Poly(arylene ether) resin composition, its method of manufacture and molded article containing same
A poly(arylene ether) resin composition with specific additives improves flame retardation and mechanical properties, addressing thermal runaway issues in electric vehicle batteries.
Patent Information
- Application Number
- JP2024505648
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-06
- Filing Date
- 2023-07-11
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-07-11
AI Technical Summary
Poly(arylene ether) resins used in electric vehicle batteries face challenges with insufficient flame retardation properties during thermal runaway, which can lead to fires, and existing flame retardants compromise mechanical properties.
A poly(arylene ether) resin composition incorporating 12 to 17 parts by weight of two organic phosphorus flame retardants with different phosphorus contents, 10 to 40 parts by weight of glass fiber, 0.5 to 5 parts by weight of ground mica, and 1 to 4 parts by weight of alkaline earth metal sulfate with a specific particle size, enhancing flame retardation and mechanical properties.
The composition achieves excellent mechanical properties, heat resistance, and flame retardation during thermal runaway, ensuring safety and stability in electric vehicle battery components.
Smart Images

Figure 2024536971000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0110704 filed on September 1, 2022 and Korean Patent Application No. 10-2023-0087697 refiled on July 6, 2023 based thereon, and all contents disclosed in the documents of the Korean patent application are incorporated as part of this specification.
[0002] The present invention relates to a poly(arylene ether) resin composition, a production method thereof, and a molded article containing the same. More specifically, the present invention relates to a poly(arylene ether) resin composition which has excellent mechanical properties such as impact strength, tensile strength, and flexural strength, heat resistance, and flame retardancy, and is also excellent in flame retardancy during thermal runaway, thereby ensuring safety, a production method thereof, and a molded article containing the same. [Background technology]
[0003] Poly(arylene ether) resins are thermoplastics that possess high glass transition temperatures, high dimensional stability, low specific gravity, hydrolytic stability and good mechanical performance.
[0004] However, poly(arylene ether) resins have the disadvantage of poor molding characteristics due to the need for high processing temperatures when used alone. For this reason, they are used in the form of a mixture with rubber-reinforced polystyrene containing rubber, which is an aromatic vinyl polymer. In particular, polyphenylene ether resins containing rubber-reinforced polystyrene have compatibility in all ranges regardless of their respective contents, so that they have the characteristic of complementing each other's properties, and have excellent mechanical properties, so they are widely used in various industrial fields such as products used under high heat, for example, automobile parts, electric and electronic parts, and building materials. In addition, in some applications requiring even better flexural modulus and flexural strength, poly(arylene ether) resins are used reinforced with glass fibers.
[0005] However, molded products made from the resin composition have excellent physical properties such as impact strength, tensile strength, appearance, and heat resistance, but generally have the drawback of being flammable. In particular, when used as a part of an electric vehicle battery, flame retardancy during thermal runaway is required for safety reasons in addition to flame retardancy. Thermal runaway, which is the main cause of fires in electric vehicle batteries, is a phenomenon in which heat is generated when stress is applied to the battery cell due to various reasons. When the internal temperature of the battery rises above a certain level due to a short circuit such as overvoltage or overdischarge, a flame occurs, but lithium-ion batteries are highly reactive with water and therefore cannot easily be extinguished with water in the event of a fire.
[0006] In order to improve this, a halogen-based compound and an antimony-based compound are applied together to a poly(arylene ether) resin composition containing a poly(arylene ether) resin to impart flame retardancy and flame retardant properties. As the halogen-based compound, polybromodiphenyl ether, tetrabromobisphenol A, bromine-substituted epoxy compounds, chlorinated polyethylene, etc. are mainly used. As the antimony-based compound, antimony trioxide and antimony pentoxide are mainly used. The method of imparting flame retardancy by applying both a halogen and an antimony compound has the advantage that it is easy to ensure flame retardancy and there is almost no deterioration in physical properties, but the flame retardant properties are insufficient and the hydrogen halide gas generated during processing is likely to have a fatal effect on the human body. Flame retardants that do not use halogens are named non-halogen flame retardants, and the most widely used non-halogen flame retardants are phosphorus-based flame retardants containing phosphorus. However, since phosphorus-based flame retardants have significantly inferior flame retardancy compared to halogen-containing flame retardants, in order to obtain excellent flame retardancy and flame retardancy properties, a large amount of phosphorus-based flame retardants must be added, which has the disadvantage of deteriorating the physical properties of the resin composition.
[0007] Although the above-mentioned methods can impart flame retardancy to the resin composition, there are problems in that the flame retardancy required to suppress thermal runaway in electric vehicle batteries is insufficient and the mechanical properties are deteriorated.
[0008] Therefore, there is a need to develop a resin composition that has excellent mechanical properties, heat resistance, and flame retardancy, as well as excellent flame retardancy during thermal runaway, and thus can meet the quality requirements for electrical components such as electric vehicle batteries. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 2-187456 Summary of the Invention [Problem to be solved by the invention]
[0010] In order to solve the problems of the prior art as described above, the present disclosure aims to provide a poly(arylene ether) resin composition that has excellent mechanical properties such as impact strength, tensile strength, and bending strength, heat resistance, and flame retardancy, and also has excellent flame retardancy during thermal runaway, thereby ensuring safety.
[0011] Another object of the present disclosure is to provide a method for producing the poly(arylene ether) resin composition.
[0012] The present disclosure also provides molded articles made from the poly(arylene ether) resin compositions.
[0013] The above and other objects of the present disclosure can all be achieved by the disclosure as set forth below. [Means for solving the problem]
[0014] In order to achieve the above object, the present disclosure provides a poly(arylene ether) resin composition comprising: (a-1) 100 parts by weight of a base resin containing 75 to 95% by weight of a poly(arylene ether) resin and (a-2) 5 to 25% by weight of a polystyrene resin; (b) 12 to 17 parts by weight of two or more organic phosphorus-based flame retardants having different phosphorus contents; (c) 10 to 40 parts by weight of glass fiber; (d) 0.5 to 5 parts by weight of pulverized mica; and (e) 1 to 4 parts by weight of an alkaline earth metal sulfate having an average particle size of 0.05 to 3 μm.
[0015] II) In the above I), the (a-1) poly(arylene ether) resin may preferably have an intrinsic viscosity of 0.2 to 0.8 dl / g.
[0016] III) In the above I) or II), the (a-2) polystyrene resin may preferably be general purpose polystyrene, high-impact polystyrene, or a mixture thereof.
[0017] IV) In the above I) to III), the (b) two or more organic phosphorus-based flame retardants having different phosphorus contents can preferably include (b-1) an organic phosphorus-based flame retardant having a phosphorus content of 5 to 15% by weight, and (b-2) an organic phosphorus-based flame retardant having a phosphorus content of 20 to 35% by weight.
[0018] V) In the above I) to IV), the weight ratio (b-1:b-2) of the organophosphorus flame retardant (b-1) to the organophosphorus flame retardant (b-2) may preferably be 6:4 to 8.5:1.5.
[0019] VI) In the above I) to V), the (b-1) organophosphorus flame retardant having a phosphorus content of 5 to 15% by weight may preferably be one or more selected from the group consisting of bisphenol-A-bis(diphenyl phosphate) (BPADP), triphenyl phosphate (TPP), and resorcinol bis diphenyl phosphate (RDP).
[0020] VII) In the above I) to VI), the (b-2) organophosphorus flame retardant having a phosphorus content of 20 to 35% by weight may preferably be one or more selected from the group consisting of a dialkylphosphinate represented by the following chemical formula 3, a diphosphinate represented by the following chemical formula 4, and a polymer of any one or more of these.
