Ferromagnetic powder composition and method for obtaining same
The use of an aqueous silicate coating and acidic treatment to convert it into silica, combined with bismuth(III) oxide and organic compounds, addresses the environmental concerns of organic solvent-based coatings in ferromagnetic powders, enhancing magnetic properties and performance.
Patent Information
- Application Number
- JP2024522205
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-15
- Filing Date
- 2022-10-17
- Publication Date
- 2024-10-23
AI Technical Summary
Existing ferromagnetic powder compositions rely on organic solvents for coating processes, which are environmentally unfriendly and may compromise the quality of the magnetic properties of soft magnetic iron-based core particles.
A ferromagnetic powder composition is developed using an aqueous silicate coating followed by an acidic treatment to convert the silicate into silica, which is then coated with bismuth(III) oxide and an organic compound, eliminating the need for organic solvents and enhancing magnetic properties.
The process results in a ferromagnetic powder composition with improved magnetic properties and reduced environmental impact, achieving comparable or better performance than traditional methods while using environmentally friendly materials.
Smart Images

Figure 2024538775000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to ferromagnetic powder compositions comprising soft magnetic iron-based core particles and methods for making same. [Background technology]
[0002] Soft magnetic composite (SMC) powders are known in the art and are based on soft magnetic, usually iron-based core particles with an electrically insulating coating on each particle. SMC parts are typically obtained by compacting insulating particles using known powder metallurgy compacting processes, typically with lubricants and / or known binders.
[0003] Two important properties of an iron core component are its magnetic permeability and core loss properties. The magnetic permeability of a material is a measure of its ability to magnetize or hold magnetic flux. Magnetic permeability is defined as the ratio of the induced magnetic flux to the magnetizing force or magnetic field strength. When a magnetic material is exposed to a varying magnetic field, energy losses occur due to both hysteresis and eddy current losses. Hysteresis losses (DC losses), which account for a large proportion of the overall core loss in most electric motor applications, are caused by the energy expenditure required to overcome the holding magnetic forces in the iron core components. The magnetic forces can be minimized by improving the purity and quality of the base powder, but most importantly by increasing the temperature and / or time of heat treatment (i.e., stress relief) of the components. Eddy current losses (AC losses) are caused by the generation of electric currents in the iron core components due to magnetic flux changes caused by alternating current (AC) conditions. Each individual iron-based particle must be more or less completely electrically insulated from the others to minimize eddy current losses. The level of electrical resistance required to minimize AC losses depends on the type of application (operating frequency), particle size distribution and component size.
[0004] EP 2252419 B1 discloses a ferromagnetic powder composition comprising soft magnetic iron-based core particles, the surface of which is The general formula: (1) R1 [(R1)x (R2) y (M2)] n O n-1 R1 (In the formula, - M2 is a central atom selected from Si, Ti, Al or Zr; -O is oxygen; -R1 is a hydrolyzable group; -R2 is an organic moiety, and at least one R2 contains at least one amino group; - n is the number of repeating units, and n = 2 to 20; x is 0 or 1; and y is 1 or 2), coated with a first phosphorus-based inorganic insulating layer and at least one organometallic layer located outside the first layer of a metal-organic compound in acetone having the formula: A metal or semi-metallic particulate compound having a Mohs hardness of less than −3.5 is attached to the at least one organometallic layer; the powder composition further comprises a particulate lubricant; and the metal or semi-metallic particulate compound is bismuth (III) oxide.
[0005] The fundamental problem of the coating process in EP 2252419 is the reliance on organic solvents for the coating process of the organometallic layer. The present invention aims at a solution to overcome this fundamental problem.
[0006] US Patent No. 10,741,316 discloses a ferromagnetic powder composition comprising soft magnetic iron-based core particles, the surface of which is coated with at least one phosphorus-based inorganic insulating layer and then at least partially coated with metal organic compound(s), the total amount of the metal organic compound(s) being 0.005-0.05% by weight of the powder composition, and the powder composition further comprising a lubricant.
[0007] Soileau et al., in US Pat. Nos. 4,601,753 and 4,601,765, tested the feasibility of contacting iron powder with silicates to improve the magnetic properties of the same uncoated iron powder.
[0008] The utilization of solvents to prepare coatings for metal powders is a problem in the state of the art. It is desired to provide a ferromagnetic powder composition comprising soft magnetic iron-based core particles that is produced in a more environmentally friendly manner compared to the methods used today, while at the same time not resulting in a lower quality of powder compared to the methods used today.
