Dialkylphosphinic acid hybrid salts and their preparation and use
A dialkyl phosphinic acid hybrid salt with a specific composition addresses the limitations of dialkyl phosphinates by enhancing flame retardant efficiency, thermal stability, and reducing dust and particle size issues, ensuring uniform distribution and improved physical properties in polymeric materials.
Patent Information
- Application Number
- JP2024521762
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-04-19
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-04-19
AI Technical Summary
Existing dialkyl phosphinates used as flame retardants for polymeric materials suffer from low flame retardant efficiency, poor thermal stability, and issues with particle size and dust generation, leading to non-uniform distribution and poor physical properties, especially in high-temperature processing applications like nylon 66.
Development of a dialkyl phosphinic acid hybrid salt with a specific composition, characterized by a formula (I) where at least two acid salt ions of diethylphosphinate, ethylpropylphosphinate, and dipropylphosphinate pair with the same metal atom, offering improved thermal stability and larger particle size for uniform mixing, while maintaining high flame retardancy.
The dialkyl phosphinic acid hybrid salt achieves high flame retardant efficiency, excellent thermal stability, and reduces dust generation, enabling uniform distribution and improved physical properties in polymeric materials, particularly in high-temperature processing applications.
Smart Images

Figure 2024536907000021 
Figure 2024536907000022 
Figure 2024536907000023
Abstract
Description
[Technical field]
[0001] The present application relates to a dialkylphosphinic acid hybrid salt and its preparation method and use, which are in the field of producing flame-retardant polymeric materials. [Background technology]
[0002] Dialkyl phosphinate, especially aluminum diethyl phosphinate, is widely used as a halogen-free flame retardant for polymeric materials. Dialkyl phosphinate-based flame retardant products have low density, low flame retardant usage, and good mechanical properties, but existing dialkyl phosphinates have limited flame retardant efficiency as flame retardants. For example, dialkyl phosphinate can be used as a flame retardant without glass fiber reinforced nylon, but its flame retardant efficiency is low and it can have a significant adverse effect on the physical properties of flame retardant polymeric materials when used. There are also reports of using aluminum dipropyl phosphinate to make nylon 6 flame retardant. Although aluminum dipropyl phosphinate has high flame retardant efficiency, it has low thermal stability and begins to decompose and volatilize in large amounts at 300°C, which is disadvantageous for engineering plastics that require high-temperature processing, such as nylon 66.
[0003] In addition, when dialkylphosphinate is used as a flame retardant, in addition to the flame retardant properties, it is desirable to increase the particle size and density of the flame retardant during production and use in order to shorten the filtration time and reduce dust, and to avoid a situation in which the density difference becomes too large when mixed with a polymer material, causing the free flow velocities of the two to differ in the input tank, resulting in poor distribution uniformity of the flame retardant in the flame retardant material.
[0004] Therefore, obtaining a flame retardant with excellent flame retardancy, high thermal stability, and excellent processability has become a major challenge in the industry. Surprisingly, a dialkylphosphinic acid hybrid salt having a specific composition now satisfies the above requirements well. Summary of the Invention [Problem to be solved by the invention]
[0005] In order to solve the above technical problems, the present application provides a dialkylphosphinic acid hybrid salt having a composition of formula (I), which has a small amount of addition, a high flame retardant efficiency for various polymeric materials, excellent thermal stability, and can meet the processing requirements of engineering plastics that require high temperatures, and has large particles and little dust, as well as a preparation method thereof and use thereof. [Means for solving the problem]
[0006] According to a first aspect of the present application, there is provided a dialkylphosphinic acid hybrid salt, which is at least one selected from compounds having a chemical formula represented by formula (I): [ka] provided that M is a central atom, R, R1, and R2 are each independently selected from n-propyl and isopropyl, and the diethylphosphinate ion, the ethylpropylphosphinate ion, and the dipropylphosphinate ion are all ligands, and at least two of the diethylphosphinate ion, the ethylpropylphosphinate ion, and the dipropylphosphinate ion are paired with the same metal atom, and one of the ligands must be an ethylpropylphosphinate ion; M is selected from a metal element, and the metal element is at least one selected from the group consisting of group IIA, IIIA, IVA, and VA metal elements, transition metal elements, and lanthanide metal elements; n is the valence of the metal M, n being selected from 2, 3 or 4; 0≦x≦0.80, 0.05≦y≦0.7, 0≦z≦0.95, and x+y+z=1.
[0007] Specifically, the propyl in the ethylpropylphosphinate ion and the dipropylphosphinate ion is n-propyl or isopropyl.
[0008] In the embodiment of the present application, in formula (I), when x is greater than 0.80, the flame retardancy is not good. When z is greater than 0.95, the particles are small during production, the filtration is slow, there is a lot of dust during use, and the thermal stability is low, which is disadvantageous to the production and physical properties of the flame-retardant polymer material. When y is greater than 0.7, the production cost is high, the economic efficiency is poor, and the production and physical properties of the flame-retardant polymer material are disadvantageous.
[0009] Alternatively, the lower limit of x is independently selected from 0, 0.03, 0.05, 0.10, 0.15 and the upper limit is independently selected from 0.80, 0.75, 0.70, 0.65, 0.55, 0.50, 0.45, 0.40, 0.35, 0.30.
[0010] Alternatively, the lower limit of y is independently selected from 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40 and the upper limit is independently selected from 0.70, 0.65, 0.60, 0.55, 0.50, 0.45.
[0011] Alternatively, the lower limit of z is independently selected from 0, 0.001, 0.005, 0.01, 0.02, 0.05, 0.08 and the upper limit is independently selected from 0.95, 0.9, 0.85, 0.80, 0.75, 0.7, 0.65, 0.60, 0.55, 0.50, 0.45, 0.40, 0.35, 0.3, 0.25, 0.2, 0.15, 0.10.
[0012] Optionally, the Group IIA metal element is at least one selected from Be, Mg, Ca, Sr, Ba; The group IIIA metal element is Al; The Group IVA metal element is Sn; The VA group metal element is Sb; The transition metal element is at least one selected from Fe, Zn, Cu, Ti, Zr, and Mn, The lanthanide metal element is Ce.
[0013] Optionally, the metal element is at least one selected from Al, Zn, Ca, Fe.
[0014] Optionally, the metal element is Al and n=3.
[0015] Optionally, 0≦x≦0.80, 0.05≦y≦0.70, and 0.005≦z≦0.92.
[0016] Optionally, 0≦x≦0.66, 0.30≦y≦0.70, and 0.01≦z≦0.60.
[0017] Alternatively, 0≦x≦0.30, 0.35≦y<0.70, and 0.05≦z≦0.60.
[0018] In the examples of the present application, the larger the z value, the faster the thermal weight loss of the dialkylphosphinic acid hybrid salt.
[0019] The dialkylphosphinic acid hybrid salt in the present application is not a simple physical mixture of different dialkylphosphinic acid salts, for example, not a simple mixture of aluminum diethylphosphinate and aluminum ethylpropylphosphinate, but may contain at least two types of ions among diethylphosphinic acid salt ions, ethylpropylphosphinic acid salt ions, and dipropylphosphinic acid salt ions that pair with the same aluminum atom, and one of the ligands of the hybrid salt is an ethylpropylphosphinic acid salt ion. The X-ray diffraction spectrum (XRD) of these hybrid salts is very different from the XRD spectrum of a simple physical mixture salt of dialkylphosphinic acid salts. The dialkylphosphinic acid hybrid salt having the composition of formula (I) shows a single peak in the strongest absorption peak region in the XRD spectrum. In addition, the crystal plane spacing shown by the maximum peak is different from that of aluminum diethylphosphinic acid and aluminum dipropylphosphinic acid. The maximum peak of aluminum diethylphosphinate shows a crystal plane spacing d=9.663, and the maximum peak of aluminum dipropylphosphinate shows a crystal plane spacing d=11.079, while the value of the crystal plane spacing d of the dialkylphosphinic acid hybrid salt having formula (I) is substantially between the above two. However, a physically mixed salt obtained by simply mixing aluminum diethylphosphinate and aluminum dipropylphosphinate shows two completely independent peaks in the XRD spectrum, and the d values are close to the d values of aluminum diethylphosphinate and aluminum dipropylphosphinate, respectively.
[0020] In the examples of the present application, when the dialkylphosphinic acid hybrid salt having the composition of formula (I) and aluminum diethylphosphinate or aluminum dipropylphosphinate are simply physically mixed, two independent peaks appear in the most intense absorption peak region in the XRD spectrum. These results strongly indicate that the dialkylphosphinic acid hybrid salt having the composition of formula (I) obtained by the present invention is not a simple mixture of aluminum diethylphosphinate, aluminum ethylpropylphosphinate, and aluminum dipropylphosphinate, but contains a structure in which at least two acid salt ions of diethylphosphinic acid salt, ethylpropylphosphinic acid salt, and dipropylphosphinic acid salt are paired with the same aluminum atom.
