Ball bond placement

A silver-based wire with a palladium/nickel-gold double-layer coating addresses galvanic corrosion in ball bond arrangements, ensuring high bond reliability through enhanced corrosion resistance.

JP2024538295AActive Publication Date: 2024-10-18HERAEUS MATERIALS SINGAPORE PTE LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024525562
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-11-23
Publication Date
2024-10-18
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

Existing ball bond arrangements using silver-based bonding wires with a gold-coated outer layer are prone to significant galvanic corrosion, leading to bond debonding issues, which are not effectively addressed by current methods.

Method used

A ball bond arrangement featuring a silver-based wire core with a double-layer coating of palladium or nickel (1-40 nm thick) and gold (20-500 nm thick) provides a gold coverage of 70-100% on the bonded ball surface, enhancing corrosion resistance and bond reliability.

Benefits of technology

The double-layer coating significantly reduces galvanic corrosion, ensuring high bond reliability by maintaining a substantial gold coverage on the bonded ball surface, as verified by SEM EDX analysis, thereby preventing bond debonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538295000001
    Figure 2024538295000001
  • Figure 2024538295000002
    Figure 2024538295000002
  • Figure 2024538295000003
    Figure 2024538295000003
Patent Text Reader

Abstract

1. A ball bond arrangement comprising a bond pad of a semiconductor device and a wire ball bonded to the bond pad, wherein the wire extending from the bonded ball has a diameter of 15-50 μm and comprises a silver-based wire core having a surface, the wire core having a coating layer superimposed on its surface, the coating layer being bilayer consisting of an inner layer of palladium or nickel having a thickness of 1-40 nm and an adjacent outer layer of gold having a thickness of 20-500 nm, and wherein the surface of the bonded ball has a gold coverage of 70-100%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ball bond arrangement that includes a bond pad of a semiconductor device and a wire that is ball bonded to the bond pad. Summary of the Invention [Problem to be solved by the invention]

[0002] Wire ball bonding is well known in the art. The first step of wire ball bonding is the formation of a free air ball (FAB) at the tip of a round bonding wire. The FAB formation is followed by the actual ball bonding procedure. The ball bonding of the FAB to the bond pad of a semiconductor device results in the formation of a so-called ball bond arrangement, or more precisely, a ball bond arrangement comprising the bond pad of the semiconductor device and the wire ball-bonded to the bond pad. The ball-bonded wire comprises a bonded ball that narrows towards its top, the bonded ball having a neck from which the wire extends with its original diameter. During the ball bonding procedure, the FAB is transformed into a bonded ball having a closed bell-like shape, the bottom of the closed bell having an interface with the bond pad and the wire extending from the top of the bell, i.e. the wire extends from said neck.

[0003] The term "bond pad" is used herein. It refers to a bond pad, especially a bond pad of a semiconductor device. The bond pad may consist of metal M or an alloy of metal M at more than 90% by weight, or may consist of a metal other than metal M with an outer metal M (alloy) top layer. Such a top layer may have a thickness of, for example, 0.5 to 1 μm. Metal M may be aluminum, gold, silver, copper, palladium or nickel, especially aluminum or nickel. The bond pad may have a total thickness of, for example, 0.2 to 4 μm.

[0004] Korean Patent No. 101687597(B1) discloses a silver-based bonding wire having an outer gold layer. When a FAB is formed in an air atmosphere at the tip of the gold-coated silver-based bonding wire, the gold content of the outer surface of the FAB is 5 to 35% by weight.

[0005] The applicant has found that ball bond arrangements of silver-based bonding wires having a gold-coated outer layer and ball-bonded to bond pads of semiconductor devices exhibit a significantly high gold coverage of 70-100% of the surface of the bonded ball when the bonding wire has an intermediate layer of nickel or palladium between the silver-based surface of the wire core and the gold-coated outer layer and when FAB formation is performed with a BSR (ball size ratio) (FAB diameter divided by wire diameter) in the range of 1.5-2.2. It is believed that the high gold coverage of 70-100% of the surface of the bonded ball forms the basis for significant galvanic corrosion prevention of the ball bond arrangement, or in other words, prevention of galvanic corrosion at the joints or ball bond interfaces of the ball bond arrangement. A beneficial consequence of the prevention of galvanic corrosion is the avoidance of bond debonding of the ball bond arrangement. The galvanic corrosion behavior of the ball bond arrangement can be tested by carrying out the so-called bHAST test (see "Test Method A" below).

