Aqueous negative electrode slurry composition for lithium ion storage devices
The negative electrode aqueous slurry composition with a binder and dispersant containing nitrogen-containing heterocycles and alkyl esters of (meth)acrylic acid addresses the challenge of uniform dispersion, improving the performance of negative electrodes for faster charging and discharging in batteries.
Patent Information
- Application Number
- JP2024520872
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-06
- Filing Date
- 2022-08-05
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing negative electrode slurry compositions for batteries face challenges in achieving uniform dispersion of conductive additives, which is crucial for fast charging and discharging applications, and current methods are expensive and inefficient.
A negative electrode aqueous slurry composition comprising a binder, a dispersant, and a specific combination of monomers including nitrogen-containing heterocycles and alkyl esters of (meth)acrylic acid, which enhances the uniform dispersion of conductive additives, improving the electrical contact and performance of the negative electrode.
The proposed composition achieves improved uniform dispersion of conductive additives, enabling faster charging and discharging capabilities while maintaining physical and electrical contact, thus enhancing the performance of negative electrodes in batteries.
Smart Images

Figure 2024537172000001_ABST
Abstract
Description
[Technical field]
[0001] Government Assistance Notification This invention was made with Government support under Government Contract No. 201950-140969 awarded by the Department of Defense. The Government has certain rights in this invention.
[0002] The present disclosure relates to slurry compositions that can be used in the manufacture of negative electrodes for use in electrical storage devices such as batteries. [Background technology]
[0003] The electronics industry is trending towards producing smaller devices powered by smaller and lighter batteries. As battery use moves further towards high-rate (discharge) charging applications, battery electrode coatings will need to withstand more severe operating conditions. Anodes typically use carbonaceous materials as anode active materials, optionally including conductive additives (which can also be carbonaceous); however, these materials can be difficult to disperse uniformly in aqueous electrode slurries, and current methods to improve dispersion are expensive and are typically added at higher levels to facilitate rapid (discharge) charging applications. If the conductive additives are well dispersed throughout the electrode coating while maintaining physical / electrical contact, high-rate charging and / or discharging applications can be realized. As a result, improved aqueous anode slurry compositions are desired. [Brief description of the drawings]
[0004] [Figure 1] 1 is a series of black and white photographs of coatings of carbon dispersions applied via the drawdown method onto substrates, illustrating the quality of the applied coatings.
[0005] [Diagram 2] 1 is a black and white TEM image of a carbon-containing film.
[0006] [Diagram 3] 1 is a graph showing cell data as a function of time. Summary of the Invention
[0007] The present disclosure provides a negative electrode aqueous slurry composition comprising: a binder; a dispersant, the dispersant comprising a copolymer including (a) a constituent unit including a residue of a monomer including a nitrogen-containing heterocycle, and (b) a constituent unit including a residue of an alkyl ester of (meth)acrylic acid and / or a residue of an alpha, beta-ethylenically unsaturated carboxylic acid functional monomer, the dispersant comprising 1 wt % to 50 wt % of the constituent unit including a residue of a monomer including a nitrogen-containing heterocycle, the weight % being based on the total weight of the dispersant; a negative electrode active material; and an aqueous medium.
[0008] The present disclosure also provides a negative electrode aqueous slurry composition including a binder, a poly(2-alkyl or aryl oxazoline) polymer, a negative electrode active material, and an aqueous medium.
[0009] The present disclosure further provides an anode comprising: (a) a current collector; and (b) a film formed on the current collector, the film comprising a binder; and optionally a dispersant, the dispersant comprising a copolymer comprising (a) a constituent unit comprising a residue of a monomer comprising a nitrogen-containing heterocycle, and (b) a constituent unit comprising a residue of an alkyl ester of (meth)acrylic acid and / or a residue of an acid-functional ethylenically unsaturated monomer, the dispersant comprising 1 wt % to 50 wt % of the constituent unit comprising the residue of a monomer comprising a nitrogen-containing heterocycle, the weight % being based on the total weight of the dispersant; and optionally a poly(2-alkyl or aryl oxazoline) polymer, where at least one of the dispersant and the poly(2-alkyl or aryl oxazoline) polymer is present; and an anode active material.
[0010] The present disclosure further provides an anode comprising: (a) a current collector; and (b) a film formed on the current collector, the film comprising a binder; an anode active material; and at least one of: a dispersant, the dispersant comprising a copolymer comprising (a) a constituent unit comprising a residue of a monomer comprising a nitrogen-containing heterocycle, and (b) a constituent unit comprising a residue of an alkyl ester of (meth)acrylic acid and / or a residue of an acid-functional ethylenically unsaturated monomer, the dispersant comprising 1 wt % to 50 wt % of the constituent unit comprising a residue of a monomer comprising a nitrogen-containing heterocycle, the weight % being based on the total weight of the dispersant; or a poly(2-alkyl or aryl oxazoline) polymer.
[0011] The present disclosure also provides an electricity storage device comprising: (a) a negative electrode of the present disclosure; (b) a positive electrode; and (c) an electrolyte.
[0012] The present disclosure further provides a negative electrode aqueous slurry composition comprising a negative electrode active material, a binder comprising cellulose or a cellulose derivative and a styrene-butadiene copolymer, a melamine crosslinker, and an aqueous medium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present disclosure provides a negative electrode aqueous slurry composition comprising: a binder; a dispersant, the dispersant comprising a copolymer including (a) a constituent unit including a residue of a monomer including a nitrogen-containing heterocycle, and (b) a constituent unit including a residue of an alkyl ester of (meth)acrylic acid and / or a residue of an acid-functional ethylenically unsaturated monomer, the dispersant containing 1 wt % to 50 wt % of the constituent unit including the residue of a monomer including a nitrogen-containing heterocycle, the weight % being based on the total weight of the dispersant; a negative electrode active material; and an aqueous medium.
[0014] The binder can include any suitable binder resin for the negative electrode aqueous slurry composition.For example, the binder can be fluoropolymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, and vinylidene fluoride-chlorotrifluoroethylene copolymer; polyolefin resins such as ethylene-propylene-diene ternary copolymer, polyethylene, polypropylene, ethylene-vinyl acetate copolymer, and ethylene-ethyl acrylate copolymer; polystyrene resins such as polystyrene, acrylonitrile styrene copolymer, acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-styrene copolymer, and styrene-butadiethylene rubber; polycarbonate resin, vinyl chloride resin, polyamide resin, polyimide Resins, (meth)acrylic acid resins such as polyacrylic acid, ammonium polyacrylate, sodium polyacrylate, and polymethyl methacrylate, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polylactic acid, poly-3-hydroxybutyric acid, polycaprolactone, polybutylene succinate, and polyethylene succinate / adipate; polyphenylene ether resins, modified polyphenylene ether resins, polyacetal resins, polysulfone resins, polyphenylene sulfide resins, polyvinyl alcohol resins; chitin, chitosan, and lignin; epoxy resins, urethane acrylates, phenolic acid resins, melamine resins, urea resins, and alkyd resins, and any combination thereof.
[0015] As mentioned above, the binder may optionally include a styrene butadiene copolymer. As used herein, the term "styrene butadiene copolymer" refers to a copolymer that includes styrene (or a derivative thereof) and butadiene.
[0016] The styrene butadiene copolymer may be present in the binder in an amount of at least at least 20% by weight, such as at least 30% by weight, such as at least 40% by weight, such as at least 45% by weight, such as at least 50% by weight, such as at least 65% by weight, such as at least 80% by weight, such as at least 90% by weight, such as at least 95% by weight, based on the total weight of the binder solids. The styrene butadiene copolymer may be present in the binder in an amount of 99.9% by weight, such as 95% by weight or less, such as 85% by weight or less, such as 75% by weight or less, such as 65% by weight or less, such as 55% by weight or less, such as 50% by weight or less, such as 45% by weight or less, based on the total weight of the binder solids. Styrene butadiene copolymers may be present in an amount of from 20% to 95% by weight, such as from 20% to 85% by weight, such as from 20% to 75% by weight, such as from 20% to 65% by weight, such as from 20% to 55% by weight, such as from 20% to 50% by weight, such as from 20% to 45% by weight, such as from 30% to 99.9% by weight, such as from 30% to 95% by weight, such as from 30% to 85% by weight, such as from 30% to 75% by weight, such as from 30% to 65% by weight, such as from 30% to 55% by weight, such as from 30% to 50% by weight, such as from 30% to 45% by weight, such as from 40% to 99.9% by weight, such as from 40% to 95% by weight, such as from 40% to 85% by weight, such as from 40% to 75% by weight, such as from 40% to 6 ... It may be present in the binder in an amount of 20% to 99.9% by weight, such as 5% by weight, such as 40% to 55% by weight, such as 40% to 50% by weight, such as 40% to 45% by weight, such as 50% to 99.9% by weight, such as 50% to 95% by weight, such as 50% to 85% by weight, such as 50% to 75% by weight, such as 50% to 65% by weight, such as 50% to 55% by weight, such as 65% to 99.9% by weight, such as 65% to 95% by weight, such as 65% to 85% by weight, such as 65% to 75% by weight, such as 80% to 99.9% by weight, such as 80% to 95% by weight, such as 80% to 85% by weight, such as 90% to 99.9% by weight, such as 90% to 95% by weight, such as 95% to 99.9% by weight.
[0017] The styrene butadiene copolymer may be present in the slurry composition in an amount of at least 0.1 wt%, such as at least 0.5 wt%, such as at least 1 wt%, such as at least 2 wt%, at least 3 wt%, at least 4 wt%, based on the total solids weight of the slurry composition. The styrene butadiene copolymer may be present in an amount of 10 wt% or less, such as 8 wt% or less, such as 5 wt% or less, such as 4 wt% or less, such as 3 wt% or less, such as 2 wt% or less, such as 1 wt% or less, based on the total solids weight of the slurry composition. The styrene butadiene copolymer may be present in an amount, based on the total solids weight of the slurry composition, such as 0.1 wt% to 8% wt%, such as 0.1 wt% to 5% wt%, such as 0.1 wt% to 4% wt%, such as 0.1 wt% to 3% wt%, such as 0.1 wt% to 2% wt%, such as 0.1 wt% to 1% wt%, such as 0.5 wt% to 10% wt%, such as 0.5 wt% to 8% wt%, such as 0.5 wt% to 5% wt%, such as 0.5 wt% to 4% wt%, such as 0.5 wt% to 3% wt%, such as 0.5 wt% to 2% wt%, such as 0.5 wt% to 1% wt%, It may be present in an amount of 0.1% to 10% by weight, such as 1% to 10% by weight, such as 1% to 8% by weight, such as 1% to 5% by weight, such as 1% to 4% by weight, such as 1% to 3% by weight, such as 1% to 2% by weight, such as 2% to 10% by weight, such as 2% to 8% by weight, such as 2% to 5% by weight, such as 2% to 4% by weight, such as 2% to 3% by weight, such as 3% to 10% by weight, such as 3% to 8% by weight, such as 3% to 5% by weight, such as 3% to 4% by weight, such as 4% to 5% by weight.
[0018] The styrene butadiene copolymer may be present in the slurry composition in an amount of at least 0.05 wt%, such as at least 0.25 wt%, such as at least 0.5 wt%, such as at least 1 wt%, such as at least 1.5 wt%, such as at least 2 wt%, based on the total weight of the slurry composition. The styrene butadiene copolymer may be present in an amount of 4 wt% or less, such as 3.5 wt% or less, such as 3 wt% or less, such as 2.5 wt% or less, such as 2 wt% or less, such as 1.5 wt% or less, such as 1 wt% or less, such as 0.5 wt% or less, based on the total weight of the slurry composition. The styrene butadiene copolymer may be present in an amount of from 0.05 wt% to 3.5 wt%, such as from 0.05 wt% to 3 wt%, such as from 0.05 wt% to 2.5 wt%, such as from 0.05 wt% to 2 wt%, such as from 0.05 wt% to 1.5 wt%, such as from 0.05 wt% to 1 wt%, such as from 0.05 wt% to 0.5 wt%, such as from 0.25 wt% to 4 wt%, such as from 0.25 wt% to 3.5 wt%, such as from 0.25 wt% to 3 wt%, such as from 0.25 wt% to 2.5 wt%, such as from 0.25 wt% to 2 wt%, such as from 0.25 wt% to 1.5 wt%, such as from 0.25 wt% to 1 wt%, such as from 0.25 wt% to 0.5 wt%, such as from 0.5 wt% to 4 wt%, such as from 0.5 wt% to 3.5 wt%, based on the total weight of the slurry composition. It may be present in an amount of 0.05% to 4% by weight, such as 0.5% to 3% by weight, such as 0.5% to 2.5% by weight, such as 0.5% to 2% by weight, such as 0.5% to 1.5% by weight, such as 0.5% to 1% by weight, such as 1% to 4% by weight, such as 1% to 3.5% by weight, such as 1% to 3% by weight, such as 1% to 2.5% by weight, such as 1% to 2% by weight, such as 1% to 1.5% by weight, such as 1.5% to 4% by weight, such as 1.5% to 3.5% by weight, such as 1.5% to 3% by weight, such as 1.5% to 2.5% by weight, such as 1.5% to 2% by weight, 2% to 4% by weight, such as 2% to 3.5% by weight, such as 2% to 3% by weight, such as 2% to 2.5% by weight.
[0019] The slurry composition and the binder may further include a cellulose derivative, if desired. The cellulose derivative may be, for example, carboxymethylcellulose and its salts (CMC). CMC is a cellulose ether in which a portion of the hydroxyl groups on the anhydroglucose ring is replaced with carboxymethyl groups. The degree of carboxymethyl substitution may range from 0.4 to 3. CMC is a long-chain polymer, and its viscosity in an aqueous solution depends on its molecular weight, which may vary between 50,000 and 2,000,000 g / mol on a weight average basis. Carboxymethylcellulose may have a weight average molecular weight of at least 50,000 g / mol, such as at least 100,000 g / mol, or in some cases at least 200,000 g / mol, such as at least 250,000 g / mol. The carboxymethylcellulose may have a weight average molecular weight of 2,000,000 g / mol or less, such as 1,000,000 g / mol or less, such as 500,000 g / mol or less, such as 350,000 g / mol or less, such as 300,000 g / mol. The carboxymethylcellulose may have a weight average molecular weight of 50,000 to 1,000,000 g / mol, such as 50,000 to 500,000 g / mol, such as 50,000 to 350,000 g / mol, such as 50,000 to 300,000 g / mol, such as 100,000 to 2,000,000 g / mol, such as 100,000 to 1,000,000 g / mol, such as 100,000 to 500,000 g / mol, such as 100,000 to 350, The CMC degree of substitution (DS) may be at least 0.4, such as at least 0.5, such as at least 0.6, such as at least 0.7, such as at least 0.8, such as at least 0.9, such as at least 1, such as at least 1.1, such as at least 1.2.The degree of CMC substitution (DS) may be 3 or less, such as 2 or less, such as 1.4 or less, such as 1.2 or less, such as 1 or less, such as 0.8 or less, such as 0.7 or less. The degree of CMC substitution (DS) may be 0.4-2, such as 0.4-1.4, such as 0.4-1.2, such as 0.4-1, such as 0.4-0.8, such as 0.4-0.7, such as 0.5-3, such as 0.5-2, such as 0.5-1.4, such as 0.5-1.2, such as 0.5-1, such as 0.5-0.8, such as 0.5-0.7, such as 0.6-3, such as 0.6-2, such as 0.6-1.4, such as 0.6-1.2, such as 0.6-1, such as 0.6-0.8, such as 0.6-0.7, such as 0.7-3, such as 0.7-2, such as 0.7-1.4 It may be 0.4-3, such as 0.7-1.2, such as 0.7-1, such as 0.7-0.8, such as 0.8-3, such as 0.8-2, such as 0.8-1.4, such as 0.8-1.2, such as 0.8-1, such as 0.9-3, such as 0.9-2, such as 0.9-1.4, such as 0.9-1.2, such as 0.9-1, 1-3, such as 1-2, such as 1-1.4, such as 1-1.2, such as 1.1-3, such as 1.1-2, such as 1.1-1.4, such as 1.1-1.2, such as 1.2-3, such as 1.2-2, such as 1.2-1.4.
[0020] The cellulose derivative may be present in the binder in an amount of at least 20% by weight, such as at least 30% by weight, such as at least 40% by weight, such as at least 45% by weight, such as at least 50% by weight, such as at least 65% by weight, such as at least 80% by weight, such as at least 90% by weight, such as at least 95% by weight, based on the total weight of the binder solids. The cellulose derivative may be present in the binder in an amount of 99.9% by weight, such as 95% by weight or less, such as 85% by weight or less, such as 75% by weight or less, such as 65% by weight or less, such as 55% by weight or less, such as 50% by weight or less, such as 45% by weight or less, based on the total weight of the binder solids. The cellulose derivative may be present in an amount of from 20% by weight to 95% by weight, such as from 20% by weight to 85% by weight, such as from 20% by weight to 75% by weight, such as from 20% by weight to 65% by weight, such as from 20% by weight to 55% by weight, such as from 20% by weight to 50% by weight, such as from 20% by weight to 45% by weight, such as from 30% by weight to 99.9% by weight, such as from 30% by weight to 95% by weight, such as from 30% by weight to 85% by weight, such as from 30% by weight to 75% by weight, such as from 30% by weight to 65% by weight, such as from 30% by weight to 55% by weight, such as from 30% by weight to 50% by weight, such as from 30% by weight to 45% by weight, such as from 40% by weight to 99.9% by weight, such as from 40% by weight to 95% by weight, such as from 40% by weight to 85% by weight, such as from 40% by weight to 75% by weight, such as from 40% by weight to 65% by weight, based on the total weight of the binder solids. %, such as 40% to 55% by weight, such as 40% to 50% by weight, such as 40% to 45% by weight, such as 50% to 99.9% by weight, such as 50% to 95% by weight, such as 50% to 85% by weight, such as 50% to 75% by weight, such as 50% to 65% by weight, such as 50% to 55% by weight, such as 65% to 99.9% by weight, such as 65% to 95% by weight, such as 65% to 85% by weight, such as 65% to 75% by weight, such as 80% to 99.9% by weight, such as 80% to 95% by weight, such as 80% to 85% by weight, such as 90% to 99.9% by weight, such as 90% to 95% by weight, such as 95% to 99.9% by weight.
[0021] The cellulose derivative may be present in the slurry composition in an amount of at least 0.1 wt%, such as at least 0.5 wt%, such as at least 1 wt%, such as at least 2 wt%, at least 3 wt%, at least 4 wt%, based on the total solids weight of the slurry composition. The cellulose derivative may be present in an amount of 10 wt% or less, such as 8 wt% or less, such as 5 wt% or less, such as 4 wt% or less, such as 3 wt% or less, such as 2 wt% or less, such as 1 wt% or less, based on the total solids weight of the slurry composition. The cellulose derivative may be present in an amount of from 0.1% by weight to 8% by weight, such as from 0.1% by weight to 5% by weight, such as from 0.1% by weight to 4% by weight, such as from 0.1% by weight to 3% by weight, such as from 0.1% by weight to 2% by weight, such as from 0.1% by weight to 1% by weight, such as from 0.5% by weight to 10% by weight, such as from 0.5% by weight to 8% by weight, such as from 0.5% by weight to 5% by weight, such as from 0.5% by weight to 4% by weight, such as from 0.5% by weight to 3% by weight, such as from 0.5% by weight to 2% by weight, such as from 0.5% by weight to 1% by weight, based on the total solids weight of the slurry composition. It may be present in an amount of from 0.1% to 10% by weight, such as from 1% to 8% by weight, such as from 1% to 5% by weight, such as from 1% to 4% by weight, such as from 1% to 3% by weight, such as from 1% to 2% by weight, such as from 2% to 10% by weight, such as from 2% to 8% by weight, such as from 2% to 5% by weight, such as from 2% to 4% by weight, such as from 2% to 3% by weight, such as from 3% to 10% by weight, such as from 3% to 8% by weight, such as from 3% to 5% by weight, such as from 3% to 4% by weight, such as from 4% to 5% by weight.