[0021] In the examples of the present application, at the same usage amount, pure aluminum dipropylphosphinate has excellent flame retardancy, but has low thermal stability, making it difficult to meet the requirements of polymeric materials that require high-temperature processing. In addition, pure aluminum dipropylphosphinate has a lot of dust and is difficult to handle. In addition, pure aluminum dipropylphosphinate has fine particles, so when mixed with polymeric materials, local delamination is likely to occur, resulting in poor mixing uniformity. On the other hand, the dialkylphosphinic acid hybrid salt having the composition of formula (I) has high thermal stability, large particles, no dust, and the flow speed in the input tank is close to that of polymer particles, resulting in excellent mixing uniformity.
[0022] In the examples of the present application, at the same usage amount, pure diethylphosphinic acid salt had a low flame retardant effect, which was far below that of the dialkylphosphinic acid hybrid salt having the composition of formula (I).
[0023] According to a second aspect of the present application, there is provided a method for producing the above-mentioned dialkylphosphinic acid hybrid salt, the method comprising the steps of: A step of causing a reaction I in an aqueous phase of a material containing a mixture A and a metal element source M to obtain the dialkylphosphinic acid hybrid salt, The mixture A contains diethylphosphinic acid and / or an alkali metal salt thereof, ethylpropylphosphinic acid and / or an alkali metal salt thereof, and dipropylphosphinic acid and / or an alkali metal salt thereof.
[0024] Alternatively, the metal element is Al and the pH of Reaction I is 0-4, preferably 1-3.5, more preferably 2.3-3.3.
[0025] Specifically, in the above reaction I, if the pH is too low, no precipitation occurs, whereas if the pH is too high, hydroxides of metal ions are produced and impurities are introduced.
[0026] Alternatively, the molar ratio of the diethylphosphinic acid and / or its alkali metal salt, the ethylpropylphosphinic acid and / or its alkali metal salt, the dipropylphosphinic acid and / or its alkali metal salt, and the metal element source M is close to x:y:z:q, and the propyl is selected from n-propyl and isopropyl, where q=1 / n.
[0027] The solubility of the hybrid salt in water varies depending on the M. In the case of a hybrid salt with high solubility, the molar ratio with the M source also changes because there is a difference between the values of x, y, and z of diethylphosphinic acid and / or its alkali metal salts, ethylpropylphosphinic acid and / or its alkali metal salts, and dipropylphosphinic acid and / or its alkali metal salts in the solution and the values of x, y, and z in the hybrid salt. In addition, in order to obtain a larger amount of M-containing precipitate, the molar ratio of x, y, and z of the reactants to M may exceed the theoretically calculated value.
[0028] During actual operation, the actual values of x, y, z, and q can be determined by phosphorus nuclear magnetism.
[0029] Alternatively, the molar ratio of diethylphosphinic acid and / or an alkali metal salt thereof, ethylpropylphosphinic acid and / or an alkali metal salt thereof, and dipropylphosphinic acid and / or an alkali metal salt thereof in the mixture A is the same or substantially the same as the ratio of x, y, and z in formula (I).
[0030] Optionally, the conditions of reaction I are: temperature 0-250° C., pressure 0.1 MPa-10 MPa, time 0.1-20 h.
[0031] Optionally, obtaining the mixture A comprises: The method includes a step of introducing ethylene and propylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and carrying out reaction II to obtain the mixture A.
[0032] Optionally, the molar ratio of the phosphinic acid and / or its alkali metal salt to ethylene to propylene is 1:0.05-1.8:0.2-1.95.
[0033] In actual reactions, the amount of olefin consumed is higher than the theoretical ratio due to side reactions such as the formation of long-chain dialkylphosphinate salts obtained by polymerizing ethylene and / or propylene.
[0034] Alternatively, the molar ratio of the phosphinic acid and / or its alkali metal salt to ethylene and propylene is the same as or close to the ratio of x, y and z in formula (I). During the reaction of the phosphinic acid or its alkali metal salt with ethylene or propylene, the value of y has a maximum value smaller than 1, and after reaching this maximum value, x or z increases, so that y does not reach 1. If it is necessary to make y=1, it is necessary to separate and purify the reaction intermediate product to remove diethylphosphinic acid and / or dipropylphosphinic acid or their salts, which is economically disadvantageous.
[0035] Specifically, in reaction II, the order of addition of ethylene and propylene may be reversed, they may be added simultaneously, or one may be added partially in advance.
[0036] Alternatively, in reaction II, the phosphinic acid and / or its alkali metal salt is reacted with propylene to obtain the corresponding values of y and z, and then substantially completely or completely reacted with ethylene. By "substantially completely," it is meant that the total phosphorus contained in the ethylphosphinate, propylphosphinate, and phosphinate salts in the reaction mixture is less than 5% molar of the total phosphorus in the reaction mixture.
[0037] Optionally, the weight of the water in the aqueous solution is 10-99% of the total weight of the aqueous solution.
[0038] Specifically, if the aqueous solution contains too little water, the solubility of the olefin in water decreases due to a salting-out effect, slowing down the reaction rate, whereas if the aqueous solution contains too much water, the utilization rate of the reaction vessel decreases.
[0039] Optionally, the weight of water in the aqueous solution is 20-95% of the total weight of the aqueous solution.
[0040] Optionally, the weight of water in the aqueous solution is 45-92% of the total weight of the aqueous solution.
[0041] Optionally, the weight of water in the aqueous solution is 50-90% of the total weight of the aqueous solution.
[0042] Optionally, the weight of water in the aqueous solution is 55-90% of the total weight of the aqueous solution.
[0043] Optionally, the conditions of the reaction II are: temperature 0-250° C., time 0.01-50 h, and pressure 0-3 MPa.
[0044] Specifically, if the temperature of the reaction II is too low, the reaction rate is slow, whereas if the temperature is too high, the phosphinate is likely to decompose.
[0045] Optionally, the temperature of the reaction II is 10-200°C.
[0046] Specifically, the pressure of the reaction II is higher than 3 MPa, and the pressure required for the reaction apparatus is high, making the operation difficult.
[0047] Optionally, the pressure of the reaction II is 0.2-1.5 MPa.
[0048] Alternatively, the molar ratio of the radical initiator to the phosphinic acid and / or its alkali metal salt is 0.001-0.1:1.
[0049] Optionally, the radical initiator is at least one selected from azo-based initiators, peroxide-based initiators, and photoinitiators, wherein the amount of the radical initiator added can be determined according to practical needs.
[0050] Optionally, the azo initiator is selected from cationic and / or non-cationic azo initiators, including one or more of azodiisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-amidinopropane) dichloride, 2,2'-azodipropylamidino dihydrochloride.
[0051] Alternatively, the peroxide-based initiator is preferably an inorganic peroxide and an organic peroxide radical initiator, and particularly preferably one or more of hydrogen peroxide, ammonium persulfate, potassium persulfate, sodium persulfate, sodium percarbonate, benzoyl peroxide, di-tert-butyl peroxide, tert-butyl perbenzoate, and peracetic acid.
[0052] Preferably, the radical initiator is a peroxide-based initiator, and more preferably, the radical initiator is one selected from ammonium persulfate, potassium persulfate, and sodium persulfate.
[0053] Alternatively, the molar ratio of the radical initiator to the phosphinic acid and / or its alkali metal salt is 0.003-0.05:1.
[0054] Optionally, obtaining the mixture A comprises: The method includes a step of introducing propylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator to react with each other, and stopping the introduction of propylene and continuing the introduction of ethylene to react with each other after the molar ratio of the introduced propylene to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), thereby obtaining the mixture A.
[0055] Optionally, obtaining the mixture A comprises: The method includes the steps of introducing propylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and after the propylene reaction is complete or nearly complete, introducing ethylene to continue the reaction, thereby obtaining the mixture A.
[0056] Alternatively, the method includes reacting phosphinic acid and / or its alkali metal salt with propylene to obtain monopropylphosphinic acid or its alkali metal salt equal to or close to the value of y, controlling z to be equal to or less than 0.95, then stopping the addition of propylene and adding ethylene instead, continuing the reaction in the presence of an initiator, and then reacting with the required metal salt to obtain the flame retardant having the formula (I).
