Ion-exchangeable glass with high fracture toughness

Lithium aluminosilicate glasses with tailored compositions and ion-exchange processes enhance fracture toughness and compressive stress, addressing damage from drops and scratches in electronic device cover glasses.

JP2024536343APending Publication Date: 2024-10-04CORNING INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024520560
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-04
Filing Date
2022-10-03
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Portable electronic devices such as smartphones and tablets are susceptible to damage from bending failure and sharp contact fractures when dropped, with existing ion-exchanged glasses offering limited protection against dynamic sharp contacts.

Method used

Development of lithium aluminosilicate glasses with specific compositions and ion-exchange processes to create a compressive stress layer and central tension region, enhancing fracture toughness and resistance to indentation cracks.

Benefits of technology

The glasses exhibit high fracture toughness and compressive stress, improving drop performance and resistance to scratches while maintaining thinness and manufacturability, suitable for use in cover glasses of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536343000001_ABST
    Figure 2024536343000001_ABST
Patent Text Reader

Abstract

The glass composition includes 60 mol% to 66 mol% SiO2, 14 mol% to 16 mol% Al2O3, 7 mol% to 9 mol% Li2O, 4 mol% to 6 mol% Na2O, 0.5 mol% to 3 mol% P2O5, 0.5 mol% to 6 mol% B2O3, and 0 mol% to 1 mol% TiO2. The glass composition may have a fracture toughness of 0.75 MPa√m or greater. The glass composition includes SiO2, Al2O3, Li2O, Na2O, P2O5, and B2O3, and a molar ratio of Li2O / Na2O is 1.2 to 2.0, and the glass has a liquidus viscosity in the range of 50 kP to 75 kP, and the glass has a fracture toughness of 0.75 MPa√m or greater. 0.5 Fracture toughness K IC The glass composition is chemically toughenable. The glass composition may be used in glass-based articles or consumer electronic products.
Need to check novelty before this filing date? Find Prior Art

Description

Priority

[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 251,776, filed October 4, 2021, the contents of which are relied upon and incorporated herein by reference in their entirety. [Technical field]

[0002] This disclosure relates generally to glass compositions suitable for use in cover glass for electronic devices. More particularly, this disclosure relates to ion-exchangeable glasses that can be formed into cover glass for electronic devices. [Background technology]

[0003] The portable nature of portable devices such as smartphones, tablets, portable media players, personal computers, and cameras makes these devices particularly susceptible to situations where they are accidentally dropped onto a hard surface, such as the ground. These devices typically incorporate a cover glass that can be damaged upon impact with a hard surface. In many of these devices, the cover glass acts as a cover for the display and may provide touch functionality, and thus, use of the device is adversely affected when the cover glass is damaged.

[0004] There are two primary failure modes for cover glass when the associated portable device is dropped onto a hard surface. One of these modes is bending failure, which occurs due to bending of the glass when the device is subjected to dynamic loads from impact with the hard surface. The other mode is sharp contact failure, which occurs due to the introduction of damage into the glass surface. When glass impacts with rough hard surfaces such as asphalt, granite, etc., sharp indentations can be created on the glass surface. These indentations become breakage sites in the glass surface from which cracks can initiate and propagate.

[0005] Glass can be made more resistant to bending fracture by ion-exchange techniques, which involve inducing compressive stresses in the glass surface. However, ion-exchanged glass is still vulnerable to dynamic sharp contact due to high stress concentrations caused by localized indentation of the glass by the sharp contact.

[0006] Glass manufacturers and manufacturers of handheld devices have continually worked to improve the resistance of handheld devices to breakage due to sharp contact. Solutions range from coatings on the cover glass to bezels that prevent the cover glass from directly impacting a hard surface when the device is dropped onto it. However, due to constraints of aesthetic and functional requirements, it is very difficult to completely prevent the cover glass from impacting a hard surface.

[0007] It is also desirable for portable devices to be as thin as possible. Thus, in addition to strength, it is also desirable to make the glass to be used as a cover glass in a portable device as thin as possible. Therefore, in addition to enhancing the strength of the cover glass, it is also desirable for the glass to have mechanical properties that allow it to be formed by processes that allow the production of thin glass-based articles, such as thin glass sheets. Summary of the Invention [Problem to be solved by the invention]

[0008] Thus, there is a need for glasses that can be strengthened, such as by ion exchange, and that have mechanical properties that allow them to be formed into thin glass-based articles. [Means for solving the problem]

[0009] According to an aspect (1), there is provided a glass comprising 60 mol% to 66 mol% SiO2, 14 mol% to 16 mol% Al2O3, 7 mol% to 9 mol% Li2O, 4 mol% to 6 mol% Na2O, 0.5 mol% to 3 mol% P2O5, 0.5 mol% to 6 mol% B2O3, and greater than 0 mol% to 1 mol% TiO2.

[0010] According to an embodiment (2), there is provided the glass of embodiment (1), comprising from greater than 0 mol % to 0.5 mol % or less of K2O.

[0011] According to embodiment (3), there is provided the glass of any of embodiments (1) through the immediately preceding embodiment, comprising greater than or equal to 0.1 mol % and less than or equal to 0.5 mol % TiO2.

[0012] According to embodiment (4), there is provided a glass of any of embodiments (1) to the immediately preceding embodiment, comprising from 0 mol % to 4 mol % MgO, inclusive.

[0013] According to embodiment (5), there is provided the glass of any of embodiments (1) to the immediately preceding embodiment, comprising 0.1 mol % or more and 1 mol % or less MgO.

[0014] According to embodiment (6), there is provided the glass of any of embodiments (1) to the immediately preceding embodiment, comprising greater than or equal to 0 mol % and less than or equal to 3 mol % CaO.

[0015] According to embodiment (7), there is provided the glass of any of embodiments (1) to the immediately preceding embodiment, comprising greater than or equal to 1 mol % and less than or equal to 2 mol % CaO.

[0016] According to an embodiment (8), there is provided a glass of any of the embodiments (1) to the immediately preceding embodiment, comprising greater than or equal to 0 mol % and less than or equal to 4 mol % SrO.

[0017] According to an embodiment (9), there is provided a glass of any of the embodiments (1) to the immediately preceding embodiment, comprising not less than 0.5 mol % and not more than 2 mol % SrO.

[0018] According to embodiment (10), there is provided the glass of any of embodiments (1) to the immediately preceding embodiment, comprising from greater than or equal to 0 mol % to less than or equal to 1 mol % ZnO.

[0019] According to an embodiment (11), there is provided the glass of any of the embodiments (1) to the immediately preceding embodiment, comprising greater than or equal to 0 mol % and less than or equal to 0.1 mol % SnO2.

[0020] According to an embodiment (12), there is provided the glass of any of the embodiments (1) to the immediately preceding embodiment, comprising greater than or equal to 64 mol % and less than or equal to 65 mol % SiO2.

[0021] According to an embodiment (13), there is provided the glass of any of the embodiments (1) to the immediately preceding embodiment, comprising not less than 15 mol % and not more than 16 mol % Al2O3.

[0022] According to an embodiment (14), there is provided the glass of any of the preceding embodiments (1) to (1), comprising greater than or equal to 7 mol % and less than or equal to 8 mol % LiO.

[0023] According to an embodiment (15), there is provided the glass of any of the embodiments (1) to the immediately preceding embodiment, comprising greater than or equal to 4 mol % and less than or equal to 5 mol % Na2O.

[0024] According to an embodiment (16), there is provided the glass of any of the embodiments (1) to the immediately preceding embodiment, comprising greater than or equal to 0.5 mol % and less than or equal to 1.5 mol % P2O5.

[0025] According to an embodiment (17), there is provided the glass of any of the preceding embodiments (1) to (6), comprising greater than or equal to 3 mol % and less than or equal to 4 mol % B2O3.

[0026] According to an embodiment (18), there is provided the glass of any of the embodiments (1) through the immediately preceding embodiment, wherein the glass is substantially free of Fe2O3.

[0027] According to an embodiment (19), there is provided the glass of any of the embodiments (1) through the immediately preceding embodiment, wherein the glass is substantially free of ZrO2.

[0028] According to an embodiment (20), there is provided the glass of any of the embodiments (1) to the immediately preceding embodiment, wherein the glass is substantially free of Ta2O5, HfO2, La2O3, and Y2O3.

[0029] According to an embodiment (21), there is provided the glass of any of the embodiments (1) to the immediately preceding embodiment, wherein the molar ratio of Li2O / Na2O is from 1.2 or more to 2.0 or less.

[0030] According to an embodiment (22), there is provided the glass of any of the embodiments (1) to the immediately preceding embodiment, wherein the molar ratio of Li2O / Na2O is from 1.6 or more to 2.0 or less.

[0031] According to an embodiment (23), there is provided the glass of any of the preceding embodiments through (1), wherein the glass has a liquidus viscosity in the range of from greater than 50 kP to 75 kP.

[0032] According to aspect (24), the glass has a viscosity of 0.75 MPa m 0.5 Fracture toughness K IC The glass of any of embodiment (1) to the immediately preceding embodiment is provided, having

[0033] According to an embodiment (25), there is provided a glass comprising SiO, AlO, LiO, NaO, PO, and BO, wherein a molar ratio of LiO / NaO is from 1.2 to 2.0, inclusive, the glass having a liquidus viscosity in the range of from 50 kP to 75 kP, and the glass having a liquidus viscosity of 0.75 MPa m 0.5 Fracture toughness K IC has.

[0034] According to an embodiment (26), there is provided the glass of embodiment (25), further comprising TiO2.

[0035] According to embodiment (27), there is provided the glass of any of embodiments (25) to the immediately preceding embodiment, further comprising KO.

[0036] According to embodiment (28), there is provided the glass of any of embodiments (25) to the immediately preceding embodiment, further comprising CaO.

[0037] According to embodiment (29), there is provided the glass of any of embodiments (25) to the immediately preceding embodiment, further comprising MgO.

[0038] According to embodiment (30), there is provided the glass of any of embodiments (25) through the immediately preceding embodiment, further comprising SrO.

[0039] According to embodiment (31), there is provided the glass of any of embodiments (25) through the immediately preceding embodiment, further comprising SnO2.

[0040] According to an embodiment (32), there is provided the glass of any of the embodiments (25) through the immediately preceding embodiment, wherein the glass is substantially free of Fe2O3.

[0041] According to embodiment (33), there is provided the glass of any of embodiments (25) through the immediately preceding embodiment, wherein the glass is substantially free of ZrO2.

[0042] According to embodiment (34), there is provided the glass of any of embodiments (25) to the immediately preceding embodiment, wherein the glass is substantially free of Ta2O5, HfO2, La2O3, and Y2O3.

