Method for manufacturing silicon carbide wafer and method for manufacturing silicon carbide ingot
By employing thermally conductive silicon carbide blocks with optimized flow paths, the method addresses the challenges of producing silicon carbide wafers and ingots with enhanced mechanical properties and crystallinity, achieving improved growth rates and reduced defects.
Patent Information
- Application Number
- JP2024525542
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-05
- Filing Date
- 2022-11-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing silicon carbide wafers and ingots face challenges in achieving improved mechanical properties, crystallinity, and reduced defects while maintaining high productivity.
A method involving the use of silicon carbide blocks with high thermal conductivity, arranged to facilitate uniform temperature distribution within the crucible, and incorporating channels and flow paths for efficient sublimation and deposition processes.
The method enhances the growth rate, reduces defects, and improves the crystallinity and mechanical strength of silicon carbide wafers and ingots, enabling the production of large-diameter wafers with superior quality.
Smart Images

Figure 2024538291000001_ABST
Abstract
Description
[Technical field]
[0001] The embodiments relate to a method for producing a silicon carbide wafer and a method for producing a silicon carbide ingot. [Background technology]
[0002] Silicon carbide (SiC), silicon (Si), gallium nitride (GaN), sapphire (Al 2 O 3 Single crystals such as GaN, gallium arsenide (GaAs), and aluminum nitride (AlN) are in increasing demand in industrial applications because they exhibit properties that cannot be expected from their polycrystal counterparts.
[0003] Single crystal silicon carbide (SiC) has a large energy band gap and is superior to silicon (Si) in maximum breakdown voltage and thermal conductivity. In addition, the carrier mobility of single crystal silicon carbide is comparable to that of silicon, and the electron saturation drift velocity and withstand voltage are also large. Due to these characteristics, single crystal silicon carbide is expected to be applied to semiconductor devices that require high efficiency, high withstand voltage, and large capacity.
[0004] Silicon carbide is grown by liquid phase epitaxy (LPE), seeded sublimation, chemical vapor deposition (CVD), etc. Among them, seeded sublimation has a high growth rate and can produce silicon carbide ingots, so it is the most widely used method and is also called physical vapor transport (PVT).
[0005] As a method for producing these single crystals, for example, Japanese Patent Publication No. 2001-114599 discloses growing a single crystal ingot on a seed crystal by maintaining the temperature of the seed crystal at a temperature 10 to 100° C. lower than the temperature of the raw material powder while heating it with a heater in a vacuum container (heating furnace) into which argon gas can be introduced. There are also other attempts to produce large-diameter single crystal ingots substantially free of defects. Summary of the Invention [Problem to be solved by the invention]
[0006] The embodiments provide a method for producing silicon carbide wafers and silicon carbide ingots having improved mechanical properties, excellent crystallinity, and fewer defects with improved productivity. [Means for solving the problem]
[0007] A method for manufacturing a silicon carbide wafer according to an embodiment includes the steps of placing a silicon carbide block in a crucible, sublimating the silicon carbide contained in the silicon carbide block to form a silicon carbide ingot, and processing the silicon carbide ingot.
[0008] In one embodiment, the silicon carbide block is about 1 cm 3 The apparent volume may be greater than or equal to 100 μm.
[0009] In one embodiment, the silicon carbide block may have a thermal conductivity of about 10 W / mK or greater in at least one direction.
[0010] In one embodiment, a flow passage through which sublimated silicon carbide gas can travel may be formed between the outer circumferential surface of the silicon carbide block and the inner surface of the reaction vessel.
[0011] In one embodiment, the silicon carbide block may be arranged to have a thermal conductivity of 10 W / mK or greater in the horizontal direction.
[0012] In one embodiment, the silicon carbide block may include channels through which sublimated silicon carbide gas can travel.
[0013] In one embodiment, the flow passage may be open upwards.
[0014] In one embodiment, at least a portion of the flow passage may have an increasingly larger inner diameter in the upward direction.
[0015] In one embodiment, the flow path may include a first flow path having a first inner diameter and a second flow path connected to the first flow path and having a second inner diameter larger than the first inner diameter, and the second flow path may be disposed on the first flow path.
[0016] In one embodiment, the silicon carbide blocks may include a first silicon carbide block disposed within the reaction vessel and a second silicon carbide block disposed on the first silicon carbide block.
[0017] In one embodiment, a flow passage may be formed between the first silicon carbide block and the second silicon carbide block through which sublimated silicon carbide gas can pass.
[0018] In one embodiment, silicon carbide powder may be disposed in the flow passage.
[0019] In one embodiment, the silicon carbide block may have a cylindrical, pyramidal, donut or polygonal prism shape.
[0020] In one embodiment, the growth rate of the silicon carbide ingot may be greater than or equal to 250 μm / hr.
[0021] In one embodiment, the silicon carbide block may include open pores, and the porosity of the silicon carbide block may be between 10 vol% and 50 vol%.
[0022] According to one embodiment, a method for producing a silicon carbide ingot includes the steps of placing a silicon carbide block in a crucible, placing a seed crystal in the crucible, and sublimating silicon carbide contained in the silicon carbide block to grow the seed crystal. Effect of the Invention
[0023] In the method for producing a silicon carbide wafer according to the embodiment, silicon carbide contained in a silicon carbide block is sublimated to produce a silicon carbide ingot and a silicon carbide wafer.
[0024] The raw material for forming the silicon carbide ingot has a block shape and therefore has high thermal conductivity. In particular, the silicon carbide block may be arranged to have high thermal conductivity in a horizontal direction.
[0025] This allows the heat generated in the crucible to be easily transferred to the inside of the crucible, which may form a uniform temperature gradient throughout the raw material placed inside the crucible.
[0026] Therefore, the method for producing a silicon carbide wafer and a method for producing a silicon carbide ingot according to the embodiment can easily control the temperature at each position in the crucible. Therefore, the method for producing a silicon carbide wafer and a method for producing a silicon carbide ingot according to the embodiment can prevent deviation in crystallinity and various defects due to temperature variations. As a result, the method for producing a silicon carbide wafer and a method for producing a silicon carbide ingot according to the embodiment may have improved crystallinity and mechanical strength.
[0027] In addition, since the silicon carbide block has a high thermal conductivity, the heat generated from the crucible can be efficiently transferred to the raw material placed inside the crucible. That is, the silicon carbide block may be a raw material for forming the silicon carbide wafer and a heat transfer medium for transferring heat to the inside. Therefore, the method for producing a silicon carbide wafer and a silicon carbide ingot according to the embodiment can improve the sublimation rate of silicon carbide. In addition, since the silicon carbide block has a high thermal conductivity, the temperature of the raw material can be maintained high even if the temperature near the seed crystal is low.
[0028] Therefore, the method for producing a silicon carbide wafer and a silicon carbide ingot according to the embodiment can improve not only the sublimation rate of silicon carbide but also the deposition rate on the seed crystal, and thus the method for producing a silicon carbide wafer and a silicon carbide ingot according to the embodiment can have an improved growth rate.
