Method for heat treating metal powder

The heat treatment of metal powders using a sintering inhibitor composite addresses the issue of agglomeration during high-temperature processing, maintaining uniform particle size and improving the quality of metal powders for multilayer ceramic capacitors.

JP2024536903AActive Publication Date: 2024-10-08KOREA INSTITUTE OF INDUSTRIAL TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024521215
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-16
Filing Date
2022-10-07
Publication Date
2024-10-08
Estimated Expiration
2042-10-07

AI Technical Summary

Technical Problem

High-temperature heat treatment of metal powders, such as nickel powder, leads to sintering and agglomeration, resulting in irregular particle sizes and poor quality, which is a challenge in producing ultra-thin metal electrode layers for multilayer ceramic capacitors.

Method used

A heat treatment method using a metal powder-sintering inhibitor composite, comprising metal powders dispersed with a sintering inhibitor like metal chloride and ceramic precursors, which are transformed into ceramics during heat treatment, preventing agglomeration and maintaining particle separation.

Benefits of technology

The method effectively prevents sintering between metal powders, ensuring uniform particle size and improved resistance to sintering shrinkage, enhancing the quality of metal powders for use in multilayer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536903000001_ABST
    Figure 2024536903000001_ABST
Patent Text Reader

Abstract

According to one aspect of the present invention, there is provided a method for heat treating a metal powder, comprising the steps of: preparing a metal powder-sintering inhibitor composite including metal powders dispersed and spaced apart within a sintering inhibitor; and heat treating the metal powder-sintering inhibitor composite.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technical concept of the present invention relates to a method for heat treating metal powder, and more particularly to a heat treating method which prevents aggregation and sintering between particles during high-temperature heat treatment of metal powder and provides a uniform grain size. [Background technology]

[0002] Multilayer ceramic capacitors (MLCCs) are chip-type capacitors that temporarily charge electricity in electronic circuits and remove noise, and are components that store current and then stably supply the required amount of electricity to operate electronic devices properly. Today, multilayer ceramic capacitors are in such high demand that they are called the rice of the electronics industry; for example, a personal computer or smartphone requires about 1,000 pieces, and a TV requires about 2,000 pieces.

[0003] Such multilayer ceramic capacitors need to be reduced in size and have increased storage capacitance. To achieve this, multilayer ceramic capacitors have a structure in which approximately 500 ceramic layers and metal electrode layers are alternately stacked inside. Multilayer ceramic capacitors are formed through a molding process in which a ceramic sheet is formed on a release film, a printing process in which an electrode pattern is formed on the ceramic sheet, and a lamination process in which the ceramic sheet is cut, the release film is removed, and then the ceramic sheet and metal electrode layer are laminated. The key technology for the multilayer ceramic capacitor is to laminate many metal electrode layers while making them as thin as possible, and to form them without cracking even at high temperatures of over 1000°C.

[0004] In recent years, as the multilayer ceramic capacitor becomes more compact and has a higher number of layers, there is a demand for ultra-thin internal electrodes. As the metal electrode layers continue to become finer, additional measures are required.

[0005] As part of such measures, various heat treatments have been carried out, such as adding sulfur (S) to nickel powder, which has traditionally been used as a material for the metal electrode layer, oxidizing the surface of the nickel powder, improving the crystallinity of the nickel powder, growing the crystal grains, or removing the sulfur components added during the manufacturing process.

[0006] However, since such heat treatment is usually performed at high temperatures, there is a problem that nickel particles are sintered and agglomerated during the heat treatment. When nickel particles are sintered, the particle size becomes large and the shape becomes irregular, resulting in poor quality of the nickel powder. This problem is not limited to nickel powder, but is a general problem that can occur when ordinary metal powders are heat treated at high temperatures. Summary of the Invention [Problem to be solved by the invention]

[0007] The technical problem to be solved by the technical concept of the present invention is to provide a heat treatment method that prevents aggregation due to sintering between metal powders during high-temperature heat treatment of various metal powders including nickel powder, but this problem is merely an example and the technical concept of the present invention is not limited thereto. [Means for solving the problem]

[0008] According to one aspect of the invention, a method for heat treating metal powder is provided.

