Polarizing plate and its uses

The polarizing plate with a scattering adhesive layer addresses rainbow unevenness in OLED displays by enhancing visibility and durability through a crosslinked structure and refractive index difference, improving hardness and resistance to heat and humidity.

JP2024537103AInactive Publication Date: 2024-10-10LG CHEM LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024520045
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-06-30
Filing Date
2022-10-17
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

OLED display devices experience rainbow unevenness and poor visual appearance due to increased brightness, lacking in hardness, heat resistance, and humidity resistance.

Method used

A polarizing plate comprising a polarizer with a scattering adhesive layer containing scattering particles, which includes a crosslinked structure formed by a crosslinkable polymer and a multifunctional crosslinking agent, and beads with a refractive index difference, achieving a haze of 12% to 50% and a storage modulus of 120,000 Pa or more.

Benefits of technology

The polarizing plate improves rainbow unevenness, enhances visibility, and provides excellent hardness, heat resistance, and humidity resistance, maintaining optical properties and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537103000001_ABST
    Figure 2024537103000001_ABST
Patent Text Reader

Abstract

The present application relates to a polarizing plate and its use. The present application provides a polarizing plate that can solve the problem of rainbow unevenness occurring in the appearance of an OLED display device and exhibit excellent luminance, excellent hardness, excellent heat resistance, and excellent durability against humidity and heat, and an OLED display device including the polarizing plate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to a polarizing plate and its uses.

[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0137841 filed on October 15, 2021, and Korean Patent Application No. 10-2022-0080538 filed on June 30, 2022, and all contents disclosed in the documents of the relevant Korean patent applications are incorporated herein by reference. [Background technology]

[0003] In order to improve the brightness of an OLED (Organic Light Emitting Diode) display device, various methods have been attempted to improve the performance of an OLED display panel. However, when the brightness of an OLED display panel increases, a rainbow unevenness phenomenon that does not previously occur becomes more pronounced, and the unevenness phenomenon can cause a problem of poor visibility of the appearance of the OLED display device (Patent Document 1: Korean Patent Publication No. 10-2009-0122138). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Korean Patent Publication No. 10-2009-0122138 Summary of the Invention [Problem to be solved by the invention]

[0005] The present application provides a polarizing plate that can solve the problem of rainbow unevenness occurring in the appearance of an OLED display device, and exhibits excellent luminance, excellent hardness, excellent heat resistance, and excellent durability against moist heat, and an OLED display device including the polarizing plate. [Means for solving the problem]

[0006] The present application relates to a polarizing plate. The polarizing plate may include a polarizer and a scattering adhesive layer on one surface of the polarizer.

[0007] In the present specification, the adhesive layer may be, for example, a layer of an adhesive composition. In the present specification, the term "adhesive or adhesive composition layer" may mean a layer formed by coating or curing an adhesive or adhesive composition. The term "curing of an adhesive or adhesive composition" may mean realizing a crosslinked structure in an adhesive or adhesive composition through a physical or chemical action or reaction of components contained in the adhesive or adhesive composition. Curing may be induced, for example, by maintaining at room temperature, applying moisture, applying heat, irradiating with active energy rays, or by proceeding with two or more of the above processes together, and the type of adhesive or adhesive composition in which curing is induced depending on each case may be called, for example, a room temperature curing adhesive or adhesive composition, a moisture curing adhesive or adhesive composition, a heat curing adhesive or adhesive composition, an active energy ray curing adhesive or adhesive composition, or a hybrid curing adhesive or adhesive composition.

[0008] In the present specification, the scattering adhesive layer may refer to an adhesive layer containing scattering particles capable of inducing haze in the adhesive layer. The scattering particles may be, for example, beads, which will be described later.

[0009] The polarizing plate including the scattering adhesive layer may have a haze of 12% or more. The haze does not mean the haze of the scattering adhesive layer itself, but may mean the haze of the polarizing plate including the scattering adhesive layer and the polarizer. When the polarizing plate further includes a functional layer such as a protective film, a retardation layer, and a hard layer as described below, the haze may mean the haze of the polarizing plate including the scattering adhesive layer, the polarizer, and the functional layer. Specifically, the haze may be 12% or more, 14% or more, 16% or more, 18% or more, 20% or more, 21% or more, 22% or more, 23% or more, 24% or more, 25% or more, 26% or more, 27% or more, 28% or more, 29% or more, 30% or more, 31% or more, 32% or more, 33% or more, 34% or more, 35% or more, 36% or more, 37% or more, 38% or more, 39% or more, or 40% or more, and may be 50% or less, 48% or less, 46% or less, 44% or less, 42% or less, 40% or less, 38% or less, 36% or less, 34% or less, 32% or less, 30% or less, 28% or less, 26% or less, 24% or less, 22% or less, or 20% or less. The haze of the polarizing plate may be a value measured based on a D65 light source. The haze of the polarizing plate may be a value measured based on a D65 light source. The haze of the polarizing plate may be a value measured for light with a wavelength of about 380 nm to 780 nm. The haze may be an average haze value measured for light with a wavelength of about 380 nm to 780 nm. When the haze of the polarizing plate is within the above range, it may be advantageous to improve the problem of rainbow unevenness occurring in the appearance of the OLED display device and to exhibit excellent luminance, excellent hardness, excellent heat resistance, and excellent durability against moist heat.

[0010] The scattering adhesive layer may have a storage modulus of 120,000 Pa or more at a temperature of 25° C. and a frequency of 1 rad / sec. Specifically, the storage modulus may be 125,000 Pa or more, 130,000 Pa or more, 135,000 Pa or more, 140,000 Pa or more, 145,000 Pa or more, 150,000 Pa or more, 151,000 Pa or more, 152,000 Pa or more, 153,000 Pa or more, or 154,000 Pa or more. The upper limit of the storage modulus may be, for example, 200,000 Pa or less, 190,000 Pa or less, 180,000 Pa or less, 170,000 Pa or less, 160,000 Pa or less, 155,000 Pa or less, or 153,000 Pa or less. When the storage modulus of the scattering adhesive layer is within the above range, the problem of rainbow unevenness occurring in the appearance of the OLED display device can be improved, and it can be advantageous to exhibit excellent visibility, excellent hardness, excellent heat resistance, and excellent durability against moist heat.

[0011] The scattering adhesive layer may include an adhesive resin. As one example, the adhesive resin may be an acrylic resin. The acrylic resin may be a polymer that contains an acrylic monomer as a main component and exhibits adhesiveness before or after crosslinking. In the present specification, containing an acrylic monomer as a main component may mean that the acrylic monomer is contained in an amount of 80 wt% or more, 85 wt% or more, 90 wt% or more, 95 wt% or more, or 99 wt% or more of the total monomers constituting the adhesive resin.

[0012] The adhesive resin may have an IPN (interpenetrating network) crosslinked structure. In this specification, the IPN crosslinked structure may refer to a state in which two or more crosslinked structures are simultaneously realized in the adhesive layer. The two or more crosslinked structures in the IPN may be, for example, in an entanglement state, in a physically or chemically linked state, or in a penetrating state.

[0013] The IPN crosslinked structure may include a first crosslinked structure formed by a crosslinking reaction between a crosslinkable polymer and a multifunctional crosslinking agent, and a second crosslinked structure formed by a polymerization reaction of a radical polymerizable compound. The polymerization reaction of the radical polymerizable compound may be induced by a polymerization initiator. In order for the pressure-sensitive adhesive layer to have the IPN crosslinked structure, the pressure-sensitive adhesive composition for forming the pressure-sensitive adhesive layer may include a crosslinkable polymer, a multifunctional crosslinking agent, a radical polymerizable compound, and a polymerization initiator. In the present specification, a multifunctional crosslinking agent may mean a crosslinking agent having two or more crosslinkable functional groups.

