Method for preparing thermoplastic liquid crystal polymer
Thermoplastic LCPs with hydrogen-bonded segments address the reusability issue of permanent crosslinking by enabling melt processing and reversible actuation, facilitating reconfiguration and fusion into complex designs.
Patent Information
- Application Number
- JP2024521148
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-07
- Filing Date
- 2022-10-07
- Publication Date
- 2024-10-23
AI Technical Summary
Existing thermoplastic liquid crystal polymers (LCPs) are not reprocessable and reusable due to permanent crosslinking, limiting their versatility and compatibility with traditional processing methods.
Development of thermoplastic LCPs based on segmented copolymers containing thiourethane (TU), amide, or linear bismaleimide hard segments and liquid crystal soft blocks, utilizing hydrogen bonds to form a physically cross-linked network that allows for melt processing and thermal programming, enabling reversible actuation.
The new LCPs exhibit mechanical integrity, reversible shape change, and reprocessability, allowing for reconfiguration and fusion into complex designs, with applications in soft robotics and smart textiles.
Smart Images

Figure 2024538735000017 
Figure 2024538735000018 
Figure 2024538735000019
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for preparing a thermoplastic liquid crystal polymer, and to a segmented copolymer containing a thiourethane, amide, or linear bismaleimide hard segment and a liquid crystal soft block, and a thermoplastic liquid crystal elastomer (LCE) actuator containing the same. [Background technology]
[0002] Stimuli-responsive LCEs can perform fast and reversible actuation and are readily used as soft actuators in applications such as soft robots, smart textiles, microfluidics, and artificial muscles. Macroscopic mechanical responses occur in covalently cross-linked network thermosets from an ordered to a less ordered state. Thus, exposure of responsive LCEs to an external stimulus such as heat induces a contraction of the aligned mesogen-based network along the director field and an expansion perpendicular to it, inducing a macroscopic shape change. After removal of the stimulus, the initial molecular order is restored, resulting in recovery of the shape due to the cross-linked network. A proven method for preparing aligned LCEs is by first mechanically stretching a partially cross-linked material to induce alignment and then fully photocross-linking the polymer, which locks in the desired molecular orientation of the mesogens. Currently available materials exhibit large deformations, have good mechanical properties, and are sufficiently stable, but cannot be reprocessed and reused.
[0003] One strategy to overcome the inherent limitations of permanently crosslinked polymer networks is to use dynamic covalent bonds instead. Dynamic covalent networks have been reported that demonstrate a more versatile processability of the developed dynamic LCE networks. Rearrangement of the molecular structure of such covalently exchangeable networks is driven by chemical reactions that often require a catalyst. LCE actuators based on dynamic covalent networks can be fused and reprogrammed, while melt-processable LCE actuators with programmable molecular orientation offer new possibilities for further development of materials compatible with conventional processing methods using polymer melts.
[0004] An alternative strategy to avoid permanently crosslinked networks is by introducing supramolecular interactions as dynamic physical crosslinks. Among the potential supramolecular interactions, hydrogen bonding has emerged as one of the most attractive interactions, and hydrogen-bonded liquid crystal (LC) polymers capable of reversible actuation have become an emerging research area. However, to date, supramolecularly crosslinked LCE actuators have been prepared by multi-step synthesis, but simultaneously incorporated stimuli-responsive, reprogrammable, and reworkable properties have not been reported. Summary of the Invention
[0005] It is an object of the present invention to provide a thermoplastic actuating element by using a stimuli-responsive thermoplastic liquid crystal polymer.
[0006] The invention is characterized by the appended claims. This object is achieved by a thermoplastic LCE actuator based on a segmented copolymer containing a thiourethane (TU), amide, or linear bismaleimide hard segment, and a LC soft block.
[0007] We found that the TU segments contain hydrogen bonds that form a physically cross-linked network at room temperature, ensuring sufficient mechanical integrity and excellent mechanical properties. Higher temperatures restore the thermoplastic behavior of the material, allowing the preparation of LCE actuators by melt processing and thermal programming (Figure 1). Thermoplastic LCEs with soft LC oligomer blocks of different lengths were synthesized in one step, from which the effect of block copolymer composition on structure, mechanical properties, and actuation performance was evaluated. Direct incorporation of an azobenzene photoswitch allows the actuators to be reversibly actuated in response to light in air and water. In addition, the thermoplastic LCE materials can be not only reprocessed but also configured into different shapes that exhibit different deformations triggered by stimuli.
[0008] Thermoplastic actuating elements are melt-processable polymers that reversibly change their shape when exposed to a particular stimulus (e.g., heat or light). The invention includes methods for making and processing materials and compositions to achieve desired properties. Desired properties include the thermomechanical properties of the polymer (e.g., modulus and transition temperature), (meso)phase and transition temperature, to which stimuli (e.g., temperature or light) the elastomer responds, and the extent to which the elastomer changes its shape or generates work (actuation strain and stress).
[0009] The present method for producing liquid crystal thermoplastic polymers involves a sequential addition reaction in which a difunctional mesogenic oligomer (i.e., a short polymer having (meth)acrylate, thiol, alcohol, or amine end groups) is prepared by reacting at least a liquid crystal component with a difunctional thiol or amine component, followed by a segmented copolymer by reacting at least the difunctional mesogenic oligomer with a bisacrylamide, or bismaleimide, or an isocyanate with the difunctional thiol, alcohol, or amine component.
[0010] Thus, the present invention provides a method for preparing a thermoplastic liquid crystalline polymer, comprising the steps of: a) reacting a di(meth)acrylic mesogenic monomer with a difunctional thiol or amine component to prepare a mesogenic difunctional polymer; b) reacting the mesogenic difunctional polymer of a) with a bisacrylamide, an isocyanate, or a bismaleimide, and a difunctional thiol, alcohol, or amine component to prepare a thermoplastic liquid crystal polymer; The present invention relates to a method comprising the steps of:
[0011] Thus, the present invention relates to segmented thermoplastic liquid crystal polymers produced by sequential addition reactions, where the mesogenic bifunctional polymer represented by general formula (1), later referred to as the mesogenic segment, is prepared by reacting at least a liquid crystal bisacrylate or bismethacrylate component (X), and a bifunctional thiol or amine component (L1-Z1), and the copolymer represented by general formula (2), later referred to as the hard segment, is prepared by reacting at least a mesogenic bifunctional polymer (1), a bisacrylamide, isocyanate, or bismaleimide (Y), and a bifunctional thiol, alcohol, or amine component (L2-Z2).
