Production of electrode active material, and electrode active material

A novel method for producing cathode active materials by mixing nickel-based (oxy)hydroxides with lithium and other compounds and heat treating them under controlled conditions addresses the limitations of NCM and NCA materials, resulting in improved lithium-ion battery performance.

JP2024537355APending Publication Date: 2024-10-10BASF SE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024522262
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-12
Filing Date
2022-10-05
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing lithiated nickel-cobalt-manganese oxides (NCM) and nickel-cobalt-aluminum oxides (NCA) materials in lithium-ion batteries suffer from short cycle life, significant gas generation, and increased internal resistance, limiting their practical use.

Method used

A method involving the use of a particulate (oxy)hydroxide of nickel and optionally cobalt or manganese, mixed with lithium, magnesium, or aluminum compounds, followed by heat treatment at specific temperatures and atmospheres, to produce a cathode active material with improved properties.

Benefits of technology

The method results in a cathode active material with enhanced discharge and cycling behavior, offering improved safety and performance in lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537355000001
    Figure 2024537355000001
  • Figure 2024537355000002
    Figure 2024537355000002
  • Figure 2024537355000003
    Figure 2024537355000003
Patent Text Reader

Abstract

1. A method for producing an electrode active material, the method comprising the steps of: (a) providing an (oxy)hydroxide of TM, wherein TM is a transition metal and comprises nickel and optionally at least one of cobalt and manganese, the nickel content being at least 80 mol % relative to TM; (b) mixing the (oxy)hydroxide of TM with a lithium source in an amount of 75-85 mol % relative to TM, and at least one compound of Mg or Al; (c) treating the resulting mixture at a temperature in the range of 400-700°C to obtain a powder; (d) mixing the powder from step (c) with a lithium source, at least one compound of Mg or Al, and at least one compound of Nb, Ta, W, Ti, or Zr; (e) heat treating the mixture obtained from step (d) at a temperature in the range of 550 to 800° C.; Includes.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an electrode active material, wherein the method comprises the following steps: (a) providing an (oxy)hydroxide of TM, wherein TM is a transition metal and comprises nickel and optionally at least one of cobalt and manganese, the nickel content being at least 80 mol % relative to TM; (b) mixing the (oxy)hydroxide of TM with a lithium source in an amount of 75-85 mol % relative to TM, and at least one compound of Mg or Al; (c) treating the resulting mixture at a temperature in the range of 400-700°C to obtain a powder; (d) The powder from step (c) is mixed with a lithium source and M 2 With at least one compound of M 2 is selected from Nb, Ta, W, Ti or Zr; (e) heat treating the mixture obtained from step (d) at a temperature in the range of 550 to 800° C.; Includes. [Background technology]

[0002] Lithiated transition metal oxides are currently used as electrode active materials in lithium-ion batteries. Extensive research and development has been carried out over the past few years to improve properties such as charge density, specific energy, and other properties such as cycle life degradation and capacity loss that adversely affect the life or applicability of lithium-ion batteries. Further efforts are being made to improve the manufacturing methods.

[0003] Many of the electrode active materials currently under discussion are of the lithiated nickel-cobalt-manganese oxide ("NCM material") or lithiated nickel-cobalt-aluminum oxide ("NCA material") type.

[0004] In a typical process for the preparation of cathode materials for lithium-ion batteries, a so-called precursor is first formed by co-precipitating a transition metal as a carbonate, oxide, or preferably as a hydroxide, which may or may not be basic. This precursor is then mixed with a lithium compound, e.g., LiOH, Li 2 O or especially Li 2 CO 3 (including but not limited to) and calcined at high temperature. The lithium salt(s) can be used as hydrate(s) or in dehydrated form. Calcination or calcination, also commonly referred to as thermal or heat treatment of the precursor, is usually carried out at temperatures ranging from 600 to 1000°C. During the heat treatment, a solid-state reaction takes place to form the electrode active material. If hydroxides or carbonates are used as precursors, the solid-state reaction takes place following removal of water or carbon dioxide. The heat treatment takes place in the heated zone of an oven or kiln.

[0005] To improve the capacity of the cathode active material, it has been proposed to increase the nickel content as much as possible. However, LiNiO 2 It has been confirmed that such materials have a short cycle life, significant gas generation, and a large increase in internal resistance during cycling, and there are significant challenges to be overcome before they can be put to practical use. Summary of the Invention [Problem to be solved by the invention]

[0006] It was therefore an object of the present invention to provide a cathode active material which overcomes the above-mentioned drawbacks, and to provide a method for producing such a cathode active material. [Means for solving the problem]

[0007] We have therefore found a method as defined at the outset, which hereinafter is also referred to as the method of the invention or the method according to the (present) invention, which comprises several steps, which hereinafter are also referred to as step (a), step (b) etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Steps (a) to (e) are described in detail below.

[0009] In step (a), a particulate (oxy)hydroxide of TM is provided, wherein TM is a transition metal and comprises nickel and optionally at least one of cobalt and manganese, the nickel content being at least 80 mol %, preferably at least 90 mol %, more preferably at least 98 mol %, relative to the TM.