[0021] [ka]
[0022] [ka]
[0023] (In the above Chemical Formula 3 and Chemical Formula 4, R 1 , R 2 , R 3 and R 4 are each independently a linear or branched C1-C 10 Alkyl, C1-C 10 or H; R 5 is a linear or branched C1-C 10 Alkylene, C6-C 10 Arylene, C7-C 20 or C7-C 20 M1 is an aryl alkylene; m+ and M2 m'+are each independently a nitrogen base compound (nitrogen-based compound) in which one or more atoms selected from the group consisting of Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, and K are cationized, protonated, or cationized and protonated; m is an integer of 1 to 4; n is an integer of 1 to 4; and x is an integer of 1 to 4.
[0024] VIII) In the above I) to VII), the (c) glass fibers may preferably have an average particle size of 3 to 25 μm and an average length of 1 to 15 mm.
[0025] IX) In the above I) to VIII), the (d) pulverized mica may preferably have an average particle size of 50 to 150 μm.
[0026] X) In the above I) to IX), the poly(arylene ether) resin composition may have a flame endurance time of 500 seconds or more, measured as the time required for applying a flame of a size (125 mm (500 W)) specified in ASTM D5207 to an injection test piece of 100 mm × 100 mm × 1 mm in accordance with the UL94 5V test until a hole or drip occurs in the test piece.
[0027] XI) In the above I) to X), the poly(arylene ether) resin composition preferably has a notched Izod impact strength of 7.7 kJ / m, as measured using a 4 mm thick notched test piece in accordance with ISO 180A. 2 It may be more than that.
[0028] XII) In the above I) to XI), the poly(arylene ether) resin composition may preferably have a heat distortion temperature of 120°C or higher, measured on a 4 mm-thick test piece under a stress of 1.8 MPa in accordance with ISO 75-2.
[0029] XIII) In the above I) to XII), the poly(arylene ether) resin composition may preferably contain one or more selected from the group consisting of a lubricant, an antioxidant, a compatibilizer, and an impact modifier.
[0030] The present disclosure also provides XIV) a method for producing a poly(arylene ether) resin composition, comprising a step of kneading and extruding 100 parts by weight of a base resin containing (a-1) 75 to 95 weight % of a poly(arylene ether) resin and (a-2) 5 to 25 weight % of a polystyrene resin, (b) 12 to 17 parts by weight of two or more organic phosphorus-based flame retardants having different phosphorus contents, (c) 10 to 40 parts by weight of glass fiber, (d) 0.5 to 5 parts by weight of pulverized mica, and (e) 1 to 4 parts by weight of an alkaline earth metal sulfate having an average particle size of 0.05 to 3 μm, wherein the kneading and extrusion are performed using an extruder having 9 or more kneading blocks.
[0031] The present disclosure also provides XV) a molded article comprising the poly(arylene ether) resin composition according to any one of I) to XIII). Effect of the Invention
[0032] According to the present invention, there are provided a poly(arylene ether) resin composition which has excellent mechanical properties such as impact strength, tensile strength, and bending strength, as well as excellent heat resistance and flame retardancy, and which has excellent flame retardancy during thermal runaway and can therefore be used with high quality in electrical components such as battery components for electric vehicles, a production method thereof, and a molded product containing the same.
[0033] In addition, the poly(arylene ether) resin composition of the present invention has excellent flame retardancy and excellent mechanical properties, thereby ensuring safety, and has the effect of providing a poly(arylene ether) resin composition that can minimize deformation due to vibration or impact of an automobile, and deterioration of physical properties due to changes in temperature and humidity, a manufacturing method thereof, and a molded product containing the same. [Brief description of the drawings]
[0034] [Figure 1] FIG. 1 is a schematic diagram of an extruder equipped with nine or more kneading blocks for producing the poly(arylene ether) resin composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] The poly(arylene ether) resin composition according to the present invention, its production method and molded articles containing the same are described in detail below.
[0036] The present inventors have confirmed that a poly(arylene ether) resin composition having excellent mechanical properties such as impact strength, tensile strength, and flexural strength, heat resistance, and flame retardancy as well as significantly improved flame retardancy during thermal runaway can be provided when a base resin containing predetermined contents of poly(arylene ether) resin and polystyrene resin is combined with predetermined contents of two or more organic phosphorus-based flame retardants having different phosphorus contents, glass fiber, pulverized mica, and an alkaline earth metal sulfate having a predetermined average particle size. Based on this, the present inventors have further pursued research and completed the present invention.
[0037] The poly(arylene ether) resin composition according to the present disclosure is described in detail below.
[0038] The poly(arylene ether) resin composition according to the present invention is characterized by comprising: (a-1) 100 parts by weight of a base resin containing 75 to 95% by weight of a poly(arylene ether) resin and (a-2) 5 to 25% by weight of a polystyrene resin; (b) 12 to 17 parts by weight of two or more organic phosphorus-based flame retardants having different phosphorus contents; (c) 10 to 40 parts by weight of glass fiber; (d) 0.5 to 5 parts by weight of pulverized mica; and (e) 1 to 4 parts by weight of an alkaline earth metal sulfate having an average particle size of 0.05 to 3 μm. In this case, the composition has the advantages of being excellent in mechanical properties such as impact strength, tensile strength, and flexural strength, heat resistance, flame retardancy, and flame retardancy during thermal runaway.
[0039] Hereinafter, the poly(arylene ether) resin composition of the present invention will be described in detail with respect to each component.
[0040] (a-1) Poly(arylene ether) resin The (a-1) poly(arylene ether) resin may be, for example, 75 to 95% by weight, preferably 75 to 90% by weight, more preferably 77 to 87% by weight, and even more preferably 77 to 82% by weight, based on 100 parts by weight of the total base resin. Within this range, the mechanical properties, heat resistance, and flame retardancy are excellent, and the flame retardancy during thermal runaway is excellent, thereby ensuring safety.
[0041] In this description, thermal runaway refers to a condition in which a change in temperature causes the environment to change in such a way that the change in temperature is accelerated, i.e., a mechanical process is caused by an increase in temperature, but the energy released as a result of the process increases the temperature, accelerating the process.
[0042] The (a-1) poly(arylene ether) resin may be, for example, a homopolymer or copolymer containing a unit of the following Chemical Formula 1 or Chemical Formula 2.
[0043] [ka]
[0044] [ka]
[0045] The R1, R2, R3, R4, R'1, R'2, R'3, and R'4 are substituents of an arylene group (Ar) or a phenylene group, each independently or simultaneously being hydrogen, chlorine, bromine, iodine, alkyl, allyl, phenyl, alkylbenzyl, chloroalkyl, bromoalkyl, cyanoalkyl, cyano, alkoxy, phenoxy, or a nitro group, where Ar is an arylene group having 7 to 20 carbon atoms, and the alkoxy may be an alkoxy having 1 to 4 carbon atoms.
[0046] Preferably, R1, R2, R3, R4, R'1, R'2, R'3, and R'4 are substituents of an arylene group (Ar) or a phenylene group, each independently or simultaneously being hydrogen, chlorine, bromine, iodine, methyl, ethyl, propyl, allyl, phenyl, methylbenzyl, chloromethyl, bromomethyl, cyanoethyl, cyano, methoxy, phenoxy, or a nitro group, and Ar is an arylene group having 7 to 20 carbon atoms.