[0014] In one example, the first crosslinked structure may be a crosslinked structure formed by application of heat, and the second crosslinked structure may be a crosslinked structure formed by irradiation of active energy rays. The category of "active energy rays" may include microwaves, infrared rays, ultraviolet rays, X-rays, and gamma rays, as well as particle beams such as alpha-particle beams, proton beams, neutron beams, and electron beams, and typically may be ultraviolet rays or electron beams.

[0015] In the present specification, the term "crosslinkable polymer" refers to a polymer having a crosslinkable functional group capable of reacting with a multifunctional crosslinking agent. The crosslinkable functional group and the crosslinking agent may be selected so as to react with each other than a radical reaction to realize a crosslinked structure, for example, they may react with each other through a drying or aging process to form a crosslinked structure.

[0016] The crosslinkable polymer may have a weight average molecular weight of, for example, 1,000,000 or less. The weight average molecular weight is a polystyrene equivalent value measured by GPC (gel permeation chromatography). The lower limit of the weight average molecular weight of the polymer is not particularly limited, and may be adjusted to, for example, 200,000 or 300,000 or more.

[0017] The crosslinkable polymer may include polymerized units derived from a (meth)acrylic acid ester monomer. As used herein, the term "monomer" refers to any type of compound capable of forming a polymer through a polymerization reaction, and a polymer including polymerized units derived from a certain monomer may refer to a polymer formed by polymerizing the certain monomer.

[0018] The (meth)acrylic acid ester compound may be, for example, an alkyl (meth)acrylate. The alkyl (meth)acrylate may be, for example, an alkyl (meth)acrylate having an alkyl group having 1 to 20 carbon atoms, 1 to 14 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, taking into consideration the adjustment of cohesive strength, glass transition temperature, and adhesiveness. The alkyl group may be, for example, a straight-chain alkyl group, a branched-chain alkyl group, or a cyclic alkyl group. Examples of such monomers include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, sec-butyl acrylate, 2-methylheptyl acrylate, pentyl acrylate, 2-ethylhexyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, n-octyl (meth)acrylate, isobornyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, and lauryl (meth)acrylate, and one or more of the above may be appropriately selected and used.

[0019] The crosslinkable polymer may further include a polymerized unit derived from a copolymerizable monomer having a crosslinkable functional group (hereinafter, may be referred to as a crosslinkable monomer). In this specification, the copolymerizable monomer having a crosslinkable functional group may mean a compound that has a site that can be copolymerized with other monomers contained in the polymer, such as the (meth)acrylic acid ester monomer, and has a crosslinkable functional group to impart a crosslinkable functional group to the polymer. Examples of the crosslinkable functional group include a hydroxy group, a carboxy group, an isocyanate group, a glycidyl group, an amine group, an alkoxysilyl group, or a vinyl group, and generally, a hydroxy group or a carboxy group may be used.

[0020] The crosslinkable monomer may be a copolymerizable monomer having a hydroxyl group. The copolymerizable monomer having a hydroxyl group may be a hydroxyalkyl (meth)acrylate such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, or 8-hydroxyoctyl (meth)acrylate, or a hydroxyalkylene glycol (meth)acrylate such as 2-hydroxyethylene glycol (meth)acrylate or 2-hydroxypropylene glycol (meth)acrylate. According to an embodiment of the present application, among the above monomers, a hydroxyalkyl acrylate or a hydroxyalkylene glycol acrylate may be used in consideration of reactivity with other monomers and ease of adjustment of the glass transition temperature.

[0021] In one example, the crosslinkable polymer may include polymerization units derived from 80 to 99 parts by weight of the (meth)acrylic acid ester monomer and 1 to 20 parts by weight of the crosslinkable monomer. In another example, the crosslinkable polymer may include polymerization units derived from 80 to 99 parts by weight of the (meth)acrylic acid ester monomer and 1 to 10 parts by weight of the crosslinkable monomer. In another example, the crosslinkable polymer may include polymerization units derived from 90 to 99 parts by weight of the (meth)acrylic acid ester monomer and 1 to 10 parts by weight of the crosslinkable monomer. Within this range, the pressure-sensitive adhesive layer may realize a suitable crosslinked structure.

[0022] The crosslinkable polymer may further include other optional comonomers, if necessary, for example, to adjust appropriate physical properties, etc. Examples of the comonomer include alkylene oxide group-containing monomers such as alkoxyalkylene glycol (meth)acrylates, alkoxydialkylene glycol (meth)acrylates, alkoxytrialkylene glycol (meth)acrylates, alkoxytetraalkylene glycol (meth)acrylates, alkoxypolyethylene glycol (meth)acrylates, phenoxyalkylene glycol (meth)acrylates, phenoxydialkylene glycol (meth)acrylates, phenoxytrialkylene glycol (meth)acrylates, phenoxytetraalkylene glycol (meth)acrylates, or phenoxypolyalkylene glycol (meth)acrylates; styrene-based monomers such as styrene or methylstyrene; glycidyl group-containing monomers such as glycidyl (meth)acrylate; or carboxylate vinyl esters such as vinyl acetate, but are not limited thereto. One or more suitable types of such comonomers may be selected as necessary and included in the polymer, and the comonomer may be included in the polymer in an amount of, for example, 20 parts by weight or less, or 0.1 to 15 parts by weight, based on the total weight of other compounds used as polymerization units in the polymer.

[0023] The crosslinkable polymer can be produced by selecting necessary monomers from the above-mentioned monomers, mixing the selected monomers in a desired ratio, and subjecting the mixture to a polymerization method such as solution polymerization, photo polymerization, bulk polymerization, suspension polymerization, or emulsion polymerization.

[0024] The scattering adhesive layer may include a multifunctional crosslinking agent (hardening agent) that reacts with the crosslinkable polymer to form a crosslinked structure.

[0025] The type of specific crosslinking agent that can be used in the present application is not particularly limited, and may be selected in consideration of the type of crosslinkable functional group contained in the crosslinkable polymer. As the crosslinking agent, for example, a general crosslinking agent such as an isocyanate crosslinking agent, an epoxy crosslinking agent, an aziridine crosslinking agent, and a metal chelate crosslinking agent may be used. For example, an isocyanate crosslinking agent may be used, but is not limited thereto. Specific examples of the isocyanate crosslinking agent include one or more selected from the group consisting of tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isoboron diisocyanate, tetramethylxylene diisocyanate, naphthalene diisocyanate, and a reaction product of any one of the above with a polyol (e.g., trimethylolpropane); specific examples of the epoxy crosslinking agent include ethylene glycol diglycidyl ether, triglycidyl ether, trimethylolpropane triglycidyl ether, and the like. ether, N,N,N',N'-tetraglycidylethylenediamine, and glycerin diglycidyl ether; specific examples of the aziridine crosslinker include, but are not limited to, one or more selected from the group consisting of N,N'-toluene-2,4-bis(1-aziridinecarboxamide), N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), triethylenemelamine, bisisopropyl-1-(2-methylaziridine), and tri-1-aziridinylphosphine oxide. Specific examples of the metal chelate crosslinker include, but are not limited to, compounds in which a polyvalent metal such as aluminum, iron, zinc, tin, titanium, antimony, magnesium, and / or vanadium is coordinated to acetylacetone or ethyl acetoacetate.