[0010] In one embodiment of the invention, the (oxy)hydroxide of the TM is selected from nickel hydroxide, nickel(II) oxide and nickel oxyhydroxide (hereinafter also jointly referred to as nickel oxide / nickel hydroxide). In the context of the present invention, the term nickel oxyhydroxide is not limited to stoichiometric NiOOH, but also includes compounds of nickel having only oxide and hydroxide counterions and a maximum individual content of metal impurities such as Mn or Mg of 2% by weight, relative to the total metal content of said nickel hydroxide, nickel(II) oxide or nickel oxyhydroxide. Preferably, the nickel hydroxide, nickel(II) oxide or nickel oxyhydroxide has a maximum total impurity content of 2% by weight, relative to the total metal content of said nickel hydroxide, nickel(II) oxide or nickel oxyhydroxide.

[0011] The TM (oxy)hydroxides provided in step (a) have an average particle size (D50) in the range of 2 to 20 μm, preferably 4 to 16 μm. The average particle size can be determined for example by light scattering or laser diffraction or electroacoustic spectroscopy. The particles may be composed of agglomerates from primary particles, the particle size mentioned above referring to the particle size of the secondary particles.

[0012] The preferred nickel oxide / hydroxide is freshly precipitated nickel hydroxide.

[0013] In one embodiment of the invention, TM corresponds to the general formula (I): (Ni a Co b Mn c ) (I) (In the formula, a is in the range of 0.85 to 0.99, preferably 0.90 to 0.98, b is 0 or in the range of 0.01 to 0.14, preferably 0.01 to 0.05; c is 0 or in the range of 0.01 to 0.15, preferably 0.01 to 0.09; a+b+c=1).

[0014] In one embodiment of the present invention, the nickel oxide / hydroxide provided in step (a) has a residual water content in the range of 50-1000 ppm, preferably 100-400 ppm. The residual water content can be determined by Karl Fischer titration.

[0015] In step (b), the nickel oxide / hydroxide is mixed with 75-85 mol % of a lithium source and at least one compound of Al or Mg in the absence of a solvent, such as water or an organic solvent.

[0016] A suitable compound of Mg is Mg(OH). 2 , MgO, Mg(NO 3 ) 2 , and oxalates, e.g. MgC 2 O 4 It is.

[0017] Suitable compounds of Al include the nitrates, oxides, hydroxides and oxyhydroxides, such as Al 2 O 3 , Al(OH) 3 , AlOOH, Al 2 (SO 4 ) 3 , KAl(SO 4 ) 2 , and Al(NO 3 ) 3 , alkanolates of Al, e.g. Al(C 2 H 5 O) 3(including but not limited to), Al-trisisopropoxide, and mixed salts of at least two cations, such as aluminum magnesium isopropoxide.

[0018] Additionally, a lithium source is added.

[0019] Examples of lithium sources include Li, either as anhydrous or hydrated. 2 O, LiOH, and Li 2 CO 3 , if applicable, e.g. LiOH H 2 O is one example.

[0020] The amounts of lithium source and TM (oxy)hydroxide are selected such that the molar ratio of Li to TM is in the range of 3:4 to 85:100.

[0021] The amount of Al or Mg compound preferably corresponds to 0.1-2.0 mol %, preferably 1.0-1.5 mol %, relative to TM. In embodiments where both Mg and Al are added, the total amount of dopant corresponds to the sum of Mg and Al.

[0022] The lithium source is preferably in particulate form, for example having an average diameter (D50) in the range of 3 to 10 μm, preferably 5 to 9 μm.

[0023] In one embodiment of the present invention, step (b) is carried out at a temperature in the range of 5 to 85°C, preferably 10 to 60°C.

[0024] In one embodiment of the invention, step (b) is carried out at normal pressure, however, it is preferred to carry out step (b) at elevated pressure, for example at a pressure between 10 mbar and 10 bar above normal pressure, or under suction, for example at a pressure between 50 and 250 mbar below normal pressure, preferably at a pressure between 100 and 200 mbar below normal pressure.

[0025] For example, step (b) can be carried out in a vessel that can be easily drained, e.g., located above a filter device. Such vessel can be charged with nickel oxide / hydroxide from step (a), followed by the introduction of a lithium source and a compound of Mg or Al. In other embodiments, such vessel can be charged with a lithium source and a compound of Mg or Al, followed by the introduction of nickel oxide / hydroxide from step (a). In other embodiments, the nickel oxide / hydroxide from step (a), the compound of Mg or Al, and the lithium source are introduced simultaneously.

[0026] The mixing of the nickel oxide / nickel hydroxide with the Mg or Al compound and the lithium source is carried out for 1 minute to 3 hours, preferably 5 minutes to 1 hour, and even more preferably 5 minutes to 30 minutes.

[0027] Step (b) may be supported by a mixing operation, for example by shaking, or especially by stirring or shearing, see below.

[0028] Examples of suitable equipment for carrying out step (b) include high shear mixers, tumbler mixers, ploughshare mixers and free fall mixers.

[0029] In one embodiment of the present invention, step (b) is carried out at a temperature ranging from room temperature to 200°C, preferably from 20 to 50°C.

[0030] From step (b) a powdery mixture is obtained.

[0031] Step (c) comprises subjecting the mixture from step (b) to a heat treatment. An example of step (c) is a heat treatment at a temperature in the range of 400-700° C., preferably 500-600° C. The terms "thermal treatment" and "heat treatment" are used interchangeably in the context of the present invention.

[0032] In one embodiment of the present invention, step (b) is performed by heating to 400-700° C. at a heating rate of 0.1-10° C. / min.

