Method for measuring the degree of dispersion of conductive material in an electrode for an electrochemical device
A method for quantifying conductive material dispersion in electrodes using a dispersity index and imaging techniques addresses the challenge of non-uniform distribution, improving electrical conductivity and device performance.
Patent Information
- Application Number
- JP2024519400
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-04-20
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-04-20
AI Technical Summary
Existing methods fail to accurately quantify the dispersion of conductive materials in electrodes for electrochemical devices, which affects the electrical conductivity and overall performance of batteries.
A method is developed to evaluate the dispersion of conductive materials in electrodes using a quantified dispersity index, calculated through formulas based on the perimeter and area of the conductive material region in cross-sectional samples, utilizing atomic force microscopy and scanning spreading resistance microscopy to create 2D scale maps and mask conductive material areas.
The method allows for the quantitative assessment of conductive material dispersion, ensuring uniform distribution and improved electrical conductivity within electrodes, thereby enhancing the performance of electrochemical devices.
Smart Images

Figure 2024537062000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims priority based on Korean Patent Application No. 10-2022-0049197 filed on April 20, 2022. The present invention relates to a quantified dispersibility index that can quantitatively represent the dispersibility of a conductive material for an electrochemical element. The present invention also relates to a dispersibility measurement method including a method for calculating the dispersibility index. [Background technology]
[0002] As interest in energy storage technology grows, the fields of application are expanding to include mobile phones, tablets, laptops, and video cameras, as well as the energy of electric vehicles (EVs) and hybrid electric vehicles (HEVs), and research and development on electrochemical devices is gradually increasing. Electrochemical devices are the field that has attracted the most attention in this regard, and among them, the development of rechargeable lithium-ion secondary batteries has become a focus of attention. Recently, in the development of such batteries, research and development has been carried out on new electrode and battery designs to improve capacity density and specific energy.
[0003] When manufacturing electrodes for such secondary batteries, it has been considered to increase the content of active material in the electrode in order to improve the energy density. In this case, the content of conductive material is relatively low, so it is important to distribute the conductive material uniformly in the electrode to prevent a decrease in electrical conductivity. Since the distribution of conductive material in the electrode is closely related to the electrode manufacturing process, research is required on a manufacturing method for dry electrodes that can improve the dispersion of conductive material during electrode manufacturing. In addition, in order to establish a manufacturing process that improves the dispersion of conductive material, it is necessary to develop an evaluation tool that can accurately confirm the dispersion of conductive material in the electrode. Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has an object to provide a quantified dispersibility index capable of quantitatively expressing the dispersibility of a conductive material for an electrochemical element. Another object of the present invention is to provide a dispersibility measurement method including a method for calculating the dispersibility index. It will be easily understood that the other objects and advantages of the present invention can be realized by the means or methods described in the claims, and combinations thereof. [Means for solving the problem]
[0005] A first aspect of the present invention relates to a method for evaluating the dispersion degree of a conductive material, the method comprising: measuring the perimeter (Boundary A) of a portion defined as a conductive material region in one or more arbitrary cross sections in an electrode for an electrochemical device including an electrode active material layer containing an electrode active material and a conductive material; measured ) and area (A) are defined as variables.
[0006] In a second aspect of the present invention, in the first aspect, the formula is a conductive material dispersity index 1 (Index 1) according to the following [Formula 1], or a conductive material dispersity index 2 (Index 1) according to the following [Formula 2]. [Formula 1] Index 1(μm -1 )=Boundary measured / A [Formula 2] Index 2=Boundary measured / L circle In the above formula 1, Boundary measured means the perimeter of a portion defined as a conductive material region measured at a predetermined cross section of the electrode active material layer, and A means the area of a portion defined as a conductive material region measured at a predetermined cross section of the electrode active material layer. In the above [Equation 2], L circle is the circumference of a circle having an area equal to the area of the conductive material region defined above.
[0007] A third aspect of the present invention, in the first or second aspect, includes the steps of: (Step 1) obtaining a cross-sectional sample in which an arbitrary cross section inside the electrode active material layer is exposed; (Step 2) obtaining a 2D scale map of the resistance distribution of the sample cross section; (Step 3) masking a conductive material region; and (Step 4) calculating the perimeter and area of the masked region and substituting the calculated values into the above formula 1 and / or formula 2 to confirm the degree of dispersion of the conductive material in the electrode active material layer.
[0008] A fourth aspect of the present invention is any one of the first to third aspects, wherein the electrode active material layer is formed on any one of the side surfaces of an electrode current collector, and the cross section (or multiple cross sections) is a parallel or perpendicular plane to the opposing part of the electrode active material layer with respect to the current collector.
[0009] A fifth aspect of the present invention is the method for evaluating the dispersion degree of a conductive material according to the third aspect, wherein the cross-sectional sample is prepared by etching an electrode surface to a predetermined depth by ion milling.
[0010] A sixth aspect of the present invention is directed to any one of the third to fifth aspects, wherein the step of obtaining a 2D-scale map of the resistance distribution in the cross-section of the sample is performed by Scanning Spreading Resistance Microscopy, which scans the surface of the cross-section sample using an AFM (Atomic force microscopy) device.
[0011] A seventh aspect of the present invention, in any one of the third to sixth aspects, includes a first step of processing and converting the resistance value data obtained in (Step 2) into a log scale to obtain a log scale image (log (resistance) image), a second step of extracting a [log resistance distribution histogram] in which materials constituting the sample of the electrode cross section are displayed in a divided manner in the log scale image, and a third step of setting a log(R / Ω) value corresponding to the minimum value between the conductive material peak and the electrode active material peak in the histogram as a threshold, and masking an area having a value smaller than that value as a conductive material area.
[0012] An eighth aspect of the present invention, in accordance with the seventh aspect, further comprises the step of correcting the threshold by adding a value from 0.1 to 0.5 to the minimum value.
[0013] A ninth aspect of the present invention is related to any one of the first to eighth aspects, wherein the electrode for electrochemical elements includes a current collector and an electrode active material layer formed on at least one surface of the current collector, and the electrode active material layer includes an electrode active material, a conductive material, and a binder.