[0043] According to aspect (35), there is provided a method comprising ion exchanging a glass-based substrate in a molten salt bath to form a glass-based article, the glass-based article comprising a compressive stress layer extending from a surface of the glass-based article to a compression depth, the glass-based article comprising a central tension region, the glass-based substrate being made from the glass of any of the previous aspects.

[0044] According to an embodiment (36), there is provided the method of embodiment (35), wherein the molten salt bath comprises NaNO.

[0045] According to embodiment (37), there is provided the method of any of embodiments (35) to the immediately preceding embodiment, wherein the molten salt bath comprises KNO.

[0046] According to embodiment (38), there is provided the method of any of embodiments (35) to the immediately preceding embodiment, wherein the molten salt bath is at a temperature of 380° C. or more and 470° C. or less.

[0047] According to embodiment (39), there is provided the method of any of embodiments (35) to the immediately preceding embodiment, wherein the ion exchange extends for a period of from 10 minutes or more to 24 hours or less.

[0048] According to embodiment (40), there is provided the method of any of embodiments (35) through the immediately preceding embodiment, further comprising ion exchanging the glass-based article in a second molten salt bath.

[0049] According to an embodiment (41), there is provided the method of the immediately preceding embodiment, wherein the second molten salt bath comprises KNO.

[0050] According to embodiment (42), a glass-based article is provided having a compressive stress layer extending from the surface to a compression depth of the glass-based article, a central tension region, and a composition at the center of the glass-based article comprising: 60 mol% to 66 mol% SiO2, 14 mol% to 16 mol% Al2O3, 7 mol% to 9 mol% Li2O, 4 mol% to 6 mol% Na2O, 0.5 mol% to 3 mol% PO5, 0.5 mol% to 6 mol% BO3, and greater than 0 mol% to 1 mol% TiO2.

[0051] According to embodiment (43), there is provided a glass-based article having a compressive stress layer extending from the surface of the glass-based article to a compression depth; a central tension region; and a composition at the center of the glass-based article comprising SiO2, Al2O3, Li2O, Na2O, PO5, and BO3, wherein the molar ratio of Li2O / Na2O is from ≧1.2 to ≦2.0, wherein a glass having the same composition and microstructure as the composition at the center of the glass-based article has a liquidus viscosity in the range of from ≧50 kP to 75 kP, and a viscosity of ≦0.75 MPa m 0.5 Fracture toughness K IC has.

[0052] According to an embodiment (44), there is provided the glass-based article of any of the embodiments (42) to the immediately preceding embodiment, wherein the compressive stress layer has a compressive stress of 500 MPa or more and 1500 MPa or less.

[0053] According to embodiment (45), there is provided the glass-based article of any of embodiments (42) through the immediately preceding embodiment, wherein the central tension region has a maximum central tension of 60 MPa or more and 160 MPa or less.

[0054] According to embodiment (46), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the compression depth is from 0.20t to 0.25t, inclusive, where t is the thickness of the glass-based article.

[0055] According to embodiment (47), there is provided the glass-based article of any of embodiments (42) through the immediately preceding embodiment, wherein the compressive stress layer has a compressive stress spike extending from a surface of the glass-based article to a compressive stress spike depth, the compressive stress spike depth being from 3 μm or more to 10 μm or less.

[0056] According to embodiment (48), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the glass-based article has a thickness, t, of 0.2 mm or more and 2 mm or less.

[0057] According to embodiment (49), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than 0 mol% to 0.5 mol% KO.

[0058] According to embodiment (50), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0.1 mol % and less than or equal to 0.5 mol % TiO2.

[0059] According to embodiment (51), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol% and less than or equal to 4 mol% MgO.

[0060] According to embodiment (52), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises from 0.1 mol % or more to 1 mol % or less MgO.

[0061] According to embodiment (53), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 3 mol % CaO.

[0062] According to embodiment (54), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 1 mol% or more and 2 mol% or less CaO.

[0063] According to embodiment (55), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 4 mol % SrO.

[0064] According to embodiment (56), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 0.5 mol % or more and 2 mol % or less SrO.

[0065] According to embodiment (57), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 1 mol % ZnO.

[0066] According to an embodiment (58), there is provided the glass-based article of any of the embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 0.1 mol % SnO2.

[0067] According to embodiment (59), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 64 mol% or more and 65 mol% or less of SiO2.

[0068] According to embodiment (60), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 15 mol% or more and 16 mol% or less Al2O3.

[0069] According to embodiment (61), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 7 mol% or more and 8 mol% or less LiO.

[0070] According to embodiment (62), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises from 4 mol% or more and 5 mol% or less NaO.

[0071] According to embodiment (63), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0.5 mol % and less than or equal to 1.5 mol % P2O5.

[0072] According to embodiment (64), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 3 mol % or more and 4 mol % or less B2O3.

[0073] According to embodiment (65), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of Fe2O3.

[0074] According to embodiment (66), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of ZrO2.

[0075] According to embodiment (67), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of Ta2O5, HfO2, La2O3, and Y2O3.

[0076] According to embodiment (68), there is provided the glass-based article of any of embodiments (42) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article has a molar ratio of Li2O / Na2O from 1.6 or more to 2.0 or less.

[0077] According to aspect (69), there is provided a consumer electronics product comprising: a housing having a front, a back, and a side; electrical components disposed at least partially within the housing, the electrical components including at least a controller, a memory, and a display disposed at or adjacent to the front of the housing; and a cover substrate disposed over the display, at least a portion of at least one of the housing and the cover substrate being made from the glass-based article of any of aspects (42) through the immediately preceding aspect.

[0078] Additional features and advantages are set forth in the following detailed description, and in part will be readily apparent to those skilled in the art from that description, or will be learned by practicing the embodiments described herein, including the following detailed description, the claims, and the accompanying drawings.

[0079] It should be understood that both the foregoing general description and the following detailed description describe various embodiments and are intended to provide an overview or framework for understanding the nature and character of the claimed subject matter. The accompanying drawings are included to provide a further understanding of the various embodiments, and are incorporated into and constitute a part of this specification. The drawings illustrate various embodiments described herein and, together with the description, serve to explain the principles and operation of the claimed subject matter. [Brief description of the drawings]

[0080] [Figure 1] 1 is a schematic diagram of a cross section of a glass-based article having a compressive stress region according to embodiments described and disclosed herein; [Figure 2A] FIG. 1 is a plan view of an example electronic device incorporating any of the glass-based articles disclosed herein. [Figure 2B] FIG. 2B is a perspective view of the example electronic device of FIG. [Diagram 3] 1 is a plot of stress as a function of depth into a glass-based article from a surface for a glass-based article according to an embodiment; [Figure 4] 1 is a plot of CT as a function of ion exchange time for articles formed from compositions according to certain embodiments and comparative compositions. [Diagram 5] Graph of fracture stress after surface impact as a function of surface roughness for articles formed from compositions according to certain embodiments and comparative compositions. [Figure 6] 1 is a plot of break height as a function of surface roughness for articles formed from compositions according to certain embodiments and comparative compositions in an incremental flat drop test. [Figure 7] Schematic of the specimen utilized in the double cantilever beam (DCB) procedure for determining the fracture toughness KIC and its cross section. [Figure 8] 1 is a graph of percent transmittance as a function of wavelength for articles formed from compositions according to certain embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0081] Reference will now be made in detail to lithium aluminosilicate glasses, according to various embodiments. Lithium aluminosilicate glasses have good ion exchangeability, and chemical strengthening processes have been used to achieve high strength and toughness properties in lithium aluminosilicate glasses. Lithium aluminosilicate glasses are highly ion-exchanged glasses with high glass quality. Substitution of Al2O3 in the silicate glass network increases the interdiffusivity of monovalent cations during ion exchange. Chemical strengthening in a molten salt bath (e.g., KNO3 or NaNO3) can result in glasses with high strength, high toughness, and high resistance to indentation crack formation. The stress profile achieved by chemical strengthening can have a variety of shapes that improve the drop performance, strength, toughness, and other attributes of glass-based articles.

[0082] Therefore, lithium aluminosilicate glasses with good physical properties, chemical durability, and ion exchangeability have been attracting attention for use as cover glasses. Specifically, lithium-containing aluminosilicate glasses with higher fracture toughness and reasonable raw material costs are provided herein. Through different ion exchange processes, larger central tension (CT), depth of compression (DOC), and high compressive stress (CS) can be achieved. However, the addition of lithium into aluminosilicate glasses can reduce the melting point, softening point, or liquidus viscosity of the glasses.

[0083] In the embodiments of the glass compositions described herein, concentrations of components (e.g., SiO2, Al2O3, Li2O, etc.) are given in mole percent (mol%) on an oxide basis unless otherwise specified. The components of the alkali aluminosilicate glass compositions according to the embodiments are described individually below. It should be understood that any of the various recited ranges of a component may be individually combined with any of the various recited ranges of any other component. As used herein, a trailing zero in a number is intended to represent a significant digit in that number. For example, "1.0" has two significant digits, and "1.00" has three significant digits.

[0084] As used herein, "glass substrate" refers to a piece of glass that has not been ion-exchanged. Similarly, "glass article" refers to a piece of glass that has been ion-exchanged and is formed by subjecting a glass substrate to an ion-exchange process. "Glass-based substrate" and "glass-based article" are defined accordingly and include glass substrates and glass articles, as well as substrates and articles made wholly or partially from glass, such as glass substrates and glass articles with surface coatings. Glass substrates and glass articles are sometimes referred to broadly and for convenience herein, although descriptions of glass substrates and glass articles should be understood to apply equally to glass-based substrates and glass-based articles.

[0085] High fracture toughness (K ICDisclosed herein is a lithium aluminosilicate glass composition containing P2O5 and B2O3 that exhibits a K of at least 0.75 MPa√m. In some embodiments, the glass composition has a K IC The glasses described herein are characterized by their fracture toughness values. The glasses described herein can achieve these fracture toughness values ​​without additives such as ZrO2, Ta2O5, TiO2, HfO2, La2O3, and Y2O3, which increase fracture toughness but are expensive and may have limited commercial availability. In this regard, the glasses disclosed herein offer comparable or improved performance at reduced manufacturing costs.