[0009] According to one embodiment of the present invention, the method for heat treating the metal powder includes the steps of preparing a metal powder-sintering inhibitor composite including metal powders dispersed and spaced apart within a sintering inhibitor; and heat treating the metal powder-sintering inhibitor composite.

[0010] According to an embodiment of the present invention, the sintering inhibitor may include a metal salt. The metal salt may include a metal chloride, for example, NiCl. 2, BaCl 2 , NaCl, and KCl.

[0011] According to an embodiment of the present invention, the metal powder may include at least one of nickel powder, copper powder, silver powder, iron powder, and alloy powder thereof.

[0012] According to an embodiment of the present invention, the sintering inhibitor may further include a ceramic precursor that is converted into a ceramic by heat together with the metal salt. The ceramic precursor may be Al(NO 3 ) 3 , Al 2 (SO 4 ) 3 , Ba(NO 3 ) 2 , TiCl 4 , and Mg(NO 3 ) 2 may include.

[0013] According to an embodiment of the present invention, the heat treating step may include converting the ceramic precursor into a ceramic.

[0014] According to an embodiment of the present invention, a method for manufacturing the metal powder-sintering inhibitor composite may include the steps of: preparing a sintering inhibitor solution in which a sintering inhibitor is dissolved in a solvent; adding metal powder to the sintering inhibitor solution and dispersing the metal powder to prepare a metal powder dispersion; and spray-drying the dispersed particle dispersion.

[0015] According to an embodiment of the present invention, the method may further include removing the sintering inhibitor after the heat treatment.

[0016] According to an embodiment of the present invention, the heat treatment may be performed in an atmosphere including any one of a hydrogen atmosphere, an oxidizing atmosphere, a carbonizing atmosphere, a decarburizing atmosphere, a reducing atmosphere, an inert atmosphere, an air atmosphere, a sulfurizing atmosphere, a desulfurizing atmosphere, and a vacuum atmosphere.

[0017] According to an embodiment of the present invention, the method may further include removing the sintering inhibitor and recovering the metal powder after the heat treatment step is completed, and in the step of removing the sintering inhibitor, the ceramic converted from the ceramic precursor may remain on at least a portion of the surface of the recovered metal powder. Effect of the Invention

[0018] According to the technical concept of the present invention, the sintering inhibitor inhibits sintering between metal powders during heat treatment of the metal powder at high temperatures, and thus the problem of agglomeration of the metal powder does not occur. In addition, the ceramic precursor contained in the sintering inhibitor remains on the surface of the metal powder when the sintering inhibitor is removed after being transformed into ceramic during the heat treatment, thereby improving resistance to sintering shrinkage when the metal powder is later used to manufacture a metal electrode layer of an MLCC.

[0019] The above-mentioned effects of the present invention are merely illustrative, and the scope of the present invention is not limited to these effects. [Brief description of the drawings]