[0014] A tenth aspect of the present invention is based on any one of the first to ninth aspects, wherein the cross section is in a direction parallel or perpendicular to a facing portion of the electrode active material layer against the current collector. Effect of the Invention
[0015] The method for evaluating the dispersion degree of a conductive material according to the present invention can quantitatively evaluate the dispersion degree of the conductive material in an electrode. Specifically, a conductive material region is defined from the result (2D mapping image) obtained by performing two-dimensional scale visual image processing on an arbitrary cross section of an electrode active material layer, and the perimeter and area of the part defined as the conductive material region are calculated, thereby quantitatively expressing the dispersion degree of the conductive material.
[0016] The following drawings attached to this specification are intended to illustrate preferred embodiments of the present invention, and serve to further understand the technical ideas of the present invention together with the detailed description of the invention, and therefore the present invention should not be interpreted as being limited to only the matters described in the drawings. Meanwhile, the shape, size, scale, or ratio of elements in the drawings attached to this specification may be exaggerated in order to emphasize a clearer description. [Brief description of the drawings]
[0017] [Figure 1A] FIG. 1 shows an SSRM image of the electrode of Example 4 obtained by scanning diffusion resistance microscopy. [Figure 1B] 1B is an image obtained by masking the conductive material area of FIG. 1A. [Diagram 2] 1 is a graph of a log(resistance distribution) histogram of Example 4. [Diagram 3] 1 is an SSRM image of Example 1. [Figure 4] This is an image confirmed by masking the conductive material area in Figure 3. [Diagram 5] 1 is an SSRM image of Example 2. [Figure 6] This is an image confirmed by masking the conductive material area in Figure 5. [Figure 7] SSRM image of Example 3. [Figure 8] This is an image confirmed by masking the conductive material area in FIG. 7. [Figure 9A] FIG. 1 shows a schematic diagram of a method for preparing a sample of an electrode cross section. [Figure 9B] FIG. 1 shows a schematic diagram of a method for preparing a sample of an electrode cross section. [Figure 10] 2 is an image showing the result of masking the conductive material region in FIG. 1 in the electrode of Example 4 without correction with the obtained histogram. [Figure 11] 2 is an image showing the result of masking the conductive material region of FIG. 1 after correction in the electrode of Example 4. [Figure 12]13 is an exemplary graph showing an overlapping portion of a histogram between a conductive material region and an active material region. [Figure 13] 13 shows an SSRM image of the electrode of Example 5 and an image showing the result of masking the conductive material region after correction. [Figure 14] 13 shows an SSRM image of the electrode of Example 6 and an image showing the result of masking the conductive material region after correction. [Figure 15] FIG. 13 shows a display screen showing the area and perimeter of conductive material regions calculated using Gwyddion software. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will now be described in more detail for the sake of understanding.
[0019] The terms and words used in this specification and the claims are not to be interpreted limited to their ordinary and dictionary meanings, but are to be interpreted in a meaning and concept that corresponds to the technical idea of the present invention, based on the principle that the inventor himself can appropriately define the concept of the term in order to explain the invention in the best possible way.
[0020] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. Unless otherwise clearly indicated in the context, the singular expression includes the plural expression.
[0021] Also, throughout the specification, when a part is said to "comprise" certain elements, this means that it can further include other elements, rather than excluding other elements, unless specifically stated to the contrary.
[0022] In addition, the terms "about," "substantially," and the like, used throughout this specification, when the tolerances of manufacturing and materials inherent in the referred meaning are given, are used to mean a numerical value or a close approximation of the numerical value, and are used to prevent unscrupulous infringers from unfairly taking advantage of the disclosure in which precise and absolute numerical values are recited for the understanding of this application.
[0023] Throughout this specification, the phrase "A and / or B" means "A or B, or both."
[0024] Dispersion of conductive material The present invention proposes a method for defining a conductive material region from the results (2D mapping image) obtained by performing two-dimensional scale visual image processing on an arbitrary cross section of an electrode active material layer, a method for calculating the perimeter and area of the part defined as the conductive material region, and a dispersion index that can quantitatively represent the dispersion degree of the conductive material based on the method.
[0025] In the present invention, the dispersity index can be expressed as a dispersity index 1 (Index 1) of the conductive material according to the following [Equation 1] for one or more arbitrary cross sections inside the electrode active material layer. Meanwhile, the dispersity index can be expressed as a dispersity index 2 (Index 2) of the conductive material according to the following [Equation 2] together with or independently of the index 1. The dispersity index 1 and the dispersity index 2 of the conductive material are calculated based on the perimeter (Boundary Length) of the part defined as the conductive material region measured on the cross section. measured ) and area (A) as variables.
[0026] [Formula 1] Index 1(a -1 )=Boundary measured / A In the above formula 1, Boundary measuredmeans the perimeter of a portion defined as a conductive material region measured at a predetermined cross section of the electrode active material layer, and A means the area of a portion defined as a conductive material region measured at a predetermined cross section of the electrode active material layer. In the above formula 1, a is the unit used. If the unit of perimeter is μm, the unit of the index 1 is μm. -1 It could be.
[0027] [Formula 2] Index 2=Boundary measured / L circle In the above formula 2, Boundary measured is defined as in Equation 1, and L circle is the circumference of a circle having the same area as the area of the conductive material region defined above. In any closed curve, the smallest perimeter is when the shape of the closed curve is a circle. Therefore, a virtual circle having the same area as the entire area (A) of the conductive material region is assumed, the perimeter of the circle is calculated, and the perimeter of the actual conductive material region is divided by the perimeter of the virtual circle. The larger the value of Index 2, the higher the degree of dispersion.
[0028] Said L circle can be calculated by the following formulas 1 and 2.
number
number
[0029] Therefore, the above formula 2 can be expressed as the following formula 2A.
number
[0030] In other words, the area of a circle is {(radius of the circle (r)) 2×π}, which allows the radius (r) of the imaginary circle to be found, and once the radius is found, the perimeter (circumference, 2πr) of the imaginary circle can be calculated.