[0009] definition Before the present invention is disclosed and described in detail, it is to be understood that this invention is not limited to the particular configurations, process steps, and materials disclosed herein as such configurations, process steps, and materials may vary somewhat.
[0010] It should be noted that as used in this specification and the appended claims, the terms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.
[0011] As used herein, "powder" refers to a plurality of core particles that make up the powder. The core particles are made of a metal or metal alloy and typically have an oxide on the surface.
[0012] As used herein, "powder composition" refers to soft magnetic iron-based core particles and additional compounds, including any coatings, lubricants, and binders, applied to the core particles.
[0013] The core particles may have different sizes. The particles in the powder have a particle size distribution. Within this application, the particle size distribution is measured by weighing different sieve fractions according to ISO 4497:2020. The average particle size is then calculated from the particle size distribution according to ISO 9276-2:2014.
[0014] For bismuth(III) oxide particles, particle D 50 D 50is the median or median of the particle size distribution, which is the particle size value at 50% in the cumulative distribution. It is measured according to SS-ISO13320-1.
[0015] Soft magnetic iron-based core particles (11) are known in the art and are used in many applications. For the characterization of such soft magnetic iron-based core particles (11), in the context of the present application, the inventors have measured the following parameters as a measure of the functionality of the coating: Electrical Resistivity - A measure of how well a material resists electric current (µΩm). Maximum Permeability - A unitless measurement of the magnetization a material acquires in response to an applied magnetic field. Square toroid density - The density (g / cm) of the magnetic square toroids used to evaluate the magnetic properties 3 ). Magnetic Flux - The induction obtained for a given applied magnetic field (T). Total Core Loss - The total core loss (W / kg) obtained for a given induction and frequency. Transverse rupture strength (MPa) according to SS-EN ISO3325:2000 on a bar with dimensions TRS-30x12x6mm.
[0016] All parameters were compared with commercially available soft magnetic powder compositions and were generally found to be at least comparable to the results obtained using soft magnetic powder compositions found in the prior art. Summary of the Invention
[0017] In a first aspect and embodiments thereof, there is provided a ferromagnetic powder composition comprising soft magnetic iron-based core particles (11), At least 80 wt.% of the core particles (11) have a particle size distribution in the range of 20 to 1000 μm measured according to ISO 4497:2020; The surface of the core particle (11) is formed of a compound represented by the general formula (MO) α (SiO2) β (In the formula, -α is the moles of MO and β is the moles of SiO, with the β / α molar ratio in the interval 0.5 to 4.1; - at least partially coated with a first coating (12a) comprising an aqueous silicate of - M selected from Li, Na and K, - the first coating (12a) is in direct contact with the surface of the core particles (11) of ferromagnetic powder, the silicate is present in an amount of 0.02 to 1.0 wt. %, calculated based on the total weight of the ferromagnetic powder composition; and - a ferromagnetic powder composition, wherein the first coating (12a) is acid-treated with an aqueous acidic solution after forming the first coating (12a) on the iron-based core particles (11).
[0018] In a preferred embodiment of the ferromagnetic powder composition disclosed herein, M is potassium (K).
[0019] In a further preferred embodiment of the ferromagnetic powder composition, the aqueous acid solution is either aqueous phosphoric acid or aqueous nitric acid, most preferably aqueous phosphoric acid.
[0020] In one embodiment, the ferromagnetic powder composition has bismuth (III) oxide particles (14) deposited on the first coating (12a), the bismuth (III) oxide particles (14) having a D measured according to SS-ISO13320-1 at intervals of 0.1 to 10 μm. 50 has.
[0021] In an embodiment of the ferromagnetic powder composition, the core particle (11) further comprises a second coating (12b), the first coating (12a) on the core particle (11) being located between the core particle (11) and the second coating (12b), the second coating (12b) being formed from at least one insulating water-soluble organic molecule suitable for depositing as at least a monolayer on the first coating (12a).
[0022] In an embodiment of the ferromagnetic powder composition, the at least one insulating water-based organic molecule suitable for depositing as at least a monolayer on the first coating (12a) is The following general formula: (1) R1 [(R1) x (R2) y (M2)] n O n-1 R1 (Wherein, M2 is selected from the group consisting of Si, Ti, Al and Zr; O is oxygen; R1 is a hydrolyzable group; R2 is an organic moiety, at least one R2 containing at least one amino group; n is the number of repeat units, which is an integer from 1 to 20; x is 0 or 1; and and y is 1 or 2.