[0033] In one embodiment of the present invention, the temperature is increased before reaching a desired temperature of 400 to 700° C., preferably 500 to 600° C. For example, the mixture obtained from step (c) is first heated to 350 to 400° C., then kept constant for 10 minutes to 2 hours, then heated to 500 to 700° C., and then kept at 500 to 700° C. for 10 minutes to 4 hours.

[0034] In one embodiment of the present invention, step (c) is carried out in a roller hearth kiln, a pusher kiln or a rotary kiln, or a combination of at least two of them. A rotary kiln has the advantage that the homogenization of the material produced therein is very good. In roller hearth kilns and pusher kilns, different reaction conditions for different steps can be set very easily. In laboratory scale experiments, box furnaces, tube furnaces and split tube furnaces can also be used.

[0035] In one embodiment of the present invention, step (c) is carried out in an oxygen-containing atmosphere, such as a nitrogen-air mixture, a noble gas-oxygen mixture, air, oxygen or oxygen-enriched air. In a preferred embodiment, the atmosphere in step (c) is selected from air, oxygen and oxygen-enriched air. The oxygen-enriched air can be, for example, a 50:50 volumetric ratio of air and oxygen. Other options include a 1:2 volumetric ratio of air and oxygen, a 1:3 volumetric ratio of air and oxygen, a 2:1 volumetric ratio of air and oxygen, and a 3:1 volumetric ratio of air and oxygen.

[0036] In one embodiment of the present invention, step (c) is carried out under a gas flow, such as air, oxygen and oxygen-enriched air. Such a gas flow is also called a forced gas flow. Such a gas flow has a flow rate of 0.5 to 15 m per kg of the mixture from step (b). 3 The gas flow can have a specific flow rate in the range of 1000 rpm / h. The volume is determined under normal conditions (298 Kelvin and 1 atm). The gas flow is useful for removing gaseous decomposition products such as water and carbon dioxide.

[0037] In one embodiment of the invention, step (c) has a duration ranging from 30 minutes to 24 hours, preferably from 1 hour to 10 hours. The time at temperatures above 400°C counts the heating and holding time, but the cooling time is ignored in this context.

[0038] From step (c) a powder is obtained, which may optionally be deagglomerated prior to step (d).

[0039] In step (d), the powder obtained from step (c) is treated with a lithium source and M 2 wherein M 2 is selected from Nb, Ta, W, Ti or Zr.

[0040] Suitable examples of lithium sources and Al and Mg compounds are disclosed above.

[0041] Suitable M 2 are oxides, (oxy)hydroxides and nitrates of Ti, Zr, W, Mo and Nb, e.g. TiO 2 , Ti 2 O 3 , TiO(OH) 2 , ZrO 2 , Zr(OH) 4 , TiO(NO 3 ) 2 , Ti(NO 3 ) 4 , Niobic acid, Nb 2 O 5 , Ta 2 O 5 , WO 3 , Li 2 WO 4 , Li 2 MoO 4 and MoO 3 It is. 1Further examples of compounds of the formula (I) are, by themselves or as hydrates, for example, but not limited to, ammonium metatungstate (hydrate), ammonium orthomolybdate, ammonium heptamolybdate, ammonium dimolybdate, ammonium niobate oxalate, ammonium zirconium(IV) carbonate.

[0042] In one embodiment of the present invention, the total molar amount of Al or Mg compound(s) relative to TM is in the range of 0.1-2 mol %, preferably 1-1.5 mol %.

[0043] In one embodiment of the present invention, M 2 The total molar amount of the compound(s) based on TM is in the range of 0.2 to 1 mol %, preferably 0.25 to 0.5 mol %.

[0044] In one embodiment of the present invention, the amount of lithium source used in steps (b) and (d) is adjusted to a ratio of (Li+Mg) to (TM+Al+M 2 The molar ratio of Li divided by Li is selected to be in the range of 0.99 to 1.05, preferably 1.0 to 1.03. The amount of Li means the amount from step (b) and step (d). The amount of Al or Mg may be zero.

[0045] Thus, the amount of lithium source in step (d) can range from about 15 to 30 mol % relative to TM.

[0046] As for the other devices and mixing parameters, the same devices and mixing parameters as those in step (b) can be applied.

[0047] From step (d) a mixture is obtained. In step (e), the mixture from step (b) is heat treated at a temperature in the range of 550-800° C., preferably 700-750° C. Preferably, the temperature in step (e) is higher than in step (c), e.g. at least 50° C. or at least 100° C.

[0048] In one embodiment of the present invention, the duration of step (e) ranges from 1 hour to 24 hours, preferably from 2 hours to 12 hours.

[0049] As for the apparatus and process parameters other than those mentioned above, the same apparatus and process parameters as those in step (c) can be applied.

[0050] This provides an optimal material for use as a cathode active material in lithium-ion batteries.

[0051] In one embodiment of the present invention, the material of the present invention can be treated with water followed by drying. In another embodiment of the present invention, the particles of the material of the present invention can be at least partially coated, for example, by mixing with an oxide or hydroxide, for example a compound of cobalt or alumina, or with boric acid, followed by heat treatment at 150-400° C. In another embodiment of the present invention, the particles of the material of the present invention can be at least partially coated, for example, by atomic layer deposition, for example, by alternating treatment with trimethylaluminum and water.