[0031] The higher the dispersibility index 1 and the dispersibility index 2, the more uniformly the conductive material is dispersed in the electrode active material layer, without being locally unevenly distributed due to aggregation.
[0032] In the present invention, the cross section (or a plurality of cross sections) can be formed parallel to the facing portion of the current collector of the electrode active material layer. Alternatively, the cross section (or a plurality of cross sections) can be formed in a direction parallel to the facing portion of the current collector, in a direction perpendicular to the facing portion of the current collector, or at a predetermined angle to the facing portion of the current collector. Since the present invention is intended to confirm the degree of dispersion of the conductive material inside the electrode active material layer, the angle between the exposed surface and the facing portion of the current collector is not limited to a specific range as long as the inside is exposed to an extent that the indexes 1 and 2 can be confirmed.
[0033] The Index 1 and Index 2 can be confirmed by visualizing the distribution of the electrode material, particularly the conductive material, for any cross section of the electrode active material layer, calculating the perimeter and area of the portion (conductive material region) where the conductive material is distributed, and substituting the calculated values into the above formula. The distribution of the electrode material contained in the electrode active material layer is confirmed in microscopic dimensions below the microscale. Thus, the visualization of the conductive material distribution can be confirmed by electronic visualization devices such as atomic force microscopy and scanning diffusion resistance microscopy, as described below.
[0034] Next, a method for calculating Index 1 and Index 2 will be described in detail.
[0035] The method includes a step of exposing an arbitrary cross section of an inside of an electrode for an electrochemical element to obtain a sample of the electrode cross section (Step 1); A step (Step 2) of acquiring resistance value data of the electrode active material and the conductive material of the electrode cross-section sample using a scanning diffusion resistance microscope; obtaining a log scale image and a histogram for the resistance data (Step 3); and (Step 4) calculating the index 1 and / or the index 2. Each step will be described in more detail below.
[0036] (Step 1) First, an arbitrary cross section of the inside of an electrode for an electrochemical device is exposed to prepare a sample of the electrode cross section. The electrode may include an electrode active material layer formed on at least one surface of a current collector, and the electrode active material layer includes an electrode active material, a conductive material, and a binder resin. Then, the surface of the electrode active material layer is removed to a predetermined thickness using an ion beam of ion milling to expose the inner cross section of the electrode active material layer. The ion milling refers to a method of etching a material by accelerating ions of an inert gas from a wide beam ion source to the surface of a sample in a vacuum state. The ion milling is based on the sputtering phenomenon in which ions or atoms of an inert gas (Argon) are accelerated with a voltage of an appropriate size to peel off atoms on the surface of the sample. As a result, a sample of an electrode cross section having a clean cross section without physical damage can be manufactured, and the conductive material region of the electrode can be more clearly identified.
[0037] According to an embodiment of the present invention, the inert gas may be argon. By irradiating the secondary battery electrode with an argon ion beam in this manner, a sample of the electrode cross section can be more stably manufactured.
[0038] In one embodiment of the present invention, the ion beam current of the ion milling apparatus may be 100 μA to 250 μA. Specifically, the ion beam current of the ion milling apparatus may be 110 μA to 150 μA, or 200 μA to 230 μA. By adjusting the ion beam current of the ion milling apparatus within the above range, the preparation time of the electrode cross-section sample can be shortened, and a phenomenon in which an electrode material is redeposited on the cross-section of the sample can be prevented, thereby preparing an electrode cross-section sample having a cleaner cross-section.
[0039] By using such ion milling, it is possible to obtain information on the electrode surface with a very high degree of roughness, and desired information can be obtained, such as observation through an electron microscope or visualization data.
[0040] 9A and 9B are diagrams showing a schematic diagram of a method for preparing a cross-sectional sample of an electrode, in which a portion 11s from the surface to a predetermined depth based on the thickness direction (height) of the electrode active material layer is etched and removed by ion milling to expose a predetermined plane inside the electrode active material layer (FIG. 9B).
[0041] Meanwhile, in one embodiment of the present invention, the step of preparing a sample of the electrode cross section may further include a step of impregnating the electrode with a polymer containing an epoxy group before applying the ion milling, thereby filling the internal pores of the electrode for a secondary battery with the polymer containing an epoxy group. The method of impregnating the electrode with the polymer containing an epoxy group may be performed by a method commonly used in the art. For example, the polymer containing an epoxy group may be applied onto the electrode, or the electrode may be immersed in a solution of the polymer containing an epoxy group to impregnate the electrode with the solution.
[0042] According to one embodiment of the present invention, the method for analyzing a battery electrode may further include a step of measuring a resistance value of the polymer containing an epoxy group filled in the pores of the electrode cross-section sample. By filling the internal pores of the secondary battery electrode with a polymer containing an epoxy group, the resistance value of the pores in the electrode cross-section sample may be obtained using a scanning diffusion resistance microscope. Specifically, the resistance value of the polymer material filling the pores may be measured to obtain resistance value data. This allows the area where the pores are located to be identified, and the electrode active material area, the conductive material area, and the pore area of the electrode cross-section sample to be more accurately distinguished from the merged image. (See FIG. 12)
[0043] According to an embodiment of the present invention, the epoxy group-containing polymer may be an epoxy resin polymer having a cyclic structure in its molecular structure, and more specifically, an epoxy resin polymer having an aromatic group (e.g., a phenyl group). Specific examples of the epoxy group-containing polymer having an aromatic group may include, but are not limited to, one or a mixture of two or more of biphenyl-type epoxy group-containing polymer, dicyclopentadiene-type epoxy group-containing polymer, naphthalene-type epoxy group-containing polymer, dicyclopentadiene-modified phenol-type epoxy group-containing polymer, cresol-type epoxy group-containing polymer, bisphenol-type epoxy group-containing polymer, xyloxal-type epoxy group-containing polymer, multifunctional epoxy group-containing polymer, phenol novolac epoxy group-containing polymer, triphenolmethane-type epoxy group-containing polymer, and alkyl-modified triphenolmethane epoxy group-containing polymer. Specific examples may include, but are not limited to, any one of epoxyethane (ethylene oxide), 1,3-epoxypropane (trimethylene oxide), and bisphenol-A-epichlorohydrin.