[0006] Accordingly, the present invention relates to a ball bond arrangement, the ball bond arrangement comprising a bond pad of a semiconductor device and a wire ball bonded to the bond pad, the wire extending from the bonded ball has a diameter of 15-50 μm and includes a silver-based wire core having a surface, the wire core having a coating layer overlying the surface; the coating layer is a bilayer consisting of an inner layer of palladium or preferably nickel having a thickness of 1 to 40 nm, preferably 1.5 to 15 nm, and an adjacent outer layer of gold having a thickness of 20 to 500 nm, preferably 30 to 350 nm; The surface of the bonded ball has a gold coverage of 70% to 100%.

[0007] The term "surface of the bonded ball" is used herein to mean the entire surface of the bonded ball, i.e. the visible part of the surface of the bonded ball and the non-visible part of the surface (the bonded part, i.e. the bottom), in other words the bond interface between the visible part and the bond pad. It is self-evident that the visible part of the surface does not include the surface of the wire extending from the neck of the bonded ball.

[0008] The term "gold coverage of the surface of the bonded ball" is used herein. It is intended to mean the percentage of the surface area of ​​the bonded ball that is covered with gold. This percentage can be determined by performing a SEM EDX analysis (scanning electron microscope energy dispersive X-ray analysis) of the cross section of the ball bond arrangement (see "Test Method B" below). For this purpose, the bonded ball, i.e., the ball bond arrangement, is epoxy potted and mechanically cut transversely to the center of the ball bond, and then ion milled to obtain a scratch-free cross section. The ion milled cross section is observed with a SEM; the ion milled section is dot-mapped for gold with the aid of the energy dispersive X-ray attachment of the SEM. It can be performed, for example, at a magnification in the range of 200-5000x, preferably 800-1300x; an electron beam excitation voltage in the range of, for example, 5-30 kV, preferably 5-10 kV, and a constant current in the range of, for example, 30-950 pA, preferably 30-550 pA. Dot mapping for gold means looking for the spread of gold dots along the perimeter of the bonded ball, from the neck, over the visible and invisible parts of the surface on both sides of the bonded ball, i.e. it is looked for gold dots on the left, right and bottom of the bonded ball. If gold dots are present along the entire perimeter, the gold coverage of the surface of the bonded ball is 100%. The evaluation of the percentage of gold coverage is as follows: - Poor: Less than 70% of the perimeter of the bonded ball is covered with gold. + Good: 70%-100% of the circumference of the bonded ball is covered with gold.

[0009] A gold coverage of 70% to 100% correlates with significant resistance to galvanic corrosion of the ball bond arrangement, or in other words, significant resistance to galvanic corrosion at the joint or ball bond interface of the ball bond arrangement, and therefore correlates with good ball bond reliability.

[0010] The round wire, having a thickness of 15-50 μm, comprises a wire core (hereinafter also referred to as "core" for short) having a surface, the wire core having a coating layer superimposed on its surface, the wire core itself being a silver-based wire core, the coating layer being a bilayer consisting of an inner layer of palladium or preferably nickel having a thickness of 1-40 nm, preferably 1.5-15 nm, and an adjacent outer layer of gold having a thickness of 20-500 nm, preferably 30-350 nm.

[0011] The wire core is silver-based, i.e., the wire core is made of a silver-based material in the form of doped silver, a silver alloy, or a doped silver alloy.

[0012] As used herein, the term "doped silver" refers to a silver-based material consisting of (a1) silver in an amount ranging from greater than 99.49 to 99.997% by weight, (a2) at least one doping element other than silver in a total amount of 30 to less than 5000 ppm by weight, and (a3) ​​further components (components other than silver and the at least one doping element) in a total amount of 0 to 100 ppm by weight. In a preferred embodiment, the term "doped silver" as used herein means doped silver consisting of (a1) silver in an amount ranging from greater than 99.49 to 99.997% by weight, (a2) at least one doping element selected from the group consisting of calcium, nickel, platinum, palladium, gold, copper, rhodium and ruthenium in a total amount of 30 to less than 5000 ppm by weight, and (a3) ​​further components (components other than silver, calcium, nickel, platinum, palladium, gold, copper, rhodium and ruthenium) in a total amount of 0 to 100 ppm by weight.

[0013] The term "silver alloy" as used herein means a silver-based material consisting of (b1) silver in an amount ranging from 89.99 to 99.5 wt.%, preferably 97.99 to 99.5 wt.%, (b2) at least one alloying element in a total amount ranging from 0.5 to 10 wt.%, preferably 0.5 to 2 wt.%, and (b3) further components (components other than silver and the at least one alloying element) in a total amount ranging from 0 to 100 ppm by weight. In a preferred embodiment, the term "silver alloy" as used herein means a silver alloy consisting of (b1) silver in an amount ranging from 89.99 to 99.5% by weight, preferably 97.99 to 99.5% by weight, (b2) at least one alloying element selected from the group consisting of nickel, platinum, palladium, gold, copper, rhodium and ruthenium in a total amount ranging from 0.5 to 10% by weight, preferably 0.5 to 2% by weight, and (b3) further components (components other than silver, nickel, platinum, palladium, gold, copper, rhodium and ruthenium) in a total amount of 0 to 100 ppm by weight. Silver alloys containing palladium as the only alloying element, in particular silver alloys having a palladium content of 1 to 2% by weight, in particular 1.5% by weight, are most preferred.