[0052] In one embodiment of the invention, the process comprises step (f) of adding a boron or cobalt compound to the material obtained from step (e) followed by heat treatment, for example for 1-5 hours (at 150-400°C in the case of post-treatment of a boron compound and 500-700°C in the case of post-treatment of a cobalt compound). A suitable compound of boron is LiBO 2 , B 2 O 3 and B(OH) 3 Suitable cobalt compounds are CoO, Co 2 O 3 , Co 3 O 4 , Co(NO 3 ) 2 , CoOOH, and Co(OH) 2 It is.

[0053] A further aspect of the present invention relates to a cathode active material, hereinafter also referred to as the cathode active material of the present invention or the electrode active material of the present invention. The cathode active material of the present invention has the general formula Li 1+x M 1 y1 (M 2 y2 TM) 1-x-y1 O 2 wherein TM is a transition metal and comprises nickel and, optionally, at least one of cobalt and manganese, the nickel content being at least 80 mol % relative to TM, x is in the range of 0 to 0.05, and M 1 is selected from Mg, Al, and combinations thereof; 2 is selected from Nb, Ta, W, Ti or Zr, and combinations of at least two thereof, y1 is in the range of 0.005 to 0.05, y2 is in the range of 0.0025 to 0.02, and said material has an average primary particle size in the range of 50 to 350 nm, and a span in the range of 0.5 to 1.1. The span is determined by evaluation of SEM images and refers to the primary particles. The cathode active material of the present invention is advantageously produced according to the method of the present invention.

[0054] In embodiments where a coating with a boric acid or cobalt compound has been applied, the above formula refers to the core of the cathode active material of the present invention.

[0055] In one embodiment of the present invention, the cathode active material of the present invention has an average particle size (D50) in the range of 2 to 20 μm, preferably 4 to 16 μm. The average particle size can be determined, for example, by light scattering or laser diffraction or electroacoustic spectroscopy. The particles are usually composed of aggregates from primary particles, and the particle size mentioned above refers to the particle size of the secondary particles.

[0056] A further aspect of the present invention is an electrode comprising at least one material according to the present invention. These are particularly useful in lithium-ion batteries. Lithium-ion batteries comprising at least one electrode according to the present invention show very good discharge and cycle behavior and good safety behavior.

[0057] In one embodiment of the present invention, the cathode of the present invention comprises (A) at least one material of the invention as described above, (B) carbon in a conductive state, and (C) binder, (D) Current collector Contains:

[0058] In a preferred embodiment of the present invention, the cathode of the present invention comprises, based on the sum of (A), (B) and (C), (A) 80 to 98% by mass of the material of the present invention; (B) 1 to 17 mass% carbon, (C) 1 to 10 mass % of a binder Contains:

[0059] The cathode according to the invention contains a conductive modified carbon, also called carbon (B) for short. Carbon (B) can be selected from soot, activated carbon, carbon nanotubes, graphene and graphite. Carbon (B) can be added directly during the preparation of the electrode material according to the invention.

[0060] The electrodes according to the invention may contain further components. They may contain a current collector (D), for example (but not limited to) an aluminum foil. They may further contain a binder material (C), also called binder (C) below. The current collector (D) will not be described further here.

[0061] Suitable binders (C) are preferably selected from organic (co)polymers. Suitable (co)polymers, i.e. homopolymers or copolymers, can be selected, for example, from (co)polymers obtainable by anionic, catalytic or free radical (co)polymerization, in particular from polyethylene, polyacrylonitrile, polybutadiene, polystyrene and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene. Polypropylene is also suitable. Polyisoprene and polyacrylates are furthermore suitable. Polyacrylonitrile is particularly preferred.

[0062] In the context of the present invention, polyacrylonitrile is understood to mean not only polyacrylonitrile homopolymers but also copolymers of acrylonitrile with 1,3-butadiene or with styrene. Polyacrylonitrile homopolymers are preferred.

[0063] In the context of the present invention, polyethylene refers not only to homopolyethylenes, but also to polyethylenes containing at least 50 mol % copolymerized ethylene and up to 50 mol % of at least one further comonomer, such as α-olefins, such as propylene, butylene (1-butene), 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-pentene, and also isobutene, vinyl aromatics, such as styrene, and also (meth)acrylic acid, vinyl acetate, vinyl propionate, C 10 copolymers of (meth)acrylic acid. 1 ~C 10 -alkyl esters, in particular methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and also copolymers of ethylene with maleic acid, maleic anhydride and itaconic anhydride. The polyethylene may be HDPE or LDPE.

[0064] In the context of the present invention, polypropylene is understood to mean not only homopolypropylene but also copolymers of propylene with at least 50 mol % copolymerized propylene and up to 50 mol % of at least one further comonomer, such as ethylene, and α-olefins, such as butylene, 1-hexene, 1-octene, 1-decene, 1-dodecene and 1-pentene. The polypropylene is preferably isotactic polypropylene or essentially isotactic polypropylene.

[0065] In the context of the present invention, polystyrene refers to homopolymers of styrene as well as acrylonitrile, 1,3-butadiene, (meth)acrylic acid, C 2 styrene, 1,3-butadiene, (meth)acrylic acid, 1 ~C 10 -alkyl esters, divinylbenzene, in particular 1,3-divinylbenzene, 1,2-diphenylethylene and α-methylstyrene copolymers are also understood to mean.

[0066] Another preferred binder (C) is polybutadiene.