[0022] The cellulose derivative may be present in the slurry composition in an amount of at least 0.05 wt%, such as at least 0.25 wt%, such as at least 0.5 wt%, such as at least 1 wt%, such as at least 1.5 wt%, such as at least 2 wt%, based on the total weight of the slurry composition. The cellulose derivative may be present in an amount of 4 wt% or less, such as 3.5 wt% or less, such as 3 wt% or less, such as 2.5 wt% or less, such as 2 wt% or less, such as 1.5 wt% or less, such as 1 wt% or less, such as 0.5 wt% or less, based on the total weight of the slurry composition. The cellulose derivative may be present in an amount of from 0.05 wt% to 3.5 wt%, such as from 0.05 wt% to 3 wt%, such as from 0.05 wt% to 2.5 wt%, such as from 0.05 wt% to 2 wt%, such as from 0.05 wt% to 1.5 wt%, such as from 0.05 wt% to 1 wt%, such as from 0.05 wt% to 0.5 wt%, such as from 0.25 wt% to 4 wt%, such as from 0.25 wt% to 3.5 wt%, such as from 0.25 wt% to 3 wt%, such as from 0.25 wt% to 2.5 wt%, such as from 0.25 wt% to 2 wt%, such as from 0.25 wt% to 1.5 wt%, such as from 0.25 wt% to 1 wt%, such as from 0.25 wt% to 0.5 wt%, such as from 0.5 wt% to 4 wt%, such as from 0.5 wt% to 3.5 wt%, based on the total weight of the slurry composition. It may be present in an amount of 0.05% to 4% by weight, such as 0.5% to 3% by weight, such as 0.5% to 2.5% by weight, such as 0.5% to 2% by weight, such as 0.5% to 1.5% by weight, such as 0.5% to 1% by weight, such as 1% to 4% by weight, such as 1% to 3.5% by weight, such as 1% to 3% by weight, such as 1% to 2.5% by weight, such as 1% to 2% by weight, such as 1% to 1.5% by weight, such as 1.5% to 4% by weight, such as 1.5% to 3.5% by weight, such as 1.5% to 3% by weight, such as 1.5% to 2.5% by weight, such as 1.5% to 2% by weight, 2% to 4% by weight, such as 2% to 3.5% by weight, such as 2% to 3% by weight, such as 2% to 2.5%.
[0023] According to the present disclosure, the slurry composition further comprises a dispersant, the dispersant comprising a copolymer comprising (a) a constituent unit comprising a residue of a monomer comprising a nitrogen-containing heterocycle and (b) a constituent unit comprising a residue of an alkyl ester of (meth)acrylic acid and / or a residue of an acid-functional ethylenically unsaturated monomer, the dispersant comprising 1 wt% to 50 wt% of the constituent unit comprising a residue of a monomer comprising a nitrogen-containing heterocycle, the wt% being based on the total weight of the dispersant.
[0024] The dispersant copolymer comprises at least 1 wt.%, such as at least 3 wt.%, such as at least 5 wt.%, such as at least 7 wt.%, such as at least 9 wt.%, such as at least 12 wt.%, such as at least 15 wt.%, of units comprising residues of monomers comprising nitrogen-containing heterocycles, based on the total weight of the dispersant. Non-limiting examples of ethylenically unsaturated monomers comprising nitrogen-containing heterocycles include N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylimidazole, vinylmethyloxazolidinone, among others. The dispersant copolymer comprises 50 wt.% or less, such as 30 wt.% or less, such as 20 wt.% or less, such as 15 wt.% or less, such as 12 wt.% or less, such as 10 wt.% or less, such as 7 wt.% or less, such as 5 wt.%, of units comprising residues of monomers comprising nitrogen-containing heterocycles, based on the total weight of the dispersant. The dispersant copolymer may comprise a constitutional unit comprising a residue of a monomer comprising a nitrogen-containing heterocycle, based on the total weight of the dispersant, such as from 1 wt% to 30 wt%, such as from 1 wt% to 20 wt%, such as from 1 wt% to 15 wt%, such as from 1 wt% to 12 wt%, such as from 1 wt% to 10 wt%, such as from 1 wt% to 7 wt%, such as from 1 wt% to 5 wt%, such as from 3 wt% to 50 wt%, such as from 3 wt% to 30 wt%, such as from 3 wt% to 20 wt%, such as from 3 wt% to 15 wt%, such as from 3 wt% to 12 wt%, such as from 3 wt% to 10 wt%, such as from 3 wt% to 7 wt%, such as from 3 wt% to 5 wt%, such as from 5 wt% to 50 wt%, such as from 5 wt% to 30 wt%, such as from 5 wt% to 20 wt%, such as from 5 wt% to 15 wt%, such as from 5 wt% to 12 ... Including 1% to 50% by weight, such as 5% to 10% by weight, such as 5% to 7% by weight, such as 7% to 50% by weight, such as 7% to 30% by weight, such as 7% to 20% by weight, such as 7% to 15% by weight, such as 7% to 12% by weight, such as 7% to 10% by weight, such as 9% to 50% by weight, such as 9% to 30% by weight, such as 9% to 20% by weight, such as 9% to 15% by weight, such as 9% to 12% by weight, such as 9% to 10% by weight, such as 12% to 50% by weight, such as 12% to 30% by weight, such as 12% to 20% by weight, such as 12% to 15% by weight, such as 15% to 50% by weight, such as 15% to 30% by weight, such as 15% to 20% by weight.The dispersant copolymer may comprise from 1 wt% to 30 wt%, such as from 1 wt% to 20 wt%, such as from 1 wt% to 15 wt%, such as from 1 wt% to 12 wt%, such as from 1 wt% to 10 wt%, such as from 1 wt% to 7 wt%, such as from 1 wt% to 5 wt%, such as from 3 wt% to 50 wt%, such as from 3 wt% to 30 wt%, such as from 3 wt% to 20 wt%, such as from 3 wt% to 15 wt%, such as from 3 wt% to 12 wt%, such as from 3 wt% to 10 wt%, such as from 3 wt% to 7 wt%, such as from 3 wt% to 5 wt%, such as from 5 wt% to 50 wt%, such as from 5 wt% to 30 wt%, such as from 5 wt% to 20 wt%, such as from 5 wt% to 15 wt%, such as from 5 wt% to 12 wt%, such as from 5 wt% to 5 wt%, based on the total weight of polymerizable monomers used in the reaction mixture. % to 10 wt%, such as 5 wt% to 7 wt%, such as 7 wt% to 50 wt%, such as 7 wt% to 30 wt%, such as 7 wt% to 20 wt%, such as 7 wt% to 15 wt%, such as 7 wt% to 12 wt%, such as 7 wt% to 10 wt%, such as 9 wt% to 50 wt%, such as 9 wt% to 30 wt%, such as 9 wt% to 20 wt%, such as 9 wt% to 15 wt%, such as 9 wt% to 12 wt%, such as 9 wt% to 10 wt%, such as 12 wt% to 50 wt%, such as 12 wt% to 30 wt%, such as 12 wt% to 20 wt%, such as 12 wt% to 15 wt%, such as 15 wt% to 50 wt%, such as 15 wt% to 30 wt%, such as 15 wt% to 20 wt%, such as
[0025] The dispersant copolymer further comprises constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of alpha, beta-ethylenically unsaturated carboxylic acid functional monomers. The constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of alpha, beta-ethylenically unsaturated carboxylic acid functional monomers may comprise at least at least 1% by weight, such as at least 15% by weight, such as at least 30% by weight, such as at least 35% by weight, such as at least 40% by weight, such as at least 45% by weight, such as at least 50% by weight, such as at least 55% by weight, such as at least 60% by weight, such as at least 70% by weight, such as at least 75% by weight, such as at least 80% by weight, based on the total weight of the dispersant copolymer. Constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of alpha, beta-ethylenically unsaturated carboxylic acid functional monomers may constitute 99% or less by weight, such as 90% or less, such as 85% or less, such as 80% or less, such as 75% or less, such as 70% or less, such as 65% or less, such as 60% or less, such as 50% or less, based on the total weight of the dispersant copolymer. The building blocks comprising residues of alkyl esters of (meth)acrylic acid and / or residues of alpha, beta-ethylenically unsaturated carboxylic acid functional monomers may comprise from 1 wt.% to 99 wt.%, such as from 1 wt.% to 90 wt.%, such as from 1 wt.% to 85 wt.%, such as from 1 wt.% to 80 wt.%, such as from 1 wt.% to 75 wt.%, such as from 1 wt.% to 70 wt.%, such as from 1 wt.% to 65 wt.%, such as from 1 wt.% to 60 wt.%, such as from 1 wt.% to 50 wt.%, such as from 15 wt.% to 99 wt.%, such as from 15 wt.% to 90 wt.%, such as from 15 wt.% to 85 wt.%, based on the total weight of the dispersant copolymer. %, 15% to 80% by weight, 15% to 75% by weight, 15% to 70% by weight, 15% to 65% by weight, 15% to 60% by weight, 15% to 50% by weight, 30% to 99% by weight, 30% to 90% by weight, 30% to 85% by weight, 30% to 80% by weight, 30% to 75% by weight, 30% to 70% by weight, 30% to 65% by weight, 30% to 60% by weight, 30% to 50% by weight, 35% to 99% by weight, 35% to 90% by weight,35% to 85% by weight, 35% to 80% by weight, 35% to 75% by weight, 35% to 70% by weight, 35% to 65% by weight, 35% to 60% by weight, 35% to 50% by weight, 40% to 99% by weight, 40% to 90% by weight, 40% to 85% by weight, 40% to 80% by weight, 40% to 75% by weight, 4 0% by weight to 70% by weight, etc., 40% by weight to 65% by weight, etc., 40% by weight to 60% by weight, etc., 40% by weight to 50% by weight, etc., 45% by weight to 99% by weight, etc., 45% by weight to 90% by weight, etc., 45% by weight to 85% by weight, etc., 45% by weight to 80% by weight, etc., 45% by weight to 75% by weight, etc., 45% by weight to 70% by weight, etc., 45% by weight to 65% by weight, etc., 45% by weight to 60% by weight, etc., 45 % by weight to 50% by weight, etc., 50% by weight to 99% by weight, etc., 50% by weight to 90% by weight, etc., 50% by weight to 85% by weight, etc., 50% by weight to 80% by weight, etc., 50% by weight to 75% by weight, etc., 50% by weight to 70% by weight, etc., 50% by weight to 65% by weight, etc., 50% by weight to 60% by weight, etc., 55% by weight to 99% by weight, etc., 55% by weight to 90% by weight, etc., 55% by weight to 85% by weight, etc. It may comprise 55% to 80% by weight, such as 55% to 75% by weight, such as 55% to 70% by weight, such as 55% to 65% by weight, such as 55% to 60% by weight, such as 60% to 99% by weight, such as 60% to 90% by weight, such as 60% to 85% by weight, such as 60% to 80% by weight, such as 60% to 75% by weight, such as 60% to 70% by weight, such as 60% to 65% by weight, etc. The dispersant copolymers may comprise alkyl esters of (meth)acrylic acid and / or alpha, beta-ethylenically unsaturated carboxylic acid functional monomers in an amount of from 1% to 90% by weight, such as from 1% to 85% by weight, such as from 1% to 80% by weight, such as from 1% to 75% by weight, such as from 1% to 70% by weight, such as from 1% to 65% by weight, such as from 1% to 60% by weight, such as from 1% to 50% by weight, such as from 15% to 99% by weight, such as from 15% to 90% by weight, such as from 15% to 85% by weight, such as from 15% to 80% by weight, such as from 15% to 75% by weight, such as from 15% to 70% by weight, such as from 15% to 65% by weight, such as from 15% to 60% by weight, such as from 15% to 50% by weight, based on the total weight of polymerizable monomers used in the reaction mixture.30% by weight to 99% by weight, 30% by weight to 90% by weight, 30% by weight to 85% by weight, 30% by weight to 80% by weight, 30% by weight to 75% by weight, 30% by weight to 70% by weight, 30% by weight to 65% by weight, 30% by weight to 60% by weight, 30% by weight to 50% by weight, 35% by weight to 99% by weight, 35% by weight to 90% by weight, 35% by weight to 85% by weight, 35% by weight to 80% by weight, 35% by weight to 75% by weight, 35% by weight to 70% by weight, 35% by weight % to 65% by weight, 35% to 60% by weight, 35% to 50% by weight, 40% to 99% by weight, 40% to 90% by weight, 40% to 85% by weight, 40% to 80% by weight, 40% to 75% by weight, 40% to 70% by weight, 40% to 65% by weight, 40% to 60% by weight, 40% to 50% by weight, 45% to 99% by weight, 45% to 90% by weight, 45% to 85% by weight, 45% to 80% by weight, % by weight, 45% by weight to 75% by weight, 45% by weight to 70% by weight, 45% by weight to 65% by weight, 45% by weight to 60% by weight, 45% by weight to 50% by weight, 50% by weight to 99% by weight, 50% by weight to 90% by weight, 50% by weight to 85% by weight, 50% by weight to 80% by weight, 50% by weight to 75% by weight, 50% by weight to 70% by weight, 50% by weight to 65% by weight, 50% by weight to 60% by weight, 55% by weight to 99% by weight, 55% by weight to 90% by weight, etc. It may be derived from a reaction mixture containing in an amount of 1% to 99% by weight, such as 55% to 85% by weight, such as 55% to 80% by weight, such as 55% to 75% by weight, such as 55% to 70% by weight, such as 55% to 65% by weight, such as 55% to 60% by weight, such as 60% to 99% by weight, such as 60% to 90% by weight, such as 60% to 85% by weight, such as 60% to 80% by weight, such as 60% to 75% by weight, such as 60% to 70% by weight, such as 60% to 65% by weight.
[0026] In addition to, or instead of, building blocks comprising residues of alpha, beta-ethylenically unsaturated carboxylic acids, the dispersant copolymers may comprise building blocks comprising residues of alkyl esters of (meth)acrylic acid. The alkyl ester of (meth)acrylic acid may contain 1 to 18 carbon atoms in the alkyl group, such as 1 to 12 carbon atoms, such as 1 to 8 carbon atoms, such as 1 to 6 carbon atoms, such as 1 to 4 carbon atoms, such as 1 to 3 carbon atoms, such as 1 to 2 carbon atoms, such as 2 to 18 carbon atoms, such as 2 to 12 carbon atoms, such as 2 to 8 carbon atoms, such as 2 to 6 carbon atoms, such as 2 to 4 carbon atoms, such as 2 to 3 carbon atoms, such as 3 to 18 carbon atoms, such as 3 to 12 carbon atoms, such as 3 to 8 carbon atoms, such as 3 to 6 carbon atoms, such as 3 to 4 carbon atoms, such as 4 to 18 carbon atoms, such as 4 to 12 carbon atoms, such as 4 to 11 carbon atoms, such as 4 to 10 carbon atoms, such as 4 to 9 carbon atoms, such as 4 to 8 carbon atoms, such as 4 to 7 carbon atoms, such as 4 to 6 carbon atoms. Non-limiting examples of alkyl esters of (meth)acrylic acid include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, isodecyl (meth)acrylate, stearyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate, as well as alkyl esters of (meth)acrylic acid having alicyclic groups such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate. The units comprising residues of alkyl esters of (meth)acrylic acid may constitute at least 30% by weight, such as at least 35% by weight, such as at least 40% by weight, such as at least 45% by weight, such as at least 50% by weight, such as at least 55% by weight, such as at least 60% by weight, such as at least 70% by weight, such as at least 75% by weight, such as at least 80% by weight, based on the total weight of the dispersant copolymer.The constituent units containing residues of alkyl esters of (meth)acrylic acid may constitute 99% or less by weight, such as 90% or less by weight, such as 85% or less by weight, such as 80% or less by weight, such as 75% or less by weight, such as 70% or less by weight, such as 65% or less by weight, such as 60% or less by weight, based on the total weight of the dispersant copolymer. The constituent units containing residues of alkyl esters of (meth)acrylic acid may constitute 30% to 99% by weight, such as 30% to 90% by weight, such as 30% to 85% by weight, such as 30% to 80% by weight, such as 30% to 75% by weight, such as 30% to 70% by weight, such as 30% to 65% by weight, such as 30% to 60% by weight, such as 35% to 99% by weight, such as 35% to 90% by weight, such as 35% to 85% by weight, based on the total weight of the dispersant copolymer. % to 80% by weight, 35% to 75% by weight, 35% to 70% by weight, 35% to 65% by weight, 35% to 60% by weight, 40% to 99% by weight, 40% to 90% by weight, 40% to 85% by weight, 40% to 80% by weight, 40% to 75% by weight, 40% to 70% by weight, 40% to 65% by weight, 40% to 60% by weight, 45% to 99% by weight, 45% to 90% by weight, 45% by weight to 85% by weight, 45% by weight to 80% by weight, 45% by weight to 75% by weight, 45% by weight to 70% by weight, 45% by weight to 65% by weight, 45% by weight to 60% by weight, 50% by weight to 99% by weight, 50% by weight to 90% by weight, 50% by weight to 85% by weight, 50% by weight to 80% by weight, 50% by weight to 75% by weight, 50% by weight to 70% by weight, 50% by weight to 65% by weight, 50% by weight to 60% by weight, 55% by weight to 99% by weight %, 55% by weight to 90% by weight, 55% by weight to 85% by weight, 55% by weight to 80% by weight, 55% by weight to 75% by weight, 55% by weight to 70% by weight, 55% by weight to 65% by weight, 55% by weight to 60% by weight, 60% by weight to 99% by weight, 60% by weight to 90% by weight, 60% by weight to 85% by weight, 60% by weight to 80% by weight, 60% by weight to 75% by weight, 60% by weight to 70% by weight, 60% by weight to 65% by weight, etc.The dispersant copolymer comprises an alkyl ester of (meth)acrylic acid in an amount of from 30% to 90% by weight, such as from 30% to 85% by weight, such as from 30% to 80% by weight, such as from 30% to 75% by weight, such as from 30% to 70% by weight, such as from 30% to 65% by weight, such as from 30% to 60% by weight, such as from 35% to 99% by weight, such as from 35% to 90% by weight, such as from 35% to 85% by weight, such as from 35% to 80% by weight, based on the total weight of polymerizable monomers used in the reaction mixture. 35% to 75% by weight, 35% to 70% by weight, 35% to 65% by weight, 35% to 60% by weight, 40% to 99% by weight, 40% to 90% by weight, 40% to 85% by weight, 40% to 80% by weight, 40% to 75% by weight, 40% to 70% by weight, 40% to 65% by weight, 40% to 60% by weight, 45% to 99% by weight, 45% to 90% by weight, 45% to 85% by weight, 45% by weight to 80% by weight, 45% by weight to 75% by weight, 45% by weight to 70% by weight, 45% by weight to 65% by weight, 45% by weight to 60% by weight, 50% by weight to 99% by weight, 50% by weight to 90% by weight, 50% by weight to 85% by weight, 50% by weight to 80% by weight, 50% by weight to 75% by weight, 50% by weight to 70% by weight, 50% by weight to 65% by weight, 50% by weight to 60% by weight, 55% by weight to 99% by weight, 55% by weight to 90% by weight, 5 In some embodiments, the reaction mixture may comprise from 30% to 99% by weight, such as 5% to 85% by weight, such as 55% to 80% by weight, such as 55% to 75% by weight, such as 55% to 70% by weight, such as 55% to 65% by weight, such as 55% to 60% by weight, such as 60% to 99% by weight, such as 60% to 90% by weight, such as 60% to 85% by weight, such as 60% to 80% by weight, such as 60% to 75% by weight, such as 60% to 70% by weight, such as 60% to 65% by weight.