[0086] While scratch performance is desirable, drop performance is a key attribute for glass-based articles incorporated into portable electronic devices. Fracture toughness and stress at depth are important for improving rough surface drop performance. For this reason, maximizing the amount of stress that can be provided to the glass before the frangibility limit is reached will increase stress at depth and rough surface drop performance. Fracture toughness is known to control the frangibility limit, and increasing fracture toughness increases the frangibility limit. The glass compositions disclosed herein have high fracture toughness and can achieve high compressive stress levels while remaining non-brittle. These features of the glass compositions allow for the development of improved stress profiles designed to address specific fracture modes. This capability allows ion-exchanged glass-based articles made from the glass compositions described herein to be customized with different stress profiles to address specific fracture modes of interest.

[0087] The compositions described herein are selected to achieve high fracture toughness values ​​while maintaining a desired degree of manufacturability. The compositions contain high amounts of Al2O3 and Li2O to produce the desired fracture toughness while maintaining compatibility with desired manufacturing limits. The drop performance of ion-exchanged glass-based articles formed from the glass compositions described herein is improved by increasing the depth of compression (DOC). This may be achieved at least in part by selecting a high Li / Na molar ratio. The glass compositions described herein provide improved ion-exchange performance as evidenced by increased center tensile capacity and increased ion-exchange rate, while also avoiding volatility issues at the free surface during manufacture that may be introduced with too high B2O3 and P2O5 contents.

[0088] In the glass compositions described herein, SiO2 is the majority component, and thus SiO2 is the main component of the glass network formed from the glass composition. Pure SiO2 has a relatively low CTE. However, the melting point of pure SiO2 is high. Therefore, if the concentration of SiO2 in the glass composition is too high, the formability of the glass composition will be reduced because the higher concentration of SiO2 increases the difficulty of melting the glass, which in turn adversely affects the formability of the glass. If the concentration of SiO2 in the glass composition is too low, the chemical durability of the glass may be reduced, and the glass will be susceptible to surface damage during post-molding processing. In embodiments, the glass compositions generally include SiO in an amount of from 60 mol% to 66 mol%, e.g., from 60.5 mol% to 65.5 mol%, from 61 mol% to 65 mol%, from 61.5 mol% to 64.5 mol%, from 62 mol% to 64 mol%, from 62.5 mol% to 63.5 mol%, from 63 mol% to 65 mol%, from 64 mol% to 65 mol%, and all ranges and subranges therebetween.

[0089] The glass composition includes Al2O3. Al2O3 may act as a glass network former, similar to SiO2. If the amount of Al2O3 is too high, Al2O3 may increase the viscosity of the glass composition and reduce the formability of the glass composition due to tetrahedral coordination in a glass melt formed from the glass composition. However, when the concentration of Al2O3 is balanced relative to the concentrations of SiO2 and alkali oxides in the glass composition, Al2O3 can reduce the liquidus temperature of the glass melt, thereby improving the liquidus viscosity and compatibility of the glass composition with certain forming processes. The inclusion of Al2O3 in the glass composition can provide higher fracture toughness values, as described herein. In embodiments, the glass composition includes Al2O3 in a concentration of greater than or equal to 14 mol% to less than or equal to 16 mol%, e.g., greater than or equal to 14.0 mol% to less than or equal to 16.0 mol%, greater than or equal to 14.5 mol% to less than or equal to 15.5 mol%, greater than or equal to 15.0 mol% to less than or equal to 15.5 mol%, greater than or equal to 15 mol% to less than or equal to 16 mol%, and all ranges and subranges therebetween.

[0090] The glass composition includes Li2O. The inclusion of Li2O in the glass composition allows for better control of the ion exchange process and further reduces the softening point of the glass, thereby increasing the manufacturability of the glass. The presence of Li2O in the glass composition also allows for the formation of a stress profile having a parabolic shape. The Li2O in the glass composition enables the high fracture toughness values ​​described herein. In embodiments, the glass composition includes Li2O in an amount of from 7 mol% to 9 mol%, e.g., from 7.0 mol% to 9.0 mol%, from 7.5 mol% to 8.5 mol%, from 8.0 mol% to 8.5 mol%, from 7 mol% to 8 mol%, and all ranges and subranges therebetween.

[0091] The glass compositions described herein include Na2O. Na2O aids in the ion-exchangeability of the glass composition and may also improve the formability, and thereby the manufacturability, of the glass composition. However, adding too much Na2O to the glass composition may result in too low a CTE and too high a melting point. Additionally, including too much Na2O in the glass relative to the amount of Li2O may reduce the glass's ability to achieve a large compression depth when ion-exchanged. In embodiments, the glass compositions include Na2O in an amount of 4 mol% to 6 mol%, e.g., 4.0 mol% to 6.0 mol%, 4.5 mol% to 5.5 mol%, 5.0 mol% to 5.5 mol%, 4 mol% to 5 mol%, and all ranges and subranges therebetween.

[0092] The glass compositions described herein include P2O5. The inclusion of P2O5 increases the diffusivity of ions in the glass and increases the rate of the ion exchange process. If the composition contains too much P2O5, the amount of compressive stress imparted during the ion exchange process may be reduced and volatility at the free surface during fabrication may increase to unacceptable levels. In embodiments, the glass compositions include P2O5 in an amount of from 0.5 mol% to 3 mol%, e.g., from 1.0 mol% to 3.0 mol%, from 1 mol% to 2.5 mol%, from 1.5 mol% to 2.0 mol%, from 0.5 mol% to 2 mol%, from 0.5 mol% to 1.5 mol%, and all ranges and subranges therebetween.

[0093] The glass compositions described herein include B2O3. The inclusion of B2O3 increases the fracture toughness of the glass. Specifically, the glass compositions include boron in trigonal form, which increases the Knoop scratch threshold and fracture toughness of the glass. If the composition contains too much B2O3, the amount of compressive stress imparted during the ion exchange process may decrease and volatility at the free surface during fabrication may increase to unacceptable levels. In embodiments, the glass composition includes B2O3 in an amount of from greater than or equal to 0.5 mol% to less than or equal to 6 mol%, e.g., from greater than or equal to 1.0 mol% to less than or equal to 6.0 mol%, from greater than or equal to 1 mol% to less than or equal to 5.5 mol%, from greater than or equal to 1.5 mol% to less than or equal to 5.0 mol%, from greater than or equal to 2.0 mol% to less than or equal to 5 mol%, from greater than or equal to 2 mol% to less than or equal to 4.5 mol%, from greater than or equal to 2.5 mol% to less than or equal to 4.0 mol%, from greater than or equal to 3.0 mol% to less than or equal to 4 mol%, from greater than or equal to 3 mol% to less than or equal to 3.5 mol%, from greater than or equal to 3 mol% to less than or equal to 4 mol%, and all ranges and subranges therebetween.

[0094] The glass compositions described herein generally include TiO2. If the glass composition contains too much TiO2, the glass may be prone to devitrification and / or exhibit undesirable coloration as well as undesirably alter the liquidus. The inclusion of TiO2 in the glass composition prevents undesirable discoloration of the glass when exposed to strong ultraviolet light, such as during post-fabrication processing. In embodiments, the glass compositions include an amount of TiO2 from greater than 0 mol% to less than or equal to 1 mol%, e.g., from greater than or equal to 0.1 mol% to less than or equal to 1.0 mol%, from greater than or equal to 0.2 mol% to less than or equal to 0.9 mol%, from greater than or equal to 0.3 mol% to less than or equal to 0.8 mol%, from greater than or equal to 0.4 mol% to less than or equal to 0.7 mol%, from greater than or equal to 0.5 mol% to less than or equal to 0.6 mol%, from greater than or equal to 0.1 mol% to less than or equal to 0.2 mol%, from greater than or equal to 0.1 mol% to less than or equal to 0.5 mol%, and all ranges and subranges therebetween.

[0095] The glass composition may include K2O. The inclusion of K2O in the glass composition increases potassium diffusivity in the glass, resulting in a deeper compressive stress spike depth (DOL). SP) can be achieved in shorter ion-exchange times. If the composition contains too much KO, the amount of compressive stress imparted during the ion-exchange process can be reduced. In embodiments, the glass composition contains KO in an amount from greater than 0 mol % to less than or equal to 0.5 mol %, e.g., from greater than or equal to 0.1 mol % to less than or equal to 0.4 mol %, from greater than or equal to 0.2 mol % to less than or equal to 0.3 mol %, and all ranges and subranges therebetween.

[0096] The glass compositions described herein may include MgO. MgO may reduce the viscosity of the glass, thereby improving the formability and manufacturability of the glass. The inclusion of MgO in the glass composition may also improve the strain point and Young's modulus of the glass composition. However, adding too much MgO to the glass composition may result in a liquidus viscosity that is too low for a desired forming technique. Adding too much MgO may also increase the density and CTE of the glass composition to undesirable levels. The inclusion of MgO in the glass composition may aid in achieving the high fracture toughness values ​​described herein. In embodiments, the glass composition includes MgO in an amount of from 0 mol% to 4 mol%, e.g., from greater than 0 mol% to 4.0 mol%, from 0.5 mol% to 3.5 mol%, from 1 mol% to 3 mol%, from 1.0 mol% to 3.0 mol%, from 1.5 mol% to 2.5 mol%, from 1 mol% to 2 mol%, from 2.0 mol% to 3 mol%, from 0.1 mol% to 1 mol%, and all ranges and subranges therebetween. In embodiments, the glass composition is substantially free or free of MgO. As used herein, the term "substantially free" means that the component is not intentionally added as a component of the batch materials, even if the component is present in the final glass composition in very small amounts as a contaminant, such as less than 0.1 mol%.

[0097] The glass compositions described herein may include CaO. CaO may reduce the viscosity of the glass, which may improve the formability, strain point, and Young's modulus. However, adding too much CaO to the glass composition may increase the density and CTE of the glass composition to unacceptable levels and may undesirably hinder the ion-exchangeability of the glass. The inclusion of CaO in the glass composition also aids in achieving the high fracture toughness values ​​described herein. In an embodiment, the glass composition includes an amount of CaO from 0 mol% to 3 mol%, e.g., from greater than 0 mol% to 3.0 mol%, from 0.5 mol% to 2.5 mol%, from 1 mol% to 2 mol%, from 1.0 mol% to 2.0 mol%, from 1.5 mol% to 2.0 mol%, from 1 mol% to 2 mol%, and all ranges and subranges therebetween. In an embodiment, the glass composition is substantially free or free of CaO.