[0012] [ka]
[0013] In one example, the thermoplastic liquid crystal polymer has a melting point of −100° C. to Tm, preferably a melting point of the mesogenic segments (T i ) less than T g Shows.
[0014] In one example, the thermoplastic liquid crystal polymer is T g and T m The melting point (T m,LC ) is shown.
[0015] In one example, a thermoplastic liquid crystal polymer is photoresponsive when either an azobenzene derivative or another chromophore is used partially or completely as the component represented by (X) in the mesogenic segment or added as an additive to an elastomer.
[0016] In one example, X is a mesogenic monomer containing at least two vinyl groups, two acrylic groups, or two methacrylic groups, or a combination of two of the aforementioned groups, where X is preferably: [ka] is selected from the group:
[0017] In one example, L1 and L2 are linking monomers, Z1 and Z2 are each a side group on the linking monomer, and L1, L2, Z1, and Z2 are preferably: [ka] is selected from the group:
[0018] In one example, Y is preferably [ka] The monomer is selected from the group consisting of:
[0019] The present invention will now be described in more detail. [Brief description of the drawings]
[0020] [Figure 1] We demonstrate the preparation of a supramolecularly cross-linked LCE actuator based on thermoplastic PTU as a melt-processable material. [Diagram 2] 1 shows the synthesis of segmented PTU LCEs S1-S5 using sequential addition reactions and corresponding compositions Sx. [Figure 3a] 1 shows a molecular representation of hydrogen-bonded TU segments in a segmented polythiourethane LCE. [Figure 3b]Figure 1 shows FTIR spectra of PTU LCEs S1-S5, showing the free and hydrogen-bonded TU amine and carbonyl stretching band regions as indicated by dashed lines. [Figure 3c] 1 shows the temperature dependent FTIR spectrum of compression molded PTU LCE S1. [Figure 4a] DMA storage modulus (E') and loss tangent (tan δ) profiles as a function of temperature for compression molded PTU S1-S5. [Figure 4b] 1 shows stress-strain curves at room temperature of compression molded PTU S1 to S5. [Figure 4c] 1D WAXS diffractograms of aligned PTU S1-S5 are shown. [Figure 4d] 2D WAXS diffractogram of PTU S1 before programming. [Figure 4e] 2D WAXS diffractogram of PTU S1 after programming. [Figure 5a] Images of LCE actuators S1-S5 (from left to right) at 30° C. and 110° C. are shown. [Figure 5b] The corresponding actuation strain as a function of temperature is shown. [Figure 5c] Shows an image of a PTU LCE S5 lifting an additional weight (5 g) when heated to 80° C. [Figure 5d] 1 shows the operational strain after cycling of PTU LCE S5 under load (5 g) from room temperature to 80° C. [Figure 5e] The thermal actuation of aligned LCEs S1-S5 under a constant bias stress (250 kPa) is shown. [Figure 5f] The maximum actuation strain ratio and the corresponding actuation work capacity for each LCE are shown. [Figure 6a] Images of operation in air are shown. [Figure 6b] Figure 1 shows the tip displacement of the actuator as a function of time in both air and water under UV (violet) and blue (blue) light illumination. [Figure 6c]Photoinduced trans-cis isomerization of azobenzene derivatives. [Figure 7a] The rework cycle of PTU LCE S5 is shown. [Figure 7b] The stress-strain curve at room temperature is shown. [Figure 7c] 1 shows the actuation strain as a function of temperature for pristine and reshaped samples. [Figure 7d] 13 shows the reprogramming of aligned LCE S5 into twisted ribbons as a function of temperature and the corresponding actuation. [Figure 8] FTIT spectra s1 to s5 of polydomain PTU LCE are shown. [Figure 9] 1 shows the C=OH-bond / C=Ofree ratio as a function of hard segment content. [Figure 10] DSC thermographs of PTU LCE S1 to S5 are shown. [Figure 11] Thermogravimetric profiles of PTU LCE S1 to S5 are shown. [Figure 12] Figure 2 shows a POM image of a programmed PTU LCE S5 under crossed polarizers. [Figure 13] 1D WAXS diffractograms of polydomain PTU LCEs S1-S5 are shown. [Figure 14] 2D WAXS diffractograms of polydomain PTU LCEs S1–S5 are shown. [Figure 15] Shown are 2D WAXS diffractograms of programmed PTU LCEs S1–S5. [Figure 16] Indicates PTU LCE. [Figure 17] The azimuthal profiles of 2D WAXS patterns at q = 1.43–1.46 nm−1 for PTU LCEs S1–S5 are shown. [Figure 18] 1D MAXS diffractograms of polydomain PTU LCE S1-S5 are shown. [Figure 19] 1 shows a synthetic pathway for photoresponsive PTU LCE. [Figure 20] FTIR spectrum of polydomain photoresponsive PTU LCE. [Figure 21a] 1 shows a DSC thermograph of the photoresponsive PTU LCE. [Figure 21b] 1 shows the TGA profile of the photoresponsive PTU LCE. [Figure 21c] DMA of the photoresponsive PTU LCE. [Figure 21d] 1 shows the stress-strain curves of the photoresponsive PTU LCE. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] To create supramolecularly crosslinked thermoplastic LCEs, main-chain LC polymers were prepared using sequential thiol-acrylate and thiol-isocyanate addition reactions. A one-pot method was used to synthesize segmented PTU materials with systematically altered LC soft segment lengths (Figure 2). First, thiol-functionalized LC oligomer soft segments were synthesized by a nucleophilic thiol-Michael addition reaction between a small excess of dithiol (1) and an equimolar mixture of diacrylate mesogens (2 and 3) in the presence of a phosphine catalyst (4). Subsequently, in the same flask, prepolymers were prepared by a base-catalyzed thiol-isocyanate addition reaction between the synthesized thiol-terminated oligomers and an aliphatic diisocyanate (5) mediated by an amine catalyst (6). In the final step, the prepolymers were reacted with a bifunctional thiol (7) to obtain linear LC PTUs. In our experiments, the nomenclature Sx of PTU LCEs indicates the calculated average length of the soft LC segments (Sx, i.e., the number of mesogens). The average length of the LC segment chains was controlled from 1 to 5 repeating (S1-S5) units by the stoichiometric ratio of dithiol and reactive mesogens obtained by theoretical calculation using the Carothers equation (Table S1). In contrast, the hard TU segment length was kept constant (Mn, theo=487 g mol-1). Moreover, as the soft segment length and content increase from 1 to 5 mesogens per segment, the TU segment content decreases from 31 to 10 wt%, respectively (Table S2). By precipitating the reaction mixture into cold diethyl ether, a series of white polymers was obtained in nearly quantitative yields. Of note, two different dithiols (1 and 7) were used to form the thermoplastic PTU LCE because the incorporation of only one dithiol in both segments dramatically reduced the degree of microphase separation and the properties of the materials.