[0014] The term "doped silver alloy" as used herein means a silver-based material consisting of (c1) silver in an amount ranging from greater than 89.49 to 99.497 wt%, preferably 97.49 to 99.497 wt%, (c2) at least one doping element in a total amount ranging from 30 to less than 5000 ppm by weight, (c3) at least one alloying element in a total amount ranging from 0.5 to 10 wt%, preferably 0.5 to 2 wt%, and (c4) further components (components other than silver, the at least one doping element and the at least one alloying element) in a total amount ranging from 0 to 100 ppm by weight, wherein the at least one doping element (c2) is other than the at least one alloying element (c3). In a preferred embodiment, the term "doped silver alloy" as used herein means a doped silver alloy consisting of (c1) silver in an amount of more than 89.49 to 99.497% by weight, preferably 97.49 to 99.497% by weight, (c2) at least one doping element selected from the group consisting of calcium, nickel, platinum, palladium, gold, copper, rhodium and ruthenium in a total amount of 30 to less than 5000 ppm by weight, (c3) at least one alloying element selected from the group consisting of nickel, platinum, palladium, gold, copper, rhodium and ruthenium in a total amount of 0.5 to 10% by weight, preferably 0.5 to 2% by weight, and (c4) further components (components other than silver, calcium, nickel, platinum, palladium, gold, copper, rhodium and ruthenium) in a total amount of 0 to 100 ppm by weight, wherein the at least one doping element (c2) is other than the at least one alloying element (c3).

[0015] The disclosure refers to "additional components" and "doping elements." The individual amount of any additional components is less than 30 ppm by weight. The individual amount of any doping elements is at least 30 ppm by weight. All amounts given in weight percent and ppm by weight are based on the total weight of the core or its precursor or elongated precursor member.

[0016] The wire core may contain so-called further components in a total amount ranging from 0 to 100 ppm by weight, for example from 10 to 100 ppm by weight. In this context, further components, often also referred to as "unavoidable impurities", are trace amounts of chemical elements and / or compounds resulting from impurities present in the raw materials used or from the wire core manufacturing process. A low total amount of further components of 0 to 100 ppm by weight ensures good reproducibility of the wire properties. The further components present in the core are usually not added separately. Each individual further component is contained in an amount of less than 30 ppm by weight, based on the total weight of the wire core.

[0017] The core of the wire is a homogeneous region of the bulk material. The properties of the core of the wire are understood as properties of the homogeneous region of the bulk material, since any bulk material always has a surface region that may exhibit somewhat different properties. The surface of this bulk material region may differ in terms of morphology, composition (e.g. sulfur, chlorine and / or oxygen content), and other characteristics. This surface is the interface region between the wire core and the coating layer superimposed thereon. Typically, the coating layer is completely superimposed on the surface of the wire core. In this region of the wire between the core of the wire and the coating layer superimposed thereon, a combination of materials of both the core and the coating layer may be present.

[0018] The coating layer superposed on the surface of the wire core is a bilayer consisting of an inner layer of palladium or preferably nickel having a thickness of 1-40 nm, preferably 1.5-15 nm, and an adjacent outer layer of gold having a thickness of 20-500 nm, preferably 30-350 nm. In this context, the term "thickness" or "coating layer thickness" refers to the size of the coating layer perpendicular to the longitudinal axis of the core.

[0019] In a preferred embodiment, the gold outer layer contains at least one element selected from the group consisting of antimony, bismuth, arsenic and tellurium in a total proportion ranging from 10 to 300 ppm by weight, preferably 10 to 120 ppm by weight, based on the weight of the wire (wire core + coating layer). At the same time, in one embodiment, the total proportion of at least one element selected from the group consisting of antimony, bismuth, arsenic and tellurium can be in the range of 300 to 3500 ppm by weight, preferably 300 to 2000 ppm by weight, based on the weight of gold in the gold outer layer.