[0067] Other suitable binders (C) are selected from polyethylene oxide (PEO), cellulose, carboxymethyl cellulose, polyimides and polyvinyl alcohol.

[0068] In one embodiment of the invention, the binder (C) has an average molecular weight M ranging from 50,000 g / mol to 1,000,000 g / mol, preferably up to 500,000 g / mol. W The (co)polymers are selected from those having the formula:

[0069] The binder (C) may be a crosslinked or non-crosslinked (co)polymer.

[0070] In a particularly preferred embodiment of the present invention, the binder (C) is selected from halogenated (co)polymers, in particular fluorinated (co)polymers.Halogenated or fluorinated (co)polymers are understood to mean (co)polymers that contain at least one (co)polymerized (co)monomer with at least one halogen atom or at least one fluorine atom per molecule, more preferably at least two halogen atoms or at least two fluorine atoms per molecule.Examples include polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), vinylidene fluoride-tetrafluoroethylene copolymer, perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, and ethylene-chlorofluoroethylene copolymer.

[0071] Suitable binders (C) are especially polyvinyl alcohol and halogenated (co)polymers such as polyvinyl chloride or polyvinylidene chloride, especially fluorinated (co)polymers such as polyvinyl fluoride and especially polyvinylidene fluoride and polytetrafluoroethylene.

[0072] The electrode of the present invention may contain 3 to 10 mass % of binder(s) (d) based on the total mass of the component (a), the component (b) and carbon (c).

[0073] A further aspect of the present invention is (1) at least one cathode comprising a cathode active material (A) of the present invention, carbon (B) and a binder (C); (2) at least one anode; and (3) at least one electrolyte It is a battery containing

[0074] The embodiment of the cathode (1) has already been described in detail above.

[0075] The anode (2) is made of at least one anode active material, such as carbon (graphite), TiO 2 , lithium titanium oxide, silicon or tin. The anode (2) may further contain a current collector, for example a metal foil such as copper foil.

[0076] The electrolyte (3) may include at least one non-aqueous solvent, at least one electrolyte salt, and optionally additives.

[0077] The non-aqueous solvent for the electrolyte (3) may be liquid or solid at room temperature and is preferably selected from polymers, cyclic or acyclic ethers, cyclic and acyclic acetals, and cyclic or acyclic organic carbonates.

[0078] Examples of suitable polymers are in particular polyalkylene glycols, preferably poly-C 1 ~C 4 -alkylene glycols, and in particular polyethylene glycols, where the polyethylene glycols are those containing up to 20 mol % of one or more C 1 ~C 4 The polyalkylene glycol may preferably be a polyalkylene glycol having two methyl or ethyl end caps.

[0079] The molecular weight M of suitable polyalkylene glycols, particularly suitable polyethylene glycols, W may be at least 400 g / mol.

[0080] The molecular weight M of suitable polyalkylene glycols, particularly suitable polyethylene glycols, W can be up to 5,000,000 g / mol, preferably up to 2,000,000 g / mol.

[0081] Examples of suitable acyclic ethers are, for example, diisopropyl ether, di-n-butyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, with 1,2-dimethoxyethane being preferred.

[0082] Examples of suitable cyclic ethers are tetrahydrofuran and 1,4-dioxane.

[0083] Examples of suitable acyclic acetals are, for example, dimethoxymethane, diethoxymethane, 1,1-dimethoxyethane and 1,1-diethoxyethane.

[0084] An example of a suitable cyclic acetal is 1,3-dioxane, and especially 1,3-dioxolane.

[0085] Examples of suitable acyclic organic carbonates are dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.

[0086] Examples of suitable cyclic organic carbonates are compounds of the general formulae (II) and (III) [ka] (In the formula, R 1 , R 2 and R 3 can be the same or different, hydrogen and C 1 ~C 4 -alkyl, for example selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, preferably R 2 and R 3 (Both cannot be tert-butyl).

[0087] In a particularly preferred embodiment, R 1 is methyl, R 2 and R 3 are each hydrogen or R 1 , R 2 and R 3 are hydrogen.

[0088] Another preferred cyclic organic carbonate is vinylene carbonate of formula (IV).

[0089] [ka]

[0090] Preferably, the solvent or solvents are used in an aqueous state, ie with a water content in the range of 1 ppm to 0.1% by weight, which can be determined, for example, by Karl Fischer titration.

[0091] The electrolyte (3) further comprises at least one electrolyte salt. Suitable electrolyte salts are in particular lithium salts. Examples of suitable lithium salts include LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 , LiCF 3 SO 3 , LiC(C n F 2n+1 SO 2 ) 3 , lithium imide, e.g. LiN(C n F 2n+1 SO 2 ) 2 (wherein n is an integer ranging from 1 to 20), LiN(SO 2 F) 2 , Li 2 SiF 6 , LiSbF 6 , LiAlCl 4 and the general formula (C n F 2n+1 SO 2 ) t It is the salt of YLi. where t=1 when Y is selected from oxygen and sulfur; when Y is selected from nitrogen and phosphorus, t=2; When Y is selected from carbon and silicon, t=3).

[0092] The preferred electrolyte salt is LiC(CF 3 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiPF 6 , LiBF 4 , LiClO 4 Selected from LiPF 6 and LiN(CF 3 SO 2 ) 2 is particularly preferred.