[0020] [Figure 1] 1 is a flow chart showing a method for heat treating metal powder according to the concepts of the present invention. [Diagram 2] The nickel powder and nickel powder-sintering inhibitor composite used in the experiment were observed with an SEM. [Diagram 3] 1 shows the results of observing the states of control groups 1 to 4 after heat treatment using an SEM. [Figure 4] The results are obtained by SEM observation of the state of experimental groups 3 and 4 after heat treatment (upper photograph), and the state of the nickel powder recovered after removal of the sintering inhibitor (lower photograph). [Diagram 5] This is the result of observing the state of the nickel powder recovered after removing all the sintering inhibitor from the nickel powder-sintering inhibitor composite that had completed the heat treatment using an SEM and conducting a component analysis using an EDS. [Figure 6]The graph shows the results of TGA analysis using nickel powder that has not been subjected to post-treatment and nickel powder that has been subjected to post-treatment. [Figure 7] 1 is a structure of the metal powder-sintering inhibitor composite obtained by spray drying process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. Each embodiment of the present invention is provided to more completely explain the technical idea of ​​the present invention to those skilled in the art, and the following embodiments may be modified into various other forms, and the scope of the technical idea of ​​the present invention is not limited to the following embodiments. Rather, these embodiments are provided to make the present disclosure more complete and complete, and to fully convey the technical idea of ​​the present invention to those skilled in the art. The same reference numerals refer to the same elements throughout the specification. Furthermore, various elements and regions in the drawings are illustrated in schematic form. Therefore, the technical idea of ​​the present invention is not limited by the relative sizes and spacings shown in the accompanying drawings.

[0022] FIG. 1 shows a method for producing a metal powder-sintering inhibitor composite according to an embodiment of the present invention and then heat-treating a metal powder using the same.

[0023] Referring to step S1 of Fig. 1, a step of dissolving a sintering inhibitor in a solvent to form a sintering inhibitor solution is performed. The sintering inhibitor is a material that is dissolved in a solvent and then precipitated again in the spray drying step described below. The solvent may be water or an organic solvent.

[0024] The sintering inhibitor includes a metal salt. The metal salt is, for example, NiCl. 2 , BaCl 2 , metal chlorides such as NaCl and KCl.

[0025] The sintering inhibitor may further include a ceramic precursor together with the metal salt. The ceramic precursor is a material that is transformed into a ceramic by thermal decomposition during a subsequent heat treatment process. The ceramic includes metal oxides, metal nitrides, metal carbides, and composites thereof (e.g., metal oxynitrides, etc.). For example, metal oxides include aluminum oxide (Al 2 O 3 ) and barium titanium oxide (BaTiO 3 For example, aluminum nitrate (Al(NO 3 ) 3 ) and aluminum sulfate (Al 2 (SO 4 ) 3 ) as a precursor of barium titanium oxide, and barium nitrate (Ba(NO 3 ) 2 ) and titanium chloride (TiCl 4 ) as a precursor of magnesium oxide, and magnesium nitrate (Mg(NO 3 ) 2 ).

[0026] The sintering inhibitor dissolved in the solvent may be a metal salt. Alternatively, the metal salt and the ceramic precursor may be dissolved together. When the metal salt and the ceramic precursor are dissolved together in the solvent, the sintering inhibitor precipitated in the spray drying step is precipitated as a mixture in which the metal salt and the ceramic precursor are mixed together.

[0027] Referring to step S2 of FIG. 1, metal powder is added to the solution in which the sintering inhibitor is dissolved, and dispersed in the solution to prepare a metal powder dispersion.

[0028] The metal powder may include, for example, nickel powder, copper powder, silver powder, nickel-copper alloy powder, iron powder, and alloy powders thereof (e.g., nickel-copper alloy powder, iron-cobalt alloy powder, etc.), but is not limited thereto.

[0029] Referring to step S3 of Fig. 1, a metal powder-sintering inhibitor composite is manufactured by spray drying the metal powder dispersion. In the spray drying process, the metal powder dispersion is sprayed and atomized, and then dried using hot air to instantly evaporate the liquid phase, thereby obtaining a powder phase containing the metal powder and the sintering inhibitor (hereinafter, referred to as a metal powder-sintering inhibitor composite).

[0030] The structure of a metal powder-sintering inhibitor composite obtained by spray drying is shown in Figure 7. Referring to Figure 7, the metal powder-sintering inhibitor composite may have a structure in which a plurality of metal powders (metal particles) are dispersed and spaced apart from each other within the sintering inhibitor.