[0020] It is preferred that antimony is present in the gold outer layer. It is even more preferred that antimony is present alone in the gold layer, i.e., bismuth, arsenic and tellurium are not present at the same time. In other words, in a preferred embodiment, the gold layer contains antimony in a proportion ranging from 10 to 300 ppm by weight, preferably 10 to 120 ppm by weight, most preferably 20 to 120 ppm by weight, based on the weight of the wire (wire core + coating layer), without the presence of bismuth, arsenic and tellurium in the gold layer, and at the same time, in an even more preferred embodiment, the proportion of antimony can be in the range of 300 to 3500 ppm by weight, preferably 300 to 2000 ppm by weight, based on the weight of gold in the gold layer.

[0021] In one embodiment, at least one element selected from the group consisting of antimony, bismuth, arsenic and tellurium may exhibit a concentration gradient within the gold layer, which gradient increases in a direction towards the wire core, i.e., perpendicular to the longitudinal axis of the wire core.

[0022] It is unclear in what chemical form or as what chemical species this at least one component is present in the gold layer, i.e., whether it is present in the gold layer in elemental form or in the form of a chemical compound.

[0023] A round coated wire having a thickness of 15 to 50 μm (i.e., a wire having a diameter of 15 to 50 μm and comprising a silver-based wire core having a surface, the wire core having a coating superimposed on its surface, the coating layer being bilayer, consisting of an inner layer of palladium or preferably nickel having a thickness of 1 to 40 nm and an adjacent outer layer of gold having a thickness of 20 to 500 nm) can be produced by at least the following steps (1) to (5): (1) preparing a silver-based precursor material; (2) elongating the precursor member until an intermediate diameter in the range of 30 to 200 μm is obtained to form an elongated precursor member; (3) applying onto the surface of the elongated precursor member obtained after completion of method step (2) a bilayer coating of an inner layer of palladium or preferably nickel and an adjacent outer layer of gold; (4) further stretching the coated precursor element obtained after completion of process step (3) until a desired final diameter is obtained and a bilayer is obtained consisting of an inner layer of palladium or preferably nickel having a desired final thickness in the range of 1-40 nm and an adjacent outer layer of gold having a desired final thickness in the range of 20-500 nm; (5) final strand annealing of the coated precursor obtained after completion of process step (4) at an oven set temperature in the range of 200-600° C. for an exposure time in the range of 0.4-0.8 seconds to form a coated wire; A method comprising: Step (2) may include one or more substeps of intermediate batch annealing the precursor component at an oven set temperature of 400-800° C. for an exposure time in the range of 50-150 minutes; It can be made by a method in which the application of the gold layer in step (3) is done by electroplating it from a gold electroplating bath.

[0024] A round coated wire having a thickness of 15 to 50 μm in a preferred embodiment thereof can be produced by the same method, except that the gold electroplating bath contains not only gold but also at least one element selected from the group consisting of antimony, bismuth, arsenic and tellurium.

[0025] The term "strand annealing" is used herein. It is a continuous process that allows high speed production of wire with high reproducibility. In the context of the present invention, strand annealing means that the annealing is performed dynamically while the coated precursor to be annealed is pulled or moved through a conventional annealing oven and wound on a reel after exiting the annealing oven. In this case, the annealing oven is typically in the form of a cylindrical tube of a given length. The annealing time / oven temperature parameters can be defined and set with a defined temperature profile of the annealing oven at a given annealing speed, which can be selected in the range of, for example, 10 to 60 meters / min.

[0026] The term "oven set temperature" is used herein. It means the temperature fixed in the temperature controller of the annealing oven. The annealing oven can be a chamber furnace type oven (for batch annealing) or a tubular annealing oven (for strand annealing).

[0027] The present disclosure distinguishes between precursor element, elongated precursor element, coated precursor element, coated precursor and coated wire. The term "precursor element" is used for a wire prestage that has not reached the desired final diameter of the wire core, while the term "precursor" is used for a wire prestage of the desired final diameter. After completion of method step (5), i.e. after final strand annealing of the coated precursor of the desired final diameter, a coated wire in the sense of the present invention is obtained.

[0028] The precursor member as provided in method step (1) is a silver-based precursor member, i.e., the precursor member is comprised of (a) doped silver, (b) a silver alloy, or (c) a doped silver alloy. See the preceding disclosure for the meaning of the terms "doped silver," "silver alloy," and "doped silver alloy."

[0029] In the embodiment of the silver-based precursor member, the silver-based precursor member can be obtained by alloying, doping, or alloying and doping silver with the desired amount of the required components. The doped silver or silver alloy or doped silver alloy can be prepared by conventional methods known to those skilled in the art of metal alloys, for example by melting the components together in the desired ratio. In this case, one or more conventional master alloys can be used. The melting method can be carried out, for example, by using an induction furnace, and is conveniently carried out under vacuum or in an inert gas atmosphere. The materials used can have a purity grade of, for example, 99.99% by weight or higher. The melt so produced can be cooled to form a homogenous piece of silver-based precursor member. Typically, such precursor members are in the form of rods having a diameter of, for example, 2 to 25 mm and a length of, for example, 2 to 100 m. Such rods can be made by continuous casting of the silver-based melt using a suitable mold, followed by cooling and solidification.