[0023] In an embodiment of the ferromagnetic powder composition, M2 is silicon (Si).
[0024] In an embodiment of the ferromagnetic powder composition, at least 80 wt% of the core particles are in the range of 20-75 μm as measured according to ISO 4497:2020.
[0025] In an embodiment of the ferromagnetic powder composition, at least 80 wt% of the core particles are in the range of 45 to 150 μm as measured according to ISO 4497:2020.
[0026] In an embodiment of the ferromagnetic powder composition, at least 80 wt% of the core particles are in the range of 75 to 380 μm as measured according to ISO 4497:2020.
[0027] In the second aspect and embodiments thereof, Next successive steps: a. preparing soft magnetic iron-based core particles (11); b. Soft magnetic iron-based core particles (11) represented by the general formula (MO) α (SiO2)β (In the formula, M is selected from Li, Na and K; with a first aqueous mixture containing a silicate (wherein α is the moles of MO and β is the moles of SiO, the β / α molar ratio being in the interval 0.5 to 4.1); thereby obtaining a first coating (12a) at least partially covering the core particle (11) which is in direct contact with the surface of the core particle (11), c. removing at least a portion of the water; d. reacting the silicate-coated soft magnetic iron-based core particles (11) with an acidic aqueous solution; Disclosed herein is a method for coating soft magnetic iron-based core particles (11) with an aqueous silicate solution, comprising the step of: the silicate being present in an amount of 0.02 to 1.0 wt %, calculated based on the total weight of the at least partially coated soft magnetic iron-based core particles.
[0028] In a particularly preferred embodiment of the method for coating the soft magnetic iron-based core particles (11) with an aqueous silicate solution, M is potassium (K).
[0029] In a third aspect and embodiments thereof, disclosed herein is a method for obtaining a ferromagnetic powder composition comprising the step of coating a powder comprising at least 80 wt.-% of soft magnetic iron-based core particles (11) having a particle size distribution in the range of 20-1000 μm measured according to ISO 4497:2020 using a method according to detailed aspects and embodiments herein, prior to a subsequent process step of drying and isolating the ferromagnetic powder composition.
[0030] In an embodiment of the method for obtaining a ferromagnetic powder composition, the method further comprises, prior to the next process step of drying and isolating the ferromagnetic powder composition, the further successive steps: e. Optionally, contacting the at least partially coated soft magnetic iron-based core particles from step c) with bismuth(III) oxide particles (14), wherein the D of the bismuth(III) oxide particles (14) measured according to SS-ISO13320-1 is 50 are steps with intervals of 0.1 to 10 μm, f. optionally, removing at least a portion of the water; g. A particle having the general formula: (1) R1 [(R1) x (R2) y (M2)] n O n-1 R1 (Wherein, M2 is selected from the group consisting of Si, Ti, Al and Zr; O is oxygen; R1 is a hydrolyzable group; R2 is an organic moiety, and at least one R2 contains at least one amino group; n is the number of repeat units, which is an integer from 1 to 20; x is 0 or 1; and y is 1 or 2; Equipped with.
[0031] In an embodiment of the method for obtaining a ferromagnetic powder composition, M2 is silicon (Si).