[0031] The sintering inhibitor is formed by precipitating a metal salt dissolved in a solution or a mixture of a metal salt and a ceramic precursor as a solid during the spray drying process. During the precipitation process, the sintering inhibitor is formed while covering the metal powder.

[0032] In some cases, the sintering inhibitor may contain ceramic formed as a result of transformation of some of the ceramic precursors during the spray drying process.

[0033] As shown in Fig. 7, in the metal powder-sintering inhibitor composite manufactured according to the embodiment of the present invention, the sintering inhibitor surrounds the metal powder, so that the metal powder is arranged at a physically separated distance. Therefore, even if the metal powder-sintering inhibitor composite is heat-treated at high temperature, the contact of the metal powder is blocked by the sintering inhibitor, so that the phenomenon of the metal powders coming into contact with each other during the heat treatment process and then sintering and agglomerating can be prevented.

[0034] Referring to step S4 of FIG. 1, after forming the metal powder-sintering inhibitor composite through the spray drying process, a step of heat treating the metal powder-sintering inhibitor composite may be performed.

[0035] The heat treatment is a heat treatment performed to improve or modify the properties of the metal powder. For example, in the case of nickel powder, the heat treatment may be performed to add sulfur to the surface or oxidize the surface in order to suppress sintering and shrinkage of the nickel powder during the MLCC manufacturing process. As another example, the heat treatment may be performed in a vacuum or inert atmosphere in order to improve the crystallinity of the nickel powder. As yet another example, the heat treatment may be performed in a desulfurization atmosphere in order to desulfurize the sulfur component added to the nickel powder again during the manufacturing process of the nickel powder by a chemical vapor phase method.

[0036] In addition, various atmospheres such as a reducing atmosphere, an oxidizing atmosphere, a vacuum atmosphere, an inert atmosphere, etc., may be used for modifying metal powders other than nickel powder.

[0037] During such heat treatment, the sintering inhibitor prevents sintering between the nickel powder particles.

[0038] Meanwhile, the sintering inhibitor formed by the spray drying process contains minute spaces inside through which gas can move. Therefore, when heat-treated in an oxygen or sulfur atmosphere, reactive gases such as oxygen gas or sulfur gas can reach the metal powder inside the sintering inhibitor through the sintering inhibitor.

[0039] When a ceramic precursor is included in the sintering inhibitor, the ceramic precursor may be converted to a ceramic during the heat treatment. In this case, when the heat treatment is completed, the sintering inhibitor of the metal powder-sintering inhibitor composite may contain the ceramic converted from the ceramic precursor together with the metal salt.

[0040] The ceramic formed by the transformation from the ceramic precursor serves to further improve the sintering prevention properties of the sintering inhibitor, and in some cases, the ceramic may remain on the surface of the metal powder even after the sintering inhibitor removal step described below, thereby affecting the properties of the metal powder.

[0041] For example, when the metal powder is nickel powder, aluminum oxide, magnesium oxide, barium titanium oxide, or a precursor of barium titanium oxide may remain on the surface of the nickel powder as ceramics. When ceramics remain on the surface of the nickel powder, it is possible to obtain an effect of suppressing abnormal growth of the nickel powder due to sintering at high temperatures when the nickel powder is used as an electrode for MLCC.

[0042] The heat treatment may have a section in which a predetermined temperature is maintained for a predetermined time depending on the purpose. When a ceramic precursor is included in the sintering inhibitor, the heat treatment temperature may be increased to a temperature higher than the thermal decomposition temperature of the ceramic precursor.

[0043] As another example, the heat treatment may be performed during a continuous temperature ramp, where a particular temperature is not maintained for a given time, but the ceramic precursor may transition to a ceramic during the ramp to the heat treatment temperature.

[0044] Referring to step S5 of FIG. 1, the metal powder-sintering inhibitor composite that has undergone the heat treatment step is subjected to a washing step to selectively remove the sintering inhibitor and recover the metal powder.