[0047] Examples of the homopolymer of the poly(arylene ether) resin (a-1) include poly(2,6-dimethyl-1,4-phenylene) ether, poly(2,6-diethyl-1,4-phenylene) ether, poly(2-methyl-6-propyl-1,4-phenylene) ether, poly(2,6-dipropyl-1,4-phenylene) ether, poly(2-ethyl-6-propyl-1,4-phenylene) ether, and poly(2,6-dimethoxy-1,4-phenylene) ether. The poly(2,6-dichloromethyl-1,4-phenylene) ether may be one or more selected from the group consisting of poly(2,6-dibromomethyl-1,4-phenylene) ether, poly(2,6-diphenyl-1,4-phenylene) ether, poly(2,6-diphenyl-1,4-phenylene) ether, and poly(2,5-dimethyl-1,4-phenylene) ether. In this case, the poly(2,6-dichloromethyl-1,4-phenylene) ether may be one or more selected from the group consisting of poly(2,6-dichloromethyl-1,4-phenylene) ether, poly(2,6-dibromomethyl-1,4-phenylene) ether, poly(2,6-diphenyl-1,4-phenylene) ether, and poly(2,5-dimethyl-1,4-phenylene) ether. In this case, the poly(2,6-dichloromethyl-1,4-phenylene) ether may be one or more selected from the group consisting of ...bromomethyl-1,4-phenylene) ether, poly(2,6-diphenyl-1,4-phenylene) ether, and poly(2,5-dimethyl-1,4-phenylene) ether.
[0048] In addition, the poly(arylene ether) resin copolymer may be, for example, one or more selected from the group consisting of a copolymer of 2,6-dimethylphenol and 2,3,6-trimethylphenol, a copolymer of 2,6-dimethylphenol and o-cresol, and a copolymer of 2,3,6-trimethylphenol and o-cresol. In this case, the copolymer has excellent mechanical properties such as impact strength and tensile strength, and is also excellent in processability, thereby providing the advantage of improved appearance quality.
[0049] The (a-1) poly(arylene ether) resin may preferably be a polyphenylene ether resin.
[0050] The (a-1) poly(arylene ether) resin may have, for example, a weight average molecular weight of 10,000 to 100,000 g / mol, preferably 10,000 to 70,000 g / mol, and more preferably 15,000 to 45,000 g / mol. Within this range, the resin has the effect of exhibiting excellent processability and balance of physical properties.
[0051] In this description, unless otherwise specified, the weight average molecular weight can be measured using GPC (Gel Permeation Chromatography, water breeze). As a specific example, the weight average molecular weight can be measured as a relative value to a standard PS (standard polystyrene) sample through GPC using chloroform as an eluent. In this case, as a specific measurement example, the measurement can be performed under the following conditions: solvent: chloroform, column temperature: 40°C, flow rate: 0.3 ml / min, sample concentration: 20 mg / ml, injection amount: 5 μl, column model: 1×PLgel 10 μm MiniMix-B (250×4.6 mm) + 1×PLgel 10 μm MiniMix-B (250×4.6 mm) + 1×PLgel 10 μm MiniMix-B Guard (50×4.6 mm), equipment name: Agilent 1200 series system, refractive index detector: Agilent G1362 RID, RI temperature: 35°C, data processing: Agilent ChemStation S / W, test method (Mn, Mw and PDI): OECD TG 118.
[0052] The (a-1) poly(arylene ether) resin may have an intrinsic viscosity of, for example, 0.2 to 0.8 dl / g, preferably 0.3 to 0.6 dl / g, and more preferably 0.35 to 0.5 dl / g. Within this range, the composition can have high mechanical properties such as impact strength and tensile strength while also having a fluidity suitable for molding, and has excellent compatibility with polystyrene resins.
[0053] In this description, unless otherwise specified, the intrinsic viscosity is a value measured at 25° C. using an Ubbelohde viscometer after dissolving a sample to be measured in a chloroform solvent at a concentration of 0.5 g / dl.
[0054] The (a-1) poly(arylene ether) resin may preferably be in the form of a flake or powder. In this case, it has the effect of being excellent in mechanical properties such as impact strength and tensile strength, as well as excellent processability and appearance quality.
[0055] In this description, the term "flake" refers to a thin flake shape broadly including a scale-like shape and a granular shape, and as a specific example, the flake may be a flake shape having a thickness of 1 to 20 μm and a length of 0.05 to 1 mm. As another example, the flake may be a flake shape having a ratio of length to depth (L / D) of 1.5 to 500, preferably 2 to 100, and more preferably 10 to 50.
[0056] The flakes described herein can be produced by conventional flake production methods in the art.
[0057] In this description, the thickness and length of the flakes can be measured through microscopic analysis.
[0058] The powder form can be produced by a conventional powder production method known in the art.
[0059] (a-2) Polystyrene resin The (a-2) polystyrene resin may be, for example, 5 to 25% by weight, preferably 10 to 25% by weight, more preferably 13 to 23% by weight, and even more preferably 18 to 23% by weight, based on 100 parts by weight of the base resin. Within this range, the effect of excellent mechanical properties such as impact strength, tensile strength, and flexural strength is achieved.
[0060] The (a-2) polystyrene resin may be, for example, a general purpose polystyrene resin, a high-impact polystyrene resin, or a mixture thereof, and preferably a high-impact polystyrene resin. In this case, it has the effect of being excellent in processability, dimensional stability, and tensile strength.
[0061] The general-purpose polystyrene resin may be, for example, a polymer obtained by polymerizing styrene alone, and in this case, it has an effect of being excellent in processability.
[0062] The high impact polystyrene resin may be, for example, a rubber-reinforced polystyrene resin.
[0063] The rubber may be, for example, one or more selected from the group consisting of butadiene rubbers, isoprene rubbers, butadiene-styrene copolymers, and alkyl acrylate rubbers, and is preferably butadiene rubber, which has the advantage of improving impact strength.
[0064] As an example, the rubber may be 3 to 25% by weight, preferably 6 to 14% by weight, and more preferably 8 to 12% by weight, relative to 100% by weight of the high-impact polystyrene resin. Within this range, the effect of excellent impact strength and fluidity is achieved.
[0065] The rubber may have a volume average particle diameter of, for example, 0.1 to 20 μm, preferably 1.0 to 15 μm, and within this range, the rubber has the effect of being excellent in impact strength and flowability.
[0066] The rubber-reinforced polystyrene resin may be at least one selected from the group consisting of high impact styrene-butadiene copolymer (HIPS), styrene-butadiene-styrene copolymer (SBS), styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-butadiene copolymer (SB), styrene-isoprene copolymer (SI), styrene-isoprene-styrene copolymer (SIS), α-methylstyrene-butadiene copolymer, styrene-ethylene-propylene copolymer, styrene-ethylene-propylene-styrene copolymer, and styrene-(ethylene-butylene / styrene copolymer)-styrene copolymer.
[0067] The rubber-reinforced polystyrene resin may be prepared by, for example, bulk polymerization, suspension polymerization, emulsion polymerization, or a mixture thereof of rubber and an aromatic vinyl compound. The polymerization may be performed by thermal polymerization or in the presence of a polymerization initiator. The polymerization initiator usable in the polymerization may be, for example, a peroxide-based initiator, an azo-based initiator, or a mixture thereof. The peroxide-based initiator may be preferably one or more selected from the group consisting of benzoyl peroxide, t-butyl hydroperoxide, acetyl peroxide, and cumene hydroperoxide, and the azo-based initiator may be preferably azobisisobutyronitrile.
[0068] In this description, the volume average particle size can be measured by dissolving 3 g of high impact polystyrene resin in 100 ml of methyl ethyl ketone using a Coulter Counter LS230 instrument, and then measuring the rubber particles that are dispersed in a particulate form and not dissolved by a laser scattering method.
[0069] The (a-2) polystyrene resin may have a flow index of, for example, 2 to 20 g / 10 min, preferably 3 to 15 g / 10 min, measured at 200° C. under 5 kg in accordance with ASTM D1238. Within this range, the resin has the effect of being excellent in processability and balance of physical properties.
