Optical laminate and its manufacturing method, smart window including the same, and automobile and building fittings to which the same is applied
By eliminating the separate base material and directly forming the conductive layer on a polarizing plate, the optical laminate achieves simplified manufacturing, reduced thickness, and improved light transmission and durability, addressing issues of deformation and dimming function deterioration.
Patent Information
- Application Number
- JP2024501603
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-07-16
- Filing Date
- 2022-07-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional variable transmittance optical laminates require a separate base material for forming a conductive layer, leading to complex manufacturing processes, increased thickness, and reduced light transmission due to phase differences, which can cause issues with deformation and dimming function deterioration under temperature changes.
A variable transmittance optical laminate design that eliminates the need for a separate base material by directly forming a conductive layer on a polarizing plate, utilizing two polarizers with adjusted contraction forces and a liquid crystal layer, adhered without a separate base material, to simplify manufacturing and reduce thickness while improving light transmission and durability.
The solution simplifies the manufacturing process, reduces thickness, enhances light transmission, and minimizes deformation and dimming function deterioration due to temperature changes, while maintaining excellent bending properties and light control functionality.
Smart Images

Figure 2024536668000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a variable transmittance optical laminate and a manufacturing method thereof, a smart window including the same, and automobile and building fittings to which the same is applied. [Background technology]
[0002] In general, an external light blocking coating is often applied to glass windows of vehicles and other means of transportation. However, the glass windows of conventional means of transportation have a fixed transmittance, and the external light blocking coating also has a fixed transmittance. Therefore, the total transmittance of such conventional windows of means of transportation is fixed, which may lead to accidents. For example, if the overall transmittance is set low, there is no problem during the day when there is sufficient light in the surroundings. However, there is a problem that it is difficult for drivers to properly check the surroundings of the means of transportation in the nighttime when there is insufficient light in the surroundings. Alternatively, if the overall transmittance is set high, there is a problem that it may cause glare to drivers in the daytime when there is sufficient light in the surroundings. For this reason, a variable transmittance optical laminate capable of changing the transmittance of light when a voltage is applied has been developed.
[0003] The variable transmittance optical stack is driven by applying a voltage to drive the liquid crystal to change the transmittance. The variable transmittance optical stack developed to date is manufactured by forming a conductive layer for driving the liquid crystal on a separate substrate and combining it with other elements such as a polarizing plate.
[0004] For example, Japanese Patent Application Laid-Open No. 2018-010035 also discloses a variable transmittance optical laminate including a transparent electrode layer formed on a polycarbonate (PC) substrate having a predetermined thickness.
[0005] However, when a separate substrate is used to form the conductive layer, the manufacturing process becomes complicated, which increases manufacturing costs, and the thickness of the laminate increases, resulting in a phase difference and causing a change in transmittance.
[0006] Therefore, there is a need to develop a variable transmittance optical laminate that does not require a separate substrate for forming a conductive layer, thereby simplifying the manufacturing process and reducing the thickness. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2018-010035 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a variable transmittance optical laminate that does not require a separate substrate for forming a conductive layer, and thus has a simplified manufacturing process.
[0009] Another object of the present invention is to provide a variable transmittance optical laminate that does not include a separate substrate for forming a conductive layer, and thus has a significantly reduced thickness.
[0010] Another object of the present invention is to provide a variable transmittance optical laminate having improved transmittance in a transmission mode by not including a separate substrate for forming a conductive layer.
[0011] Another object of the present invention is to provide a variable transmittance optical laminate having a curved shape by adjusting the contraction forces of two different polarizers.
[0012] Another object of the present invention is to provide a variable transmittance optical laminate in which deformation due to internal and external temperature changes is minimized by controlling the contraction forces of two different polarizers.
[0013] Another object of the present invention is to provide a variable transmittance optical laminate that can prevent deterioration of the light control function due to changes in internal and external temperature by adjusting the contraction forces of two different polarizers.
[0014] Another object of the present invention is to provide a smart window including the variable transmittance optical laminate, and a fitting for an automobile or building to which the smart window is applied.
[0015] However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0016] The present invention relates to a variable transmittance optical laminate including a first polarizer, a first transparent conductive layer formed on an inner surface of the first polarizer, a second polarizer facing the first polarizer, a second transparent conductive layer formed on the inner surface of the second polarizer and facing the first transparent conductive layer, and a liquid crystal layer provided between the first transparent conductive layer and the second transparent conductive layer, wherein at least one of the first transparent conductive layer and the second transparent conductive layer is formed in direct contact with one of the first polarizer and the second polarizer, and a contraction force F1 of the first polarizer and a contraction force F2 of the second polarizer satisfy the following formula 1. [Formula 1] 0.5≦F1 / F2≦0.8
[0017] In the first aspect of the present invention, a contraction force F1 of the first polarizer may be 1.0 to 2.0N.
[0018] In the second aspect of the present invention, a contraction force F2 of the second polarizer may be in the range of 2.0 to 4.0N.
[0019] In the third aspect of the present invention, the first polarizer may have a thickness of 1 to 10 μm.
[0020] In the fourth aspect of the present invention, the second polarizer may have a thickness of 5 to 25 μm.
[0021] In a fifth aspect of the present invention, an absorption axis of the first polarizer and an absorption axis of the second polarizer may be parallel to each other.
[0022] In a sixth aspect of the present invention, at least one of the first transparent conductive layer and the second transparent conductive layer may be formed in direct contact with either one of the first polarizing plate and the second polarizing plate without the inclusion of a separate substrate between the transparent conductive layer and either one of the first polarizing plate and the second polarizing plate.
[0023] In a seventh aspect of the present invention, at least one of the first transparent conductive layer and the second transparent conductive layer may be formed in direct contact with either one of the first polarizing plate and the second polarizing plate, including an easy-adhesion layer between the transparent conductive layer and either one of the first polarizing plate and the second polarizing plate.
[0024] In an eighth aspect of the present invention, at least one of the first transparent conductive layer and the second transparent conductive layer may contain one or more materials selected from the group consisting of transparent conductive oxides, metals, carbon-based materials, conductive polymers, conductive inks, and nanowires.
[0025] In a ninth aspect of the present invention, at least one of the first polarizing plate and the second polarizing plate may include one or more functional layers selected from the group consisting of a protective layer, a phase difference adjusting layer, and a refractive index adjusting layer.