[0093] In a preferred embodiment of the present invention, the electrolyte (3) contains at least one flame retardant. Useful flame retardants may be selected from trialkyl phosphates (wherein the alkyls are different or the same), triaryl phosphates, alkyl dialkyl phosphonates, and halogenated trialkyl phosphates. Preferred are tri-C 1 ~C 4 -Alkyl phosphate (C 1 ~C 4 -alkyl are different or the same), tribenzyl phosphate, triphenyl phosphate, C 1 ~C 4 -Alkyldi-C 1 ~C 4 -Alkyl phosphonates, and fluorinated tri-C 1 ~C 4 - alkyl phosphates.

[0094] In a preferred embodiment, the electrolyte (3) is trimethyl phosphate, CH 3 -P(O)(OCH 3 ) 2 , triphenyl phosphate, and tris-(2,2,2-trifluoroethyl) phosphate.

[0095] The electrolyte (3) may contain 1 to 10 mass % of a flame retardant based on the total mass of the electrolyte.

[0096] In an embodiment of the invention, the battery according to the invention comprises one or more separators (4) by means of which the electrodes are mechanically separated. Suitable separators (4) are polymer films, in particular porous polymer films, which are unreactive towards metallic lithium. Particularly suitable materials for the separators (4) are polyolefins, in particular film-forming porous polyethylene and film-forming porous polypropylene.

[0097] The separator (4) made of polyolefin, particularly polyethylene or polypropylene, may have a porosity in the range of 35 to 45%. The suitable pore size is, for example, in the range of 30 to 500 nm.

[0098] In another embodiment of the present invention, the separator (4) can be selected from PET nonwoven fabrics filled with inorganic particles. Such separators can have a porosity in the range of 40-55%. Suitable pore sizes are, for example, in the range of 80-750 nm.

[0099] The battery according to the invention may further comprise a housing which may have any shape, for example a cube or a cylindrical disk. In one variant, a metal foil configured as a pouch is used as the housing.

[0100] The battery according to the invention exhibits very good discharge and cycling behaviour, especially with regard to capacity loss, especially at high temperatures (above 45° C., for example up to 60° C.).

[0101] The battery according to the present invention may comprise two or more electrochemical cells that are combined with each other, for example, connected in series or connected in parallel. A series connection is preferred. In the battery according to the present invention, at least one electrochemical cell contains at least one cathode according to the present invention. Preferably, in the electrochemical cell according to the present invention, the majority of the electrochemical cells contain the cathode according to the present invention. Even more preferably, in the battery according to the present invention, all the electrochemical cells contain the cathode according to the present invention.

[0102] The present invention further provides a method for using the battery according to the present invention in equipment, especially mobile equipment.Examples of mobile equipment are vehicles, such as automobiles, bicycles, aircraft, or water vehicles, such as boats or ships.Other examples of mobile equipment are manually operated, such as computers, especially laptops, phones, or powered hand tools, for example in the construction sector, especially drills, battery-powered drivers, or battery-powered staplers.

[0103] The present invention is further illustrated by the following examples. EXAMPLES

[0104] The average particle size (D50) was determined by dynamic light scattering ("DLS"). Percentages are by weight unless otherwise stated. "rpm": revolutions per minute.

[0105] LiOH H 2 O was purchased from Rockwood Lithium. Mg(OH) 2 from Sigma Aldrich, and Al 2 O 3 from Sasol, Zr(OH) 4 from Luxfer Mel Technologies, WO 3 From Avantama, TiO 2 was purchased from Hombikat.

[0106] A blender (Kinematica) was used as the mixer.

[0107] I. Basic cathode active material LiNiO 2 Manufacturing I.1 Precursor preparation Step (a.1): By combining an aqueous solution of nickel sulfate (a 1.65 mol / kg solution) with an aqueous solution of 25% by weight of NaOH and using ammonia as a complexing agent, spherical Ni(OH) 2 The precursor was obtained. The pH value was set to 12.6. The newly precipitated Ni(OH) 2The Ni(OH) was washed with water, sieved, and dried at 120 °C for 12 h. 2 ("p-CAM.1") had an average particle size D50 of 10 μm.

[0108] II. Preparation of the cathode active material of the present invention and comparative cathode active materials II.1 Manufacturing of C-CAM.1 Step (b.1): 50 g of p-CAM.1 is dissolved in 22.80 g of LiOH H 2 0, 0.32 g Mg(OH) 2 , 0.15g Al 2 O 3 , and 0.25 g of Zr(OH) 4 and mixed.

[0109] Step (c.1): The resulting mixture was poured into an alumina crucible and heated under oxygen atmosphere (10 exchanges / hour) at 600°C for 1 hour and then at 700°C for 6 hours, with a first heating rate of 10°C / min and a second heating rate of 3°C / min. The heat treatment was carried out in a laboratory furnace (Linn High Therm). C-CAM.1 was obtained. C-CAM.1 was cooled to 120°C at a cooling rate of 10°C / min and transferred to a drying room for further processing.

[0110] Neither step (d) nor (e) was performed.

[0111] The resulting C-CAM.1 was then sieved with a mesh size of 32 μm to obtain C-CAM.1 with 1.0 mol% Mg, 0.55 mol% Al, 0.24 mol% Zr, and a molar ratio (Li+Mg) / (Ni+Al+Zr)=1.01.

[0112] II.2 Manufacturing of CAM.2 Step (b.2): A 50 g quantity of P-CAM.1 is dissolved in 17.67 g of LiOH H 2 0, 0.25 g Mg(OH) 2 and 0.15 g Al 2 O 3 and mixed.