[0029] In addition, as the diameter of the silicon carbide wafer increases, the inner diameter of the crucible must also increase. In this case, since the silicon carbide block has high thermal conductivity, the internal temperature of the crucible can be efficiently controlled even if the inner diameter of the crucible increases. As a result, the method for producing a silicon carbide wafer and the method for producing a silicon carbide ingot according to the embodiment can efficiently produce large-diameter silicon carbide wafers with improved performance. [Brief description of the drawings]
[0030] [Figure 1] FIG. 2 is an exploded perspective view showing the crucible assembly and silicon carbide block according to the first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a silicon carbide block disposed within the crucible assembly according to the first embodiment. [Diagram 3] 1 is a cross-sectional view showing an ingot growing apparatus for producing a silicon carbide ingot according to a first embodiment. [Figure 4]FIG. 11 is a cross-sectional view showing a silicon carbide block disposed within a crucible assembly according to a second embodiment. [Diagram 5] FIG. 11 is a cross-sectional view showing a silicon carbide block disposed within a crucible assembly according to a third embodiment. [Figure 6] FIG. 11 is a perspective view showing a silicon carbide block according to a fourth embodiment. [Figure 7] FIG. 10 is a cross-sectional view showing a silicon carbide block disposed within a crucible assembly according to a fourth embodiment. [Figure 8] FIG. 13 is a perspective view showing a silicon carbide block according to a fifth embodiment. [Figure 9] FIG. 13 is a cross-sectional view showing a silicon carbide block disposed within a crucible assembly according to a fifth embodiment. [Figure 10] FIG. 13 is a cross-sectional view showing a silicon carbide block disposed within a crucible assembly according to a sixth embodiment. [Figure 11] FIG. 13 is a perspective view showing a silicon carbide block 100 according to a seventh embodiment. [Figure 12] FIG. 13 is a cross-sectional view showing a silicon carbide block disposed within a crucible assembly according to a seventh embodiment. [Figure 13] FIG. 13 is a cross-sectional view showing a silicon carbide block disposed within a crucible assembly according to an eighth embodiment. [Figure 14] FIG. 13 is a cross-sectional view showing a silicon carbide block disposed within a crucible assembly according to a ninth embodiment. [Figure 15] FIG. 23 is a cross-sectional view showing one cross section of a silicon carbide block according to a tenth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS In the following, the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily carry out the present invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments set forth herein.
[0032] In this specification, when a part "comprises" a certain component, this does not mean that it excludes other components, and it may further include other components, unless specifically stated to the contrary.
[0033] In this specification, when a certain component is said to be "connected" to another component, this includes not only the case where the component is "directly connected" but also the case where the component is "connected via another component therebetween."
[0034] In this specification, the term "B is located on A" means that B is located on A in direct contact with A, or that B is located on A with another layer therebetween, and is not to be interpreted as being limited to B being located in contact with the surface of A.
[0035] As used herein, the term "combinations thereof" contained in a Markush form expression means a mixture or combination of one or more selected from the group of components set forth in the Markush form expression, and is meant to include one or more selected from the group of components set forth above.
[0036] In this specification, the phrase "A and / or B" means "A, B, or A and B."
[0037] In this specification, the singular expression is to be construed as including the singular or plural as the context requires, unless otherwise specified.
[0038] Furthermore, the embodiments can be combined with each other unless they are technically contradictory.
[0039] Fig. 1 is an exploded perspective view showing a crucible assembly and a silicon carbide block 100 according to the first embodiment. Fig. 2 is a cross-sectional view showing a state in which a silicon carbide block 100 is disposed in a crucible assembly according to the first embodiment. Fig. 3 is a cross-sectional view showing an ingot growing apparatus for producing a silicon carbide ingot 111 according to the first embodiment.
[0040] As shown in FIGS. 1 to 3 , a silicon carbide ingot 111 growth apparatus for producing silicon carbide ingots 111 and silicon carbide wafers includes a crucible body 10, a crucible lid 11, a seed crystal holder 12, a thermal insulator 20, a reaction chamber 30, and an induction coil 40.
[0041] The crucible body 10 has an internal space. The crucible body 10 accommodates raw materials for growing a silicon carbide ingot 111. The crucible body 10 includes an accommodation portion that is a space for accommodating the raw materials. The crucible body 10 may have a cylindrical shape having an opening with an open top. The crucible body 10 may have a structure that allows silicon carbide raw materials to be charged therein.
[0042] The crucible body 10 may include graphite. The crucible body 10 may be made of graphite. The crucible body 10 may be a graphite crucible. The crucible body 10 may be an electrical conductor. The crucible body 10 may be heated by resistive heat caused by an induced current generated by the induction coil 40.
[0043] The density of the crucible body 10 is 1.70 g / cm 3 ~1.90g / cm 3 may be also possible.
[0044] The crucible lid 11 covers the inlet of the crucible body 10. The crucible lid 11 may have a circular plate shape. The crucible lid 11 may entirely cover the inlet of the crucible body 10. The crucible lid 11 may have a shape corresponding to the inlet of the crucible body 10.
[0045] The crucible lid 11 may have a thickness of about 10 mm to about 50 mm. The crucible lid 11 may have a thickness of about 15 mm to about 40 mm.
[0046] The density of the crucible lid 11 is 1.70 g / cm 3 ~1.90g / cm 3The crucible lid 11 may include graphite. The crucible lid 11 may be substantially made of graphite. The crucible lid 11 may have a shape that covers the entire opening of the crucible body 10.
[0047] The crucible lid 11 may cover a part of the opening of the crucible body 10 or may include a through hole (not shown). In this case, the transfer speed of the vapor in the crystal growth atmosphere described later can be adjusted.
[0048] The crucible body 10 and the crucible lid 11 may form a crucible assembly. The seed crystal 110 is disposed within the crucible assembly. The seed crystal holder 12 may be disposed within the crucible body 10. The seed crystal holder 12 may also be disposed below the crucible lid 11. That is, the seed crystal holder 12 may be disposed on the lower surface of the crucible lid 11. The seed crystal holder 12 may be formed integrally with the crucible lid 11.
[0049] The seed crystal holder 12 may include graphite. The seed crystal holder 12 may be made of graphite.
[0050] The seed crystal holder 12 may have a size of about 1 mm to about 20 mm. The seed crystal holder 12 may have a thickness of about 2 mm to about 10 mm.
[0051] The heat insulating material 20 is disposed around the crucible assembly. The heat insulating material 20 surrounds the crucible assembly. The heat insulating material 20 surrounds the outer periphery of the crucible body 10. The heat insulating material 20 may also be disposed on the crucible lid 11. The heat insulating material 20 may also be disposed under the crucible body 10.
[0052] The thermal insulation material 20 may affect the temperature gradient inside the crucible body 10 or inside the reaction vessel in a growth atmosphere. Specifically, the thermal insulation material 20 may include a graphite thermal insulation material 20, and more specifically, the thermal insulation material 20 may include a rayon-based graphite felt or a pitch-based graphite felt.
[0053] The density of the insulating material 20 may be about 0.12 g / cc to about 0.30 g / cc. The density of the insulating material 20 may be about 0.13 g / cc to about 0.25 g / cc. The density of the insulating material 20 may be about 0.14 g / cc to about 0.20 g / cc.
[0054] When the density of the insulation material 20 is within the above range, the silicon carbide ingot 111 can be appropriately formed convexly, and the occurrence of 6H-SiC polymorphism and the deterioration of the quality of the silicon carbide ingot 111 can be prevented.
[0055] When the density of the insulating material 20 is within the above range, the edge growth rate can be appropriately increased, and the occurrence of cracks in the silicon carbide ingot 111 can be suppressed.
[0056] When the insulation material 20 has a density of 0.12 g / cc to 0.30 g / cc, the quality of the ingot can be further improved, and when the insulation material has a density of 0.14 g / cc to 0.20 g / cc, it is better to control the crystal growth atmosphere during the ingot growth process and grow an ingot of better quality.
[0057] The insulating material 20 may have a porosity of about 73 vol% to about 95 vol%. The insulating material 20 may have a porosity of about 76 vol% to about 93 vol%. The insulating material 20 may have a porosity of about 81 vol% to about 91 vol%. When an insulating material 20 having such a porosity is used, the frequency of cracking of the ingot can be further reduced.
[0058] The heat insulating material 20 may have a compressive strength of about 0.21 MPa or more. The heat insulating material 20 may have a compressive strength of about 0.49 MPa or more. The heat insulating material 20 may have a compressive strength of about 0.78 MPa or more. The heat insulating material 20 may have a compressive strength of about 3 MPa or less, or about 25 MPa or less. When the heat insulating material 20 has these compressive strengths, it is possible to produce a SiC ingot of better quality by having excellent thermal / mechanical stability and a reduced probability of ash generation.
[0059] The heat insulating material 20 may be applied in a thickness of about 20 mm or more, and may be applied in a thickness of about 30 mm or more. The heat insulating material 20 may be applied in a thickness of about 150 mm or less, about 120 mm or less, and about 80 mm or less. When the heat insulating material 20 is applied in these thickness ranges, a sufficient heat insulating effect can be obtained without unnecessary waste of the heat insulating material 20.