[0026] The crosslinking agent may be included in an amount of 0.01 to 10 parts by weight or 0.01 to 5 parts by weight based on 100 parts by weight of the crosslinkable polymer. If the content of the crosslinking agent is less than 0.01 parts by weight, the cohesive strength of the adhesive layer may decrease, and if it exceeds 10 parts by weight, interlayer peeling or lifting may occur, resulting in a decrease in durability and reliability.

[0027] The second crosslinked structure may be formed by a polymerization reaction of a radical polymerizable compound. That is, the pressure-sensitive adhesive layer may further include a polymer of a multifunctional radical polymerizable compound having two or more, for example, 2 to 6, radical polymerizable functional groups in order to realize an IPN structure, and may also include a radical initiator for inducing polymerization of the radical polymerizable compound.

[0028] The type of the radically polymerizable compound is not particularly limited, but for example, a polyfunctional acrylate having 2 to 6 (meth)acryloyl groups as the radically polymerizable functional group can be used.

[0029] The type of the multifunctional acrylate is not particularly limited, and examples thereof include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentylglycol adipate di(meth)acrylate, hydroxypivalic acid, and the like. acid) neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, caprolactone modified dicyclopentenyl di(meth)acrylate, ethylene oxide modified di(meth)acrylate, di(meth)acryloxyethyl isocyanurate, allyl cyclohexyl di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, ethylene oxide modified hexahydrophthalic acid di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, neopentyl glycol modified trimethylpropane di(meth)acrylate, adamantane di(meth)acrylate or 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorine, etc. difunctional acrylates such as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, trifunctional urethane (meth)acrylate or tris(meth)acryloxyethyl isocyanurate; tetrafunctional acrylates such as diglycerol tetra(meth)acrylate or pentaerythritol tetra(meth)acrylate; pentafunctional acrylates such as propionic acid modified dipentaerythritol penta(meth)acrylate; and dipentaerythritol hexa(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate or urethane (meth)acrylate (ex.Examples of suitable functional acrylates include, but are not limited to, the reaction product of an isocyanate monomer and trimethylolpropane tri(meth)acrylate.

[0030] In the present application, one or more of the multifunctional acrylates may be used in combination. In particular, it is advantageous to use an acrylate having a molecular weight of 5,000 or less, 4,000 or less, 3,000 or less, 2,000 or less, or 1,000 or less and a functionality of 3 or more in terms of realizing durability.

[0031] The polyfunctional acrylate may be a polyfunctional acrylate having a cyclic structure and / or a urethane bond in its molecular structure. The cyclic structure contained in the acrylate is not particularly limited and may be a carbocyclic structure or a heterocyclic structure; or a monocyclic or polycyclic structure. Specifically, examples of the cyclic structure contained in the polyfunctional acrylate include cycloalkyl ring structures having 3 to 12 carbon atoms, preferably 3 to 8 carbon atoms, such as cyclopentane, cyclohexane, or cycloheptane, and the acrylate may contain one or more, for example, 1 to 5 or 1 to 3, of the cyclic structures, and may contain one or more heteroatoms such as O, S, or N.

[0032] Specific examples of polyfunctional acrylates containing a ring structure include monomers having an isocyanurate structure such as tris(meth)acryloxyethyl isocyanurate, and isocyanurate-modified urethane acrylates (e.g., reaction products of an isocyanate compound having a ring structure in the molecule (e.g., isoboron diisocyanate) and an acrylate compound (e.g., trimethylolpropane tri(meth)acrylate or pentaerythritol tri(meth)acrylate)), but are not limited thereto.

[0033] The scattering adhesive layer may contain the radical polymerizable compound in an amount of 3 to 25 parts by weight based on 100 parts by weight of the crosslinkable polymer. In this range, an IPN structure that can secure suitable physical properties may be realized.

[0034] The type of radical initiator capable of inducing the polymerization reaction of the radical polymerizable compound is not particularly limited. For example, one or more selected from the group consisting of photoinitiators and thermal initiators can be used as the radical initiator, and the photoinitiator and thermal initiator may be used simultaneously as necessary. For example, the initiator may be included in an amount of 0.1 parts by weight to 10 parts by weight based on 100 parts by weight of the radical polymerizable compound, but is not limited thereto.

[0035] As the photoinitiator, any photoinitiator can be used as long as it can induce the polymerization reaction of the radical polymerizable compound described above during the curing process by irradiation with light, etc., to realize the second crosslinking structure. For example, benzoin-based, hydroxyketone-based, aminoketone-based, or phosphine oxide-based photoinitiators can be used. Specifically, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylacenoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2 ... ketone, benzophenone, p-phenylbenzophenone, 4,4-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide. In the present application, one or more of the above may be used, but is not limited thereto.

[0036] The thermal initiator is not particularly limited and may be appropriately selected in consideration of the properties to be realized. For example, a thermal initiator having a 10-hour half-life temperature of 40° C. or more and less than 100° C. may be used. By setting the half-life temperature of the thermal initiator as above, the pot-life can be sufficiently secured and the drying temperature for decomposition of the thermal initiator can be appropriately maintained.

[0037] The type of thermal initiator is not particularly limited as long as it has the above-mentioned physical properties, and for example, a typical initiator such as an azo compound, a peroxide compound, or a redox compound can be used. Examples of the azo compounds include 2,2-azobis(2-methylbutyronitrile), 2,2-tolylazobis(isobutyronitrile), 2,2-tolylazobis(2,4-dimethylvaleronitrile), 2,2-nitrazobis-2-hydroxymethylpropionitrile, dimethyl-2,2-methylazobis(2-methylpropionate), and 2,2-ioazobis(4-methoxy-2,4-dimethylvaleronitrile). Examples of the peroxide compounds include inorganic peroxides such as potassium perlactate, ammonium persulfate, and hydrogen peroxide; or diacyl peroxides, peroxydicarbonates, peroxyesters, tetramethylbutylperoxyneodecanoate (e.g., Perocta ND, manufactured by NOF), bis(4-butylcyclohexyl)peroxydicarbonate (e.g., Perocta ND, manufactured by NOF), and the like. TCP, NOF (manufactured)), di(2-ethylhexyl) peroxycarbonate, butyl peroxyneodecanoate (ex. Perbutyl ND, NOF (manufactured)), dipropyl peroxydicarbonate (ex. Peroyl NPP, NOF (manufactured)), diisopropyl peroxydicarbonate (ex. Peroyl IPP, NOF (manufactured)), diethoxyethyl peroxydicarbonate (ex. Peroyl EEP, NOF (manufactured)), diethoxyhexyl peroxydicarbonate (ex. Peroyl OEP, NOF (manufactured)), hexyl peroxydicarbonate (ex. Perhexyl ND, NOF (manufactured)), dimethoxybutyl peroxydicarbonate (ex. Peroyl MBP, NOF (manufactured)), bis(3-methoxy-3-methoxybutyl) peroxydicarbonate (ex. Peroyl SOP, NOF Co., Ltd.), dibutyl peroxydicarbonate, dicetyl peroxydicarbonate, dimyristyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxypivalate, hexyl peroxypivalate (ex.Perhexyl PV, NOF), butyl peroxypivalate (ex. Perbutyl, NOF), trimethylhexanoyl peroxide (ex. Peroyl 355, NOF), dimethylhydroxybutyl peroxyneodecanoate (ex. Luperox 610M75, Atofina), amyl peroxyneodecanoate (ex. Luperox 546M75, Atofina), butyl peroxyneodecanoate (ex. Luperox 10M75, Atofina), t-butyl peroxyneoheptanoate, amyl peroxypivalate (ex. Luperox Examples of organic peroxides include organic peroxides such as 546M75, Alofina, t-butyl peroxypivalate, t-amyl peroxy-2-ethylhexanoate, lauryl peroxide, dilauroyl peroxide, didecanoyl peroxide, benzoyl peroxide, and dibenzoyl peroxide, and examples of redox compounds include mixtures of peroxide compounds and reducing agents, but are not limited thereto. In the present application, one or a mixture of two or more of the above azo, peroxide, or redox compounds may be used.