[0113] Step (c.2): The resulting mixture is poured into a metal valve that is part of a rotary kiln and heated at 10° C. / min under oxygen atmosphere (10 exchanges / hour). -1 The mixture was heated to 600° C. for 1 h at a heating rate of 1000 rpm. The rotation speed was 20 rpm. An intermediate was obtained. The intermediate was cooled to room temperature at a cooling rate of 10° C. / min and transferred to a drying chamber for further processing. The composition was 63% by weight Ni, 0.13% by weight Al, 0.19% by weight Mg and 5.8% by weight Li.

[0114] Step (d.2): Using a blender, mix 15 g of the intermediate from step (c.2) with 1.70 g of LiOH H 2 O and 0.07 g Zr(OH) 4 A mixture was obtained.

[0115] Step (e.2): The mixture from step (d.2) was poured into an alumina crucible and heated in a laboratory furnace under oxygen atmosphere (10 exchanges / hour) at a heating rate of 3°C / min to 700°C for 6 hours. The resulting CAM.2 was heated at 10°C / min. -1 The mixture was cooled to 120° C. at a cooling rate of 0.15 to 120° C. and transferred to a drying room for further processing.

[0116] CAM.2 was then sieved with a mesh size of 32 μm to obtain CAM.2 with 0.74 mol% Mg, 0.49 mol% Al, 0.25 mol% Zr, and a molar ratio (Li+Mg) / (Ni+Al+Zr) = 1.01. The span of the primary particles was in the range of 0.5–1.1 by evaluation of SEM images.

[0117] II.3 Manufacturing of CAM.3 Step (b.3): A 50 g quantity of P-CAM.1 is dissolved in 17.67 g of LiOH H 2 0, 0.25 g Mg(OH) 2 and 0.15 g Al 2 O 3 and mixed.

[0118] Step (c.3): The resulting mixture is poured into a metal valve that is part of a rotary kiln and heated at 10° C. / min under oxygen atmosphere (10 exchanges / hour). -1 The mixture was heated to 600° C. for 1 h at a heating rate of 1000 rpm. The rotation speed was 20 rpm. An intermediate was obtained. The intermediate was cooled to room temperature at a cooling rate of 10° C. / min and transferred to a drying chamber for further processing. The composition was 63% by weight Ni, 0.13% by weight Al, 0.19% by weight Mg and 5.8% by weight Li.

[0119] Step (d.3): Using a blender, mix 15 g of the intermediate from step (c.2) with 1.70 g of LiOH H 2 0 and 0.03 g TiO 2 A mixture was obtained.

[0120] Step (e.3): The mixture from step (d.3) was poured into an alumina crucible and heated in a laboratory furnace under oxygen atmosphere (10 exchanges / hour) at a heating rate of 3°C / min to 700°C for 6 hours. The resulting CAM.3 was heated at 10°C / min. -1 The mixture was cooled to 120° C. at a cooling rate of 0.15 to 120° C. and transferred to a drying room for further processing.

[0121] CAM.3 was then sieved with a mesh size of 32 μm to obtain CAM.3 with 0.74 mol% Mg, 0.49 mol% Al, 0.24 mol% Ti, and a molar ratio (Li+Mg) / (Ni+Al+Ti) = 1.03. The span of the primary particles was in the range of 0.5-1.1 by evaluation of SEM images.

[0122] II.4 Manufacturing of CAM.4 Step (b.4): A 50 g quantity of P-CAM.1 is dissolved in 17.67 g of LiOH H 2 0, 0.25 g Mg(OH) 2 and 0.15 g Al 2 O 3 and mixed.

[0123] Step (c.4): The resulting mixture is poured into a metal valve that is part of a rotary kiln and heated at 10° C. / min under oxygen atmosphere (10 exchanges / hour).-1 The mixture was heated to 600° C. for 1 h at a heating rate of 1000 rpm. The rotation speed was 20 rpm. An intermediate was obtained. The intermediate was cooled to room temperature at a cooling rate of 10° C. / min and transferred to a drying chamber for further processing. The composition was 63% by weight Ni, 0.13% by weight Al, 0.19% by weight Mg and 5.8% by weight Li.

[0124] Step (d.4): Using a blender, mix 15 g of the intermediate from step (c.4) with 1.70 g of LiOH H 2 0 and 0.09 g WO 3 A mixture was obtained.

[0125] Step (e.4): The mixture from step (d.4) was poured into an alumina crucible and heated in a laboratory furnace under oxygen atmosphere (10 exchanges / hour) at a heating rate of 3°C / min to 700°C for 6 hours. The resulting CAM.4 was heated at 10°C / min. -1 The mixture was cooled to 120° C. at a cooling rate of 0.15 to 120° C. and transferred to a drying room for further processing.

[0126] CAM.4 was then sieved with a mesh size of 32 μm to obtain CAM.4 with 0.74 mol% Mg, 0.47 mol% Al, 0.22 mol% W, and a molar ratio (Li+Mg) / (Ni+Al+W) = 1.03. The span of the primary particles was in the range of 0.5-1.1 by evaluation of SEM images.