[0032] In a fourth aspect and embodiments thereof, there is provided a method of producing an object from a ferromagnetic powder composition according to the present disclosure, comprising the steps of: h. taking the ferromagnetic powder composition from step f and mixing the ferromagnetic powder composition with at least one lubricant; i. optionally preheating the die to a temperature below the melting temperature of the added particulate lubricant; j. compressing the composition in the mold at a compression pressure in the range of 300 to 2000 MPa, preferably 400 to 1200 MPa; k. Removing the resulting green body; and l. Heat treating the base material in a non-reducing atmosphere containing preferably 0 to 2.2 wt%, more preferably 0.5 to 2 wt%, O2 at a temperature in the range of 300 to 800 ° C, preferably 400 to 750 ° C, more preferably 600 to 700 ° C. A method is detailed herein comprising: [Brief description of the drawings]
[0033] [Figure 1] 1 is a schematic diagram of a partially coated particle of the present invention. [Diagram 2] Effect of acid concentration on magnetic properties. [Diagram 3] Effect of acid concentration on suspension turbidity. [Figure 4] Effect of acid concentration on suspension turbidity, comparison of phosphoric and nitric acids. [Diagram 5] SEM and EDS images of iron-based powder coated with potassium silicate, scale 100 μm. [Figure 6] SEM and EDS images of iron-based powder coated with potassium silicate, scale 5 μm. [Figure 7] SEM and EDS images of iron-based powder coated with potassium silicate, A: scale 250 μm, B: scale 100 μm. [Figure 8] SEM and EDS images of iron-based powders coated with potassium silicate treated with different concentrations of H3PO4, scale 25 μm. [Figure 9] SEM and EDS images of iron-based powders coated with potassium silicate treated with H3PO4 and subsequently added with B2O3 particles. [Figure 10] SEM and EDS images of iron-based powder treated with H3PO4, with B2O3 particles added later, and coated with potassium silicate with a top coating of Dynasylan®. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] It should be understood that the embodiments shown in the drawings are for the purpose of illustrating the invention and are not to be construed as limiting the invention. Unless otherwise indicated, the drawings are intended to be read together with the specification (e.g., cross-hatching, arrangement of parts, proportion, degree, etc.) and are to be considered part of the entire written description of the present disclosure. Detailed Description
[0035] In the present disclosure, all embodiments and aspects detailed herein rely on ferromagnetic powder compositions comprising soft magnetic iron-based core particles (11), as disclosed below: The surface of the core particle (11) is represented by the general formula (MO) α (SiO2) β (In the formula, -α is the moles of MO and β is the moles of SiO, with the β / α molar ratio in the interval 0.5 to 4.1; - at least partially coated with a first coating (12a) comprising an aqueous silicate of - M selected from Li, Na and K, - the first coating (12a) is in direct contact with the surface of the core particles (11) of ferromagnetic powder, The silicate is present in an amount of 0.02 to 1.0 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0036] To obtain a ferromagnetic powder composition suitable for the application contemplated herein, it is generally desirable for at least 80 wt. % of the core particles (11) to have a particle size distribution within the range of 20 to 1000 μm measured according to ISO 4497:2020, however, as will be readily understood by the skilled artisan, the particles are prepared in an aqueous solution and therefore any particle size and any particle distribution can be subject to coating using the present method according to the examples below, provided that appropriate adjustments for volume and concentration are undertaken in accordance with the common general knowledge of the skilled artisan.
[0037] In a first aspect and embodiments thereof, there is provided a ferromagnetic powder composition comprising soft magnetic iron-based core particles (11), At least 80 wt.% of the core particles (11) have a particle size distribution in the range of 20 to 1000 μm measured according to ISO 4497:2020; The surface of the core particle (11) is formed of a compound represented by the general formula (MO) α (SiO2) β (In the formula, -α is the moles of MO and β is the moles of SiO, with the β / α molar ratio in the interval 0.5 to 4.1; - at least partially coated with a first coating (12a) comprising an aqueous silicate of - M selected from Li, Na and K, - the first coating (12a) is in direct contact with the surface of the core particles (11) of ferromagnetic powder, the silicate is present in an amount of 0.02 to 1.0 wt. %, calculated based on the total weight of the ferromagnetic powder composition; and Disclosed herein is a ferromagnetic powder composition, wherein the first coating (12a) is acid-treated with an aqueous acidic solution after forming the first coating (12a) on the iron-based core particle (11).
[0038] In a preferred embodiment of the ferromagnetic powder composition, M is potassium (K).
[0039] As discussed in the examples presented herein, the ferromagnetic powders according to the present disclosure have a number of advantageous properties when compared to ferromagnetic powders known in the art. As shown in the examples detailed herein, upon acid treatment with an aqueous acidic solution, the silicate of the first coating (12a) undergoes a chemical change that makes it chemically different from the silicate coatings detailed elsewhere by Soileau et al. in U.S. Pat. Nos. 4,601,753 and 4,601,765.
[0040] In a further preferred embodiment of the ferromagnetic powder composition, the aqueous acid solution is either aqueous phosphoric acid or aqueous nitric acid, most preferably aqueous phosphoric acid.