[0027] In addition to or instead of the units containing residues of alkyl esters of (meth)acrylic acid, the dispersant copolymer may contain units containing residues of alpha, beta-ethylenically unsaturated carboxylic acids. Non-limiting examples of alpha, beta-ethylenically unsaturated carboxylic acids include those containing up to 18 carbon atoms, such as up to 16 carbon atoms, such as up to 12 carbon atoms, such as up to 10 carbon atoms, such as acrylic acid and methacrylic acid. Non-limiting examples of other unsaturated acids are alpha, beta-ethylenically unsaturated dicarboxylic acids, such as maleic acid or its anhydride, fumaric acid and itaconic acid. Also, half esters of these dicarboxylic acids may be used. The units containing residues of alpha, beta-ethylenically unsaturated carboxylic acids may constitute at least 0.1 wt%, such as at least 0.5 wt%, such as at least 1 wt%, such as at least 1.5 wt%, such as at least 3 wt%, such as at least 5 wt%, such as at least 7 wt%, such as at least 10 wt%, based on the total weight of the dispersant copolymer. Units comprising residues of alpha, beta-ethylenically unsaturated carboxylic acids may constitute 30% or less by weight, such as 20% or less, such as 15% or less, such as 10% or less, such as 8% or less, such as 6% or less, such as 5% or less, such as 4% or less, such as 3% or less, such as 2% or less, such as 1.5% or less, such as 1.0% or less, based on the total weight of the dispersant copolymer.The constitutional units comprising residues of alpha, beta-ethylenically unsaturated carboxylic acids may be present in an amount of from 0.1 wt.% to 20 wt.%, such as from 0.1 wt.% to 15 wt.%, such as from 0.1 wt.% to 10 wt.%, such as from 0.1 wt.% to 8 wt.%, such as from 0.1 wt.% to 6 wt.%, such as from 0.1 wt.% to 5 wt.%, such as from 0.1 wt.% to 4 wt.%, such as from 0.5 wt.% to 3 wt.%, such as from 0.1 wt.% to 2 wt.%, such as from 0.1 wt.% to 1.5 wt.%, such as from 0.1 wt.% to 1.0 wt.%, such as from 0.5 wt.% to 30 wt.%, such as from 0.5 wt.% to 20 wt.%, based on the total weight of the dispersant copolymer. 0.5% by weight to 15% by weight, etc., 0.5% by weight to 10% by weight, etc., 0.5% by weight to 8% by weight, etc., 0.5% by weight to 6% by weight, etc., 0.5% by weight to 5% by weight, etc., 0.5% by weight to 4% by weight, etc., 0.5% by weight to 3% by weight, etc., 0.5% by weight to 2% by weight, etc., 0.5% by weight to 1.5% by weight, etc., 0.5% by weight to 1.0% by weight, etc., 1% by weight to 30% by weight, etc., 1% by weight to 20% by weight, etc., 1% by weight to 15% by weight, etc., 1% by weight to 10% by weight, etc., 1% by weight to 8% by weight, etc., 1% by weight to 6% by weight, etc., 1% by weight to 5% by weight, etc., 1% by weight to 4% by weight etc., 1% by weight to 3% by weight, etc., 1% by weight to 2% by weight, etc., 1% by weight to 1.5% by weight, etc., 1.5% by weight to 30% by weight, etc., 1.5% by weight to 20% by weight, etc., 1.5% by weight to 15% by weight, etc., 1.5% by weight to 10% by weight, etc., 1.5% by weight to 8% by weight, etc., 1.5% by weight to 6% by weight, etc., 1.5% by weight to 5% by weight, etc., 1.5% by weight to 4% by weight, etc., 1.5% by weight to 3% by weight, etc., 1.5% by weight to 2% by weight, etc., 3% by weight to 30% by weight, etc., 3% by weight to 20% by weight, etc., 3% by weight to 15% by weight, etc., 3% by weight to 10% by weight, etc., 3% by weight to 8% by weight, %, such as 3% by weight to 6% by weight, such as 3% by weight to 5% by weight, such as 3% by weight to 4% by weight, such as 5% by weight to 30% by weight, such as 5% by weight to 20% by weight, such as 5% by weight to 15% by weight, such as 5% by weight to 10% by weight, such as 5% by weight to 8% by weight, such as 5% by weight to 6% by weight, such as 7% by weight to 30% by weight, such as 7% by weight to 20% by weight, such as 7% by weight to 15% by weight, such as 7% by weight to 10% by weight, such as 7% by weight to 8% by weight, such as 10% by weight to 30% by weight, such as 10% by weight to 20% by weight, such as 10% by weight to 15% by weight.The dispersant copolymers may comprise from 0.1 wt% to 20 wt%, such as from 0.1 wt% to 15 wt%, such as from 0.1 wt% to 10 wt%, such as from 0.1 wt% to 8 wt%, such as from 0.1 wt% to 6 wt%, such as from 0.1 wt% to 5 wt%, such as from 0.1 wt% to 4 wt%, such as from 0.5 wt% to 3 wt%, such as from 0.1 wt% to 2 wt%, such as from 0.1 wt% to 1.5 wt%, such as from 0.1 wt% to 1.0 wt%, such as from 0.5 wt% to 30 wt%, such as from 0.5 wt% to 20 wt%, based on the total weight of polymerizable monomers used in the reaction mixture. %, 0.5% by weight to 15% by weight, 0.5% by weight to 10% by weight, 0.5% by weight to 8% by weight, 0.5% by weight to 6% by weight, 0.5% by weight to 5% by weight, 0.5% by weight to 4% by weight, 0.5% by weight to 3% by weight, 0.5% by weight to 2% by weight, 0.5% by weight to 1.5% by weight, 0.5% by weight to 1.0% by weight, 1% by weight to 30% by weight, 1% by weight to 20% by weight, 1% by weight to 15% by weight, 1% by weight to 10% by weight, 1% by weight to 8% by weight, 1% by weight to 6% by weight, 1% by weight to 5% by weight, 1% by weight to 4% by weight, etc. 1% by weight to 3% by weight, 1% by weight to 2% by weight, 1% by weight to 1.5% by weight, 1.5% by weight to 30% by weight, 1.5% by weight to 20% by weight, 1.5% by weight to 15% by weight, 1.5% by weight to 10% by weight, 1.5% by weight to 8% by weight, 1.5% by weight to 6% by weight, 1.5% by weight to 5% by weight, 1.5% by weight to 4% by weight, 1.5% by weight to 3% by weight, 1.5% by weight to 2% by weight, 3% by weight to 30% by weight, 3% by weight to 20% by weight, 3% by weight to 15% by weight, 3% by weight to 10% by weight, 3% by weight to 8% by weight, 3 In some embodiments, the reaction mixture may include an amount of from 0.1% to 30% by weight, such as from 3% to 5% by weight, such as from 3% to 4% by weight, such as from 5% to 30% by weight, such as from 5% to 20% by weight, such as from 5% to 15% by weight, such as from 5% to 10% by weight, such as from 5% to 8% by weight, such as from 5% to 6% by weight, such as from 7% to 30% by weight, such as from 7% to 20% by weight, such as from 7% to 15% by weight, such as from 7% to 10% by weight, such as from 7% to 8% by weight, such as from 10% to 30% by weight, such as from 10% to 20% by weight, such as from 10% to 15% by weight.The inclusion of a unit comprising a residue of an alpha, beta-ethylenically unsaturated carboxylic acid in the dispersant copolymer results in a dispersant copolymer comprising at least one carboxylic acid group. The carboxylic acid group resulting from the inclusion of the alpha, beta-ethylenically unsaturated carboxylic acid can react with a separately added crosslinker that contains a functional group reactive with the carboxylic acid group, such as, for example, carbodiimides, polyepoxides, polyoxazolines, and polyaziridines.
[0028] The dispersant may optionally include a unit comprising a residue of an ethylenically unsaturated monomer comprising a hydroxyl functional group. Non-limiting examples of ethylenically unsaturated monomers comprising a hydroxyl functional group include hydroxyalkyl esters such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate. The unit comprising a residue of an ethylenically unsaturated monomer comprising a hydroxyl functional group may comprise at least 0.1% by weight, such as at least 0.5% by weight, such as at least 1% by weight, such as at least 1.5% by weight, such as at least 3% by weight, such as at least 5% by weight, such as at least 7% by weight, such as at least 8% by weight, based on the total weight of the dispersant. Units comprising residues of ethylenically unsaturated monomers containing hydroxyl functionality may constitute 25% by weight or less, such as 20% by weight or less, such as 15% by weight or less, such as 10% by weight or less, such as 8% by weight or less, such as 6% by weight or less, such as 5% by weight or less, such as 3% by weight or less, such as 2% by weight or less, such as 1% by weight or less, based on the total weight of the dispersant.The constitutional units comprising residues of ethylenically unsaturated monomers containing hydroxyl functionality may be from 0.1 wt% to 20 wt%, such as from 0.1 wt% to 15 wt%, such as from 0.1 wt% to 10 wt%, such as from 0.1 wt% to 8 wt%, such as from 0.1 wt% to 6 wt%, such as from 0.1 wt% to 5 wt%, such as from 0.1 wt% to 3 wt%, such as from 0.1 wt% to 2 wt%, such as from 0.1 wt% to 1 wt%, 0.5 wt% to 25 wt%, such as from 0.5 wt% to 20 wt%, 0.5 wt% to 15 wt%, such as from 0.1 wt% to 25 wt%, such as from 0.5 wt% to 20 wt%, based on the total weight of the dispersant. % by weight, 0.5% by weight to 10% by weight, 0.5% by weight to 8% by weight, 0.5% by weight to 6% by weight, 0.5% by weight to 5% by weight, 0.5% by weight to 3% by weight, 0.5% by weight to 2% by weight, 0.5% by weight to 1% by weight, 1% by weight to 25% by weight, 1% by weight to 20% by weight, 1% by weight to 15% by weight, 1% by weight to 10% by weight, 1% by weight to 8% by weight, 1% by weight to 6% by weight, 1% by weight to 5% by weight, 1% by weight to 3% by weight, 1% by weight to 2% by weight, etc. , 1.5% by weight to 25% by weight, etc., 1.5% by weight to 20% by weight, etc., 1.5% by weight to 15% by weight, etc., 1.5% by weight to 10% by weight, etc., 1.5% by weight to 8% by weight, etc., 1.5% by weight to 6% by weight, etc., 1.5% by weight to 5% by weight, etc., 1.5% by weight to 3% by weight, etc., 1.5% by weight to 2% by weight, etc., 3% by weight to 25% by weight, etc., 3% by weight to 20% by weight, etc., 3% by weight to 15% by weight, etc., 3% by weight to 10% by weight, etc., 3% by weight to 8% by weight, etc., 3% by weight to 6% by weight, etc., 3% by weight to 5% by weight, %, such as 5 wt% to 25 wt%, such as 5 wt% to 20 wt%, such as 5 wt% to 15 wt%, such as 5 wt% to 10 wt%, such as 5 wt% to 8 wt%, such as 5 wt% to 6 wt%, such as 7 wt% to 25 wt%, such as 7 wt% to 20 wt%, such as 7 wt% to 15 wt%, such as 7 wt% to 10 wt%, such as 7 wt% to 8 wt%, such as 8 wt% to 25 wt%, such as 8 wt% to 20 wt%, such as 8 wt% to 15 wt%, such as 8 wt% to 10 wt%, etc.The dispersant may optionally comprise from 0.1 wt % to 20 wt %, such as from 0.1 wt % to 15 wt %, such as from 0.1 wt % to 10 wt %, such as from 0.1 wt % to 8 wt %, such as from 0.1 wt % to 6 wt %, such as from 0.1 wt % to 5 wt %, such as from 0.1 wt % to 3 wt %, such as from 0.1 wt % to 2 wt %, such as from 0.1 wt % to 1 wt %, such as from 0.5 wt % to 25 wt %, 0.5 wt % to 20 wt %, etc., based on the total weight of polymerizable monomers used in the reaction mixture. , 0.5% by weight to 15% by weight, etc., 0.5% by weight to 10% by weight, etc., 0.5% by weight to 8% by weight, etc., 0.5% by weight to 6% by weight, etc., 0.5% by weight to 5% by weight, etc., 0.5% by weight to 3% by weight, etc., 0.5% by weight to 2% by weight, etc., 0.5% by weight to 1% by weight, etc., 1% by weight to 25% by weight, etc., 1% by weight to 20% by weight, etc., 1% by weight to 15% by weight, etc., 1% by weight to 10% by weight, etc., 1% by weight to 8% by weight, etc., 1% by weight to 6% by weight, etc., 1% by weight to 5% by weight, etc., 1% by weight to 3% by weight, etc. %, 1.5% by weight to 25% by weight, 1.5% by weight to 20% by weight, 1.5% by weight to 15% by weight, 1.5% by weight to 10% by weight, 1.5% by weight to 8% by weight, 1.5% by weight to 6% by weight, 1.5% by weight to 5% by weight, 1.5% by weight to 3% by weight, 1.5% by weight to 2% by weight, 3% by weight to 25% by weight, 3% by weight to 20% by weight, 3% by weight to 15% by weight, 3% by weight to 10% by weight, 3% by weight to 8% by weight, 3% by weight to 6% by weight, 3% by weight to 5% by weight, 5% by weight to 6% by weight, 5% by weight to 7% by weight, 5% by weight to 8% by weight, 5% by weight to 9% by weight, 5% by weight to 10% by weight, 5% by weight to 15% by weight, 5% by weight to 10% by weight, 5% by weight to 8% by weight, 5% by weight to 6% by weight, 5% by weight to 5 ... The dispersant may be derived from a reaction mixture comprising 0.1% to 25% by weight, such as 5% to 25% by weight, such as 5% to 20% by weight, such as 5% to 15% by weight, such as 5% to 10% by weight, such as 5% to 8% by weight, such as 5% to 6% by weight, such as 7% to 25% by weight, such as 7% to 20% by weight, such as 7% to 15% by weight, such as 7% to 10% by weight, such as 7% to 8% by weight, such as 8% to 25% by weight, such as 8% to 20% by weight, such as 8% to 15% by weight, such as 8% to 10% by weight. Inclusion of a constitutional unit comprising a residue of an ethylenically unsaturated monomer containing a hydroxyl functionality in the dispersant results in a dispersant containing at least one hydroxyl group (although the hydroxyl group may be included by other methods).The hydroxyl groups resulting from the inclusion of hydroxyalkyl esters (or incorporated by other means) can react with a separately added crosslinker that contains functional groups that react with hydroxyl groups, e.g., aminoplasts, phenolplasts, polyepoxides, etc., having groups that react with hydroxyl groups are incorporated into the dispersant.
[0029] Alternatively, the dispersant may be substantially free, essentially free, or completely free of constitutional units comprising residues of ethylenically unsaturated monomers that contain hydroxyl functionality.
[0030] The dispersant may be substantially free, essentially free, or completely free of constitutional units comprising residues of alkyl esters of (meth)acrylic acid containing at least 8 carbon atoms in the alkyl group.
[0031] As used herein, a dispersant is "substantially free" of structural units containing residues of monomers, and if monomers are present, they are present in an amount of less than 0.1 wt. %, based on the total weight of the dispersant. As used herein, a dispersant is "essentially free" of structural units containing residues of monomers, and if monomers are present, they are present in an amount of less than 0.01 wt. %, based on the total weight of the dispersant. As used herein, if no monomers are present in the dispersant, the dispersant is "completely free" of structural units containing residues of monomers, i.e., 0.000 wt. %, based on the total weight of the dispersant.
[0032] The dispersant copolymer may further comprise a unit comprising a residue of a vinyl aromatic compound. Non-limiting examples of vinyl aromatic compounds include styrene, alpha-methylstyrene, alpha-chlorostyrene, and vinyltoluene. The unit comprising a residue of a vinyl aromatic compound may comprise at least 0.1% by weight, such as at least 1% by weight, such as at least 5% by weight, such as at least 10% by weight, such as at least 15% by weight, such as at least 20% by weight, such as at least 25% by weight, based on the total weight of the dispersant copolymer. The unit comprising a residue of a vinyl aromatic compound may comprise 50% by weight or less, such as 40% by weight or less, such as 30% by weight or less, such as 20% by weight or less, such as 15% by weight or less, such as 10% by weight or less, based on the total weight of the dispersant copolymer. The constituent units comprising residues of vinyl aromatic compounds may comprise from 0.1 wt% to 50 wt%, such as from 0.1 wt% to 40 wt%, such as from 0.1 wt% to 30 wt%, such as from 0.1 wt% to 20 wt%, such as from 0.1 wt% to 15 wt%, such as from 0.1 wt% to 10 wt%, such as from 1 wt% to 50 wt%, such as from 1 wt% to 40 wt%, such as from 1 wt% to 30 wt%, such as from 1 wt% to 20 wt%, such as from 1 wt% to 15 wt%, such as from 1 wt% to 10 wt%, such as from 5 wt% to 50 wt%, such as from 5 wt% to 40 wt%, such as from 5 wt% to 3 ... % to 20% by weight, etc., 5% by weight to 15% by weight, etc., 5% by weight to 10% by weight, etc., 10% by weight to 50% by weight, etc., 10% by weight to 40% by weight, etc., 10% by weight to 30% by weight, etc., 10% by weight to 20% by weight, etc., 10% by weight to 15% by weight, etc., 15% by weight to 50% by weight, etc., 15% by weight to 40% by weight, etc., 15% by weight to 30% by weight, etc., 15% by weight to 20% by weight, etc., 20% by weight to 50% by weight, etc., 20% by weight to 40% by weight, etc., 20% by weight to 30% by weight, etc., 25% by weight to 50% by weight, etc., 25% by weight to 40% by weight, etc., 25% by weight to 30% by weight, etc.The dispersant copolymer may comprise a vinyl aromatic compound in an amount of from 0.1 wt% to 50 wt%, such as from 0.1 wt% to 40 wt%, such as from 0.1 wt% to 30 wt%, such as from 0.1 wt% to 20 wt%, such as from 0.1 wt% to 15 wt%, such as from 0.1 wt% to 10 wt%, such as from 1 wt% to 50 wt%, such as from 1 wt% to 40 wt%, such as from 1 wt% to 30 wt%, such as from 1 wt% to 20 wt%, such as from 1 wt% to 15 wt%, such as from 1 wt% to 10 wt%, such as from 5 wt% to 50 wt%, such as from 5 wt% to 40 wt%, such as from 5 wt% to 3 ... based on the total weight of polymerizable monomers used in the reaction mixture. 20% by weight, such as 5% to 15% by weight, such as 5% to 10% by weight, such as 10% to 50% by weight, such as 10% to 40% by weight, such as 10% to 30% by weight, such as 10% to 20% by weight, such as 10% to 15% by weight, such as 15% to 50% by weight, such as 15% to 40% by weight, such as 15% to 30% by weight, such as 15% to 20% by weight, such as 20% to 50% by weight, such as 20% to 40% by weight, such as 20% to 30% by weight, such as 25% to 50% by weight, such as 25% to 40% by weight, such as 25% to 30% by weight.
[0033] The dispersant may optionally include building blocks containing residues of other alpha, beta-ethylenically unsaturated monomers. Non-limiting examples of other alpha, beta-ethylenically unsaturated monomers include organic nitriles such as acrylonitrile and methacrylonitrile; allyl monomers such as allyl chloride and allyl cyanide; monomeric dienes such as 1,3-butadiene and 2-methyl-1,3-butadiene; acetoacetoxyalkyl (meth)acrylates such as acetoacetoxyethyl methacrylate (AAEM) (which may be self-crosslinked); difunctional unsaturated monomers such as ethylene glycol dimethacrylate, hexanediol diacrylate; vinyl esters such as vinyl acetate; N-vinyl acyclic amides; (meth)acrylamides such as acrylamide, N-butoxymethylol acrylamide, N-methylol acrylamide, isopropyl acrylamide, and diacetone acrylamide. Building blocks containing residues of other alpha, beta-ethylenically unsaturated monomers may comprise at least at least 0.5% by weight, such as at least 1% by weight, such as at least 1.5% by weight, based on the total weight of the dispersant. Units comprising residues of other alpha, beta-ethylenically unsaturated monomers may constitute 20% by weight, such as 15% by weight or less, such as 8% by weight or less, such as 6% by weight or less, such as 5% by weight or less, such as 4% by weight or less, such as 3% by weight or less, such as 2% by weight or less, such as 1.5% by weight or less, such as 1.0% by weight or less, based on the total weight of the dispersant.The building blocks containing residues of other alpha, beta-ethylenically unsaturated monomers may be present in an amount of from 0.5% to 15% by weight, such as from 0.5% to 10% by weight, such as from 0.5% to 8% by weight, such as from 0.5% to 6% by weight, such as from 0.5% to 5% by weight, such as from 0.5% to 4% by weight, such as from 0.5% to 3% by weight, such as from 0.5% to 2% by weight, such as from 0.5% to 1.5% by weight, such as from 0.5% to 1.0% by weight, such as from 1% to 20% by weight, such as from 1% to 15% by weight, such as from 1% to 10% by weight, based on the total weight of the dispersant. It may constitute 0.5% to 20% by weight, such as 1% to 8% by weight, such as 1% to 6% by weight, such as 1% to 5% by weight, such as 1% to 4% by weight, such as 1% to 3% by weight, such as 1% to 2% by weight, such as 1% to 1.5% by weight, such as 1.5% to 20% by weight, such as 1.5% to 15% by weight, such as 1.5% to 10% by weight, such as 1.5% to 8% by weight, such as 1.5% to 6% by weight, such as 1.5% to 5% by weight, such as 1.5% to 4% by weight, such as 1.5% to 3% by weight, such as 1.5% to 2% by weight. The dispersant may optionally be present in the reaction mixture in the form of other alpha, beta-ethylenically unsaturated monomers, such as from 0.5% to 15% by weight, such as from 0.5% to 10% by weight, such as from 0.5% to 8% by weight, such as from 0.5% to 6% by weight, such as from 0.5% to 5% by weight, such as from 0.5% to 4% by weight, such as from 0.5% to 3% by weight, such as from 0.5% to 2% by weight, such as from 0.5% to 1.5% by weight, such as from 0.5% to 1.0% by weight, such as from 1% to 20% by weight, such as from 1% to 15% by weight, such as from 1% to 10% by weight, based on the total weight of polymerizable monomers used in the reaction mixture. In some embodiments, the reaction mixture may include an amount of from 0.5 wt% to 20 wt%, such as from 1 wt% to 8 wt%, such as from 1 wt% to 6 wt%, such as from 1 wt% to 5 wt%, such as from 1 wt% to 4 wt%, such as from 1 wt% to 3 wt%, such as from 1 wt% to 2 wt%, such as from 1 wt% to 1.5 wt%, such as from 1.5 wt% to 20 wt%, such as from 1.5 wt% to 15 wt%, such as from 1.5 wt% to 10 wt%, such as from 1.5 wt% to 8 wt%, such as from 1.5 wt% to 6 wt%, such as from 1.5 wt% to 5 wt%, such as from 1.5 wt% to 4 wt%, such as from 1.5 wt% to 3 wt%, such as from 1.5 wt% to 2 wt%.