[0057] Optionally, obtaining the mixture A comprises: The method includes a step of introducing a part of propylene and ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator, reacting the propylene and ethylene, and stopping the introduction of the propylene after the molar ratio of the ethylene to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof becomes smaller than (2x+y) / 1 in formula (I) and the molar ratio of the propylene to be introduced to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), and continuing the introduction of the remaining ethylene to react the propylene and ethylene to obtain the mixture A.
[0058] Optionally, obtaining the mixture A comprises: The method includes the steps of introducing a portion of propylene and ethylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and after the portion of the propylene and ethylene has reacted completely or almost completely, introducing the remaining ethylene and continuing the reaction to obtain the mixture A, The molar ratio of the total amount of ethylene to the propylene is 0.026-9:1.
[0059] Optionally, obtaining the mixture A comprises: The method includes the steps of: introducing a portion of ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator; setting a molar ratio of the portion of ethylene to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof to not more than (2x+y) / 1 in formula (I); after the portion of ethylene has completely reacted, continuing the introduction of propylene to cause the reaction; and, after the molar ratio of the propylene to be introduced to the total phosphorus of the starting phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of propylene and continuing the introduction of the remaining ethylene to cause the reaction, thereby obtaining the mixture A.
[0060] Optionally, obtaining the mixture A comprises: The method includes the steps of: introducing a part of ethylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator; after the part of the ethylene is completely or almost completely reacted, introducing propylene to continue the reaction; and after the propylene is completely or almost completely reacted, introducing the remaining ethylene to continue the reaction, thereby obtaining the mixture A; The molar ratio of the total amount of ethylene to the propylene is 0.026-9:1.
[0061] Optionally, the metal element source M is at least one selected from metal element M salts.
[0062] Optionally, the metal element M salt is at least one selected from the group consisting of a nitrate, a sulfate, a hydrochloride, an acetate, and an oxide of the metal element M.
[0063] Alternatively, phosphinic acid and / or its alkali metal salt are reacted simultaneously with a portion of propylene and ethylene in the presence of a radical initiator, the amount of propylene and ethylene is controlled, and after the mole % of propylphosphinic acid or its alkali metal salt in the reaction system is close to the value of y, the mole % of dipropylphosphinic acid or its alkali metal salt is close to the value of z, and z is less than or equal to 0.95, the addition of propylene is stopped, the remaining ethylene is added, and the reaction is continued until completion in the presence of an initiator, and then reacted with the required metal salt to obtain a dialkylphosphinic acid hybrid salt having formula (I).
[0064] Optionally, obtaining the mixture A comprises: The method includes a step of introducing ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator, controlling the amount of ethylene, and stopping the introduction of ethylene after the molar ratio of the introduced ethylene to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes (y+2x) / 1 in formula (I), and further continuing the addition of propylene to continue the reaction in the presence of the initiator until completion, thereby obtaining the mixture A.
[0065] Specifically, after completion of reaction II, the next reaction may be carried out without separating diethylphosphinic acid, ethylpropylphosphinic acid, dipropylphosphinic acid or a mixture of alkali metals thereof.
[0066] According to a third aspect of the present application, there is further provided a flame retardant comprising at least one of the above dialkylphosphinic acid hybrid salts.
[0067] Optionally, the flame retardant further contains at least one selected from phosphate ions, phosphite ions, alkylphosphonate ions, and alkylphosphinate ions, the molar content of these phosphorus-containing acid salt ions in the flame retardant being 10% or less, and the number of moles of the flame retardant being calculated in terms of the number of moles of phosphorus element contained therein.
[0068] According to a fourth aspect of the present application, there is provided a flame retardant material comprising a flame retardant P and a thermoplastic polymeric material, The flame retardant P is at least one selected from the dialkylphosphinic acid hybrid salts and the flame retardants.
[0069] Optionally, the content of the flame retardant P in the flame retardant material is 1-35% by weight.
[0070] Optionally, the flame retardant material comprises 1-35 wt% of flame retardant P and 65-99 wt% of thermoplastic polymeric material.
[0071] The thermoplastic polymer material in this application refers to a plastic that has the property of softening when heated and hardening when cooled.
[0072] Specifically, the amount of the flame retardant P used depends on the thermoplastic polymer material.
[0073] Optionally, the content of the flame retardant P in the flame retardant material is 3-20% by mass.
[0074] Optionally, the flame retardant material further comprises a functional additive; The functional additive is at least one selected from a reinforcing agent, an anti-drip agent, a stabilizer, a pigment, a dye, a carbonization catalyst, a dispersant, a nucleating agent, an inorganic filler, and an antioxidant.
[0075] Optionally, the reinforcing agent is selected from glass fibers.
[0076] Optionally, the anti-drip agent is selected from Teflon.
[0077] Optionally, the inorganic filler is at least one selected from mica, calcium carbonate, calcium oxide, and silica.
[0078] Optionally, the content of the functional additive in the flame retardant material is 5-40% by weight.
[0079] Optionally, the flame retardant material further comprises a flame retardant Q; The flame retardant Q is at least one selected from a nitrogen-based flame retardant and a boron-based flame retardant.
[0080] Optionally, the nitrogen-based flame retardant is at least one selected from melamine cyanurate, melamine polyphosphate, and ammonium polyphosphate. The boron-based flame retardant is selected from zinc borates.
[0081] Optionally, the content of the flame retardant Q in the flame retardant material is 0.5-20% by mass.
[0082] Optionally, the thermoplastic polymeric material is at least one selected from polyamide and polyester.
[0083] Optionally, the polyamide is at least one selected from an aliphatic polyamide, an aromatic polyamide, a semi-aromatic polyamide, and a copolymer of a semi-aromatic polyamide and an aliphatic polyamide.
[0084] According to common knowledge in the art, polyamide, also called polyamide fiber or nylon, is a general term for polymers having -NH-C(O)-amide as a structural unit, and is synthesized by condensation or ring-opening reaction of one or more dicarboxylic acids with one or more diamines, and / or one or more amino acids, and / or one or more lactams. Polyamides are generally classified into aliphatic polyamides, aromatic polyamides, and semi-aromatic polyamides according to the main chain components. Semi-aromatic polyamides refer to those having an aromatic group in at least one monomer structure in the synthetic monomer.
[0085] Optionally, the aliphatic polyamide is a mixture of any one or more selected from a copolymer of polyamide 6 and polyamide 66, polyamide 6, and polyamide 66.
[0086] Alternatively, the semi-aromatic polyamide can be produced from any one or more aromatic dicarboxylic acids and any one or more aliphatic diamines, or from any one or more aromatic diamines and any one or more aliphatic dicarboxylic acids. Furthermore, one or more selected from dicarboxylic acids, diamines, lactams and amino acids can be added to the system to produce polyamide copolymers with corresponding properties. The added dicarboxylic acids are aromatic dicarboxylic acids and / or aliphatic dicarboxylic acids. The added diamines are aromatic diamines and / or aliphatic diamines. The added lactams can be aliphatic lactams or aromatic lactams. The added amino acids can be aromatic amino acids or aliphatic amino acids.
[0087] Optionally, the semi-aromatic polyamide is prepared from any one or more aromatic dicarboxylic acids selected from terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, and one or more aliphatic diamines selected from butylenediamine, hexadiamine, octanediamine, decanediamine, and 2-methylpentanediamine.
[0088] Optionally, the semi-aromatic polyamide is prepared from an aliphatic diamine, an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid.
[0089] Alternatively, the semi-aromatic polyamide may be prepared from an aliphatic diamine and an aromatic dicarboxylic acid, and optionally an aliphatic dicarboxylic acid may be added, and the molar percentage of the aliphatic dicarboxylic acid is 0-45% of the total dicarboxylic acid, i.e., moles of aliphatic dicarboxylic acid / (moles of aliphatic dicarboxylic acid+moles of aromatic dicarboxylic acid)=0-45%.
[0090] Optionally, the aromatic dicarboxylic acid is any one or more selected from terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, the aliphatic diamine is any one or more selected from butylenediamine, hexadiamine, octanediamine, decanediamine, and 2-methylpentanediamine, and the aliphatic dicarboxylic acid is any one or more selected from adipic acid, succinic acid, sebacic acid, and octanoic acid.
[0091] Optionally, the polyamide is selected from the group consisting of poly(hexamethylene terephthalate) (abbreviated as PA6T), polyhexamethylene isophthalamide (abbreviated as PA6I), terephthalic acid / hexadiamine / caprolactam copolymer (abbreviated as PA6T / 6), terephthalic acid / hexadiamine / adipic acid copolymer (abbreviated as PA6T / 66), terephthalic acid / hexadiamine / adipic acid / isophthalic acid copolymer (abbreviated as PA6T / 6I / 66), polynonamethylene terephthalamide (abbreviated as PA9T), polydecamethylene terephthalate (abbreviated as PA6T), polyhexamethylene isophthalamide (abbreviated as PA6I ... and any one or more selected from poly(dodecamethylene terephthalamide) (abbreviated as PA10T), poly(dodecamethylene terephthalamide) (abbreviated as PA12T), terephthalic acid / hexadiamine / laurolactam copolymer (abbreviated as PA6T / 12), polymetaxylylene adipamide (abbreviated as MXD6), terephthalic acid / hexadiamine / 2-methylpentanediamine copolymer (abbreviated as PA6T / 2-MPMDT), and terephthalic acid / 2,2,4-trimethylhexanediamine / 2,4,4-trimethylhexanediamine copolymer.