[0044] (Step 2) Next, when the electrode cross-section sample is prepared in Step 1, a 2D-scale map of the resistance distribution of the cross-section of the sample is obtained using a conductive network analysis method (Scanning Spreading Resistance Microscopy). Figure 1A is an exemplary diagram showing a 2D-scale map image of Example 4 obtained by the above method.
[0045] Specifically, an AFM (Atomic Force Microscopy) device can be used to scan the surface of the cross-sectional sample to obtain an image converted to a 2D scale. The above measurement produces a map in which the high and low electrical resistance values are indicated by shades of color, and the distribution of surface resistance can be visually confirmed by the difference in color tone (shade).
[0046] First, a sample is prepared for measurement using an AFM (Atomic Force Microscopy) device. The cross-sectional sample prepared in the above process is attached to a metal disk for AFM with the cross-section facing upward, and silver paste is applied to the metal disk for AFM so that a conductive path can be formed between the part other than the milled cross-section and the part. The sample for AFM measurement prepared in this way is loaded into the device, and after laser alignment, the cross-section is selected as the measurement part using an optical microscope. Then, an atomic microscope probe is contacted with the electrode cross-section, and the current flowing through the sample between the atomic microscope probe and the contact electrode is measured, and the diffusion resistance is obtained from the measured current.
[0047] According to an embodiment of the present invention, the operating conditions of the scanning diffusion resistance microscope for analyzing the electrode cross-section sample are, for example, as follows.
[0048] The AFM device is not particularly limited as long as it can visually image the resistance distribution by the scanning diffusion resistance microscope method. For example, cypher ES (Oxford Instruments) can be used. In a specific example of the present invention, Dual-gain ORCA can be used as the cantilever holder, and AR (Oxford Instruments) can be used as the driving software.
[0049] As specific driving conditions, a contact mode is set, the image pixels to be acquired can be set from 512×512 to 1024×1024, the scan rate can be set to 0.2 Hz or more and 1.0 Hz or less, the bias can be set to 2.0 V or less, and the set point can be set to 1.0 V or less. For example, the image pixels can be set to 512×512, the scan rate can be set to 0.5 Hz, the bias can be set to 2.0 V or less, and the set point can be set to 0.2 V. As the AFM probe, solid diamond AFM probes (AD-40-As, Adama) made of boron-doped single crystal diamond can be used.
[0050] Meanwhile, in one embodiment of the present invention, it is preferable to perform AFM measurement on the obtained cross-sectional sample under conditions where it is not exposed to the atmosphere, such as in a glove box, etc. In this case, the cross-sectional sample can be loaded into a closed cell body to maintain a state where it is not exposed to the atmosphere.
[0051] (Step 3) When the 2D scale map is obtained by Step 2, the conductive material region is defined. The term "definition" is used to refer to a method of visual display, or it can be called "masking". For example, Figs. 10 and 11 are diagrams showing the conductive material region identified from the histogram for the electrode of Example 4, masked in black. The method of defining the conductive material region can be described in detail as follows.
[0052] First, the resistance data obtained using a scanning diffusion resistance microscope is processed and converted to a log scale, and a log scale image (log (resistance) image) can be obtained. Once such a log scale image is obtained, a log resistance distribution histogram is extracted from it, which classifies and displays the materials that make up the sample on the electrode cross section.
[0053] It can be determined whether the corresponding area of each pixel on the histogram is an electrode active material area, a pore or binder area, or a conductive material area, and the conductive material area distribution in the 2D mapping image can be quantified using information on each pixel whose corresponding area has been determined.
[0054] Specifically, the log(R / Ω) value corresponding to the minimum value between the conductive material peak and the electrode active material peak in the histogram is set as a threshold, and the area having a value smaller than that value is masked as the conductive material area. In this case, the minimum value can be adjusted by adding or subtracting 0.1 to 0.5 to obtain more accurate data for the conductive material area.
[0055] In one embodiment, the correction may be a value of 0.1 to 0.5 added to the log(R / Ω) value corresponding to the minimum value. This is to correct the portion of the histogram where the active material region and the conductive material region overlap and are not displayed as the conductive material region. For example, the correction value may be determined by dividing the conductive material region of the histogram into left and right sides based on the peak of the conductive material region, and correcting the low point of the right side region to have the same value as the horizontal distance from the peak to the low point on the left side.
[0056] By making the correction as described above, even the areas that overlap with the electrode active material area and are not displayed as conductive material areas can be displayed as conductive material areas, so that more accurate dispersion degree data can be obtained.
[0057] FIG. 2 is a diagram showing a log resistance distribution histogram extracted based on the log scale image (log (resistance) image) for the electrode of Example 4. Referring to this, the conductive material peak and the electrode active material peak can be confirmed, and the minimum value between them can be identified. However, as described above, even in the section after the minimum value, there is a conductive material section that overlaps with the active material region and is not displayed, so the numerical values are corrected as described above. FIG. 12 is an example diagram showing the predicted shape of the overlap between the active material region and the conductive material region.
[0058] On the other hand, FIG. 10 is a diagram showing the masking of the conductive material region in the SSRM image based on the value before correction. The masking of the conductive material region is done with a color not present in the original image, and in the embodiment of the present application, it is shown masked in black. When checking the circle portion shown by the dotted line in FIG. 10, it is confirmed that although it is conductive, it is not masked and remains. When the color of the unmasked portion is confirmed, it is confirmed that the portion maintained in blue. On the other hand, FIG. 11 shows the masking of the conductive material region based on the value after correction, and it is confirmed that the unmasked portion in FIG. 10 (the portion maintained in blue) is masked in black in FIG. 11.
[0059] Meanwhile, among the regions masked with the conductive material, the regions located within the active material are removed to remove errors. This is due to errors that occur during the manufacturing process of the sample, such as conductive material adhering to the exposed cross-section of the active material during the manufacturing process of the cross-section sample, or errors that occur during image processing, and it is clear that the conductive material is not actually distributed inside the active material in the electrode, so it is desirable to remove it.