[0022] For all materials synthesized, Fourier transform infrared spectroscopy (FTIR) confirmed the formation of polymers as indicated by the disappearance of thiol and isocyanate stretching bands at 2560 and 2270 cm-1, respectively. In addition, characteristic amine and carbonyl vibrations were observed for all materials indicating successful formation of the TU moiety. The observed number average molecular weights (85000-157000 g mol-1) and relatively low polydispersities (2.0-2.7) of all materials from gel permeation chromatography (GPC) indicate successful synthesis of polythiourethanes (Table S3).
[0023] The hydrogen-bonding properties of the PTU LCEs were investigated by FTIR spectroscopy (Fig. 3; Fig. 8). The extent of hydrogen bonding in the TU segments was assigned to the absorptions in the TU amine region (3200–3400 cm-1) and carbonyl region (1600–1800 cm-1) (Fig. 3b). The hydrogen-bonded (NH H-bond) and free (NH free) TU amine stretching bands were observed at 3315 and 3440 cm-1, respectively. The NH H-bond stretching bands appeared as sharp vibrations for all PTU LCEs, while the NH free could be weakly observed, indicating the formation of well-organized hydrogen-bonded TU segments. The well-ordered hydrogen-bonded (C=OH bond) and free (C=O free) carbonyl stretching bands of the TU segments were observed at 1638 and 1677 cm-1, respectively. As expected, the absorption of hydrogen-bonded TU amine and the carbonyl stretching vibrations increased consistently with increasing TU segment content from LCEs S5 to S1. In contrast, the absorption of free TU amine decreased with increasing TU segment content. The absorption band of hydrogen-bonded carbonyl groups is larger than that of free carbonyl groups, and the corresponding ratio (C=OH bond / C=O free) increases with TU segment content (Figure 9). These results suggest that the higher the TU segment concentration, the greater the degree of hydrogen bonding, and the shorter the LC segment length, the greater the degree of microphase separation between the LC and TU segments. Nevertheless, the prepared samples show strong hydrogen-bonding interactions acting as supramolecular physical bridges in the TU segments.
[0024] Upon heating the material, the hydrogen bonds remain largely unaffected up to 110 °C, as indicated by minor changes in the hydrogen bonded and free stretching bands (Figure 3c). However, at 120 °C, the spectrum shows a sudden drop in absorbance of the hydrogen bonded amine and the carbonyl stretching vibration associated with the onset of hydrogen bond dissociation. With further increase in temperature, the hydrogen bonded carbonyl peak gradually drops and shifts to higher wavenumbers until it completely disappears at 200 °C, accompanied by a gradual increase in the free carbonyl peak. Also, the hydrogen bonded amine vibration drops and shifts to higher wavenumbers. These findings hold true for all PTUs, revealing three characteristic temperatures. At temperatures below 120 °C, the hydrogen bonds are maintained, forming a physically crosslinked network, ensuring the mechanical stability of the material such that it preserves its shape and alignment upon thermal actuation. Conversely, between 120 °C and 200 °C, the hydrogen bonds are partially broken, allowing strain-induced alignment of the LCE that is fixed upon cooling due to the thermal reversibility of hydrogen bonds. Furthermore, physical crosslinks are almost completely absent at 200° C., ensuring melt processability (see below).
[0025] The thermal properties of the developed materials were evaluated using differential scanning calorimetry (DSC) and thermogravimetric analysis (TGA). The DSC thermograms show a transition ranging from -15 to -6 °C during heating, which was assigned to the glass transition temperature (Tg) of the LC segment (Table S4 and Figure 10). With increasing the LC segment chain length from S1 to S5, the Tg shifts to lower temperatures due to the decrease in physical crosslink density and increase in segment mobility of the LC segment. An endothermic melting peak (Tm) of the TU segment domain was observed from 164 to 177 °C. With increasing the TU segment content from S5 to S1, the area under Tm and therefore the enthalpy of the transition also increases. These results indicated the presence of distinct LC and TU segments in the PTU LCEs. Furthermore, an exothermic peak is observed for LCEs S3 to S5 around 35 °C, independent of the LC segment content. The TGA profiles revealed two transitions for all materials corresponding to the decomposition of the TU and ester moieties (Figure 11). The thermoplastic LCEs exhibited a 1% weight loss at approximately 245°C due to polymer decomposition, which is well above the processing temperature exhibiting the desired thermal stability.
[0026] Dynamic mechanical analysis (DMA) was performed to characterize the dynamic viscoelastic properties of the thermoplastic PTU LCEs (Table S4). In the thermograms, a storage modulus (E') inflection point and loss tangent (tan δ) peak maximum were observed at approximately 10 °C, corresponding to the α-relaxation of the LC segments (Figure 4a). Additionally, a shoulder was observed at approximately 40 °C for LCEs S3-S5. Between 65 °C and 150 °C, a rubbery plateau was observed. With increasing LC segment length and decreasing TU segment content from S1 to S5, the α-relaxation transition shifts to lower temperatures, and the magnitude of E' at the rubbery plateau region decreases consistently. This decrease in temperature and rubbery modulus results from a decrease in the concentration of TU segment domains acting as physical crosslinks. The onset of the melting transition of the crystalline TU segment domains is manifested by a clear increase in tan δ and a decrease in E' at higher temperatures, where the material enters the viscoelastic flow region. With further increase in temperature, the material exhibits viscous flow and loses elastic properties. The observed trends of α relaxation and melting temperature transitions are consistent with the Tg of the LC segment and the Tm of the TU segment obtained in DSC. Similar to the temperature-dependent FTIR measurements, the DMA temperature profile of tan δ shows that the developed material exhibits three distinct temperature regions. In the rubbery region, tan δ is constant, indicating that the physical crosslinks are maintained and the material acts as a covalently crosslinked system. In the viscoelastic flow region, the supramolecular network is partially destroyed, allowing strain-induced orientation of the material upon stretching, while at higher temperatures, due to viscous flow, it becomes melt processable.