[0060] The density of the insulating material 20 may be 0.12 g / cc to 0.30 g / cc, and the porosity of the insulating material 20 may be 72 vol% to 90 vol%. When these insulating materials 20 are used, it is possible to prevent the shape of the ingot from growing to be concave or excessively convex, and it is possible to reduce the phenomenon of the deterioration of the polymorph quality or the occurrence of cracks in the ingot.
[0061] The reaction chamber 30 may accommodate the crucible body 10, the crucible cover 11, the seed crystal holder 12, and the insulating material 20. The reaction chamber 30 may adjust the internal atmosphere of the crucible body 10. The reaction chamber 30 may adjust the internal gas atmosphere and pressure of the crucible body 10. That is, the reaction chamber 30 accommodates the crucible body 10, etc., and adjusts the internal gas atmosphere and pressure to adjust the overall reaction conditions.
[0062] The induction coil 40 is disposed outside the reaction chamber 30. The induction coil 40 can generate an induction current. The induction coil 40 can generate the AC current to generate an induction current in the crucible body 10. That is, the induction coil 40 can be a heating means for heating the crucible body 10.
[0063] Silicon carbide raw material is placed in the crucible body 10 to form the silicon carbide ingot 111. The silicon carbide raw material includes a silicon carbide block 100. The silicon carbide raw material may be mostly composed of the silicon carbide block 100. For example, the silicon carbide block 100 may be about 70% by weight or more based on the entire silicon carbide raw material. The silicon carbide block 100 may be about 80% by weight or more based on the entire silicon carbide raw material. The silicon carbide block 100 may be about 90% by weight or more based on the entire silicon carbide raw material.
[0064] The silicon carbide block 100 may have a block shape. One silicon carbide block 100 may be included in the crucible body 10. Alternatively, a plurality of silicon carbide blocks 100 may be included in the crucible body 10.
[0065] The apparent volume of the silicon carbide block 100 is approximately 1 cm 3 The apparent volume of the silicon carbide block 100 may be about 5 cm 3 The apparent volume of the silicon carbide block 100 may be about 10 cm 3 The apparent volume of the silicon carbide block 100 may be about 20 cm 3 The apparent volume of the silicon carbide block 100 may be about 100 cm 3 The apparent volume of the silicon carbide block 100 may be about 1000 cm 3 The apparent volume of the silicon carbide block 100 may be about 5000 cm 3The apparent volume of the silicon carbide block 100 is smaller than the volume of the internal space of the crucible body 10. The apparent volume of the silicon carbide block 100 is about 1 cm 3 It may be the following.
[0066] In this case, the apparent volume may be a volume measured based on the outer shape of the silicon carbide block 100. That is, the apparent volume may be a volume measured under the assumption that there are no pores in the silicon carbide block 100. That is, the apparent volume may be a value obtained by adding the volume of silicon carbide in the silicon carbide block 100 and the volume of pores in the silicon carbide block 100.
[0067] The silicon carbide block 100 may have a columnar shape such as a cylinder or a polygonal column. The silicon carbide block 100 may have a polyhedral shape. The silicon carbide block 100 may have a plate shape. The silicon carbide block 100 may have a pyramidal shape such as a cone or a polygonal pyramid. The silicon carbide block 100 may have a donut shape. The silicon carbide block 100 may have a shape with a part cut off.
[0068] The silicon carbide block 100 may be a single crystal or a polycrystal. The silicon carbide block 100 may be a sintered body. That is, the silicon carbide block 100 may be formed into a block shape by sintering silicon carbide particles or the like.
[0069] The silicon carbide block 100 may be formed by depositing silicon carbide by chemical vapor deposition. The silicon carbide block 100 may be formed by depositing silicon carbide by physical vapor deposition.
[0070] The silicon carbide block 100 may comprise alpha phase silicon carbide or beta phase silicon carbide.
[0071] The silicon carbide block 100 may have high thermal conductivity. The thermal conductivity of the silicon carbide block 100 may be about 10 W / mK or more. The thermal conductivity of the silicon carbide block 100 may be about 20 W / mK or more. The thermal conductivity of the silicon carbide block 100 may be about 30 W / mK or more. The thermal conductivity of the silicon carbide block 100 may be about 50 W / mK or more. The thermal conductivity of the silicon carbide block 100 may be about 70 W / mK or more. The thermal conductivity of the silicon carbide block 100 may be about 100 W / mK or more. The thermal conductivity of the silicon carbide block 100 may be about 110 W / mK or more. The upper limit of the thermal conductivity of the silicon carbide block 100 may be about 2000 W / mK.
[0072] Moreover, the silicon carbide block 100 may have anisotropic thermal conductivity. In this case, the silicon carbide block 100 may be arranged so as to have a thermal conductivity of about 10 W / mK or more in the horizontal direction. The silicon carbide block 100 may be arranged so as to have a thermal conductivity of about 20 W / mK or more in the horizontal direction. The silicon carbide block 100 may be arranged so as to have a thermal conductivity of about 30 W / mK or more in the horizontal direction. The silicon carbide block 100 may be arranged so as to have a thermal conductivity of about 40 W / mK or more in the horizontal direction. The silicon carbide block 100 may be arranged so as to have a thermal conductivity of about 50 W / mK or more in the horizontal direction. The silicon carbide block 100 may be arranged so as to have a thermal conductivity of about 70 W / mK or more in the horizontal direction. The silicon carbide block 100 may be arranged so as to have a thermal conductivity of about 100 W / mK or more in the horizontal direction. The silicon carbide block 100 may be arranged to have a thermal conductivity of about 110 W / mK or greater in the horizontal direction. The upper limit of the thermal conductivity of the silicon carbide block 100 in the horizontal direction may be about 2000 W / mK.
[0073] The silicon carbide block 100 may include single crystal silicon carbide or polycrystalline silicon carbide. The silicon carbide block 100 may be formed by growing silicon carbide into a single crystal or polycrystal. That is, the silicon carbide block 100 may be substantially free of pores. The porosity of the silicon carbide block 100 may be about 10 vol% or less. The porosity of the silicon carbide block 100 may be about 5 vol% or less. The porosity of the silicon carbide block 100 may be about 3 vol% or less. The porosity of the silicon carbide block 100 may have a lower limit of about 0.001 vol%. When the silicon carbide block 100 has a low porosity, it may have a high thermal conductivity.
[0074] Since the silicon carbide block 100 has a thermal conductivity within the above range, heat generated from the crucible body 10 can be efficiently transferred to the center of the internal space of the crucible body 10. As a result, a temperature gradient in the horizontal direction inside the crucible body 10 can be minimized. Therefore, the method for manufacturing a silicon carbide ingot and a silicon carbide wafer according to the embodiment can effectively control the internal temperature of the crucible body 10. Therefore, the silicon carbide ingot 111 manufactured by the silicon carbide block 100 may have a fast growth rate and improved crystal properties.
[0075] The diameter of the silicon carbide block 100 may be substantially the same as the inner diameter of the crucible body 10. As a result, the silicon carbide block 100 may be almost filled in the lower part of the crucible body 10. Also, at least a part of the outer surface of the silicon carbide block 100 may be in direct contact with the inner surface of the crucible body 10. The portion of the outer circumferential surface of the silicon carbide block 100 that is in contact with the inner surface of the crucible body 10 may be about 20% or more.
[0076] As described above, when the crucible body 10 and the silicon carbide block 100 are partially in contact with each other, the heat generated in the crucible body 10 can be easily transferred to the silicon carbide block 100 .
[0077] A silicon carbide wafer according to an embodiment can be manufactured as follows.
[0078] First, the silicon carbide ingot 111 can be manufactured. The silicon carbide ingot 111 is manufactured by applying a physical vapor transport (PVT) method so that the silicon carbide ingot 111 has a large area and few defects.
[0079] A method for producing a silicon carbide ingot according to one embodiment may include a preparation stage, a feedstock charging stage, and a growth stage.
[0080] The preparation step is a step of preparing a crucible assembly including the crucible body 10 having an internal space and a crucible lid 11 for covering the crucible body 10.
[0081] The step of loading the raw material includes loading the silicon carbide raw material including the silicon carbide block 100 into the crucible assembly, and disposing a seed crystal 110 on the raw material at a fixed distance from the raw material.