[0034] Alternatively, the dispersant may be substantially free, essentially free, or completely free of constitutional units comprising residues of any of the other alpha, beta-ethylenically unsaturated monomers mentioned above.
[0035] The monomers and relative amounts may be selected such that the resulting dispersant may have a Tg of +100° C. or less. The resulting dispersant may have a Tg of at least at least −70° C., such as at least −60° C., such as at least −55° C., such as at least −50° C., such as at least −40° C., such as at least −30° C., such as at least −20° C., such as at least −15° C., such as at least −10° C., such as at least −5° C., such as at least 0° C. The resulting dispersant may have a Tg of at most +50° C., such as at most +40° C., such as at most +25° C., such as at most +15° C., such as at most +10° C., such as at most +5° C., such as at most 0° C. The resulting dispersion may be, for example, -70~+100°C, -70~+50°C, -70~+40°C, -70~+25°C, -70~+20°C, -70~+15°C, -70~+10°C, -70~+5°C, -70~0°C, -60~+100°C, -60~+50°C, -60~+40°C, -60~+25°C, -60~+20°C, -60~+15°C, -6 0~+10℃, -60~+5℃, -60~0℃, -55~+100℃, -55~+50℃, -55~+40℃, -55~+25℃, -55~+20℃, -55~+15℃, -55~+10℃, -55~+5℃, -55~0℃, -50~+100℃, -50~+50℃, -50~+40℃, -50~+25℃, -50~+20℃ -50~+15℃, -50~+10℃, -50~+5℃, -50~0℃, -40~+100℃, -40~+50℃, -40~+40℃, -40~+25℃, -40~+20℃, -40~+15℃, -40~+10℃, -40~+5℃, -40~0℃, -30~+100℃, -30~+50℃, -30~+40℃ +25℃, -30~+20℃, -30~+15℃, -30~+10℃, -30~+5℃, -30~0℃, -20~+100℃, -20~+50℃, -20~+40℃, -20~+25℃, -20~+20℃, -20~+15℃, -20~+10℃, -20~+5℃, -20~0℃, -15~+100℃, -15~+50℃,-15~+40℃, -15~+25℃, -15~+20℃, -15~+15℃, -15~+10℃, -15~+5℃, -15~0℃, -10~+100℃, -10~+50℃, -10~+40℃, -10~+25℃, -10~+20℃, -10~+15℃, -10~+10℃, -10~+5℃ , such as -10 to 0°C, -5 to +100°C, -5 to +50°C, -5 to +40°C, -5 to +25°C, -5 to +20°C, -5 to +15°C, -5 to +10°C, -5 to +5°C, -5 to 0°C, 0 to +100°C, 0 to +50°C, 0 to +40°C, 0 to +25°C, 0 to +20°C, 0 to +15°C, etc. A Tg of less than 0°C may be desirable to ensure acceptable battery performance at low temperatures.
[0036] The dispersant may have a weight average molecular weight of at least 2,000 g / mol, such as at least 5,000 g / mol, such as at least 20,000 g / mol, such as at least 50,000 g / mol, such as at least 75,000 g / mol, such as at least 95,000 g / mol. The dispersant may have a weight average molecular weight of 1,000,000 g / mol or less, such as 500,000 g / mol or less, such as 200,000 g / mol or less, such as 150,000 g / mol or less, such as 100,000 g / mol. Dispersants are 2,000~500,000g / mol, 2,000~200,000g / mol, 2,000~150,000g / mol, 2,000~100,000g / mol, 5,000~1,000,000g / mol, 5,000~500,000g / mol, 5,000~200,000g / mol, 5,000~150,000g / mol, 5,000~100,000g / mol, 20,000~1,000,000g / mol, 20,000~500,000g / mol, 20,000~200,000g / mol, 20,000~150,000g / mol, 20,000~100,000g / mol, 50,000~1,000,000g / mol, 50,000~ 500,000g / mol, 50,000~200,000g / mol, 50,000~150,000g / mol, 50,000~100,000g / mol, 75,000~1,000,000g / mol, 75,000~500,000g / mol, 75,000~200,000g / mol, 75,000~150,000g / mol , such as 75,000 to 100,000 g / mol, such as 95,000 to 1,000,000 g / mol, such as 95,000 to 500,000 g / mol, such as 95,000 to 200,000 g / mol, such as 95,000 to 150,000 g / mol, such as 95,000 to 100,000 g / mol.
[0037] The dispersants may be prepared by conventional free radical initiated solution polymerization techniques in which polymerizable monomers are dissolved in an organic medium containing a solvent or mixture of solvents and polymerized in the presence of a free radical initiator until conversion is complete.
[0038] Examples of free radical initiators are those that are soluble in organic media such as azobisisobutyronitrile, azobis(alpha,gamma-methylvaleronitrile), tertiary butyl perbenzoate, tertiary butyl peracetate, benzoyl peroxide, di-tertiary butyl peroxide, and tertiary amyl peroxy 2-ethylhexyl carbonate.
[0039] Optionally, chain transfer agents may be used that are soluble in mixtures of monomers such as alkyl mercaptans, e.g., tertiary dodecyl mercaptan, ketones such as methyl ethyl ketone, chlorinated hydrocarbons such as chloroform, etc. The chain transfer agents provide control over molecular weight to give products with the necessary viscosities for various coating applications.
[0040] To prepare the dispersant, the solvent may first be heated to reflux, and then a mixture of polymerizable monomers and a mixture of free radical initiator in an organic medium may be added separately to the refluxing solvent over a period of time. The reaction mixture is then held at polymerization temperature to reduce the free monomer content to below 1.0 percent, typically below 0.5 percent, based on the total weight of the mixture of polymerizable monomers.
[0041] After polymerization in the organic medium and prior to dispersion in the aqueous medium, the carboxylic acid groups of the dispersing agent, if present, may be at least partially neutralized by contacting the dispersing agent with a neutralizing base. Examples of suitable neutralizing bases include, but are not limited to, tertiary amines such as dimethylethanolamine (DMEA), trimethylamine, methyldiethanolamine, ethylmethylethanolamine, dimethylethylamine, dimethylpropylamine, dimethyl 3-hydroxy-1-propylamine, dimethylbenzylamine, dimethyl 2-hydroxy-1-propylamine, diethylmethylamine, dimethyl 1-hydroxy-2-propylamine, triethylamine, tributylamine, N-methylmorpholine, etc.; ammonia; hydrazine; metallic aluminum; metallic zinc; water-soluble oxides of the elements Li, Na, K, Mg, Ca, Fe(II), and Sn(II); water-soluble hydroxides of the elements Li, Na, K, Mg, Ca, Fe(II), and Sn(II); water-soluble carbonates of the elements Li, Na, K, Mg, Ca, Fe(II), and Sn(II); and combinations thereof. The neutralizing base may include a tertiary amine. The neutralizing base may include dimethylethanolamine (DMEA).
[0042] The solution polymerized dispersant may be substantially dissolved and / or dispersed in water before, during, or after the addition of the neutralizing base. The solution polymerized dispersant may be substantially dissolved and / or dispersed in water during the addition of the neutralizing base. Thus, the solution polymerized dispersant may be formed in a solvent and then substantially dissolved and / or dispersed in water. The solution polymerized dispersant may be formed in a solvent and then substantially dissolved in water. The solution polymerized dispersant has sufficient functionality so that it can be substantially dissolved in water.
[0043] The dispersants may also be prepared by conventional emulsion polymerization techniques. The dispersants may be prepared by conventional emulsion batch or continuous processes. In one example of a batch process, the monomer composition is fed into a heated reactor that is initially charged with water over a period of 1 hour to 4 hours. The initiator may be fed simultaneously, may be part of the monomer composition, or may be charged to the reactor prior to being fed to the monomer composition. The optimum temperature will depend on the particular initiator used. The length of time may range from 2 hours to 6 hours, and the reaction temperature may range from 25°C to 90°C.
[0044] In another example, a small portion of the water and monomer composition may be charged to the reactor along with a small amount of surfactant and free radical initiator to form a seed. The remaining monomer, surfactant, and water pre-emulsion is fed along with initiator for a predetermined period of time (e.g., 3 hours) at a reaction temperature of about 80°C to 85°C using a nitrogen blanket. After a 1 hour hold, once the monomer feed is complete, a post redox feed is added to the reactor to reduce the remaining free monomers (including hydrogen peroxide / isoascorbic acid). The latex product is then neutralized to a pH of 7 to 8.
[0045] The emulsion polymerization reaction mixture may include a surfactant. The surfactant may be an anionic, cationic, or nonionic type of stabilizer. Suitable examples of anionic surfactants include, but are not limited to, alkyl sulfates, such as sodium dodecyl sulfate or sodium polyoxyethylene alkyl ether sulfate; aryl sulfonates, such as sodium dodecyl benzene sulfonate; sulfosuccinates, such as sodium diisobutyl sulfosuccinate, sodium dioctyl sulfosuccinate, and sodium dicyclohexyl sulfosuccinate; and combinations thereof. Suitable examples of nonionic emulsifiers include, but are not limited to, fatty alcohol ethoxylates, such as polyethylene glycol monolauryl ether; fatty acid ethoxylates, such as polyethylene glycol monostearate or polyethylene glycol monolaurate; polyether block polymers, such as polyethylene glycol / polypropylene glycol block polymers, also known as Pluronics (commercially available products of this type include Tergitol (RTM) XJ, XH, or XD, available from Dow Chemical), and combinations thereof. Suitable examples of cationic emulsifiers include, but are not limited to, amine salts such as cetyltrimethylammonium chloride or benzyldodecyldimethylammonium bromide, and combinations thereof. It will be understood by those skilled in the art that a mixture of anionic and cationic emulsifiers may not be desirable. Also, reactive surfactants may be used, in which the surfactant contains unsaturated groups, such as allyl groups, that allow copolymerization with ethylenically unsaturated monomers. Suitable examples include, but are not limited to, Adeka Reasoap SR-10, Hitenol BC-1025, and Maxemul 6106.
[0046] To carry out the polymerization of ethylenically unsaturated monomers, a free radical initiator is usually present. Both water-soluble and oil-soluble initiators may be used. The addition of certain initiators, such as redox initiators, can produce a strong exothermic reaction, so it is generally desirable to add the initiator to the other components just before the reaction is carried out. Examples of water-soluble initiators include ammonium peroxydisulfate, potassium peroxydisulfate, and hydrogen peroxide. Examples of oil-soluble initiators include t-butyl hydroperoxide, dilauryl peroxide, t-butyl perbenzoate, and 2,2'-azobis(isobutyronitrile). Redox initiators such as ammonium peroxydisulfate / sodium metabisulfite or t-butyl hydroperoxide / isoascorbic acid may be utilized herein.
[0047] Alternatively, dispersions in aqueous media can be prepared by high stress techniques such as microfluidization by using a MICROFLUIDIZER® emulsifier available from Microfluidics Corporation of Newton, Mass. The MICROFLUIDIZER® high pressure impingement emulsifier is disclosed in U.S. Pat. No. 4,533,254, which is incorporated herein by reference. The device operates at high pressures (up to 1.4×10 5 It consists of a 20,000 psi (300 kPa) pump and an interaction chamber where emulsification takes place. The pump forces a mixture of reactants in an aqueous medium into the chamber where the reactants are split into at least two streams that pass at very high speeds through at least two slits, colliding and resulting in atomization of the mixture into small particles. Typically, the flow rate is 3.5×10 4 ~1×10 5The reaction mixture is passed through the emulsifier once at a pressure of 5,000-15,000 psi (kPa). Multiple passes can result in smaller average particle sizes and narrower particle size distribution ranges. When using the aforementioned MICROFLUIDIZER® emulsifier, the stress is applied by liquid-liquid impingement as described. However, it should be understood that other modes of applying stress to the pre-emulsified mixture can be utilized if desired, so long as sufficient stress is applied to achieve the required particle size distribution, i.e., such that less than 20% of the polymer particulates have an average diameter greater than 5 microns after polymerization. For example, one alternative mode of applying stress would be the use of ultrasonic energy.
[0048] Once polymerization is complete, the resulting product is a stable dispersion of dispersant in aqueous medium. Thus, the aqueous medium may be substantially free of water-soluble dispersant. The resulting dispersant is, of course, insoluble in aqueous medium. As used herein, "substantially free" means that the aqueous medium contains 30% or less by weight of dissolved dispersant, such as 15% or less by weight, based on the total weight of dispersant. "Stably dispersed" means that the polymer microparticles do not settle on standing and do not essentially coagulate or aggregate during production or standing.
[0049] The particle size of the dispersant in the aqueous medium may be uniformly small, i.e., after polymerization, less than 20% by weight of the dispersant has an average diameter greater than 5 microns, such as greater than 1 micron. Generally, the dispersant has an average diameter of 0.01 microns to 10 microns. The average diameter of the dispersant after polymerization may range from 0.05 microns to 0.5 microns. The particle size may be measured with a particle size analyzer, such as the Coulter N4 instrument available from Coulter. The instrument is provided with detailed instructions for particle size measurement. However, briefly, a sample of the aqueous dispersion is diluted with water until the sample concentration is within the specified limits required by the instrument. The measurement time is 10 minutes.
[0050] The dispersant copolymer may be present in the binder in an amount of at least 0.1 wt%, such as at least 1 wt%, such as at least 3 wt%, such as at least 5 wt%, such as at least 7 wt%, such as at least 9 wt%, such as at least 10 wt%, based on the total weight of the binder solids. The dispersant may be present in the binder in an amount of no more than 20 wt%, such as no more than 15 wt%, such as no more than 10 wt%, such as no more than 25 wt%, based on the total weight of the binder solids. The dispersant may be present in the binder in an amount of no more than 0.1 wt%, such as from 0.1 wt% to 20 wt%, such as from 0.1 wt% to 15 wt%, such as from 0.1 wt% to 10 wt%, such as from 1 wt% to 25 wt%, such as from 1 wt% to 20 wt%, such as from 1 wt% to 15 wt%, such as from 1 wt% to 10 wt%, such as from 3 wt% to 20 wt%, such as from 3 wt% to 15 wt%, such as from 3 wt% to 10 wt%, such as from 5 wt% to 20 wt%, based on the total weight of the binder solids. It may be present in the binder in an amount of 0.1% to 25% by weight, such as 5% to 15% by weight, such as 5% to 10% by weight, such as 7% to 20% by weight, such as 7% to 15% by weight, such as 7% to 10% by weight, such as 9% to 20% by weight, such as 9% to 15% by weight, such as 9% to 10% by weight, such as 10% to 20% by weight, such as 10% to 15% by weight.
[0051] The dispersant may be present in the slurry composition in an amount of at least 0.01 wt%, such as at least 0.05 wt%, such as at least 0.1 wt%, such as at least 0.3 wt%, based on the total solids weight of the slurry composition. The dispersant may be present in an amount of 3 wt% or less, such as 2 wt% or less, such as 1 wt% or less, such as 0.5 wt% or less, based on the total solids weight of the slurry composition. The dispersant may be present in an amount of 0.01 wt% to 3 wt%, such as 0.01 wt% to 2 wt%, such as 0.01 wt% to 1 wt%, such as 0.01 wt% to 0.5 wt%, such as 0.05 wt% to 3 wt%, such as 0.05 wt% to 2 wt%, such as 0.05 wt% to 1 wt%, such as 0.05 wt% to 0.5 wt%, such as 0.1 wt% to 3 wt%, such as 0.1 wt% to 2 wt%, such as 0.1 wt% to 1 wt%, such as 0.1 wt% to 0.5 wt%, such as 0.3 wt% to 3 wt%, such as 0.3 wt% to 2 wt%, such as 0.3 wt% to 1 wt%, such as 0.3 wt% to 0.5 wt%, based on the total solids weight of the slurry composition.
[0052] The dispersant may be present in the slurry composition in an amount of at least 0.005 wt%, such as at least 0.02 wt%, such as at least 0.05 wt%, such as at least 0.15 wt%, based on the total weight of the slurry composition. The dispersant may be present in an amount of 1.5 wt% or less, such as 1 wt% or less, such as 0.5 wt% or less, such as 0.3 wt% or less, based on the total weight of the slurry composition. The dispersant may be present in an amount of 0.005 wt% to 1 wt%, such as 0.005 wt% to 0.5 wt%, such as 0.005 wt% to 0.3 wt%, such as 0.02 wt% to 1.5 wt%, such as 0.02 wt% to 1 wt%, such as 0.02 wt% to 0.5 wt%, such as 0.02 wt% to 0.3 wt%, such as 0.05 wt% to 1.5 wt%, such as 0.05 wt% to 1 wt%, such as 0.05 wt% to 0.5 wt%, such as 0.05 wt% to 0.3 wt%, such as 0.15 wt% to 1.5 wt%, such as 0.15 wt% to 1 wt%, such as 0.15 wt% to 0.5 wt%, such as 0.15 wt% to 0.3 wt%, based on the total weight of the slurry composition.
[0053] The slurry composition of the present disclosure further comprises an aqueous medium. As used herein, the term "aqueous medium" refers to a liquid medium comprising more than 50 wt% water, based on the total weight of the aqueous medium. The aqueous medium may comprise water in an amount of at least 60 wt%, such as at least 70 wt%, such as at least 80 wt%, such as at least 90 wt%, based on the total weight of the aqueous medium. The aqueous medium may comprise water in an amount of 51 wt% to 100 wt%, such as 60 wt% to 100 wt%, such as 70 wt% to 100 wt%, such as 80 wt% to 100 wt%, such as 90 wt% to 100 wt%, based on the total weight of the aqueous medium. The aqueous medium may be present in an amount of at least 30 wt%, such as at least 35% wt%, such as at least 40% wt%, such as at least 45 wt%, based on the total weight of the slurry composition. The aqueous medium may be present in an amount of 60 wt% or less, such as 55 wt% or less, such as 50 wt% or less, based on the total weight of the slurry composition. The aqueous medium may be present in an amount such as 30% to 60% by weight, such as 30% to 55% by weight, such as 30% to 50% by weight, such as 35% to 60% by weight, such as 35% to 55% by weight, such as 35% to 50% by weight, such as 40% to 60% by weight, such as 40% to 55% by weight, such as 40% to 50% by weight, such as 45% to 60% by weight, such as 45% to 55% by weight, such as 45% to 50% by weight, based on the total weight of the slurry composition.
