causing an internal short circuit. This series of reactions accelerates the decomposition of the electrolyte, increasing gas generation, increasing the interfacial resistance and self-discharge of the negative electrode, and resulting in low-voltage failure.

[0024] An object of the present invention is to provide a nonaqueous electrolyte for a lithium secondary battery that can remove Lewis acids that cause such deterioration and poor behavior, and can form strong coatings on the surfaces of the positive electrode and negative electrode, thereby suppressing additional elution and electrodeposition of transition metal ions, and a lithium secondary battery containing the same.

[0025] Nonaqueous electrolyte for lithium secondary batteries One embodiment of the present invention provides a non-aqueous electrolyte for a lithium secondary battery.

[0026] The nonaqueous electrolyte for a lithium secondary battery is A lithium salt, a non-aqueous organic solvent; and a compound represented by the following chemical formula 1:

[0027] [ka]

[0028] In the above Chemical Formula 1, R is an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 1 to 6 carbon atoms, or an alkynyl group having 1 to 6 carbon atoms; R1 is an alkylene group having 1 to 3 carbon atoms, X is O or S.

[0029] (1) Lithium salt The lithium salt may be any one that is commonly used in electrolytes for lithium secondary batteries, and may be any one of the lithium salts that is commonly used in electrolytes for lithium secondary batteries. For example, the lithium salt may be a cation such as Li + and as an anion, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO4 - , PF6 -, CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - , and SCN - In addition to these, any lithium salt that is normally used in the electrolyte of a lithium secondary battery can be used without any restrictions.

[0030] Specifically, the lithium salts include LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10, LiAlCl4, LiAlO4, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiN(SO2F)2 (Lithium bis(fluorosulfonyl)imide, LiFSI), LiN(SO2CF2CF3)2 (lithium bis(perfluoroethanesulfonyl)imide, LiBETI), and LiN(SO2CF3)2 (lithium bis(trifluoromethanesulfonyl)imide, LiTFSI), and more specifically, may include at least one selected from the group consisting of LiBF4, LiClO4, LiPF6, LiN(SO2F)2, LiN(SO2CF2CF3)2, and LiN(SO2CF3)2.

[0031] The lithium salt can be varied as appropriate within a range that is normally usable, but in order to obtain the optimum effect of forming a corrosion-preventing coating on the electrode surface, it may be contained in the electrolyte at a concentration of 0.8 M to 3.0 M, specifically 1.0 M to 3.0 M. When the concentration of the lithium salt satisfies the above range, the viscosity of the nonaqueous electrolyte can be controlled to achieve optimum impregnation, and the mobility of lithium ions can be improved, thereby obtaining an effect of improving the capacity characteristics and cycle characteristics of the lithium secondary battery.

[0032] (2) Non-aqueous organic solvent The non-aqueous organic solvent of the present invention may include a cyclic carbonate organic solvent, a linear carbonate organic solvent, or a mixed organic solvent thereof.

[0033] The cyclic carbonate organic solvent is a highly viscous organic solvent that has a high dielectric constant and therefore easily dissociates the lithium salt in the electrolyte solution. Specific examples of the cyclic carbonate organic solvent include at least one organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and among these, ethylene carbonate may be included.

[0034] The linear carbonate organic solvent is an organic solvent having low viscosity and low dielectric constant, and a representative example thereof may be at least one organic solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and specifically may include dimethyl carbonate (DMC).

[0035] In the present invention, in order to ensure high ionic conductivity of the nonaqueous electrolyte, the cyclic carbonate organic solvent and the linear carbonate organic solvent may be mixed at a volume ratio of 10:90 to 50:50, specifically 15:85 to 30:70.

[0036] In addition, in order to prepare an electrolyte solution having high ionic conductivity, the non-aqueous organic solvent may further include at least one organic solvent selected from the group consisting of a linear ester organic solvent and a cyclic ester organic solvent, which have a lower melting point and higher storage stability at high temperatures than the cyclic carbonate organic solvent and / or the linear carbonate organic solvent.

[0037] Specific examples of such linear ester-based organic solvents include at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.

[0038] The cyclic ester organic solvent may be at least one organic solvent selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.

[0039] The non-aqueous organic solvent may further contain, if necessary, any organic solvent commonly used in electrolytes for lithium secondary batteries, including, for example, at least one of an ether-based organic solvent, an amide-based organic solvent, and a nitrile-based organic solvent.