[0092] Optionally, the aliphatic polyamide is at least one selected from polyamide 6, polyamide 66, and a copolymer of polyamide 6 and polyamide 66.
[0093] Optionally, the semi-aromatic polyamide is selected from polyphthalamide (PPA).
[0094] Optionally, the polyester is selected from polybutylene terephthalate (PBT).
[0095] In the embodiment of the present application, the values of x, y and z in formula (I) are x+y+z=1 and x+z>0, without considering the amount of other phosphorus-containing impurities. The flame retardant having the composition of formula (I) may contain trace amounts of other phosphorus-containing ions. Due to impurities in the raw materials or impurities generated during the synthesis process, some trace amounts of phosphate ions, phosphite ions, alkyl phosphonate ions, and alkyl phosphinate ions may be present in the flame retardant. Oligomeric products of ethylene and propylene polymerization, such as ethyl n-butyl phosphinate ions, ethylhexyl phosphinate ions, butyl butyl phosphinate ions, butyl hexyl phosphinate ions, and propylhexyl phosphinate ions, also exist as impurities in the flame retardant having the composition of formula (I). However, as long as the total amount of these other phosphorus-containing acid salt ions does not exceed 5% mole of the total phosphorus, it will not affect the normal operation of the flame retardant having the composition of formula (I).
[0096] In the examples of the present application, the ratio of x, y and z in formula (I) is determined as follows after the flame retardant is decomposed by alkali or acid: 31 It can be determined by P-NMR (nuclear magnetism). Diethylphosphinate, ethyl n-propylphosphinate, ethyl isopropylphosphinate, di-n-propylphosphinate, and n-propyl isopropylphosphinate are different. 31 P chemical shift, 31The P-NMR spectrum shows five independent peaks, and the peak areas of the five peaks correspond to the molar concentrations of the five dialkylphosphinate ions, respectively. In some cases, long-chain dialkylphosphinate ions are present, but their amount is small, and their chemical shifts are close to the corresponding dialkylphosphinate ions, so that they are integrated and incorporated into the corresponding dialkylphosphinate ions. In this way, the values of x, y, and z can be easily calculated from the ratio of the peak areas. For example, the molar concentration of diethylphosphinate is x, the sum of the molar concentrations of ethyl n-propylphosphinate and ethyl isopropylphosphinate (abbreviated as ethylpropylphosphinate molar concentration) is y, and the sum of the molar concentrations of di-n-propylphosphinate and n-propylisopropylphosphinate (abbreviated as dipropylphosphinate molar concentration) is z, and the ratio of these three is the values of x, y, and z. Effect of the Invention
[0097] The beneficial effects that the present invention can achieve are as follows:
[0098] (1) The dialkylphosphinic acid hybrid salt having the composition of formula (I) according to the present invention has a small amount of addition, is easy to filter large particles, produces little dust, has high thermal stability, is highly efficient in rendering polymeric materials flame retardant, and is economical. It not only overcomes the disadvantages of diethylphosphinic acid salts, such as low flame retardancy for polymeric materials, but also overcomes the disadvantages of dipropylphosphinic acid salts, such as low thermal stability and high dust, and can be widely used in rendering polymeric materials flame retardant that require high-temperature processing.
[0099] (2) The method for producing a dialkylphosphinic acid hybrid salt according to the present invention avoids the drawback of having to produce different dialkylphosphinic acids separately, and uses water as a reaction solvent, which is environmentally friendly. The raw materials are easily available, and the method is economical. [Brief description of the drawings]
[0100] [Figure 1]FIG. 2 is a graph showing the thermal weight loss curves of dialkylphosphinic acid hybrid salts, aluminum diethylphosphinate, and aluminum dipropylphosphinate having different values of x, y, and z. [Figure 2a] 1 shows XRD curves of dialkylphosphinic acid hybrid salts, aluminum diethylphosphinate, and aluminum dipropylphosphinate having different values of x, y, and z. [Figure 2b] 2b is an XRD curve of a dialkylphosphinic acid hybrid salt, aluminum diethylphosphinate, and aluminum dipropylphosphinate having different values of x, y, and z, which is a partial enlargement of the strongest absorption peak in FIG. 2a. [Diagram 3] 3 is a 31P-NMR spectrum of the dialkylphosphinic acid hybrid salt of Example 7 after alkaline decomposition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0101] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0102] Unless otherwise stated, all materials in the examples herein were obtained commercially.
[0103] The raw materials used in the examples are as follows:
[0104] PA66 (also called polyamide 66 or nylon 66): Zytel 70G35 HSL NC010 from DuPont, USA, with a glass fiber content of 35% by mass.
[0105] PA6 (also called polyamide 6 or nylon 6): Zytel 73G30L NC010 from DuPont, USA, with a glass fiber content of 30% by mass.
[0106] ADP: aluminum diethylphosphinate, Exolit OP1230 from Clariant, Germany.
[0107] Antioxidant 1010: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], Shanghai MACKLIN Co., Ltd.
[0108] Antioxidant 168: Tris(2,4-di-tert-butylphenyl)phosphite, Strem Corporation, USA.
[0109] Composite antioxidant: Antioxidant 1010 (pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]) and Antioxidant 168 (tris(2,4-di-tert-butylphenyl)phosphite) mixed in a 1:1 mass ratio.
[0110] Flame test standard: GB / T 2408-2008 standard.
[0111] Nuclear magnetic resonance (NMR) test: The model number of the equipment used was AVANCE III 400MHz, Bruker, Germany.
[0112] Nuclear magnetic resonance phosphorus spectrum ( 31 P-NMR) test method: pre-delay D1=10 seconds, 32 scans, peak area ratio is the molar ratio of diethylphosphinic acid salt ion, ethylpropylphosphinic acid salt ion, and dipropylphosphinic acid salt ion.
[0113] X-ray diffraction (XRD) test: The model of the equipment used was D8 ADVANCED AVINCI, Bruker, Germany.
[0114] TGA thermogravimetry: The equipment used was model Q500, manufactured by TA, USA, in nitrogen atmosphere, with a heating rate of 10°C / min.
[0115] Particle size D50: Heloise-oasis HELOS (H3938), a laser particle size analyzer from Sympatek, Germany, dry test.
[0116] In the present application, R, R1, and R2 are any one selected from n-propyl and isopropyl, and two different propyls may be in the same unit structure represented by y or z. That is, in the same unit structure represented by y, R has both n-propyl and isopropyl, but in a specific embodiment, the value of R is not a unique value, so the specific value cannot be defined in detail. It is not necessary to define the required content of n-propyl and isopropyl for each unit structure represented by y or z, as long as the total amount meets the criteria. The applicant has provided a specific explanation in Table 1 as an example, for example, the subscript of the bis mixture structural formula corresponds to y, and includes bis mixture 1 (R = isopropyl) and bis mixture 2 (R = n-propyl).
[0117] [Example 1: Preparation of a hybrid salt having the composition of formula (I), where x=0, y=0.086, z=0.914, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated 0.75 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 9 hours, the introduction of propylene was stopped, and the introduction of ethylene was started. After 16 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0118] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 1.
[0119] [Table 1] Note: Bis-addition products: products in which two PH bonds on the phosphinate are added to an olefin double bond; Mono-addition products: products in which one PH bond on the phosphinate is added to an olefin double bond; Bis-mixture 1: ethyl isopropyl phosphinate ion (R = isopropyl); Bis-mixture 2: ethyl n-propyl phosphinate ion (R = n-propyl); Diethyl: diethyl phosphinate ion; Dipropyl: n-propyl isopropyl phosphinate ion (R1 ≠ R 2、 n-propyl and isopropyl, respectively) and di-n-propylphosphinate ion (R1 = R2 = n-propyl); monoethyl: monoethylphosphinate ion; monopropyl1: monoisopropylphosphinate ion; monopropyl2: mono-n-propylphosphinate ion; monoxide: the sum of ethylphosphinate ion and propylphosphinate ion. The same applies below.