[0038] If necessary, the scattering adhesive layer may further include one or more additives selected from the group consisting of known antistatic agents, silane coupling agents, tackifier resins, epoxy resins, UV stabilizers, antioxidants, color-matching agents, reinforcing agents, fillers, defoamers, surfactants, and plasticizers in addition to the above-mentioned components. The scattering adhesive layer may further include beads. The storage modulus of the scattering adhesive layer and the haze of the polarizing plate may refer to the storage modulus of the adhesive layer and the haze of the polarizing plate in a state where the beads are included. The refractive index of the beads may be different from that of the crosslinkable polymer and / or the polymer of the radical polymerizable compound. The adhesive layer may include beads to impart haze to the adhesive layer, thereby improving the visibility of rainbow unevenness that may occur during the manufacture of an OLED display device.

[0039] In one embodiment, the difference (AB) between the refractive index (A) of the crosslinkable polymer and the refractive index (B) of the beads may be 0.05 or more. The larger the refractive index difference between the crosslinkable polymer and the beads, the more advantageous it is for realizing haze, so that even a small amount of the beads can realize high haze. The upper limit of the refractive index difference (AB) may be, for example, 0.1 or less. The refractive index is a value measured using an Abbe refractometer at a temperature of 25° C. for a light source having a wavelength of 350 nm to 1450 nm. If the refractive index difference is too small, it is difficult to realize a desired level of haze, and if the refractive index difference is too large, the optical properties may be deteriorated due to loss of light traveling straight ahead, so that the refractive index difference may be within the above range. In one embodiment, the refractive index of the beads may be within a range of 1.415 to 1.425.

[0040] The content of the beads may be appropriately selected within a range that does not impair the object of the present application. In one example, the beads may be included in a range of 1 to 3 parts by weight when the weight of the total components of the scattering adhesive is 100 parts by weight. In this specification, the weight of the total components of the scattering adhesive may mean the sum of the weights of all crosslinkable polymers, radical polymerizable compounds, crosslinking agents, initiators, additives and beads contained in the scattering adhesive. Alternatively, in this specification, the weight of the total components of the scattering adhesive layer may mean the sum of the weights of all components excluding the solvent from the adhesive composition. More specifically, the beads may be included in an amount of 1 part by weight or more, 1.2 parts by weight or more, 1.4 parts by weight or more, 1.5 parts by weight or more, 1.6 parts by weight or more or 1.8 parts by weight or more, and 3 parts by weight or less, 2.8 parts by weight or less, 2.6 parts by weight or less, 2.4 parts by weight or less or 2.2 parts by weight or less, based on 100 parts by weight of the total components of the scattering adhesive. In another example, the beads may be included in an amount of 3 parts by weight or more relative to 100 parts by weight of the adhesive resin. Specifically, the beads may be included in an amount of 3.1 parts by weight or more, 3.2 parts by weight or more, 3.4 parts by weight or more, 3.6 parts by weight or more, 3.8 parts by weight or more, 4.0 parts by weight or more, 4.2 parts by weight or more, 4.4 parts by weight or more, 4.6 parts by weight or more, 4.8 parts by weight or more, 5.0 parts by weight or more, 5.2 parts by weight or more, 5.4 parts by weight or more, 5.6 parts by weight or more, 5.8 parts by weight or more, or 6.0 parts by weight or more relative to 100 parts by weight of the adhesive resin, and may be included in an amount of 10 parts by weight or less, 9.5 parts by weight or less, 9 parts by weight or less, 8.5 parts by weight or less, 8 parts by weight or less, 7.5 parts by weight or less, 7 parts by weight or less, 6.5 parts by weight or less, 6 parts by weight or less, 5.5 parts by weight or less, 5 parts by weight or less, 4.5 parts by weight or less, 4 parts by weight or less, or 3.5 parts by weight or less. When the bead content is within the above range, it is advantageous to improve the problem of rainbow unevenness occurring in the appearance of the OLED display device and to exhibit excellent visibility, excellent hardness, excellent heat resistance, and excellent durability against humidity and heat. On the other hand, when the bead content is excessively high, there is a possibility that a camera may recognize the beads during the attachment process and erroneously set the reference line, resulting in an attachment error, so it is advantageous to keep the bead content within the above range.

[0041] In one embodiment, the beads may be organic beads. The organic beads may include, for example, a silicone resin. The silicone resin may include, for example, a silsesquioxane. The silsesquioxane may be [RSiO 3 / 2 ]n, where R=H, alkyl, aryl, or alkoxy. In one embodiment, the silicone resin can be polymethylsilsesquioxane.

[0042] In one embodiment, the beads may be spherical particles. The size of the beads may be appropriately selected within a range that does not impair the object of the present application. In one embodiment, the average particle size (D50) of the beads may be 6 μm or less. Specifically, the average particle size (D50) of the beads may be 5.8 μm or less, 5.6 μm or less, 5.4 μm or less, 5.2 μm or less, 5.0 μm or less, 4.8 μm or less, 4.6 μm or less, 4.4 μm or less, 4.2 μm or less, 4.0 μm or less, 3.8 μm or less, 3.6 μm or less, 3.4 μm or less, 3.2 μm or less, 3.0 μm or less, 2.9 μm or less, 2.8 μm or less, 2.7 μm or less, 2.6 μm or less, or 2.5 μm or less. The average particle size (D50) of the beads may be, for example, 1 μm or more, 1.5 μm or more, 2.0 μm or more, or 2.2 μm or more. When the average particle size of the beads is within the above range, it is advantageous to improve the problem of rainbow unevenness occurring in the appearance of the OLED display device and to exhibit excellent visibility, excellent hardness, excellent heat resistance, and excellent durability against humidity and heat. Meanwhile, in terms of preventing the sparkling phenomenon and / or camera recognition errors during the attachment process, the average particle size (D50) of the beads may be 3 μm or less, 2.5 μm or less, or 2.0 μm or less.

[0043] The thickness of the scattering adhesive layer may be within a range of 15 μm to 25 μm. Specifically, the thickness of the scattering adhesive layer may be 16 μm or more, 17 μm or more, or 18 μm or more, and 24 μm or less, 23 μm or less, or 22 μm or less. When the thickness of the scattering adhesive layer is within the above range, it may be advantageous to improve the problem of rainbow unevenness occurring in the appearance of the OLED display device, and to exhibit excellent visibility, excellent hardness, excellent heat resistance, and excellent durability against moist heat.

[0044] The scattering adhesive layer may have excellent hardness. In one example, the scattering adhesive layer may have a glass pressing distance of 210 μm or less measured at 800 gf for 1000 seconds. The glass pressing distance may be specifically 205 μm or less, 200 μm or less, 195 μm or less, or 190 μm or less. The lower the glass pressing distance, the higher the hardness of the sample, and when the hardness of the adhesive layer is high, there is an advantage that the deformation of the adhesive layer is minimized because the resistance to external deformation is high. The lower limit of the glass pressing distance may be, for example, 160 μm or more, 170 μm or more, 180 μm or more, 190 μm or more, or 195 μm or more.