[0045] The sintering inhibitor can be removed by washing with a cleaning solution that can dissolve the sintering inhibitor. For example, if the sintering inhibitor is a water-soluble metal chloride such as NiCl 2 Or BaCl 2 In the case where the resin contains , these can be completely dissolved and removed by washing with water. Alternatively, an organic solvent or an acid / alkali solution can be used as the washing liquid.

[0046] Hereinafter, experimental results will be presented to facilitate understanding of the present invention. It should be understood that these experimental results are merely illustrative examples to facilitate understanding of the present invention, and that the present invention is not limited thereto.

[0047] First experiment

[0048] Metal powders include NiCl 2 and H 2 Nickel powder (average diameter 200 nm) produced by chemical vapor synthesis using as a raw material was used. Figure 2(a) shows the results of SEM observation of the produced nickel powder.

[0049] As a sintering inhibitor, the metal salt NiCl 2 and BaCl 2 NiCl was used. 2 and BaCl 2 207.6 g of each of the above was dissolved in 450 ml of water to prepare sintering inhibitor solutions. Nickel powder was added to each of the prepared sintering inhibitor solutions to prepare metal powder dispersions. The metal powder dispersions were spray-dried at 180°C to prepare metal powder-sintering inhibitor composites.

[0050] In Fig. 2(b) and (c), NiCl was used as a sintering inhibitor. 2 and BaCl 2 The results of SEM observation of a nickel particle-sintering inhibitor composite using NiCl2 are shown. 2 and BaCl 2 It can be confirmed that the sintering inhibitor is well dispersed in the specimen. When the components of the sintering inhibitor were analyzed using EDS (energy dispersive spectroscopy), Ni and Cl were detected in the test piece in Figure 2(b), and Ba and Cl were detected in the test piece in Figure 2(c), confirming that the sintering inhibitor was manufactured correctly.

[0051] The produced metal powder-sintering inhibitor composite was heated with hydrogen (H 2 ) or oxygen (O 2 After heat treatment in a 100% atmosphere, the metal powder was measured for sintering, grain size, and nickel oxide (NiO) content. Table 1 shows the types of test pieces used in the first experiment and the post-treatment experimental conditions.

[0052] [Table 1]

[0053] In Table 1, control groups 1 to 4 are nickel powders (hereinafter referred to as CVS nickel powders) that did not contain a sintering inhibitor and were heat-treated at different temperatures in a hydrogen atmosphere. The above treatments were carried out to confirm that the nickel powder is sintered by the temperature.

[0054] In experimental groups 1 to 4, the sintering inhibitor was BaCl 2 The nickel particle-sintering inhibitor composite was heat-treated at different temperatures in a hydrogen atmosphere, and the above treatment was carried out to increase the crystal grain size of the nickel powder while preventing agglomeration.

[0055] In experimental groups 5 and 6, the sintering inhibitor was NiCl 2 The nickel particle-sintering inhibitor composite was heat-treated at different temperatures in an oxygen atmosphere, and the above treatment was carried out to oxidize and heat-treat the nickel powder while preventing agglomeration.

[0056] The heat treatment was carried out by increasing the temperature from room temperature to the heat treatment temperature over a period of 40 minutes, maintaining the heat treatment temperature for 5 minutes, and then cooling the material in the furnace.

[0057] After the heat treatment, the nickel particles-sintering inhibitor of the control group and the experimental group were washed with water to remove all of the sintering inhibitor, and then the nickel powder was recovered.

[0058] Referring to Table 1, in the case of the control group, sintering between nickel powder particles did not occur at 300° C. because the temperature was too low, but sintering occurred at all temperatures higher than that.

[0059] Figure 3 shows the results of SEM observation of the state after heat treatment of Control Groups 1 to 4. Referring to Figure 3, it can be seen that sintering of the nickel powder actively occurs from 400°C onwards, and that sintering causes aggregation between particles and drastic changes in shape.