[0098] The glass compositions described herein may include SrO. SrO may reduce the viscosity of the glass, which may improve formability, strain point, and Young's modulus. However, adding too much SrO to the glass composition may increase the density and CTE of the glass composition to unacceptable levels and may undesirably hinder the ion-exchangeability of the glass. The inclusion of SrO in the glass composition also aids in achieving the high fracture toughness values ​​described herein. In embodiments, the glass composition includes an amount of SrO from 0 mol% to 4 mol%, e.g., from greater than 0 mol% to 4.0 mol%, from 0.5 mol% to 3.5 mol%, from 1 mol% to 3 mol%, from 1.0 mol% to 3.0 mol%, from 1.5 mol% to 2.5 mol%, from 1 mol% to 2 mol%, from 2.0 mol% to 3 mol%, from 0.5 mol% to 2 mol%, and all ranges and subranges therebetween. In embodiments, the glass composition is substantially free or free of SrO.

[0099] The glass compositions described herein may include ZnO. ZnO may reduce the viscosity of the glass, which may improve formability, strain point, and Young's modulus. However, adding too much ZnO to the glass composition may increase the density and CTE of the glass composition to unacceptable levels. The inclusion of ZnO in the glass composition also helps achieve the high fracture toughness values ​​described herein and provides protection against UV-induced discoloration. In embodiments, the glass compositions include an amount of ZnO from 0 mol% to 1 mol%, e.g., from greater than 0 mol% to 1.0 mol%, from 0.1 mol% to 0.9 mol%, from 0.2 mol% to 0.8 mol%, from 0.3 mol% to 0.7 mol%, from 0.4 mol% to 0.6 mol%, from 0.1 mol% to 0.5 mol%, from 0 mol% to 0.3 mol%, and all ranges and subranges therebetween. In embodiments, the glass composition is substantially free or free of ZnO.

[0100] The glass composition may optionally include one or more fining agents. In embodiments, an example of a fining agent may include SnO2. In embodiments, SnO2 may be present in the glass composition in an amount of 0.2 mol% or less, such as from 0 mol% to 0.2 mol%, from 0 mol% to 0.1 mol%, from 0 mol% to 0.05 mol%, from 0.1 mol% to 0.2 mol%, and all ranges and subranges therebetween. In some embodiments, the glass composition may be substantially free or free of SnO2. In embodiments, the glass composition may be substantially free of one or both of arsenic and antimony. In other embodiments, the glass composition may be free of one or both of arsenic and antimony.

[0101] The glass compositions described herein may be formed primarily from SiO2, Al2O3, Li2O, Na2O, P2O5, and B2O3. In embodiments, the glass compositions are substantially free or free of components other than SiO2, Al2O3, Li2O, Na2O, P2O5, B2O3, and TiO2. In embodiments, the glass compositions are substantially free or free of components other than SiO2, Al2O3, Li2O, Na2O, P2O5, B2O3, TiO2, and fining agents. In embodiments, the glass compositions are substantially free or free of components other than SiO2, Al2O3, Li2O, Na2O, P2O5, B2O3, TiO2, K2O, CaO, MgO, SrO, and fining agents.

[0102] In embodiments, the glass compositions may be substantially free or free of Fe2O3. Iron is often present in the raw materials utilized to form the glass compositions, and as a result, may be detectable in the glass compositions described herein even when not actively added to the glass batch.

[0103] In embodiments, the glass compositions may be substantially free or free of ZrO2. The inclusion of ZrO2 in the glass composition may result in the formation of undesirable zirconia inclusions in the glass, due at least in part to the low solubility of ZrO2 in the glass. The inclusion of ZrO2 in the glass may increase fracture toughness, but there are cost and supply constraints, as well as the devitrification issues described above, that may make the use of these ingredients undesirable for commercial purposes. Stated another way, the ability of the glass compositions described herein to achieve high fracture toughness values ​​by including ZrO2 provides cost and manufacturability advantages.

[0104] In embodiments, the glass composition may be substantially free of, or free of, at least one of Ta2O5, HfO2, La2O3, and Y2O3. In embodiments, the glass composition may be substantially free of, or free of, Ta2O5, HfO2, La2O3, and Y2O3. These components, when included, may increase the fracture toughness of the glass, but there are cost and supply constraints that make these components undesirable for commercial purposes. Stated another way, the ability of the glass compositions described herein to achieve high fracture toughness values ​​by including Ta2O5, HfO2, La2O3, and Y2O3 provides cost and manufacturability advantages.

[0105] The glass compositions described herein may be described in terms of a lithium to sodium molar ratio (Li2O / Na2O). A high Li2O / Na2O molar ratio can achieve a high depth of compaction (DOC) when the glass composition is ion-exchanged. The increased DOC capacity attributable to a high Li2O / Na2O molar ratio can allow ion-exchanged articles formed from the glass composition to exhibit improved drop performance, particularly on rough surfaces. In embodiments, the glass compositions are characterized by a Li2O / Na2O molar ratio of 1.2 or more to 2.0 or less, e.g., 1.3 or more to 1.9 or less, 1.4 or more to 1.8 or less, 1.5 or more to 1.7 or less, 1.6 or more to 2.0 or less, and all ranges and subranges therebetween.

[0106] The physical properties of the glass compositions disclosed above are now described.

[0107] Glass compositions according to embodiments have high fracture toughness. Without intending to be bound by any particular theory, high fracture toughness may provide glass compositions with improved drop performance. The high fracture toughness of the glass compositions described herein increases the damage resistance of the glass and allows the glass to be highly stressed by ion exchange without becoming brittle, as characterized by central tension. As used herein, fracture toughness is defined as the K value, as measured by the Chevron Notched Small Square Bar Method, unless otherwise specified.IC The value is called K IC The chevron notched small square bar (CNSB) method used to measure the Y * m is disclosed in Reddy, KPR et al., "Fracture Toughness Measurement of Glass and Ceramic Materials Using Chevron-Notched Specimens," J. Am. Ceram. Soc., 71 [6], C-310-C-313 (1988), except that it is calculated using Equation 5 in Bubsey, RT et al., "Closed-Form Expressions for Crack-Mouth Displacement and Stress Intensity Factors for Chevron-Notched Short Bar and Short Rod Specimens Based on Experimental Compliance Measurements," NASA Technical Memorandum 83796, pp. 1-30 (October 1992). IC The value is the K before the glass-based substrate is ion-exchanged to form the glass-based article. IC The K values ​​mentioned here are measured on unstrengthened glass samples. IC Values ​​are reported in MPa√m unless otherwise noted.

[0108] In an embodiment, the glass composition has a K of 0.75 MPa√m or more, e.g., 0.76 MPa√m or more, 0.77 MPa√m or more, 0.8 MPa√m or more, or more. IC In an embodiment, the glass composition has a K value of from 0.75 MPa√m or more to 0.8 MPa√m or less, e.g., from 0.76 MPa√m or more to 0.79 MPa√m or less, e.g., from 0.77 MPa√m or more to 0.78 MPa√m or less, and all ranges and subranges therebetween. IC Indicates the value.

[0109] The glass compositions described herein have liquidus viscosities compatible with manufacturing processes that are particularly suited for forming thin glass sheets. For example, the glass compositions are compatible with down-draw processes, such as fusion draw and slot draw. Glass-based substrate embodiments may be described as fusion formable (i.e., formable using a fusion draw process). The fusion process employs a drawing vessel having a passageway for receiving molten raw glass material. The passageway has a weir on either side of the passageway that is open at the top along the length of the passageway. When the passageway is filled with molten material, the molten glass overflows the weir. The molten glass flows down the exterior surfaces of the drawing vessel as two flowing glass films due to gravity. These exterior surfaces of the drawing vessel extend downward and inward to meet at the lower edge of the drawing vessel. The two flowing glass films meet at this edge and fuse to form a flowing glass-based article. The fusion of these glass films creates a fusion line in the glass-based substrate that can identify a fusion-formed glass-based substrate without the need for additional knowledge of its manufacturing history. The fusion draw process offers the advantage that, as the two glass films overflowing the passageway fuse together, none of the exterior surfaces of the resulting glass-based article come into contact with any part of the equipment. Thus, the surface properties of the glass-based article produced by the fusion draw process are not affected by such contact.

[0110] The glass compositions described herein may be selected to have a liquidus viscosity that is compatible with the fusion draw process. Thus, the glass compositions described herein are compatible with existing forming processes, increasing the manufacturability of glass-based articles formed from the glass compositions. As used herein, the term "liquidus viscosity" refers to the viscosity of molten glass at its liquidus temperature, where the liquidus temperature refers to the temperature at which crystals first appear as the molten glass cools from the melting temperature, or the temperature at which the last crystals melt away as the temperature is increased from room temperature. Unless otherwise specified, the liquidus viscosity values ​​disclosed in this application are determined by the following method. First, the liquidus temperature of the glass is measured according to ASTM C829-81 (2015), entitled "Standard Practice for Measurement of Liquidus Temperature of Glass by the Gradient Furnace Method". The viscosity of the glass at its liquidus temperature is then measured according to ASTM C965-96 (2012), entitled "Standard Practice for Measuring Viscosity of Glass Above the Softening Point." As used herein, the term "Vogel-Fulcher-Tamman ("VFT") relationship" describes the temperature dependence of viscosity and is given by the following equation:

[0111]

number

[0112] where η is the viscosity. VFT A, VFT B, and VFT T O The viscosity of the glass composition is measured over a range of temperatures to determine A, B, and T. The raw viscosity vs. temperature data is then fitted by a least squares method with the VFT equation to obtain A, B, and T. OThese values ​​allow the calculation of the viscosity point at any temperature above the softening point (e.g., 200P, 35000P, and 200000P temperatures). Unless otherwise specified, the liquidus viscosity and temperature of a glass composition or article are measured before the composition or article is subjected to any ion exchange process or any other strengthening process. In particular, the liquidus viscosity and temperature of a glass composition or article are measured before the composition or article is exposed to, e.g., immersed in, an ion exchange solution.

[0113] In embodiments, the liquidus viscosity of the glass composition can be 50 kP or more, e.g., 55 kP or more, 60 kP or more, 65 kP or more, 70 kP or more, 75 kP or more, or more. In embodiments, the liquidus viscosity of the glass composition can be 50 kP or more to 80 kP or less, e.g., 55 kP or more to 75 kP or less, 60 kP or more to 70 kP or less, 50 kP or more to 65 kP or less, 50 kP or more to 75 kP or less, and all ranges and subranges therebetween. A lower liquidus viscosity corresponds to a higher K IC However, if the liquidus viscosity is too low, the manufacturability of the glass composition is reduced.

[0114] The glass composition may be described in terms of the components contained therein and the properties the glass exhibits. In an embodiment, the glass comprises SiO2, Al2O3, Li2O, Na2O, P2O5, and B2O3, has a Li2O / Na2O molar ratio of ≧1.2 to ≦2.0, has a liquidus viscosity in the range of ≧50 kP to ≦75 kP, and has a fracture toughness K of ≧0.75 MPa√m. IC has.