[0045] The polarizing plate may have excellent durability. As one example, the polarizing plate may have a haze change rate after heat resistance, ΔHa, as expressed by Equation 1, and a haze change rate after wet heat resistance, ΔHb, as expressed by Equation 2, of 2% or less. Specifically, ΔHa may be 1.8% or less, 1.6% or less, 1.4% or less, or 1.2% or less. Specifically, ΔHb may be 1.8% or less, 1.6% or less, 1.4% or less, 1.2% or less, 1.0% or less, 0.8% or less, 0.6% or less, or 0.4% or less.

[0046] [Formula 1] △Ha=(H1-H2) / H1×100% [Formula 2] △Hb=(H3-H4) / H3×100% In Equation 1, H1 is the haze of the polarizing plate at a temperature of 25° C., and H2 is the haze of the polarizing plate after storage for 500 hours at a temperature of 80° C. In Equation 2, H3 is the haze of the polarizing plate at a temperature of 25° C., and H4 is the haze of the polarizing plate after storage for 500 hours at a temperature of 60° C. and a relative humidity of 90%.

[0047] The term "polarizer" as used herein means a film, sheet, or element having a polarizing function. A polarizer is a functional element that can extract light vibrating in one direction from incident light vibrating in various directions.

[0048] The polarizer may be an absorptive polarizer. In this specification, an absorptive polarizer refers to an element that exhibits selective transmission and absorption characteristics for incident light. The absorptive polarizer can transmit light that vibrates in one direction among incident light that vibrates in various directions, and absorb light that vibrates in the remaining directions.

[0049] The polarizer may be a linear polarizer. In this specification, a linear polarizer refers to a polarizer that selectively transmits light that is linearly polarized light vibrating in one direction and selectively absorbs light that is linearly polarized light vibrating in a direction perpendicular to the vibration direction of the linearly polarized light.

[0050] The polarizer may be, for example, a polarizer in which a polymer stretched film such as a PVA stretched film is dyed with iodine, or a guest-host type polarizer in which a liquid crystal polymerized in an oriented state is used as a host and an anisotropic dye aligned along the orientation of the liquid crystal is used as a guest, but is not limited thereto.

[0051] The type of polyvinyl alcohol resin or its derivative for forming the PVA-based polarizer is not particularly limited, and any PVA resin or its derivative that has been known to be capable of forming a PVA-based polarizer can be used without any particular limitation. However, representative examples of the PVA-based resin derivative include polyvinyl formal resin and polyvinyl acetal resin. Additionally, the PVA-based polarizer may be formed using a PVA-based commercially available film that is commonly used in the art for manufacturing polarizers, such as P30, PE30, PE60 from Kuraray Co., Ltd., M2000, M3000, M6000 from Nippon Gosei Co., Ltd., etc.

[0052] The resin contained in the PVA-based polarizer may have a degree of polymerization of, for example, about 1,000 to 10,000, or within a range of 1,500 to 5,000. When the degree of polymerization is within the above range, the molecules move freely, which may be advantageous for flexibly mixing with iodine or a dichroic dye.

[0053] According to one embodiment of the present application, the polarizer may be a PVA stretched film. The transmittance or polarization degree of the polarizer may be appropriately adjusted in consideration of the object of the present application. For example, the transmittance of the polarizer may be 42.5% to 55%, and the polarization degree may be 65% to 99.9997%. The transmittance and polarization degree may be values ​​measured for light with a wavelength of about 550 nm.

[0054] In one embodiment, the polarizer may further include a protective film on one or both sides of the polarizer, and the protective film may be attached to the polarizer via an adhesive layer.

[0055] The protective film for the polarizer may be a triacetyl cellulose (TAC) film, a cyclic olefin polymer (COP) film, a cyclic olefin copolymer (COC) film, or an acrylic film. In consideration of excellent visibility and optical properties of the display device, it is preferable that the protective film for the polarizer has high transparency with a light transmittance of 85% to 100%.

[0056] The polarizing plate may further include a surface treatment layer. The surface treatment layer may be formed on one side of the protective film of the polarizer. Specifically, the surface treatment layer may be formed on one side of the protective film of the polarizer located on the opposite side of the polarizer where the scattering adhesive layer is formed. Examples of the surface treatment layer include, but are not limited to, a hard coating layer, a low reflection layer, an anti-glare layer, and an anti-fingerprint layer. The surface treatment layer may be disposed on the outermost edge of the polarizing plate.

[0057] The thickness of the protective film for the polarizer may be within a range of 20 μm to 100 μm. When the thickness of the protective film for the polarizer satisfies the above range, it is possible to ensure mechanical strength capable of protecting the polarizer and to ensure workability in a roll process.

[0058] The adhesive layer for attaching the polarizer and the protective film may be formed by any method that has been used to bond the polarizer and the protective film. As an example, the adhesive layer may be a UV-curable adhesive. The thickness of the adhesive layer may be 0.5 μm to 4.0 μm, and good coating uniformity may be ensured by the adhesive layer satisfying this range.

[0059] The polarizing plate may further include a retardation layer between the polarizer and the scattering adhesive layer. The retardation layer may be, for example, a liquid crystal layer or a stretched polymer layer. The liquid crystal layer may include a polymerizable liquid crystal compound in a polymerized state. In the present specification, the term "polymerizable liquid crystal compound" may mean a compound that includes a portion capable of exhibiting liquid crystallinity, such as a mesogen skeleton, and includes one or more polymerizable functional groups. The polymerizable functional group may be, for example, an acryloyl group, a methacryloyl group, an acryloyloxy group, or a methacryloyloxy group. As the stretched polymer layer, for example, a polymer layer including a polyolefin such as polyethylene or polypropylene, a cycloolefin polymer (COP: acryloyloxy group) such as polynorbornene, a polyester such as polyvinyl chloride, polyacrylonitrile, polysulfone, an acrylic resin, polycarbonate, or polyethylene terephthalate, a cellulose ester polymer such as polyacrylate, polyvinyl alcohol, or TAC (Triacetyl cellulose), or a copolymer of two or more monomers among the monomers forming the polymer may be used.

[0060] The retardation layer may have, for example, a quarter-wavelength phase retardation characteristic. In this specification, the term n-wavelength phase retardation characteristic means a characteristic that can retard the phase of incident light by n times the wavelength of the incident light at least in a part of the wavelength range. The quarter-wavelength phase retardation characteristic may be a characteristic that converts incident linearly polarized light into elliptically polarized light or circularly polarized light, and conversely, converts incident elliptically polarized light or circularly polarized light into linearly polarized light. In one example, the retardation layer may have a phase retardation of 90 nm to 300 nm for light with a wavelength of 550 nm. In other examples, the phase retardation may be 100 nm or more, 105 nm or more, 110 nm or more, 115 nm or more, 120 nm or more, 125 nm or more, or 130 nm or more. In addition, the phase difference can be 290 nm or less, 280 nm or less, 270 nm or less, 260 nm or less, 250 nm or less, 240 nm or less, 230 nm or less, 220 nm or less, 210 nm or less, 200 nm or less, 190 nm or less, 180 nm or less, 170 nm or less, 160 nm or less, 150 nm or less, or 145 nm or less.

[0061] The polarizing plate may further include a hard layer between the polarizer and the scattering adhesive layer. An example of the hard layer may be an adhesive layer. A UV-curable adhesive layer may be used as the adhesive layer. The thickness of the adhesive layer may be within a range of 0.5 μm to 4.0 μm, and by having the thickness of the adhesive layer satisfy this range, good coating uniformity can be ensured.