[0060] On the other hand, after the conductive material area is masked, an image in which only the conductive material area is displayed is extracted (contrast masked) as shown in Figures 1B, 4, 6, 8, the lower part of Figure 13, and the lower part of Figure 14, and is used for the calculation in Step 4.
[0061] In one embodiment of the present invention, the masking of the conductive material region can be performed using a program for visualizing data obtained by scanning probe microscopy such as AFM. In one embodiment of the present invention, the masking can be performed using Gwyddion software. Meanwhile, if there are many images in which the pixel size of the image is too small, it is difficult to accurately confirm the perimeter and area of the conductive material region, and this may act as noise when calculating the degree of dispersion, resulting in an error. Therefore, during the masking, pixel images that are too small can be removed. For example, when using the Gwyddion program, fine regions of less than 3 pixels can be removed using a grain-filtering function so that they are not masked by the conductive material region. When fine regions of less than 3 pixels are included, the perimeter of the conductive material region may be calculated as an excessively high value, so they are removed and measured. Meanwhile, FIG. 2 is a diagram showing a histogram obtained by the above method, and it is confirmed that the active material region and the conductive material region are separated.
[0062] (Step 4) When the masking of the conductive material area is completed in step 3 (i.e., the conductive material area is determined), the perimeter and area of the masked area are confirmed, and the Index 1 can be calculated according to the above formula 1. In the above formula 1, the perimeter value of the masked area is Boundary measured and the area value of the masking region is applied to A.
[0063] In addition, the radius of a circle having the same area as the area of the masking region can be calculated, and the circumference of the circle can be calculated by the calculation of the radius of the circle. circle By substituting the above, Index 2 can be calculated using [Equation 2].
[0064] Meanwhile, in the present invention, the area and perimeter of the masked conductive material region can be calculated using an image processing program such as Gwyddion software. Figure 15 shows a display screen showing the area and perimeter calculated by the program.
[0065] Electrodes for electrochemical devices In the present invention, the electrode to be evaluated for the degree of dispersion of the conductive material is not particularly limited as long as it is an electrode for an electrochemical device. The electrochemical device may include any device that performs an electrochemical reaction. Specific examples of the electrochemical device include all kinds of primary batteries, secondary batteries, fuel cells, solar cells, and capacitors such as supercapacitor devices. The secondary battery may be a lithium ion secondary battery in which a lithium salt is used as an ion conductive salt. In one embodiment of the present invention, the electrode may include a current collector and an electrode active material layer disposed on at least one surface of the current collector. In addition, the electrode active material layer may include an electrode active material, a conductive material, and a binder material.
[0066] electrode active material The electrode active material layer may include a positive electrode active material or a negative electrode active material depending on the polarity of the battery.
[0067] Non-limiting examples of the positive electrode active material include lithium transition metal oxides or lithium metal iron phosphates, and are not limited to metal oxides, such as layered compounds such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2), and compounds substituted with one or more transition metals, and compounds represented by the chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as LiMnO4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; and vanadium oxides with the chemical formula LiNi 1-x M x O2 (where M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x=0.01 to 0.3), and LiMn 2-x M x Lithium manganese composite oxides represented by Li2Mn3MO8 (where M=Co, Ni, Fe, Cr, Zn, or Ta, and x=0.01 to 0.1) or Li2Mn3MO8 (where M=Fe, Co, Ni, Cu, or Zn) and lithium metal phosphate oxides represented by LiMn2O4 (where M=Fe, Co, Ni, or Mn) in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion, lithium metal phosphate oxide LiMPO4 (where M=Fe, Co, Ni, or Mn), and lithium nickel-manganese-cobalt oxide Li 1+x (Ni a Co b Mn c ) 1-x O2 (x=0~0.03, a=0.3~0.95, b=0.01~0.35, c=0.01~0.5, a+b+c=1) and lithium nickel-manganese-cobalt oxide in which part of the oxide is replaced by aluminum, Li 1+x (Ni a Co b Mn c Al d ) 1-xO2 (where x = 0 to 0.03, a = 0.3 to 0.95, b = 0.01 to 0.35, c = 0.01 to 0.5, d = 0.001 to 0.03, a + b + c + d = 1), and an oxide in which part of the lithium nickel - manganese - cobalt oxide is substituted with another transition metal, Li 1+x (Ni a Co b Mn c M d ) 1-x O2 (where x = 0 to 0.03, a = 0.3 to 0.95, b = 0.01 to 0.35, c = 0.01 to 0.5, d = 0.001 to 0.03, a + b + c + d = 1, and M is any one selected from the group consisting of Fe, V, Cr, Ti, W, Ta, Mg, and Mo), a disulfide compound, and Fe2(MoO4)3, etc. are mentioned, but not limited thereto.
[0068] Non - limiting examples of the negative electrode active material include carbon such as graphitizable carbon and graphite - based carbon, and Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0 < x ≤ 1, 1 ≤ y ≤ 3, 1 ≤ z ≤ 8) and other metal composite oxides, lithium metal, lithium alloys, silicon - based alloys, tin - based alloys, silicon - based oxides such as SiO, SiO / C, SiO2, metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5, conductive polymers such as polyacetylene, and Li - Co - Ni - based materials can be used.
[0069] Binder Material In the present invention, the binder material can achieve binding of materials contained in the electrode such as the electrode active material, and binding between the electrode active material layer and the separator or current collector facing it, and is not limited to a specific one as long as it can be used as a binder material for secondary batteries.
[0070] Conductive material The conductive material can be included in the electrode mixed powder and introduced into the electrode active material layer. The conductive material is not particularly limited as long as it has conductivity without causing chemical changes in the battery, and can be, for example, graphite such as natural graphite or artificial graphite, carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, summer black, conductive fiber such as carbon fiber or metal fiber, metal powder such as carbon fluoride, aluminum, nickel powder, conductive whisker such as zinc oxide, potassium titanate, conductive metal oxide such as titanium oxide, conductive material such as polyphenylene derivative, etc., but more specifically, in order to uniformly mix the conductive material and improve the conductivity, it can include one or more selected from the group consisting of activated carbon, graphite, carbon black, and carbon nanotubes, and more specifically, it can include activated carbon.