[0120] A portion of the above solution (551.94 g, containing 0.6 moles of phosphorus) was slowly mixed with an aqueous solution containing 66.64 grams of aluminum sulfate octahydrate at a concentration of 10% by mass, and the reaction temperature was controlled at 70°C, the pH value was adjusted to 3.0 or less, and a large amount of precipitate was obtained. After the addition and mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 93 grams of a white solid. The sample was dissolved in an aqueous solution of sodium hydroxide, and phosphorus nuclear magnetic analysis was performed, which showed that the total amount of ethylpropylphosphinate ions was 8.6 mol%, the total amount of dipropylphosphinate ions was 91.0 mol%, and the total amount of propylphosphonate ions was 0.4%. Normalization gave x=0, y=0.086, and z=0.914.
[0121] The sample was subjected to particle size testing and found to be D 50 =53.71 μm.
[0122] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 11.109 Å (100%).
[0123] [Example 2: Preparation of a hybrid salt having the composition of formula (I), where x=0, y=0.192, z=0.808, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated 0.75 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 8.5 hours, the introduction of propylene was stopped and the introduction of ethylene was started. After 15.5 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0124] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 2.
[0125] [Table 2]
[0126] A portion of the above solution (559.8 g, containing 0.6 moles of phosphorus) was slowly mixed with 66.64 grams of an aqueous solution containing aluminum sulfate octahydrate at a concentration of 10% by mass, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, resulting in a large amount of precipitate. After the end of the mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 90 grams of white solid, with a yield of 98.4%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the total amount of dipropylphosphinate ions was 80.8 mol% and the total amount of ethylpropylphosphinate ions was 19.2 mol%. Therefore, x=0, y=0.192, and z=0.808.
[0127] The sample was subjected to particle size testing and found to be D 50 =24.66 μm.
[0128] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 11.024 Å (100%).
[0129] [Example 3: Preparation of a hybrid salt having the composition of formula (I), where x=0, y=0.412, z=0.588, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated about 0.70 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 6 hours, the introduction of propylene was stopped, and the introduction of ethylene was started, maintaining the pressure at 0.8 MPa. After 17.5 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0130] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 3.
[0131] [Table 3]
[0132] A portion of the above solution (559.94 g, containing 0.6 mol of phosphorus) was slowly mixed with an aqueous solution containing 66.64 g of aluminum sulfate octahydrate at a concentration of 10% by mass, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the end of the mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 87.3 g of a white solid, with a yield of 98%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the total amount of dipropylphosphinate ions was 58.3 mol%, the total amount of ethylpropylphosphinate ions was 40.9 mol%, and the remaining 0.8 mol% was other phosphorus-containing impurities, and the phosphorus-containing impurities included monopropylphosphinate ions, propylphosphonate ions, etc. Normalization gave x=0, y=0.412, and z=0.588.
[0133] The sample was subjected to particle size testing and found to be D 50 =27.69 μm.
[0134] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 10.841 Å (100%).
[0135] [Example 4: Preparation of a hybrid salt having the composition of formula (I), where x=0.033, y=0.610, z=0.357, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated about 0.70 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 5.5 hours, the introduction of propylene was stopped, and the introduction of ethylene was started, maintaining the pressure at 0.8 MPa. After 16 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0136] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 4.
[0137] [Table 4]
[0138] A portion of the above solution (536.33 g, containing 0.6 moles of phosphorus) was slowly mixed with 66.64 grams of an aqueous solution containing aluminum sulfate octahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the end of the mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 86.1 grams of white solid, with a yield of 98%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the diethylphosphinate ion was 3.3 mol%, the total dipropylphosphinate ion was 35.7 mol%, and the total ethylpropylphosphinate ion was 61.0 mol%, with x=0.033, y=0.610, and z=0.357.
[0139] The sample was subjected to particle size testing and found to be D 50 =29.98 μm.
[0140] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 10.750 Å (100%).
[0141] [Example 5: Preparation of a hybrid salt having the composition of formula (I), where x=0.082, y=0.694, z=0.224, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated about 0.70 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 5 hours, the introduction of propylene was stopped, and the introduction of ethylene was started, maintaining the pressure at 0.8 MPa. After 15 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0142] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 5.
[0143] [Table 5]
[0144] A portion of the above solution (548.44 g, containing 0.6 moles of phosphorus) was slowly mixed with 66.64 grams of an aqueous solution containing aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the addition and mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 84 grams of white solid, with a yield of 99%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the diethylphosphinate ion was 8.1 mol%, the total of dipropylphosphinate ion was 22.2 mol%, the total of ethylpropylphosphinate ion was 68.5 mol%, and the total of other phosphorus-containing impurities, such as monopropylphosphinate ion and propylphosphonate ion, was 1.3 mol%. After normalization, the results were x = 0.082, y = 0.694, and z = 0.224.
[0145] The sample was subjected to particle size testing and found to be D 50 =49.26 μm.
[0146] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 10.603 Å (100%).
[0147] [Example 6: Preparation of a hybrid salt having the composition of formula (I), where x=0.251, y=0.647, z=0.102, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated about 0.70 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 4.5 hours, the introduction of propylene was stopped, and the introduction of ethylene was started, maintaining the pressure at 0.8 MPa. After 15.5 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0148] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 6.
[0149] [Table 6]
[0150] A portion of the above solution (544.38 g, containing 0.6 moles of phosphorus) was slowly mixed with 66.64 grams of an aqueous solution containing aluminum sulfate octahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the end of the mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 80.4 grams of white solid, with a yield of 96%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the diethylphosphinate ion was 25.1 mol%, the total dipropylphosphinate ion was 10.2 mol%, and the total ethylpropylphosphinate ion was 64.7 mol%, with x=0.251, y=0.647, and z=0.102.
[0151] The sample was subjected to particle size testing and found to be D 50 =49.85 μm.
[0152] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 10.449 Å (100%).
[0153] [Example 7: Preparation of a hybrid salt having the composition of formula (I), where x=0.257, y=0.652, z=0.091, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated about 0.70 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 5 hours, the introduction of propylene was stopped, and the introduction of ethylene was started, maintaining the pressure at 0.8 MPa. After 15.5 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0154] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 7.
[0155] [Table 7]
[0156] A part of the above solution (471.95 g, containing 0.54 mol of phosphorus) was slowly mixed with 59.98 g of an aqueous solution containing aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the addition and mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 72 g of a white solid, with a yield of 96%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the diethylphosphinate ion was 25.7 mol%, the total of dipropylphosphinate ion was 9.1 mol%, the total of ethylpropylphosphinate ion and long-chain alkanediylphosphinate ion was 65.2 mol%, and x=0.257, y=0.652, and z=0.091.
[0157] The sample was subjected to particle size testing and found to be D 50 =62.31 μm.
[0158] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 10.350 Å (100%).
[0159] The hybrid salt obtained in this example was subjected to alkaline decomposition and then nuclear magnetic measurement. 31 The P-NMR (nuclear magnetic) spectrum is shown in FIG. 3. The peak areas of the six peaks correspond to the molar concentrations of the six phosphinates, respectively. Therefore, the values of x, y, and z can be easily calculated from the ratio of the peak areas. In the calculation, the peak area of the long-chain dialkylphosphinate ion and the peak area of the ethylpropylphosphinate ion were combined.
[0160] [Example 8: Preparation of a hybrid salt having the composition of formula (I), where x=0.544, y=0.436, z=0.020, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated about 0.70 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 5 hours, the introduction of propylene was stopped, and the introduction of ethylene was started, maintaining the pressure at 0.8 MPa. After 14.5 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0161] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 8.
[0162] [Table 8]
[0163] A part of the above solution (458.58 g, containing 0.54 moles of phosphorus) was slowly mixed with 59.98 g of an aqueous solution containing aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the end of the mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 56.3 grams of white solid, with a yield of 93%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the diethylphosphinate ion was 54.4 mol%, the total dipropylphosphinate ion was 2.0 mol%, and the total ethylpropylphosphinate ion was 43.6 mol%, with x=0.544, y=0.436, and z=0.020.
[0164] The sample was subjected to particle size testing and found to be D 50 =70.79 μm.
[0165] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 10.100 Å (100%).
[0166] [Example 9: Preparation of a hybrid salt having the composition of formula (I), where x=0.631, y=0.351, z=0.018, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated about 0.70 MPa. Then, a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the reactor, and the amount of olefin introduced was measured with a gas flow meter. After 3 hours, the introduction of propylene was stopped, and the introduction of ethylene was started, maintaining the pressure at 0.8 MPa. After 12 hours, the reactor pressure no longer decreased, so the temperature was lowered to release the pressure, and the reactor was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0167] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 9.