[0040] (3) Compound represented by chemical formula 1 The nonaqueous electrolyte for a lithium secondary battery of the present invention may contain a compound represented by the following Chemical Formula 1 as a first additive.

[0041] [ka]

[0042] In the above Chemical Formula 1, R is an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 1 to 6 carbon atoms, or an alkynyl group having 1 to 6 carbon atoms; R1 is an alkylene group having 1 to 3 carbon atoms, X is O or S.

[0043] The compound represented by Formula 1 contains a nitrogen-containing isocyanate (-NCO) or isothiocyanate (-NCS) terminal group within its structure. The unshared electron pair of the nitrogen reacts with and bonds with a Lewis acid, e.g., HF, generated as a decomposition product of the electrolyte salt, forming a complex that effectively scavenges the Lewis acid. Furthermore, the compound represented by Formula 1 is reduced on the surfaces of the negative and positive electrodes prior to the non-aqueous organic solvent, forming a stable passivation film. This prevents the elution of transition metals from the positive electrode and further inhibits electrolyte decomposition, resulting in reduced gas generation during high-temperature storage and improved high-temperature cycling.

[0044] Specifically, in the above Chemical Formula 1, R may be a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, or a substituted or unsubstituted alkynyl group having 1 to 6 carbon atoms.

[0045] In addition, in the above chemical formula 1, R may be a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms, or a substituted or unsubstituted alkynyl group having 1 to 4 carbon atoms.

[0046] In this case, the substitutable substituent may be selected from, as a representative example, an alkyl group having 1 to 4 carbon atoms and at least one fluorine atom.

[0047] Preferably, the compound represented by Chemical Formula 1 may be at least one of the compounds represented by Chemical Formulas 1-1 to 1-4 below.

[0048] [ka]

[0049] [ka]

[0050] [ka]

[0051] [ka]

[0052] The compound represented by Chemical Formula 1 may be included in an amount of 0.3 wt % to 5 wt % based on the total weight of the non-aqueous electrolyte solution for lithium secondary batteries.

[0053] When the compound represented by Chemical Formula 1 is contained within the above range, a secondary battery with improved performance can be manufactured. For example, when the content of the compound represented by Chemical Formula 1 is 0.3 wt % or less, the SEI formation effect is minimal, and the gas reduction effect during high-temperature storage and the improvement effect of high-temperature cycle characteristics may be minimal. Specifically, when the content of the compound represented by Chemical Formula 1 is 0.3 wt % or more, a stabilizing effect and an elution prevention effect are obtained during the formation of the SEI film. When the content of the compound represented by Chemical Formula 1 is 5 wt % or less, an increase in the viscosity of the electrolyte due to excess compound is prevented, while minimizing the increase in resistance. Furthermore, excessive film formation is suppressed, effectively preventing an increase in battery resistance. Therefore, the elution prevention effect can be maximized within the allowable increase in resistance.

[0054] Specifically, the compound represented by Chemical Formula 1 may be included in an amount of 0.5 wt % to 3 wt % based on the total weight of the non-aqueous electrolyte solution for lithium secondary batteries.

[0055] (4) Other additives In addition, the non-aqueous electrolyte of the present invention may further contain a second other additive to prevent the non-aqueous electrolyte from being decomposed in a high-power environment, which may cause the collapse of the negative electrode, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and the effect of suppressing battery expansion at high temperatures.

[0056] Examples of such other additives include at least one selected from the group consisting of cyclic carbonate compounds, halogen-substituted carbonate compounds, sultone compounds, sulfate compounds, phosphate or phosphite compounds, borate compounds, benzene compounds, amine compounds, silane compounds, and lithium salt compounds.

[0057] Examples of the cyclic carbonate compounds include vinylene carbonate (VC) and vinyl ethylene carbonate (VEC).

[0058] Examples of the halogen-substituted carbonate compounds include fluoroethylene carbonate (FEC).

[0059] The sultone compound may be, for example, at least one compound selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.

[0060] The sulfate-based compound may be, for example, ethylene sulfate (Esa), trimethylene sulfate (TMS), methyl trimethylene sulfate (MTMS), or the like.

[0061] The phosphate- or phosphite-based compound may be, for example, one or more compounds selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.