[0030] In method step (2), the precursor member is stretched until an intermediate diameter in the range of 30-200 μm is obtained to form an elongated precursor member. Techniques for stretching the precursor member are known and are considered useful in the context of the present invention. Preferred techniques include rolling, swaging, die drawing, and the like, of which die drawing is particularly preferred. In the latter case, the precursor member is drawn in several method steps until the desired intermediate diameter is reached. Such wire die drawing methods are well known to those skilled in the art. Conventional tungsten carbide and diamond drawing dies can be employed, and conventional drawing lubricants can be employed to assist in the drawing.

[0031] Step (2) of the method of the present invention may include one or more substeps of intermediate batch annealing the elongated precursor member at an oven set point temperature in the range of 400-800° C. for an exposure time in the range of 50-150 minutes. The optional intermediate batch annealing may be carried out, for example, with the rod drawn to a diameter of 2 mm and wound on a drum.

[0032] The optional intermediate batch annealing of method step (2) can be carried out under an inert or reducing atmosphere. Numerous types of inert and reducing atmospheres are known in the art and are used to purge annealing ovens. Of the known inert atmospheres, nitrogen or argon are preferred. Of the known reducing atmospheres, hydrogen is preferred. Another preferred reducing atmosphere is a mixture of hydrogen and nitrogen. A preferred mixture of hydrogen and nitrogen is 90-98% by volume nitrogen and correspondingly 2-10% by volume hydrogen, these volume percentages totaling 100% by volume. Preferred mixtures of nitrogen / hydrogen are equal to 93 / 7, 95 / 5, and 97 / 3 vol% / vol%, based on the total volume of the mixture, respectively.

[0033] In method step (3), a coating in the form of a bilayer coating of an inner layer of palladium or preferably nickel and an adjacent outer layer of gold is applied onto the surface of the elongated precursor member obtained after completion of method step (2), with the coating overlapping said surface.

[0034] The skilled person knows how to calculate the thickness of such a coating on the elongated precursor member, i.e. after the final elongation of the coated precursor member, which ultimately results in a coating with the layer thickness disclosed for the wire embodiment. The skilled person knows numerous techniques for forming a coating layer of material according to the embodiment on a silver-based surface. Preferred techniques are plating, such as electroplating and electroless plating, sputtering, ion plating, deposition of material from the gas phase, such as vacuum deposition and physical vapor deposition, and deposition of material from the melt. The palladium inner layer or the preferred nickel inner layer is preferably applied by electroplating.

[0035] The gold layer is applied by electroplating. Gold electroplating is carried out with the aid of a gold electroplating bath, i.e. an electroplating bath that allows a palladium or nickel cathode surface to be electroplated with gold. In other words, a gold electroplating bath is a composition that allows gold in elemental metallic form to be applied directly onto a palladium or nickel surface that is wired as a cathode. A gold electroplating bath comprises gold. The concentration of gold in the gold electroplating bath can be, for example, in the range of 8 to 40 g / l (grams per liter), preferably 10 to 20 g / l.

[0036] As already mentioned above, the gold electroplating bath may comprise at least one component selected from the group consisting of antimony, bismuth, arsenic and tellurium, where the gold electroplating bath is a composition that allows not only the deposition of elemental gold, but also the deposition of at least one component selected from the group consisting of antimony, bismuth, arsenic and tellurium in the gold layer. It is unclear what chemical species this at least one component is, i.e. whether it is present in the gold layer in elemental form or as a chemical compound. Such a gold electroplating bath can be made by adding a suitable chemical form of at least one of the above-mentioned components (e.g. compounds such as Sb2O3, BiPO4, As2O3 or TeO2) to an aqueous composition containing gold as a dissolved salt or salts. Examples of such aqueous compositions to which at least one component can be added are Aurocor® K24HF from Atotech, and Auruna® 558 and Auruna® 559 from Umicore. Alternatively, a gold electroplating bath can be used that already contains at least one component selected from the group consisting of antimony, bismuth, arsenic, and tellurium, such as, for example, MetGold Pure ATF manufactured by Metalor. The gold concentration in the gold electroplating bath can be, for example, in the range of 8 to 40 g / l (grams per liter), preferably 10 to 20 g / l. The concentration of the at least one component selected from the group consisting of antimony, bismuth, arsenic, and tellurium in the gold electroplating bath can be, for example, in the range of 15 to 1000 ppm by weight.