[0168] [Table 9]
[0169] A portion of the above solution (376.79 g, containing 0.45 mol of phosphorus) was slowly mixed with 49.98 g of an aqueous solution containing aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, resulting in a large amount of precipitate. After the addition and mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 56.3 g of a white solid, with a yield of 94%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that diethylphosphinate ions were 62.7 mol%, the total of dipropylphosphinate ions was 1.7 mol%, the total of ethylpropylphosphinate ions was 34.9 mol%, propylphosphonate ions were 0.4%, and other phosphorus-containing compounds were 0.3%. After normalization, the results were x = 0.631, y = 351, and z = 0.018.
[0170] The sample was subjected to particle size testing and found to be D 50 =79.96 μm.
[0171] XRD testing was performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 9.9988 Å (100%).
[0172] [Example 10: Preparation of a hybrid salt having the composition of formula (I), where x=0.764, y=0.231, z=0.005, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated about 0.50 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 3 hours, the introduction of propylene was stopped, and the introduction of ethylene was started, maintaining the pressure at 0.8 MPa. After 13.5 hours, the pressure in the vessel no longer decreased, so the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0173] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 10.
[0174] [Table 10]
[0175] A portion of the above solution (449.42 g, containing 0.54 moles of phosphorus) was slowly mixed with 59.98 g of an aqueous solution containing aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the end of the mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 68.1 grams of white solid, with a yield of 96%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the diethylphosphinate ion was 76.4 mol%, the total of dipropylphosphinate ion was 0.5 mol%, and the total of ethylpropylphosphinate ion was 23.1 mol%, with x=0.764, y=0.231, and z=0.005.
[0176] The sample was subjected to particle size testing and found to be D 50 =69.99 μm.
[0177] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 9.8537 Å (100%).
[0178] Example 11 (Comparative Example) Preparation of a hybrid salt having the composition of formula (I), where x=0.902, y=0.096, z=0.002, M=Al, and n=3. 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with ethylene until the pressure reached 0.8 MPa. The reaction liquid was heated to about 90°C, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, ethylene was continuously introduced into the reactor, and the amount of olefin introduced was measured with a gas flow meter. After 4.5 hours, the introduction of ethylene was stopped, and the introduction of propylene was started, maintaining the pressure at about 0.8 MPa. After 10.5 hours, the reactor pressure did not decrease, so the temperature was lowered to release the pressure, and the reactor was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0179] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 11.
[0180] [Table 11]
[0181] A part of the above solution (759.4 g, containing 0.93 moles of phosphorus) was slowly mixed with 103.29 g of an aqueous solution containing aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the end of the mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 116.6 g of a white solid, with a yield of 97%. The sample was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the diethylphosphinate ion was 90.2 mol%, the total dipropylphosphinate ion was 0.2 mol%, the total ethylpropylphosphinate ion was 9.6 mol%, and the values of x=0.902, y=0.096, and z=0.002.
[0182] The sample was subjected to particle size testing and found to be D 50 =80.56 μm.
[0183] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 9.7317 Å (100%).
[0184] Example 12 (Comparative Example) Preparation of a hybrid salt having the composition of formula (I), where x=0.969, y=0.031, z=0, M=Al, and n=3. 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with ethylene until the pressure reached 0.8 MPa. The reaction liquid was heated to about 90°C, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, ethylene was continuously introduced into the reactor, and the amount of olefin introduced was measured with a gas flow meter. After 6.5 hours, the introduction of ethylene was stopped, and the introduction of propylene was started, maintaining the pressure at about 0.8 MPa. After 9.5 hours, the reactor pressure did not decrease, so the temperature was lowered to release the pressure, and the reactor was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.
[0185] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 12.
[0186] [Table 12]
[0187] A portion of the above solution (751.4 g, containing 0.93 moles of phosphorus) was slowly mixed with 103.29 g of an aqueous solution containing aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the end of the mixing, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 115.2 grams of a white solid, with a yield of 97%. A small amount of the white solid was dissolved in an aqueous sodium hydroxide solution and subjected to nuclear magnetic analysis. The phosphorus spectrum showed that the diethylphosphinate ion was 96.3 mol%, the total of dipropylphosphinate ion was 0 mol%, the total of ethylpropylphosphinate ion was 3.1 mol%, and the propylphosphonate ion was 0.6 mol%. Normalization gave x=0.969, y=0.031, and z=0.
[0188] The sample was subjected to particle size testing and found to be D 50 =76.33μm.
[0189] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 9.6702 Å (100%).
[0190] The results of TGA tests on the dialkylphosphinic acid hybrid salts, aluminum dipropylphosphinate, and ADP obtained in Examples 1-12 are shown in Figure 1, which shows the thermal weight loss curves (TGA) of the hybrid salts, ADP, and aluminum dipropylphosphinate with different values of x, y, and z. As can be seen from the figure, the larger the z value, the lower the thermal stability of the hybrid salt, and the larger the x value, the higher the thermal stability.
[0191] Figure 2a is the XRD diagram of the dialkylphosphinic acid hybrid salt, aluminum dipropylphosphinate, ADP, and the physical mixed salt of aluminum dipropylphosphinate and ADP obtained in Examples 1-12. As can be seen from Figure 2b, the simple physical mixed salt has two independent peaks in the strongest absorption peak region in the XRD spectrum diagram, and their d values are close to the d values of aluminum diethylphosphinate and aluminum dipropylphosphinate, respectively, while the hybrid salt having the composition of formula (I) has only one peak or overlapping peaks, and the d value is substantially between the d value of aluminum diethylphosphinate and the d value of aluminum dipropylphosphinate. This shows that the dialkylphosphinic acid hybrid salt having the composition of formula (I) according to the present invention is not a simple mixture of aluminum diethylphosphinate, aluminum ethylpropylphosphinate, and aluminum dipropylphosphinate, but is a hybrid salt containing a structure in which at least two acid salt ions of diethylphosphinic acid salt, ethylpropylphosphinic acid salt, and dipropylphosphinic acid salt are paired with the same aluminum atom.
[0192] [Example 13] Polyamide PA66, the hybrid salt produced in Example 1, and the composite antioxidant were mixed in a mass ratio of 79.6:20:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, and maintained at 10 MPa for 5 minutes, and then cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94V-1.
[0193] [Example 14] Polyamide PA6, the hybrid salt produced in Example 1, and the composite antioxidant were mixed in a mass ratio of 79.6:20:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-1.
[0194] [Examples 15-51] For the hybrid salts prepared in Examples 1-10, samples were prepared and tested in polyamide PA66 and PA6 according to the methods of Examples 13 and 14, respectively. The results are shown in Tables 14, 15 and 16.
[0195] [Comparative Example 1 Aluminum dipropylphosphinate] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with propylene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated 0.8 MPa. Then, a 4% by mass aqueous solution of sodium persulfate was injected at a constant rate of 10 ml / h, propylene was continuously introduced into the reactor, and the amount of propylene introduced was measured with a gas flow meter. After 15.5 hours, the pressure in the system no longer decreased, so the reaction was stopped, the temperature was lowered to release the pressure, and the system was purged with N2 and discharged to obtain a transparent reaction liquid.
[0196] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 13.
[0197] [Table 13]
[0198] A portion of the above solution (525 g, containing 0.6 moles of phosphorus) was slowly mixed with an aqueous solution containing 66.64 g of aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, the pH value was adjusted to 3.0 or less, and a large amount of precipitate was obtained. After the addition and mixing were completed, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filtration was slow. The filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 92.8 g of a white solid, with a yield of 98%.
[0199] The sample was subjected to particle size testing and found to be D 50 =5.21 μm.
[0200] XRD tests were performed on the sample, and the corresponding layer spacing of the characteristic peak with the highest relative intensity measured by XRD was 11.079 Å (100%).
[0201] [Comparative Example 2 Aluminum diethylphosphinate] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel. The vessel was replaced twice with nitrogen gas, evacuated, and then filled with ethylene until the pressure reached 0.8 MPa. The reaction liquid was heated to about 90°C, and then a 4% by mass aqueous solution of sodium persulfate was injected at a constant rate of 10 ml / h, and ethylene was continuously introduced into the vessel. The amount of ethylene introduced was measured using a gas flow meter. After 8 hours, the pressure in the system did not decrease, so the reaction was stopped, the temperature was lowered to release the pressure, and the reaction liquid was purged with N2 and discharged to obtain a transparent reaction liquid. After the reaction was completed, a sample was taken and subjected to nuclear magnetic analysis. 31According to the P-NMR results, A portion of the above solution (190 g, containing 0.24 moles of phosphorus) was slowly mixed with 26.66 g of an aqueous solution containing aluminum sulfate octadecahydrate at a concentration of 10% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, to obtain a large amount of precipitate. After the addition and mixing were completed, the mixture was kept warm for 0.5 hours. The mixture was filtered while still hot, and the filtration was slow. The filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 29.8 g of a white solid, with a yield of 95.4%.