[0026] In a tenth aspect of the present invention, at least one of the first polarizing plate and the second polarizing plate may have a thickness of 30 to 200 μm.
[0027] In an eleventh aspect of the present invention, the liquid crystal layer may include one or more spacers selected from the group consisting of a ball spacer and a column spacer.
[0028] In a twelfth aspect of the present invention, the ball spacer may have a diameter of 1 to 10 μm.
[0029] In a thirteenth aspect of the present invention, an area of the ball spacer in the liquid crystal layer may be 0.01% to 10% of an area of the liquid crystal layer.
[0030] In a fourteenth aspect of the present invention, the variable transmittance optical laminate may further include one or more layers selected from the group consisting of an alignment film, an adhesive layer, an ultraviolet absorbing layer, and a hard coating layer.
[0031] The present invention also relates to a method for producing the variable transmittance optical laminate.
[0032] The present invention also relates to a smart window including the variable transmittance optical laminate.
[0033] The present invention also relates to an automobile in which the smart window is applied to at least one of a front window, a rear window, a side window, a sunloop window, and an interior partition.
[0034] The present invention also relates to a building fixture including the smart window. Effect of the Invention
[0035] According to the variable transmittance optical laminate of the present invention, the steps of forming a conductive layer on a substrate and bonding it to other components required for forming a conventional optical laminate can be omitted, and the manufacturing process can be simplified compared to conventional optical laminates.
[0036] In addition, according to the variable transmittance optical laminate of the present invention, a conductive layer is formed directly on one side of a polarizing plate, and a separate substrate for forming the conductive layer is not required, thereby significantly reducing the thickness compared to conventional optical laminates.
[0037] In addition, according to the variable transmittance optical laminate of the present invention, a conductive layer is formed directly on one side of a polarizing plate, and a separate substrate for forming the conductive layer is not required, thereby improving the transmittance in a light transmission mode compared to conventional optical laminates.
[0038] In addition, the variable transmittance optical laminate according to the present invention can have a curved portion by adjusting the contraction forces of the two different polarizers.
[0039] In addition, the variable transmittance optical laminate according to the present invention can minimize deformation caused by internal and external temperature changes compared to conventional optical laminates by controlling the contraction forces of two different polarizers.
[0040] In addition, according to the variable transmittance optical laminate of the present invention, the contraction forces of two different polarizers are adjusted to minimize deterioration of the light control function due to internal and external temperature changes compared to conventional optical laminates. [Brief description of the drawings]
[0041] [Figure 1] FIG. 1 is a diagram showing a layered structure of a variable transmittance optical layered body according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing a laminate structure of a polarizing plate according to one or more embodiments of the present invention. [Diagram 3] FIG. 3 is a diagram showing a layered structure of a variable transmittance optical layered body according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0042] The present invention relates to a variable transmittance optical laminate having a curved portion, and more particularly, to a variable transmittance optical laminate in which a conductive layer for driving liquid crystal is directly formed on one side of a polarizing plate, thereby reducing the thickness of the laminate since no separate substrate is required for forming the conductive layer, and the transmittance in a light transmission mode is improved, and deformation due to internal and external temperature changes and deterioration of a dimming function can be minimized by controlling the contraction force of two polarizers facing each other.
[0043] More specifically, the present invention relates to a variable transmittance optical laminate including a first polarizer, a first transparent conductive layer formed on an inner surface of the first polarizer, a second polarizer facing the first polarizer, a second transparent conductive layer formed on the inner surface of the second polarizer and facing the first transparent conductive layer, and a liquid crystal layer provided between the first transparent conductive layer and the second transparent conductive layer, wherein at least one of the first transparent conductive layer and the second transparent conductive layer is formed in direct contact with one of the first polarizer and the second polarizer, and a contraction force F1 of the first polarizer and a contraction force F2 of the second polarizer satisfy the following formula 1. [Formula 1] 0.5≦F1 / F2≦0.8
[0044] The variable transmittance optical laminate of the present invention is particularly suitable for technical fields in which light transmittance can be changed by applying a voltage, and can be used, for example, in smart windows.
[0045] A smart window is an optical structure that controls the amount of light or heat passing through by changing the light transmittance according to the application of an electric signal. That is, a smart window is designed to be able to change to a transparent, opaque or translucent state according to a voltage, and is also called variable transmittance glass, light control glass or smart glass.
[0046] A smart window can be used as a partition for dividing or protecting privacy in the interior space of a vehicle or building, or as a light window placed in an opening of a building. It can also be used as a highway sign, a bulletin board, a number board, a clock or an advertising screen, and can be used to replace glass in vehicles such as windows or sunroofs of automobiles, buses, airplanes, ships or trains.
[0047] The variable transmittance optical laminate of the present invention can also be used in smart windows in the various technical fields described above, but since the transparent conductive layer is directly formed on the polarizing plate, no separate substrate is required for forming the transparent conductive layer, and therefore the thickness is thin and the flexibility is advantageous, making it particularly suitable for use as a smart window for vehicles or buildings. In one or more embodiments, the smart window to which the variable transmittance optical laminate of the present invention is applied can be used as a front window, rear window, side window, and sunroof window of an automobile, or a building fixture, and can be used not only for blocking external light, but also for dividing the interior space of an automobile or building, such as an interior partition, or for privacy protection.
[0048] Hereinafter, the embodiments of the present invention will be described in more detail with reference to the drawings. However, the following drawings attached to this specification are intended to illustrate preferred embodiments of the present invention and to facilitate a better understanding of the technical concept of the present invention together with the above-mentioned content of the invention, and therefore the present invention should not be interpreted as being limited only to the matters described in these drawings.
[0049] The terms used herein are for the purpose of describing the embodiments and are not intended to limit the present invention. In this specification, the singular form includes the plural form unless otherwise specified in the phrase. For example, the term "polarizer" used in this specification may mean at least one polarizer of the first polarizer and the second polarizer, and the term "transparent conductive layer" may mean at least one transparent conductive layer of the first transparent conductive layer and the second transparent conductive layer.
[0050] As used herein, the terms "comprises" and / or "comprising" are used in a sense that does not exclude the presence or addition of one or more other components, steps, operations and / or elements other than the stated components, steps, operations and / or elements. The same reference numerals refer to the same components throughout the specification.