[0062] 1 to 3 each exemplarily show the structure of the polarizing plate of the present application. As shown in FIG. 1, the polarizing plate may include a scattering adhesive layer 100, a retardation layer 200, a polarizer protection film 300, a polarizer 400, a polarizer protection film 500, and a surface treatment layer 600 in this order. Alternatively, as shown in FIG. 2, the polarizing plate may include a scattering adhesive layer 100, a polarizer protection film 300, a polarizer 400, a polarizer protection film 500, and a surface treatment layer 600 in this order. Alternatively, as shown in FIG. 3, the polarizing plate may include a scattering adhesive layer 100, a hard layer 700, a polarizer 400, a polarizer protection film 500, and a surface treatment layer 600 in this order.

[0063] The polarizing plate may be provided with a release film attached to one side of the scattering adhesive layer, and the release film may be removed when the polarizing plate is attached to the display panel. The release film may protect the scattering adhesive layer before the polarizing plate is attached to the display panel. The release film may be any release film widely known in the art, such as, but not limited to, an acrylic film, a polyethylene terephthalate (PET) film, a triacetyl cellulose (TAC) film, a polynorbornene (PNB) film, a cycloolefin polymer (COP) film, a polycarbonate (PC) film, etc.

[0064] The present application also relates to an OLED display device. The OLED display device may include an OLED display panel and the polarizing plate disposed on one side of the OLED display panel. In this case, one side of the scattering adhesive layer of the polarizing plate may be in direct contact with the OLED display panel. The polarizing plate may be disposed on the viewing side of the OLED display panel. When the polarizing plate of the present application is applied to an OLED display device, it may be advantageous to improve the problem of rainbow unevenness occurring in the appearance of the OLED display device and to exhibit excellent visibility, excellent hardness, excellent heat resistance, and excellent durability against humidity and heat.

[0065] The OLED display panel may include a substrate, a lower electrode, an organic light-emitting layer, and an upper electrode, in that order. The organic light-emitting layer may include an organic material capable of emitting light when a voltage is applied to the lower electrode and the upper electrode. One of the lower electrode and the upper electrode may be an anode, and the other may be a cathode. The anode is an electrode into which holes are injected and may be made of a conductive material with a high work function, and the cathode is an electrode into which electrons are injected and may be made of a conductive material with a low work function. In general, the anode may be a transparent metal oxide layer such as ITO or IZO having a high work function, and the anode may be a metal electrode having a low work function. Generally, since the organic light-emitting layer is transparent, a transparent display may be realized when the upper and lower electrodes are made transparent. In one example, a transparent display may be realized when the thickness of the metal electrode is made very thin.

[0066] The OLED display panel may further include a sealing substrate that prevents moisture and / or oxygen from entering from the outside onto the upper electrode. Additional layers may be included between the lower electrode and the organic light-emitting layer and between the upper electrode and the organic light-emitting layer. The additional layers may include, but are not limited to, a hole transporting layer, a hole injecting layer, an electron injecting layer, and an electron transporting layer for balancing electrons and holes.

[0067] The polarizer may be disposed on the side where light is emitted from the OLED display panel. For example, in the case of a bottom emission structure where light is emitted toward the base substrate, the polarizer may be disposed on the outside of the base substrate, and in the case of a top emission structure where light is emitted toward the encapsulation substrate, the polarizer may be disposed on the outside of the encapsulation substrate. When the polarizer includes a retardation layer, it can prevent external light from being reflected by a reflective layer made of metal such as an electrode and wiring of the OLED panel and emitting to the outside of the OLED panel, thereby improving visibility and performance of the display device. Effect of the Invention

[0068] The present application relates to a polarizing plate and its use. The present application provides a polarizing plate that can solve the problem of rainbow unevenness occurring in the appearance of an OLED display device and exhibit excellent luminance, excellent hardness, excellent heat resistance, and excellent durability against humidity and heat, and an OLED display device including the polarizing plate. [Brief description of the drawings]

[0069] [Figure 1] 1 shows an example of the structure of the polarizing plate of the present application. [Diagram 2] 1 shows an example of the structure of the polarizing plate of the present application. [Diagram 3] 1 shows an example of the structure of the polarizing plate of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0070] Hereinafter, the present application will be described in detail through examples according to the present application and comparative examples not in accordance with the present application, but the scope of the present application is not limited to the examples presented below.

[0071] Example 1 100 parts by weight of a mixture of a crosslinkable polymer and a trifunctional radical polymerizable compound (AD-705, LG Chem), 0.08 parts by weight of a curing agent (T-39M, Soken), 0.74 parts by weight of an initiator (AD-PI2, LG Chem), 0.05 parts by weight of a silane coupling agent (AD-M812, LG Chem), 0.28 parts by weight of an antistatic agent (HQ115, 3M), and 4 parts by weight of beads (Tospearl 145, Momentive) were added to a reaction vessel, and then 20 parts by weight of a solvent (Ethyl acetate) was added relative to 100 parts by weight of the crosslinkable polymer (AD-705) to prepare an adhesive composition. The crosslinkable polymer is a polymer of 99 parts by weight of BA (butyl acrylate) and 1 part by weight of 4-HBA (4-hydroxybutyl acrylate). The trifunctional radical polymerizable compound is a trifunctional acrylate. The beads contain a silicone resin and are spherical particles with an average particle size (D50) of about 4.5 μm. The refractive index of the crosslinkable polymer is 1.47, and the refractive index of the beads is 1.42, measured using an Abbe refractometer at a temperature of 25° C. and a light source with a wavelength of 350 nm to 1450 nm.

[0072] The adhesive composition was mixed in a mixer (Stirrer) for 50 minutes, then coated on a first release film (MRP38, Mitsubishi Plastics) with a thickness of 38 μm so that the thickness after drying would be about 22 μm, and dried at a temperature of 80° C. for 3 minutes to form a scattering adhesive. A second release film (MRP, Mitsubishi Plastics) with a thickness of 38 μm and a different peel strength from the first release film was laminated on the scattering adhesive formed on the first release film. After lamination, light (about 150 mJ / 250 mW) was irradiated from a mercury high pressure lamp (light amount 80 W) for about 15 seconds to produce an adhesive film.

[0073] A first protective film (TAC film) having a thickness of 65 μm was laminated on one side of a polarizer (a PVA-based stretched film dyed with iodine) having a thickness of 25 μm, and a second protective film (TAC film) having a thickness of 45 μm was laminated on the other side of the polarizer. A low-reflection layer having an average reflectance of about 2% for wavelengths of 380 nm to 780 nm was formed on one side of the first protective film for surface treatment. A quarter-wave plate (liquid crystal layer) was formed on one side of the second protective film. After removing the second release film from the prepared adhesive film, a polarizing plate was prepared by laminating the scattering adhesive so that it was attached to the quarter-wave plate.

[0074] Example 2 A polarizing plate was manufactured in the same manner as in Example 1, except that the content of the beads was changed to 3 parts by weight.

[0075] Example 3 A polarizing plate was manufactured in the same manner as in Example 1, except that the content of the beads was changed to 4.5 parts by weight.

[0076] Example 4 A mixture of a crosslinkable polymer and a trifunctional radical polymerizable compound (AD-705, LG Chem) of 100 parts by weight, a curing agent (T-39M, Soken) of 0.26 parts by weight, an initiator (AD-PI2, LG Chem) of 1.76 parts by weight, a silane coupling agent (AD-M812, LG Chem) of 0.05 parts by weight, an antistatic agent (HQ115, 3M) of 1.10 parts by weight, and beads (TSR 9000, Momentive) of 3.35 parts by weight were put into a reaction vessel, and then a solvent (Ethyl acetate) was added to prepare a pressure-sensitive adhesive composition. The crosslinkable polymer is a polymer of 99 parts by weight of BA (butyl acrylate) and 1 part by weight of 4-HBA (4-hydroxybutyl acrylate). The trifunctional radical polymerizable compound is a trifunctional acrylate. The beads contain a silicone resin and are spherical particles with an average particle size (D50) of about 2.2 μm to 2.5 μm. The refractive index of the crosslinkable polymer is 1.47 and that of the beads is 1.42, measured using an Abbe refractometer at a temperature of 25° C. and a light source having a wavelength of 350 nm to 1450 nm.