[0202] The sample was subjected to particle size testing and found to be D 50 =29.5 μm.
[0203] [Comparative Example 3] Polyamide PA66, aluminum dipropylphosphinate and composite antioxidant prepared in Comparative Example 1 were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and after 5 minutes, the mixture was removed, cooled and dried. It was then filled into a mold, preheated for 10 minutes in a press vulcanizer at 280°C, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, a sample was cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94V-0.
[0204] [Comparative Example 4] Polyamide PA66, aluminum dipropylphosphinate and composite antioxidant prepared in Comparative Example 1 were mixed in a mass ratio of 87.1:12.5:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and after 5 minutes, the mixture was removed, cooled and dried. It was then filled into a mold, preheated for 10 minutes in a press vulcanizer at 280°C, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardancy rating of the 1.6 mm sample was UL94 V-0.
[0205] [Comparative Example 5] Polyamide PA66, aluminum dipropylphosphinate and composite antioxidant prepared in Comparative Example 1 were mixed in a mass ratio of 89.6:10:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and after 5 minutes, the mixture was removed, cooled and dried. It was then filled into a mold, preheated for 10 minutes in a press vulcanizer at 280°C, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-1.
[0206] [Comparative Example 6] Polyamide PA6, aluminum dipropylphosphinate and composite antioxidant prepared in Comparative Example 1 were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and after 5 minutes, the mixture was removed, cooled and dried. It was then filled into a mold, preheated for 10 minutes in a press vulcanizer at 260°C, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL-94 V-1.
[0207] [Comparative Example 7] Polyamide PA66, aluminum diethylphosphinate and composite antioxidant prepared in Comparative Example 2 were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and after 5 minutes, the mixture was removed, cooled and dried. It was then filled into a mold, preheated for 10 minutes in a press vulcanizer at 280°C, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 non-rated.
[0208] [Comparative Example 8] Polyamide PA6, aluminum diethylphosphinate and composite antioxidant prepared in Comparative Example 2 were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and after 5 minutes, the mixture was removed, cooled and dried. It was then filled into a mold, preheated for 10 minutes in a press vulcanizer at 260°C, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL-94 unrated.
[0209] [Comparative Example 9] Polyamide PA66, ADP and complex antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and removed after 5 minutes, cooled and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 non-rated.
[0210] [Comparative Example 10] Polyamide PA6, ADP and complex antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and removed after 5 minutes, cooled and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL-94 unrated.
[0211] [Comparative Example 11] Polyamide PA66, the hybrid salt prepared in Example 11, and the composite antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 non-rated.
[0212] [Comparative Example 12] Polyamide PA6, the hybrid salt prepared in Example 11, and the composite antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL-94 unrated.
[0213] [Comparative Example 13] Polyamide PA66, the hybrid salt produced in Example 12, and the composite antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and after 5 minutes, the mixture was removed, cooled, and dried. It was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, maintained at 10 MPa for 5 minutes, and then cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 non-rated.
[0214] [Comparative Example 14] Polyamide PA6, the hybrid salt prepared in Example 12, and the composite antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL-94 unrated.
[0215] The test results of Comparative Example 3-14 are shown in Table 17.
[0216] [Table 14]
[0217] [Table 15]
[0218] [Table 16]
[0219] [Table 17] *: No NG grade
[0220] Examples 15-51 show that the flame retardant containing the dialkylphosphinic acid hybrid salt described in the present invention has excellent flame retardant efficiency for polyamide. When preparing flame retardant polyamide, there was no obvious dust in the operation. The prepared flame retardant PA66 sample had excellent toughness and no obvious decomposition. Comparative Example shows that under the same conditions, the particle size of the obtained aluminum dipropylphosphinate and aluminum diethylphosphinate is smaller than that of the hybrid salt, and the large particle size of the hybrid salt is unexpected. Comparative Example 3-6 shows that the dipropylphosphinic acid salt has a certain flame retardancy, but the flame retardant efficiency for polyamide is not as high as that of the hybrid salt having the structure of formula (I) described in the present invention, see Examples 17, 21, 22, 27, 30, 31, 34, 35, 40, 44 and 47. When preparing flame retardant polyamide, it was observed that the dust of the dipropylphosphinic acid salt was large and the operation environment was poor. Also, as can be seen from FIG. 1, the thermal stability is too low, and the flame-retardant PA66 produced is very brittle and decomposed seriously. Comparative Examples 7-10 show that pure aluminum diethylphosphinate has low flame-retardant efficiency for polyamide. Comparative Examples 11-14 show that when the proportion of diethylphosphinate in the hybrid salt having the structure of formula (I) is too high, i.e., x>0.8, the flame-retardant efficiency of the hybrid salt for polyamide is reduced.
[0221] The above are merely some embodiments of the present invention, and are not intended to limit the present invention in any way, and the present invention is disclosed in the above preferred embodiments, but they are not intended to limit the present invention. Those skilled in the art can make slight changes or modifications using the technical contents disclosed above without departing from the scope of the technical proposal of this application, which are equivalent to equivalent implementation examples and fall within the scope of the technical proposal.
[0222] (Additional Note) (Appendix 1) At least one compound selected from the group consisting of compounds having the chemical formula shown in formula (I): [ka] provided that M is a central atom, R, R1, and R2 are each independently selected from n-propyl and isopropyl, and the diethylphosphinate ion, the ethylpropylphosphinate ion, and the dipropylphosphinate ion are all ligands, and at least two of the diethylphosphinate ion, the ethylpropylphosphinate ion, and the dipropylphosphinate ion are paired with the same metal atom, and one of the ligands must be an ethylpropylphosphinate ion; M is selected from a metal element, and the metal element is at least one selected from the group consisting of group IIA, IIIA, IVA, and VA metal elements, transition metal elements, and lanthanide metal elements; n is the valence of the metal M, n being selected from 2, 3 or 4; A dialkylphosphinic acid hybrid salt, characterized in that 0≦x≦0.80, 0.05≦y≦0.7, 0≦z≦0.95, and x+y+z=1.
[0223] (Appendix 2) The Group IIA metal element is at least one selected from Be, Mg, Ca, Sr, and Ba; The group IIIA metal element is Al; The Group IVA metal element is Sn; The VA group metal element is Sb; The transition metal element is at least one selected from Fe, Zn, Cu, Ti, Zr, and Mn, The dialkylphosphinic acid hybrid salt according to claim 1, wherein the lanthanum-based metal element is Ce.
[0224] (Appendix 3) 0≦x≦0.80, 0.05≦y≦0.70, and 0.005≦z≦0.92; Preferably, 0≦x≦0.66, 0.30≦y≦0.70, and 0.01≦z≦0.60; Preferably, the dialkylphosphinic acid hybrid salt according to appendix 1 is characterized in that 0≦x≦0.30, 0.35≦y<0.70, and 0.05≦z≦0.60.
[0225] (Appendix 4) The dialkylphosphinic acid hybrid salt according to claim 1, wherein M=Al and n=3.
[0226] (Appendix 5) A step of causing a reaction I in an aqueous phase of a material containing a mixture A and a metal element source M to obtain the dialkylphosphinic acid hybrid salt, The method for producing a dialkylphosphinic acid hybrid salt according to any one of claims 1 to 4, wherein the mixture A contains diethylphosphinic acid and / or an alkali metal salt thereof, ethylpropylphosphinic acid and / or an alkali metal salt thereof, and dipropylphosphinic acid and / or an alkali metal salt thereof.
[0227] (Appendix 6) The mixture A is obtained by The method includes the steps of introducing ethylene and propylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and carrying out a reaction II to obtain the mixture A, Preferably, the mass of the water in the aqueous solution is 10-99% of the total mass of the aqueous solution; Preferably, the reaction conditions are: temperature 0-250° C., time 0.01-50 h, and pressure 0-3 MPa; Preferably, the molar ratio of the radical initiator to the total amount of the phosphinic acid and / or its alkali metal salt is 0.001-0.1:1; Preferably, the molar ratio of the phosphinic acid and / or its alkali metal salt to ethylene to propylene is 1:0.05-1.8:0.2-1.95; Preferably, the obtaining of the mixture A comprises: The method includes a step of introducing propylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator to react with each other, and after the molar ratio of the introduced propylene to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of propylene and continuing the introduction of ethylene to react with each other to obtain the mixture A, Preferably, the obtaining of the mixture A comprises: a step of introducing a part of propylene and ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator, reacting the propylene and ethylene so that the molar ratio of the ethylene to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof is smaller than (2x+y) / 1 in formula (I) and, after the molar ratio of the propylene introduced to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of the propylene and continuing the introduction of the remaining ethylene to react the propylene and the ethylene, thereby obtaining the mixture A; Preferably, the obtaining of the mixture A comprises: a step of introducing a part of ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator, making the molar ratio of the part of ethylene to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof equal to or less than (2x+y) / 1 in formula (I), and continuing the introduction of propylene to react after the part of ethylene has completely reacted, and stopping the introduction of propylene and continuing the introduction of the remaining ethylene to react after the molar ratio of the propylene to be introduced to the total phosphorus of the starting phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), thereby obtaining the mixture A; Preferably, the metal element source M is at least one selected from the group consisting of metal element M salts, Preferably, the salt of the metal element M is at least one selected from the group consisting of a nitrate, a sulfate, a hydrochloride, an acetate, and an oxide of the metal element M.