[0051] Spatially relative terms such as "below," "bottom," "lower," "upper," "top," and the like, may be used to easily describe the relationship of one element or component to another element or component as depicted in the drawings. Spatially relative terms should be understood to include different orientations of elements in use or operation in addition to the orientation depicted in the drawings. For example, if an element depicted in the drawings is turned upside down, an element described as "below" or "below" another element may be placed "above" the other element. Thus, the exemplary term "below" can include both an orientation of below and above. Elements may be oriented in other directions, and thus the spatially relative terms may be interpreted accordingly.
[0052] The "shrinkage force" used in this specification is defined as a value measured using a DMA Q800 (Dynamic mechanical analyzer, TA Corporation) after cutting a polarizer into a size of 30 mm x 2 mm so that the absorption axis direction of the polarizer is the long side.
[0053] FIG. 1 is a diagram showing the laminate structure of a variable transmittance optical laminate according to one embodiment of the present invention, FIG. 2 is a diagram showing the laminate structure of a polarizing plate according to one or more embodiments of the present invention, and FIG. 3 is a diagram showing the laminate structure of a variable transmittance optical laminate according to another embodiment of the present invention.
[0054] Referring to FIG. 1, a variable transmittance optical stack according to one embodiment of the present invention includes a first polarizer 100-1, a second polarizer 100-2, a first transparent conductive layer 200-1, a second transparent conductive layer 200-2, and a liquid crystal layer 300, and may have a curved portion.
[0055] The direction in which the curved portion is formed may be appropriately selected according to the needs of the user. For example, the curved portion may be formed so that the central region of the optical laminate faces outward.
[0056] 2, the polarizing plate 100 includes a polarizer 110 and may further include functional layers, such as a protective layer 120, a phase difference control layer 130, and a refractive index control layer 140, on one or both sides of the polarizer 110. For example, the polarizing plate 100 may include a polarizer 110 and a protective layer 120 stacked on one or both sides of the polarizer 110 (see FIGS. 2a and 2b). The polarizing plate 100 may also include a polarizer 110, a protective layer 120 stacked on one side of the polarizer 110, and a phase difference control layer 130 stacked on the other side of the polarizer 110 opposite to the one side (see FIG. 2c). The polarizing plate 100 may include a polarizer 110, a protective layer 120 stacked on one surface of the polarizer, and a phase difference control layer 130 and a refractive index control layer 140 stacked in sequence on the other surface of the polarizer 110 opposite the one surface (see FIG. 2d). The polarizing plate 100 may include a polarizer 110, a protective layer 120 stacked on one surface of the polarizer, and a protective layer 120 and a phase difference control layer 130 stacked in sequence on the other surface of the polarizer 110 opposite the one surface (see FIG. 2e).
[0057] The polarizer 110 may be any conventional or later developed polarizer, such as a stretched type polarizer or a coated type polarizer.
[0058] In one embodiment, the stretched polarizer may include a stretched polyvinyl alcohol (PVA)-based resin. The polyvinyl alcohol (PVA)-based resin may be a polyvinyl alcohol-based resin obtained by saponifying a polyvinyl acetate-based resin. Examples of the polyvinyl acetate-based resin include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate and other monomers copolymerizable therewith. The other monomers may be unsaturated carboxylic acid-based, unsaturated sulfonic acid-based, olefin-based, vinyl ether-based, and acrylamide-based monomers having an ammonium group. The polyvinyl alcohol (PVA)-based resin may be modified, for example, polyvinyl formal or polyvinyl acetal modified with aldehydes.
[0059] In an embodiment, the coating type polarizer may be formed using a liquid crystal coating composition, and the liquid crystal coating composition may include a reactive liquid crystal compound and a heterochromatic dye.
[0060] The reactive liquid crystal compound may refer to a compound that includes, for example, a mesogen skeleton and further includes one or more polymerizable functional groups. Such reactive liquid crystal compounds are variously known under the name of RM (Reactive Mesogen). The reactive liquid crystal compound can be polymerized by light or heat to form a cured film in which a polymer network is formed while maintaining the liquid crystal alignment.
[0061] The reactive liquid crystal compound may be a monofunctional or polyfunctional reactive liquid crystal compound. The monofunctional reactive liquid crystal compound is a compound having one polymerizable functional group, and the polyfunctional reactive liquid crystal compound is a compound having two or more polymerizable functional groups.
[0062] The heterochromatic dye is a component contained in the liquid crystal coating composition and provides a polarizing property, and has a property that the absorbance in the long axis direction of the molecule is different from that in the short axis direction. The heterochromatic dye may be a conventional or later developed heterochromatic dye, and may include at least one dye selected from the group consisting of azo dyes, anthraquinone dyes, perylene dyes, merocyanine dyes, azomethine dyes, phthaloperylene dyes, indigo dyes, dioxazine dyes, polythiophene dyes, and phenoxazine dyes.
[0063] The liquid crystal coating composition may further include a solvent capable of dissolving the reactive liquid crystal compound and the different color dye, such as propylene glycol monomethyl ether acetate (PGMEA), methyl ethyl ketone (MEK), xylene, chloroform, etc. Also, the liquid crystal coating composition may further include a labeling agent, a polymerization initiator, etc., within a range that does not inhibit the polarization properties of the coating film.
[0064] In one embodiment, the first polarizer provided in the first polarizing plate 100-1 and the second polarizer provided in the second polarizing plate 100-2 may have different contraction forces. When the first polarizer and the second polarizer have different contraction forces, it is possible to easily form a curved portion of the optical laminate and to further improve the durability of the optical laminate having the curved portion.
[0065] For example, as shown in FIG. 1, the contraction force F2 of the second polarizer provided in the second polarizing plate 100-2 may be greater than the contraction force F1 of the first polarizer provided in the first polarizing plate 100-1, in which case the optical stack may have a shape that is curved so that the central region of the optical stack faces the second direction.
[0066] The contraction force F1 of the first polarizer and the contraction force F2 of the second polarizer may be appropriately set within a range that does not impair the object of the present invention, but it is preferable that they satisfy the following formula 1. [Formula 1] 0.5≦F1 / F2≦0.8
[0067] If the ratio F1 / F2 of the contraction force F1 of the first polarizer to the contraction force F2 of the second polarizer is less than 0.5, the light control function may be reduced due to excessive bending of the optical laminate, and if it exceeds 0.8, it may be disadvantageous in forming a curved shape of the optical laminate.