[0071] Current collector On the other hand, in one embodiment of the present invention, the current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, copper or aluminum, or stainless steel whose surface is surface-treated with carbon, nickel, titanium, silver, etc. Also, the current collector can have fine irregularities on its surface to improve the adhesive strength of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0072] Meanwhile, in one embodiment of the present invention, the current collector may be entirely or partially coated with a conductive primer for reducing surface resistance and improving adhesion. Here, the conductive primer may include a conductive material and a binder, and the conductive material may be, for example, a carbon-based material, as long as it is a conductive material. The binder may include a solvent-soluble fluorine-based binder (including PVDF and PVDF copolymers), an acrylic binder, and a water-based binder.
[0073] Meanwhile, in the present invention, the method for producing the electrode is not particularly limited. For example, the electrode can be produced by applying a wet method in which a slurry for forming an electrode active material layer is applied to a current collector, or a dry method in which electrode mixed particles are compressed to form a layer structure.
[0074] The electrode manufacturing method by the wet method can be described as follows. First, electrode materials such as an electrode active material, a conductive material, and a binder are added to a suitable solvent to prepare a slurry for forming an electrode active material layer. In addition to the above-mentioned electrode materials, additives capable of improving electrochemical performance and dispersibility of the slurry can be further added to the slurry. Then, the slurry is applied to an electrode collector. The application method can be a known application method such as slot die, gravure coating, dip coating, blade coating, etc., and is not limited to a specific method. Then, the solvent is removed to obtain an electrode having an electrode active material layer disposed on the surface of the collector. The slurry can be dried by natural drying or air drying, and can be heated to promote drying. Then, a pressurization process can be further performed to ensure a suitable thickness and loading amount of the electrode active material.
[0075] The dry method may involve preparing a dry mixture containing an electrode material or mixed particles containing an electrode material, and then compressing the powdered material without the intervention of a solvent to form a layered structure.
[0076] The dry manufacturing method according to an embodiment of the present invention can be described as follows. First, powdered electrode materials are mixed in a dry manner. Here, the electrode materials may further include an electrode active material, a binder, and a conductive material. In addition to the above-mentioned electrode materials, additives capable of promoting electrochemical performance and particle formation may be added to the mixed particles. Then, a shear force is applied to the mixture obtained above to fiberize the binder. The shear force can be applied by mixing the electrode materials at high speed or by kneading. Here, the applied shear force in the kneading may be lower than that in the mixing. In one embodiment of the present invention, the kneading can be performed at a high temperature, for example, a temperature of 80° C. or more, 100° C. or more. Meanwhile, the temperature can be controlled to 200° C. or less, preferably 150° C. or less. Through this process, the binder resin is fiberized and the electrode materials are entangled to obtain mixed particles of a desired size. Meanwhile, a mixed mass can be obtained through the kneading process, and a pulverization process can be further performed to produce mixed particles of a desired size. The mixed particles may contain a binder resin that can be fiberized by shear force, such as polytetrafluoroethylene (PTFE) or polyolefin. When the mixed particles are obtained in this way, they are pressed to produce a plate-shaped electrode film, and then the electrode film and a current collector are bonded to obtain an electrode. Alternatively, a method of directly spraying the mixed particles on a current collector and pressing them can be applied. Meanwhile, in the method of producing the mixed particles, the electrode material is put into a solvent to produce a slurry, and then the slurry is spray-dried to produce the mixed particles. In such a case, a binder resin such as SBR can be used. However, in the present invention, the electrode for measuring the dispersion degree of the conductive material is not limited to a specific shape or production method, and it goes without saying that any electrode can be applied as long as the above-mentioned dispersion degree measurement method can be applied.
[0077] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the present invention will be described in detail based on examples, comparative examples, and experimental examples in order to enable those skilled in the art to easily understand the present invention.
[0078] [Example] Electrode fabrication Example 1 Lithium nickel cobalt manganese aluminum composite oxide (Li(Ni,Co,Mn,Al)O2), carbon black (specific surface area 1400m 2 1.5:2.5 / g) and polytetrafluoroethylene (PTFE) were put into a blender in a ratio of 96.0:1.5:2.5 and mixed at 10,000 rpm for 1 minute to prepare a mixture. Then, the mixture was pulverized in a jet mill process (feeding pressure 50 psi, grinding pressure 45 psi) to obtain a mixed powder for an electrode. The mixed powder for an electrode was put into a first lap calendar (roll diameter: 88 mm, roll temperature: 100°C, 20 rpm) and pressed to prepare a dry electrode film. Then, the obtained dry electrode film was placed on both sides of an aluminum thin film (thickness 19 μm) and bonded by a lamination process maintained at 150°C to obtain an electrode. The thickness of the electrode active material layer on one side of the obtained electrode was about 80 μm. Meanwhile, the lithium nickel cobalt manganese aluminum composite oxide had a bimodal distribution and contained large particles (secondary particles) with a diameter of about 10 μm and single particles with a diameter of about 5 μm. FIG. 3 is an SSRM image of Example 1, and FIG. 4 is a diagram showing an image confirmed by masking the conductive material region.