[0062] Examples of the borate-based compounds include tetraphenylborate, lithium oxalyldifluoroborate (LiODFB) which can form a coating on the surface of the negative electrode, and lithium bisoxalateborate (LiB(C2O4)2, LiBOB).

[0063] The benzene-based compound may be fluorobenzene, the amine-based compound may be triethanolamine, ethylenediamine, or the like, and the silane-based compound may be tetravinylsilane, or the like.

[0064] The lithium salt compound is a compound different from the lithium salt contained in the non-aqueous electrolyte, and examples thereof include LiPO2F2 and LiBF4.

[0065] Among these other additives, at least one selected from the group consisting of vinylene carbonate, vinylethylene carbonate, fluoroethylene carbonate (FEC), propene sultone, ethylene sulfate, LiBF4, and lithium oxalyl difluoroborate (LiODFB), which have an excellent effect of forming a coating on the surface of the negative electrode, may be included in order to form a stronger SEI coating on the surface of the negative electrode during the initial activation step.

[0066] The other additives may be used as a mixture of two or more compounds, and may be contained in an amount of 0.01 to 20% by weight, specifically 0.01 to 10% by weight, based on the total weight of the non-aqueous electrolyte solution.

[0067] When the other additives are contained in the above ranges, a secondary battery with further improved performance can be manufactured. For example, when the other additives are contained in an amount of 0.01 wt % or more, the durability of the SEI film is improved, and when the other additives are contained in an amount of 20 wt % or less, the increase in resistance is minimized and the SEI film can be maintained for a long period of time within a tolerable increase in resistance.

[0068] Lithium secondary battery In addition, another embodiment of the present invention provides a lithium secondary battery including a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and the non-aqueous electrolyte of the present invention described above.

[0069] The lithium secondary battery of the present invention can be manufactured by forming an electrode assembly in which a positive electrode, a negative electrode, and a separator are sequentially laminated between the positive electrode and the negative electrode, housing the electrode assembly in a battery case, and then injecting the non-aqueous electrolyte of the present invention.

[0070] The lithium secondary battery of the present invention can be manufactured by a conventional method known in the art, and the manufacturing method of the lithium secondary battery of the present invention is specifically as described below.

[0071] (1) Positive electrode The positive electrode according to the present invention includes a positive electrode active material layer containing a positive electrode active material, and optionally, the positive electrode active material layer may further contain a conductive material and / or a binder.

[0072] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, may include a lithium composite metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium.

[0073] Specifically, the positive electrode active material is a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-Z Ni Z O4 (where 0 < Z < 2), etc.), a lithium-nickel-cobalt-based oxide (e.g., LiNi 1-Y1 Co<{ Y1 O2 (where 0 < Y1 < 1), etc.), a lithium-manganese-cobalt-based oxide (e.g., LiCo 1-Y2 MnY2 O2 (where 0 < Y2 < 1), LiMn 2-Z1 Co Z1 O4 (where 0 < Z1 < 2), etc.), lithium-nickel-manganese-cobalt-based oxide (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r < 2, p1 + q1 + r2 = 2), etc.), lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r3 M s2 )O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, Ti, and Mo, and p2, q2, r3, and s2 are atomic fractions of independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1), etc. may be included, and any one or two or more of these compounds may be included.

[0074] Among them, from the viewpoint of being able to enhance the capacity characteristics and stability of the battery, the positive electrode active material may include at least one selected from the group consisting of lithium-cobalt-based oxide, lithium-manganese-based oxide, lithium-nickel-manganese-cobalt-based oxide, and lithium-nickel-cobalt-transition metal (M) oxide.

[0075] Specifically, the positive electrode active material may include at least one selected from a lithium-nickel-manganese-cobalt-based oxide having a nickel content of 55 atm% or more and a lithium-nickel-cobalt-transition metal (M) oxide having a nickel content of 55 atm% or more. Specifically, the positive electrode active material may include a lithium-nickel-manganese-cobalt-based oxide represented by the following Chemical Formula 2.