[0054] In addition to or in place of the dispersants described above, the slurry composition may include a poly(2-alkyl or aryl oxazoline) polymer. As used herein, "poly(2-alkyl or aryl oxazoline) polymer" refers to a polymer prepared by polymerizing 2-alkyl or aryl oxazoline monomers by a cationic ring-opening polymerization reaction resulting in an acyl-substituted linear polyethyleneimine polymer, and also refers to a copolymer containing residues of 2-alkyl or aryl oxazoline monomers. Non-limiting examples of 2-alkyl or aryl oxazoline monomers include 2-methyl-2-oxazoline, 2-ethyl-2-oxazoline, 2-phenyl-2-oxazoline, 2-butyl-2-oxazoline, 2-isopropenyl-2-oxazoline, and 2-isopropyl-2-oxazoline, among others. For example, poly(2-alkyl or aryl oxazoline) polymers can be prepared according to the following schematic diagram, where R is a C1-C 10 The initiator X may be an alkyl or aryl group such as an alkyl group, such as a C1-C6 alkyl group, such as a C1-C4 alkyl group, such as a C1-C2 alkyl group, or a phenyl group, and the initiator X may be an alkyl tosylate (X1 is methyl and X2 is toluenesulfonate, etc.) or a triflate (X1 is an alkyl or aryl group and X2 is a triflate anion), or an alkyl halide such as benzyl bromide. The initiator may also contain other functional groups such as, for example, olefins, alkynes, esters, amides, urethanes, and / or ether groups, so long as they do not react during the polymerization. [ka] A nucleophilic terminator Y can be used to terminate the polymerization. Common examples include water, alcohols (aliphatic or aromatic), ammonia, amines (aliphatic or aromatic), thiols (aliphatic or aromatic), and / or carboxylic acids (aliphatic or aromatic), and the corresponding carboxylate salts. Terminators can also contain other functional groups, such as ethylenically unsaturated, for example, acrylic acid and methacrylic acid. The corresponding polyoxazolines containing functional initiators and / or terminators can be incorporated into other polymer systems by covalent bonding reactions. A non-limiting example of a poly(2-alkyl or aryl oxazoline) polymer is a poly(2-ethyl-2-oxazoline) polymer, where R in the above schematic is an ethyl group. Other non-limiting examples of poly(2-alkyl or aryl oxazoline) polymers, where R is a hydrocarbyl group including methyl, ethyl, propyl, butyl, propenyl, crotyl, or benzyl, or an acyl group including formyl, acetyl, propionyl, butyryl, acrylol, or crotonyl, or any combination thereof. The polymerization reaction may be terminated by any suitable means, such as, for example, reaction with water, an alcohol, an acid, an amine, or a nucleophile.
[0055] The poly(2-alkyl or aryl oxazoline) polymer may be present in an amount of from 0.1 wt.% to 20 wt.%, such as from 0.1 wt.% to 15 wt.%, such as from 0.1 wt.% to 10 wt.%, such as from 1 wt.% to 25 wt.%, such as from 1 wt.% to 20 wt.%, such as from 1 wt.% to 15 wt.%, such as from 1 wt.% to 10 wt.%, such as from 3 wt.% to 20 wt.%, such as from 3 wt.% to 15 wt.%, such as from 3 wt.% to 1 It may be present in an amount of 0.1% to 25% by weight, such as 0% by weight, such as 5% to 20% by weight, such as 5% to 15% by weight, such as 5% to 10% by weight, such as 7% to 20% by weight, such as 7% to 15% by weight, such as 7% to 10% by weight, such as 9% to 20% by weight, such as 9% to 15% by weight, such as 9% to 10% by weight, such as 10% to 20% by weight, such as 10% to 15% by weight. The poly(2-alkyl or aryl oxazoline) polymer may be present in an amount of 0.005 wt% to 1 wt%, such as 0.005 wt% to 0.5 wt%, such as 0.005 wt% to 0.3 wt%, such as 0.02 wt% to 1.5 wt%, such as 0.02 wt% to 1 wt%, such as 0.02 wt% to 0.5 wt%, such as 0.02 wt% to 0.3 wt%, such as 0.05 wt% to 1.5 wt%, such as 0.05 wt% to 1 wt%, such as 0.05 wt% to 0.5 wt%, such as 0.05 wt% to 0.3 wt%, such as 0.15 wt% to 1.5 wt%, such as 0.15 wt% to 1 wt%, such as 0.15 wt% to 0.5 wt%, such as 0.15 wt% to 0.3 wt%, based on the total solids weight of the slurry composition. The poly(2-alkyl or aryl oxazoline) polymer may be present in an amount of 0.005 wt% to 1 wt%, such as 0.005 wt% to 0.5 wt%, such as 0.005 wt% to 0.3 wt%, such as 0.02 wt% to 1.5 wt%, such as 0.02 wt% to 1 wt%, such as 0.02 wt% to 0.5 wt%, such as 0.02 wt% to 0.3 wt%, such as 0.05 wt% to 1.5 wt%, such as 0.05 wt% to 1 wt%, such as 0.05 wt% to 0.5 wt%, such as 0.05 wt% to 0.3 wt%, such as 0.15 wt% to 1.5 wt%, such as 0.15 wt% to 1 wt%, such as 0.15 wt% to 0.5 wt%, such as 0.15 wt% to 0.3 wt%, based on the total weight of the slurry composition.
[0056] Surprisingly, it has been discovered that the use of a dispersant copolymer and / or a poly(2-alkyl or aryl oxazoline) polymer in the anode aqueous slurry effectively breaks down aggregates of the carbonaceous material, maintaining a continuous carbon network to promote sufficient electrical contact.
[0057] The slurry composition may further include a crosslinking agent, if desired. The crosslinking agent should be soluble or dispersible in aqueous media and reactive with the active hydrogen groups of the dispersant copolymer, such as carboxylic acid groups and hydroxyl groups, if present. Non-limiting examples of suitable crosslinking agents include aminoplast resins, phenoplast resins, carbodiimides, polyoxazolines, polyaziridines, blocked polyisocyanates, and polyepoxides.
[0058] Examples of aminoplast resins for use as crosslinkers are those formed by reacting triazines such as melamine or benzoguanamine with formaldehyde. These reaction products contain reactive N-methylol groups. These reactive groups are usually etherified with methanol, ethanol, butanol, including mixtures thereof, to adjust their reactivity. For chemical preparation and use of aminoplast resins, see "The Chemistry and Applications of Amino Crosslinking Agents or Aminoplast", Vol. V, Part II, page 21 ff., edited by Dr. Oldring; John Wiley & Sons / Cita Technology Limited, London, 1998. These resins are commercially available under the trademark MAPRENAL®, such as MAPRENAL MF980, and under the trademark CYMEL®, such as CYMEL 303 and CYMEL 1128, available from Cytec Industries.
[0059] Blocked polyisocyanate crosslinkers are typically diisocyanates such as toluene diisocyanate, 1,6-hexamethylene diisocyanate, and isophorone diisocyanate, which contain isocyanate dimers and trimers in which the isocyanate groups are reacted ("blocked") with materials such as epsilon-caprolactone and methyl ethyl ketoxime. At curing temperatures, the blocking agent unblocks to expose isocyanate functional groups that are reactive with the hydroxyl functional groups associated with the reactive polymer of the binder. Blocked polyisocyanate crosslinkers are commercially available from Covestro as DESMODUR BL.
[0060] Phenoplast resins are formed by the condensation of aldehydes with phenols. Suitable aldehydes include formaldehyde and acetaldehyde. Methylene and aldehyde releasing agents such as paraformaldehyde and hexamethylenetetramine may also be utilized as aldehyde agents. Various phenols may be used, such as phenol itself, cresol, or substituted phenols in which a hydrocarbon radical having either a straight-chain, branched-chain, or cyclic structure replaces the hydrogen of the aromatic ring. Also, mixtures of phenols may be used. Some specific examples of suitable phenols are unsaturated hydrocarbon-substituted phenols such as p-phenylphenol, p-tert-butylphenol, p-tert-amylphenol, cyclopentylphenol, and monobutenylphenol, which contains butenyl groups in the ortho, meta, or para positions and in which the double bonds occur at various positions in the hydrocarbon chain.
[0061] The carbodiimide crosslinker may be in monomeric or polymeric form, or a mixture thereof. Carbodiimide crosslinker refers to a compound having the following structure: [ka] wherein R and R' may each individually comprise an aliphatic group, an aromatic group, an alkylaromatic group, a carboxylic acid group, or a heterocyclic group. Examples of commercially available carbodiimide crosslinkers include those sold under the trade name CARBODILITE available from Nisshinbo Chemical Inc., such as, for example, CARBODILITE V-02-L2, CARBODILITE SV-02, CARBODILITE E-02, CARBODILITE SW-12G, CARBODILITE V-10, and CARBODILITE E-05.
[0062] Examples of polyoxazoline include compounds or polymers that have two or more oxazoline groups in a molecule.Unlike the poly(2-alkyl or aryl oxazoline) polymers discussed above, which are prepared by polymerizing 2-alkyl or aryl oxazoline monomers by cationic ring-opening polymerization reaction to produce acyl-substituted linear polyethyleneimine polymers, polyoxazoline crosslinkers contain at least two oxazoline groups in a molecule.Some or all of the hydrogen atoms of the oxazoline groups can be replaced with other groups. Non-limiting examples of divalent oxazoline compounds include 2,2'-bis(2-oxazoline), 2,2'-bis(4-methyl-2-oxazoline), 2,2'-bis(4,4-dimethyl-2-oxazoline), 2,2'-bis(4-ethyl-2-oxazoline), 2,2'-bis(4,4'-diethyl-2-oxazoline), 2,2'-bis(4-propyl-2-oxazoline), 2,2'-bis(4-butyl-2-oxazoline), 2,2'-bis(4-hexyl-2-oxazoline), 2,2'-bis(4-phenyl-2-oxazoline), 2,2'-bis(4-cyclohexyl-2-oxazoline), and 2,2'-bis(4-benzyl-2-oxazoline).Non-limiting examples of polyoxazoline polymers include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-4-ethyl-2-oxazoline, 2-vinyl-4-propyl-2-oxazoline, 2-vinyl-4-butyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-vinyl-5-ethyl-2-oxazoline, 2-vinyl-5-propyl-2-oxazoline, 2-vinyl-5-butyl-2-oxazoline, 2-isopropenyl ... Examples of the polyoxazoline curing agent include those containing the residue of an oxazoline group-containing monomer, including 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-4-ethyl-2-oxazoline, 2-isopropenyl-4-propyl-2-oxazoline, 2-isopropenyl-4-butyl-2-oxazoline, 2-isopropenyl-5-methyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline, 2-isopropenyl-5-propyl-2-oxazoline, and 2-isopropenyl-5-butyl-2-oxazoline. These oxazoline group-containing monomers can be used alone or in combination of two or more of them in any ratio, and may be polymerized with other ethylenically unsaturated monomers. Non-limiting examples of commercially available polyoxazoline curing agents include the EPOCROS family of crosslinking agents available from NIPPON SHOKUBAI CO.,LTD.
[0063] Examples of polyepoxide crosslinkers are epoxy-containing (meth)acrylic polymers such as those prepared from glycidyl methacrylate copolymerized with other vinyl monomers, polyglycidyl ethers of polyhydric phenols such as diglycidyl ether of bisphenol A; and alicyclic polyepoxides such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and bis(3,4-epoxy-6-methylcyclohexyl-methyl)adipate.
[0064] The crosslinking agent may be present in the slurry composition in an amount of at least 0.1% by weight, such as at least 0.3% by weight, such as at least 0.5% by weight, such as at least 1.0% by weight, such as at least 1.25% by weight, such as at least 1.5% by weight, such as at least 2.0% by weight, such as at least 2.5% by weight, based on the total weight of the binder solids. The crosslinking agent may be present in the slurry composition in an amount of 25% by weight or less, such as 20% by weight or less, such as 15% by weight or less, such as 12.5% by weight or less, such as 10% by weight or less, such as 7.5% by weight or less, such as 5% by weight or less, such as 3% by weight or less, such as 1.5% by weight or less, based on the total weight of the binder solids. The crosslinker may be present in an amount of from 0.1 wt.% to 20 wt.%, such as from 0.1 wt.% to 15 wt.%, such as from 0.1 wt.% to 12.5 wt.%, such as from 0.1 wt.% to 10 wt.%, such as from 0.1 wt.% to 7.5 wt.%, such as from 0.1 wt.% to 5 wt.%, such as from 0.1 wt.% to 3 wt.%, such as from 0.1 wt.% to 1.5 wt.%, such as from 0.3 wt.% to 25 wt.%, such as from 0.3 wt.% to 20 wt.%, such as from 0.3 wt.% to 25 ... 15% by weight, 0.3% to 12.5% by weight, 0.3% to 10% by weight, 0.3% to 7.5% by weight, 0.3% to 5% by weight, 0.3% to 3% by weight, 0.3% to 1.5% by weight, 0.5% to 25% by weight, 0.5% to 20% by weight, 0.5% to 15% by weight, 0.5% to 12.5% by weight, 0.5% to 10% by weight, 0. 5% by weight to 7.5% by weight, 0.5% by weight to 5% by weight, 0.5% by weight to 3% by weight, 0.5% by weight to 1.5% by weight, 1.0% by weight to 25% by weight, 1.0% by weight to 20% by weight, 1.0% by weight to 15% by weight, 1.0% by weight to 12.5% by weight, 1.0% by weight to 10% by weight, 1.0% by weight to 7.5% by weight, 1.0% by weight to 5% by weight, 1.0% by weight to 3% by weight, 1.0% by weight to 1.5% by weight, etc., 1.25% by weight to 25% by weight, etc., 1.25% by weight to 20% by weight, etc., 1.25% by weight to 15% by weight, etc., 1.25% by weight to 12.5% by weight, etc., 1.25% by weight to 10% by weight, etc., 1.25% by weight to 7.5% by weight, etc., 1.25% by weight to 5% by weight, etc., 1.25% by weight to 3% by weight, etc., 1.25% by weight to 1.5% by weight, etc., 1.5% by weight to 25% by weight, etc.5% by weight to 20% by weight, etc., 1.5% by weight to 15% by weight, etc., 1.5% by weight to 12.5% by weight, etc., 1.5% by weight to 10% by weight, etc., 1.5% by weight to 7.5% by weight, etc., 1.5% by weight to 5% by weight, etc., 1.5% by weight to 3% by weight, etc., 2.0% by weight to 25% by weight, etc., 2.0% by weight to 20% by weight, etc., 2.0% by weight to 15% by weight, etc., 2.0% by weight to 12.5% by weight, etc., 2.0% by weight to 10% by weight, etc., 2.0% by weight to 7 It may be present in the slurry composition in an amount of 0.1% to 25% by weight, such as 0.5% by weight, such as 2.0% to 5% by weight, such as 2.0% to 3% by weight, such as 2.5% to 25% by weight, such as 2.5% to 20% by weight, such as 2.5% to 15% by weight, such as 2.5% to 12.5% by weight, such as 2.5% to 10% by weight, such as 2.5% to 7.5% by weight, such as 2.5% to 5% by weight, such as 2.5% to 3% by weight.
[0065] As used herein, the term "binder solids" refers to the resinous components of the slurry composition and includes at least the binder resin (e.g., styrene butadiene copolymer), cellulose or cellulose derivative, dispersant copolymer, poly(2-alkyl or aryl oxazoline) polymer, and crosslinker.
[0066] The binder solids may be present in the slurry composition in an amount of at least 1 wt%, such as at least 1.5 wt%, such as at least 2 wt%, such as at least 3 wt%, such as at least 4 wt%, based on the total solids weight of the slurry. The binder solids may be present in the slurry composition in an amount of 10 wt% or less, such as 7.5 wt% or less, such as 5 wt% or less, such as 4 wt% or less, such as 3 wt% or less, based on the total solids weight of the slurry. The binder solids may be present in the slurry composition in an amount of 1 wt% to 10 wt%, such as 1 wt% to 7.5 wt%, such as 1 wt% to 5 wt%, such as 1 wt% to 4 wt%, such as 1 wt% to 3 wt%, such as 1.5 wt% to 10 wt%, such as 1.5 wt% to 7.5 wt%, such as 1.5 wt% to 5 wt%, such as 1.5 wt% to 4 wt%, such as 1.5 wt% to 3 wt%, such as 2 wt% to 10 wt%, such as 2 wt% to 7.5 wt%, such as 2 wt% to 5 wt%, such as 2 wt% to 4 wt%, such as 2 wt% to 3 wt%, such as 3 wt% to 10 wt%, such as 3 wt% to 7.5 wt%, such as 3 wt% to 5 wt%, such as 3 wt% to 4 wt%, such as 4 wt% to 10 wt%, such as 4 wt% to 7.5 wt%, such as 4 wt% to 5 wt%, such as 4 wt% to 5 wt%, based on the total solids weight of the slurry.
[0067] The slurry composition further includes a negative electrode active material. The material constituting the negative electrode active material contained in the slurry is not particularly limited, and a suitable material can be selected according to the type of the target electric storage device. The negative electrode active material can include graphite, silicon, silicon oxide, tin, germanium, silver, aluminum, barium, bismuth, copper, gallium, indium, nickel, phosphorus, lead, antimony, silicon, tin, strontium, zinc, titanium, or a combination thereof.
[0068] The negative electrode active material may be present in the slurry composition in an amount of at least 80 wt%, such as at least 85 wt%, such as at least 90 wt%, such as at least 91 wt%, such as at least 92 wt%, such as at least 93 wt%, such as at least 94 wt%, such as at least 95 wt%, such as at least 97 wt%, such as at least 98 wt%, such as 93 wt%, such as 94 wt%, such as 95 wt%, such as 97 wt%, such as 98 wt%, based on the total solids weight of the slurry composition. The negative electrode active material may be present in the slurry composition in an amount of 98.9 wt% or less, such as 97 wt% or less, such as 95 wt% or less, based on the total solids weight of the slurry composition. The negative electrode active material may comprise, based on the total solids weight of the slurry composition, 80 wt% to 97 wt%, such as 80 wt% to 95 wt%, such as 85 wt% to 98.9 wt%, such as 85 wt% to 97 wt%, such as 85 wt% to 95 wt%, such as 90 wt% to 98.9 wt%, such as 90 wt% to 97 wt%, such as 90 wt% to 95 wt%, such as 91 wt% to 98.9 wt%, such as 91 wt% to 97 wt%, such as 91 wt% to 95 wt%, such as 92 wt% to 98.9 wt%, ... The slurries may be present in the slurry composition in an amount of from 80% to 98.9% by weight, such as from 92% to 95% by weight, such as from 93% to 98.9% by weight, such as from 93% to 97% by weight, such as from 93% to 95% by weight, such as from 94% to 98.9% by weight, such as from 94% to 97% by weight, such as from 94% to 95% by weight, such as from 95% to 98.9% by weight, such as from 95% to 97% by weight, such as from 97% to 98.9% by weight, such as from 98% to 98.9% by weight.
[0069] The negative electrode active material may be present in the slurry composition in an amount of at least 35 wt%, such as at least 40 wt%, such as at least 42 wt%, such as at least 44 wt%, such as at least 45 wt%, such as at least 47 wt%, such as at least 49 wt%, such as at least 51 wt%, based on the total weight of the slurry composition. The negative electrode active material may be present in the slurry composition in an amount of 54 wt% or less, such as 52 wt% or less, such as 48.9 wt% or less, such as 48 wt% or less, such as 46 wt% or less, based on the total weight of the slurry composition. The negative electrode active material may be, based on the total weight of the slurry composition, 35 wt% to 52 wt%, such as 35 wt% to 48.9 wt%, such as 35 wt% to 48 wt%, such as 35 wt% to 46 wt%, such as 40 wt% to 54 wt%, such as 40 wt% to 52 wt%, such as 40 wt% to 48.9 wt%, such as 40 wt% to 48 wt%, such as 40 wt% to 46 wt%, such as 42 wt% to 54 wt%, such as 42 wt% to 52 wt%, such as 42 wt% to 48.9 wt%, such as 42 wt% to 48 ... The slurry composition may be present in an amount of from 35% to 54% by weight, such as from 42% to 46% by weight, such as from 45% to 54% by weight, such as from 45% to 52% by weight, such as from 45% to 48.9% by weight, such as from 45% to 48% by weight, such as from 45% to 46% by weight, such as from 47% to 54% by weight, such as from 47% to 52% by weight, such as from 47% to 48.9% by weight, such as from 47% to 48% by weight, such as from 49% to 54% by weight, such as from 49% to 52% by weight.
[0070] The slurry composition of the present disclosure may further include a conductive additive, if necessary. The conductive additive is a material that has a higher electrical conductivity than graphite. Non-limiting examples of the conductive additive include carbonaceous materials such as activated carbon, carbon black such as acetylene black and furnace black, graphene, carbon nanotubes including single-walled carbon nanotubes and / or multi-walled carbon nanotubes, carbon fibers, fullerenes, and combinations thereof.