[0115] In one or more embodiments, the glass compositions described herein may form glass-based articles that exhibit an amorphous microstructure and may be substantially free of crystals or crystallites. In other words, glass-based articles formed from the glass compositions described herein may exclude glass-ceramic materials.

[0116] As mentioned above, in embodiments, the glass compositions described herein can be strengthened, such as by ion exchange, to produce glass-based articles that are damage resistant for applications such as, but not limited to, display covers. Referring to FIG. 1, a glass-based article is shown having a first region under compressive stress (e.g., first and second compressive stress layers 120, 122 in FIG. 1) extending from the surface of the glass-based article to a depth of compression (DOC) and a second region under tensile stress or central tension (CT) (e.g., central region 130 in FIG. 1) extending from the DOC to a central or interior region of the glass-based article. As used herein, DOC refers to the depth at which stress within a glass-based article changes from compression to tension. At the DOC, the stress crosses from positive (compressive) stress to negative (tensile) stress, and therefore exhibits a stress value of zero.

[0117] According to common conventions in the art, compression or compressive stress is expressed as a negative (<0) stress, and tension or tensile stress is expressed as a positive (>0) stress. However, throughout this specification, CS is expressed as a positive or absolute value. That is, as set forth herein, CS=|CS|. Compressive stress (CS) has a maximum value at or near the surface of the glass-based article, and CS varies with distance d from the surface according to a function. Referring again to FIG. 1, the first section 120 extends from the first surface 110 to a depth d1, and the second section 122 extends from the second surface 112 to a depth d2. These sections together define the compression or CS of the glass-based article 100. Compressive stress (including surface CS) is measured by a surface stress meter (FSM) using commercially available equipment such as the FSM-6000 manufactured by Orihara Seisakusho Co., Ltd. (Japan). Surface stress measurements rely on precise measurement of the stress optical coefficient (SOC), which is related to the birefringence of the glass. The SOC is then measured according to Procedure C (Glass Disk Method) described in ASTM Standard C770-16, entitled "Standard Test Method for Measurement of Glass Stress-Optical Coefficient," the contents of which are incorporated herein in their entirety.

[0118] In an embodiment, the CS of the glass-based article is from 500 MPa to 1500 MPa, e.g., from 550 MPa to 1500 MPa, from 600 MPa to 1500 MPa, from 650 MPa to 1450 MPa, from 700 MPa to 1400 MPa, from 750 MPa to 1350 MPa, from 800 MPa to 1300 MPa, from 850 MPa to 1250 MPa, from 900 MPa to 1200 MPa, from 950 MPa to 1150 MPa, from 1000 MPa to 1150 MPa, from 1050 MPa to 1500 MPa, from 1200 MPa to 1300 MPa, and all ranges and sub-ranges therebetween.

[0119] In one embodiment, Na + and K. + ions are exchanged into the glass-based article, + The ion is K + ions diffuse into glass-based articles to greater depths than K + The depth of penetration of ions ("potassium DOL") is distinct from the DOC because it represents the depth of potassium penetration as a result of the ion exchange process. The potassium DOL is typically smaller than the DOC for the glass articles described herein. The potassium DOL is measured using a surface stress meter, such as the commercially available FSM-6000 surface stress meter manufactured by Orihara Seisakusho Co., Ltd. (Japan). This surface stress meter relies on precise measurements of the stress optical coefficient (SOC), as described above with respect to CS measurements. The potassium DOL is determined by the depth of the compressive stress spike (DOL SP ), where the stress profile transitions from a steep spike region to a less steep deep region. The deep region extends from the base of the spike region to the compression depth. SP can be from 3 μm to 10 μm, for example, from 4 μm to 9 μm, from 5 μm to 8 μm, from 6 μm to 7 μm, and all ranges and subranges therebetween.

[0120] The compressive stresses on both major surfaces (110, 112 in FIG. 1) are balanced by a stored tension in the central region (130) of the glass-based article. The maximum central tension (CT) and DOC may be measured using a scattered light polariscope (SCALP) as known in the art. The refractive near-field (RNF) method or SCALP may be used to determine the stress profile of the glass-based article. When the RNF method is used to measure the stress profile, the maximum CT value given by SCALP is used in the RNF method. Specifically, the stress profile determined by RNF is force balanced and calibrated against the maximum CT value given by the SCALP measurement. This RNF method is described in U.S. Pat. No. 8,854,623, entitled "Systems and methods for measuring a profile characteristic of a glass sample," which is incorporated herein by reference in its entirety. Specifically, the RNF method includes placing a glass-based article adjacent to a reference block, generating a polarization-switched light beam that is switched between orthogonal polarizations at a rate between 1 Hz and 50 Hz, measuring the amount of power of the polarization-switched light beam, and generating a polarization-switched reference signal, where the measured amounts of power of each of the orthogonal polarizations are within 50% of each other. The method further includes transmitting the polarization-switched light beam through the glass sample and the reference block for different depths in the glass sample, and then relaying the transmitted polarization-switched light beam using relay optics to a signal photodetector, which generates a polarization-switched detector signal. The method also includes dividing the detector signal by the reference signal to form a normalized detector signal, and determining a profile indicative of the glass sample from the normalized detector signal.

[0121] The measurement of maximum CT value is an indication of the total amount of stress stored in the strengthened article due to the force balance described above. For this reason, the ability to achieve higher CT values ​​correlates to the ability to achieve higher strengthening and improved performance. In embodiments, the glass-based article may have a maximum CT of 60 MPa or more, e.g., 70 MPa or more, 80 MPa or more, 90 MPa or more, 100 MPa or more, 110 MPa or more, 120 MPa or more, 130 MPa or more, 140 MPa or more, 150 MPa or more, or more. In embodiments, the glass-based article may have a maximum CT of 60 MPa or more to 160 MPa or less, e.g., 70 MPa or more to 160 MPa or less, 80 MPa or more to 160 MPa or less, 90 MPa or more to 160 MPa or less, 100 MPa or more to 150 MPa or less, 110 MPa or more to 140 MPa or less, 120 MPa or more to 130 MPa or less, and all ranges and subranges therebetween.

[0122] The high fracture toughness values ​​of the glass compositions described herein may also allow for improved performance. The brittleness limit of glass-based articles manufactured utilizing the glass compositions described herein depends at least in part on the fracture toughness. For this reason, the high fracture toughness of the glass compositions described herein allows the glass-based articles formed therefrom to have a large amount of stored strain energy without becoming brittle. The increased amount of stored strain energy that may be included in the glass-based article may then allow the glass-based article to exhibit increased fracture resistance, which may be observed through the drop performance of the glass-based article. The relationship between brittleness limit and fracture toughness is described in U.S. Patent Application Publication No. 2020 / 0079689A1, entitled "Glass-based Articles with Improved Fracture Resistance," published March 12, 2020, which is incorporated herein by reference in its entirety. The relationship between fracture toughness and drop performance is described in U.S. Patent Application Publication No. 2019 / 0369672 A1, entitled "Glass with Improved Drop Performance," published on December 5, 2019, which is incorporated herein by reference in its entirety.

[0123] As mentioned above, the DOC is measured using a scattered light polarimeter (SCALP) as known in the art. The DOC is given herein as a fraction of the thickness (t) of the glass-based article in some embodiments. In embodiments, the glass-based article may have a depth of compression (DOC) of 0.20t or more to 0.25t or less, such as 0.21t or more to 0.24t or more, or 0.22t or more to 0.23t or less, and all ranges and subranges therebetween. The high DOC values ​​that result when the glass compositions described herein are ion-exchanged provide improved fracture resistance, especially for situations where deep scratches may be introduced. For example, a deep DOC improves fracture resistance when dropped onto a rough surface.

[0124] The thickness (t) of the glass-based article 100 is measured between the surface 110 and the surface 112. In embodiments, the thickness of the glass-based article 100 can be in the range of 0.1 mm to 4 mm, e.g., 0.2 mm to 3.5 mm, 0.3 mm to 3 mm, 0.4 mm to 2.5 mm, 0.5 mm to 2 mm, 0.6 mm to 1.5 mm, 0.7 mm to 1 mm, 0.2 mm to 2 mm, and all ranges and subranges therebetween. The glass substrate utilized to form the glass-based article can have a thickness similar to that desired for the glass-based article.

[0125] The compressive stress layer may be formed in the glass by exposing the glass to an ion-exchange medium. In embodiments, the ion-exchange medium may be a molten nitrate salt. In embodiments, the ion-exchange medium may be a molten salt bath and may include KNO3, NaNO3, or combinations thereof. In embodiments, other sodium and potassium salts may be used in the ion-exchange medium, such as, for example, sodium or potassium nitrates, phosphates, or sulfates. In embodiments, the ion-exchange medium may include a lithium salt, such as LiNO3. The ion-exchange medium may additionally include additives commonly included when ion-exchanging glasses, such as silicic acid. The ion-exchange process is performed on the glass-based substrate to form a glass-based article that includes a compressive stress layer and a central tension region that extend from the surface to the compression depth of the glass-based article. The glass-based substrate utilized in the ion-exchange process may include any of the glass compositions described herein.

[0126] In an embodiment, the ion exchange medium includes NaNO3. The sodium in the ion exchange medium exchanges with lithium ions in the glass to create a compressive stress. In an embodiment, the ion exchange medium may include 95% or less by weight NaNO3, e.g., 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or less. In an embodiment, the ion exchange medium may include 5% or more by weight NaNO3, e.g., 10% or more, 20% or more, 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or more. In embodiments, the ion exchange medium may comprise NaNO3 in an amount of from 0 to 100% by weight, such as from 10 to 90% by weight, from 20 to 80% by weight, from 30 to 70% by weight, from 40 to 60% by weight, from 50 to 90% by weight, and all ranges and subranges therebetween. In embodiments, the molten ion exchange medium comprises 100% NaNO3 by weight.

[0127] In embodiments, the ion exchange medium comprises KNO3. In embodiments, the ion exchange medium may comprise 95% by weight or less, e.g., 90% by weight or less, 80% by weight or less, 70% by weight or less, 60% by weight or less, 50% by weight or less, 40% by weight or less, 30% by weight or less, 20% by weight or less, 10% by weight or less, or less than that. In embodiments, the ion exchange medium may comprise 5% by weight or more, e.g., 10% by weight or more, 20% by weight or more, 30% by weight or more, 40% by weight or more, 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, or more than that. In embodiments, the ion exchange medium may comprise from 0% to 100% by weight KNO3, for example, from 10% to 90% by weight, from 20% to 80% by weight, from 30% to 70% by weight, from 40% to 60% by weight, from 50% to 90% by weight, and all ranges and subranges therebetween. In embodiments, the molten ion exchange medium comprises 100% KNO3.