[0070] (b) Two or more organophosphorus flame retardants with different phosphorus contents The (b) two or more organic phosphorus-based flame retardants having different phosphorus contents may be, for example, 12 to 17 parts by weight, preferably 12.5 to 16 parts by weight, and more preferably 12.7 to 15.5 parts by weight, based on 100 parts by weight of the base resin. In this case, the effect of having excellent flame retardancy and excellent mechanical properties is achieved.
[0071] The (b) two or more organic phosphorus-based flame retardants having different phosphorus contents may, for example, include (b-1) an organic phosphorus-based flame retardant having a phosphorus content of 5 to 15% by weight, and (b-2) an organic phosphorus-based flame retardant having a phosphorus content of 20 to 35% by weight, and preferably (b-1) an organic phosphorus-based flame retardant having a phosphorus content of 7 to 12% by weight, and (b-2) an organic phosphorus-based flame retardant having a phosphorus content of 22 to 30% by weight. In this case, while reducing the amount of flame retardant used, there are effects such as better flame retardancy, excellent flame retardancy during thermal runaway, and excellent impact resistance.
[0072] In this description, the phosphorus content means the weight % of phosphorus calculated from the molecular weight of phosphorus contained in the molecular structure of the organophosphorus flame retardant.
[0073] The weight ratio (b-1:b-2) of the (b-1) organic phosphorus-based flame retardant and the (b-2) organic phosphorus-based flame retardant may be, for example, 6:4 to 8.5:1.5, preferably 7:3 to 8:2, and more preferably 7.5:2.5 to 8:2. Within this range, there is an effect that the flame retardancy, the flame retardancy characteristics during thermal runaway, and the mechanical properties are further improved.
[0074] The (b-1) organophosphorus flame retardant having a phosphorus content of 5 to 15% by weight may be, for example, one or more selected from the group consisting of bisphenol-A-bis(diphenyl phosphate) (BPADP), triphenyl phosphate (TPP), and resorcinol bis diphenyl phosphate (RDP), and may be preferably bisphenol-A-bis(diphenyl phosphate). In this case, there is an effect that high flame retardancy can be imparted with a small amount while maintaining mechanical properties.
[0075] The (b-2) organic phosphorus-based flame retardant having a phosphorus content of 20 to 35% by weight may be, for example, at least one selected from the group consisting of dialkylphosphinate represented by the following chemical formula 3, diphosphinate represented by the following chemical formula 4, and polymers of at least one of these. In this case, high flame retardancy can be achieved with a small amount of flame retardant while maintaining mechanical properties, and there is an effect of excellent flame retardancy.
[0076] [ka]
[0077] [ka]
[0078] (In the above Chemical Formula 3 and Chemical Formula 4, R 1 , R 2 , R 3 and R 4 are each independently a linear or branched C1-C 10 Alkyl, C1-C 10 or H; R 5 is a linear or branched C1-C 10 Alkylene, C6-C 10 Arylene, C7-C20 or C7-C 20 M1 is an aryl alkylene; m+ and M2 m'+ are each independently a nitrogen base compound in which one or more atoms selected from the group consisting of Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, and K are cationized, protonated, or cationized and protonated; m is an integer of 1 to 4; n is an integer of 1 to 4; and x is an integer of 1 to 4.
[0079] In the above formulas 3 and 4, cycloalkyl may be independently preferably cyclohexyl or cyclohexadimethyl.
[0080] R 1 , R 2 , R 3 and R 4 may preferably each independently be methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl or phenyl.
[0081] R 5 may preferably be methylene, ethylene, n-propylene, isopropylene, n-butylene, tert-butylene, n-pentylene, n-octylene, n-dodecylene, phenylene, naphthylene, methylphenylene, ethylphenylene, tert-butylphenylene, methylnaphthylene, ethylnaphthylene, tert-butylnaphthylene, phenylmethylene, phenylethylene, phenylpropylene or phenylbutylene.
[0082] M1 m+ and M2 m'+ may each preferably be independently one or more selected from the group consisting of Mg, Ca, Al, Ti and Zn.
[0083] R 1 and R 2 , and R3 and R 4 can be bonded to each other to form a ring with the adjacent phosphorus atom. 1 and R 2 , and R 3 and R 4 are bonded to each other to form a ring together with the adjacent phosphorus atom, which is a heterocycle having the phosphorus atom as a heteroatom constituting the ring, and the number of atoms constituting such a ring may be, for example, 4 to 20, preferably 5 to 16. The heterocycle having a phosphorus atom may be a bicyclo ring or may have a substituent.
[0084] The dialkylphosphinate represented by Chemical Formula 3 may be preferably one or more selected from the group consisting of calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, magnesium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, calcium methylphenylphosphinate, magnesium methylphenylphosphinate, aluminum methylphenylphosphinate, zinc methylphenylphosphinate, calcium diphenylphosphinate, magnesium diphenylphosphinate, aluminum diphenylphosphinate, and zinc diphenylphosphinate.
[0085] The diphosphinate represented by Chemical Formula 4 may be at least one selected from the group consisting of calcium methylene bis(methylphosphinate), magnesium methylene bis(methylphosphinate), aluminum methylene bis(methylphosphinate), zinc methylene bis(methylphosphinate), calcium 1,4-phenylene bis(methylphosphinate), magnesium 1,4-phenylene bis(methylphosphinate), aluminum 1,4-phenylene bis(methylphosphinate), and zinc 1,4-phenylene bis(methylphosphinate).
[0086] The (b-2) organic phosphorus flame retardant may more preferably be one or more selected from the group consisting of calcium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, aluminum diethylphosphinate, and zinc diethylphosphinate, and may further preferably be aluminum diethylphosphinate. In this case, high flame retardancy can be achieved with a small amount of flame retardant while maintaining mechanical properties, and there is an effect of excellent flame retardancy.
[0087] The (b-2) organophosphorus flame retardant may have, for example, an average particle size of 0.1 to 100 μm, preferably 0.5 to 50 μm, and more preferably 1 to 40 μm. Within this range, there is an advantage in that the flame retardancy and mechanical properties are excellent.
[0088] In this description, the average particle size of an organophosphorus flame retardant means a number-average particle size determined from the frequency distribution of particle size and particle number measured using a laser diffraction particle size distribution analyzer, using a dispersion of an organophosphorus flame retardant dispersed in a medium such as water as a measurement sample.
[0089] The (b-1) organic phosphorus-based flame retardant having a phosphorus content of 5 to 15% by weight may be preferably bisphenol A bis(diphenyl phosphate), and the (b-2) organic phosphorus-based flame retardant having a phosphorus content of 20 to 35% by weight may be preferably aluminum diethyl phosphinate. In this case, there is a synergistic effect in which excellent flame retardancy is exhibited even with a small amount of flame retardant.
[0090] (c) Glass fiber The (c) glass fiber may be, for example, 10 to 40 parts by weight, preferably 15 to 35 parts by weight, and more preferably 20 to 30 parts by weight, based on 100 parts by weight of the base resin. Within this range, there are advantages in that the mechanical properties are excellent, as well as the heat resistance, flame retardancy, and flame retardancy during thermal runaway, and the appearance properties of the final product are excellent.
[0091] The (c) glass fiber may have an average particle size of, for example, 3 to 25 μm, preferably 5 to 20 μm, and more preferably 7 to 15 μm. Within this range, the mechanical strength with the resin is improved, and the appearance characteristics of the final product are excellent.
[0092] The (c) glass fiber may have an average length of, for example, 1 to 15 mm, preferably 2 to 10 mm, and more preferably 3 to 6 mm. Within this range, the mechanical strength with the resin is improved, and the appearance characteristics of the final product are excellent.
[0093] The (c) glass fiber may be, for example, chopped glass fiber, which has the advantage of excellent compatibility.
[0094] In the present description, the chopped glass fiber is not particularly limited as long as it is a chopped fiber glass commonly used in the technical field to which the present invention pertains.