[0060] Referring to Table 1, it can be seen that no sintering occurred at any of the temperatures in Experimental Groups 1 to 4, and the grain size increased as the heat treatment temperature increased. The grain size was measured by X-ray diffraction.

[0061] Figure 4 shows the results of SEM observation of the state of the nickel powder before removing the sintering inhibitor after heat treatment (upper photograph) and the state of the nickel powder recovered after removing the sintering inhibitor (lower photograph) in experimental groups 3 and 4. As shown in Figure 4, in both experimental groups 3 and 4, the sintering inhibitor BaCl 2 This makes it possible to confirm that the nickel powder particles are prevented from coming into contact with each other and being sintered.

[0062] Referring to Table 1, it can be seen that in experimental groups 5 and 6, no sintering occurred at any temperature, and the crystal grain size of the nickel powder increased as the heat treatment temperature increased. In addition, the X-ray diffraction analysis confirmed that nickel oxide (NiO) was formed. This confirms that according to the technical idea of ​​the present invention, nickel oxide with high crystallinity can be formed on the surface of nickel particles at high temperatures while preventing sintering between metal powder particles.

[0063] Second experiment

[0064] Table 2 shows the types of test pieces and the corresponding experimental conditions in the second experiment. 2 207.6g and the aluminum oxide precursor Al(NO 3 ) 3 0.19g of CVS nickel powder was dissolved in 450ml of water to prepare a sintering inhibitor solution, and 5g of the CVS nickel powder used in the first experiment was added and dispersed in the solution. The metal powder dispersion was spray-dried at 180°C to prepare a nickel particle-sintering inhibitor composite. The sintering inhibitor was analyzed by EDS to detect Ba, Al, and Cl components, and therefore the sintering inhibitor was determined to be BaCl 2 and Al(NO 3 ) 3 It can be seen that it is a mixture of

[0065] [Table 2]

[0066] Next, this was placed in a heat treatment furnace and heat-treated in a hydrogen atmosphere at temperatures of 300° C., 400° C., and 500° C. The heat treatment conditions from heating to furnace cooling were the same as those in the first experiment.

[0067] The heat-treated nickel particle-sintering inhibitor composite test pieces of experimental groups 7 to 9 were analyzed by EDS, and Ba, Al, and Cl were detected in all test pieces. In addition, X-ray diffraction analysis revealed that aluminum oxide (Al 2 O 3 This is because Al(NO), which has a thermal decomposition temperature of about 200°C, was detected in the sintering inhibitor during the heat treatment process. 3 ) 3 This means that the sintering inhibitor in the nickel particle-sintering inhibitor composite after heat treatment is thermally decomposed at a temperature of 300°C or higher and converted to aluminum oxide. 2 and Al 2 O 3 The mixture is a mixture of Al(NO 3 ) 3 Calculating from the amount of Al in the sintering inhibitor, 2 O 3 It can be seen that the content is about 10 wt%.

[0068] After the heat treatment, the nickel particle-sintering inhibitor composites of experimental groups 7 to 9 were washed with water to remove the sintering inhibitor, and the nickel powder was then recovered. The recovered nickel powder was observed with an SEM, and it was confirmed that no sintering occurred in any of the nickel powders, regardless of the heat treatment temperature.

[0069] FIG. 5 shows the nickel powder recovered after the post-treatment corresponding to experimental group 9, i.e., the nickel particle-sintering inhibitor composite that had been heat-treated at 500°C was washed with water to remove all of the sintering inhibitor. The nickel powder was observed by SEM and analyzed by EDS.

[0070] 5, it can be seen that aluminum components are also detected in the recovered nickel powder, suggesting that aluminum oxide formed from the precursor during the heat treatment process is also formed on the surface of the nickel particles and remains on the surface of the nickel particles even after the sintering inhibitor is removed.