[0071] The conductive additive may be present in the slurry in an amount of at least 0.01 wt%, such as at least 0.05 wt%, such as at least 0.1 wt%, such as at least 0.5 wt%, such as at least 1 wt%, such as at least 1.5 wt%, such as at least 2 wt%, based on the total solids weight of the slurry. The conductive additive may be present in the slurry in an amount of 10 wt% or less, such as 7.5 wt% or less, such as 5 wt% or less, such as 4 wt% or less, such as 3 wt% or less, such as 2.5 wt% or less, such as 2 wt% or less, such as 1.5 wt% or less, based on the total solids weight of the slurry.The conductive additive may be, based on the total solids weight of the slurry, from 0.01 wt.% to 7.5 wt.%, such as from 0.01 wt.% to 5 wt.%, such as from 0.01 wt.% to 4 wt.%, such as from 0.01 wt.% to 3 wt.%, such as from 0.01 wt.% to 2.5 wt.%, such as from 0.01 wt.% to 2 wt.%, such as from 0.01 wt.% to 1.5 wt.%, such as from 0.05 wt.% to 10 wt.%, such as from 0.05 wt.% to 7.5 wt.%, such as from 0.05 wt.% to 5 wt.%, such as from 0.05 wt.% to 4 wt.%, such as from 0.05 wt.% to 5 ...%, such as from 0.05 wt.%, such as from 0.0 Amount% to 3% by weight, etc., 0.05% to 2.5% by weight, etc., 0.05% to 2% by weight, etc., 0.05% to 1.5% by weight, etc., 0.1% to 10% by weight, etc., 0.1% to 7.5% by weight, etc., 0.1% to 5% by weight, etc., 0.1% to 4% by weight, etc., 0.1% to 3% by weight, etc., 0.1% to 2.5% by weight, etc., 0.1% to 2% by weight, etc., 0.1% to 1.5% by weight, etc., 0.5% to 10% by weight, etc., 0.5% to 7.5% by weight, etc. % by weight, 0.5% by weight to 5% by weight, 0.5% by weight to 4% by weight, 0.5% by weight to 3% by weight, 0.5% by weight to 2.5% by weight, 0.5% by weight to 2% by weight, 0.5% by weight to 1.5% by weight, 1% by weight to 10% by weight, 1% by weight to 7.5% by weight, 1% by weight to 5% by weight, 1% by weight to 4% by weight, 1% by weight to 3% by weight, 1% by weight to 2.5% by weight, 1% by weight to 2% by weight, 1% by weight to 1.5% by weight, 1.5% by weight It may be present in the slurry in an amount of from 0.01% to 10% by weight, such as from 1.5% to 7.5% by weight, such as from 1.5% to 5% by weight, such as from 1.5% to 4% by weight, such as from 1.5% to 3% by weight, such as from 1.5% to 2.5% by weight, such as from 1.5% to 2% by weight, such as from 2% to 10% by weight, such as from 2% to 7.5% by weight, such as from 2% to 5% by weight, such as from 2% to 4% by weight, such as from 2% to 3% by weight, such as from 2% to 2.5% by weight.
[0072] The negative electrode aqueous slurry composition may have a solids content of at least 30 wt%, such as at least 35 wt%, such as at least 40 wt%, such as at least 45 wt%, such as at least 50 wt%, such as at least 55 wt%, such as at least 60 wt%, based on the total weight of the slurry. The negative electrode aqueous slurry composition may have a solids content of 70 wt% or less, such as 60 wt% or less, such as 55 wt% or less, such as 50 wt% or less, such as 45 wt% or less, such as 40 wt% or less, such as 35 wt% or less, based on the total weight of the slurry. The negative electrode aqueous slurry composition may be, based on the total weight of the slurry, 30 wt% to 60 wt%, such as 30 wt% to 55 wt%, such as 30 wt% to 50 wt%, such as 30 wt% to 45 wt%, such as 30 wt% to 40 wt%, such as 30 wt% to 35 wt%, such as 35 wt% to 70 wt%, such as 35 wt% to 60 wt%, such as 35 wt% to 55 wt%, such as 35 wt% to 50 wt%, such as 35 wt% to 45 wt%, such as 35 wt% to 40 wt%, such as 40 wt% to 70 wt%, Such as, for example, 40% to 60% by weight, such as 40% to 55% by weight, such as 40% to 50% by weight, such as 40% to 45% by weight, such as 45% to 70% by weight, such as 45% to 60% by weight, such as 45% to 55% by weight, such as 45% to 50% by weight, such as 50% to 70% by weight, such as 50% to 60% by weight, such as 50% to 55% by weight, such as 55% to 70% by weight, such as 55% to 60% by weight.
[0073] As used herein, "solids content" or "total solids" refers to the content of non-volatile matter in a slurry composition, i.e., materials that will not volatilize when heated at 150° C. for 60 minutes.
[0074] The negative electrode aqueous slurry composition may include a negative electrode active material, a binder including a styrene-butadiene copolymer and cellulose or a cellulose derivative, a dispersant copolymer, and an aqueous medium, and may further include a crosslinker and / or a conductive additive, as necessary.
[0075] The negative electrode aqueous slurry composition may include a negative electrode active material, a binder including a styrene butadiene copolymer and cellulose or a cellulose derivative, a melamine crosslinker, and an aqueous medium.
[0076] A negative electrode aqueous slurry composition including an aqueous medium, a negative electrode active material, a binder (which may include a separately added crosslinker), a dispersant copolymer, and optional ingredients such as a conductive additive, may be prepared by combining the ingredients to form a slurry. These materials may be mixed together by stirring with known means such as a stirrer, a bead mill, or a high pressure homogenizer.
[0077] For mixing and stirring for the preparation of the electrode slurry composition, a mixer that can stir these components to a degree that satisfies the dispersion conditions should be selected. The degree of dispersion can be measured by a grain gauge, and mixing and dispersion can ensure that there are no agglomerates of 100 microns or larger. Examples of mixers that meet this condition include ball mills, sand mills, pigment dispersers, grinders, extruders, rotor stators, pug mills, ultrasonic dispersers, homogenizers, planetary mixers, Hobart mixers, and combinations thereof.
[0078] The present disclosure is also directed to a negative electrode comprising: (a) a current collector; and (b) a film formed on the current collector, the film comprising a binder; a dispersant, the dispersant comprising a copolymer comprising (a) a constituent unit comprising a residue of a monomer comprising a nitrogen-containing heterocycle, and (b) a constituent unit comprising a residue of an alkyl ester of (meth)acrylic acid and / or a residue of an acid-functional ethylenically unsaturated monomer, the constituent unit comprising the residue of a monomer comprising a nitrogen-containing heterocycle being 1 wt% to 50 wt%, the weight percentage being based on the total weight of the dispersant; and a negative electrode active material. The film may be deposited from the above-mentioned negative electrode aqueous slurry composition. The negative electrode may be manufactured by applying the above-mentioned slurry composition to the surface of the current collector to form a coating film, and then drying and / or curing the coating film. The coating film may have a thickness of at least 1 micron, such as at least 1-500 microns (μm), such as at least 10-100 microns, such as at least 10-70 microns, such as at least 10-50 microns, such as at least 10-30 microns, such as at least 20-100 microns, such as at least 20-70 microns, such as at least 20-50 microns, such as at least 20-30 microns, such as at least 25-100 microns, such as at least 25-70 microns, such as at least 25-50 microns, such as at least 35-100 microns, such as at least 35-70 microns, such as at least 35-50 microns. The coating film may comprise a crosslinked coating, and the film may further comprise residues of a crosslinking agent. The current collector may comprise a conductive material, and the conductive material may comprise metals such as iron, copper, aluminum, nickel, and alloys thereof, and stainless steel. For example, the current collector may comprise aluminum or copper in the form of a mesh, sheet, or foil. The shape and thickness of the current collector are not particularly limited, but the current collector may have a thickness of about 0.001 to 0.5 mm, such as a mesh, sheet, or foil having a thickness of about 0.001 to 0.5 mm.
[0079] The binder can enable the fabrication of a negative electrode containing graphite as the negative electrode active material that has good charge density. For example, the electrode can have a charge density of at least 1.0 mAh / cm 2 etc., at least 2.0mAh / cm 2etc., at least 2.5mAh / cm 2 etc., at least 3.0mAh / cm 2 etc., at least 3.5mAh / cm 2 etc., at least 4.0mAh / cm 2 etc., at least 4.5mAh / cm 2 etc., at least 5.0mAh / cm 2 etc., at least 6.0mAh / cm 2 etc., at least 7.0mAh / cm 2 etc., at least 8.0mAh / cm 2 etc., at least 10.0mAh / cm 2 At least 0.5mAh / cm 2 The electrode may have an areal capacity of 8.0 mAh / cm 2 For example, 7.0mAh / cm 2 For example, 6.0mAh / cm 2 For example, 5.0mAh / cm 2 For example, 4.5mAh / cm 2 For example, 4.0mAh / cm 2 For example, 3.5mAh / cm 2 For example, 3.0mAh / cm 2 For example, 2.5mAh / cm 2 For example, 2.0mAh / cm 2 For example, 1.5mAh / cm 2 For example, 1.0mAh / cm 2 10.0mAh / cm 2 The electrodes may have an areal capacity of 0.5 to 8.0 mAh / cm 2 etc., 0.5~7.0mAh / cm 2 etc., 0.5~6.0mAh / cm 2 etc., 0.5~5.0mAh / cm 2 etc., 0.5~4.5mAh / cm 2 etc., 0.5~4.0mAh / cm 2 etc., 0.5~3.5mAh / cm 2 etc., 0.5~3.0mAh / cm 2 etc., 0.5~2.5mAh / cm 2 etc., 0.5~2.0mAh / cm 2etc., 0.5~2.0mAh / cm 2 etc., 0.5~1.5mAh / cm 2 etc., 0.5~1.0mAh / cm 2 etc., 1.0~10.0mAh / cm 2 etc., 1.0~8.0mAh / cm 2 etc., 1.0~7.0mAh / cm 2 etc., 1.0~6.0mAh / cm 2 etc., 1.0~5.0mAh / cm 2 etc., 1.0~4.5mAh / cm 2 etc., 1.0~4.0mAh / cm 2 etc., 1.0~3.5mAh / cm 2 etc., 1.0~3.0mAh / cm 2 etc., 1.0~2.5mAh / cm 2 etc., 1.0~2.0mAh / cm 2 etc., 1.0~2.0mAh / cm 2 etc., 1.0~1.5mAh / cm 2 etc., 1.5~10.0mAh / cm 2 etc., 1.5~8.0mAh / cm 2 etc., 1.5~7.0mAh / cm 2 etc., 1.5~6.0mAh / cm 2 etc., 1.5~5.0mAh / cm 2 etc., 1.5~4.5mAh / cm 2 etc., 1.5~4.0mAh / cm 2 etc., 1.5~3.5mAh / cm 2 etc., 1.5~3.0mAh / cm 2 etc., 1.5~2.5mAh / cm 2 etc., 1.5~2.0mAh / cm 2 etc., 1.5~2.0mAh / cm 2 etc., 2.0~10.0mAh / cm 2 etc., 2.0~8.0mAh / cm 2 etc., 2.0~7.0mAh / cm 2 etc., 2.0~6.0mAh / cm 2 etc., 2.0~5.0mAh / cm 2 etc., 2.0~4.5mAh / cm 2etc., 2.0~4.0mAh / cm 2 etc., 2.0~3.5mAh / cm 2 etc., 2.0~3.0mAh / cm 2 etc., 2.0~2.5mAh / cm 2 etc., 2.5~10.0mAh / cm 2 etc., 2.5~8.0mAh / cm 2 etc., 2.5~7.0mAh / cm 2 etc., 2.5~6.0mAh / cm 2 etc., 2.5~5.0mAh / cm 2 etc., 2.5~4.5mAh / cm 2 etc., 2.5~4.0mAh / cm 2 etc., 2.5~3.5mAh / cm 2 etc., 2.5~3.0mAh / cm 2 etc., 3.0~10.0mAh / cm 2 etc., 3.0~8.0mAh / cm 2 etc., 3.0~7.0mAh / cm 2 etc., 3.0~6.0mAh / cm 2 etc., 3.0~5.0mAh / cm 2 etc., 3.0~4.5mAh / cm 2 etc., 3.0~4.0mAh / cm 2 etc., 3.0~3.5mAh / cm 2 etc., 3.5~10.0mAh / cm 2 etc., 3.5~8.0mAh / cm 2 etc., 3.5~7.0mAh / cm 2 etc., 3.5~6.0mAh / cm 2 etc., 3.5~5.0mAh / cm 2 etc., 3.5~4.5mAh / cm 2 etc., 3.0~4.0mAh / cm 2 etc., 3.0~3.5mAh / cm 2 etc., 3.5~10.0mAh / cm 2 etc., 3.5~8.0mAh / cm 2 etc., 3.5~7.0mAh / cm 2 etc., 3.5~6.0mAh / cm 2 etc., 3.5~5.0mAh / cm 2etc., 3.5~4.5mAh / cm 2 etc., 3.5~4.0mAh / cm 2 etc., 4.0~10.0mAh / cm 2 etc., 4.0~8.0mAh / cm 2 etc., 4.0~7.0mAh / cm 2 etc., 4.0~6.0mAh / cm 2 etc., 4.0~5.0mAh / cm 2 etc., 4.0~4.5mAh / cm 2 etc., 4.5~10.0mAh / cm 2 etc., 4.5~8.0mAh / cm 2 etc., 4.5~7.0mAh / cm 2 etc., 4.5~6.0mAh / cm 2 etc., 4.5~5.0mAh / cm 2 etc., 5.0~10.0mAh / cm 2 etc., 5.0~8.0mAh / cm 2 etc., 5.0~7.0mAh / cm 2 etc., 5.0~6.0mAh / cm 2 etc., 6.0~10.0mAh / cm 2 etc., 6.0~8.0mAh / cm 2 etc., 6.0~7.0mAh / cm 2 etc., 7.0~10.0mAh / cm 2 etc., 7.0~8.0mAh / cm 2 etc., 8.0~10.0mAh / cm 2 0.5 to 10.0 mAh / cm 2 The area capacity may be 100 μm.
[0080] In addition, the current collector may be pretreated with a pretreatment composition prior to depositing the slurry composition. As used herein, the term "pretreatment composition" refers to a composition that, upon contact with the current collector, reacts with the current collector surface, chemically alters the current collector surface, and bonds to the current collector surface to form a protective layer. The pretreatment composition may be a pretreatment composition that includes a Group IIIB metal and / or a Group IVB metal. As used herein, the term "Group IIIB metal and / or Group IVB metal" refers to, for example, a pretreatment composition that includes a Group IIIB metal and / or a Group IVB metal, as described in Handbook of Chemistry and Physics, 63 (1999), pp. 111-115, 2001. rd edition (1983). Where applicable, the metal itself may be used, however, Group IIIB metal compounds and / or Group IVB metal compounds may also be used. As used herein, the term "Group IIIB metal compounds and / or Group IVB metal compounds" refers to compounds that include at least one element that is in Group IIIB or Group IVB of the CAS Periodic Table of Elements. Suitable pretreatment compositions and methods for pretreating current collectors are described in U.S. Pat. No. 9,273,399, column 4, line 60 to column 10, line 26, the cited portions of which are incorporated herein by reference. The pretreatment compositions may be used to treat current collectors that are used to produce positive or negative electrodes.
[0081] The method of applying the slurry composition to the current collector is not particularly limited. The slurry composition may be applied by doctor blade coating, dip coating, reverse roll coating, direct roll coating, gravure coating, extrusion coating, immersion, or brushing. The amount of the slurry composition applied is not particularly limited, but the thickness of the coating formed per side of the current collector after the aqueous medium is removed may be at least 1 micron, such as 1 to 500 microns (μm), such as 150 to 500 μm, such as 200 to 500 μm, or thicker. For example, the thickness of the coating formed may be 200 microns or thicker than 200 microns per side.
[0082] Drying and / or crosslinking of the coating film after application, if applicable, may be accomplished by heating at elevated temperatures, such as at least 40°C, such as at least 50°C, such as at least 60°C, such as 40-145°C, such as 50-120°C, such as 60-100°C. Heating times will depend somewhat on temperature. Generally, the higher the temperature, the less time required for curing. Typically, curing times are at least 30 seconds, such as at least 2 minutes, such as at least 5 minutes, and may range up to 60 minutes. The temperature and time should be sufficient so that the binder in the cured film (if applicable) is crosslinked, i.e., covalent bonds are formed between co-reactive groups, such as carboxylic acid groups and hydroxyl groups on the polymer of the binder, and the N-methylol and / or N-methylol ether groups of the aminoplast, the isocyanate groups of the blocked polyisocyanate crosslinker. Other methods of drying the coating film include ambient temperature drying, microwave drying, and infrared drying, and other methods of curing the coating film include electron beam curing and UV curing.
[0083] During discharge of a lithium ion storage device, lithium ions are released from the negative electrode and can conduct electrical current to the positive electrode. This process may involve a process known as deintercalation. During charging, lithium ions migrate from the electrochemically active material of the positive electrode to the negative electrode and become embedded in the electrochemically active material present in the negative electrode. This process may involve a process known as intercalation.
[0084] The present invention is also directed to an electrical storage device. An electrical storage device according to the present disclosure may be manufactured by using the above negative electrode prepared from the negative electrode aqueous slurry composition of the present disclosure. The electrical storage device may further include a positive electrode, an electrolyte, and a polymer separator. The positive electrode includes a positive electrode active material, non-limiting examples of the positive electrode active material including the active material may include materials capable of incorporating lithium (including uptake via lithium intercalation / deintercalation), materials capable of lithium conversion, or combinations thereof. Non-limiting examples of electrochemically active materials capable of incorporating lithium include LiCoO2, LiNiO2, LiFePO4, LiCoPO4, LiMnO2, LiMn2O4, Li(Ni x Mn y Co z )O2 (also known as "NMC", where x+y+z is approximately 1, e.g., LiNiO, abbreviated as NMC111 or NMC333) 0.333 Mn 0.333 Co 0.333 O2, LiNi, abbreviated as NMC532 (or NCM523) 0.5 Mn 0.3 Co 0.2 O2, LiNi abbreviated as NMC622 0.6 Mn 0.2 Co 0.2 O2, and LiNi, abbreviated as NMC811 0.8 Mn 0.1 Co 0.1 O2), Li(NiCoAl)O2, carbon-coated LiFePO4, and combinations thereof. Non-limiting examples of lithium convertible materials include sulfur, LiO2, FeF2, and FeF3, Si, aluminum, tin, SnCo, Fe3O4, and combinations thereof. Power storage devices according to the present disclosure include cells, batteries, battery packs, secondary batteries, capacitors, and supercapacitors.
[0085] The power storage device can be manufactured by including an electrolyte and using components such as a separator according to a commonly used method. A more specific manufacturing method is to assemble a negative electrode and a positive electrode together with a separator therebetween, roll or fold the resulting assembly according to the shape of the battery, place the battery container, inject the electrolyte into the battery container, and seal the battery container. The shape of the battery can be coin, button, or sheet-like, cylindrical, square, or flat.
[0086] The electrolyte may be a liquid or a gel, and the electrolyte that can effectively function as a battery may be selected from among known electrolytes used in power storage devices according to the types of negative and positive active materials. The electrolyte may be a solution containing an electrolyte dissolved in a suitable solvent. The electrolyte may be a conventionally known lithium salt for lithium ion secondary batteries. Examples of lithium salts include LiClO4, LiBF4, LiPF6, LiCF3CO2, LiAsF6, LiSbF6, LiB 10 Cl 10 , LiAlCl4, LiCl, LiBr, LiB(C2H5)4, LiB(C6H5)4, LiCF3SO3, LiCH3SO3, LiC4F9SO3, Li(CF3SO2)2N, LiB4CH3SO3Li, and CF3SO3Li. The solvent for dissolving the above electrolyte is not particularly limited, and examples thereof include organic carbonate compounds such as propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate, lactone compounds such as γ-butyl lactone, ether compounds such as trimethoxymethane, 1,2-dimethoxyethane, diethyl ether, 2-ethoxyethane, tetrahydrofuran, and 2-methyltetrahydrofuran, and sulfoxide compounds such as dimethyl sulfoxide. The concentration of the electrolyte in the electrolytic solution can be 0.5 to 3.0 mol / L, for example, 0.7 to 2.0 mol / L.
[0087] As used herein, the term "polymer" broadly refers to oligomers, and both homopolymers and copolymers. The term "resin" is used interchangeably with "polymer."
[0088] The terms "acrylic acid" and "acrylate" are used interchangeably (unless doing so changes the intended meaning) and include acrylic acid, their anhydrides and derivatives, C1-C5 alkyl esters, lower alkyl substituted acrylic acids, such as methacrylic acid, C1-C2 substituted acrylic acids such as 2-ethylacrylic acid, and C1-C4 alkyl esters thereof, unless expressly indicated otherwise. The term "(meth)acrylic acid" or "(meth)acrylate" is intended to cover both the acrylic acid / acrylate and methacrylic acid / methacrylate forms of the indicated material, such as a (meth)acrylate monomer. The term "(meth)acrylic polymer" refers to a polymer prepared from one or more (meth)acrylic monomers.