[0068] In one or more embodiments, the contraction force F1 of the first polarizer may be 1.0 to 2.0 N, and preferably 1.3 to 1.8 N. The contraction force F2 of the second polarizer may be 2.0 to 4.0 N, and preferably 2.2 to 3.8 N. When the contraction force F1 of the first polarizer and the contraction force F2 of the second polarizer satisfy the above ranges, it is easy to form a curved shape of the optical laminate, the deterioration of the photochromic function of the optical laminate due to the curved portion does not occur, and the deterioration of durability due to the internal and external temperature change of the optical laminate can be minimized.
[0069] In one or more embodiments, the first polarizer may have a thickness of 1 to 10 μm, and preferably 3 to 10 μm. The second polarizer may have a thickness of 5 to 25 μm, and preferably 10 to 25 μm. When the thicknesses of the first polarizer and the second polarizer are within the above ranges, it is easy to form a curved shape of the optical laminate, the light control function of the optical laminate is not deteriorated due to the curved portion, and deterioration of durability due to internal and external temperature changes of the optical laminate can be minimized.
[0070] The absorption axis of the first polarizer and the absorption axis of the second polarizer may be appropriately arranged within a range that does not impair the object of the present invention, and for example, the absorption axis of the first polarizer and the absorption axis of the second polarizer may be parallel to each other.
[0071] The protective layer 120 serves to preserve the polarization characteristics of the polarizer 110 from post-processing and external environments, and may be implemented in the form of a protective film.
[0072] 2a and 2b, the protective layer 120 may be formed on one or both sides of the polarizer 110 in direct contact therewith, but is not limited thereto. For example, the protective layer may be used as a multi-layer structure in which one or more protective layers are continuously stacked, or may be formed in direct contact with other functional layers.
[0073] In one or more embodiments, the protective layer 120 may include at least one selected from the group consisting of polyethylene terephthalate (PET), polyethylene isophthalate (PEI), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), diacetyl cellulose (diacetyl cellulose), triacetyl cellulose (TAC), polycarbonate (PC), polyethylene (PE), polypropylene (PP), polymethyl acrylate (PMA), polymethyl methacrylate (PMMA), polyethyl acrylate (PEA), polyethyl methacrylate (PEMA), and cyclic olefin polymer (COP).
[0074] The retardation control layer 130 is for complementing the optical properties of the optical laminate and may be implemented in the form of a retardation film, etc., or may use a conventional or later developed retardation film, etc. For example, a quarter wave plate (1 / 4 wave plate) or a half wave plate (1 / 2 wave plate) for delaying the phase of light may be used, and these may be used alone or in combination.
[0075] The phase difference adjusting layer 130 may be formed on one surface of the polarizer 110 in direct contact therewith, as shown in Fig. 2c and Fig. 2d, but is not limited thereto. For example, as shown in Fig. 2e, the phase difference adjusting layer 130 may be formed on one surface of the protective layer 120, and the polarizer 110, the protective layer 120, and the phase difference adjusting layer 130 may be sequentially stacked.
[0076] The retardation adjusting layer 130 may be a polymer stretched film obtained by stretching a polymer film capable of imparting optical anisotropy by stretching in an appropriate manner, or a liquid crystal polymer film.
[0077] In one embodiment, the polymer stretched film may be a polymer layer including polyolefins such as polyethylene (PE) or polypropylene (PP), cycloolefin polymers (COP) such as polynorbornene, polyesters such as polyvinyl chloride (PVC), polyacrylonitrile (PAN), polysulfone (PSU), acrylic resins, polycarbonate (PC), polyethylene terephthalate (PET), polyacrylate, cellulose ester polymers such as polyvinyl alcohol (PVA) or triacetyl cellulose (TAC), or copolymers of two or more monomers among the monomers forming the polymers.
[0078] The method for obtaining the polymer stretched film is not particularly limited, and for example, the polymer material is molded into a film and then stretched. The method for forming the film is not particularly limited, and the film can be molded into a film by known methods such as injection molding, sheet molding, blow molding, injection blow molding, inflation molding, extrusion molding, foam molding, and cast molding, and secondary processing molding methods such as compressed air molding and vacuum molding may also be used. Among them, extrusion molding and cast molding are preferably used. At this time, for example, an extruder equipped with a T-die, a circular die, or the like can be used to extrude the unstretched film. When obtaining a molded product by extrusion molding, a material in which various resin components, additives, etc. are melt-kneaded in advance can be used, or the product can be molded through melt-kneading during extrusion molding. In addition, various resin components can be dissolved using a solvent common to various resin components, such as chloroform or methylene dichloride, and then cast-dried and solidified to cast-mold the unstretched film.
[0079] The polymer stretched film may be produced by uniaxially stretching the formed film in the mechanical direction (MD; mechanical direction, lengthwise or longitudinal direction) or uniaxially stretching in a direction perpendicular to the mechanical direction (TD; transverse direction, widthwise or transverse direction). Alternatively, a biaxially stretched film may be produced by stretching the formed film using a sequential biaxial stretching method of roll stretching and tenter stretching, a simultaneous biaxial stretching method using tenter stretching, or a biaxial stretching method using tubular stretching.
[0080] The liquid crystal polymer film may include a reactive liquid crystal compound in a polymerized state. The reactive liquid crystal compound may be the same as that of the coating type polarizer.
[0081] In one or more embodiments, the thickness of the retardation adjusting layer 130 may be 10 to 100 μm in the case of a polymer stretched film, and may be 0.1 to 5 μm in the case of a liquid crystal polymer film.
[0082] The refractive index adjustment layer 140 is provided to compensate for the refractive index difference of the optical laminate caused by the transparent conductive layer 200, and may serve to improve visibility by reducing the refractive index difference. The refractive index adjustment layer 140 may also be provided to correct a hue caused by the transparent conductive layer 200. Meanwhile, when the transparent conductive layer has a pattern, the refractive index adjustment layer 140 can compensate for a transmittance difference between a patterned region where the pattern is formed and a non-patterned region where the pattern is not formed.
[0083] Specifically, the transparent conductive layer 200 is stacked adjacent to another member (e.g., the polarizer 110, etc.) having a different refractive index from the transparent conductive layer 200, and a difference in light transmittance may be induced due to the difference in refractive index between the adjacent layers, and in particular, when a pattern is formed on the transparent conductive layer, a problem may occur in which the patterned region and the non-patterned region are visually distinguishable. Therefore, by including the refractive index control layer 140, the refractive index is compensated for, and the difference in light transmittance of the optical laminate is reduced, and in particular, when a pattern is formed on the transparent conductive layer, the patterned region and the non-patterned region are visually distinguishable.