[0079] Examples 2 to 4 Lithium nickel cobalt manganese aluminum composite oxide (Li(Ni,Co,Mn,Al)O2), carbon black and polytetrafluoroethylene (PTFE) were put into a blender in a ratio of 96.0:1.5:2.5, and mixed at 10,000 rpm for 1 minute to prepare a mixture. Then, the temperature of the kneader was stabilized at 150°C, and the mixture was put into the kneader and kneaded under a pressure of 1.1 atm to obtain a mixture lump. In Examples 2 and 4, the kneading speed was controlled to be different from 40 rpm to 70 rpm, and the kneading time was controlled to be different from 3 minutes to 7 minutes. The mixture lump was put into a blender, pulverized for 40 seconds under the condition of 10,000 rpm, and classified with a sieve with a pore size of 1 mm to obtain a mixed powder for an electrode. Then, the mixed powder for an electrode was put into a first lap calender (roll diameter: 88 mm, roll temperature: 100°C, 20 rpm) and pressed to prepare a dry electrode film. Next, the obtained dry electrode film was placed on both sides of an aluminum thin film (thickness 19 μm) and bonded by a lamination process maintained at 150 ° C. to obtain an electrode. The thickness of the electrode active material layer on one side of the obtained electrode was about 80 μm. Meanwhile, the lithium nickel cobalt manganese aluminum composite oxide has a bimodal distribution and contains large particles (secondary particles) with a diameter of about 10 μm and single particles with a diameter of about 5 μm. In addition, the conductive materials used in Example 2 and Example 4 were different from each other. Figures 1A and 1B are diagrams showing SSRM images of the electrode of Example 4 and images confirmed by masking the conductive material area. Figure 5 is a diagram showing SSRM images of the electrode of Example 2, and Figure 6 is a diagram showing an image confirmed by masking the conductive material area. Figure 7 is a diagram showing SSRM images of the electrode of Example 3, and Figure 8 is a diagram showing an image confirmed by masking the conductive material area.
[0080] Examples 5 and 6 Lithium nickel cobalt manganese aluminum composite oxide (Li(Ni,Co,Mn,Al)O2), carbon black (specific surface area 1400m 21 / g) and polytetrafluoroethylene (PTFE) were put into a blender and mixed at 10,000 rpm for 1 minute to prepare a mixture. Then, the temperature of the kneader was stabilized at 150°C, and the mixture was put into the kneader and kneaded under a pressure of 1.1 atm to obtain a mixture mass. In Example 5 and Example 6, the kneading speed was controlled to be different from 40 rpm to 70 rpm, and the kneading time was controlled to be different from 3 minutes to 7 minutes. The mixture mass was put into a blender, pulverized for 40 seconds under the condition of 10,000 rpm, and classified with a sieve with a pore size of 1 mm to obtain a mixed powder for an electrode. Then, the mixed powder for an electrode was put into a first lap calendar (roll diameter: 88 mm, roll temperature: 100°C, 20 rpm) and pressed to prepare a dry electrode film. Then, the obtained dry electrode film was placed on both sides of an aluminum thin film (thickness 19 μm) and bonded by a lamination process maintained at 150°C to obtain an electrode. The thickness of the electrode active material layer on one surface of the obtained electrode was about 80 μm. On the other hand, the lithium nickel cobalt manganese aluminum composite oxide had a monomodal distribution, and single particles with a diameter of about 5 μm were used. Example 4 is a lithium nickel cobalt manganese aluminum composite oxide (Li(Ni, Co, Mn, Al)O2), carbon black (specific surface area 1400 m 2 The ratio of SSRM (polytetrafluoroethylene (PTFE)) was 96.0:1.8:2.2 in Example 5 and 96.2:1.6:2.2 in Example 6. Fig. 13 shows an SSRM image of Example 5 and an image confirmed by masking the conductive material area. Fig. 14 shows an SSRM image of Example 6 and an image confirmed by masking the conductive material area.
[0081] Preparation of electrode cross-section samples A solution containing an epoxy-based polymer having a weight-average molecular weight of about 700 g / mol or less was prepared as a polymer containing an epoxy group.
[0082] The positive electrodes prepared in Examples 1 to 6 above were impregnated with the prepared epoxy polymer solution to fill the pores with the polymer. Then, using an ion milling device (IB19520CCP, Jeol Co.) that irradiates an argon ion beam, the positive electrodes for secondary batteries were irradiated with a focused argon (Ar) ion beam to scrape off the surface, and a cross-sectional sample with a clean cross section was prepared. In the argon ion beam irradiation, the ion beam current was set to 170 μA, and the gas flow rate was 1.5 cm. 3 / min and irradiation was carried out for 3 hours.
[0083] SSRM analysis conditions Equipment used: cypher ES (Oxford Instrument), Dual-gain ORCA cantilever holder [Parameters] Mode:contact Sample / line: 512×512, Scan rate: 0.5Hz Bias:~2V, Deflection Setpoint Volts:~0.2 Scan Angle: 90° [AFM Mode] Model: AD-40-As (Manufacturer: Adama) Tip: Highly doped (B) single crystal diamond, tip height 300nm Cantilever&bulk tip:diamond coated silicon, Reflexcoating(Au) F=180kHz, k=40N / m Typical contact resistance:~10kΩ
[0084] How SSRM is analyzed After ion milling, the sample was moved to a glove box under conditions not exposed to the atmosphere, and then loaded into an AFM puck. Then, silver (Ag) paste was applied between the electrode portion other than the fabricated cross section and the AFM puck to form an additional conductive path. Then, the sample with the additional conductive path formed was loaded into a closed cell body and attached to an AFM device while maintaining a state not exposed to the atmosphere. After laser alignment, the milled portion was selected as the measurement portion with an optical microscope and measured under Ar flow. SSRM images were obtained in this manner. Figures 3, 5, 7, and 1A are SSRM images of the electrodes of Examples 1, 2, 3, and 4, respectively. Also, the upper drawings of Figures 13 and 14 are SSRM images of the electrodes of Examples 5 and 6, respectively. The size of the observed images was 30 μm x 30 μm.
[0085] Masking conductive areas The conductive material regions were masked using Gwyddion software on the SSRM images obtained above.
[0086] First, a log(resistance) image was obtained, and a histogram of the log(resistance) distribution in the image was obtained. This was obtained using the Height distribution function of the Calculate 1D Statistical function provided by the software. A threshold was determined by adding 0.2 to the log(R / Ω) value corresponding to the lowest point between the peak corresponding to the conductive material and the peak corresponding to the electrode active material in the histogram. FIG. 2 shows a histogram for electrode 3, and log(R / Ω)=7.2 was set as the threshold. Based on this, the conductive material area was masked. In this case, the grain filtering function was used to delete areas corresponding to pixels smaller than 3 pixels, and areas located within the electrode active material were deleted. It was confirmed from FIG. 2 that pixels corresponding to the electrode active material and the conductive material were classified on the histogram obtained from the log scale image. In other words, it was found that the distribution of the conductive material area could be easily quantified using information on each pixel whose corresponding area was determined.