[0082] The seed crystal 110 is provided to produce the silicon carbide ingot 111. The seed crystal 110 may be any of wafers having an off-angle selected from the range of 0 to 8 degrees with respect to the
[0001] plane.
[0083] The silicon carbide seed crystal 110 may be a substantially single crystalline 4HSiC ingot with minimal defects or polymorphic inclusions, or may consist essentially of 4HSiC.
[0084] The seed crystal 110 may have a diameter of 4 inches or more, 5 inches or more, or even 6 inches or more. More specifically, the seed crystal 110 may have a diameter of 4 to 12 inches, 4 to 10 inches, or 6 to 8 inches.
[0085] The seed crystal 110 is adhered to the seed crystal holder 12. The seed crystal holder 12 comprises graphite. The seed crystal holder 12 may be made of graphite. The seed crystal holder 12 may comprise anisotropic graphite. More specifically, the seed crystal holder 12 may be made of anisotropic graphite.
[0086] The seed holder 12 may have a high thermal conductivity. The seed holder 12 may have a high thermal conductivity in the horizontal direction. The seed holder 12 may have a thermal conductivity of about 100 W / mK or more in at least one direction. The seed holder 12 may have a thermal conductivity of about 110 W / mK or more in at least one direction.
[0087] The crucible lid 11 and the seed crystal holder 12 may be integrally formed with each other. The crucible lid 11 and the seed crystal holder 12 may be made of graphite. In this case, the crucible lid 11 and the seed crystal holder 12 may have a thermal conductivity of about 100 W / mK or more in at least one of the horizontal directions. In this case, the crucible lid 11 and the seed crystal holder 12 may have a thermal conductivity of about 110 W / mK or more in at least one of the horizontal directions. The crucible lid 11 and the seed crystal holder 12 may have substantially the same thermal conductivity in different directions.
[0088] The seed crystal 110 and the seed crystal holder 12 are bonded together by an adhesive layer, which includes a graphite filler and a carbide such as a phenolic resin, and may have a low porosity.
[0089] The seed crystal 110 may be arranged so that the C-plane faces downward.
[0090] Then, raw materials including the silicon carbide block 100 are charged into the crucible to produce the silicon carbide ingot 111 .
[0091] The crucible assembly at the stage of charging the raw materials may have a weight ratio (Rw) of 0.3 to 0.8 times when the weight of the raw materials is taken as 1. Here, the weight of the crucible assembly means the weight of the crucible assembly excluding the raw materials, specifically, the weight of the crucible assembly including the seed crystal 110 excluding the weight of the raw materials charged therein, regardless of whether the seed crystal holder 12 is applied to the crucible assembly.
[0092] The growing step is a step of adjusting the internal space of the crucible body 10 to a crystal growing atmosphere, transferring the raw material to the seed crystal 110 as a vapor and depositing the raw material on the seed crystal 110, and providing a silicon carbide ingot 111 grown from the seed crystal 110.
[0093] The growth step includes a process of adjusting the internal space of the crucible assembly to a crystal growth atmosphere, and specifically, the growth step can be performed by surrounding the crucible assembly with a thermal insulator 20, providing a reaction vessel (not shown) including the crucible assembly and the thermal insulator 20 surrounding it, placing the reaction vessel in a reaction chamber such as a quartz tube, and then heating the crucible by a heating means.
[0094] The reaction vessel is located within the reaction chamber 42, and the internal space of the crucible body 10 is heated to a temperature suitable for the crystal growth atmosphere by an induction coil 40. Such temperature is one of the important factors in the crystal growth atmosphere, and a more suitable crystal growth atmosphere is formed by adjusting conditions such as pressure and gas movement. A heat insulating material 20 is located between the reaction chamber 42 and the reaction vessel, which can help to form and control the crystal growth atmosphere more easily.
[0095] The crystal growth atmosphere can be generated by heat generated in the crucible by an induction coil 40 outside the reaction chamber 42. The crucible can be heated simultaneously or separately to remove air by reducing the pressure, and the crystal growth atmosphere can be reduced pressure and / or inert atmosphere (e.g., Ar atmosphere, N2 atmosphere, or a mixture thereof).
[0096] The crystal growth atmosphere induces the growth of silicon carbide crystals by vapor transport of source material to the surface of seed crystal 110 , which grows into an ingot 111 .
[0097] The crystal growth atmosphere can be under conditions of a growth temperature of 2100° C. to 2450° C. and a growth pressure of 1 torr to 100 torr. When such temperatures and pressures are applied, silicon carbide ingot 111 can be produced more efficiently.
[0098] Specifically, the crystal growth atmosphere may be such that the surface temperature of the upper and lower parts of the crucible is 2100°C to 2450°C, the growth temperature is 1 torr to 50 torr, and more specifically, the surface temperature of the upper and lower parts of the crucible is 2150°C to 2450°C, the growth pressure is 1 torr to 40 torr.
[0099] More specifically, the conditions of a growth temperature of 2150 to 2350° C. in which the surface temperatures at the top and bottom of the crucible are in the range of 1 torr to 30 torr can be applied.
[0100] Application of the above-mentioned crystal growth atmosphere is advantageous in producing a higher quality silicon carbide ingot by the production method of the present invention.
[0101] The silicon carbide ingot contains 4HSiC and may have a convex or flat surface.
[0102] If the surface of the silicon carbide ingot is formed concavely, in addition to the intended 4H—SiC crystals, other polymorphs such as 6H—SiC may be mixed in, which may degrade the quality of the silicon carbide ingot 111. Also, if the surface of the silicon carbide ingot 111 is formed excessively convexly, cracks may occur in the ingot itself or the crystals may break when processed into wafers.
[0103] At this time, whether the silicon carbide ingot is an excessively convex ingot is determined based on the degree of warpage, and the silicon carbide ingot 111 produced in this specification has a warpage of 20 mm or less.
[0104] The warpage is evaluated by placing a sample of a silicon carbide ingot on a surface plate, measuring the height between the center and edge of the ingot based on the rear surface of the ingot with a height gauge, and determining the value of (center height - edge height). A positive value of the warpage indicates a convex shape, a value of 0 indicates a flat shape, and a negative value indicates a concave shape.
[0105] Specifically, the silicon carbide ingot may have a convex or flat surface and a warpage of 0 mm to 14 mm, 0 mm to 11 mm, or 0 mm to 8 mm. Silicon carbide ingots having these degrees of warpage are easier to process into wafers and can reduce the occurrence of cracks.
[0106] The silicon carbide ingot may be a substantially single crystal 4HSiC ingot with minimal defects or polymorphic inclusions. The silicon carbide ingot may be substantially made of 4HSiC and may have a convex or flat surface.
[0107] The silicon carbide ingot has reduced defects that may occur in silicon carbide ingots, and can provide silicon carbide wafers of higher quality.
[0108] The silicon carbide ingot produced by the method of the present invention has reduced surface pits, and specifically, the pits contained in the surface of an ingot having a diameter of 4 inches or more are reduced to 10k / cm 2 It may be the following.
[0109] In this specification, the surface pits of the silicon carbide ingot are measured by observing a total of five locations using an optical microscope: one location in the center of the surface of the ingot excluding facets, and four locations at the 3 o'clock, 6 o'clock, 9 o'clock, and 12 o'clock positions located approximately 10 mm inward toward the center of the edge of the silicon carbide ingot, and measuring the number of surface pits per unit area (1 cm 2 ) and then evaluate it as the average value.
[0110] For example, the silicon carbide ingot may be subjected to external grinding equipment to grind the outer edge of the ingot, slice it to a certain thickness, and then perform processing such as grinding the edge and grinding and polishing the surface.
[0111] The slicing step is a step of slicing a silicon carbide ingot to have a certain off-angle to provide a sliced crystal. The off-angle is based on the
[0001] plane of 4HSiC. Specifically, the off-angle may be an angle selected from 0 to 15 degrees, an angle selected from 0 to 12 degrees, or an angle selected from 0 to 8 degrees.
[0112] The slicing can be performed by any slicing method that is normally applied in the manufacture of wafers. Examples of the slicing method that can be used include cutting using a diamond wire or a wire to which diamond slurry is applied, and cutting using a blade or wheel to which diamond is partially applied, but are not limited to these.