[0027] To further study the mechanical properties and LC segment length effect, tensile tests were performed (Table S5). From the stress-strain curves, it is observed that Young's modulus decreases with increasing LC segment size from S1 to S5 (Figure 4b), which is consistent with the observed trend of rubbery plateaus in DMA. Furthermore, the plateau region in the stress-strain curves gradually lengthens with increasing LC segment length. The elongation at break increases and the tensile strength decreases accordingly. These observations arise from a lower concentration of physical crosslinking points in the material due to the relative decrease in TU segment content. The observed plateaus in the stress-strain curves are characteristic of LCEs, where the polydomain material is gradually oriented along the stretching direction, and are essential for the preparation of aligned LCEs, where the alignment is programmed.
[0028] To demonstrate the reversible shape morphing behavior of the developed thermoplastic PTU LCE, an aligned actuator was first prepared (Figure 1). Polydomain samples were obtained by compression molding the material at 200 °C, which is well above the melting transition and below the decomposition temperature. The compression molded polydomain samples were uniaxially stretched (ε = 100%) at room temperature and subsequently annealed at 130 °C for 30 min. Here, new physical crosslinks were formed as this temperature is just above the onset temperature of hydrogen bond dissociation. As the material is programmed at a higher temperature where the molecular order is pulled down, the stretched thermoplastic LCE spontaneously elongates upon cooling to room temperature. This is due to the LC segments spontaneously organizing into an ordered mesophase. After this process, the resulting aligned LCE appears transparent (Figure 1). Under polarized optical microscopy (POM), the stretched material exhibited birefringence, indicating alignment, when the sample was rotated 45° between crossed polarizers (Figure 12).
[0029] To verify the molecular orientation and segment organization, the aligned PTU LCEs were studied by wide-angle and medium-angle X-ray scattering experiments (WAXS and MAXS). It is important to note that the oriented samples were measured without any externally applied load. In the wide-angle diffractograms, multiple diffraction peaks at q = 10.2, 14.5, 17.2, and 21.3 nm-1, as well as amorphous halos, were observed due to scattering of the LC segment chains and TU segment moieties (Figure 4c). Decreasing the TU segment content from 31 wt% (S1) to 10 wt% (S5) resulted in weaker diffraction. These peaks therefore appear to correspond to scattering of the TU moieties, suggesting the formation of well-crystallized TU domains at higher TU segment contents and increased crystallinity of the LCEs. The diffraction peaks at q = 14.5 and 17.2 nm-1 correspond to d-spacings of 0.43 and 0.37 nm, respectively, which are assignable to the characteristic intermolecular spacing between TU moieties, orthogonal to the hydrogen-bonding direction. Both the meso-type soft segment chains and the TU hard segment moieties undergo strain-induced orientation upon stretching during the orientation process, as indicated by the stronger diffraction peaks in the diffraction profile of the aligned LCE (Fig. 4c) compared to the unaligned LCE (Fig. 13). The 2D WAXS diffractogram of the initial polydomain sample showed a ring-shaped isotropic pattern, suggesting a random orientation of the segmented domains (Fig. 4d; Fig. 14). In contrast, the wide-angle 2D X-ray diffraction pattern of the aligned LCE showed typical diffraction spots with orientation arrangement, orthogonal to the stretching direction (Fig. 4e; Fig. 15). These patterns arise from the associated scattering of well-oriented LC and TU domains, which is promoted by the director alignment of the aligned LCE. The aligned sample also exhibits a four-point pattern at an azimuth angle of 60° from the stretching direction due to scattering of the TU structures (Figure 16). It is believed that the TU moieties adopt a chevron shape that is oriented along the alignment direction upon stretching, which results in four-point scattering. The corresponding scattering peak was observed at q = 10.2 nm-1 (d = 0.62 nm), reflecting the characteristic length of the TU moieties.The above observations indicate that the material is aligned during the orientation process, resulting in anisotropic LCEs. Furthermore, the aligned LCEs show order parameters between 0.39 and 0.43 with the same degree of stretching during the orientation process (Figure 17). In contrast, the unaligned samples show a diffuse halo with very low orientational order, likely induced by sample handling. Note that the order parameter is a measure of the entire material, since the observed signals of the LC and TU segments overlapped. In the small-angle region of the medium-angle diffractogram, a peak is observed that originates from the interdomain spacing, due to the formation of a microphase-separated morphology (Figure 4f). As the LC segment length increases, the interdomain spacing of the microphase-separated segments increases from 12.6 nm to 22.4 nm for elastomers S1 and S5, respectively. On the other hand, as the LC segment length increases, the intensity of the signal is pulled down, since the relative amount of TU segments becomes smaller. Comparing the MAXS diffraction profiles before and after aligning the LCE showed similar interdomain spacing trends, indicating that the microphase-separated morphology is unaffected upon forming an oriented LCE (Figure 18). The obvious interdomain spacing indicates the formation of a well-defined microphase-separated structure consisting of LC domains and hydrogen-bonded TU domains, which act as reversible switching segments and supramolecular bridges, respectively, in the thermoplastic LCE.