[0076] [Chemical Formula 2] Li(Ni) a Co b Mn c M d )O2

[0077] In the above Chemical Formula 2, M is W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, or Mo; a, b, c, and d are the atomic fractions of each independent element; 0.55≦a<1, 0 <b≦0.3、0<c≦0.3、0≦d≦0.1、a+b+c+d=1である。

[0078] Specifically, the a, b, c, and d may be 0.60≦a≦0.95, 0.01≦b≦0.20, 0.01≦c≦0.20, and 0≦d≦0.05, respectively.

[0079] Specifically, the positive electrode active material is, for example, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2, Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, and Li(Ni 0.9 Co 0.06 Mn 0.03 Al 0.01 ) O2.

[0080] The positive electrode active material may be included in an amount of 80 wt% to 99 wt%, specifically 90 wt% to 99 wt%, based on the total weight of the solid content in the positive electrode slurry. If the content of the positive electrode active material is less than 80 wt%, the energy density may be reduced, resulting in a decrease in capacity.

[0081] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive, and examples thereof include carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, and graphite with highly developed crystal structures; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0082] The conductive material is usually added in an amount of 1 to 30% by weight based on the total weight of the solid content in the positive electrode active material layer.

[0083] The binder is a component that functions to improve adhesion between positive electrode active material particles and between the positive electrode active material and the current collector, and is typically added in an amount of 1 to 30 wt% based on the total weight of the solids in the positive electrode active material layer. Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.

[0084] The positive electrode of the present invention may be manufactured by a method known in the art. For example, the positive electrode may be manufactured by a method of dissolving or dispersing a positive electrode active material, a binder, and / or a conductive material in a solvent to prepare a positive electrode slurry, which is then coated on a positive electrode current collector, followed by drying and rolling to form a positive electrode active material layer, or by a method of casting the positive electrode active material layer on a separate support, peeling off the support, and laminating the resulting film on a positive electrode current collector.

[0085] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, or the like may be used.

[0086] The solvent may include an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a suitable viscosity when the positive electrode active material, and optionally a binder and a conductive material, are contained. For example, the solvent may be contained so that the solids concentration in the active material slurry containing the positive electrode active material, and optionally a binder and a conductive material, is 10 wt % to 90 wt %, preferably 30 wt % to 80 wt %.

[0087] (2) Negative electrode Next, the negative electrode will be described.

[0088] The negative electrode according to the present invention includes a negative electrode active material layer containing a negative electrode active material, and the negative electrode active material layer may further include a conductive material and / or a binder, as necessary.

[0089] The negative electrode active material may be any of various negative electrode active materials used in the art, such as a carbon-based negative electrode active material, a silicon-based negative electrode active material, or a mixture thereof.

[0090] According to one embodiment, the negative electrode active material may include a carbon-based negative electrode active material, and the carbon-based negative electrode active material may be any of various carbon-based negative electrode active materials used in the art, such as graphite-based materials such as natural graphite, artificial graphite, and Kish graphite; pyrolytic carbon, mesophase pitch-based carbon fiber, mesocarbon microbeads, mesophase pitches, and high-temperature-calcined carbon such as petroleum or coal tar pitch-derived cokes; soft carbon; and hard carbon. The shape of the carbon-based negative electrode active material is not particularly limited, and various shapes such as amorphous, plate-like, flake-like, spherical, and fibrous may be used.

[0091] Preferably, the negative electrode active material is at least one carbon-based negative electrode active material selected from natural graphite and artificial graphite. In order to increase the adhesive strength with the current collector and suppress detachment of the active material, both natural graphite and artificial graphite may be used.

[0092] According to another embodiment, the negative electrode active material may include a silicon-based negative electrode active material in addition to the carbon-based negative electrode active material.

[0093] The silicon-based negative electrode active material is, for example, metal silicon (Si), silicon oxide (SiO x, where 0 < x < 2), silicon carbide (SiC), and Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si) may be included. The element Y may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0094] Since the silicon-based negative electrode active material exhibits higher capacity characteristics than the carbon-based negative electrode active material, when the silicon-based negative electrode active material is further included, even more excellent capacity characteristics can be obtained. However, a negative electrode containing a silicon-based negative electrode active material contains more oxygen (O)-rich components in the SEI film than a graphite negative electrode, and an SEI film containing an O-rich component tends to be further decomposed when a Lewis acid such as HF or PF5 is present in the electrolyte. Therefore, in order for a negative electrode containing a silicon-based negative electrode active material to maintain a stable SEI film, it is necessary to suppress the generation of Lewis acids such as HF and PF5 in the electrolyte or to remove (or scavenge) the generated Lewis acids. The non-aqueous electrolyte according to the present invention forms stable films on the positive and negative electrodes and contains an electrolyte additive having an excellent Lewis acid removal effect, so that the decomposition of the SEI film can be effectively suppressed when using a negative electrode containing a silicon-based active material.