[0084] In one embodiment, the refractive index of the refractive index adjusting layer 140 may be appropriately selected depending on the material of other adjacent members, and may be preferably 1.4 to 2.6, and more preferably 1.4 to 2.4. In this case, light loss due to a sharp refractive index difference between other members such as the polarizer 110 and the transparent conductive layer 200 can be prevented.
[0085] The refractive index adjustment layer 140 is not particularly limited as long as it can prevent a sharp refractive index difference between other components such as the polarizer 110 and the transparent conductive layer 200. The refractive index adjustment layer 140 may be formed from a compound used to form a conventional or later developed refractive index adjustment layer, for example, a refractive index adjustment layer-forming composition containing a polymerizable isocyanurate compound.
[0086] In one embodiment, the polarizing plate 100 may further include other functional layers in addition to the above-mentioned functional layers to supplement or enhance the properties of the polarizer, for example, an overcoat layer to further improve mechanical durability.
[0087] In one or more embodiments, the polarizing plate 100 may have a thickness of 30 to 200 μm, preferably 30 to 170 μm, and more preferably 50 to 150 μm, in which case the polarizing plate 100 can be used to manufacture an optical laminate having a small thickness while maintaining optical properties.
[0088] The transparent conductive layer 200 is provided for driving the liquid crystal layer 300, and may be formed in direct contact with the polarizer 100. For example, as shown in Fig. 1, a first transparent conductive layer 200-1 and a second transparent conductive layer 200-2 may be formed in direct contact with a first polarizer 100-1 and a second polarizer 100-2, respectively.
[0089] Conventional optical laminates used in the manufacture of smart windows, etc., are manufactured by forming a conductive layer for driving liquid crystal on one side of a substrate and bonding the other side of the substrate with a polarizing plate. However, the variable transmittance optical laminate according to the present invention is characterized in that it does not include a separate substrate for forming a conductive layer, but directly forms a conductive layer on one side of a polarizing plate, thereby reducing the thickness of the laminate and improving the transmittance and bending characteristics in a light transmission mode.
[0090] In one embodiment, the transparent conductive layer 200 may be formed by direct deposition on one surface of the polarizer 100. In this case, the transparent conductive layer 200 may be formed by directly contacting the pre-treated surface of the polarizer 100 after performing a pre-treatment such as a corona treatment or a plasma treatment on one surface of the polarizer 100 in order to improve adhesion to the polarizer 100. The pre-treatment is not limited to a corona treatment or a plasma treatment, and any conventional or later developed pre-treatment process may be used within the scope of the present invention.
[0091] In another embodiment, the transparent conductive layer 200 may be formed in direct contact with the polarizer 100 via an easy-adhesion layer (not shown) provided on one side of the polarizer 100 in order to improve adhesion to the polarizer 100.
[0092] The transparent conductive layer 200 preferably has a visible light transmittance of 50% or more, and may include, for example, one or more selected from the group consisting of transparent conductive oxides, metals, carbon-based materials, conductive polymers, conductive inks, and nanowires, but is not limited thereto, and any conventional or later developed transparent conductive layer material may be used.
[0093] In one or more embodiments, the transparent conductive oxide may include one or more selected from the group consisting of indium tin oxide (ITO), indium zinc oxide (IZO), indium zinc tin oxide (IZTO), aluminum zinc oxide (AZO), gallium zinc oxide (GZO), florin tin oxide (FTO), zinc oxide (ZnO), etc. The metal may include one or more selected from the group consisting of gold (Au), silver (Ag), copper (Cu), aluminum (Al), platinum (Pt), palladium (Pd), chromium (Cr), titanium (Ti), tungsten (W), niobium (Nb), tantalum (Ta), vanadium (V), iron (Fe), manganese (Mn), cobalt (Co), nickel (Ni), zinc (Zn), and alloys containing at least one of these, and may include, for example, a silver-palladium-copper (APC) alloy or a copper-calcium (CuCa) alloy. The carbon-based material may include at least one selected from the group consisting of carbon nanotubes (CNTs) and graphene, and the conductive polymer may include at least one selected from the group consisting of polypyrrole, polythiophene, polyacetylene, PEDOT, polyaniline, etc. The conductive ink may be an ink in which a metal powder and a curable polymer binder are mixed, and the nanowires may be, for example, silver nanowires (AgNWs).
[0094] In addition, the transparent conductive layer 200 may be formed in a two-layer structure by combining the above materials, for example, in a two-layer structure including a metal layer and a transparent conductive oxide layer to reduce the reflectance and increase the transmittance of incident light.
[0095] The transparent conductive layer 200 may be formed by a method commonly used in the art, for example, a coating process such as spin coating, roller coating, bar coating, dip coating, gravure coating, curtain coating, die coating, spray coating, doctor coating, kneader coating, etc.; a printing process such as screen printing, spray printing, inkjet printing, relief printing, intaglio printing, lithographic printing, etc.; and a deposition process such as CVD (chemical vapor deposition), PVD (physical vapor deposition), PECVD (plasma enhanced chemical vapor deposition), etc.
[0096] The liquid crystal layer 300 can change the driving mode of the optical stack by controlling the transmittance of light incident from one or more directions by an electric field.
[0097] The liquid crystal layer 300 may include a liquid crystal compound and may be located, for example, in a space provided by a sealant layer (not shown) and a spacer (not shown) provided between the first polarizer 100-1 and the second polarizer 100-2 in the light control region.
[0098] The liquid crystal behavior mode of the liquid crystal layer 300 is not particularly limited, and for example, a twisted nematic (TN) mode, a super twisted nematic (STN) mode, a vertical alignment (VA) mode, etc. may be used.
[0099] The liquid crystal compound is not particularly limited as long as it is driven by an electric field and can control the light transmittance, and any conventional or later developed liquid crystal compound may be used. For example, the contents regarding the reactive liquid crystal compound of the coating type polarizer described above may be similarly applied.
[0100] The sealant may include a curable resin as a base resin. The base resin may be a UV-curable resin or a thermosetting resin known in the art to be used for sealants. The UV-curable resin may be a polymer of a UV-curable monomer. The thermosetting resin may be a polymer of a thermosetting monomer.