[0128] The ion exchange medium may include a mixture of sodium and potassium. In embodiments, the ion exchange medium is a mixture of potassium and sodium, such as a molten salt bath containing both NaNO3 and KNO3. In embodiments, the ion exchange medium may include any combination of NaNO3 and KNO3 in the amounts described above, such as a molten salt bath containing 80% NaNO3 and 20% KNO3 by weight.

[0129] The glass composition may be exposed to an ion exchange medium by immersing a glass substrate made from the glass composition in a bath of the ion exchange medium, spraying the ion exchange medium onto a glass substrate made from the glass composition, or otherwise physically applying the ion exchange medium to a glass substrate made from the glass composition to form an ion exchanged glass-based article. The ion exchange medium may be at a temperature of from 360° C. to 500° C. during exposure to the glass composition, according to embodiments, such as from 370° C. to 490° C., from 380° C. to 480° C., from 390° C. to 470° C., from 400° C. to 460° C., from 410° C. to 450° C., from 420° C. to 440° C., from 430° C. to 470° C., from 400° C. to 470° C., from 380° C. to 470° C., and all ranges and subranges therebetween. In embodiments, the glass composition may be exposed to the ion exchange solution for a period of from 10 minutes to 48 hours, e.g., from 10 minutes to 24 hours, from 0.5 hours to 24 hours, from 1 hour to 18 hours, from 2 hours to 12 hours, from 4 hours to 8 hours, and all ranges and subranges therebetween.

[0130] The ion exchange process may include a second ion exchange process. In embodiments, the second ion exchange process may include ion exchanging the glass-based article in a second molten salt bath. The second ion exchange process may utilize any of the ion exchange media described herein. In embodiments, the second ion exchange process utilizes a second molten salt bath including KNO3.

[0131] The ion exchange process may be carried out in an ion exchange medium under processing conditions that provide an improved compressive stress profile, such as those disclosed in U.S. Patent Application Publication No. 2016 / 0102011, which is incorporated herein by reference in its entirety. In some embodiments, the ion exchange process may be selected to produce a parabolic stress profile in the glass-based article, such as the stress profile described in U.S. Patent Application Publication No. 2016 / 0102014, which is incorporated herein by reference in its entirety.

[0132] It should be understood that after the ion-exchange process has been performed, the composition at the surface of the ion-exchanged glass-based article will differ from the composition of the as-formed glass substrate (i.e., the glass substrate before the ion-exchange process has been performed). + or K + Replaced by larger alkali metal ions such as Li + or Na + Such glass compositions may result from one type of alkali metal ion in the as-formed glass substrate, such as ion-exchanged glass, ion-exchanged glass, etc. However, the glass composition at or near the center of the depth of the glass-based article will, in embodiments, still have the composition of the as-formed, non-ion-exchanged glass substrate utilized to form the glass-based article. As used herein, the center of a glass-based article refers to any location in the glass-based article that is at least 0.5t away from all of its surfaces, where t is the thickness of the glass-based article.

[0133] The glass-based articles disclosed herein may be incorporated into another article, such as an article with a display (or display article) (e.g., consumer electronics including cell phones, tablets, computers, navigation systems, etc.), a building article, a transportation article (e.g., automobiles, trains, aircraft, ships, etc.), an appliance, or any article requiring some degree of transparency, scratch resistance, abrasion resistance, or a combination thereof. An exemplary article incorporating any of the glass-based articles disclosed herein is shown in Figures 2A and 2B. In particular, Figures 2A and 2B show a consumer electronics device 200 comprising a housing 202 having a front surface 204, a back surface 206, and a side surface 208; at least partially inside or completely within the housing, electrical components (not shown) including at least a controller, memory, and a display 210 at or adjacent to the front surface of the housing; and a cover 212 at or on the front surface of the housing to cover the display. In an embodiment, at least a portion of at least one of the cover 212 and the housing 202 may include any of the glass-based articles described herein. EXAMPLES

[0134] The embodiments will be further clarified by the following examples, which should be understood as not limiting the embodiments described above.

[0135] Glass compositions were prepared and analyzed. The analyzed glass compositions contained the components listed in Table I below and were prepared by conventional glass forming methods. In Table I, all components are expressed in mole percent and are K. ICThe fracture toughness was primarily measured by the Chevron Notch (CNSB) method described herein. The Poisson's ratio (ν), Young's modulus (E), and shear modulus (G) of the glass compositions were measured by the general type of resonant ultrasonic spectroscopy technique described in ASTM E2001-13, entitled "Standard Guide for Resonant Ultrasound Spectroscopy for Defect Detection in Both Metallic and Non-metallic Parts". The refractive index and stress optical coefficient (SOC) at 589.3 nm of the substrates are also reported in Table I. The density of the glass compositions was determined using the buoyancy method of ASTM C693-93 (2013).

[0136] Alternative fracture toughness K ICMeasurements of were performed on several specimens by the double cantilever beam (DCB) technique and are also reported in Table I. The geometry of the DCB specimens is shown in Figure 7, with the important parameters being the crack length a, the applied load P, the cross-sectional dimensions w and 2h, and the thickness b of the crack induction groove. The specimens were cut into rectangles with width 2h = 1.25 cm and thickness ranging from w = 0.3 mm to 1 mm, and the total length of the specimens varied from 5 cm to 10 cm, but this is not a critical dimension. Holes were drilled at both ends with a diamond drill to provide a means of attaching the specimen to a specimen holder and load. The crack "induction groove" was cut the length of the specimen on both flat sides using a wafer dicing saw equipped with a diamond blade, leaving a "web" of material approximately half the total thickness of the plate (dimension b in Figure 7) with a height of 180 μm, corresponding to the thickness of the blade. The high precision dimensional tolerances of the dicing saw allow for minimal variation between specimens. This dicing saw was also used to cut the initial crack with a = 15 mm. This final operation resulted in the formation of a very thin wedge of material near the crack tip (due to the curvature of the blade), making it easier for crack initiation within the sample. The sample was mounted in a metal sample holder with a steel wire in the hole at the bottom of the sample. The sample was supported at the opposite end to keep it horizontal under low load conditions. The top hole was hooked to a spring in series with a load cell (FUTEK, LSB200), which was then stretched and gradually loaded using a rope and precision slide. The crack was monitored using a microscope with a resolution of 5 μm attached to a digital camera and computer. The following equation:

[0137]

number

[0138] Using the applied stress intensity K PFor each specimen, a crack was first initiated at the leading edge of the web, and then the initiating crack was carefully grown subcritically until the dimension ratio a / h was greater than 1.5 in order to accurately calculate the stress intensity. At this point, the length of the crack, a, was measured and recorded using a moving microscope with a resolution of 5 μm. A drop of toluene was then placed in the crack groove and carried along the entire length of the groove by capillary forces, pinning the crack against movement until the fracture toughness was reached. The load was then increased until the specimen broke, and the critical stress intensity, K, was calculated from the fracture load and specimen dimensions. IC We calculated K P is the measurement method, K IC is equal to.

[0139] As used herein, the term "anneal point" refers to the point at which the viscosity of a glass composition is reduced to 1×10 13.18 As used herein, the term "strain point" refers to the temperature at which the viscosity of a glass composition is 1×10 14.68 The strain point and anneal point of the glass compositions were determined using the fiber elongation method of ASTM C336-71(2015) or the beam bending viscosity (BBV) method of ASTM C598-93(2013).

[0140] As used herein, the term "softening point" refers to the point at which the viscosity of a glass composition is reduced to 1×10 7.6 The softening point of a glass composition is measured using the fiber elongation method of ASTM C336-71(2015) or similar to ASTM C1351M, as a function of temperature, at a rate of 10 7 From 10 9 The poise was determined using the parallel plate viscosity (PPV) method, which measures the viscosity of inorganic glasses.

[0141] The coefficient of linear thermal expansion (CTE) over the temperature range of 0-300° C. is expressed in ppm / ° C. and was determined using a push rod dilatometer according to ASTM E228-11.

[0142] [Table 1-01a]

[0143]

Table 1-01b

[0144]

Table 1-02a

[0145]

Table 1-02b

[0146]

Table 1-03a

[0147]

Table 1-03b

[0148]

Table 1-04a

[0149]

Table 1-04b

[0150]

Table 1-05a

[0151]

Table 1-05b

[0152]

Table 1-06a

[0153]

Table 1-06b

[0154]

Table 1-07a

[0155]

Table 1-07b

[0156]

Table 1-08a

[0157]

Table 1-08b

[0158]

Table 1-09a

[0159]

Table 1-09b

[0160]

Table 1-10a

[0161]

Table 1-10b

[0162]

Table 1-11a

[0163] [Table 1-11b]

[0164] [Table 1-12a]

[0165] [Table 1-12b]

[0166] [Table 1-13a]

[0167] [Table 1-13b]

[0168] [Table 1-14a]

[0169] [Table 1-14b]

[0170] Substrates having a thickness of 0.5 mm were formed from the compositions in Table I and subsequently ion-exchanged to form the exemplary articles. The ion-exchange involved immersing the substrate in a molten salt bath. The salt bath contained 100% by weight NaNO3 and had a temperature of 420°C. In Table II, the length of the ion-exchange, the mass gain resulting from the ion-exchange process, and the maximum central tension (CT) of the ion-exchanged articles are reported. The maximum central tension (CT) was measured according to the method described herein.

[0171] [Table 2-01]

[0172]

Table 2-02

[0173]

Table 2-03

[0174]

Table 2-04

[0175]

Table 2-05

[0176]

Table 2-06

[0177]

Table 2-07

[0178]

Table 2-08

[0179]

Table 2-09

[0180]

Table 2-10

[0181]

Table 2-11

[0182] [Table 2-12]

[0183] Substrates were formed from composition 31 and comparative composition C1 of Table I. Comparative composition C1 analyzed contained 63.31 mol% SiO2, 15.2 mol% Al2O3, 6.74 mol% B2O3, 4.30 mol% Na2O, 6.82 mol% Li2O, 1.00 mol% MgO, 1.55 mol% CaO, 1.02 mol% SrO, and 0.05 mol% SnO2. Articles DD, DE, and DF of Table III were formed from comparative composition D1 and are comparative examples for this reason. The substrates were subjected to a two-step ion-exchange process of immersion in a first molten salt bath and immersion in a second molten salt bath. All molten salt baths were at a temperature of 420°C, and the composition and ion-exchange time for each bath are reported in Table III. The thickness of the substrates, the refractive index at 589.3 nm, and the stress optical coefficient (SOC) are also reported in Table III. The central tension of the article was measured after ion-exchanging in the first ion-exchange bath (CT1) and after completing the ion-exchange treatment in the second ion-exchange bath (CT2). In addition, the compressive stress and spike depth (DOL) of the article were measured. sp ) was measured after completion of the ion exchange treatment with the second ion exchange bath.