[0228] (Appendix 7) A flame retardant, which is at least one selected from the dialkylphosphinic acid hybrid salt according to any one of appendices 1 to 4 and the dialkylphosphinic acid hybrid salt produced by the method according to any one of appendices 5 and 6.
[0229] (Appendix 8) A flame retardant P and a thermoplastic polymeric material are included, The flame retardant material, wherein the flame retardant P is at least one selected from the flame retardants described in Appendix 7.
[0230] (Appendix 9) The flame-retardant material according to claim 8, wherein the content of the flame retardant P in the flame-retardant material is 1-35 mass %.
[0231] (Appendix 10) The flame retardant material further comprises a functional additive, The functional additive is at least one selected from a reinforcing agent, an anti-drip agent, a stabilizer, a pigment, a dye, a carbonization catalyst, a dispersant, a nucleating agent, an inorganic filler, and an antioxidant; Preferably, the content of the functional additive in the flame-retardant material is 5-40 mass %.
[0232] (Appendix 11) The flame retardant material further comprises a flame retardant Q; 11. The flame-retardant material according to claim 10, wherein the flame retardant Q is at least one selected from a nitrogen-based flame retardant and a boron-based flame retardant.
[0233] (Appendix 12) 12. The flame-retardant material according to claim 11, wherein the content of the flame retardant Q in the flame-retardant material is 0.5-20 mass %.
[0234] (Appendix 13) The flame-retardant material according to claim 8, wherein the thermoplastic polymer material is at least one selected from polyamide and polyester.
Claims
1. At least one compound selected from the group consisting of compounds having the chemical formula shown in formula (I): [Formula 1] where M is the central atom, and R, R 1 , R 2 are each independently selected from n-propyl and isopropyl, and the diethylphosphinate ion, the ethylpropylphosphinate ion, and the dipropylphosphinate ion are all ligands, and at least two of the diethylphosphinate ion, the ethylpropylphosphinate ion, and the dipropylphosphinate ion are paired with the same metal atom, and one of the ligands must be an ethylpropylphosphinate ion; M is selected from a metal element, and the metal element is at least one selected from the group consisting of metal elements of groups IIA, IIIA, IVA, and VA, transition metal elements, and lanthanide metal elements; n is the valence of the metal M, n being selected from 2, 3 or 4; A dialkylphosphinic acid hybrid salt, characterized in that 0≦x≦0.80, 0.05≦y≦0.7, 0≦z≦0.95, and x+y+z=1.
2. The Group IIA metal element is at least one selected from Be, Mg, Ca, Sr, and Ba; The Group IIIA metal element is Al; The Group IVA metal element is Sn; The VA group metal element is Sb; The transition metal element is at least one selected from Fe, Zn, Cu, Ti, Zr, and Mn, The dialkylphosphinic acid hybrid salt according to claim 1, wherein the lanthanum-based metal element is Ce.
3. 0≦x≦0.80, 0.05≦y≦0.70, and 0.005≦z≦0.92; Preferably, 0≦x≦0.66, 0.30≦y≦0.70, and 0.01≦z≦0.60; The dialkylphosphinic acid hybrid salt according to claim 1, characterized in that 0≦x≦0.30, 0.35≦y<0.70, and 0.05≦z≦0.60 are preferably satisfied.
4. 2. The dialkylphosphinic acid hybrid salt according to claim 1, wherein M=Al and n=3.
5. A step of causing a reaction I in an aqueous phase of a material containing a mixture A and a metal element source M to obtain the dialkylphosphinic acid hybrid salt, The method for producing a dialkylphosphinic acid hybrid salt according to any one of claims 1 to 4, characterized in that the mixture A contains diethylphosphinic acid and / or an alkali metal salt thereof, ethylpropylphosphinic acid and / or an alkali metal salt thereof, and dipropylphosphinic acid and / or an alkali metal salt thereof.
6. The mixture A is obtained by The method includes the steps of introducing ethylene and propylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and carrying out reaction II to obtain the mixture A; Preferably, the mass of the water in the aqueous solution is 10-99% of the total mass of the aqueous solution; Preferably, the conditions of the reaction II are a temperature of 0-250° C., a time of 0.01-50 h, and a pressure of 0-3 MPa; Preferably, the molar ratio of the radical initiator to the total amount of the phosphinic acid and / or its alkali metal salt is 0.001-0.1:1; Preferably, the molar ratio of the phosphinic acid and / or its alkali metal salt to ethylene to propylene is 1:0.05-1.8:0.2-1.95; Preferably, the obtaining of the mixture A comprises: The method includes a step of introducing propylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator to react with each other, and stopping the introduction of propylene and continuing the introduction of ethylene to react with each other after the molar ratio of the introduced propylene to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), thereby obtaining the mixture A, Preferably, the obtaining of the mixture A comprises: a step of introducing a part of propylene and ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator, reacting the propylene and ethylene so that a molar ratio of ethylene to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof is smaller than (2x+y) / 1 in formula (I) and, after the molar ratio of the propylene introduced to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of propylene and continuing the introduction of the remaining ethylene to react the propylene and ethylene, thereby obtaining the mixture A; Preferably, the obtaining of the mixture A comprises: a step of introducing a part of ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator, making the molar ratio of the part of ethylene to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof equal to or less than (2x+y) / 1 in formula (I), and continuing the introduction of propylene to react after the part of ethylene has completely reacted, stopping the introduction of propylene and continuing the introduction of the remaining ethylene to react after the molar ratio of the propylene to be introduced to the total phosphorus of the starting phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), thereby obtaining the mixture A; Preferably, the metal element source M is at least one selected from the group consisting of metal element M salts, The method according to claim 5, wherein the salt of the metal element M is at least one selected from the group consisting of a nitrate, a sulfate, a hydrochloride, an acetate, and an oxide of the metal element M.
7. A flame retardant, which is at least one selected from the dialkylphosphinic acid hybrid salt according to any one of claims 1 to 4 and the dialkylphosphinic acid hybrid salt produced by the method according to any one of claims 5 or 6.
8. comprising a flame retardant P and a thermoplastic polymeric material; 8. A flame-retardant material, characterized in that the flame retardant P is at least one selected from the flame retardants defined in claim 7.
9. The flame-retardant material according to claim 8, characterized in that the content of the flame retardant P in the flame-retardant material is 1-35 mass %.
10. The flame retardant material further comprises a functional additive, The functional additive is at least one selected from a reinforcing agent, an anti-drip agent, a stabilizer, a pigment, a dye, a carbonization catalyst, a dispersant, a nucleating agent, an inorganic filler, and an antioxidant; The flame-retardant material according to claim 8, wherein the content of the functional additive in the flame-retardant material is preferably 5-40% by mass.
11. The flame retardant material further comprises a flame retardant Q, 11. The flame-retardant material according to claim 10, wherein the flame retardant Q is at least one selected from a nitrogen-based flame retardant and a boron-based flame retardant.
12. The flame-retardant material according to claim 11, characterized in that the content of the flame retardant Q in the flame-retardant material is 0.5-20 mass %.
13. The flame retardant material according to claim 8, wherein the thermoplastic polymer material is at least one selected from polyamide and polyester.
Citation Information
Patent Citations
Dialkyl phosphinic acid salt and preparation method thereof
CN103073577A
Flame retardant ABS (Acrylonitrile Butadiene Styrene) and preparation method and product thereof
CN103113708A
Inflaming retarding acrylonitrile butadiene styrene (ABS) / copolyester alloy, preparation method thereof and product thereof
CN103146117A
Preparation method of aluminum diethylphosphinate
CN103772428A
Polydialkyl phosphinic acid metal composite salt and / or mixture thereof, and uses thereof
CN111825883A
Cited By
Dialkylphosphinic acid hybrid salts, method for preparing the same, and use thereof