[0087] In addition, Fig. 1B is a diagram in which the conductive material regions are masked for the SSRM image of the electrode of Example 4, Fig. 4 is a diagram in which the SSRM image of the electrode of Example 1 (Fig. 3), Fig. 6 is a diagram in which the SSRM image of the electrode of Example 2 (Fig. 5), and Fig. 8 is a diagram in which the SSRM image of the electrode of Example 3 (Fig. 7) are masked, and only the masked conductive material regions are displayed in shades of color. In addition, the lower drawings in Figs. 13 and 14 are diagrams in which only the masked conductive material regions are displayed in shades of color in the electrodes of Examples 5 and 6, respectively.
[0088] Afterwards, the Grain-Summary function was used to check the perimeter and area of the masked region.
[0089] Next, the indexes 1 and 2 were calculated by substituting the respective values into the above [Formula 1] and [Formula 2], and the results are shown in the following [Table 1]. As can be seen from [Table 1], it was confirmed that the indexes 1 and 2 were calculated differently depending on the type and / or content of the conductive material in the electrode active material layer and the electrode manufacturing process, and the dispersion degree of the conductive material could be quantitatively confirmed. In this way, the conductive material index of the present invention can be used to quantitatively confirm the dispersion degree of the conductive material in the electrode. In addition, the conductive material dispersion index can be used to select the content and / or type of the conductive material during electrode manufacturing, select the electrode manufacturing method, and set the electrode manufacturing process conditions.
[0090] [Table 1] [Explanation of symbols]
[0091] 10 electrodes 11 Electrode active material layer 11s The area from the surface to a specified depth 11f Part of the current collector at a specified height from the opposing part 12 Current collector
Claims
1. In an electrode for an electrochemical element including an electrode active material layer including an electrode active material and a conductive material, the perimeter (boundary measured A method for evaluating the degree of dispersion of a conductive material based on a mathematical formula defined using the surface area (A) and surface area (B) as variables.
2. The method for evaluating the dispersibility of a conductive material according to claim 1, wherein the formula is a dispersibility index 1 (Index 1) of the conductive material according to the following [Formula 1], or a dispersibility index 2 of the conductive material according to the following [Formula 2]. [Formula 1] Index 1 (μm -1 )=Boundary measured / A [Formula 2] Index 2=Boundary measured / L circle In the above formula 1, Boundary measured means the perimeter of a portion defined as a conductive material region measured at a predetermined cross section of the electrode active material layer, and A means the area of a portion defined as a conductive material region measured at a predetermined cross section of the electrode active material layer. In the above [Formula 2], Boundary measured is the same as in formula 1 above, and L circle is the circumference of a circle having the same area as the area of the conductive material region defined above. [0010] It is.
3. (Step 1) obtaining a cross-sectional sample in which an arbitrary cross section of the inside of an electrode active material layer is exposed; (Step 2) obtaining a 2D scale map of the resistance distribution of the sample cross section; (Step 3) masking the conductive material area; (Step 4) calculating the perimeter and area of the masked region and substituting the calculated perimeter and area into the above formula 1 and / or formula 2 to confirm the degree of dispersion of the conductive material in the electrode active material layer; The method for evaluating the dispersion degree of the conductive material according to claim 1 , comprising:
4. 4. The method for evaluating a dispersion degree of a conductive material according to claim 1, wherein the electrode active material layer is formed on any one of side surfaces of an electrode current collector, and the cross section (or a plurality of cross sections) is a parallel plane or a perpendicular plane to a facing portion of the electrode active material layer with respect to the current collector.
5. 4. The method for evaluating the dispersion degree of a conductive material according to claim 3, wherein the cross-sectional sample is prepared by etching the electrode surface to a predetermined depth by ion milling.
6. 4. The method for evaluating the dispersion degree of the conductive material according to claim 3, wherein the step of obtaining a 2D-scale map of the resistance distribution of the cross-section of the sample is performed by scanning spreading resistance microscopy, which scans the surface of the cross-section sample using an AFM (Atomic force microscopy) device.
7. The step of masking the conductive material region comprises: A first step of converting and processing the resistance value data obtained in the step 2 into a log scale image (log (resistance) image); A second step of extracting a log resistance distribution histogram in which materials constituting the sample at the electrode cross section are displayed in a divided manner from the log scale image; a third step of masking a region having a value smaller than a log(R / Ω) value corresponding to a minimum value between a conductive material peak and an electrode active material peak in the [log resistance distribution histogram] as a threshold value as a conductive material region; The method for evaluating the dispersion degree of the conductive material according to claim 3, comprising:
8. The method for evaluating the degree of dispersion of a conductive material according to claim 7 , further comprising the step of correcting the threshold value by adding a value of 0.1 to 0.5 to the minimum value.
9. 2. The method for evaluating the dispersion degree of a conductive material according to claim 1, wherein the electrode for an electrochemical element comprises a current collector and an electrode active material layer formed on at least one surface of the current collector, the electrode active material layer comprising an electrode active material, a conductive material, and a binder.
10. The method for evaluating the dispersion degree of a conductive material according to claim 1 , wherein the cross section is in a direction parallel or perpendicular to a facing portion of the electrode active material layer against the current collector.
Citation Information
Patent Citations
Degree-of-dispersion inspecting apparatus for particles of electricity storage material in electricity storage device
CN104778730A
Negative electrode mix for lithium battery, negative electrode for lithium battery, lithium battery, device, and manufacturing method of negative electrode mix for lithium battery
JP2009283344A
Device for inspecting dispersion degree of particle of electricity storage material in power storage device
JP2015133253A
Negative electrode
JP2020119774A
Device and method for predicting the order quantity of store material
KR1020230111559A