[0037] The electroplating application of the gold layer is carried out by guiding the palladium- or nickel-coated elongated precursor member, which is wired as a cathode, through a gold electroplating bath. The gold-coated precursor member thus obtained, exiting the gold electroplating bath, may be rinsed and dried before carrying out method step (4). As rinsing medium it is expedient to use water, but alcohol and alcohol / water mixtures are further examples of rinsing media. This gold electroplating, in which the palladium- or nickel-coated elongated precursor member is passed through the gold electroplating bath, may be carried out at a direct voltage, for example, in the range of 0.2 to 20 V, and at a current, for example, in the range of 0.001 to 5 A, in particular 0.001 to 1 A, or 0.001 to 0.2 A. Typical contact times may range, for example, from 0.1 to 30 seconds, preferably from 2 to 8 seconds. The current densities used in this context are, for example, from 0.01 to 150 A / dm 2 The gold electroplating bath may have a temperature in the range of, for example, 45 to 75°C, preferably 55 to 65°C.

[0038] The thickness of the gold coating layer can be adjusted as desired essentially via the following parameters: chemical composition of the gold electroplating bath, contact time of the elongated precursor member with the gold electroplating bath, current density. In this context, the thickness of the gold layer can generally be increased by increasing the concentration of gold in the gold electroplating bath, by increasing the contact time of the elongated precursor member, wired as a cathode, with the gold electroplating bath, and by increasing the current density.

[0039] In method step (4), the coated precursor element obtained after completion of method step (3) is further stretched until (4) the desired final cross section or diameter of the wire is obtained, having a bilayer consisting of an inner layer of palladium or preferably nickel having a desired final thickness in the range of 1-40 nm, preferably 1.5-15 nm, and an adjacent outer layer of gold having a desired final thickness in the range of 20-500 nm, preferably 30-350 nm. The technique for stretching the coated precursor element is the same stretching technique as described above in the disclosure of method step (2).

[0040] In process step (5), the coated precursor obtained after completion of process step (4) is final strand annealed at an oven set temperature in the range of 200-600° C., preferably 350-500° C., for an exposure time in the range of 0.4-0.8 seconds to form a coated wire. Process step (5) can be carried out under air or with a nitrogen or forming gas purging.

[0041] In a preferred embodiment, the final strand annealed coated precursor, i.e., the still hot coated wire, is quenched in water, which in one embodiment may contain one or more additives, e.g., 0.01-0.2 vol. % of additives. Quenching in water means cooling the final strand annealed coated precursor instantly or rapidly, i.e., within 0.2-0.8 seconds, from the temperature experienced in process step (5) to room temperature, e.g., by immersion or dripping.

[0042] After completion of method step (5) and optional quenching, the coated wire is complete and can be ball bonded to a bond pad of a semiconductor device.

[0043] The ball bond arrangement of the present invention may be produced by a method comprising the following steps (i) and (ii) as disclosed below. Thus, in one embodiment, the present invention provides a method for manufacturing a ball bond arrangement, comprising the following steps: (i) providing a semiconductor having a bond pad and a wire according to any of the previously disclosed embodiments; (ii) ball bonding the wire to the bond pad, the ball bonding comprising forming a FAB with a BSR in the range of 1.5 to 2.2; The present invention relates to a method comprising the steps of:

[0044] In step (i), a semiconductor having a bond pad and a wire according to any of the previously disclosed embodiments is provided, see above for methods for manufacturing such a wire.

[0045] In step (ii), the wire is ball-bonded to a bond pad of a semiconductor device. For this purpose, first a FAB is prepared at the tip of the wire by performing an electric flame-off (EFO) firing in an ambient atmosphere. It is essential to prepare the FAB with a BSR in the range of 1.5-2.2, preferably 1.6-2.0, and therefore it is possible to work with an EFO current in the range of, for example, 20-120 mA, preferably 40-70 mA, most preferably 40-50 mA, and an EFO time in the range of, for example, 75-1400 μs, preferably 140-550 μs, most preferably 140-350 μs, and a wand gap (distance between the EFO electrode tip and the broken wire tip) in the range of, for example, 625-1125 μm, preferably 700-900 μm. Examples of well known bonders include IConn-KNS bonders, Shinkawa bonders, and ASM bonders, to name just a few.