[0041] Based on the experiments presented herein, it was possible to conclude that the aforementioned chemical changes in the presence of an aqueous acidic solution cause at least a partial reaction of the deposited silicate to form silica as the first coating. Furthermore, it was possible to conclude that under optimal reaction conditions, complete conversion of silicate to silica occurs under the influence of the aqueous acidic solution.
[0042] Based on the experiments shown herein, it was possible to define an internal standard comprising a test for when the silicate of the first coating (12a) is treated with an aqueous acid solution, for example preferably with phosphoric acid or nitric acid, most preferably with phosphoric acid, i.e. the silicate coated surface shows a significant increase in the detected level of at least one element characteristic of the aqueous acid solution used when the silicate coated surface is measured before and after the aqueous acid solution treatment, the detection being by energy dispersive spectroscopy (EDS), the measurements being made at a distance (working distance) of 10 mm using an acceleration voltage of 20 kV, a penetration depth of 1.5 μm and a detection area diameter of 1 μm, and the detection result of the detected level of the characteristic element is the average of at least four independent detections.
[0043] Because the coatings of Soileau et al. do not rely on further chemical modification, detection of an increased level of at least one element characteristic of the aqueous acid solution used is a sensitive measurement that distinguishes the present coatings from those of Soileau et al.
[0044] From the experiments, it was observed that the acid treatment and associated pH reduction results in the precipitation of nanosilica, which promotes the distribution of silicate into a complete coverage, as evidenced by turbidity measurements (see Example 12, Figures 3 and 4).The acid treated first coating is thus a covered silicate coating.
[0045] The acid treatment on the silicate surface reacts with cations (potassium ions (K) in the experiment) to form nano-sized patches. +It was observed that increasing the acid concentration caused a concentration of SiO2 / K2O in the underlying coating. These patches have a lower (SiO2 / K2O) ratio relative to the underlying coating between the patches. The patches eventually become smaller and better distributed as the acid concentration is increased, contributing to the observed beneficial effects on tribology (internal lubrication and protection from cold welding during compression) and finally completing the complete transition from silicate to silica.
[0046] Thus, in one embodiment, the first coating (12a) is an at least partial silica coating, hi that embodiment, the first coating (12a) is a fully formed silica coating.
[0047] Moreover, as observed in the experiments with phosphoric acid, many acids, after finally complete conversion of the silicate to silica, further react with potassium, thereby forming the observed K3PO4 nanocrystallites.
[0048] To that end, it is possible to define an internal test for the reaction of silicate to silica by comparing the EDS-measured content of alkali metal ions (in the experiments potassium (K)) in the patch after coating and before acid treatment with the content of alkali metal ions after acid treatment, as defined above (see Example 14), a decrease in the alkali metal ion content is decisive for the reaction of silicate to silicate, and the absence of a further decrease in the alkali metal ion content after a first decrease is decisive for the complete reaction of the silicate present on the coated core particles to silica.
[0049] The measured reductions on the patches (see Table 14) were 14.4 / 4.2-3.4 (8.5 g / l H3PO4) and 14.4 / 0.47-30.6 (75 g / l H3PO4) factors for the partially reacted and fully reacted surfaces, respectively.
[0050] In one embodiment, the core particle (11) comprises a partial first silica coating (12a) on the core particle (11) after aqueous acid treatment if the reduction in EDS-measured alkali metal content is reduced by at least a factor of two compared to the core particle (11) comprising the first silicate coating (12a) that has not been treated with the aqueous acid solution. As the proportion of partial first silica coating (12a) increases, the reduction in EDS-measured alkali metal content is reduced, preferably by at least a factor of three or four, prior to further coating with the second insulating coating (12b).
[0051] Thus, in an embodiment, the EDS measured alkali metal content is reduced by treatment of the first coating (12a) with an aqueous acidic solution.
[0052] In one embodiment, the ferromagnetic powder composition has bismuth (III) oxide particles (14) deposited on the first coating (12a), the bismuth (III) oxide particles (14) having a D measured according to SS-ISO13320-1 at intervals of 0.1 to 10 μm. 50 has.
[0053] In one embodiment of the ferromagnetic powder composition, the core particle (11) further comprises a second coating (12b), wherein the first coating (12a) on the core particle (11) is located between the core particle (11) and the second coating (12b), and the second coating (12b) is formed from at least one insulating water-soluble organic molecule suitable for depositing as at least a monolayer on the first coating (12a).