[0030] Unbiased reversible shape changes of the oriented thermoplastic LCE were observed when it was heated and cooled between 30 and 110 °C, showing a maximum actuation strain ratio of 32% (Figure 5a, b). Heating above 130 °C results in the disappearance of the strain-induced orientation and the loss of the reversible actuation behavior. Therefore, the LCE is heated to a maximum temperature of 110 °C where the degree of hydrogen bonding is maintained (see above). In thermal cycling experiments, the LCE immediately contracted with the programmed director field when heated and fully recovered to its initial length upon cooling. Increasing the LC segment length from LCE S1 to S5 significantly increases the magnitude of the actuation strain. This is attributed to the higher LC content and the decrease in the stiffness of the material. This indicates that the LC segment content dominates the thermal actuation behavior. To demonstrate the immediate reversible response and lifting capability of the developed actuator, LCE S5 was repeatedly heated and cooled while loading various weights. The loaded actuator rapidly contracted when heated to approximately 80 °C and fully recovered to its initial length upon removal of the heat source (Figure 5c). Furthermore, the thermoplastic LCE actuator loaded with a weight of 5 grams exhibited fully reversible actuation over at least five heating-cooling actuation cycles, indicating the maintenance of the alignment and thermal stability of the supramolecular crosslinked actuator (Figure 5d; Video S1). As the load was increased from 5 grams to 30 grams, the actuation strain gradually decreased until finally the sample barely contracted (Video S2). Furthermore, the thermal actuation performance of the oriented thermoplastic LCE was characterized as a function of temperature during DMA when exposed to an initial bias stress of 250 kPa (Figure 5e). The observed actuation shows a similar trend and magnitude of actuation strain for all samples previously observed for unbiased actuation. In addition, the work capacity of the actuator was calculated by a maximum energy density of 102 kJ m-3, which corresponds to an actuation strain of 32% for LCE S5 (Figure 5f).
[0031] Light-driven actuation of the developed thermoplastic materials is demonstrated by the incorporation of an azobenzene photoswitch, which is often used in conventional LC polymer actuators. Again, similar to the one-pot synthesis described previously, a light-responsive LCE is synthesized based on PTU S5 (Table S6) by simply adding the azobenzene derivative 8 (3 mol%) together with the diacrylate mesogen (Figure 19). Polymerization was confirmed by GPC and FTIR (Table S7 and Figure 20).
[0032] Meanwhile, the thermal and mechanical properties were characterized by DSC, TGA, DMA, and tensile tests (Figure 21). The LCE film bends toward the light source upon irradiation with UV light (365 nm) in air due to the absorption of the azobenzene derivative (Figure 6a, Figure 6b; Video S3). The azobenzene derivative undergoes photoinduced isomerization from its rod-like trans state to a bent cis isomer via the absorption of UV light (Figure 6c). This trans-cis isomerization is accompanied by a disruption of molecular order due to conformational changes in the isomers, which converts the absorbed light energy into mechanical action by inducing anisotropic contraction and expansion with the molecular director. Due to the relatively high azobenzene content, a cis-trans gradient is generated throughout the film, causing the exposed surface to contract and result in macroscopic bending. After removing the UV light, the film partially unbends and then remains temporarily stable (Figure 6a, Figure 6b). This partial unbending motion is most likely the result of a photothermal effect. UV light absorption of the azobenzene chromophore leads to photothermal heating and contraction of the film, which reversibly expands to its temporary deformed state when the light is turned off. Photoinduced reverse isomerization of the trans azobenzene moiety can be immediately triggered by exposure to blue light (455 nm), resulting in mechanical relaxation and large bending back deformation. However, only after turning off the blue light does the film fully bend back to its initial state. This behavior can also be related to the photoabsorption of the azobenzene chromophore when exposed to blue light, which leads to photothermal heating of the film. Underwater actuation of the photoresponsive thermoplastic LCE demonstrates little photoinduced heating of the actuator because the generated heat is immediately lost to its surroundings, as indicated by the small bending back motion after removing both UV and blue light (Figure 6b; Video S4). In addition, the amplitude of deformation in water is smaller than in air, because the same light intensity is used for both surroundings, and the intensity of the incident light in air is higher due to the light absorption of water. These observations demonstrate that both photomechanical and photothermal effects contribute to the light-driven actuation of azobenzene containing PTU LCEs, with the former being the main driver enabling light-induced actuation both in air and water.
[0033] Finally, the dynamic properties of the hydrogen-bonding motifs can be exploited to reuse, reprogram, and fuse LCE materials, demonstrating the functional benefits of incorporating physical crosslinks. To demonstrate reusability, pristine films of PTU LCE S5 were cut into pieces and remolded up to two times (Fig. 7a). The reprocessed materials exhibited similar mechanical properties, as observed from the stress-strain curves, with increased elongation at break and tensile strength (Fig. 7b). Upon heating and cooling, the pristine and recycled materials exhibited the same actuation behavior (Fig. 7c). By reprogramming the shape of the aligned actuators, the materials could be reconfigured and actuated again, exhibiting different types of deformation. Twisted ribbons were obtained by twisting one end of the actuator while fixing the other end prior to thermal programming (Fig. 7d; Video S5). The reprogrammed actuators contract and untwist upon heating, accompanied by a slight bending of the sample. During cooling, the actuators restored their shape and conformation to their initial design. In addition, it has been shown that two programmed shapes can be fused together to form a single actuator. For example, the ends of a programmed strip and a twisted ribbon are fused vertically together to form a different shape that exhibits reversible temperature-triggered actuation (Video S6). The ease of reprogramming and fusion allows for the fabrication of more complex shape designs and associated deformations.
[0034] We successfully developed a new generation of melt-processable supramolecularly crosslinked LCEs based on segmented PTU and demonstrated processing methods to obtain actuators by molding and stretching. The formation of distinct TU domains imparts supramolecular crosslinks in the material through hydrogen bonding to achieve the desired mechanical stability during actuation, while the reversibility of hydrogen bonding allows for melt-processable materials with programmable molecular alignment. This approach is consistent with typical processing methods of thermoplastic polymers using polymer melts and allows for alignment of LCEs by enabling processability of the network upon heating. Upon heating, LCE actuators undergo reversible contraction capable of lifting a load. The material properties can be systematically controlled by varying the LC segment length. Reversible light-driven actuation in both air and water is achieved by incorporating azobenzene derivatives. Reprocessing of LCE films has been demonstrated, and reconfiguration of actuators into alternative shapes exhibiting different shape changes upon application of an external stimulus was achieved by reprogramming and fusing. We anticipate that these supramolecularly cross-linked LCEs will provide an innovative approach to (re)programmable and reusable stimuli-responsive materials. The properties of these LCEs can further be readily tuned and extended by the reactive LC chemistry toolbox that has been previously used to prepare covalently cross-linked LC polymers.