[0071] When high melting point aluminum oxide is formed on the nickel surface in this manner, the nickel powder has high resistance to sintering shrinkage during the MLCC manufacturing process, which means that the occurrence of problems due to sintering shrinkage is reduced.

[0072] Figure 6(a) shows the results of measuring the weight increase due to oxidation in air and the final oxidation end temperature for CVS nickel powder that had not undergone any post-treatment using TGA, while Figure 6(b) shows the results of TGA analysis using nickel powder recovered after post-treatment corresponding to experimental group 9.

[0073] 6(a) and 6(b), the oxidation end temperature for the CVS nickel powder that was not post-treated was 670°C, while the oxidation end temperature for the nickel powder recovered after post-treatment corresponding to experimental group 9 was 770°C, which was about 100°C higher. The higher the oxidation end temperature, the higher the sintering temperature in the firing process during the MLCC manufacturing process, which means higher resistance to sintering shrinkage.

[0074] It will be apparent to those having ordinary skill in the art to which the technical idea of ​​the present invention pertains that the technical idea of ​​the present invention described above is not limited to the above-mentioned embodiments and the accompanying drawings, and that various substitutions, modifications and alterations are possible within the scope not departing from the technical idea of ​​the present invention.

Claims

1. As a method for heat treating metal powder, providing a metal powder-sintering inhibitor composite including metal powders dispersed and spaced apart within a sintering inhibitor; and heat treating the metal powder-sintering inhibitor composite.

2. The method of claim 1 , wherein the sintering inhibitor comprises a metal salt.

3. The method of claim 2 , wherein the sintering inhibitor further comprises a ceramic precursor that is converted to a ceramic by heat.

4. The heat treatment step includes: The method of claim 3 , further comprising the step of transforming the ceramic precursor into a ceramic.

5. The method for producing the metal powder-sintering inhibitor composite includes the steps of: preparing a sintering inhibitor solution in which a sintering inhibitor is dissolved in a solvent; Adding metal powder to the sintering inhibitor solution and dispersing the metal powder to prepare a metal powder dispersion; and 10. The method of claim 1, further comprising the step of spray drying the dispersed particle dispersion.

6. The method of claim 1 , further comprising the step of removing the sintering inhibitor after the heat treating step.

7. 6. The method of claim 5, wherein the sintering inhibitor comprises a metal salt.

8. The method of claim 7 , wherein the sintering inhibitor further comprises a ceramic precursor that is converted to a ceramic by heat.

9. The method for heat treating a metal powder according to claim 1 or 5, wherein the metal powder includes at least one of nickel powder, copper powder, silver powder, iron powder, and alloy powder thereof.

10. The method of claim 1 or 7, wherein the metal salt comprises a metal chloride.

11. The metal chloride is NiCl 2 , BaCl 2 11. The method of claim 10, wherein the metal powder comprises NaCl and KCl.

12. The ceramic precursor is Al(NO 3 ) 3 , Al 2 (SO 4 ) 3 , (Ba(NO 3 ) 2 ), TiCl 4 and (Mg(NO 3 ) 2 9. The method of claim 3 or 8, further comprising the steps of:

13. The heat treatment step includes:

2. The method for heat treating metal powder according to claim 1, wherein the heat treatment is performed in an atmosphere including any one of a hydrogen atmosphere, an oxidizing atmosphere, a carbonizing atmosphere, a decarburizing atmosphere, a reducing atmosphere, an inert atmosphere, an air atmosphere, a sulfurizing atmosphere, a desulfurizing atmosphere, and a vacuum atmosphere.

14. The method further includes removing the sintering inhibitor and recovering the metal powder after the heat treatment step is completed, 4. The method of claim 3, wherein in the step of removing the sintering inhibitor, the ceramic transformed from the ceramic precursor remains on at least a portion of the surface of the recovered metal powder.

Citation Information

Patent Citations

  • Method for manufacturing nickel powder

    JP2004339601A