[0054] In one embodiment of the ferromagnetic powder composition, the at least one insulating water-based organic molecule suitable for depositing as at least a monolayer on the first coating (12a) is The following general formula: (1) R1 [(R1) x (R2) y (M2)] n O n-1R1 (Wherein, M2 is selected from the group consisting of Si, Ti, Al and Zr; O is oxygen; R1 is a hydrolyzable group; R2 is an organic moiety, at least one R2 containing at least one amino group; n is the number of repeat units, which is an integer from 1 to 20; x is 0 or 1; and and y is 1 or 2.
[0055] In one embodiment of the ferromagnetic powder composition, M2 is silicon (Si).
[0056] In one embodiment of the ferromagnetic powder composition, at least 80 wt% of the core particles are in the range of 20-75 μm as measured according to ISO 4497:2020.
[0057] In one embodiment of the ferromagnetic powder composition, at least 80 wt% of the core particles are in the range of 45 to 150 μm as measured according to ISO 4497:2020.
[0058] In one embodiment of the ferromagnetic powder composition, at least 80 wt% of the core particles are in the range of 75 to 380 μm as measured according to ISO 4497:2020.
[0059] In one embodiment of the ferromagnetic powder composition, the silicate is present in the ferromagnetic powder composition in an amount of 0.05 to 1.0 wt %, calculated based on the total weight of the ferromagnetic powder composition, and preferably the silicate is present in an amount of 0.10 to 0.5 wt %.
[0060] In one embodiment of the ferromagnetic powder composition, the potassium silicate is present in an amount of 0.1 to 0.6 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0061] In one embodiment of the ferromagnetic powder composition, the β / α molar ratio of the silicate is in the interval 2.5-4.1, preferably 2.9-3.5, more preferably 3.1-3.4.
[0062] In one embodiment of the ferromagnetic powder composition, the D of the bismuth (III) oxide particles (14) measured according to SS-ISO13320-1 50 are in intervals of 0.5 to 2 μm.
[0063] In one embodiment of the ferromagnetic powder composition, the bismuth (III) oxide particles (14) are present in an amount of 0.05 to 0.30 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0064] In one embodiment of the ferromagnetic powder composition, the bismuth (III) oxide particles (14) are present in an amount of 0.10 to 0.30 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0065] In one embodiment of the ferromagnetic powder composition, the bismuth(III) oxide particles are present in an amount of 0.10 to 0.25 wt %, and the metal organic compound is present in an amount of 0.10 to 0.25 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0066] In one embodiment of the ferromagnetic powder composition, the metal organic compound (13) is present in an amount of 0.15 to 0.30 wt %, preferably in the range of 0.10 to 0.25 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0067] In one embodiment of the ferromagnetic powder composition, potassium silicate is present in an amount of 0.10 to 0.30 wt %, calculated based on the total weight of the ferromagnetic powder composition, bismuth (III) oxide particles (14) are present in an amount of 0.10 to 0.20 wt %, and metal organic compound (13) is present in an amount of 0.10 to 0.20 wt %.
[0068] In one embodiment of the ferromagnetic powder composition, the metal organic compound is selected from the group consisting of alkoxy terminated amino silsesquioxanes, amino siloxanes, oligomeric 3-aminopropyl alkoxy silanes, 3-aminopropyl alkoxy silanes.
[0069] In one embodiment of the ferromagnetic powder composition, the metal organic compound is selected from the group consisting of N-aminoethyl-3-aminopropylalkoxysilane and N-aminoethyl-3-aminopropylmethylalkoxysilane.
[0070] In one particularly preferred embodiment of the disclosure, a ferromagnetic powder composition is disclosed herein comprising soft magnetic iron-based core particles (11), wherein at least 80 wt% of all of the core particles (11) are within the range of 20 to 1000 μm as measured according to ISO 4497:2020, and the surface of the core particles (11) is represented by the general formula (KO) α (SiO2) β wherein α is the moles of K2O and β is the moles of SiO2, the β / α molar ratio being in the interval of 0.5 to 4.1, the first coating (12a) being in direct contact with the surface of the core particles (11) of the ferromagnetic powder, and the silicate being present in an amount of 0.02 to 1.0 wt% calculated on the total weight of the ferromagnetic powder composition.