[0127] III. Electrochemical Testing III.1 Cathode fabrication, general protocol: Electrode preparation: The electrodes contained 94% of the respective CAM or C-CAM.1, 3% carbon black (Super C65), and 3% binder (polyvinylidene fluoride, Solef 5130). A slurry with 61% total solids was mixed in N-methyl-2-pyrrolidone (planetary mixer, 24 min, 2,000 rpm) and cast on aluminum foil tape with a box coater. The electrode tape was dried in vacuum at 120 °C for 16 h and calendered, after which circular electrodes with a diameter of 14 mm were punched out, weighed, and dried under vacuum at 120 °C for 12 h and then placed in an Ar-filled glove box. Average loading: 8 mg / cm 2 , Electrode density: 3g / cm 3 .

[0128] III.2 Coin Cell Manufacturing A coin-type electrochemical cell was assembled in an argon-filled glove box. Anode: 0.58 mm thick Li foil separated from the cathode by a glass fiber separator (Whatman GF / D). 95 μl of 1 M LiPF in ethylene carbonate (EC):ethyl methyl carbonate (EMC) in a mass ratio of 3:7. 6 was used as the electrolyte. After assembly, the cell was crimped and closed using an automatic crimping machine. The cell was then transferred to a thermostatic chamber and connected to a battery cycler (Series 4000, MACCOR).

[0129] III.3 Coin Cell Testing All tests were performed at 25° C. The cells were cycled galvanostatically at room temperature between 3.0 and 4.3 V using a Maccor 4000 battery cycler, applying the following C-rates until the cells reached 70% of their initial discharge capacity at one discharge step:

[0130] The test protocol consisted of two cycles at C / 10, an initial formation portion, and a rate test portion. The voltage window was set to 3.0–4.3 V for all cycles. The initial 1C rate was 200 mA g -1was assumed. For all subsequent cycles, charging was set to CCCV at C / 2 and 4.3V for 30 minutes or until the current fell below C / 100. The cells were discharged at C / 5 for 5 cycles, followed by stepwise increasing discharge rates (C / 10, C / 5, C / 2, 1C, 2C, 3C). The 1C rate was then adapted to the capacity of the 1C discharge. After the rate test and C / 5 discharge cycles, two more C / 10 discharge cycles and 50 1C discharge cycles were performed. The C / 10 discharge cycles were then measured.

[0131] [Table 1]

Claims

1. The following steps: (a) providing an (oxy)hydroxide of TM, TM being a transition metal comprising nickel and optionally at least one of cobalt and manganese, the nickel content being at least 80 mol % relative to TM; (b) mixing said TM (oxy)hydroxide with 75-85 mol % of a lithium source relative to TM and at least one compound of Mg or Al; (c) treating the resulting mixture at a temperature in the range of 400-700° C. to obtain a powder; (d) The powder from step (c) is mixed with a lithium source and M 2 With at least one compound of M 2 is selected from Nb, Ta, W, Ti or Zr; (e) heat treating the mixture resulting from step (d) at a temperature in the range of 550 to 800° C.; The method for producing an electrode active material includes the steps of:

2. 10. The method of claim 1, further comprising the step (f) of adding a compound of boron or cobalt to the material resulting from step (e) followed by heat treatment.

3. 3. The method according to claim 1 or 2, wherein in step (a), the (oxy)hydroxide contains both Co and Mn.

4. TM is a compound represented by the general formula (I): (Ni a Co b Mr c ) (I) (wherein a is in the range of 0.85 to 0.99; b is 0 or in the range of 0.01 to 0.14; c is 0 or in the range of 0.01 to 0.15; a + b + c = 1) The method according to claim 1 or 2, which corresponds to

5. 3. The method according to claim 1 or 2, wherein the heat treatment in step (e) is carried out at a lower temperature than in step (c).

6. 3. The method of claim 1 or 2, wherein step (e) is carried out under an atmosphere of at least 80% by volume of oxygen.

7. 3. The process according to claim 1 or 2, wherein the temperature in step (c) is higher than the temperature in step (e).

8. General formula Li 1+x M 1 y1 (M 2 y2 T.M. 1-x-y1 O 2 A particulate electrode active material according to claim 1, wherein TM is a transition metal and comprises nickel and, optionally, at least one of cobalt and manganese, the nickel content being at least 80 mol % relative to TM, x being in the range of 0 to 0.05, and M 1 is selected from Mg, Al, and combinations thereof; 2 is selected from Nb, Ta, W, Ti or Zr, and combinations of at least two thereof, y1 is in the range of 0.005 to 0.05, y2 is in the range of 0.0025 to 0.02, and the material has an average primary particle size in the range of 50 to 350 nm, a span in the range of 0.5 to 1.1, and an average particle size (D50) of secondary particles in the range of 2 to 20 μm.

9. An electrode active material obtainable by the method according to claim 1.

10. (A) at least one particulate electrode active material according to claim 8 or 9; (B) carbon in a conductive state; and (C) a binder, a cathode.

11. (A) 80 to 98 mass % of a particulate electrode active material; (B) 1 to 17% by weight of carbon, and (C) 1 to 10% by mass of a binder The cathode of claim 10 comprising:

12. 11. An electrochemical cell comprising at least one cathode according to claim 10.

Citation Information

Patent Citations

  • Lithium-ion secondary battery

    JP2006351379A

  • Precursors and methods for preparing Ni-based cathode materials for rechargeable lithium-ion batteries

    JP2020510971A

  • Process for precipitating a mixed hydroxide, and cathode active materials made from such hydroxide

    WO2020207901A1

  • Cathode material and process

    WO2021123747A1