[0035] 4. Experimental Section Materials: 1,4-bis-[4-(3-acryloyloxypropyloxy)benzoyloxy]-2-methylbenzene (2) and 1,4-bis-[4-(6-acryloyloxyhexyloxy)benzoyloxy]-2-methylbenzene (3) were obtained from Merck. Dimethylphenylphosphine (4, 99%) and N,N-dimethylacetamide (DMAc, ≥99%) were purchased from Sigma-Aldrich. 2,2'-(ethylenedioxy)diethanethiol (1, ≥97%), hexamethylene diisocyanate (5, ≥98%), triethylamine (6, ≥99%), and 1,6-hexanedithiol (7, ≥97%) were purchased from Tokyo Chemical Industry Co., Ltd. (TCI). Diethyl ether (Et2O, ≥99.5%) was obtained from Biosolve. 4,4'-Bis(6-acryloyloxyhexyloxy)azobenzene (8, ≧95%) was obtained from Synthon. All reagents were used as received without further purification.
[0036] Synthesis procedure: A reaction vessel (100 mL) was charged with diacrylate mesogens 2 and 3 (50 wt%) in DMAc and stirred at 50° C. under an inert atmosphere until completely dissolved. The solution was cooled to room temperature and dithiol chain extender 1 was added with stirring followed by nucleophilic catalyst 4 (0.1 wt%). The resulting reaction mixture was allowed to react at room temperature for 2 hours. Diisocyanate 5 (50 wt%) in DMAc was then added immediately to the oligomer mixture followed by base catalyst 6 (0.1 wt%) and stirred at room temperature for 15 minutes. During this time the mixture became viscous and additional DMAc (30 wt%) was added to the prepolymer mixture. Dithiol 7 was then added dropwise and after addition was complete the reaction mixture was heated at 60° C. and allowed to react overnight. The crude mixture was poured into cold Et2O (500 mL) with vigorous stirring and the polymer was allowed to precipitate over time. The product was added to fresh Et2O (200 mL) and stirred overnight. The solvent was decanted and the final polymer was dried under vacuum at 40 °C to give a white solid (>97% recovery). The molar ratios and formulations of the synthesized thermoplastic PTU LCEs can be found in the Supplementary Information (Tables S1, S2). Photoresponsive PTU LCEs were synthesized following the same synthetic procedure by adding azobenzene derivative 8 together with diacrylate mesogens 2 and 3 into the mesogens in the first addition reaction step (Table S6 and Figure 19).
[0037] Characterization: FTIR spectra were recorded on a Varian 670 IR spectrometer equipped with an attenuated total reflectance (ATR) sampling accessory using a diamond crystal over the range of 4000-650 cm-1 with 50 scans per spectrum and a spectral resolution of 4 cm-1. All spectra were recorded at room temperature unless otherwise stated. The spectra obtained were processed by Varian Resolutions. Gel permeation chromatography (GPC) was performed on a Waters HPLC system equipped with a PSS PFG (8 × 50 mm, 7 μm) and two PFG linear XL columns (8 × 300 mm, 7 μm) in series. 1,1,3,3,3-hexafluoro-2-propanol (HFIP) at 35 °C and potassium trifluoroacetate (20 mM) were used as the mobile phase delivered at a flow rate of 0.8 mL min-1. Samples were prepared at room temperature in HFIP with potassium trifluoroacetate (20 mM) and toluene (20 mM). Molecular weights were determined using a refractive index detector against poly(methyl methacrylate) standards. DSC measurements were performed using a TA Instruments Q1000 DSC instrument with a sealed T-zero aluminum sample pan. All scans were performed with 10 ± 1 mg of polymer over the temperature range of -50 °C to 200 °C under nitrogen atmosphere at a heating and cooling rate of 10 °C min-1. A second heating and cooling cycle was used to determine the enthalpy and transition temperatures of all samples. TGA was performed with 4 ± 0.5 mg of polymer on a TA instruments Q50 instrument at a heating rate of 5 °C min-1 over the temperature range of 28 to 800 °C. DMA was performed in vertical tensile mode on a TA Instruments Q800 instrument with 8 × 5.3 × 0.4 mm3 (L × W × T) samples cut from the compression molded films. Thermographs were measured from -50°C to 250°C with a heating rate of 5°C min-1, a single oscillation frequency of 1 Hz, an amplitude of 10 μm, and a preload of 0.01 N. Stress-strain curves were obtained on a Lloyd-Ametek EZ20 tensile tester using a 500 N load cell. Strain was defined as (lL) / L, where L is the initial length and l is the length at a particular time.Dog-bone specimens with a cross-sectional area of 2 × 0.4 mm2 (W × T) were cut from the compression molded films and stretched uniaxially with a gauge length of 20 mm at an extension rate of 10 mm min-1 until fracture. X-ray scattering measurements were performed on a Ganesha experimental setup equipped with a Genix-Cu ultra-low divergence source generating X-ray photons of wavelength and flux of 0.154 nm and 1 × 108 photons s-1, respectively. Diffraction patterns were obtained using a Pilatus 300K silicon pixel detector with 487 × 619 pixels of 172 × 172 μm2. Silver behenate was used as a calibration standard. The sample-to-detector distance was 89 mm in the wide-angle (WAXS) configuration, whereas at the medium angle (MAXS), the detector was operated at 439.5 mm. The collected data was reduced and analyzed using custom Python scripts with the PyFAI software package. The D-spacing was calculated using the equation d=2π / q. The orientational order parameter was calculated from the diffraction patterns using the Kratky method. POM was performed with a Leica DM2700 M microscope and crossed polarizers.