[0095] On the other hand, the mixing ratio of the carbon-based negative electrode active material and the silicon-based negative electrode active material may be 50:50 to 99:1, preferably 85:15 to 95:5, by weight. When the mixing ratio of the carbon-based negative electrode active material and the silicon-based negative electrode active material satisfies the above range, the capacity characteristics can be improved, the volume expansion of the silicon-based negative electrode active material can be suppressed, and excellent cycle performance can be ensured.

[0096] On the other hand, the negative electrode active material may, if necessary, be replaced with a carbon-based negative electrode active material or a silicon-based negative electrode active material, and at least one selected from the group consisting of lithium metal, an alloy of a metal and lithium, a metal composite oxide, and a transition metal oxide may be used.

[0097] As the alloy of the metal and lithium, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn or an alloy of these metals and lithium can be used.

[0098] Examples of the metal composite oxide include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3 (0 ≦ x ≦ 1), Li x WO2 (0 ≦ x ≦ 1), and Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, elements of Group 1, Group 2, Group 3 of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8) can be selected from the group consisting of.

[0099] Examples of the transition metal oxide include lithium-containing titanium composite oxide (LTO), vanadium oxide, lithium vanadium oxide, etc.

[0100] The negative electrode active material may be contained at 80% to 99% by weight based on the total weight of the solid content in the negative electrode slurry.

[0101] The conductive material is a component for further improving the conductivity of the negative electrode active material and may be added in an amount of 1 to 20 wt % based on the total weight of the solid content in the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause chemical changes in the battery and has conductivity, and examples thereof include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0102] The binder is a component that aids in bonding between the conductive material, active material, and current collector, and is typically added in an amount of 1 to 30 wt % based on the total weight of the solids in the negative electrode active material layer. Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.

[0103] The negative electrode may be manufactured by a method known in the art, for example, by coating a negative electrode active material slurry prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent onto a negative electrode current collector, rolling and drying the resulting slurry to form a negative electrode active material layer, or by casting the negative electrode active material layer onto a separate support, peeling off the support, and laminating the resulting film onto the negative electrode current collector.

[0104] The negative electrode current collector generally has a thickness of 3 to 500 μm. There are no particular limitations on the negative electrode current collector, so long as it does not cause chemical changes in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, or the like, or an aluminum-cadmium alloy may be used. Furthermore, as with the positive electrode current collector, the bonding strength of the negative electrode active material may be strengthened by forming fine irregularities on the surface, and the negative electrode current collector may be used in various forms, such as a film, sheet, foil, net, porous material, foam, or nonwoven fabric.

[0105] The solvent may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a suitable viscosity when containing the negative electrode active material, and optionally a binder, a conductive material, etc. For example, the solvent may be included so that the solids concentration in the active material slurry containing the negative electrode active material, and optionally a binder and a conductive material, is 50 wt % to 75 wt %, preferably 40 wt % to 70 wt %.

[0106] (3) Separator The separator included in the lithium secondary battery of the present invention may be a commonly used conventional porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, either alone or in a laminate thereof, or a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, polyethylene terephthalate fiber, or the like, but is not limited thereto.

[0107] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0108] Hereinafter, the present invention will be described in detail with reference to examples. However, the examples of the present invention can be modified into various other forms, and the scope of the present invention should not be construed as being limited to the examples detailed below. The examples of the present invention are provided to more completely explain the present invention to those skilled in the art.

[0109] Example Example 1 (Manufacturing non-aqueous electrolytes for lithium secondary batteries) LiPF6 was dissolved in a non-aqueous organic solvent prepared by mixing ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio of 30:70 to a concentration of 1.0 M, and then 0.3 wt% of the compound represented by Formula 1-1, 2.0 wt% of vinylene carbonate (VC), and 1.0 wt% of 1,3-propane sultone (PS) were added to prepare a non-aqueous electrolyte (see Table 1 below).