[0113] The thickness of the sliced crystal can be adjusted in consideration of the thickness of the wafer to be manufactured, and the crystal can be sliced to an appropriate thickness in consideration of the thickness after polishing in the polishing step described below.
[0114] The polishing step is a step of polishing the sliced crystal to a thickness of 300 to 800 μm to form a silicon carbide wafer.
[0115] The polishing step may be performed using a polishing method that is generally used in wafer manufacturing. For example, a method in which processes such as lapping and / or grinding are performed, followed by polishing, etc. may be used.
[0116] In the method for producing silicon carbide wafers according to the embodiment, silicon carbide contained in a silicon carbide block 100 is sublimated to produce a silicon carbide ingot and a silicon carbide wafer.
[0117] The raw material for forming the silicon carbide ingot has a block shape and therefore has high thermal conductivity. In particular, the silicon carbide block 100 may be arranged to have high thermal conductivity in the horizontal direction.
[0118] This allows the heat generated in the crucible to be easily transferred to the inside of the crucible, which may form a uniform temperature gradient throughout the raw material placed inside the crucible.
[0119] Therefore, the method for manufacturing a silicon carbide wafer and a method for manufacturing a silicon carbide ingot according to the embodiment can easily control the temperature at each position in the crucible. Therefore, the method for manufacturing a silicon carbide wafer and a method for manufacturing a silicon carbide ingot according to the embodiment can prevent deviations in crystallinity and various defects due to temperature variations. As a result, the method for manufacturing a silicon carbide wafer and a method for manufacturing a silicon carbide ingot according to the embodiment can have improved crystallinity and mechanical strength.
[0120] In addition, since the silicon carbide block 100 has high thermal conductivity, the heat generated from the crucible can be efficiently transferred to the raw material placed inside the crucible. That is, the silicon carbide block 100 may be a raw material for forming the silicon carbide wafer, and may also be a heat transfer medium for transferring heat to the inside. Therefore, the method for producing a silicon carbide wafer and a silicon carbide ingot according to the embodiment can improve the sublimation rate of silicon carbide. In addition, since the silicon carbide block 100 has high thermal conductivity, the temperature of the raw material can be maintained high even if the temperature near the seed crystal 110 is low.
[0121] The silicon carbide block 100 may have high thermal conductivity and may be arranged to have high thermal conductivity in the horizontal direction. As a result, the raw material in the crucible body 10 may have high thermal conductivity in the horizontal direction as a whole. Therefore, the method for producing a silicon carbide ingot and a wafer according to the embodiment can reduce the temperature gradient in the horizontal direction. In addition, since the temperature difference between the center part and the outer part of the raw material is not large, the temperature difference between the vicinity of the seed crystal 110 and the upper part of the raw material may be large. That is, the temperature gradient in the vertical direction in the crucible body 10 may be large. As a result, the sublimation rate of silicon carbide in the vicinity of the raw material may be increased, and the deposition rate in the seed crystal 110 may also be increased.
[0122] Therefore, the method for producing a silicon carbide wafer and a silicon carbide ingot according to the embodiment can not only improve the sublimation rate of silicon carbide, but also improve the deposition rate on the seed crystal 110. Therefore, the method for producing a silicon carbide wafer and a silicon carbide ingot according to the embodiment can have an improved growth rate.
[0123] In addition, as the diameter of the silicon carbide wafer increases, the inner diameter of the crucible body 10 must also increase. At this time, since the silicon carbide block 100 has high thermal conductivity, the internal temperature of the crucible body 10 can be efficiently controlled even if the inner diameter of the crucible body 10 increases. As a result, the method for producing a silicon carbide wafer and the method for producing a silicon carbide ingot according to the embodiment can efficiently produce large-diameter silicon carbide wafers with improved performance.
[0124] 4 is a cross-sectional view showing a state in which a silicon carbide block is disposed in a crucible assembly according to a second embodiment. In the description of this embodiment, the description of the method for manufacturing silicon carbide ingots and wafers described above will be referred to, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0125] 4, a first flow passage 120 may be formed between the silicon carbide block 100 and an inner surface of the crucible body 10. The first flow passage 120 may be an empty space between an outer circumferential surface of the silicon carbide block 100 and an inner surface of the crucible body 10. That is, the first flow passage 120 may be formed such that the outer circumferential surface of the silicon carbide block 100 and the inner surface of the crucible body 10 are spaced apart from each other.
[0126] The width (D) of the first flow passage 120 may be about 0.1 mm to about 30 mm. The width (D) of the first flow passage 120 may be about 0.5 mm to about 20 mm. The width (D) of the first flow passage 120 may be about 1 mm to about 10 mm.
[0127] The first flow passage 120 may be formed on the entire outer circumferential surface of the silicon carbide block 100. The first flow passage 120 may be formed on a part of the outer circumferential surface of the silicon carbide block 100. The first flow passage 120 may be formed on about 10% to about 90% of the outer circumferential surface of the silicon carbide block 100. The first flow passage 120 may be formed on about 20% to about 80% of the outer circumferential surface of the silicon carbide block 100. The first flow passage 120 may be formed on about 30% to about 70% of the outer circumferential surface of the silicon carbide block 100.
[0128] The first flow passage 120 may extend from a lower portion to an upper portion of the silicon carbide block 100. The first flow passage 120 may extend from a bottom of the crucible body 10 toward an upper portion of the crucible body 10. The first flow passage 120 may extend in the vertical direction.
[0129] Through the first flow passage 120, silicon carbide gas sublimated at the outer circumferential surface of the silicon carbide block 100 and at the bottom of the silicon carbide block 100 can effectively move to the top of the crucible body 10. As a result, the method for producing silicon carbide ingots and wafers according to the present embodiment can have an improved growth rate.
[0130] 5 is a cross-sectional view showing a state in which a silicon carbide block is disposed in a crucible assembly according to a third embodiment. In the description of this embodiment, reference is made to the description of the method for manufacturing silicon carbide ingots and wafers described above, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0131] 5, the first flow passage 120 contains silicon carbide powder. The first flow passage 120 may be filled with the silicon carbide powder. That is, the first flow passage 120 may be packed with the silicon carbide powder.
[0132] The silicon carbide powder includes silicon carbide. The silicon carbide powder may be made of silicon carbide. The silicon carbide powder may have a particle size of about 75 μm or less and may be contained in an amount of 15 wt % or less, 10 wt % or less, or 5 wt % or less based on the total raw material.
[0133] The silicon carbide powder may have a D50 particle size of about 130 μm to about 400 μm.The silicon carbide powder may have a D50 particle size of about 170 μm to about 300 μm.
[0134] The silicon carbide powder is disposed between the silicon carbide block 100 and the crucible body 10, and can transfer heat generated from the crucible body 10 to the silicon carbide block 100. That is, the silicon carbide powder fills the gap between the silicon carbide block 100 and the crucible body 10, and can improve the heat transfer characteristics between the crucible body 10 and the silicon carbide block 100. In addition, since the first flow passage 120 is filled with the silicon carbide powder, the sublimated silicon carbide can efficiently move to the spaces between the particles contained in the silicon carbide powder.
[0135] Therefore, the method for manufacturing silicon carbide ingots and wafers according to the present embodiment can provide ingots and wafers with improved crystal properties, reduced defects, and improved growth rates.
[0136] FIG 6 is a perspective view of a silicon carbide block according to the fourth embodiment. FIG 7 is a cross-sectional view of a silicon carbide block disposed in a crucible assembly according to the fourth embodiment. In the description of this embodiment, the description of the method for manufacturing silicon carbide ingots and wafers described above will be referred to, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0137] As shown in FIGS. 6 and 7, the silicon carbide blocks may include a first silicon carbide block 101, a second silicon carbide block 102, and a third silicon carbide block 103.
[0138] The first silicon carbide block 101, the second silicon carbide block 102, and the third silicon carbide block 103 may be stacked in sequence.
[0139] That is, the first silicon carbide block 101 may be placed on the bottom surface of the crucible body 10, the second silicon carbide block 102 may be placed on the first silicon carbide block 101, and the third silicon carbide block 103 may be placed on the second silicon carbide block 102.