[0101] The base resin of the sealant may be, for example, an acrylate-based resin, an epoxy-based resin, a urethane-based resin, a phenol-based resin, or a mixture of the resins. In one embodiment, the base resin may be an acrylate-based resin, and the acrylate-based resin may be a polymer of an acrylic monomer. The acrylic monomer may be, for example, a polyfunctional acrylate. In another embodiment, the sealant may further include a monomer component in the base resin. The monomer component may be, for example, a monofunctional acrylate. In this specification, a monofunctional acrylate may mean a compound having one acrylic group, and a polyfunctional acrylate may mean a compound having two or more acrylic groups. The curable resin may be cured by irradiation with ultraviolet light and / or heating. The ultraviolet irradiation conditions or heating conditions may be appropriately performed within a range that does not impair the object of the present application. The sealant may further include an initiator, for example, a photoinitiator or a thermal initiator, as necessary.
[0102] The sealant may be formed by a method commonly used in the art, for example, by drawing the sealant onto the outer periphery (i.e., non-active area) of the liquid crystal layer using a dispenser equipped with a nozzle.
[0103] The spacer may include at least one of a ball spacer and a column spacer, and is preferably a ball spacer. The number of ball spacers may be one or more, and the ball spacer preferably has a diameter of 1 to 10 μm. In addition, when viewed in a planar direction, the area of the ball spacer in the liquid crystal layer 130 is preferably 0.01 to 10% of the area of the liquid crystal layer 300 in terms of improving the user's visibility and the transmittance in the light-transmitting mode.
[0104] In one embodiment, the liquid crystal layer 300 may further include an alignment film 400 (see FIG. 3a) if necessary, for example, formed on both sides of the liquid crystal layer 300 containing the liquid crystal compound.
[0105] The alignment film 400 is not particularly limited as long as it is capable of imparting alignment to the liquid crystal compound. For example, the alignment film 400 may be manufactured by applying and curing an alignment film coating composition including an alignment polymer, a photopolymerization initiator, and a solvent. The alignment polymer is not particularly limited, and may be a polyacrylate resin, a polyamic acid resin, a polyimide resin, a polymer including a cinnamate group, or a conventional or later developed polymer capable of exhibiting alignment.
[0106] The variable transmittance optical laminate of the present invention may further include other components within the scope of the present invention, for example, may further include an adhesive layer 500 (see FIG. 3b), or may further include an ultraviolet absorbing layer, a hard coating layer, etc.
[0107] The adhesive layer 500 may be formed using an adhesive or pressure-sensitive adhesive, and preferably has an appropriate adhesive strength so as to prevent peeling, air bubbles, etc. from occurring when the optical laminate is handled, as well as transparency and thermal stability.
[0108] The adhesive may be any conventional or later developed adhesive, for example a light curable adhesive.
[0109] The photocurable adhesive is crosslinked and cured by exposure to active energy rays such as ultraviolet (UV) and electron beam (EB) to exhibit strong adhesive strength, and may be composed of a reactive oligomer, a reactive monomer, a photopolymerization initiator, etc.
[0110] The reactive oligomer is an important component that determines the properties of the adhesive, and forms a polymer bond by photopolymerization to form a hardened coating. Usable reactive oligomers include polyester resins, polyether resins, polyurethane resins, epoxy resins, polyacrylic resins, silicone resins, etc.
[0111] The reactive monomer functions as a crosslinking agent and a diluent for the reactive oligomer, and affects the adhesive properties. Usable reactive monomers include monofunctional monomers, polyfunctional monomers, epoxy monomers, vinyl ethers, cyclic ethers, and the like.
[0112] The photopolymerization initiator absorbs light energy to generate radicals or cations to initiate photopolymerization, and an appropriate one may be selected and used depending on the photopolymerizable resin.
[0113] The adhesive may be any adhesive that has been used in the past or will be developed in the future, and in one or more embodiments, may be an acrylic adhesive, a rubber adhesive, a silicone adhesive, a urethane adhesive, a polyvinyl alcohol adhesive, a polyvinylpyrrolidone adhesive, a polyacrylamide adhesive, a cellulose adhesive, a vinyl alkyl ether adhesive, etc. The adhesive is not particularly limited as long as it has adhesive strength and viscoelasticity, but in terms of availability, etc., it may be preferably an acrylic adhesive, and may contain, for example, a (meth)acrylate copolymer, a crosslinking agent, and a solvent.
[0114] The crosslinking agent may be a conventional or later developed crosslinking agent, and may include, for example, a polyisocyanate compound, an epoxy resin, a melamine resin, a urea resin, a dialdehyde, a methylol polymer, or the like, and preferably includes a polyisocyanate compound.
[0115] The solvent may include a typical solvent used in the field of resin compositions, such as alcohol-based compounds such as methanol, ethanol, isopropanol, butanol, and propylene glycol methoxy alcohol; ketone-based compounds such as methyl ethyl ketone, methyl butyl ketone, methyl isobutyl ketone, diethyl ketone, and dipropyl ketone; acetate-based compounds such as methyl acetate, ethyl acetate, butyl acetate, and propylene glycol methoxy acetate; cellosolve-based compounds such as methyl cellosolve, ethyl cellosolve, and propyl cellosolve; and hydrocarbon-based compounds such as hexane, heptane, benzene, toluene, and xylene. These may be used alone or in combination of two or more.
[0116] The thickness of the adhesive layer 500 may be appropriately determined depending on the type of resin acting as an adhesive, adhesive strength, the environment in which the adhesive is used, etc. In one embodiment, the adhesive layer may have a thickness of 0.01 μm to 50 μm, preferably 0.05 μm to 20 μm, and more preferably 0.1 μm to 10 μm in order to ensure sufficient adhesive strength and minimize the thickness of the optical laminate, but is not limited thereto.