[0110] (Secondary battery manufacturing) Cathode active material (Li(Ni) 0.8 Mn 0.1 Co 0.1)O2), conductive material (carbon black), and binder (polyvinylidene fluoride) were added to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 97.5:1:1.5 to prepare a cathode slurry (solid content: 50 wt%). The cathode slurry was applied to a 12 μm-thick aluminum (Al) thin film as a cathode current collector, dried, and then roll-pressed to prepare a cathode.

[0111] Anode active material (graphite and SiO = 90:10 weight ratio), binder (SBR-CMC), and conductive material (carbon black) were mixed with water as a solvent in a weight ratio of 97.5:1.5:1.0 to prepare anode slurry (solid content: 60 wt%). The anode slurry was applied to a 6 μm-thick copper (Cu) thin film as anode current collector, dried, and then roll-pressed to prepare anode.

[0112] The positive electrode, a polyolefin-based porous separator coated with inorganic particles (Al2O3), and a negative electrode were sequentially stacked to prepare an electrode assembly, which was then wound into a jelly roll shape and placed in a cylindrical battery case. The non-aqueous electrolyte for lithium secondary batteries was then poured into the battery case to prepare a cylindrical lithium secondary battery having a driving voltage of 4.2 V or more.

[0113] Example 2. A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery including the same were manufactured in the same manner as in Example 1, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including a compound represented by Chemical Formula 1-2 instead of the compound represented by Chemical Formula 1-1.

[0114] Example 3. A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery containing the same were manufactured in the same manner as in Example 1, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including a compound represented by Chemical Formula 1-3 instead of the compound represented by Chemical Formula 1-1.

[0115] Example 4. A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery containing the same were manufactured in the same manner as in Example 1, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including a compound represented by Chemical Formula 1-4 instead of the compound represented by Chemical Formula 1-1.

[0116] Example 5. A non-aqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery containing the same were manufactured in the same manner as in Example 1, except that LiPF was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent prepared by mixing ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio of 30:70, and then 5.0 wt % of the compound represented by Chemical Formula 1-1, 2.0 wt % of vinylene carbonate (VC), and 1.0 wt % of 1,3-propane sultone (PS) were added to prepare a non-aqueous electrolyte for a lithium secondary battery.

[0117] Example 6 A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery including the same were manufactured in the same manner as in Example 5, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including the compound represented by Chemical Formula 1-2 instead of the compound represented by Chemical Formula 1-1.

[0118] Example 7 A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery containing the same were manufactured in the same manner as in Example 5, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including a compound represented by Chemical Formula 1-3 instead of the compound represented by Chemical Formula 1-1.

[0119] Example 8 A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery containing the same were manufactured in the same manner as in Example 5, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including a compound represented by Chemical Formula 1-4 instead of the compound represented by Chemical Formula 1-1.

[0120] Comparative Example 1 A non-aqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery containing the same were manufactured in the same manner as in Example 1, except that LiPF was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent prepared by mixing ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio of 30:70, and then 2.0 wt % of vinylene carbonate (VC) and 1.0 wt % of 1,3-propane sultone (PS) were added to prepare a non-aqueous electrolyte for a lithium secondary battery.

[0121] Comparative Example 2 A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery including the same were manufactured in the same manner as in Example 1, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including a compound represented by the following Chemical Formula 3 instead of the compound represented by Chemical Formula 1-1.

[0122] [ka]

[0123] Comparative Example 3. A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery including the same were manufactured in the same manner as in Example 1, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including a compound represented by the following Chemical Formula 4 instead of the compound represented by Chemical Formula 1-1.

[0124] [ka]

[0125] Comparative Example 4. A nonaqueous electrolyte for a lithium secondary battery and a cylindrical lithium secondary battery including the same were manufactured in the same manner as in Example 5, except that the nonaqueous electrolyte for a lithium secondary battery was manufactured by including the compound represented by Chemical Formula 4 instead of the compound represented by Chemical Formula 1-1.

[0126] [Table 1]

[0127] In Table 1, the abbreviations for the compounds have the following meanings: EC: Ethylene carbonate DMC: Dimethyl carbonate VC: vinylene carbonate PS: 1,3-propane sultone

[0128] Experimental Example Experimental Example 1: Evaluation of capacity retention rate after high temperature (60°C) storage The lithium secondary batteries prepared in Examples 1 to 8 and the lithium secondary batteries prepared in Comparative Examples 1 to 4 were charged at 25°C under constant current / constant voltage (CC / CV) conditions of 0.5C / 4.2V, and then discharged under constant current conditions of 0.5C / 2.5V. The measured discharge capacity was defined as the initial discharge capacity.