[0071] FIG. 1 shows a schematic cross-sectional view of a partially coated core particle (10). The dimensions of the coating and its components are greatly exaggerated relative to the core particle for illustrative purposes. It is intended to show the principle of the core particle (10) and the different layers. The labels exemplarily show a soft magnetic iron-based core (11); a first coating (12a); a second coating (12b); a metal-organic compound as defined in description (13); and a bismuth (III) oxide particle (14). As detailed in the experiments, the silicate acid reaction may proceed so that the silicate layer may be partially (as shown in FIG. 1) or completely coated with an acid-reacted silicate layer (not shown). As shown in the experiments, a completely coated with an acid-reacted silicate layer provides the greatest improvement in the magnetic properties of the particles and powders and is therefore preferred.
[0072] The size of the particles may vary widely, but experiments have shown that the present coating is suitable for any particle size, both fine and coarse.
[0073] A suitable size range for the core particles in the powder composition as determined by the end use is for the core particles to have an average size in the range of 20 to 1000 μm. The size of the core particles may suitably be and is measured herein in accordance with ISO 4497:2020, and the average size is suitably calculated from the particle size distribution as measured in accordance with ISO 9276-2:2014.
[0074] Once the iron-based core particle is in direct contact with the silicate-containing first coating (12a), the iron-based core (11) is at least partially coated and therefore some uncoated areas are present on the surface of the iron-based core (11).
[0075] This means that the spots may be on at least some of the core particles that are not covered by the first coating, and some of the core particles are completely coated by the first coating.
[0076] However, as shown in this experiment, when the acid silicate reaction proceeds to cessation, the intact silicate coating is primarily observed with optimal magnetic properties.
[0077] During the manufacture of the component from the ferromagnetic composition according to the invention, the entire iron-based core will be coated with the silicate layer according to the invention.
[0078] The iron-based core (11) treated with the aqueous silicate solution allows for the subsequent application of an insulating aqueous coating, thereby providing a ferromagnetic powder composition that is substantially free of organic solvents such as acetone.
[0079] The preferred silicate according to the invention is potassium silicate, or alternatively named K-silicate, K-water glass, potassium water glass or simply silicate herein. It has been demonstrated by the inventors that an aqueous mixture containing silicate may be applied directly onto the iron-based core. This is the first coating (12a) in the presented experiment according to the invention.
[0080] The technical effect is demonstrated in the examples, where potassium silicate was used.
[0081] This product can be considered an intermediate product, and further insulating aqueous coatings, such as acetone-free aqueous coatings, can be applied as subsequent layers.
[0082] The silicate has a molar ratio of 0.5 to 4.1. In one embodiment, the molar ratio β / α is in the interval from 2.50 to 3.75. In another embodiment, the molar ratio β / α is in the interval from 2.9 to 3.5. In a further embodiment, the molar ratio β / α is in the interval from 3.1 to 3.4.
[0083] The silicate is present in an amount of 0.02 to 1.0 wt%, calculated based on the total weight of the composition, which is the amount that shows the best effect as can be seen in the examples.
[0084] The amount of at least one silicate is calculated by the weight of the silicate relative to the weight of the entire ferromagnetic powder composition. When the ferromagnetic powder composition is produced, it is assumed that all the silicate becomes a coating on the metal particles. While this may be an estimate, following the method outlined in the examples, it has been found that the loss of material is so low that this estimate is good enough.
[0085] In another aspect, the inventors define a ferromagnetic powder composition according to the previous embodiment, wherein the surface of the core particle (11) is coated with a second coating (12b) outside the first coating, the second coating (12b) being i) a bismuth(III) oxide particle (14), and the D of the bismuth(III) oxide particle (14) measured according to SS-ISO13320-1 is 50 is 0.1 to 10 μm apart, and ii) bismuth (III) oxide particles (14) having the following general formula: (1) R1 [(R1) x (R2) y (M2)] n O n-1 R1 wherein M2 is selected from the group consisting of Si, Ti, Al, and Zr; O is oxygen; R1 is a hydrolyzable group; R2 is an organic moiety, and at least one R2 comprises at least one amino group; n is the number of repeat units, which is an integer from 1 to 20; x is 0 or 1; and y is 1 or 2.
[0086] In this embodiment, the ferromagnetic powder composition includes a second coating (12b). The second coating is on the outside of the first coating (12a). If the first coating (12a) does not cover the entire core particle, then the second coating is on both the outside of the first coating and the outside of the core particle (11). The second coating (12b) is in direct contact with the first coating. If the first coating (12a) does not completely cover the core (11), then the second coating (12b) is in direct contact with both the first coating (12a) and the core particle (11). Good performance and high resistivity of the resulting material are desired, then it is preferred that at least the second coating (12b) completely covers at least most of the core particles in the powder.