[0046] As already mentioned above, the ball bonding procedure itself, i.e. lowering the formed FAB into contact with the bond pads of the semiconductor device and ball bonding the wires, is well known to those skilled in the art and does not involve methodological peculiarities. A conventional ball bonding machine can be used, in particular one of the three well-known bonders disclosed above. The bonding process parameters can be, for example, a bonding force in the range of 22-30 g, an ultrasonic energy in the range of 78-94 mA, a temperature in the range of 170-250° C., a contact speed in the range of 6-20 μm / ms.

[0047] Wire Examples 98.5 wt. % silver (Ag) and 1.5 wt. % palladium (Pd), each exhibiting a purity of at least 99.99 wt. % ("4N"), were melted in a crucible. Wire-core precursors in the form of 8 mm rods were then continuously cast from the melt. The rods were then drawn in several drawing passes to form wire-core precursors having a circular cross-section with a diameter of 2 mm. These wire-core precursors were subjected to intermediate batch annealing at an oven setpoint of 500° C. for an exposure time of 60 minutes. The rods were further drawn in several drawing passes to form wire-core precursors having a circular cross-section with a diameter of 46 μm.

[0048] The wire core precursor was electroplated with an outer layer of gold according to Table 1.

[0049] In wire examples 1 and 2, the gold layer was electroplated directly onto the wire core precursor without pre-coating with a palladium or nickel inner layer. In wire examples where antimony was present in the gold layer, the wire core precursor, whilst wired as the cathode, was passed through a 61°C gold electroplating bath (based on MetGold Pure ATF from Metalor) with a gold content of 14.5 g / l, the antimony content of the various electroplating baths employed being in the range of 20-100 ppm by weight in each case.

[0050] For wire examples having a nickel inner layer, the wire core precursor was electroplated with a double layer coating of a nickel inner layer and an adjacent gold outer layer. To this end, the wire core precursor, while wired as a cathode, was passed through a nickel electroplating bath (containing 90 g / l (grams per liter) Ni(SO3NH2)2, 6 g / l NiCl2, and 35 g / l H3BO3) at 60°C, followed by a gold electroplating bath at 61°C.

[0051] All coated wire precursors were further drawn to a final diameter of 20 μm, followed by a final strand anneal at an oven set temperature of 430° C. for an exposure time of 0.6 seconds, after which the so-obtained coated wires were immediately quenched in an aqueous quenching solution (deionized water containing 0.07% by volume of a surfactant). The contact time of each wire with the aqueous quenching solution was 0.3 seconds.

[0052] Wire samples of all wires were bonded under ambient air atmosphere (T=20° C. and RH=50%) using an IConn-KNS bonder with the respective bonding parameters specified in Table 1. The FAB was lowered from a predefined height (tip of 203.2 μm) with a contact speed of 6.4 μm / ms onto an Al-0.5 wt.% Cu bond pad of a 16pSOP device (plastic small outline package device, i.e., a surface mount integrated circuit package well known in the semiconductor industry). Upon contact with the bond pad, a set of predefined bonding parameters (bond force of 30 g, ultrasonic energy of 90 mA, and bonding time of 15 ms) was applied to deform the FAB and form a bonded ball. After forming the bonded ball, the capillary was raised to a predefined height (kink height of 152.4 μm and loop height of 254 μm) to form a loop. After forming the loop, the capillary was lowered onto the lead to form a stitch. After forming the stitch, the capillary was raised and the wire clamp was closed to cut the wire, resulting in a defined tail length (254 μm tail extension length).

[0053] Test Method All tests and measurements were performed at T=20° C. and relative humidity RH=50%.

[0054] A. Biased highly accelerated stress test (bHAST) of ball bond configuration: Each wire sample was ball bonded to ten 16pSOP devices mounted on a strip. Each strip was epoxy molded and tested for reliability by performing standard highly accelerated stress tests in a HAST chamber at 130°C, 85% RH and +20V bias. The 16 bonded balls of each of the ten 16pSOP devices were daisy-chained and monitored for electrical resistance evolution. An increase in electrical resistance of 10% or more within 480 hours or sooner indicated device failure due to ball bond interconnect failure. Wire samples were indicated as passing the test if the electrical resistance remained constant over the entire test period of 480 hours.

[0055] Additionally, all bonded balls were examined under an optical microscope at 1000x magnification to check for any potentially detached bonded balls. For this purpose, the tested 16p SOP devices were carefully removed from the encapsulation and examined for detached bonded balls, i.e., mechanical integrity with the bond pads. Any detached bonded balls were indicative of an interfacial galvanic corrosion failure type.