[0129] Next, each lithium secondary battery was charged to SOC 100% under the same conditions as the above charging conditions, and then stored at a high temperature of 60° C. for 30 days.

[0130] Thereafter, the battery was charged at 25°C under constant current / constant voltage (CC / CV) conditions of 0.5C / 4.2V and discharged under constant current conditions of 0.5C / 2.5V. The measured discharge capacity was defined as the discharge capacity after high-temperature storage.

[0131] The measured initial discharge capacity and discharge capacity after high-temperature storage were substituted into the following equation 1 to measure the capacity retention, and the results are shown in Table 2 below.

[0132] [Formula 1] Capacity retention rate (%) = (discharge capacity after high-temperature storage / initial discharge capacity) x 100

[0133] [Table 2]

[0134] Referring to Table 2 above, it can be seen that the lithium secondary batteries of Examples 1 to 8 of the present invention are all superior to the lithium secondary batteries of Comparative Examples 1 to 4 in capacity retention rate after high-temperature storage.

[0135] In particular, under the condition that the additive content is equal, the lithium secondary batteries of Examples 1 to 4 have a superior capacity retention rate after high-temperature storage compared to the lithium secondary batteries of Comparative Examples 2 and 3, and the secondary batteries of Examples 5 to 8 have a superior capacity retention rate after high-temperature storage compared to the lithium secondary battery of Comparative Example 4.

[0136] Experimental Example 2: Evaluation of resistance increase rate after high temperature (60°C) storage The lithium secondary batteries prepared in Examples 1 to 8 and Comparative Examples 1 to 4 were charged at 25°C under constant current / constant voltage (CC / CV) conditions of 0.5C / 4.2V and discharged under constant current conditions of 0.5C / 2.5V to adjust the state of charge of the batteries to a state of SOC of 50%. After that, a discharge pulse was applied at a constant current of 0.5C for 10 seconds, and the voltage drop that occurred when this was measured was used to obtain the initial resistance value.

[0137] Next, each lithium secondary battery was charged to SOC 100% under the same conditions as the above charging conditions, and then stored at a high temperature of 60° C. for 30 days.

[0138] Then, the battery was charged at 25°C under constant current / constant voltage (CC / CV) conditions of 0.5C / 4.2V and discharged at constant current conditions of 0.5C / 2.5V to adjust the battery state of charge to 50% SOC. After that, a discharge pulse was applied at a constant current of 0.5C for 10 seconds, and the voltage drop that occurred when this was measured was used to obtain the resistance value after high-temperature storage.

[0139] The measured initial resistance value and resistance value after high-temperature storage were substituted into the following equation 2 to calculate the resistance increase rate (capacity retention), and the results are shown in Table 3 below.

[0140] [Formula 2] Resistance increase rate (%) = {(resistance after high-temperature storage - initial resistance) / initial discharge capacity} x 100

[0141] [Table 3]

[0142] Referring to Table 3, it can be seen that the lithium secondary batteries of Examples 1 to 8 of the present invention have improved resistance increase rates after high-temperature storage compared to the lithium secondary battery of Comparative Example 1.

[0143] In particular, under the condition that the additive content is the same, the lithium secondary batteries of Examples 1 to 4 have an improved resistance increase rate after high-temperature storage compared to the lithium secondary batteries of Comparative Examples 2 and 3, and the secondary batteries of Examples 5 to 8 have an improved resistance increase rate after high-temperature storage compared to the lithium secondary battery of Comparative Example 4.

[0144] Experimental Example 3: Evaluation of gas generation rate after high temperature (60°C) storage The lithium secondary batteries manufactured in Examples 1 to 8 and the lithium secondary batteries manufactured in Comparative Examples 1 to 4 were charged to an SOC of 100% and then stored at a high temperature of 60° C. for 30 days.

[0145] After that, the amount of gases generated inside the battery, such as CO and CO2, was measured.

[0146] The relative gas generation amount of each battery was measured based on the gas generation amount measured in Comparative Example 1, and the results are shown in Table 4 below.