[0184] [Table 3]

[0185] The stress profile of Item DB in Table III was measured by RNF, as shown in Figure 3. Item DB had a depth of compression (DOC) of 111 μm, which is about 22% of the thickness.

[0186] Substrates were formed from composition 31 and comparative composition C1 of Table I. All of the substrates had the same thickness of 0.5 mm. The substrates were subjected to ion exchange in a molten salt bath having a composition of 100 wt. % NaNO3 at a temperature of 420°C for a time ranging from 2.5 to 5 hours. The CT of the articles produced by this ion exchange process was measured. The CT is plotted as a function of ion exchange time in Figure 4. The substrate formed from composition 31 (triangles) achieved a higher CT than the substrate formed from comparative composition C1 (circles), as shown in Figure 4.

[0187] The article DB was subjected to a surface impact test with the impact surface having various grit levels. The fracture stress was measured using a four-point bending test after the surface impact. A comparative article was formed by ion-exchanging a 0.5 mm thick substrate formed from comparative composition C2 in a first molten salt bath having a composition of 40% NaNO3 and 60% KNO3 by weight at a temperature of 430°C for a time of 1 hour 25 minutes, followed by ion-exchanging in a second molten salt bath having a composition of 1% NaNO3 and 99% KNO3 by weight at a temperature of 380°C for a time of 25 minutes. The comparative composition C2 analyzed contained 59.09 mol% SiO2, 17.94 mol% Al2O3, 4.08 mol% B2O3, 8.79 mol% Na2O, 8.00 mol% Li2O, 0.07 mol% K2O, 1.23 mol% MgO, 0.01 mol% ZnO, 0.02 mol% CaO, 0.66 mol% P2O5, and 0.04 mol% SnO2. The comparative article formed from the comparative composition C2 exhibited higher CT values ​​and lower DOC when compared to the article DB. The comparative article formed from the comparative composition C2 was subjected to the same surface impact test and four-point bend test as the article DB. The results of the surface impact test and four-point bend test are shown in FIG. 5. The article DB showed improved performance at deeper scratch depths, at least in part due to the deeper DOC.

[0188] Articles formed from Article DB and Comparative Composition C2 were also subjected to incremental flat surface drop tests on rough surfaces. The test articles were attached to a pack simulating a portable electronic device and dropped at progressively increasing heights onto surfaces having either 80 grit or 180 grit roughness. Eighteen samples were tested for each surface roughness. For 180 grit, both Article DB and the articles formed from Comparative Composition C2 survived the largest drop height with a large number of samples. The Article DB samples had an average break height 8% greater than the C2 samples. For 80 grit, the Article DB samples had an average break height 39% greater than the C2 samples. The improved performance of the Article DB samples may be due to the increased DOC when compared to the C2 samples, especially for the rough surfaces. The drop test results are shown in FIG. 6.

[0189] A substrate was formed from composition 66 of Table I and then ion-exchanged to form the exemplary article. The ion-exchange included immersing the substrate in a molten salt bath. The transmittance of the ion-exchanged exemplary article was measured at a depth of 0.7 mm. The percent transmittance is shown as a function of wavelength in FIG. 8. The ion-exchanged exemplary article exhibited a transmittance of 90.5% or greater over the wavelength range of 380 nm to 2000 nm. The refractive index of the compressive stress layer of the ion-exchanged exemplary article was also measured at 590 nm and found to be 1.52. The photoelastic constant of the ion-exchanged exemplary article was measured to be 30.8 nm / cm / MPa. The Vickers hardness was measured at a load of 200 g for the exemplary substrate (before ion-exchange) and the ion-exchanged exemplary article (after ion-exchange), and was found to be 595 kgf / mm, respectively. 2 and 670kgf / mm 2 The values ​​of 0.01 to 0.05 were obtained. The ion-exchanged exemplary articles were tested for chemical durability by immersion in a solvent at a given temperature for a given time. The resulting mass loss per surface area was measured as shown in Table IV.

[0190] [Table 4]

[0191] The dielectric constant and loss tangent of the ion-exchanged exemplary articles formed from Composition 66 were also measured at various frequencies, as reported in Table V.

[0192] [Table 5]

[0193] All compositional components, relationships, and ratios described herein are given in mole percent unless otherwise specified. All ranges disclosed herein include any and all ranges and subranges encompassed by the broadly disclosed range, whether or not a range is expressly set forth before or after the disclosure.

[0194] It will be apparent to those skilled in the art that various modifications and variations can be made to the embodiments disclosed herein without departing from the spirit and scope of the claimed subject matter. Therefore, it is intended that this specification cover modifications and variations of the various embodiments described herein, provided such modifications and variations come within the scope of the appended claims and their equivalents.

[0195] Preferred embodiments of the present invention will be described below in detail.

[0196] EMBODIMENT 1 In glass, 60 mol% or more and 66 mol% or less of SiO2; 14 mol% or more and 16 mol% or less of Al2O3; 7 mol% or more and 9 mol% or less of Li2O; 4 mol% or more and 6 mol% or less of Na2O, 0.5 mol% or more and 3 mol% or less of P2O5, 0.5 mol% to 6 mol% B2O3, and greater than 0 mol% to 1 mol% or less of TiO2; Including glass.

[0197] EMBODIMENT 2 from greater than 0 mol % to 0.5 mol % or less of K2O; 2. The glass of embodiment 1, comprising:

[0198] EMBODIMENT 3 0.1 mol % or more and 0.5 mol % or less of TiO2; 3. The glass of embodiment 1 or 2, comprising:

[0199] EMBODIMENT 4 0 mol % or more and 4 mol % or less of MgO; The glass of any one of claims 1 to 3, comprising:

[0200] EMBODIMENT 5 0.1 mol % or more and 1 mol % or less of MgO; 5. The glass of any one of the preceding claims, comprising:

[0201] EMBODIMENT 6 0 mol% or more and 3 mol% or less of CaO; 6. The glass of any one of the preceding claims, comprising:

[0202] EMBODIMENT 7 1 mol% or more and 2 mol% or less of CaO; 7. The glass of any one of the preceding claims, comprising:

[0203] EMBODIMENT 8 0 mol % or more and 4 mol % or less of SrO; The glass of any one of the preceding claims, comprising:

[0204] EMBODIMENT 9 0.5 mol % or more and 2 mol % or less of SrO; 9. The glass of any one of the preceding claims, comprising:

[0205] EMBODIMENT 10 ZnO, from 0 mol% to 1 mol% 10. The glass of any one of the preceding claims, comprising:

[0206] EMBODIMENT 11 0 mol% to 0.1 mol% SnO2, 11. The glass of any one of the preceding claims, comprising:

[0207] EMBODIMENT 12 64 mol% or more and 65 mol% or less of SiO2; 12. The glass of any one of the preceding claims, comprising:

[0208] EMBODIMENT 13 15 mol% or more and 16 mol% or less of Al2O3; 13. The glass of any one of the preceding claims, comprising:

[0209] EMBODIMENT 14 7 mol% or more and 8 mol% or less of Li2O; 14. The glass of any one of the preceding claims, comprising:

[0210] EMBODIMENT 15 4 mol% or more and 5 mol% or less of Na2O, 15. The glass of any one of the preceding claims, comprising:

[0211] EMBODIMENT 16 0.5 mol % or more and 1.5 mol % or less of P2O5, 16. The glass of any one of the preceding claims, comprising:

[0212] EMBODIMENT 17 3 mol% or more and 4 mol% or less of B2O3; 17. The glass of any one of the preceding claims, comprising:

[0213] EMBODIMENT 18 18. The glass of any one of the preceding claims, wherein the glass is substantially free of Fe2O3.

[0214] EMBODIMENT 19 19. The glass of any one of the preceding claims, wherein the glass is substantially free of ZrO2.

[0215] EMBODIMENT 20 20. The glass of any one of the preceding claims, wherein the glass is substantially free of Ta2O5, HfO2, La2O3, and Y2O3.

[0216] EMBODIMENT 21 21. The glass of any one of the preceding embodiments, wherein the molar ratio of Li2O / Na2O is from 1.2 to 2.0, inclusive.

[0217] EMBODIMENT 22 22. The glass of any one of the preceding embodiments, wherein the molar ratio of Li2O / Na2O is from 1.6 to 2.0, inclusive.

[0218] EMBODIMENT 23 23. The glass of any one of the preceding claims, wherein the glass has a liquidus viscosity in the range of from greater than or equal to 50 kP to 75 kP.

[0219] EMBODIMENT 24 The glass has a viscosity of 0.75 MPa m 0.5 Fracture toughness K IC 24. The glass of any one of the preceding claims, having the following structure:

[0220] EMBODIMENT 25 Glass is SiO2, Al2O3, LiO, NaO, P2O5, and B2O3, Including, The molar ratio of Li2O / Na2O is 1.2 or more and 2.0 or less, The glass has a liquidus viscosity in the range of from 50 kP to 75 kP; The glass has a resistance of 0.75 MPa m 0.5 Fracture toughness K IC Glass having

[0221] EMBODIMENT 26 26. The glass of embodiment 25, further comprising TiO2.

[0222] EMBODIMENT 27 27. The glass of embodiment 25 or 26, further comprising KO.

[0223] EMBODIMENT 28 28. The glass of any one of embodiments 25 to 27, further comprising CaO.

[0224] EMBODIMENT 29 29. The glass of any one of embodiments 25 to 28, further comprising MgO.

[0225] EMBODIMENT 30 30. The glass of any one of embodiments 25 to 29, further comprising SrO.

[0226] EMBODIMENT 31 The glass of any one of embodiments 25 to 30, further comprising SnO2.

[0227] EMBODIMENT 32 32. The glass of any one of claims 25 to 31, wherein the glass is substantially free of Fe2O3.

[0228] EMBODIMENT 33 33. The glass of any one of claims 25 to 32, wherein the glass is substantially free of ZrO2.

[0229] EMBODIMENT 34 34. The glass of any one of claims 25 to 33, wherein the glass is substantially free of Ta2O5, HfO2, La2O3, and Y2O3.

[0230] EMBODIMENT 35 In the method, ion exchanging the glass-based substrate in a molten salt bath to form a glass-based article; Including, 35. The method of claim 34, wherein the glass-based article comprises a compressive stress layer extending from a surface of the glass-based article to a compression depth, the glass-based article comprises a central tension region, and the glass-based substrate is made from the glass of any one of claims 1 to 34.