[0095] The (c) glass fiber may have, for example, an aspect ratio (L / D), which is the ratio of the average length (L) to the average diameter (D), of 200 to 550, preferably 220 to 450, more preferably 250 to 350, and even more preferably 270 to 320. Within this range, the glass fiber has excellent compatibility with resins, and thus has the advantage of excellent surface appearance.
[0096] In this description, the average particle size, average length, aspect ratio, etc. of glass fibers are calculated by averaging 30 pieces measured by microscopic analysis.
[0097] The (c) glass fiber may be, for example, surface-treated with a silane-based compound or a urethane-based compound, and preferably, surface-treated with one or more surface treatment agents selected from the group consisting of aminosilane-based compounds, epoxysilane-based compounds, and urethane-based compounds. More preferably, the glass fiber is surface-treated with an aminosilane-based compound. In this case, a chemical bond is formed with the poly(arylene ether) resin to improve dispersibility and surface wettability, and as a result, there is an effect that the mechanical properties of the resin composition, including the tensile strength, are improved.
[0098] The surface treatment agent may be contained in an amount of, for example, 0.1 to 10% by weight, preferably 0.1 to 5% by weight, more preferably 0.1 to 3% by weight, even more preferably 0.1 to 0.8% by weight, and even more preferably 0.2 to 0.5% by weight, relative to 100% by weight of the total of the surface-treated glass fiber (glass fiber + surface treatment agent). Within this range, there is an effect of excellent mechanical properties, balance of physical properties, and appearance of the final product.
[0099] The aminosilane compound is not particularly limited as long as it is an aminosilane that is generally used as a coating agent for glass fibers. For example, it may be one or more selected from the group consisting of γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, 3-mercaptopropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-isocyanatepropyltriethoxysilane, γ-acetoacetatepropyltrimethoxysilane, γ-acetoacetatepropyltriethoxysilane, γ-cyanoacetyltrimethoxysilane, γ-cyanoacetyltriethoxysilane, and acetoxyacetotrimethoxysilane. In this case, there is an effect that the surface properties of the extruded product are excellent while having excellent mechanical properties and heat resistance.
[0100] The epoxy silane compound is not particularly limited as long as it is an epoxy silane that is generally used as a coating agent for glass fibers. For example, the epoxy silane compound may be at least one selected from the group consisting of 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropyl(dimethoxy)methylsilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. In this case, the epoxy silane compound has an effect of providing excellent surface properties of the extruded product while providing excellent mechanical properties and heat resistance.
[0101] The (c) glass fiber may be appropriately selected from the range of ordinary use in the art as long as it complies with the definition of the present invention, and the cross-sectional shape, such as cylindrical or elliptical, is not particularly limited.
[0102] (d) Crushed mica The (d) pulverized mica may be, for example, 0.5 to 5 parts by weight, preferably 0.7 to 4 parts by weight, more preferably 1 to 3.5 parts by weight, and even more preferably 1 to 3 parts by weight, based on 100 parts by weight of the base resin. Within this range, the effect of excellent mechanical properties, heat resistance, flame retardancy, and flame retardancy during thermal runaway is achieved.
[0103] For purposes of this description, crushed mica may be defined as mica that has been crushed one or more times to an average particle size of 500 μm or less.
[0104] The (d) pulverized mica may have an average particle size of, for example, 50 to 150 μm, preferably 70 to 130 μm, and more preferably 80 to 110 μm. Within this range, the compatibility with resins is excellent, and therefore mechanical properties, heat resistance, flame retardancy, and flame retardancy during thermal runaway are all improved, resulting in excellent appearance quality of molded articles.
[0105] The (d) pulverized mica may have, for example, an aspect ratio of 40 to 60, preferably 45 to 55. Within this range, there is an effect that the appearance quality of the molded article is excellent.
[0106] In this description, the aspect ratio of crushed mica refers to the ratio of the major to minor axis lengths in a two-dimensional model.
[0107] In this description, the average particle size, average length, and aspect ratio of pulverized mica are calculated by averaging 30 particles measured by microscopic analysis.
[0108] (e) Sulfates of alkaline earth metals with an average particle size of 0.05 to 3 μm The (e) alkaline earth metal sulfate having an average particle size of 0.05 to 3 μm may be, for example, 1 to 4 parts by weight, preferably 1.2 to 3.8 parts by weight, and more preferably 1.4 to 3.6 parts by weight, based on 100 parts by weight of the base resin. Within this range, the flame retardancy during thermal runaway is improved while the impact resistance is excellent.
[0109] The (e) alkaline earth metal sulfate may have an average particle size of, for example, 0.05 to 3 μm, preferably 0.1 to 2.5 μm, more preferably 0.5 to 2 μm, and even more preferably 0.7 to 1.5 μm. Within this range, the compatibility is excellent, and therefore, there is an effect of improving mechanical properties, heat resistance, flame retardancy, and flame retardancy during thermal runaway.
[0110] The alkaline earth metal of the (e) alkaline earth metal sulfate is, for example, one or more elements selected from the group consisting of elements in Group II of the periodic table, preferably one or more elements selected from the group consisting of calcium, barium, strontium, and magnesium, more preferably calcium, barium, or a mixture thereof, and even more preferably barium, in which case there is an effect of improving mechanical properties.
[0111] As a preferred example, the (e) alkaline earth metal sulfate may be barium sulfate, in which case there is an effect of improving mechanical properties.
[0112] The (e) alkaline earth metal sulfate may be contained in an amount greater than that of the (d) ground mica, and in this case, the mechanical properties such as tensile strength, flexural strength, and impact strength, and heat resistance are more excellent.
[0113] Poly(arylene ether) resin composition The poly(arylene ether) resin composition may have a flame endurance time of 500 seconds or more, more preferably 550 seconds or more, and even more preferably 600 seconds or more, as measured by applying a flame of 125 mm (500 W) as specified in ASTM D5207 to an injection test piece of 100 mm × 100 mm × 1 mm in accordance with the UL94 5V test until a hole or drip occurs in the test piece. Within this range, the composition has an excellent balance of physical properties and excellent flame retardancy during thermal runaway of electrical components such as battery components for electric vehicles, thereby ensuring safety.
[0114] The poly(arylene ether) resin composition preferably has a notched Izod impact strength of 7.7 kJ / m, measured at room temperature using a 4 mm thick notched test piece in accordance with ISO 180A. 2 More preferably, 8.5 kJ / m 2 More preferably, 9 kJ / m 2 More preferably, 9 to 13 kJ / m 2 Within this range, the material has excellent balance of physical properties and excellent mechanical strength, and therefore, when applied to electrical components, it is possible to minimize changes due to the external environment, such as vibrations of an automobile.
[0115] In this description, the notched Izod impact strength is measured on notched test specimens with a thickness of 4 mm using an IT from Toyoseiki Co., Ltd. in accordance with ISO 180A.
[0116] In this description, normal temperature may be a point within the range of 20±5°C.
[0117] The poly(arylene ether) resin composition preferably has a tensile strength of 67 MPa or more, more preferably 73 MPa or more, even more preferably 80 MPa or more, still more preferably 90 MPa or more, and particularly preferably 90 to 120 MPa, as measured in accordance with ISO 527 using a test piece with a thickness of 4 mm and a measurement speed of 5 mm / min. Within this range, the composition has an excellent balance of physical properties and excellent mechanical strength, and therefore has the effect of minimizing deformation due to vibrations and impacts of an automobile and deterioration of physical properties due to changes in temperature and humidity when used in electrical components.
[0118] In this description, the tensile strength is measured according to ISO 527 using a UTM (manufacturer: Instron, model name: 4466) at a cross head speed of 5 mm / min.