[0077] The adhesive composition was mixed in a mixer (Stirrer) for 50 minutes, then coated on a first release film (MRP38, Mitsubishi Plastics) with a thickness of 38 μm so that the thickness after drying was about 22 μm, and dried at a temperature of 80° C. for 3 minutes to form a scattering adhesive layer. A second release film (MRP38, Mitsubishi Plastics) with a thickness of 38 μm and a different peeling force from the first release film was laminated on the scattering adhesive layer formed on the first release film. After lamination, light (about 150 mJ / 250 mW) was irradiated from a mercury high pressure lamp (light amount 80 W) for about 15 seconds to produce an adhesive film.

[0078] A first protective film (TAC film) having a thickness of 65 μm was laminated on one side of a polarizer (a PVA-based stretched film dyed with iodine) having a thickness of 25 μm, and a second protective film (TAC film) having a thickness of 45 μm was laminated on the other side of the polarizer. A low-reflection layer having an average reflectance of about 2% for wavelengths of 380 nm to 780 nm was formed on one side of the first protective film for surface treatment. A ¼ wavelength plate (liquid crystal layer) was formed on one side of the second protective film. After removing the second release film from the prepared adhesive film, a scattering adhesive layer was laminated so as to be attached to the ¼ wavelength plate to prepare a polarizing plate.

[0079] Example 5 A polarizing plate was manufactured in the same manner as in Example 4, except that the content of beads was changed to 6 parts by weight per 100 parts by weight of the mixture of crosslinkable polymer and trifunctional radical polymerizable compound (AD-705, LG Chem).

[0080] Example 6 A polarizing plate was manufactured in the same manner as in Example 4, except that the beads were changed to spherical particles (Tospearl 145, Momentive) having an average particle size (D50) of about 4.5 μm, and the content of the beads was changed to 4.50 parts by weight per 100 parts by weight of the mixture of a crosslinkable polymer and a trifunctional radical polymerizable compound (AD-705, LG Chem).

[0081] Example 7 A polarizing plate was manufactured in the same manner as in Example 4, except that the beads were changed to spherical particles (Tospearl 145, Momentive) having an average particle size (D50) of about 4.5 μm, and the content of the beads was changed to 6 parts by weight per 100 parts by weight of a mixture of a crosslinkable polymer and a trifunctional radical polymerizable compound (AD-705, LG Chem).

[0082] Example 8 A polarizing plate was manufactured in the same manner as in Example 4, except that the content of beads was changed to 3 parts by weight per 100 parts by weight of the mixture of crosslinkable polymer and trifunctional radical polymerizable compound (AD-705, LG Chem).

[0083] Comparative Example 1 100 parts by weight of acrylic polymer (LC-6BB, Soken), 0.01 parts by weight of hardener (T-743L, Soken), 0.45 parts by weight of hardener (T-706BB, Soken), 0.02 parts by weight of silane coupling agent (T-789J, Soken), 0.29 parts by weight of antistatic agent (FC4400, 3M) and 4 parts by weight of beads (Tospearl 145, Momentive) were added to a reaction vessel, and then 20 parts by weight of solvent (Ethyl acetate) was added relative to 100 parts by weight of acrylic polymer (LC-6BB) to prepare an adhesive composition. The acrylic polymer is a polymer of 94 parts by weight of BA (butyl acrylate) and 4 parts by weight of AA (acrylic acid). The beads contain silicone resin and are spherical particles with an average particle size (D50) of about 4.5 μm. The refractive index of the acrylic polymer is 1.46, and the refractive index of the beads is 1.42. The refractive index is measured using an Abbe refractometer at a temperature of 25° C. and a light source having a wavelength of 350 nm to 1450 nm.

[0084] The adhesive composition was mixed in a mixer (Stirrer) for 50 minutes, then coated onto a first release film (MRP38, Mitsubishi Plastics) with a thickness of 38 μm so that the thickness after drying would be about 22 μm, and dried at a temperature of 80° C. for 3 minutes to form a scattering adhesive. A second release film (MRP, Mitsubishi Plastics) with a thickness of 38 μm and a different peel strength from the first release film was laminated onto the scattering adhesive formed on the first release film.

[0085] A first protective film (TAC film) having a thickness of 65 μm was laminated on one side of a polarizer (a PVA-based stretched film dyed with iodine) having a thickness of 25 μm, and a second protective film (TAC film) having a thickness of 45 μm was laminated on the other side of the polarizer. A low-reflection layer having an average reflectance of about 2% for wavelengths of 380 nm to 780 nm was formed on one side of the first protective film for surface treatment. A quarter-wave plate (liquid crystal layer) was formed on one side of the second protective film. After removing the second release film from the manufactured adhesive film, the adhesive was laminated so as to be attached to the quarter-wave plate to manufacture a polarizing plate.

[0086] Comparative Example 2 A polarizing plate was manufactured in the same manner as in Example 1, except that the beads were not added.

[0087] Comparative Example 3 A polarizing plate was prepared in the same manner as in Example 4, except that the beads were not added.

[0088] Comparative Example 4 A polarizing plate was manufactured in the same manner as in Example 4, except that the beads were changed to spherical particles (Tospearl 145, Momentive) with an average particle size (D50) of about 4.5 μm and a refractive index of 1.42, and the content of the beads was changed to 0.60 parts by weight per 100 parts by weight of a mixture of a crosslinkable polymer and a trifunctional radical polymerizable compound (AD-705, LG Chem). The beads (Tospearl 145, Momentive) contain a silicone resin and have a refractive index of 1.42.

[0089] Comparative Example 5 A polarizing plate was manufactured in the same manner as in Example 4, except that the content of beads was changed to 0.5 parts by weight per 100 parts by weight of the mixture of crosslinkable polymer and trifunctional radical polymerizable compound (AD-705, LG Chem).

[0090] The storage modulus and haze were measured for Examples 1 to 8 and Comparative Examples 1 to 5, and the results are shown in Table 1.

[0091] Measurement example 1. Haze measurement The polarizing plate was cut into a size of 5 cm x 5 cm to prepare a sample, and the haze was measured at 25° C. using a haze meter (HM-150, Murakami color research laboratory). The haze was measured for light with wavelengths of 380 nm to 780 nm.

[0092] Measurement example 2. Storage modulus measurement The scattering adhesive layer was folded and laminated into 16 layers to prepare a sample with a size of 15cm x 20cm (horizontal x vertical). The storage modulus was measured at a temperature of 25°C and a strain of 50% using an ARES-G2 (TA Instruments) device, and the value at a frequency of 1rad / sec was extracted.