[0140] The first silicon carbide block 101, the second silicon carbide block 102, and the third silicon carbide block 103 may have various shapes, as described above, in addition to the plate shape shown in FIG.
[0141] The number of silicon carbide blocks arranged in the crucible body 10 may be three or more. That is, a plurality of silicon carbide blocks may be arranged in a stacked manner in the crucible body 10. The silicon carbide blocks 100 may have various shapes that are the same as each other or different from each other.
[0142] In the method for producing silicon carbide ingots and wafers according to this embodiment, a plurality of silicon carbide blocks are used as silicon carbide raw materials, and the raw materials can be stacked to a desired height. In addition, in the method for producing silicon carbide ingots and wafers according to this embodiment, a plurality of silicon carbide blocks are appropriately arranged in the crucible body 10, and the overall thermal conductivity can be efficiently designed. In addition, in the method for producing silicon carbide ingots and wafers according to this embodiment, a plurality of silicon carbide blocks are arranged to form a flow path so that the sublimated silicon carbide gas can efficiently move to the seed crystal 110.
[0143] Therefore, the method for manufacturing silicon carbide ingots and wafers according to the present embodiment can provide ingots and wafers with improved crystal properties, reduced defects, and improved growth rates.
[0144] FIG. 8 is a perspective view of a silicon carbide block according to the fifth embodiment. FIG. 9 is a cross-sectional view of a silicon carbide block disposed in a crucible assembly according to the fifth embodiment. In the description of this embodiment, the description of the method for manufacturing silicon carbide ingots and wafers described above will be referred to, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0145] The silicon carbide raw material may further include spacers as shown in Figures 8 and 9. The spacers may be disposed between the silicon carbide blocks.
[0146] A first spacer 131 may be disposed between the first silicon carbide block 101 and the second silicon carbide block 102. Also, a second spacer 132 may be disposed between the second silicon carbide block 100 and the third silicon carbide block 103.
[0147] The spacer may include silicon carbide. The spacer may be made of silicon carbide. The spacer may include 99 mass % or more of silicon carbide.
[0148] The spacer may also be a silicon carbide block 100. That is, the spacer may be a silicon carbide ingot having a certain size or larger.
[0149] The first spacer 131 forms a space between the first silicon carbide block 101 and the second silicon carbide block 102. The first spacer 131 forms a second flow path 121 between the first silicon carbide block 101 and the second silicon carbide block 102. The second flow path 121 may extend in a horizontal direction.
[0150] The width of the second flow path 121 may be about 0.5 mm to about 30 mm. The width of the second flow path 121 may be about 1 mm to about 20 mm. The width of the second flow path 121 may be about 5 mm to about 10 mm. The width of the second flow path 121 may be determined by the height of the first spacer 131.
[0151] The second flow passage 121 may be connected to the first flow passage 120. That is, the second flow passage 121 may be connected to the space between the second silicon carbide block 102 and the inner surface of the crucible body 10.
[0152] The second spacer 132 forms a space between the second silicon carbide block 102 and the third silicon carbide block 103. The second spacer 132 forms a third flow path 122 between the second silicon carbide block 102 and the third silicon carbide block 103. The third flow path 122 may extend in a horizontal direction.
[0153] The width of the third flow path 122 may be about 0.5 mm to about 30 mm. The width of the third flow path 122 may be about 1 mm to about 20 mm. The width of the third flow path 122 may be about 5 mm to about 10 mm. The width of the third flow path 122 may be determined by the height of the second spacer 132.
[0154] The third flow passage 122 may be connected to the first flow passage 120. That is, the third flow passage 122 may be connected to the space between the third silicon carbide block 103 and the inner surface of the crucible body 10.
[0155] Although not shown in the drawings, a third spacer may also be disposed between the first silicon carbide block 101 and the bottom surface of the crucible body 10. The third spacer can form a fourth flow path between the first silicon carbide block 101 and the bottom surface of the crucible body 10.
[0156] The second flow path 121, the third flow path 122, and the fourth flow path may extend inside the crucible body 10 in a direction intersecting the vertical direction.
[0157] As a result, silicon carbide gas generated by sublimation on the upper surface of the first silicon carbide block 101 and the third spacer can be efficiently transmitted to the seed crystal 110 via the fourth flow path and the first flow path 120.
[0158] In addition, silicon carbide gas sublimated at the underside of the first silicon carbide block 101, the underside of the second silicon carbide block 102, and the first spacer 131 can be efficiently transmitted to the seed crystal 110 via the second flow path 121 and the first flow path 120.
[0159] In addition, silicon carbide gas sublimated at the upper surface of the second silicon carbide block 102, the lower surface of the third silicon carbide block 103, and the second spacer 132 can be efficiently transmitted to the seed crystal 110 via the third flow path 122 and the first flow path 120.
[0160] The method for producing silicon carbide ingots and wafers according to this embodiment can efficiently transport sublimated silicon carbide gas upward by using a flow path extending in a direction intersecting the vertical direction, for example, horizontally.
[0161] Therefore, the method for producing silicon carbide ingots and wafers according to the present embodiment can provide ingots and wafers with improved growth rates, fewer defects, and improved crystal properties.
[0162] 10 is a cross-sectional view showing a state in which a silicon carbide block is disposed in a crucible assembly according to a sixth embodiment. In the description of this embodiment, the description of the method for manufacturing silicon carbide ingots and wafers described above will be referred to, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0163] 10, silicon carbide powder may be disposed in a first flow path 120, a second flow path 121, and a third flow path 122. The silicon carbide powder may be packed in the first flow path 120, the second flow path 121, and the third flow path 122.
[0164] Although not shown in the drawing, the silicon carbide powder may also be disposed in the fourth flow path.
[0165] Moreover, the first spacer 131, the second spacer 132, and the third spacer can be omitted. That is, the spacer functions of the first spacer 131, the second spacer 132, and the third spacer can be substituted by the silicon carbide powder.
[0166] The silicon carbide powder improves the heat transfer characteristics in each flow path, and the gas transfer performance of the sublimated silicon carbide can be maintained due to the spaces between the particles contained in the silicon carbide powder.
[0167] Thus, the method for producing silicon carbide ingots and wafers according to the present embodiment may have a uniform temperature gradient in the horizontal direction overall, thereby providing ingots and wafers with improved growth rates, fewer defects, and improved crystal properties.
[0168] FIG. 11 is a perspective view of a silicon carbide block according to the seventh embodiment. FIG. 12 is a cross-sectional view of a silicon carbide block disposed in a crucible assembly according to the seventh embodiment. In the description of this embodiment, the description of the method for manufacturing silicon carbide ingots and wafers described above will be referred to, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0169] 11 and 12, the silicon carbide block 100 includes a fifth flow passage 124. The fifth flow passage 124 may be formed in a central portion of the silicon carbide block 100. The fifth flow passage 124 may be formed to extend upward from the inside of the silicon carbide block 100. Furthermore, the fifth flow passage 124 may be open upward from the inside of the silicon carbide block 100.
[0170] In this case, the depth of the fifth flow passage 124 may be about ½ to about 1 / 1 of the height of the silicon carbide block 100. The depth of the fifth flow passage 124 may be about ⅔ to about 9 / 10 of the height of the silicon carbide block 100. The depth of the fifth flow passage 124 may be about ¾ to about 4 / 5 of the height of the silicon carbide block 100.
[0171] The fifth flow passage 124 may penetrate the silicon carbide block 100 in the vertical direction. That is, the fifth flow passage 124 may penetrate the silicon carbide block 100 from the lower surface to the upper surface.
[0172] The fifth flow passage 124 may have a cylindrical shape. The silicon carbide block 100 may have a donut shape.
[0173] The diameter of the fifth flow passage 124 may be about 1 / 10 to about 1 / 2 of the diameter of the silicon carbide block 100. The diameter of the fifth flow passage 124 may be about 1 / 5 to about 1 / 3 of the diameter of the silicon carbide block 100. The diameter of the fifth flow passage 124 may be about 3 / 10 to about 1 / 2 of the diameter of the silicon carbide block 100.
[0174] Furthermore, the diameter of the fifth flow path 124 may be about 1 cm to about 30 cm. The diameter of the fifth flow path 124 may be about 3 cm to about 20 cm. The diameter of the fifth flow path 124 may be about 5 cm to about 10 cm.