[0119] The poly(arylene ether) resin composition may preferably have a flexural strength of 110 MPa or more, more preferably 115 MPa or more, even more preferably 125 MPa or more, still more preferably 130 MPa or more, and particularly preferably 130 to 170 MPa, as measured in accordance with ISO 527 using a test piece with a thickness of 4 mm and a measurement speed of 2 mm / min. Within this range, the composition has an excellent balance of physical properties and excellent mechanical strength, and therefore has the effect of minimizing changes due to the external environment, such as automobile vibrations, when used in electrical components.
[0120] The poly(arylene ether) resin composition may preferably have a heat distortion temperature of 120° C. or higher, more preferably 125° C. or higher, even more preferably 130° C. or higher, still more preferably 135° C. or higher, and particularly preferably 135 to 150° C., as measured on a 4 mm-thick test piece under a stress of 1.8 MPa in accordance with ISO 75-2. Within this range, the composition has the advantage of having excellent balance of physical properties and heat resistance.
[0121] For example, the poly(arylene ether) resin composition may have a flame retardancy of V-0 or higher as measured in accordance with the UL94 standard (Vertical Burning Test) using an injection test piece having a size of 127 mm x 12.7 mm x 1.5 mm. In this case, the composition has the advantages of having an excellent balance of physical properties, heat resistance, and flame retardancy during thermal runaway.
[0122] The poly(arylene ether) resin composition may include, by way of example, one or more additives selected from the group consisting of lubricants, antioxidants, compatibilizers, and impact modifiers.
[0123] The total amount of the above additives may be, for example, 5 to 10 parts by weight, preferably 6 to 9.5 parts by weight, and more preferably 7 to 9 parts by weight, relative to 100 parts by weight of the base resin. Within this range, there are advantages in that the mechanical properties, heat resistance, and flame retardancy are excellent, as well as excellent flame retardancy during thermal runaway.
[0124] In addition to the additives, the poly(arylene ether) resin composition may further contain, relative to 100 parts by weight of the base resin, 0.001 to 5 parts by weight, preferably 0.01 to 3 parts by weight, and more preferably 0.05 to 2 parts by weight of one or more selected from the group consisting of a flame retardant auxiliary, a plasticizer, a heat stabilizer, an anti-dripping agent, a light stabilizer, a pigment, a dye, an inorganic additive (excluding glass fiber), and a carbon fiber. Within this range, the inherent physical properties of the poly(arylene ether) resin composition described herein are not deteriorated, and the required physical properties can be satisfactorily achieved.
[0125] Method for producing poly(arylene ether) resin composition The method for producing the poly(arylene ether) resin composition according to the present invention includes a step of kneading and extruding 100 parts by weight of a base resin containing (a-1) 75-95% by weight of poly(arylene ether) resin and (a-2) 5-25% by weight of polystyrene resin, (b) 12-17 parts by weight of two or more organic phosphorus-based flame retardants having different phosphorus contents, (c) 10-40 parts by weight of glass fiber, (d) 0.5-5 parts by weight of crushed mica, and (e) 1-4 parts by weight of an alkaline earth metal sulfate having an average particle size of 0.05-3 μm, wherein the kneading and extrusion are carried out using an extruder having 9 or more kneading blocks. In this case, there is an advantage that mechanical properties such as impact strength, tensile strength, and bending strength, heat resistance, flame retardancy, and flame retardancy during thermal runaway are all excellent.
[0126] The kneading and extrusion can be carried out at a barrel temperature in the range of, for example, 200 to 350°C, preferably 220 to 330°C, and more preferably 240 to 320°C. In this case, there are advantages that while the throughput per unit time is high, sufficient melt kneading is possible and problems such as thermal decomposition of the resin component are not caused.
[0127] The kneading and extrusion can be carried out under conditions where the screw rotation speed is, for example, 100 to 500 rpm, preferably 150 to 400 rpm, and more preferably 200 to 350 rpm. Within this range, the throughput per unit time is high, and the process efficiency is excellent.
[0128] The poly(arylene ether) resin composition obtained through the kneading and extrusion may be preferably provided in a pellet form.
[0129] molded product The molded article described herein is characterized by containing the poly(arylene ether) resin composition described herein, and in this case, has the advantages of being excellent in all of mechanical properties such as impact strength and tensile strength, heat resistance, electrical insulation, and flame retardancy.
[0130] The molded product may be, for example, one formed by injection molding or extrusion molding.
[0131] The molded article can be used, for example, as an electrical component or a battery component.
[0132] The battery part may be, for example, a plastic upper cover of an electric vehicle battery, a module housing, or a busbar.
[0133] The method for producing a molded article according to the present invention preferably includes the steps of kneading and extruding 100 parts by weight of a base resin containing 75-95% by weight of (a-1) poly(arylene ether) resin and 5-25% by weight of (a-2) polystyrene resin, 12-17 parts by weight of two or more organic phosphorus-based flame retardants having different phosphorus contents, 10-40 parts by weight of (c) glass fiber, 0.5-5 parts by weight of (d) crushed mica, and 1-4 parts by weight of an alkaline earth metal sulfate having an average particle size of 0.05-3 μm to produce poly(arylene ether) resin composition pellets, and injecting the produced pellets to produce a molded article, wherein the kneading and extrusion are carried out using an extruder having 9 or more kneading blocks. In this case, there is an advantage that mechanical properties such as impact strength, tensile strength, and bending strength, heat resistance, flame retardancy, and flame retardancy during thermal runaway are all excellent.
[0134] The injection may be performed according to a method and conditions commonly used in the technical field to which the present invention pertains, without any particular limitation, and may be appropriately selected and applied as necessary.
[0135] In the description of the poly(arylene ether) resin composition, molded article, and manufacturing method thereof described herein, other conditions not specifically indicated (e.g., the configuration and specifications of the extruder and injector, extrusion and injection conditions, additives, etc.) are not particularly limited as long as they are within the range normally used in the industry, and can be appropriately selected as necessary.
[0136] The present invention will now be described with reference to the drawings.
[0137] FIG. 1, below, is a schematic diagram of an extruder equipped with nine or more kneading blocks for producing the poly(arylene ether) resin compositions described herein.
[0138] The type of the extruder is not particularly limited, and may be appropriately selected from those commonly used in the industry. For example, a single-screw extruder having one screw or a multi-screw extruder having multiple screws may be used. Considering uniform mixing of materials, ease of processing, and economy, it is preferable to use a twin-screw extruder having two screws.
[0139] The extruder is composed of a feeder for supplying materials into the barrel, a screw for transporting and kneading the materials supplied into the barrel, and a die for extruding the kneaded materials, and the screw is composed of a plurality of screw elements to provide various functions.
[0140] The number of the raw material supplying devices may be one or more, and two or more may be selectively provided as necessary. For example, a main inlet and a selective auxiliary inlet may be provided, and two or more auxiliary inlets may be provided as necessary.
[0141] As a specific example, a base resin, two or more organic phosphorus-based flame retardants having different phosphorus contents, glass fiber, crushed mica, and an alkaline earth metal sulfate may be fed all at once into the main feeding port, and as another example, all of the components except for the two or more organic phosphorus-based flame retardants having different phosphorus contents may be fed into the main feeding port, and the flame retardant may be fed into the auxiliary feeding port.
[0142] As yet another example, all of the components except for two or more organic phosphorus-based flame retardants having different phosphorus contents may be fed into the main inlet, the two or more organic phosphorus-based flame retardants having different phosphorus contents may be fed into the auxiliary inlet 1, and additives such as lubricants, antioxidants, compatibilizers, and impact modifiers may be fed into the auxiliary inlet 2.
[0143] As yet another example, it is possible to feed a base resin into the main inlet, feed two or more types of organic phosphorus flame retardants with different phosphorus contents, glass fiber, crushed mica, and a portion of an alkaline earth metal sulfate into auxiliary inlet 1, and then feed the remaining amount into auxiliary inlet 2.