[0093] [Table 1]

[0094] For Examples 1 to 8 and Comparative Examples 1 to 5, the glass creep distance, the presence or absence of unevenness, the heat resistance reliability, and the moist heat resistance reliability were evaluated, and the results are shown in Tables 2 and 3. Measurement Example 3: Glass Creep Distance Measurement The polarizing plate was cut to a size of 10mm x 100mm. After peeling off the first release film from the polarizing plate, the adhesive layer of the polarizing plate was attached to a central area of ​​a glass plate (soda lime glass) with dimensions of 30mm x 40mm x 0.8mm so that the adhesive layer of the polarizing plate was in contact with the glass plate to prepare a test piece. The test piece was degassed for 15 minutes at 50°C and 5 atm, and the pushed distance was measured. Specifically, the test piece was loaded into a Texture analyzer (Stable micro system, XT plus) to fix the polarizing plate part and the glass plate part. The polarizing plate was pulled in one direction for 1000 seconds with a force of 800gf, and the distance (unit: μm) that the polarizing plate was pushed from the glass substrate was measured. Generally, saturation (the pressed distance does not increase any more and becomes uniform) occurs within 1000 seconds, and in this experiment, the pressed distance at the final 1000 seconds was measured and listed in Table 2 below. The lower the glass pressed distance, the higher the hardness of the sample.

[0095] Evaluation example 1. Presence or absence of unevenness The polarizing plate was cut to A4 size, the first release film was removed from the polarizing plate, and the polarizing plate was attached to an OLED panel (Micro lens array OLED, LGD). The OLED panel was operated, and the occurrence of unevenness was visually observed.

[0096] Evaluation example 2. Heat resistance reliability and moisture and heat resistance reliability evaluation (A) The polarizing plate was cut to a size of 160mm x 90mm, attached to an A4 size glass plate (soda lime glass), and degassed to prepare a sample. The sample was placed in a chamber that maintained the conditions of heat resistance reliability (temperature 80°C) and humidity and heat resistance reliability (temperature 60°C, relative humidity 90%) and was maintained for 500 hours. The sample was observed for the presence or absence of bubbles, and the reliability was evaluated according to the following criteria.

[0097] ◎: No bubbles ○: Less than 5 bubbles △: 5 or more bubbles ×: Polarizing plate floating occurs

[0098] [Table 2]

[0099] Evaluation example 3. Heat resistance reliability and moisture and heat resistance reliability evaluation (B) The heat resistance change rate (ΔHa) of the following formula 1 and the humidity and heat resistance change rate (ΔHb) of the following formula 2 were measured, and the results are shown in Table 3 below. Specifically, the polarizing plate was cut to a size of 47 mm x 47 mm, and then attached to a glass plate (soda lime glass) with a size of 50 mm x 50 mm x 0.8 mm and degassed to prepare a sample. The sample was placed in a chamber maintained under the conditions of heat resistance reliability (temperature 80° C.) and humidity and heat resistance reliability (temperature 60° C., relative humidity 90%), and then maintained for 500 hours. The haze measured at 25° C. before being placed in the chamber is H1 of the following formula 1 and H3 of the following formula 2, the haze measured after maintaining the chamber under the heat resistance reliability condition (temperature 80° C.) for 500 hours is H2 of the following formula 1, and the haze measured after maintaining the chamber under the humidity and heat resistance reliability condition (temperature 60° C., relative humidity 90%) for 500 hours is H4 of the following formula 2.

[0100] [Formula 1] △Ha=(H1-H2) / H1×100% [Formula 2] △Hb=(H3-H4) / H3×100%

[0101] [Table 3]

[0102] For Examples 4 to 8 and Comparative Examples 3 to 5, the sparkling phenomenon and camera recognition evaluation were performed and the results are shown in Table 4.

[0103] Evaluation example 4. Sparkling phenomenon evaluation The polarizing plate was cut into A4 size, the first release film was removed from the polarizing plate, and the plate was attached to a green-based monitor, and then the plate was visually observed in a dark room at room temperature to see if there was any sparkling. The degree of sparkling was evaluated as follows:

[0104] Lv0: No sparkling phenomenon Lv1: Sparkling phenomenon weak Lv2: Sparkling Phenomenon Weak Lv3: Sparkling phenomenon Lv4: Sparkling Phenomenon Medium Strong Lv5: Sparkling Phenomenon Strong

[0105] Evaluation example 5. Camera recognition evaluation After cutting the polarizing plate to A4 size, a random red line was drawn on the release film surface with the polarizing plate, and the distribution of beads around the line was observed using an optical microscope (x50 magnification). If the distribution of beads is high, the camera may recognize the beads during the attachment process and misread the reference line, resulting in an attachment error.

[0106] [Table 4] [Explanation of symbols]

[0107] 100: Scattering adhesive layer 200: Retardation layer 300: Polarizer protection film 400: Polarizer 500: Polarizer protection film 600: Surface treatment layer 700: Hard layer

Claims

1. A polarizing plate comprising a polarizer and a scattering adhesive layer present on one surface of the polarizer, The scattering adhesive layer has a storage modulus of 120,000 Pa or more at a temperature of 25° C. and a frequency of 1 rad / sec; The polarizing plate has a haze of 12% or more.

2. The polarizing plate of claim 1 , wherein the scattering adhesive layer comprises an adhesive resin and beads.

3. The scattering adhesive layer contains an adhesive resin, The polarizing plate according to claim 2 , wherein the adhesive resin has an IPN crosslinked structure.

4. The polarizing plate according to claim 3 , wherein the IPN crosslinked structure includes a first crosslinked structure formed by a crosslinking reaction between a crosslinkable polymer and a multifunctional crosslinking agent, and a second crosslinked structure formed by a polymerization reaction of a radical polymerizable compound.

5. 5. The polarizing plate according to claim 4, wherein the difference (A-B) between the refractive index (A) of the crosslinkable polymer and the refractive index (B) of the beads is within the range of 0.05 to 0.

1.

6. The polarizer of claim 2 , wherein the beads comprise a silicone resin.

7. 3. The polarizing plate according to claim 2, wherein the beads are contained in an amount ranging from 2 parts by weight to 10 parts by weight based on 100 parts by weight of the adhesive resin.

8. 2. The polarizing plate according to claim 1, wherein the thickness of the scattering adhesive layer is in the range of 15 μm to 25 μm.

9. 2. The polarizing plate according to claim 1, wherein the scattering adhesive layer has a glass pressing distance measured at 800 gf for 1000 seconds within a range of 150 to 210 μm.

10. The polarizing plate has a haze change rate ΔHa after heat resistance represented by the following formula 1 and a haze change rate ΔHb after wet heat resistance represented by the following formula 2 of 2% or less, [Formula 1] △Ha=(H 1 -H 2 ) / H 1 ×100% [Formula 2] △Hb=(H 3 -H 4 ) / H 3 ×100% In Formula 1, H 1 is the haze of the polarizing plate at a temperature of 25° C., and H 2 is the haze of the polarizing plate after storage for 500 hours at a temperature of 80° C., In Formula 2, H 3 is the haze of the polarizing plate at a temperature of 25° C., and H 4 is the haze of the polarizing plate after storage for 500 hours at a temperature of 60° C. and a relative humidity of 90%.

11. 10. The polarizing plate of claim 1, further comprising a polarizer protective film present on one or both sides of the polarizer.

12. The polarizing plate according to claim 1 , further comprising a retardation layer between the polarizer and the scattering adhesive layer.

13. An OLED display device comprising an OLED display panel and the polarizer of claim 1 disposed on one side of the OLED display panel.

14. 14. The OLED display device of claim 13, wherein the polarizer is disposed on the light-exiting side of the OLED display panel.

Citation Information

Patent Citations

  • Adhesive sheet and optical laminate

    JP2020002239A

  • Composite polarizing plate, laminated optical member, and image display device using them

    WO2009025360A1

  • Adhesive composition, adhesive agent, and adhesive sheet

    WO2015145633A1

  • Polarizer for oeld having improved brightness

    KR1020090122138A