[0056] B. SEM EDX analysis of cross section of ball bond arrangement: The ball bond arrangement was epoxy potted, mechanically cut transversely to the center of the ball bond, and then ion milled to obtain a scratch-free cross-section. The ion milled cross-section was observed with a SEM; the ion milled section was dot-mapped for gold with the aid of an energy dispersive X-ray attachment of the SEM, at a magnification of 1300x; an electron beam excitation voltage of 10 kV, a constant current of 250 pA, an aperture of 60 μm, and a working distance of 10 mm. Dot mapping for gold was performed by locating the spread of gold dots along the entire circumference of the bonded ball, from its neck to its left side, its right side, and its bottom. For this purpose, the X-ray counts of elemental gold were counted and imaged as gold dots; the accumulation of gold dots in the observed cross-sectional area confirmed the presence of elemental gold, while black areas indicated the absence of gold. The assessment of the percentage of gold coverage was as follows: - Poor: Less than 70% of the perimeter of the bonded ball is covered with gold. + Good: 70%-100% of the circumference of the bonded ball is covered with gold.

[0057] [Table 1]

Claims

1. 1. A ball bond arrangement comprising a bond pad of a semiconductor device and a wire ball bonded to the bond pad, the wire extending from the bonded ball has a diameter of 15-50 μm and includes a silver-based wire core having a surface, the wire core having a coating layer overlying the surface; the coating layer is a bilayer consisting of an inner layer of palladium or nickel having a thickness of 1-40 nm and an adjacent outer layer of gold having a thickness of 20-500 nm; A ball bond arrangement, wherein the surface of the bonded ball has a gold coverage of 70-100%.

2. 2. The ball bond arrangement of claim 1, wherein the gold outer layer comprises at least one element selected from the group consisting of antimony, bismuth, arsenic, and tellurium in a total percentage ranging from 10 to 300 ppm by weight based on the weight of the wire.

3. 3. The ball bond arrangement of claim 2, wherein the total percentage of the at least one element selected from the group consisting of antimony, bismuth, arsenic, and tellurium is in the range of 300 to 3500 ppm by weight based on the weight of the gold in the gold outer layer.

4. The ball bond arrangement of any one of claims 1 to 3, wherein the silver-based material of the wire core is doped silver, a silver alloy, or a doped silver alloy.

5. 5. The ball bond arrangement of claim 4, wherein said silver alloy includes palladium as the only alloying element.

6. The ball bond arrangement of any one of claims 1 to 5, wherein antimony is present in the gold outer layer.

7. 7. The ball bond arrangement of claim 1, wherein the bond pad is made of a metal M, an alloy of metal M with more than 90% by weight, or a metal other than metal M having an outer metal M (alloy) top layer, the metal M being aluminum, gold, silver, copper, palladium, or nickel.

8. A method for manufacturing a ball bond arrangement according to any one of claims 1 to 7, comprising the steps of: (i) providing a semiconductor having a bond pad and a wire having a diameter of 15-50 μm and including a silver-based wire core having a surface, the wire core having a coating layer disposed on the surface; the coating layer is a bilayer consisting of an inner layer of palladium or nickel having a thickness of 1-40 nm and an adjacent outer layer of gold having a thickness of 20-500 nm; (ii) ball bonding the wire to the bond pad, the ball bonding comprising forming a FAB with a BSR in the range of 1.5 to 2.

2.

9. 9. The method of claim 8, wherein the gold outer layer comprises at least one element selected from the group consisting of antimony, bismuth, arsenic, and tellurium in a total percentage ranging from 10 to 300 ppm by weight based on the weight of the wire.

10. 10. The method of claim 9, wherein the total percentage of the at least one element selected from the group consisting of antimony, bismuth, arsenic, and tellurium is in the range of 300 to 3500 ppm by weight based on the weight of the gold in the gold outer layer.

11. The method according to any one of claims 8 to 10, wherein the silver-based material of the wire core is doped silver, a silver alloy, or a doped silver alloy.

12. The method of claim 11 , wherein the silver alloy includes palladium as the only alloying element.

13. A method according to any one of claims 8 to 12, wherein antimony is present in the gold outer layer.

14. 14. The method of any one of claims 8 to 13, wherein the bond pad is made of a metal M, an alloy of metal M with more than 90% by weight, or a metal other than metal M having an outer metal M (alloy) top layer, the metal M being aluminum, gold, silver, copper, palladium or nickel.

Citation Information

Patent Citations

  • Bonding wire

    JP2004014884A

  • Noble metal-coated silver wire for ball bonding and manufacturing method of the same, and semiconductor device using noble metal-coated silver wire for ball bonding and manufacturing method of the same

    JP2019186246A

  • Noble metal-coated silver wire for ball bonding and manufacturing method of the same, and semiconductor device using noble metal-coated silver wire for ball bonding and manufacturing method of the same

    JP2019186248A

  • Insulated Wire

    JP2019504472A

  • Insulated Wire

    JP2019508882A