[0117] The ultraviolet absorbing layer is not particularly limited as long as it is used to prevent deterioration of the optical laminate due to ultraviolet rays. For example, it may be a salicylic acid-based ultraviolet absorber (phenyl salicylate, p-tert-butyl salicylate, etc.), a benzophenone-based ultraviolet absorber (2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, etc.), a benzotriazole-based ultraviolet absorber (2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-(3'',4'',5'',6''-tetrahydrophthalimidomethyl)-5'-methylphenyl)benzotriazole, 2,2-methylenebis(4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazole), azol-2-yl)phenol), 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-(2-octyloxycarbonylethyl)-phenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-(1-methyl-1-phenylethyl)-5'-(1,1,3,3-tetramethylbutyl)-phenyl)benzotriazole, 2-(2H-benzotriazol-2-yl)-6-( Linear and branched dodecyl)-4-methylphenol, mixture of octyl-3-[3-tert-butyl-4-hydroxy-5-(chloro-2H-benzotriazol-2-yl)phenyl]propionate and 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate, etc.), cyanoacrylate UV absorbers (2'-ethylhexyl-2-cyano-3,3-diphenyl acrylate, ethyl-2-cyano-3-(3',4'-methylenedioxyphenyl)-acrylate, triazine-based ultraviolet absorbers, etc. may be used, of which benzotriazole-based ultraviolet absorbers and triazine-based ultraviolet absorbers are preferred because they are highly transparent and have an excellent effect of preventing deterioration of the polarizing plate and the transmittance variable layer, and benzotriazole-based ultraviolet absorbers with a more suitable spectral absorption spectrum are particularly preferred. The benzotriazole-based ultraviolet absorbers may be bis(Bis)-modified, for example, 6,6'-methylenebis(2-(2H-benzo[d][1,2,3]triazol-2-yl)-4-(2,4,4-trimethylpentan-2-yl)phenol), 6,6'-methylenebis(2-(2H-benzo[d][1,2,3]triazol-2-yl)-4-(2-hydroxyethyl)phenol), etc.,
[0118] The hard coating layer is not particularly limited as long as it is for protecting components such as a polarizing plate and a transmittance variable layer from external physical and chemical impacts, and any conventional or later developed hard coating layer may be used.
[0119] In one embodiment, the hard coating layer may be formed by applying a composition for forming a hard coating layer onto another member and curing the composition with light or heat. The composition for forming a hard coating layer is not particularly limited and may include, for example, a photocurable compound and a photoinitiator.
[0120] The photocurable compound and photoinitiator may be any compound commonly used in the art without any limitation. For example, the photocurable compound may be a photopolymerizable monomer, a photopolymerizable oligomer, etc., and examples of the photocurable compound include monofunctional and / or polyfunctional (meth)acrylates, and examples of the photoinitiator include oxime esters, etc.
[0121] In addition to the variable transmittance optical laminate, the present invention includes a smart window including the same. The present invention also includes an automobile in which the smart window is applied to at least one of a front window, a rear window, a side window, a sun loop window, and an interior partition, and a building fixture including the smart window.
[0122] Hereinafter, the present invention will be described in detail with reference to the embodiments. However, the present invention is not limited to the embodiments disclosed below, and may be embodied in various different forms. However, the embodiments are provided to fully disclose the present invention and to fully inform those skilled in the art of the present invention of the scope of the invention, and the present invention is defined only by the scope of the claims. EXAMPLES
[0123] Examples and Comparative Examples: Production of Optical Laminates Example 1 A swelling step was performed by immersing a polyvinyl alcohol resin film in a swelling solution containing deionized water, boric acid, chloride, inorganic acid, inorganic salt, water-soluble organic solvent, and alcohol at a temperature of 20° C. to 30° C. for 60 to 240 seconds to secure a space for dyeing. A dyeing step was performed by immersing the substrate film in an aqueous solution containing 0.1 parts by weight of iodine and 5 parts by weight of potassium iodide per 100 parts by weight of water at a temperature of 20° C. to 35° C. for 60 to 300 seconds to dye the substrate film. A boric acid treatment step was performed by immersing the dyed substrate film in an aqueous solution containing 5 parts by weight of boric acid per 100 parts by weight of water. A drying step was performed by drying the substrate film at a temperature of 50° C. to 80° C., to manufacture a polarizer having a thickness of 8 μm.
[0124] A first polarizing plate was manufactured by laminating different protective films on both sides of the polarizer via an adhesive layer. The different protective films were a triacetyl cellulose resin film having a thickness of 25 μm and a cycloolefin resin film having a thickness of 25 μm. The polarizer contraction force of the first polarizing plate was 1.74 N.
[0125] Meanwhile, a second polarizing plate was fabricated in the same manner as the first polarizing plate, except that the polarizer had a thickness of 18 μm. The polarizer contraction force of the second polarizing plate was 2.67 N.
[0126] A transparent conductive layer was formed on the cycloolefin resin film surface of each of the first and second polarizers, and then an alignment film was formed thereon.The first and second polarizers were then bonded with a liquid crystal layer sandwiched therebetween to fabricate a variable transmittance optical laminate (size: 180 mm wide x 100 mm long) consisting of a first polarizer / transparent conductive layer / alignment film / liquid crystal layer / alignment film / transparent conductive layer / second polarizer.The absorption axis directions of the first and second polarizers were the same, and a liquid crystal layer driven in VA (Vertical Alignment) mode was used.
[0127] Example 2 The variable transmittance optical laminate of Example 2 was manufactured in the same manner as in Example 1, except that the polarizer of the first polarizing plate had a thickness of 8 μm and the polarizer of the second polarizing plate had a thickness of 12 μm.
[0128] Example 3 The variable transmittance optical laminate of Example 3 was manufactured in the same manner as in Example 1, except that the polarizer of the first polarizing plate had a thickness of 8 μm and the polarizer of the second polarizing plate had a thickness of 24 μm.
[0129] Comparative Example 1 A variable transmittance optical laminate of Comparative Example 1 was manufactured in the same manner as in Example 1, except that the polarizer of the first polarizing plate had a thickness of 12 μm and the polarizer of the second polarizing plate had a thickness of 12 μm. However, in the boric acid treatment step, the temperature of the chemical solution used in manufacturing the second polarizer was lowered by 3° C. compared to the manufacturing of the first polarizer.
[0130] Comparative Example 2 The variable transmittance optical laminate of Comparative Example 2 was manufactured in the same manner as in Example 1, except that the polarizer of the first polarizing plate had a thickness of 8 μm and the polarizer of the second polarizing plate had a thickness of 28 μm.
[0131] Experimental Example Polarizer shrinkage force evaluation The polarizers used in the first and second polarizing plates of each of the variable transmittance optical laminates of Examples 1 to 3 and Comparative Examples 1 to 2 were cut into a size of 30 mm x 2 mm so that the absorption axis direction of the polarizer was the long side, and then the contraction force was measured using a DMA Q800 (Dynamic mechanical analyzer, TA Co.) and the results are shown in Table 1. At this time, the measurement was performed using a minimum pre-load in order to keep the polarizer in a taut state before the measurement.