[0175] Since the fifth flow passage 124 is open upward, the silicon carbide gas sublimated to the inner surface of the fifth flow passage 124 can be efficiently transferred upward. The inner surface of the fifth flow passage 124 may be disposed along the inner surface of the crucible body 10. This allows the heat from the crucible body 10 to be uniformly transferred to the inner surface of the fifth flow passage 124. That is, the interval between the inner surface of the fifth flow passage 124 and the inner surface of the crucible body 10 may be uniform depending on the position, and the heat from the crucible body 10 can be uniformly transferred to the inner surface of the fifth flow passage 124.
[0176] Therefore, the method for manufacturing a silicon carbide ingot and a wafer according to the embodiment can uniformly adjust the temperature of the inner surface of the fifth flow passage 124. Furthermore, the method for manufacturing a silicon carbide ingot and a wafer according to the embodiment can efficiently sublimate silicon carbide gas from the inner surface of the fifth flow passage 124.
[0177] As a result, the method for producing silicon carbide ingots and wafers according to the present invention can provide ingots and wafers with improved crystal properties, reduced defects, and improved growth rates.
[0178] 13 is a cross-sectional view showing a state in which a silicon carbide block is disposed in the crucible assembly according to the eighth embodiment of the present invention. In the description of this embodiment, the description of the method for manufacturing silicon carbide ingots and wafers described above will be referred to, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0179] 13, the silicon carbide block 100 includes a sixth flow passage 125. The sixth flow passage 125 may be formed in a central portion of the silicon carbide block 100. The sixth flow passage 125 may be formed to extend upward from the inside of the silicon carbide block 100. Furthermore, the sixth flow passage 125 may be open upward from the inside of the silicon carbide block 100.
[0180] In this case, the depth of the sixth flow passage 125 may be about ½ to about 1 / 1 of the height of the silicon carbide block 100. The depth of the sixth flow passage 125 may be about ⅔ to about 9 / 10 of the height of the silicon carbide block 100. The depth of the sixth flow passage 125 may be about ¾ to about ⅓ of the height of the silicon carbide block 100.
[0181] The sixth flow passage 125 may have an average inner diameter of about 1 cm to about 30 cm. The sixth flow passage 125 may have an average inner diameter of about 3 cm to about 20 cm. The sixth flow passage 125 may have an average inner diameter of about 5 cm to about 10 cm.
[0182] The sixth flow passage 125 may penetrate the silicon carbide block 100 in the vertical direction. That is, the sixth flow passage 125 may penetrate the silicon carbide block 100 from the lower surface to the upper surface.
[0183] Furthermore, the inner surface of the sixth flow channel 125 may be inclined with respect to the vertical direction. The sixth flow channel 125 may have an inner diameter that becomes larger toward the top. Here, the inner diameter of the flow channel means the diameter of a circle having the same area as the cross-sectional area of the flow channel in the horizontal direction of the flow channel. The average inclination of the inner surface of the sixth flow channel 125 may be 0.5 to 10. The average inclination of the inner surface of the sixth flow channel 125 may be about 1 to about 5. The average inclination of the inner surface of the sixth flow channel 125 may be about 1.5 to about 3.
[0184] Here, the average gradient is a value obtained by dividing the depth of the sixth flow passage 125 by the difference between the inner diameter of the lowest portion of the sixth flow passage 125 and the inner diameter of the highest portion of the sixth flow passage 125. The average gradient is expressed by the following Equation 1.
[0185] [Formula 1] Depth of channel / (ID at top of channel - ID at bottom of channel)
[0186] The sixth flow passage 125 may have a truncated cone shape. The sixth flow passage 125 may have a truncated polygonal pyramid shape. The inner diameter of the sixth flow passage 125 may tend to become larger toward the top.
[0187] Since the sixth flow passage 125 is open upward, the silicon carbide gas sublimated to the inner surface of the sixth flow passage 125 can be efficiently transferred upward. In addition, since the inner surface of the sixth flow passage 125 is inclined, it may have a large surface area.
[0188] In addition, the induction coil 40 may reduce the amount of heat applied from the lower portion to the upper portion of the crucible body 10 in the region where the silicon carbide block 100 is disposed. As a result, even if the inner surface of the sixth passage 125 is inclined, the temperature of the inner surface of the sixth passage 125 may be uniformly adjusted.
[0189] Therefore, the method for manufacturing silicon carbide ingots and wafers according to the embodiment can increase the amount of silicon carbide gas sublimated from the inner surface of the sixth flow passage 125.
[0190] As a result, the method for producing silicon carbide ingots and wafers according to the present invention can provide ingots and wafers with improved crystal properties, reduced defects, and improved growth rates.
[0191] 14 is a cross-sectional view showing a state in which a silicon carbide block is disposed in a crucible assembly according to a ninth embodiment. In the description of this embodiment, the description of the method for manufacturing silicon carbide ingots and wafers described above will be referred to, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0192] 14, a flow channel formed in a central portion of a silicon carbide block 100 may have a stepped shape. An inner surface of the flow channel may have a stepped shape. An inner surface of the flow channel may have a step.
[0193] The silicon carbide block 100 may include a seventh passage 126, an eighth passage 127, and a ninth passage 128.
[0194] The seventh flow passage 126 is disposed in the lower portion of the silicon carbide block 100. The seventh flow passage 126 is disposed adjacent to the lower surface of the silicon carbide block 100. The seventh flow passage 126 may penetrate the lower surface of the silicon carbide block 100.
[0195] The eighth flow passage 127 is connected to the seventh flow passage 126 and disposed above the seventh flow passage 126 .
[0196] The ninth flow passage 128 is disposed on the eighth flow passage 127. In addition, the ninth flow passage 128 is connected to the eighth flow passage 127. The ninth flow passage 128 is disposed on the upper part of the silicon carbide block 100. The ninth flow passage 128 penetrates the upper surface of the silicon carbide block 100. The ninth flow passage 128 opens upward from the upper surface of the silicon carbide block 100.
[0197] The average inner diameter of the ninth flow passage 128 is larger than the average inner diameter of the eighth flow passage 127. In addition, the average inner diameter of the eighth flow passage 127 is larger than the average inner diameter of the ninth flow passage 128.
[0198] The average inner diameter of the ninth flow passage 128 may be about 1.1 to about 2 times larger than the average inner diameter of the eighth flow passage 127. Furthermore, the average inner diameter of the eighth flow passage 127 may be about 1.1 to about 2 times larger than the average inner diameter of the seventh flow passage 126.
[0199] Since the ninth flow passage 128 is open upward, the silicon carbide gas sublimated to the inner surfaces of the seventh flow passage 126, the eighth flow passage 127, and the ninth flow passage 128 can be efficiently transferred upward. In addition, the inner surfaces of the seventh flow passage 126, the eighth flow passage 127, and the ninth flow passage 128 may have a large surface area because they have steps.
[0200] In addition, the induction coil 40 may reduce the heat applied from the lower portion to the upper portion of the crucible body 10 in the region where the silicon carbide block 100 is disposed. As a result, even if the inner surfaces of the seventh flow passage 126, the eighth flow passage 127, and the ninth flow passage 128 have steps, the temperatures of the inner surfaces of the seventh flow passage 126, the eighth flow passage 127, and the ninth flow passage 128 may be uniformly adjusted.
[0201] Therefore, the method for manufacturing silicon carbide ingots and wafers according to the embodiment can increase the amount of silicon carbide gas sublimated from the inner surface of the sixth flow passage 125.
[0202] As a result, the method for producing silicon carbide ingots and wafers according to the present invention can provide ingots and wafers with improved crystal properties, reduced defects, and improved growth rates.
[0203] 15 is a cross-sectional view showing one section of a silicon carbide block according to a tenth embodiment. In the description of this embodiment, the description of the method for manufacturing silicon carbide ingots and wafers described above will be referred to, and the modified parts will be further described. The description of the above embodiment can be essentially combined with the description of this embodiment, except for the modified parts.