[0089] As used herein, molecular weight is determined by gel permeation chromatography using polystyrene standards. Unless otherwise indicated, molecular weight is on a weight average basis. As used herein, "weight average molecular weight" or "(M w The term "weight average molecular weight (M)" refers to the weight average molecular weight (M) determined by gel permeation chromatography using polystyrene standards with ASTM D6579-11 ("Standard Practice for Molecular Weight Averages and Molecular Weight Distribution of Hydrocarbon, Rosin and Terpene Resins by Size Exclusion Chromatography"; UV detector; 254 nm; solvent: destabilized THF; retention time marker: toluene; sample concentration: 2 mg / ml. w As used herein, "number average molecular weight" or "(M nThe term "number average molecular weight (M)" refers to the number average molecular weight (M) determined by gel permeation chromatography using polystyrene standards with ASTM D6579-11 ("Standard Practice for Molecular Weight Averages and Molecular Weight Distribution of Hydrocarbon, Rosin and Terpene Resins by Size Exclusion Chromatography"; UV detector; 254 nm; solvent: destabilized THF; retention time marker: toluene; sample concentration: 2 mg / ml. n )
[0090] The term "glass transition temperature" as used herein is a theoretical value and is defined in TG Fox, Bull. Am. Phys. Soc. (Ser. II) 1, 123 (1956) and J. Brandrup, EH Immergut, Polymer Handbook 3 rd The glass transition temperature is calculated by the Fox method based on the monomer composition and monomer charge according to the John Wiley, New York, 1989 edition.
[0091] As used herein, unless otherwise defined, the term substantially free means that a component is present, if at all, in an amount less than 5% by weight, based on the total weight of the slurry composition.
[0092] As used herein, unless otherwise defined, the term essentially free means that a component is present, if at all, in an amount of less than 1 wt. %, based on the total weight of the slurry composition.
[0093] As used herein, unless otherwise defined, the term completely free means that the component is not present in the slurry composition, i.e., 0.00 wt.% based on the total weight of the slurry composition.
[0094] As used herein, the term "total solids" refers to the non-volatile components of the slurry compositions of the present disclosure, and specifically excludes the aqueous medium.
[0095] As used herein, the term "consisting essentially of" includes recited materials or steps, as well as those that do not materially affect the basic and novel characteristics of the claimed disclosure.
[0096] As used herein, the term "consisting of" excludes any element, step, or ingredient not listed.
[0097] For the purposes of detailed description, it should be understood that the present disclosure may assume various alternative variations and step sequences unless expressly specified to the contrary. Moreover, other than in any operating example or unless otherwise indicated, all numbers, such as those expressing values, amounts, percentages, ranges, subranges, and fractions, can be read as if preceded by the word "about", even if the term does not explicitly appear. Thus, unless otherwise indicated to the contrary, the numerical parameters set forth in the following specification and appended claims are approximations that may vary depending on the desired properties obtained by the present disclosure. At the very least, and without any attempt to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should be construed at least in light of the number of reported significant digits and by applying ordinary rounding techniques. When closed or open-ended numerical ranges are set forth herein, all numbers, values, amounts, percentages, subranges, and fractions within or encompassed by the numerical ranges are deemed to be specifically included in and belong to the original disclosure of this application, as if those numbers, values, amounts, percentages, subranges, and fractions were expressly written out in their entireties.
[0098] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the disclosure are approximations, the numerical values set forth in the specific examples are reported as precisely as possible, however, any numerical values inherently contain certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0099] As used herein, unless otherwise indicated, plural terms can include their singular counterparts, and vice versa. For example, although reference is made herein to "a" negative electrode active material, "a" dispersant copolymer, and "an" conductive additive, combinations (i.e., multiples) of these components can be used. In addition, unless otherwise specifically stated herein, the use of "or" means "and / or," although in certain cases "and / or" can be explicitly used.
[0100] As used herein, "including," "containing," and similar terms are understood to be synonymous with "comprising" in the context of this application and are therefore open ended and do not exclude the presence of additional undescribed or unexplained elements, materials, components, or method steps. As used herein, in the context of this application, "consisting of" is understood to exclude the presence of any unspecified elements, components, or method steps. As used herein, in the context of this application, "consisting essentially of" is understood to include specified elements, materials, components, or method steps, and those that do not "materially affect the basic and novel characteristics" of what is being described. Although various embodiments of the present disclosure are described in terms of "comprising," embodiments that consist essentially of or consist of are also within the scope of the present disclosure.
[0101] As used herein, the terms "on," "onto," "applied on," "applied onto," "formed on," "deposited on," and "deposited onto" mean formed, superimposed, deposited, or provided on a surface, but not necessarily in contact with the surface. For example, a composition "deposited onto" a substrate does not exclude the presence of one or more other intervening coating layers of the same or different composition located between the electrodepositable coating composition and the substrate.
[0102] Although specific embodiments of the present disclosure have been described in detail, it will be understood by those skilled in the art that various modifications and alternatives to those details may be developed in light of the overall teachings of the present disclosure.The specific configurations disclosed are therefore intended to be illustrative only and not limiting on the scope of the present disclosure, which is given the full scope of the appended claims and any and all equivalents thereof.Each of the features and examples described herein, and combinations thereof, is said to be encompassed by the present disclosure.
[0103] The following examples illustrate the present disclosure but are not to be construed as limiting the disclosure to the details thereof. Unless otherwise indicated, all parts and percentages in the following examples, as well as throughout the specification, are by weight. EXAMPLES
[0104] EX-A: Preparation of Dispersant Copolymers Preparation of Comparative Dispersant A: 114 grams of Dowanol PM was added to a four-neck round bottom flask equipped with a mechanical stirring blade, thermocouple, and reflux condenser. Under a nitrogen atmosphere, the solvent was heated to a set point of 125° C. A monomer solution containing 228.8 grams of ethyl acrylate and 25.42 grams of acrylic acid was mixed thoroughly in a separate vessel. An initiator solution of 2.47 grams of tert-amyl peroctoate and 44.5 grams of Dowanol PM was prepared in a separate vessel. The initiator and monomer solutions were simultaneously co-charged into the flask using an addition funnel over a period of 210 and 180 minutes, respectively. After the initiator and monomer feeds were completed, the monomer addition funnel was rinsed with 12.2 grams of Dowanol PM. The resulting dispersant mixture was held at a set point of 125° C. for 1 hour. A second initiator solution of 1.52 grams of tert-amyl peroctoate and 13.3 grams of Dowanol PM was prepared. Half of the second initiator solution was fed into the flask using an addition funnel over 30 minutes. The dispersant mixture was held at a set point of 125°C for 30 minutes. The remainder of the initiator solution was added over 30 minutes. The initiator addition funnel was then rinsed with 6.08 grams of Dowanol PM. The dispersant mixture was then held at a set point of 125°C for 30 minutes. After the 30 minute hold, the mixture was cooled to 70°C. After cooling to 70°C, 31.43 grams of dimethylethanolamine were added over 10 minutes. After addition, the mixture was held at 70°C for 10 minutes. Then, 258 grams of warm (70°C) deionized water was added over 60 minutes, followed by mixing for 15 minutes. After mixing, the resin dispersion was poured into a suitable container. The total solids of the dispersant copolymer solution was determined to be 36.05% solids.
[0105] Preparation of Dispersant B: 114 grams of Dowanol PM was added to a four-neck round bottom flask equipped with a mechanical stirring blade, thermocouple, and reflux condenser. Under a nitrogen atmosphere, the solvent was heated to a set point of 125° C. A monomer solution containing 204.6 grams of ethyl acrylate, 24.2 grams of N-vinylpyrrolidone, and 25.42 grams of acrylic acid was mixed thoroughly in a separate vessel. An initiator solution of 2.47 grams of tert-amyl peroctoate and 44.5 grams of Dowanol PM was prepared in a separate vessel. The initiator and monomer solutions were simultaneously co-charged into the flask using an addition funnel over 210 and 180 minutes, respectively. After the initiator and monomer feeds were completed, the monomer addition funnel was rinsed with 12.2 grams of Dowanol PM. The resulting dispersant mixture was held at a set point of 125° C. for 1 hour. A second initiator solution of 1.52 grams of tert-amyl peroctoate and 13.3 grams of Dowanol PM was prepared. Half of the second initiator solution was fed into the flask using an addition funnel over 30 minutes. The dispersant mixture was held at a set point of 125°C for 30 minutes. The remainder of the initiator solution was added over 30 minutes. The initiator addition funnel was then rinsed with 6.08 grams of Dowanol PM. The dispersant mixture was then held at a set point of 125°C for 30 minutes. After the 30 minute hold, the mixture was cooled to 70°C. After cooling to 70°C, 31.43 grams of dimethylethanolamine were added over 10 minutes. After addition, the mixture was held at 70°C for 10 minutes. Then, 258 grams of warm (70°C) deionized water was added over 60 minutes, followed by mixing for 15 minutes. After mixing, the resin dispersion was poured into a suitable container. The total solids of the dispersant copolymer solution was determined to be 36.00% solids.
[0106] Preparation of Dispersant C: 108 grams of Dowanol PM was added to a four-neck round bottom flask equipped with a mechanical stirring blade, thermocouple, and reflux condenser. Under a nitrogen atmosphere, the solvent was heated to a set point of 125° C. A monomer solution containing 193.9 grams of butyl acrylate, 22.9 grams of N-vinylpyrrolidone, and 24.1 grams of acrylic acid was mixed thoroughly in a separate vessel. An initiator solution of 2.34 grams of tert-amyl peroctoate and 42.1 grams of Dowanol PM was prepared in a separate vessel. The initiator and monomer solutions were simultaneously co-charged into the flask using an addition funnel over 210 and 180 minutes, respectively. After the initiator and monomer feeds were completed, the monomer addition funnel was rinsed with 11.5 grams of Dowanol PM. The resulting dispersant mixture was held at a set point of 125° C. for 1 hour. A second initiator solution of 1.44 grams of tert-amyl peroctoate and 12.6 grams of Dowanol PM was prepared. Half of the second initiator solution was fed into the flask using an addition funnel over 30 minutes. The dispersant mixture was held at a set point of 125°C for 30 minutes. The remainder of the initiator solution was added over 30 minutes. The initiator addition funnel was then rinsed with 5.76 grams of Dowanol PM. The dispersant mixture was then held at a set point of 125°C for 30 minutes. After the 30 minute hold, the mixture was cooled to 70°C. After cooling to 70°C, 29.8 grams of dimethylethanolamine were added over 10 minutes. After addition, the mixture was held at 70°C for 10 minutes. Then, 244.4 grams of warm (70°C) deionized water was added over 60 minutes, followed by mixing for 15 minutes. After mixing, the resin dispersion was poured into a suitable container. The total solids of the dispersant copolymer solution was determined to be 35.60% solids.
[0107] Preparation of Dispersant D: 108 grams of Dowanol PM was added to a four-neck round bottom flask equipped with a mechanical stirring blade, thermocouple, and reflux condenser. Under a nitrogen atmosphere, the solvent was heated to a set point of 125° C. A monomer solution containing 193.9 grams of 2-ethylhexyl acrylate, 22.9 grams of N-vinylpyrrolidone, and 24.1 grams of acrylic acid was mixed thoroughly in a separate vessel. An initiator solution of 2.34 grams of tert-amyl peroctoate and 42.1 grams of Dowanol PM was prepared in a separate vessel. The initiator and monomer solutions were simultaneously co-charged into the flask using an addition funnel over 210 and 180 minutes, respectively. After the initiator and monomer feeds were completed, the monomer addition funnel was rinsed with 11.5 grams of Dowanol PM. The resulting dispersant mixture was held at a set point of 125° C. for 1 hour. A second initiator solution of 1.44 grams of tert-amyl peroctoate and 12.6 grams of Dowanol PM was prepared. Half of the second initiator solution was fed into the flask using an addition funnel over 30 minutes. The dispersant mixture was held at a set point of 125°C for 30 minutes. The remainder of the initiator solution was added over 30 minutes. The initiator addition funnel was then rinsed with 5.76 grams of Dowanol PM. The dispersant mixture was then held at a set point of 125°C for 30 minutes. After the 30 minute hold, the mixture was cooled to 70°C. After cooling to 70°C, 29.8 grams of dimethylethanolamine were added over 10 minutes. After addition, the mixture was held at 70°C for 10 minutes. Then, 244.4 grams of warm (70°C) deionized water was added over 60 minutes, followed by mixing for 15 minutes. After mixing, the resin dispersion was poured into a suitable container. The total solids of the dispersant copolymer solution was determined to be 35.4% solids.
[0108] Preparation of Dispersant E: 114 grams of Dowanol PM was added to a four-neck round bottom flask equipped with a mechanical stirring blade, thermocouple, and reflux condenser. Under a nitrogen atmosphere, the solvent was heated to a set point of 125° C. A monomer solution containing 204.6 grams of ethyl acrylate, 24.2 grams of N-vinylpyrrolidone, and 25.42 grams of poly(ethylene glycol) methyl ether methacrylate (Mn500) was mixed thoroughly in a separate vessel. An initiator solution of 2.47 grams of tert-amyl peroctoate and 44.5 grams of Dowanol PM was prepared in a separate vessel. The initiator and monomer solutions were simultaneously co-charged into the flask using an addition funnel over a period of 210 and 180 minutes, respectively. After the initiator and monomer feeds were completed, the monomer addition funnel was rinsed with 12.2 grams of Dowanol PM. The resulting dispersant mixture was held at a set point of 125° C. for 1 hour. A second initiator solution of 1.52 grams of tert-amyl peroctoate and 13.3 grams of Dowanol PM was prepared. Half of the second initiator solution was fed into the flask using an addition funnel over 30 minutes. The dispersant mixture was held at a set point of 125°C for 30 minutes. The remainder of the initiator solution was added over 30 minutes. The initiator addition funnel was then rinsed with 6.08 grams of Dowanol PM. The dispersant mixture was then held at a set point of 125°C for 30 minutes. After the 30 minute hold, the mixture was cooled to 70°C. The dispersant was poured into a suitable container. The total solids of the dispersant copolymer solution was measured to be 36.1% solids.
[0109] Preparation of carbon dispersion Comparative Example 1: CMC Control - No Dispersant Copolymer: To a plastic cup was added 14.8 g carboxymethylcellulose ("CMC", Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 8.0 g deionized water, and 0.5 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was hand mixed for 60 seconds and then mixed in a centrifugal mixer at 2000 rpm for a total of 2 minutes at 30 second intervals, periodically checking the quality of the carbon dispersion via drawdown.
[0110] Comparative Example 2: Dispersant A: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 7.5 g deionized water, 0.22 g Dispersant A (36.05% solids), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was hand mixed for 60 seconds and then mixed in a centrifugal mixer at 2000 rpm for a total of 2 minutes at 30 second intervals, periodically checking the quality of the carbon dispersion via drawdown.
[0111] Example 3: Dispersant B: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 9.5 g deionized water, 0.22 g Dispersant B (36% solids), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was hand mixed for 60 seconds and then mixed in a centrifugal mixer at 2000 rpm for a total of 2 minutes at 30 second intervals, periodically checking the quality of the carbon dispersion via drawdown.
[0112] Example 4: Dispersion C: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 11.0 g deionized water, 0.22 g Dispersion C (35.6% solids), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was hand mixed for 60 seconds and then mixed in a centrifugal mixer at 2000 rpm for a total of 2 minutes at 30 second intervals, periodically checking the quality of the carbon dispersion via drawdown.
[0113] Example 5: Dispersant D: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 12.0 g deionized water, 0.22 g Dispersant D (35.4% solids), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was hand mixed for 60 seconds and then mixed in a centrifugal mixer at 2000 rpm for a total of 2 minutes at 30 second intervals, periodically checking the quality of the carbon dispersion via drawdown.
[0114] Example 6: Dispersant E with 10% MPEG, 80.5% EA, and 9.5% NVP: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 13.0 g deionized water, 0.22 g Dispersant E (36.1% solids), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was hand mixed for 60 seconds and then mixed in a centrifugal mixer at 2000 rpm for a total of 2 minutes at 30 second intervals, periodically checking the quality of the carbon dispersion via drawdown.
[0115] Comparative Example 7: 0.3% PVP: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 14.0 g deionized water, 0.08 g PVP (Sigma Aldrich), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was hand mixed for 60 seconds and then mixed in a centrifugal mixer at 2000 rpm for a total of 2 minutes at 30 second intervals, periodically checking the quality of the carbon dispersion via drawdown.
[0116] Carbon Dispersion Evaluation: The final dispersions were applied via drawdown and visually evaluated. As shown in Figure 1, Dispersants B and C provided carbon dispersions that were at least equivalent to Comparative Dispersant A and PVP, and better than the Comparative Example 1 control, which lacked dispersant. The longer alkyl chain in Dispersant D from the use of EHA appears to have slightly degraded dispersion quality. In addition, the lack of acrylic acid and the inclusion of MPEG in Dispersant E significantly reduced dispersion quality.
[0117] Preparation of aqueous negative electrode slurry Comparative Example 1: CMC / SBR Control: In a plastic cup, 14.8 g of CMC (Sigma Aldrich, DS=1.2, M w =250,000, 2.66% solids), 8.0 g deionized water, and 0.5 g carbon (TIMCAL C-NERGY™ SUPER C45) were added. The mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Then, 25 g graphite (Superior 1506T) was added and the mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Finally, 0.9 g SBR (40% solids, Zeon BM-451B) was added and the mixture was hand stirred for 60 seconds before being coated using a 4 mil drawdown bar to give a copper foil with a density of 4.67 mg cm -2 A coating weight of 100 g was obtained.
[0118] Comparative Example 2: Comparative Dispersant A: In a plastic cup, 13.36 g of CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 7.5 g of deionized water, 0.22 g of Comparative Dispersant A (36.05% solids), and 0.53 g of carbon (TIMCAL C-NERGY™ SUPER C45) were added. The mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Then, 25 g of graphite (Superior 1506T) was added, and the mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Finally, 0.9 g of styrene butadiene rubber ("SBR", (40% solids, Zeon BM-451B) was added and the mixture was hand stirred for 60 s and then coated using a 5 mil drawdown bar to yield 4.71 mg cm on the copper foil. -2 A coating weight of 100 g was obtained.
[0119] Example 3: Dispersant B: To a plastic cup, 13.36 g of CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 9.5 g of deionized water, 0.22 g of Dispersant B (36% solids), and 0.53 g of carbon (TIMCAL C-NERGY™ SUPER C45) were added. The mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Then, 25 g of graphite (Superior 1506T) was added and the mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Finally, 0.9 g of SBR (40% solids, Zeon BM-451B) was added and the mixture was hand stirred for 60 seconds before being coated using a 5 mil drawdown bar to give a coating density of 4.71 mg cm on copper foil. -2 A coating weight of 100 g was obtained.
[0120] Example 4: Dispersant C: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 11.0 g deionized water, 0.22 g Dispersant C (35.6% solids), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Then, 25 g graphite (Superior 1506T) was added and the mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Finally, 0.9 g SBR (40% solids, Zeon BM-451B) was added and the mixture was hand stirred for 60 seconds before being coated using a 5 mil drawdown bar to give a coating density of 4.77 mg cm on copper foil. -2 A coating weight of 100 g was obtained.
[0121] Example 5: Dispersant D: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 12.0 g deionized water, 0.22 g Dispersant D (35.4% solids), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Then, 25 g graphite (Superior 1506T) was added and the mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Finally, 0.9 g SBR (40% solids, Zeon BM-451B) was added and the mixture was hand stirred for 60 seconds before being coated using a 5 mil drawdown bar to give a coating density of 4.71 mg cm on copper foil. -2 A coating weight of 100 g was obtained.
[0122] Example 6: Dispersant E: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 13.0 g deionized water, 0.22 g Dispersant E (36.1% solids), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Then, 25 g graphite (Superior 1506T) was added and the mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Finally, 0.9 g SBR (40% solids, Zeon BM-451B) was added and the mixture was hand stirred for 60 seconds before being coated using a 5 mil drawdown bar to give a 4.8 mg cm2 SBR coating on copper foil. -2 A coating weight of 100 g was obtained.