[0147] [Table 4]

[0148] Referring to Table 4, it can be seen that, under the condition that the additive contents are equal, the lithium secondary batteries of Examples 1 to 4 have a reduced amount of gas generated after high-temperature storage compared to the lithium secondary batteries of Comparative Examples 2 and 3, and the secondary batteries of Examples 5 to 8 have a reduced amount of gas generated after high-temperature storage compared to the lithium secondary battery of Comparative Example 4.

[0149] Experimental Example 4: Evaluation of capacity retention rate after rapid charge / discharge at high temperature (40°C) The lithium secondary batteries manufactured in Examples 1 to 8 and the lithium secondary batteries manufactured in Comparative Examples 1 to 4 were subjected to 50 cycles of constant current / constant voltage (CC / CV) charging at 1.0 C / 4.2 V and constant current discharging at 1.0 C / 2.85 V at high temperature (40°C).

[0150] In this case, the discharge capacity measured in one run was set as the initial capacity.

[0151] Thereafter, the initial discharge capacity (100%) and the 50th discharge capacity were substituted into the above-mentioned formula 1 to measure the capacity retention rate, and the results are shown in Table 5 below.

[0152] [Table 5]

[0153] Referring to Table 5, it can be seen that the lithium secondary batteries of Examples 1 to 8 of the present invention have superior capacity retention rates after high-temperature rapid charge / discharge compared to the lithium secondary batteries of Comparative Examples 1 to 4.

Claims

1. A lithium salt; A non-aqueous organic solvent; A non-aqueous electrolyte for a lithium secondary battery comprising a compound represented by the following chemical formula 1: [Formula 1] (In the above Chemical Formula 1, R is a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, a substituted or unsubstituted alkenyl group having 1 to 6 carbon atoms, or a substituted or unsubstituted alkynyl group having 1 to 6 carbon atoms; R 1 is an alkylene group having 1 to 3 carbon atoms, X is O or S.

2. 2. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, wherein in Chemical Formula 1, R is a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, or a substituted or unsubstituted alkynyl group having 1 to 6 carbon atoms.

3. 2. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, wherein in Chemical Formula 1, R is a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms, or a substituted or unsubstituted alkynyl group having 1 to 4 carbon atoms.

4. 2. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, wherein in Chemical Formula 1, the substitutable substituent is at least one selected from the group consisting of an alkyl group having 1 to 4 carbon atoms and at least one fluorine atom.

5. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the compound represented by Chemical Formula 1 is at least one of the compounds represented by Chemical Formulas 1-1 to 1-4 below. [chemical 2] [C3] [C4] [C5]

6. 2. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, wherein the compound represented by Formula 1 is contained in an amount of 0.3 to 5 wt % based on the total weight of the non-aqueous electrolyte for a lithium secondary battery.

7. 2. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, wherein the compound represented by Formula 1 is contained in an amount of 0.5 to 3 wt % based on the total weight of the non-aqueous electrolyte for a lithium secondary battery.

8. 2. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, further comprising at least one other additive selected from the group consisting of cyclic carbonate compounds, halogen-substituted carbonate compounds, sultone compounds, sulfate compounds, phosphate or phosphite compounds, borate compounds, benzene compounds, amine compounds, silane compounds, and lithium salt compounds.

9. A negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and a non-aqueous electrolyte solution, A lithium secondary battery, wherein the nonaqueous electrolyte solution comprises the nonaqueous electrolyte solution for lithium secondary batteries according to claim 1 .

10. 10. The lithium secondary battery according to claim 9, wherein the positive electrode active material includes at least one selected from the group consisting of lithium-cobalt-based oxides, lithium-manganese-based oxides, lithium-nickel-manganese-cobalt-based oxides, and lithium-nickel-cobalt-transition metal (M) oxides.

Citation Information

Patent Citations

  • Electrolyte, electrochemical device including same and electronic device

    CN111740162A

  • Electrolyte, preparation method thereof and lithium ion battery

    CN112531211A

  • Nonaqueous electrolyte secondary battery

    JP2013038072A

  • Electrolyte, battery, battery pack, electronic device, electric vehicle, power storage device and electric power system

    JP2016154079A

  • Nonaqueous electrolyte, and nonaqueous electrolyte secondary battery using the same

    JP2019109997A