[0038] Manufacturing procedure: First, the polymer was dried at 60°C for at least 1 hour before processing. The material was then uniformly loaded into a 20x40x0.1mm3 (LxWxT) mold and covered on both sides with polytetrafluoroethylene (PTFE) protective sheets (T=0.12mm). The mold was heated to 200°C in a Collin P200E press and subjected to 5 press cycles at 50 bar mold pressure. A final compression molding process was carried out at 100 bar and 200°C for 2 minutes, after which the mold was immediately quenched to room temperature to form a polydomain polymer film. Dogbone-shaped specimens with dimensions 35x2x0.4mm3 (LxWxT) were cut from the compression molded polymer film and uniaxially strained at room temperature using a custom-made stretching device until the elongation reached 100%. The strained specimens were then heated to 130°C for 30 minutes and subsequently cooled to room temperature while maintaining the strain. During cooling, the aligned samples were observed to spontaneously elongate beyond the initially applied strain. Finally, the aligned LCEs were annealed at room temperature for 48 hours before characterization and testing. For reuse, the films were cut into small pieces and compression molded according to the procedure described above. A torsional ribbon actuator was obtained by twisting one end of the aligned LCE while fixing the other end, then heating to 130 °C for 30 min and cooling to room temperature. Fusion was performed by overlapping the ends of the two actuators and heating to 200 °C for 2 min.
[0039] Actuation measurements: Thermal actuation measurements were performed by placing the aligned samples on a black anodized aluminum sheet on top of a hot plate. The samples were heated by gradually increasing the temperature from 30°C to 110°C in 10°C intervals. The samples were then cooled to room temperature. All samples were subjected to a complete heating and cooling cycle to erase the thermal history before the actuation measurements. Photographs were taken at each temperature using a camera (Olympus OM-D E-M10 Mark III) and the resulting images were analyzed using ImageJ. Weight-lifting tests were performed by attaching various weights to the samples using paper clamps (1.26g) and heating them to around 80°C using a heat gun. The actuation strain was measured with a TA Instruments Q800 DMA by monitoring the sample length as a function of temperature. Samples with dimensions of 8×1.3×0.3 mm (L×W×T) were measured in controlled force mode from −50° C. to 120° C. at a heating rate of 5° C. min-1 under an initial bias stress of 250 kPa (constant force). All samples were heated to 110° C. for 3 min before measurement to ensure that the thermal history was erased. Considering that the bias stress depends on the cross-sectional area of the sample, which changes during actuation, the corresponding work capacity was calculated from Eq. 1.
[0040] Working capacity=W / V=F_biasΔL / LWT=F_bias / WT·ΔL / L=σ_biasε_bias[kJ m^(-3)](1) Photo-actuation was performed by suspending the aligned film with dimensions of 19.11×1.52×0.23 mm (L×W×T) at a distance of about 10 cm from a collimated light source emitting at 365 nm (UV light, Thorlabs M365L2) or 455 nm (blue light, Thorlabs M455L3-C2). A LED driver (Thorlabs DC4104) was used to control the light intensity of the LEDs. Photo-actuation in air was performed at room temperature with the UV and blue light intensities set to 25.2 mW cm-2 and 34.5 mW cm-2, respectively. For photo-actuation in water, the sample was immersed in a transparent container of tap water at room temperature and irradiated with UV and blue light at intensities of 20.1 mW cm-2 and 28.5 mW cm-2, respectively. Photo-actuation was recorded using a camera (see above).
[0041] Figure 1. Preparation of supramolecularly crosslinked LCE actuators based on thermoplastic PTU as a melt-processable material. One-pot polymerization of monomers yields segmented block copolymers, and the resulting material is compression molded to yield polydomain films. Subsequent programming by stretching the material at elevated temperatures allows for a uniform director field (n).
[0042] Figure 2. Synthesis of segmented PTU LCEs S1–S5 using sequential addition reactions and corresponding compositions S. Blue rectangles and gray bars represent TU and LC segments, respectively.
[0043] Figure 3. a) Molecular representation of hydrogen-bonded TU segments in segmented polythiourethane LCEs. b) FTIR spectra of PTU LCEs S1-S5 showing the free and hydrogen-bonded TU amine and carbonyl stretching band regions as indicated by the dotted lines. c) Temperature-dependent FTIR spectrum of compression molded PTU LCE S1. Black arrows indicate the increase and decrease of vibrations upon heating.
[0044] Figure 4. a) DMA storage modulus (E') and loss tangent (tan δ) profiles as a function of temperature for compression molded PTU S1-S5. Black arrows indicate the corresponding axes. b) Stress-strain curves at room temperature for compression molded PTU S1-S5. c) 1D WAXS diffractograms of aligned PTU S1-S5. d) 2D WAXS diffractograms of PTU S1 before and e) after programming. White arrows indicate the alignment direction. f) 1D MAXS diffractograms of aligned PTU S1-S5.
[0045] Figure 5. a) Images of LCE actuators S1-S5 (left to right) at 30 °C and 110 °C. b) Corresponding actuation strain as a function of temperature. c) Image of PTU LCE S5 lifting an additional weight (5 g) when heated to 80 °C. d) Actuation strain after cycling of PTU LCE S5 with a load (5 g) from room temperature to 80 °C. Red and blue boxes correspond to heating and cooling of the actuator. e) Thermal actuation of aligned LCEs S1-S5 under constant bias stress (250 kPa). f) Maximum actuation strain ratio per LCE and corresponding actuation work capacity.
[0046] Figure 6a. Images of actuation in air: (i) the actuator at room temperature before irradiation with UV light (25.2 mW cm). (ii) -2 ) induced bending motion; (iii) the transient stable state of the actuator after removal of UV irradiation; (iv) blue light (34.5 mW cm -2a) induced bending back motion; (v) full bending back to the initial state after blue light is turned off. The actuator bends towards the light source when illuminated from the left side. b) Tip displacement of the actuator as a function of time in both air and water during UV (violet) and blue (blue) light illumination. Numbered regions correspond to images in a). c) Schematic of the reversible light-driven bending motion resulting from the light-induced trans-cis isomerization of an azobenzene derivative and the geometrical change of the azobenzene moiety in response to light. The grey and orange bars represent the LC and the photoresponsive azobenzene moiety, respectively. Exposure to UV light leads to a light absorption (i.e., cis-trans) gradient in the film, indicated by the darker orange color.
[0047] Figure 7. a) Reworking cycle of PTU LCE S5 showing cutting and reshaping of the film, b) stress-strain curves at room temperature, and c) actuation strain as a function of temperature for pristine and reshaped samples. d) Reprogramming of aligned LCE S5 into twisted ribbons and corresponding actuation as a function of temperature.