[0204] 15, the silicon carbide block 100 may have micropores 129. The micropores 129 may have an inner diameter of about 1 μm to about 500 μm. The micropores 129 are open pores. That is, the micropores 129 may be open to the outside of the silicon carbide block 100. The micropores 129 may be connected to each other up to the inside of the silicon carbide block 100.
[0205] In order to form the micropores 129, the silicon carbide block 100 may be formed by sintering. That is, silicon carbide powder may be packed into a desired shape and sintered to form the silicon carbide block 100. In the sintering process, particles contained in the silicon carbide powder may be connected to each other to form the silicon carbide block 100. In addition, spaces between particles contained in the silicon carbide powder may form the micropores 129 in the sintering process.
[0206] The spacer may also have a structure similar to that of the silicon carbide block 100. That is, the spacer may also include micropores 129.
[0207] The silicon carbide block 100 has high thermal conductivity since silicon carbide particles are connected to each other, and since it contains the micropores 129, the sublimated silicon carbide gas can be efficiently released.
[0208] Therefore, the method for producing a silicon carbide ingot and a wafer according to the embodiment can increase the amount of silicon carbide gas sublimated from the inner surface of the micropores 129 .
[0209] As a result, the method for producing silicon carbide ingots and wafers according to the present invention can provide ingots and wafers with improved crystal properties, reduced defects, and improved growth rates.
[0210] The above-mentioned embodiments can be combined with each other if they are not technically contradictory. For example, silicon carbide powder may be arranged in the fourth flow path, the fifth flow path 124, the sixth flow path 125, the seventh flow path 126, the eighth flow path 127, and the ninth flow path 128. The silicon carbide powder may also be arranged in the spaces between the silicon carbide blocks 100. The spacers may be arranged in various positions to form the flow paths.
[0211] The following examples are provided to provide a more detailed description of the embodiments. The following examples are merely illustrative for understanding the embodiments, and the scope of the present invention is not limited thereto.
[0212] Examples 1 to 5 and Comparative Examples The doughnut-shaped sintered body #1 was placed inside the graphite crucible body. A silicon carbide seed crystal and a seed crystal holder were placed on the top of the silicon carbide block. At this time, the silicon carbide seed crystal (4HSiC single crystal, 6 inches) was fixed in place in a conventional manner so that the C-face of the seed crystal faces the bottom of the crucible. The crucible lid and the seed crystal holder were integrally manufactured from graphite, and both the crucible lid and the seed crystal holder had a disk shape.
[0213] The crucible body was covered with a crucible lid on which the seed crystal and the seed crystal holder were placed, and was surrounded by a heat insulating material, and then placed in a reaction chamber equipped with a heating coil as a heating means.
[0214] In this case, graphite felt with a density of 0.19 g / cc, a porosity of 85%, and a compressive strength of 0.37 MPa is used as the heat insulating material.
[0215] After creating a vacuum inside the crucible, argon gas was gradually introduced until the inside of the crucible reached atmospheric pressure, and the inside of the crucible was gradually depressurized. At the same time, the inside temperature of the crucible was gradually increased to 2000° C. at a rate of about 5° C. / min, and then to 2350° C. at a rate of about 3° C. / min.
[0216] Then, a SiC ingot was grown from the silicon carbide seed crystal at a temperature of 2350° C. and a pressure of 20 torr for 100 hours.
[0217] The silicon carbide ingot was then cut using a diamond wire saw and processed through a chamfering process, a grinding process, and a polishing process, thereby producing silicon carbide wafers with an off-angle of 4 degrees relative to the (0001) plane.
[0218] JPEG2024538291000002.jpg92121
[0219] 1) Donut-shaped silicon carbide sintered body #1 is formed by sintering silicon carbide powder having a D50 particle size of about 150 μm at a temperature of about 2200° C. for about 5 hours, and has the shape shown in FIG. 10, an outer diameter of about 175 mm, an inner diameter of about 30 mm, a height of about 80 mm, and a porosity of about 45 vol%.
[0220] 2) Donut-shaped silicon carbide sintered body #2 Silicon carbide powder having a D50 particle size of about 150 μm is sintered at a temperature of about 2200° C. for about 5 hours to form a silicon carbide sintered body having the shape of a silicon carbide block shown in FIG. 13, an outer diameter of about 170 mm, a height of about 80 mm, a smallest inner diameter of about 30 mm, a largest inner diameter of about 100 mm, and a porosity of about 46 vol%.
[0221] 3) Cylindrical sintered silicon carbide A powder having a D50 particle size of about 150 μm is sintered at a temperature of about 2200° C. for about 5 hours to form a silicon carbide sintered body having an outer diameter of about 170 mm, a height of about 80 mm, and a porosity of about 43 vol%.
[0222] 4) Cylindrical polycrystalline silicon carbide block A polycrystalline silicon carbide block having an outer diameter of about 170 mm and a height of about 80 mm.
[0223] 5) Cylindrical single crystal silicon carbide block A single crystal silicon carbide block having an outer diameter of about 170 mm and a height of about 80 mm.
[0224] 6) Silicon carbide powder Silicon carbide powder with a D50 particle size of approximately 150 μm.
[0225] Methods for producing silicon carbide ingots and wafers according to embodiments have improved growth rates and low defects.
[0226] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention. [Industrial Applicability]
[0227] The method for manufacturing a silicon carbide wafer and the method for manufacturing a silicon carbide ingot according to the embodiment can be applied to technical fields such as power semiconductors.
Claims
1. placing a silicon carbide block in a crucible; sublimating the silicon carbide contained in the silicon carbide block to form a silicon carbide ingot; processing the silicon carbide ingot; Including, A method for manufacturing silicon carbide wafers.
2. The silicon carbide block is 1 cm 3 having an apparent volume of at least The method for producing the silicon carbide wafer according to claim 1 .
3. The silicon carbide block has a thermal conductivity of 10 W / mK or more in at least one direction. The method for producing the silicon carbide wafer according to claim 1 .
4. A flow path is formed between the outer peripheral surface of the silicon carbide block and the inner surface of the crucible through which sublimated silicon carbide gas can move. The method for producing the silicon carbide wafer according to claim 1 .
5. The silicon carbide block is arranged so as to have a thermal conductivity of 10 W / mK or more in a horizontal direction. The method for producing the silicon carbide wafer according to claim 1 .
6. The silicon carbide block includes a flow path through which sublimated silicon carbide gas can travel. The method for producing the silicon carbide wafer according to claim 1 .
7. The flow path is open upward. The method for producing a silicon carbide wafer according to claim 6.
8. At least a portion of the flow path has an increasingly larger inner diameter going upward; The method for producing a silicon carbide wafer according to claim 7.
9. The flow path includes a first flow path having a first inner diameter; a second flow passage connected to the first flow passage and having a second inner diameter greater than the first inner diameter; Including, The second flow path is disposed on the first flow path. The method for producing a silicon carbide wafer according to claim 6.
10. The silicon carbide block is a first silicon carbide block disposed within the crucible; a second silicon carbide block disposed on the first silicon carbide block; Including, The method for producing the silicon carbide wafer according to claim 1 .
11. A flow path is formed between the first silicon carbide block and the second silicon carbide block through which sublimated silicon carbide gas can pass. The method for producing a silicon carbide wafer according to claim 10.
12. Silicon carbide powder is disposed in the flow path. The method for producing a silicon carbide wafer according to claim 11.
13. The silicon carbide block has a cylindrical, conical, donut or polygonal prism shape. The method for producing the silicon carbide wafer according to claim 1 .
14. The growth rate of the silicon carbide ingot is 250 μm / hr or more. The method for producing the silicon carbide wafer according to claim 1 .
15. the silicon carbide block comprises open porosity; The porosity of the silicon carbide block is 10 vol% to 50 vol%; The method for producing the silicon carbide wafer according to claim 1 .
16. placing a silicon carbide block in a crucible; placing a seed crystal in the crucible; growing the seed crystal by sublimating silicon carbide contained in the silicon carbide block; Including, A method for producing silicon carbide ingots.
Citation Information
Patent Citations
Method for growing silicon carbide single crystal by using high-density material block
CN102021653A
Method for manufacturing silicon carbide single crystal
JP2019156660A
Methods for forming SiC volume shapes and boules
JP2020515504A