[0123] Comparative Example 7: 0.3% PVP: To a plastic cup was added 13.36 g CMC (Sigma Aldrich, DS=1.2, Mw=250,000, 2.66% solids), 14.0 g deionized water, 0.08 g polyvinylpyrrolidone ("PVP" (Sigma Aldrich), and 0.53 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Then, 25 g graphite (Superior 1506T) was added and the mixture was mixed in a centrifugal mixer at 2000 rpm for a total of 5 minutes with 30 second intervals. Finally, 0.9 g SBR (40% solids, Zeon BM-451B) was added and the mixture was hand stirred for 60 seconds before being coated using a 5 mil drawdown bar to produce a 4.61 mg cm2 SBR coating on copper foil. -2 A coating weight of 100 g was obtained.
[0124] Full Cell Coin Cell Evaluation Control 90 / 5 / 5 Positive electrode control: 90 wt% LiNi as the positive electrode active material 0.5 Mn 0.3 Co 0.2A positive electrode having O2, 5 wt. % SUPER P conductive carbon as a conductive additive, and 5 wt. % fluoropolymer-based binder was used as the electrode in the fabrication of all coin cells described below.
[0125] Coin Cells: Full coin cells were fabricated using a 90 / 5 / 5 cathode electrode control for the specified anode electrode. A ceramic-coated 20 μm thick Celgard separator was used as the separator and was immersed in 75 μL of electrolyte solution consisting of 1.2 M LiPF6 in 3:7 ratio of EC:EMC with 2 wt% VC. Coin cells were fabricated using 316 stainless steel casing, with a 1.0 cm diameter cathode electrode mated with a 1.2 cm diameter anode electrode. Cells were evaluated in a Bio-Logic BCS-805 tester using three formation cycles at 0.1 C followed by five cycles at each rate specified in Tables 1 and 2. [Table 1] [Table 2]
[0126] As shown in Table 1, each of Examples 3-6 provided comparable performance at each cycle compared to Comparative Example 1 and the controls Comparative Examples 2 and 7. Each of Examples 3-6 outperformed the Comparative Example 1 control at 12C.
[0127] As shown in Table 2, each of Examples 3-6 provided comparable performance at each cycle compared to Comparative Example 1 and the controls Comparative Examples 2 and 7. Each of Examples 3-6 outperformed the Comparative Example 1 control at 3C, 6C, and 12C.
[0128] EX-B: Preparation of carbon films Example B1: CMC / SBR: In a plastic cup, 15 g of CMC (Nipon, DS=0.7, Mw=350,000, 2% solids) and 0.4 g of carbon (TIMCAL C-NERGY™ SUPER C45) were added. The mixture was mixed in a centrifugal mixer with ZrO2 milling beads (Glen mills, ultra-high density zirconium oxide, 5 mm) at 2000 rpm for 3 minutes. 4.85 g of deionized water was added and mixed in the centrifugal mixer for 30 seconds. Finally, 0.75 g of SBR (40% solids, Zeon BM-451B) was added and the mixture was mixed in the centrifugal mixer for 30 seconds before being coated on a polytetrafluoroethylene film using a 10-mil drawdown bar. The film was dried sequentially in an electric oven at 55° C. for 2 minutes and at 100° C. for 4 minutes.
[0129] Example B2: CMC / SBR + 0.1 wt% Dispersant F: In a plastic cup, 14.5 CMC (Nipon, DS=0.7, Mw=350,000, 2% solids) and 0.4 g Dispersant F (available from Sigma Aldrich as poly(2-ethyl-2-oxazoline, 5 wt% solution in deionized water) with MW=50,000, PDI=3-4 were added. The mixture was mixed for 30 minutes in a centrifugal mixer at 2,000 rpm. 0.4 g carbon (TIMCAL C-NERGY™ SUPER C45) and ZrO2 milling beads (Glen mills, ultra-high density zirconium oxide, 5 mm) were added and mixed for 3 minutes at 2000 rpm. The carbon dispersion was diluted with 4.97 g deionized water and mixed for 30 seconds in a centrifugal mixer. Finally, 0.72 g SBR (40% solids, Zeon BM-451B) was added, the mixture was mixed in a centrifugal mixer for 30 seconds, and then coated onto a polytetrafluoroethylene film using a 10-mil drawdown bar. The film was dried sequentially in an electric oven at 55°C for 2 minutes and at 100°C for 4 minutes.
[0130] Transmission electron microscopy (TEM) evaluation of carbon microstructure: A small amount of each film sample was embedded in EMBed-812 epoxy and cured at 60°C for 24 hours. Thin sections (<80 nm) were then ultrafine cut and collected on Cu TEM grids. Images were acquired on a Tecnai T20 TEM while operating at 200 kV. The TEM image of the carbon film in Figure 2 shows clear areas containing nano-sized carbon particles (black spheres) interspersed in the polymer binder network (lighter, grey areas). In Example B1, there are areas where the nano-sized carbon network is disrupted, as highlighted by the circles in the left portion of the figure. When this analysis is repeated using the carbon film prepared in Example B2, there are significantly fewer discontinuities in the carbon particle network. Once again, a continuous carbon particle path from top to bottom can be easily traced in the TEM image of Example 2. A more continuous, fractal carbon network is expected to result in a more conductive coating with improved power performance, for example, in Example B2 compared to B1.
[0131] Multi-layer pouch cell rate capacity: Control 92 / 4.5 / 3.5 cathode: 92 wt% LiNi as the cathode active material 0.6 Mn 0.2 Co 0.2 A positive electrode having O2, 4.5 wt% SUPER P conductive carbon as a conductive additive, and 3.5 wt% fluoropolymer-based binder was used as the electrode in the fabrication of all pouch cells described below.
[0132] Example B3 94 / 2 / 4 Control Anode: To a 10L mixing pot was added 3.99 kg of CMC (Nipon, DS=0.7, Mw=350,000, 2% solids), and 106 g of carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was mixed for 1 hour with a dual helical mixer at 40 rpm and a high speed disperser blade at 1600 rpm. 5 kg of graphite (Superior 1506-T) was added along with 605 g of deionized water and mixed for 1 hour with a dual helical mixer at 40 rpm and a high speed disperser blade at 1600 rpm. An additional 605 g of water was then added and mixed for 2 hours with a dual helical mixer at 40 rpm and a high speed disperser blade at 1600 rpm. After mixing overnight in a dual helical mixer at 40 rpm, 332 g of SBR (40% solids, Zeon BM-451B) was added and the mixture was mixed for 5 minutes in a dual helical mixer at 40. The slurry was filtered through a 150 μm filter and coated on copper foil at 6.7 mg / cm using a reverse comma coater. 2 The coating was carried out at a loading of 1000g / g.
[0133] Example B4 94 / 2 / 4 Dispersant C Anode: To a 5L mixing pot was added 1.80 kg CMC (Nipon, DS=0.7, Mw=350,000, 2% solids) and 39.89 g Dispersant C (20% solids). The mixture was mixed for 5 minutes with a dual helical mixer at 40 rpm. 53.2 g carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was mixed for 1 hour with a dual helical mixer at 40 rpm and a high speed disperser blade at 1600 rpm. 2.5 kg graphite (Superior 1506-T) was added along with 387 g deionized water and mixed for 1 hour with a dual helical mixer at 40 rpm and a high speed disperser blade at 1600 rpm. An additional 387 g water was then added and mixed for 2 hours with a dual helical mixer at 40 rpm and a high speed disperser blade at 1600 rpm. After mixing overnight in a dual helical mixer at 40 rpm, 156 g of SBR (40% solids, Zeon BM-451B) was added and the mixture was mixed for 5 minutes in a dual helical mixer at 40. The slurry was filtered through a 150 μm filter and coated on copper foil at 6.7 mg / cm using a reverse comma coater. 2 The coating was carried out at a loading of 1000g / g.
[0134] Example B5 94 / 2 / 4 Dispersant F Anode: To a 5 L mixing pot was added 1.93 kg of CMC (Nipon, DS=0.7, Mw=350,000, 2% solids) and 53.2 g of Dispersant F (poly(2-ethyl-2-oxazoline, MW=50,000, PDI=3-4, 5 wt % solution in deionized water available from Sigma-Aldrich). The mixture was mixed for 5 minutes in a dual helical mixer at 40 rpm. 53.2 g of carbon (TIMCAL C-NERGY™ SUPER C45). The mixture was mixed for 1 hour in a dual helical mixer at 40 rpm and high speed dispersing blade at 1600 rpm. 2.5 kg of graphite (Superior) was added along with 160 g of deionized water. 1506-T) was added and mixed with the dual helical mixer at 40 rpm and the high speed disperser blade at 1600 rpm for 1 hour. An additional 160 g of water was then added and mixed with the dual helical mixer at 40 rpm and the high speed disperser blade at 1600 rpm for 2 hours. After mixing overnight with the dual helical mixer at 40 rpm, 163 g of SBR (40% solids, Zeon BM-451B) was added and the mixture was mixed with the dual helical mixer at 40 for 5 minutes. The slurry was filtered through a 150 μm filter and coated on copper foil at 6.7 mg / cm using a reverse comma coater. 2 The coating was carried out at a loading of 1000g / g.
[0135] Multi-layer pouch cells with a capacity of 1.1 Ah were fabricated using a 92 / 4.5 / 3.5 cathode electrode control for the specified anode electrode. A partially automated Z-folder stacker was used to assemble the cells with four cathodes and five anodes using an Entek 12 EPH separator soaked in 4.4 g of electrolyte solution consisting of 1 M LiPF6 in EC:EMC in a 3:7 ratio with 2 wt% VC. Cell evaluation was performed in a 10A Maccor tester using four formation cycles at 0.1C followed by five cycles at each rate specified in Table 3. [Table 3] [Table 4]
[0136] As shown in Table 3, Examples B4 and B5 each exhibited increased discharge capacity when discharged at a rate of 9C compared to the control formulation.
[0137] As shown in Table 4, Examples B4 and B5 exhibited higher normalized storage capacity when discharged at a rate of 9C compared to the control formulation.
[0138] Low temperature performance rating: Single layer pouch cells with a capacity of 30 mAh were prepared in a similar manner as described above for the multi-layer pouch cells, however, in this example, only one layer of the cathode and anode are used. The cells were filled with 0.6 g LiPF6 at 1 M in 2:2:6 EC:PC:EMC (volume %) with 2 wt % VC electrolyte. After four 0.1 C formation cycles at room temperature, the cells were placed in an Espec BTZ-475 thermal chamber at -18°C and equilibrated at this temperature for 6 hours. The cells were then charged at 0.1 C and discharged at -12 C. As shown in Figure 3, the cell containing Example B5 outperformed the control Example B3 by taking several seconds longer to reach the cutoff voltage of the experiment 2 V. The improved low temperature performance indicates the lower internal resistance of the Example B5 single layer pouch cell. The reduced internal resistance upon incorporation of Dispersant F correlates to the improvement of the conductive carbon dispersion.
[0139] EX-C: Preparation of aqueous negative electrode slurry Comparative Example C1-PVP: The slurry was mixed with 0.079 g of PVP as a dispersant, 13.356 g of CMC (Sigma Aldrich, DS=1.2, M wA slurry of 0.5 g of SBR (40% solids, Zeon BM-451B) was prepared in a manner similar to Comparative Example 1 of EX-A using 0.5 g of carbon (TIMCAL C-NERGY™ SUPER C45), 25.0 g of graphite (Superior 1506T), and 0.888 g of SBR (40% solids, Zeon BM-451B). The percent solids of the slurry was 53.9 wt.% based on the total composition. A graphite anode film was cast using a 4 mil drawdown bar to a thickness of 4.5 mg cm on copper foil. -2 A coating weight of 100 g was obtained.
[0140] Comparative Example C2 - Dispersant G: This slurry was mixed with 0.039 g PVP, 0.039 g poly(2-ethyl-2-oxazoline) (commercially available from Sigma-Aldrich as a powder with MW=50,000, PDI=3-4), 13.356 g CMC (Sigma Aldrich, DS=1.2, M w A slurry was prepared in a manner similar to Comparative Example 1 for EX-A using 0.01 g of ... -2 A coating weight of 100 g was obtained.
[0141] Example C3 - Dispersant H: This slurry was mixed with 0.175 Dispersant C (22.55% solids based on total weight), 0.039 g poly(2-ethyl-2-oxazoline) (commercially available from Sigma-Aldrich as a powder having MW=50,000, PDI=3-4), 13.356 g CMC (Sigma Aldrich, DS=1.2, M wA dispersant was prepared in a manner similar to Comparative Example 1 for EX-A using 0.01 g of 10000 sulphate (TIMCAL C-NERGY™ SUPER C45), ... -2 A coating weight of 100 g was obtained.
[0142] Full Cell Coin Cell Evaluation Control 92 / 4 / 4 Positive electrode control: 92 wt% LiNi as the positive electrode active material 0.5 Mn 0.3 Co 0.2 A positive electrode having O2, 4 wt. % SUPER P conductive carbon as a conductive additive, and 4 wt. % fluoropolymer-based binder was used as the electrode in the fabrication of all coin cells described below.
[0143] Coin Cells: Full coin cells were fabricated using a 92 / 4 / 4 cathode electrode control for the specified anode electrode. A ceramic-coated 20 μm thick Celgard separator was used as the separator and was immersed in 75 μL of electrolyte solution consisting of 1.2 M LiPF6 in 3:7 ratio of EC:EMC with 2 wt% VC. Coin cells were fabricated using 316 stainless steel casing, with a 1.0 cm diameter cathode electrode mated with a 1.2 cm diameter anode electrode. The cells were evaluated in a Bio-Logic BCS-805 tester using three formation cycles at 0.1 C followed by five cycles at each rate specified in Tables 5 and 6. [Table 5] [Table 6]
[0144] As shown in Tables 5 and 6, the use of Dispersant H (C3) provided equal or better absolute capacity and the best storage capacity at high C-rates (6C and 12C) compared to PVP (C1) or Dispersant G (C2). Unexpectedly, in combination with poly(2-alkyl-2-oxazoline) or poly(2-aryl-2-oxazoline) dispersants, a degradation of electrochemical performance was observed when high levels (greater than 50%) of nitrogen-containing heterocyclic monomers were present in the dispersant.
[0145] It will be appreciated by those skilled in the art that numerous modifications and variations are possible in light of the above disclosure without departing from the broad inventive concept described and illustrated herein. It is therefore to be understood that the foregoing disclosure is merely illustrative of various exemplary aspects of the present application, and that numerous modifications and variations within the spirit and scope of the present application and the appended claims may be readily made by those skilled in the art.
Claims
1. A negative electrode aqueous slurry composition, A binder; a dispersant comprising a copolymer comprising (a) constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, and (b) constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of alpha, beta-ethylenically unsaturated carboxylic acid functional monomers, the dispersant comprising 1 wt % to 50 wt % constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, the wt % being based on the total weight of the dispersant; A negative electrode active material; and an aqueous medium.
2. The negative electrode aqueous slurry composition according to claim 1 , wherein the monomer containing a nitrogen-containing heterocycle comprises vinylpyrrolidone.
3. 2. The anode aqueous slurry composition according to any one of the preceding claims, wherein the dispersant comprises 1 wt% to 99 wt% of constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of the alpha, beta-ethylenically unsaturated carboxylic acid functional monomers.
4. 2. The anode aqueous slurry composition of any one of the preceding claims, wherein the dispersant further comprises an ethylenically unsaturated monomer containing a hydroxyl functionality.
5. 2. The negative electrode aqueous slurry composition of any one of the preceding claims, wherein the dispersant has a glass transition temperature of -70 to +100°C.
6. The negative electrode aqueous slurry composition according to any one of the preceding claims, wherein the dispersant has a weight average molecular weight of 2,000 to 1,000,000 g / mol.
7. 20. The negative electrode aqueous slurry composition of any one of the preceding claims, further comprising a poly(2-alkyl or aryl oxazoline) polymer.
8. A negative electrode aqueous slurry composition, A binder; a poly(2-alkyl or aryl oxazoline) polymer; A negative electrode active material; and an aqueous medium.
9. 2. The negative electrode aqueous slurry composition of any one of the preceding claims, wherein the binder comprises a styrene-butadiene copolymer.
10. The negative electrode aqueous slurry composition of claim 9 , wherein the binder further comprises cellulose or a cellulose derivative.
11. 2. The negative electrode aqueous slurry composition of any one of the preceding claims, wherein the negative electrode active material comprises graphite, silicon, silicon oxide, tin, germanium, silver, aluminum, barium, bismuth, copper, gallium, indium, nickel, phosphorus, lead, antimony, silicon, tin, strontium, zinc, titanium, or a combination thereof.
12. 2. The negative electrode aqueous slurry composition of any one of the preceding claims, further comprising a conductive additive comprising conductive carbon, carbon nanotubes, graphene, or any combination thereof.
13. The negative electrode aqueous slurry composition of any one of the preceding claims, further comprising a cross-linking agent.
14. Based on the total solids weight of the composition, 1% to 10% by weight of said binder; optionally, 0.1 wt. % to 1 wt. % of said dispersant, said dispersant comprising a copolymer comprising (a) constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, and (b) constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of alpha, beta-ethylenically unsaturated carboxylic acid functional monomers, said wt. % to 50 wt. % of constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, said wt. % being based on the total weight of the dispersant; Optionally, 0.005% to 1.5% by weight of said poly(2-alkyl or aryl oxazoline) polymer, wherein at least one of said dispersant and said poly(2-alkyl or aryl oxazoline) polymer is present; 90% to 98.9% by weight of said negative electrode active material.
15. Based on the total weight of the composition, 0.5% to 5% by weight of said binder; optionally, 0.01 wt. % to 0.5 wt. % of said dispersant, said dispersant comprising a copolymer comprising (a) constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, and (b) constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of alpha, beta-ethylenically unsaturated carboxylic acid functional monomers, said weight % being based on the total weight of the dispersant; Optionally, 0.005% to 1.5% by weight of said poly(2-alkyl or aryl oxazoline) polymer, wherein at least one of said dispersant and said poly(2-alkyl or aryl oxazoline) polymer is present; 45% by weight to 48.9% by weight of the negative electrode active material; 45% to 50% by weight of said aqueous medium.
16. Based on the total binder solids weight of the composition, 75% to 99.9% by weight of said binder; optionally, 0.1% to 25% by weight of said dispersant, said dispersant comprising a copolymer comprising (a) constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, and (b) constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of alpha, beta-ethylenically unsaturated carboxylic acid functional monomers, said constitutional units comprising 1% to 50% by weight of constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, said weight percentages being based on the total weight of the dispersant; 13. The anode aqueous slurry composition of any one of the preceding claims comprising, optionally, 0.1 wt. % to 25 wt. % of said poly(2-alkyl or aryl oxazoline) polymer, and wherein at least one of said dispersant and said poly(2-alkyl or aryl oxazoline) polymer is present.
17. A negative electrode, (a) a current collector; (b) a film formed on the current collector, the film comprising: A binder; A negative electrode active material; below: A dispersant, the dispersant comprising a copolymer comprising (a) constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, and (b) constitutional units comprising residues of alkyl esters of (meth)acrylic acid and / or residues of acid-functional ethylenically unsaturated monomers, the dispersant comprising 1 wt % to 50 wt % constitutional units comprising residues of monomers comprising a nitrogen-containing heterocycle, the wt % being based on the total weight of the dispersant; or and a film comprising at least one of a poly(2-alkyl or aryl oxazoline) polymer.
18. The electrode of claim 17, wherein the film is deposited from the anode aqueous slurry composition of any one of claims 1 to 16.
19. 19. An electricity storage device comprising: (a) the negative electrode according to claim 17 or 18; (b) a positive electrode; and (c) an electrolyte.
20. The power storage device according to claim 19 , wherein the electrolyte (c) comprises a lithium salt dissolved in a solvent.
21. The power storage device according to claim 20 , wherein the lithium salt is dissolved in an organic carbonate.
22. The power storage device according to any one of claims 19 to 21, wherein the power storage device comprises a cell, a battery pack, a secondary battery, a capacitor, or a supercapacitor.
23. A negative electrode active material; a binder comprising cellulose or a cellulose derivative and a styrene-butadiene copolymer; A melamine crosslinker; and an aqueous medium.
24. The anode aqueous slurry composition of claim 23, further comprising a dispersant and / or a poly(2-alkyl or aryl oxazoline) polymer as defined in any one of claims 1 to 8.
25. The negative electrode aqueous slurry composition according to claim 23 or 24, wherein the negative electrode aqueous slurry composition is a composition defined in any one of claims 1 to 16.
Citation Information
Patent Citations
Secondary-battery binder composition, slurry composition for secondary-battery electrode, secondary-battery negative electrode, and secondary battery
WO2014188724A1
Electrodes having conformal coatings deposited onto porous electrical current collectors