[0132] Bending property evaluation of optical laminates The variable transmittance optical laminates of Examples 1 to 3 and Comparative Examples 1 and 2 were attached between two sheets of 0.5T glass (8 inch size) using an acrylic adhesive, and left at 80°C for 250 hours, and then left at 23°C and 50% relative humidity for 2 hours. The difference in the height of the panel curvature was measured using a three-dimensional measuring device (VMR-6555, Nikon Corporation), and the position of the highest point on the flat plate was measured, and the results are shown in Table 1 below. In this case, the second polarizing plate direction (towards the room side) was marked as "+".
[0133] Evaluation of light control uniformity of optical laminates The variable transmittance optical laminates of Examples 1 to 3 and Comparative Examples 1 and 2 were bonded between glass substrates by applying an adhesive to both sides thereof, and the light transmittance across the entire surface was compared and shown in Table 1 below. <Dimming uniformity evaluation criteria> ○: Light blocking effect is uniform over 95% △: The uniform area of the light blocking effect is 90% or more but less than 95% X: The uniform area of the light blocking effect is less than 90%, or significant light leakage occurs
[0134] [Table 1]
[0135] Referring to Table 1, the variable transmittance optical laminates of Examples 1 to 3, in which the ratio of the contraction force of the first polarizer to the contraction force of the second polarizer is in the range of 0.5 to 0.8, have a bending characteristic evaluation result of 1.2 to 1.8 mm. Not only do they have excellent bending characteristics, but also have a light blocking effect with a uniform area of 90% or more, and thus have excellent light control functions.
[0136] On the other hand, the variable transmittance optical laminate of Comparative Example 1, in which the ratio of the contraction force of the first polarizer to the contraction force of the second polarizer exceeds 0.8, had a bending characteristic evaluation result of 0.8 mm, indicating that the bending characteristics are disadvantageous compared to the optical laminates of the Examples.
[0137] In addition, it can be seen that the variable transmittance optical laminate of Comparative Example 2, in which the ratio of the contraction force of the first polarizer to the contraction force of the second polarizer is less than 0.5, has a disadvantageous dimming function compared to the optical laminates of the Examples due to excessive bending of the liquid crystal layer. [Industrial Applicability]
[0138] According to the variable transmittance optical laminate of the present invention, the steps of forming a conductive layer on a substrate and bonding it to other components required for forming a conventional optical laminate can be omitted, and the manufacturing process can be simplified compared to conventional optical laminates.
Claims
1. a first polarizing plate including a first polarizer; a first transparent conductive layer formed on an inner surface of the first polarizing plate; a second polarizing plate including a second polarizer facing the first polarizing plate; a second transparent conductive layer formed on an inner surface of the second polarizing plate and facing the first transparent conductive layer; a liquid crystal layer provided between the first transparent conductive layer and the second transparent conductive layer, At least one of the first transparent conductive layer and the second transparent conductive layer is formed in direct contact with one of the first polarizing plate and the second polarizing plate, The contraction force F of the first polarizer 1 and the contraction force F of the second polarizer 2 and A variable transmittance optical laminate, which satisfies the following formula 1. [Equation 1] 0.5 ≦ F 1 / F 2 ≦0.8
2. The contraction force F of the first polarizer 1 The variable transmittance optical laminate according to claim 1, wherein the transmittance is 1.0 to 2.0 N.
3. The contraction force F of the second polarizer 2 The variable transmittance optical laminate according to claim 1, wherein the thickness is 2.0 to 4.0 N.
4. The variable transmittance optical laminate according to claim 1 , wherein the first polarizer has a thickness of 1 to 10 μm.
5. The variable transmittance optical stack according to claim 1 , wherein the second polarizer has a thickness of 5 to 25 μm.
6. The variable transmittance optical stack according to claim 1 , wherein the absorption axis of the first polarizer and the absorption axis of the second polarizer are parallel to each other.
7. 2. The variable transmittance optical laminate of claim 1, wherein at least one of the first transparent conductive layer and the second transparent conductive layer is formed in direct contact with either one of the first polarizer and the second polarizer without a separate substrate between the transparent conductive layer and either one of the first polarizer and the second polarizer.
8. The variable transmittance optical laminate of claim 1 , wherein at least one of the first transparent conductive layer and the second transparent conductive layer includes an easy-adhesion layer between either one of the first polarizing plate and the second polarizing plate and is formed in direct contact with the first polarizing plate and the second polarizing plate.
9. 2. The variable transmittance optical stack of claim 1, wherein at least one of the first transparent conductive layer and the second transparent conductive layer comprises at least one selected from the group consisting of transparent conductive oxides, metals, carbon-based materials, conductive polymers, conductive inks, and nanowires.
10. 2. The variable transmittance optical laminate according to claim 1, wherein at least one of the first polarizing plate and the second polarizing plate includes one or more functional layers selected from the group consisting of a protective layer, a phase difference adjusting layer, and a refractive index adjusting layer.
11. The variable transmittance optical laminate according to claim 1 , wherein at least one of the first polarizing plate and the second polarizing plate has a thickness of 30 to 200 μm.
12. The variable transmittance optical laminate according to claim 1 , wherein the liquid crystal layer comprises at least one selected from the group consisting of a ball spacer and a column spacer.
13. The variable transmittance optical stack according to claim 12, wherein the ball spacer has a diameter of 1 to 10 μm.
14. The variable transmittance optical laminate according to claim 12, wherein the area of the ball spacer in the liquid crystal layer is 0.01% to 10% of the area of the liquid crystal layer.
15. The variable transmittance optical laminate according to claim 1 , further comprising at least one layer selected from the group consisting of an alignment film, an adhesive layer, an ultraviolet absorbing layer, and a hard coating layer.
16. A method for producing the variable transmittance optical laminate according to any one of claims 1 to 15.
17. A smart window comprising the variable transmittance optical stack according to any one of claims 1 to 15.
18. 20. A car comprising the smart window of claim 17 applied to at least one of a front window, a rear window, a side window, a sunloop window, and an interior partition.
19. 20. A building fixture comprising the smart window of claim 17.
Citation Information
Patent Citations
Light control film
JP2018010035A