[0048] Table S1. Molar ratios of monomers used in the synthesis of thermoplastic PTU LCEs S1–S5.
[0049] [Table 1]
[0050] Table S2. Formulations of thermoplastic PTU LCEs S1–S5. The number of repeat units (n) of the LC and TU segment lengths obtained by theoretical calculation using the Carothers equation. The corresponding theoretical number average molecular weights (Mn,theo), and the contents of the LC and TU segments.
[0051] [Table 2]
[0052] Table S3. GPC results of thermoplastic PTU LCEs S1–S5.
[0053] [Table 3]
[0054] Figure 8. FTIT spectra s1–s5 of polydomain PTU LCEs.
[0055] Figure 9. C=O as a function of hard segment content H-bond / C=O free ratio.
[0056] Table S4. DSC and DMA results of thermoplastic PTU LCEs S1–S5.
[0057] [Table 4]
[0058] Figure 10. DSC thermographs of PTU LCEs S1–S5 showing the second heating run.
[0059] Figure 11. Thermogravimetric profiles of PTU LCEs S1–S5.
[0060] Table S5. Summary of mechanical properties of thermoplastic PTU LCEs S1–S5.
[0061] [Table 5]
[0062] Figure 12. POM image of programmed PTU LCE S5 under crossed polarizers. The crossed arrows indicate the polarizer direction (p) and the single arrow indicates the molecular director of the aligned material (n). Scale bar is 200 μm.
[0063] Figure 13. 1D WAXS diffractograms of polydomain PTU LCEs S1–S5.
[0064] Figure 14. 2D WAXS diffractograms of polydomain PTU LCEs S1–S5. The observed orientation is due to sample preparation and handling.
[0065] Figure 15. 2D WAXS diffractograms of programmed PTU LCEs S1–S5. The molecular director of the aligned materials is horizontal.
[0066] Figure 16. q = 1.00-1.05 nm for PTU LCE S1 -1 Azimuthal profile of the 2D WAXS diffractogram at .
[0067] Figure 17. q = 1.43-1.46 nm for PTU LCE S1-S5 -1 Azimuthal profile of the 2D WAXS pattern at 1000 nm. The order parameter was obtained by fitting a Kratky function to the azimuthal angle by a custom script.
[0068] Figure 18. 1D MAXS diffractograms of polydomain PTU LCEs S1–S5. An additional peak at q = 1.37 nm originates from the spacing between mesogens in the soft segments (d = 4.6 nm). -1 The longer the LC segment length of the sample, the stronger the signal.
[0069] Table S6. Molar ratios of monomers used in the synthesis of photoresponsive thermoplastic PTU LCEs.
[0070] [Table 6]
[0071] Figure 19. Synthetic route of photoresponsive PTU LCE.
[0072] Table S7. GPC results of photoresponsive PTU LCEs.
[0073] [Table 7]
[0074] Figure 20. FTIR spectra of polydomain photoresponsive PTU LCEs.
[0075] Figure 21. a) DSC thermograph, b) TGA profile, c) DMA, and d) stress-strain curve of the photoresponsive PTU LCE.
Claims
1. 1. A method for preparing a thermoplastic liquid crystalline polymer, comprising: a) reacting a di(meth)acrylic mesogenic monomer with a difunctional thiol or amine component to prepare a mesogenic difunctional polymer; b) reacting the mesogenic difunctional polymer of a) with a bisacrylamide, an isocyanate, or a bismaleimide, and a difunctional thiol, alcohol, or amine component to prepare the thermoplastic liquid crystal polymer; method.
2. In step a), a mesogenic bifunctional polymer represented by the general formula (1) is prepared by reacting at least a liquid crystal bisacrylate or bismethacrylate component (X) with a bifunctional thiol or amine component (L 1 -Z 1 In step (b), a copolymer represented by the general formula (2) is prepared by reacting the mesogenic bifunctional polymer (1) of step (a) with a bisacrylamide, isocyanate, or bismaleimide (Y) and a bifunctional thiol, alcohol, or amine component (L 2 -Z 2 ) with The method of claim 1. 【Chemistry 1】
3. X is a mesogenic monomer containing at least two vinyl groups, two acrylic groups, or two methacrylic groups, or a combination of two of said groups, The method of claim 2.
4. X is: 【Chemistry 2】 selected from the group The method according to claim 3.
5. L1 and L2 are linking monomers, and Z1 and Z2 are each a side group on the linking monomer; The method according to any one of claims 2 to 4.
6. L1, L2, Z1, and Z2 are: 【Chemistry 3】 selected from the group The method according to claim 5.
7. Y: 【Chemistry 4】 is a monomer selected from the group The method according to any one of claims 2 to 4.
8. The formula: 【Chemistry 5】 and a liquid crystal soft block according to During the ceremony, X is a liquid crystal bisacrylate or bismethacrylate moiety; (L 1 -Z 1 ) is a bifunctional thiol or amine moiety; (Y) is a bisacrylamide, an isocyanate, or a bismaleimide; (L 2 -Z 2 ) is a difunctional thiol, alcohol, or amine moiety; k is the average number of repeat units in the liquid crystal soft segment; m is the average number of repeat units in the hard segments; n is the average number of repeat units in the polymer; Segmented copolymers.
9. -100℃~T m T g , preferably the isotropy temperature (T i ) less than T g 9. The segmented copolymer of claim 8, wherein
10. T g and T m The melting point (T m 10. The segmented copolymer of claim 8 or 9, wherein the copolymer has a structure of:
11. A thermoplastic liquid crystal elastomer (LCE) actuator comprising the segmented copolymer of any one of claims 8 to 10.
12. 12. Preparation of the thermoplastic liquid crystal elastomer (LCE) actuator of claim 11 by melt processing and thermal programming.
Citation Information
Patent Citations
Preparation method of multi-shape memory material
CN113461941A
Systems and methods of creating liquid crystal polymers using stepped reactions
US20160009863A1
Liquid-crystal urethane compound, thermally responsive liquid-crystal polyurethane elastomer, and production method therefor
WO2017002681A1