[0144] As yet another example, a base resin and an alkaline earth metal sulfate may be fed into the main inlet, two or more organic phosphorus flame retardants having different phosphorus contents and crushed mica may be fed into the auxiliary inlet 1, and glass fiber may be fed into the auxiliary inlet 2.
[0145] The kneading block of the present invention is an example of the screw element, and specifically, it is composed of a plurality of disks, preferably 3 to 7, 5 to 7, 3 to 5, or 4 to 5 disks, usually with a polygonal or elliptical cross section, and is continuously arranged in the material transport direction. In the kneading block, the phase angle of the disks (meaning the movement angle between the disks) is preferably 45 to 90°.
[0146] In addition, the kneading blocks include forward kneading blocks with the ability to transport, distribute and mix materials, neutral kneading blocks with only the ability to distribute and mix materials without the ability to transport materials, and backward kneading blocks that transport materials in the opposite direction to the transport direction.
[0147] The poly(arylene ether) resin composition according to the present invention may be produced by a step of kneading and extruding using an extruder having, for example, 9 or more, preferably 10 or more, more preferably 12 or more, preferably 9 to 18, more preferably 10 to 18, and even more preferably 12 to 16 kneading blocks. In this case, it is effective to use a combination of kneading blocks in the order of forward, perpendicular, and reverse to the flow direction of the resin, and a combination of continuous or separated blocks can be used depending on the mixing method. In this case, the dispersibility of glass fiber and pulverized mica, the compatibility of the composition, etc. are further improved, and a poly(arylene ether) resin composition of even higher quality can be provided.
[0148] For example, nine or more kneading blocks may be continuously arranged, or, for example, they may be discontinuously arranged between the screws. As a specific example, 3 to 6 kneading blocks may be continuously arranged between the main inlet and the auxiliary inlet 1, 3 to 8 kneading blocks may be continuously arranged between the auxiliary inlet 1 and the auxiliary inlet 2, and 2 to 5 kneading blocks may be continuously arranged between the auxiliary inlet 2 and the discharge port (not shown). When arranged in this manner, there are advantages in that local heat generation during melt kneading can be controlled to prevent thermal deformation of the raw materials, and excessive cutting of glass fibers is prevented, so that mechanical properties, flame retardancy, and flame retardancy during thermal runaway are not deteriorated.
[0149] Below, preferred examples are presented to aid in understanding the present description. However, the following examples are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present description. Naturally, such changes and modifications also fall within the scope of the appended claims.
[0150] [Example] The materials used in the following examples and comparative examples are as follows. *(a-1) Poly(arylene ether) resin: Poly(2,6-dimethyl-1,4-phenylene) ether (PPE; Bluestar's LXR040) *(a-2): Polystyrene resin: HIPS (High Impact polystyrene) resin (Kumho Petrochemical's HI450PG) *(b) Two or more organic phosphorus flame retardants with different phosphorus contents: (b-1) bisphenol A bis(diphenyl phosphate) with a phosphorus content of 9% by weight (FCA's BPADP), (b-2) aluminum diethyl phosphinate with a phosphorus content of 25% by weight (Clariant's OP1230) *(c) Glass fiber: Chopped glass fiber with an average particle size of 10 to 13 μm and an average length of 3 to 4 mm, surface-treated with aminosilane (Owens Corning, 910A-13P). *(d) Crushed mica: Crushed mica with an average particle size of 90 μm and an aspect ratio of 50 (Kurary's 200D) *(e-1) Sulfates of alkaline earth metals with an average particle size of 0.05 to 3 μm: Barium sulfate with an average particle size of 1 μm (Solvay's HD80) *(e-2) Sulfates of alkaline earth metals: Barium sulfate with an average particle size of 4 μm (Solvay's Blanc FIX G) *(f) Additives: A mixture of lubricant (Pentaerythritol Fatty Acid Ester), antioxidant (Tris(2,4-di-tert-butyl-phenyl)Phosphite and Pentaeryl thritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate)), compatibilizer (Fumari acid PPO), and impact modifier (Maleated, Styrene-ethylene-butylene Block copolymer rubber).
[0151] Examples 1 to 15 and Comparative Examples 1 to 14 (a-1) poly(arylene ether) resin, (a-2) polystyrene resin, (b-1) organic phosphorus-based flame retardant with phosphorus content of 9% by weight, (b-2) organic phosphorus-based flame retardant with phosphorus content of 25% by weight, (c) glass fiber, (d) crushed mica, (e) alkaline earth metal sulfate, and (f) additives were melt-kneaded and extruded into pellets at the contents shown in Tables 1 to 4 below using a twin-screw extruder (SM T40) with 10 mixing blocks, set at a temperature of 250 to 310 ° C and a rotation speed (rpm) of 300 rpm, and produced into pellets. The pellets were used to produce test pieces for evaluation using an injector (Engel, 80 ton). The produced test pieces were left at room temperature for 48 hours or more, and then the physical properties were measured and shown in Tables 1 to 4 below.
[0152] In this case, the twin-screw extruder has a total of two or more input ports, and the base resin and alkaline earth metal sulfate are input into the main input port, two or more types of organic phosphorus-based flame retardants with different phosphorus contents and crushed mica are input into the auxiliary input port 1, and glass fiber is input into the auxiliary input port 2.
[0153] [Test example] The properties of the test pieces prepared in Examples 1 to 15 and Comparative Examples 1 to 14 were measured in the following manner, and the results are shown in Tables 1 to 4 below.
[0154] Measurement method *Tensile strength (MPa): According to ISO 527, the point at which a 4 mm thick test piece breaks was measured after pulling it at a cross head speed of 5 mm / min using a UTM (manufacturer: Instron, model name: 4466). *Flexural strength (MPa): Measured in accordance with ISO 527 using a UTM (manufacturer: Instron, model name: 4466) at a cross head speed of 2 mm / min using a test piece with a thickness of 4 mm. *Impact strength (kJ / m 2): Izod impact strength was measured under standard conditions of constant temperature and humidity using IT equipment from Toyoseiki Co., Ltd. in accordance with ISO 180A. The test specimens were 4 mm thick and notched. *Heat distortion temperature (℃): The heat distortion temperature was measured under a stress of 45 MPa using a 4 mm thick test piece in accordance with ISO 75-2. *Flame retardancy: Measured in accordance with the UL94 standard (Vertical Burning Test) using an injection test piece of 127mm x 12.7mm x 1.5mm. *Flame Endurance Time (sec): A flame of the size specified in ASTM D5207 (125mm (500W)) was applied to a 100mm x 100mm x 1mm injection test piece in accordance with the UL94 5V test, and the time it took for the flame to be applied until a hole or drip occurred in the test piece was measured. *Appearance evaluation: The appearance of the molded product was visually evaluated at an injection temperature of 290~300℃, injection speed of 50mm / sec, holding pressure of 60bar, holding time of 5sec, and cooling time of 20sec. The product was rated as "excellent" if it was completely molded without any gas marks or unformed areas, and "poor" if there were any unformed areas or gas marks, reducing the appearance quality.
[0155] [Table 1]
[0156] [Table 2]
[0157] [Table 3]
[0158] [Table 4]
[0159] As shown in Tables 1 to 4, the poly(arylene ether) resin compositions of the present invention (Examples 1 to 15) have excellent mechanical properties such as tensile strength, flexural strength, and impact strength, heat distortion temperature, heat resistance, and flame retardancy, as well as excellent fire resistance time of 500 seconds or more, compared to Comparative Examples 1 to 14, and therefore have excellent flame retardancy properties during thermal runaway of a battery.