[0231] EMBODIMENT 36 36. The method of embodiment 35, wherein the molten salt bath comprises NaNO.

[0232] EMBODIMENT 37 37. The method of embodiment 35 or 36, wherein the molten salt bath comprises KNO.

[0233] EMBODIMENT 38 38. The method of any one of embodiments 35 to 37, wherein the molten salt bath is at a temperature of from 380° C. or more to 470° C. or less.

[0234] EMBODIMENT 39 39. The method of any one of embodiments 35 to 38, wherein the ion exchange is for a period of from 10 minutes to 24 hours.

[0235] EMBODIMENT 40 40. The method of any one of claims 35 to 39, further comprising ion exchanging the glass-based article in a second molten salt bath.

[0236] EMBODIMENT 41 41. The method of embodiment 40, wherein the second molten salt bath comprises KNO3.

[0237] EMBODIMENT 42 In glass-based articles, a compressive stress layer extending from the surface of the glass-based article to a compression depth; a central tension area, and 60 mol% or more and 66 mol% or less of SiO2; 14 mol% or more and 16 mol% or less of Al2O3; 7 mol% or more and 9 mol% or less of Li2O; 4 mol% or more and 6 mol% or less of Na2O, 0.5 mol% or more and 3 mol% or less of P2O5, 0.5 mol% to 6 mol% B2O3, and greater than 0 mol% to 1 mol% or less of TiO2; A composition at the center of the glass-based article comprising: A glass-based article having the above structure.

[0238] EMBODIMENT 43 In glass-based articles, a compressive stress layer extending from the surface of the glass-based article to a compression depth; a central tension area, and SiO2, Al2O3, LiO, NaO, P2O5, and B2O3, A composition at the center of the glass-based article comprising: having The molar ratio of Li2O / Na2O is 1.2 or more and 2.0 or less, and a glass having the same composition and microstructure as the composition at the center of the glass-based article is produced with a liquidus viscosity in the range of 50 kP or more and 75 kP or more, and a liquidus viscosity of 0.75 MPa m 0.5 Fracture toughness K IC The glass-based article has

[0239] EMBODIMENT 44 44. The glass-based article of claim 42 or 43, wherein the compressive stress layer has a compressive stress of from 500 MPa or more to 1500 MPa or less.

[0240] EMBODIMENT 45 45. The glass-based article of any one of claims 42 to 44, wherein the central tension zone has a maximum central tension of 60 MPa or more and 160 MPa or less.

[0241] EMBODIMENT 46 46. ​​The glass-based article of any one of claims 42 to 45, wherein the compression depth is from 0.20t to 0.25t, inclusive, where t is a thickness of the glass-based article.

[0242] EMBODIMENT 47 47. The glass-based article of any one of claims 42 to 46, wherein the compressive stress layer has a compressive stress spike extending from a surface of the glass-based article to a compressive stress spike depth, the compressive stress spike depth being from 3 μm or more to 10 μm or less.

[0243] EMBODIMENT 48 48. The glass-based article of any one of claims 42 to 47, wherein the glass-based article has a thickness, t, of 0.2 mm or more and 2 mm or less.

[0244] EMBODIMENT 49 The composition at the center of the glass-based article is from greater than 0 mol % to 0.5 mol % or less of K2O; 49. The glass-based article of any one of claims 42 to 48, comprising:

[0245] EMBODIMENT 50 The composition at the center of the glass-based article is 0.1 mol % or more and 0.5 mol % or less of TiO2; 50. The glass-based article of any one of claims 42 to 49, comprising:

[0246] EMBODIMENT 51 The composition at the center of the glass-based article is 0 mol % or more and 4 mol % or less of MgO; 51. The glass-based article of any one of embodiments 42 to 50, comprising:

[0247] EMBODIMENT 52 The composition at the center of the glass-based article is 0.1 mol % or more and 1 mol % or less of MgO; 52. The glass-based article of any one of claims 42 to 51, comprising:

[0248] EMBODIMENT 53 The composition at the center of the glass-based article is 0 mol% or more and 3 mol% or less of CaO; 53. The glass-based article of any one of claims 42 to 52, comprising:

[0249] EMBODIMENT 54 The composition at the center of the glass-based article is 1 mol% or more and 2 mol% or less of CaO; 54. The glass-based article of any one of claims 42 to 53, comprising:

[0250] EMBODIMENT 55 The composition at the center of the glass-based article is 0 mol % or more and 4 mol % or less of SrO; 55. The glass-based article of any one of claims 42 to 54, comprising:

[0251] EMBODIMENT 56 The composition at the center of the glass-based article is 0.5 mol % or more and 2 mol % or less of SrO; 56. The glass-based article of any one of claims 42 to 55, comprising:

[0252] EMBODIMENT 57 The composition at the center of the glass-based article is ZnO, from 0 mol% to 1 mol% 57. The glass-based article of any one of claims 42 to 56, comprising:

[0253] EMBODIMENT 58 The composition at the center of the glass-based article is 0 mol% to 0.1 mol% SnO2, 58. The glass-based article of any one of claims 42 to 57, comprising:

[0254] EMBODIMENT 59 The composition at the center of the glass-based article is 64 mol% or more and 65 mol% or less of SiO2; 59. The glass-based article of any one of claims 42 to 58, comprising:

[0255] EMBODIMENT 60 The composition at the center of the glass-based article is 15 mol% or more and 16 mol% or less of Al2O3; 60. The glass-based article of any one of claims 42 to 59, comprising:

[0256] EMBODIMENT 61 The composition at the center of the glass-based article is 7 mol% or more and 8 mol% or less of Li2O; 61. The glass-based article of any one of claims 42 to 60, comprising:

[0257] EMBODIMENT 62 The composition at the center of the glass-based article is 4 mol% or more and 5 mol% or less of Na2O, 62. The glass-based article of any one of claims 42 to 61, comprising:

[0258] EMBODIMENT 63 The composition at the center of the glass-based article is 0.5 mol % or more and 1.5 mol % or less of P2O5, 63. The glass-based article of any one of claims 42 to 62, comprising:

[0259] EMBODIMENT 64 The composition at the center of the glass-based article is 3 mol% or more and 4 mol% or less of B2O3; 64. The glass-based article of any one of claims 42 to 63, comprising:

[0260] EMBODIMENT 65 65. The glass-based article of any one of claims 42 to 64, wherein the composition at the center of the glass-based article is substantially free of Fe2O3.

[0261] EMBODIMENT 66 66. The glass-based article of any one of claims 42 to 65, wherein the composition at the center of the glass-based article is substantially free of ZrO2.

[0262] EMBODIMENT 67 67. The glass-based article of any one of claims 42 to 66, wherein the composition at the center of the glass-based article is substantially free of Ta2O5, HfO2, La2O3, and Y2O3.

[0263] EMBODIMENT 68 68. The glass-based article of any one of claims 42 to 67, wherein the composition at the center of the glass-based article has a molar ratio of Li2O / Na2O from 1.6 or more to 2.0 or less.

[0264] EMBODIMENT 69 In consumer electronics, a housing having a front, a back, and sides; Electrical components disposed at least partially within said housing, the electrical components including at least a controller, a memory, and a display disposed on or adjacent a front surface of the housing; and a cover substrate disposed over the display; Equipped with 69. A consumer electronic product, wherein at least a portion of at least one of the housing and the cover substrate is made from the glass-based article of any one of claims 42 to 68. [Explanation of symbols]

[0265] 100 Glass-based products 110 First Surface 112 Second Surface 120 First Section 122 Second Section 130 Central area 200 Household electronics 202 Case 204 Front 206 Back 208 Side 210 Display 212 Cover

Claims

1. In glass, 60 mol % or more to 66 mol % or less of SiO 2 , 14 mol% or more and 16 mol% or less of Al 2 O 3 , 7 mol% to 9 mol% Li 2 O. 4 mol% to 6 mol% Na 2 O. 0.5 mol % to 3 mol % P 2 O 5 , 0.5 mol % to 6 mol % B 2 O 3 , and More than 0 mol% to 1 mol% or less of TiO 2 , Including glass.

2. K from more than 0 mol% to 0.5 mol% 2 O. The glass of claim 1 , comprising:

3. 0 mol % to 4 mol % MgO, The glass of claim 1 or 2, comprising:

4. 0 mol% or more and 3 mol% or less of CaO; The glass of claim 1 or 2, comprising:

5. 0 mol % to 4 mol % SrO, The glass of claim 1 or 2, comprising:

6. ZnO from 0 mol% to 1 mol% The glass of claim 1 or 2, comprising:

7. In glass-based articles, a compressive stress layer extending from the surface of the glass-based article to a compression depth; a central tension area, and 60 mol % or more to 66 mol % or less of SiO 2 , 14 mol% or more and 16 mol% or less of Al 2 O 3 , 7 mol% to 9 mol% Li 2 O. 4 mol% to 6 mol% Na 2 O. 0.5 mol % to 3 mol % P 2 O 5 , 0.5 mol % to 6 mol % B 2 O 3 , and More than 0 mol% to 1 mol% or less of TiO 2 , A composition at the center of the glass-based article comprising: A glass-based article having the above structure.

8. The compressive stress layer is A compressive stress of 500 MPa or more and 1500 MPa or less, and / or a compressive stress spike extending from the surface of the glass-based article to a compressive stress spike depth of 3 μm or more and 10 μm or less; The glass-based article according to claim 7, comprising at least one of:

9. 9. The glass-based article of claim 7 or 8, wherein the central tension region has a maximum central tension of 60 MPa or more and 160 MPa or less.

10. 9. The glass-based article of claim 7 or 8, wherein the compression depth is from 0.20t to 0.25t, inclusive, where t is the thickness of the glass-based article.

11. In consumer electronics, a housing having a front, a back, and sides; Electrical components disposed at least partially within said housing, the electrical components including at least a controller, a memory, and a display disposed on or adjacent a front surface of the housing; and a cover substrate disposed over the display; Equipped with 9. A consumer electronic product, wherein at least a portion of at least one of the housing and the cover substrate is made from the glass-based article of claim 7 or 8.

Citation Information

Patent Citations

  • High-aluminum glass, high-aluminum tempered glass and preparation method of high-aluminum tempered glass

    CN113149428A

  • Peraluminous lithium aluminosilicate with high liquidus viscosity

    JP2021501108A

  • Ion-exchangeable alkali aluminosilicate glass compositions having improved mechanical durability

    WO2021108314A1