[0160] Specifically, Comparative Example 1, which contained 3.13 parts by weight of one phosphorus-based flame retardant, had low flame retardancy and fire resistance time, while Comparative Example 2, which contained 7.5 parts by weight of one phosphorus-based flame retardant, had poor mechanical properties in all respects.
[0161] In addition, (d) Comparative Examples 3 and 4, which did not contain crushed mica, and Comparative Example 5, in which the contents of the two phosphorus-based flame retardants were below the range of the present invention, exhibited poor flame retardancy and fire resistance time.
[0162] In addition, in Comparative Example 6, in which the composition ratio of the base resin was outside the range of the present invention, the heat distortion temperature and fire resistance time were reduced, and in Comparative Example 7, in which the content of the two flame retardants was excessive, the fire resistance time was very short and the heat distortion temperature was also low.
[0163] In addition, (d) Comparative Example 8, which contained less than the range of pulverized mica according to the present invention, had a very short fire resistance time and reduced flame retardancy, while (d) Comparative Example 9, which contained more than the range of pulverized mica according to the present invention, had reduced impact strength.
[0164] In addition, (e-1) Comparative Examples 10 and 11, in which the content of barium sulfate was outside the range of the present invention, also showed a shortened fire resistance time and were unable to prevent thermal runaway when applied to battery parts of electric vehicles.
[0165] In addition, in Comparative Example 12 containing barium sulfate (e-2) whose average particle size was outside the range of the present invention, the fire resistance time was shortened.
[0166] In addition, in Comparative Example 13, in which the amount of (C) glass fiber was less than the range of the present invention, the mechanical properties, heat distortion temperature, flame retardancy, and fire resistance time were all decreased, and in Comparative Example 14, in which the amount of (C) glass fiber was more than the range of the present invention, the mechanical properties, heat distortion temperature, flame retardancy, and fire resistance time were excellent, but the fluidity was decreased, and the moldability and the appearance of the molded product were poor.
[0167] In conclusion, the poly(arylene ether) resin composition according to the present invention, which contains a base resin containing a poly(arylene ether) resin and a polystyrene resin in predetermined contents, two or more organic phosphorus-based flame retardants having different phosphorus contents, glass fiber, pulverized mica, and a sulfate of an alkaline earth metal having a predetermined average particle size in predetermined contents, has excellent mechanical properties such as impact strength, tensile strength, and flexural strength, heat resistance, and flame retardancy, and also has excellent flame retardancy during thermal runaway, and therefore has the effect of satisfying the properties required for electrical parts such as electric vehicle batteries.
Claims
1. (a-1) 100 parts by weight of a base resin containing 75 to 95% by weight of a poly(arylene ether) resin and (a-2) 5 to 25% by weight of a polystyrene resin; (b) 12 to 17 parts by weight of two or more organic phosphorus flame retardants having different phosphorus contents; (c) 10 to 40 parts by weight of glass fibers; (d) 0.5 to 5 parts by weight of crushed mica; (e) 1 to 4 parts by weight of an alkaline earth metal sulfate having an average particle size of 0.05 to 3 μm.
2. The poly(arylene ether) resin composition according to claim 1, wherein the (a-1) poly(arylene ether) resin has an intrinsic viscosity of 0.2 to 0.8 dl / g.
3. 2. The poly(arylene ether) resin composition of claim 1, wherein the (a-2) polystyrene resin is general purpose polystyrene, high-impact polystyrene, or a mixture thereof.
4. The poly(arylene ether) resin composition according to claim 1, wherein the (b) two or more organic phosphorus-based flame retardants having different phosphorus contents include (b-1) an organic phosphorus-based flame retardant having a phosphorus content of 5 to 15% by weight, and (b-2) an organic phosphorus-based flame retardant having a phosphorus content of 20 to 35% by weight.
5. The poly(arylene ether) resin composition according to claim 4, wherein the weight ratio (b-1:b-2) of the organic phosphorus flame retardant (b-1) to the organic phosphorus flame retardant (b-2) is 6:4 to 8.5:1.
5.
6. The poly(arylene ether) resin composition according to claim 4, wherein the (b-1) organophosphorus flame retardant having a phosphorus content of 5 to 15 wt% is at least one selected from the group consisting of bisphenol-A-bis(diphenyl phosphate) (BPADP), triphenyl phosphate (TPP), and resorcinol bis diphenyl phosphate (RDP).
7. The poly(arylene ether) resin composition according to claim 4, wherein the (b-2) organic phosphorus-based flame retardant having a phosphorus content of 20 to 35% by weight is at least one selected from the group consisting of a dialkylphosphinate represented by the following chemical formula 3, a diphosphinate represented by the following chemical formula 4, and at least one polymer thereof. [C7] [C8] (In the above Chemical Formula 3 and Chemical Formula 4, R 1 , R 2 , R 3 and R 4 are each independently a linear or branched C 1 -C 10 Alkyl, C 1 -C 10 or H; R 5 is a linear or branched C 1 -C 10 Alkylene of C 6 -C 10 Arylene, C 7 -C 20 or C 7 -C 20 is an aryl alkylene of the formula M 1 m+ and M. 2 m'+are each independently a nitrogen base compound in which one or more atoms selected from the group consisting of Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, and K are cationized, protonated, or cationized and protonated; m is an integer of 1 to 4; n is an integer of 1 to 4; and x is an integer of 1 to 4.
8. 2. The poly(arylene ether) resin composition according to claim 1, wherein the (c) glass fibers have an average particle size of 3 to 25 μm and an average length of 1 to 15 mm.
9. 2. The poly(arylene ether) resin composition according to claim 1, wherein the (d) crushed mica has an average particle size of 50 to 150 μm.
10. 2. The poly(arylene ether) resin composition according to claim 1, wherein the poly(arylene ether) resin composition has a flame endurance time of 500 seconds or more, as measured in accordance with a UL94 5V test in which a flame of a magnitude (125 mm (500 W)) specified in ASTM D5207 is applied to an injection test specimen of 100 mm x 100 mm x 1 mm until a hole or drip is generated in the test specimen.
11. The poly(arylene ether) resin composition has a notched Izod impact strength of 7.7 kJ / m, as measured on a 4 mm thick notched test specimen in accordance with ISO 180A. 2 The poly(arylene ether) resin composition according to claim 1 .
12. 2. The poly(arylene ether) resin composition of claim 1, wherein the poly(arylene ether) resin composition has a heat distortion temperature of 120° C. or more, measured on a 4 mm thick test specimen under a stress of 1.8 MPa according to ISO 75-2.
13. (a-1) 100 parts by weight of a base resin containing 75 to 95% by weight of a poly(arylene ether) resin and (a-2) 5 to 25% by weight of a polystyrene resin; (b) 12 to 17 parts by weight of two or more organic phosphorus-based flame retardants having different phosphorus contents; (c) 10 to 40 parts by weight of glass fiber; (d) 0.5 to 5 parts by weight of pulverized mica; and (e) 1 to 4 parts by weight of an alkaline earth metal sulfate having an average particle size of 0.05 to 3 μm, and the steps of kneading and extruding the resulting mixture; The method for producing a poly(arylene ether) resin composition, wherein the kneading and extrusion are carried out using an extruder having 9 or more kneading blocks.
14. A molded article comprising the poly(arylene ether) resin composition of any one of claims 1 to 12.
Citation Information
Patent Citations
Thermoplastic resin composition, method for producing same, and molded product manufactured therefrom
EP4036171A1
Flame-retardant conductive polyphenylene ether-based composition
JP1994502684A
Polyphenylene ether resin composition and molded body, and production method of polyphenylene ether resin composition
JP2015209518A
Poly(phenylene ether) compositions and articles
JP2016520702A
Halogen-free flame-retardant resin composition
JP2019523802A