[0087] The second coating (12a) contains bismuth(III) oxide particles (14). 50 is measured according to SS-ISO13320-1. D of bismuth(III) oxide particles (14) 50 is in the range of 0.1 to 10 μm. Therefore, the bismuth(III) oxide particles (14) are smaller than the core particles (11).
[0088] The second coating (12b) also includes a metal organic compound (13). The metal organic compound has the following general formula: (1)R1[(R1) x (R2) y (M2)] n O n-1 Has R1.
[0089] R1 in the metal organic compound is, in one embodiment, an alkoxy group having less than 4, preferably less than 3, carbon atoms.
[0090] R2 is an organic moiety, which means that the R2 group comprises an organic part or moiety. R2 in one embodiment comprises 1-6, preferably 1-3 carbon atoms. R2 may further comprise one or more heteroatoms selected from the group consisting of N, O, S and P. The R2 group may be linear, branched, cyclic or aromatic. R2 may comprise one or more of the following functional groups: amine, diamine, amide, imide, epoxy, hydroxyl, ethylene oxide, ureido, urethane, isocyanato, acrylate, glyceryl acrylate, benzylamino, vinylbenzylamino. The R2 group may vary between any of the R2 groups of the mentioned functional groups and a hydrophobic alkyl group with repeatable units.
[0091] It was also not suitable for direct application onto the iron-based core as a water suspension. By providing a coating (12a), the inventors have made the surface of the iron-based core (11) suitable for application of bismuth (III) oxide particles (14) and metal-organic compounds (13).
[0092] According to this embodiment, the second layer (12b) comprises an oligomer of a metal-organic compound.
[0093] In one embodiment, the general formula (1) R1 [(R1) x (R2) y (M2)] n O n-1 The metal organic compound having R1 is at least one metal organic compound selected from the group consisting of N-aminoethyl-3-aminopropylalkoxysilane and N-aminoethyl-3-aminopropyl / methylalkoxysilane. These two metal organic compounds are secondary amines, which react slightly slower than, for example, primary amines.
[0094] In one embodiment of the ferromagnetic powder composition according to any one of the previous embodiments, at least 80 wt% of the core particles are in the range of 20-75 μm as measured according to ISO 4497: 2020. In the context of this disclosure, particles within this size range are considered to be fine sized or simply fine.
[0095] The size imparted to the particles makes them suitable for high frequency applications such as sensors, inductors, and converters. Example 6 shows that the coating is useful for such particles.
[0096] In one embodiment, in a ferromagnetic powder composition according to any of the other embodiments, at least 80 wt% of the core particles are in the range of 45-150 μm as measured according to ISO 4497: 2020. In the context of the present disclosure, particles falling within this size range are considered to be intermediate size or simply intermediate.
[0097] The size range of the intermediate size particles is suitable for low to medium frequency applications such as electric motors, generators, and converters. Examples 4 and 5 show that the coating works for these intermediate size particles.
[0098] In another embodiment, in a ferromagnetic powder composition according to any other embodiment, at least 80 wt% of the core particles are in the range of 75 to 380 μm as measured according to ISO 4497: 2020. In the context of the present disclosure, particles within this size range are considered to be coarse sized or simply coarse.
[0099] The size imparted to the particles is suitable for low frequency applications such as electric motors, generators, and actuators. Examples 1-5 and 7-10 show that the coating works for these relatively coarse particles.
[0100] In some embodiments, the preferred amounts of at least one of the silicate, the bismuth (III) oxide particles (14), and the metal organic compound (13) depend on the size of the core particles (11). Accordingly, some embodiments are shown with different average sizes of the core particles (11). The intervals of the different average sizes of the core particles are 20-75 μm, 45-150 μm, and 75-380 μm. The ranges overlap; however, they nevertheless provide a relative guide to the preferred ranges for the different components as fine particles, medium particles, and coarse particles, respectively.
[0101] In another embodiment, in a ferromagnetic powder composition according to any one of the previous embodiments, the silicate is present in the ferromagnetic powder composition in an amount of 0.05 to 0.5 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0102] It has been experimentally observed that these amounts of silicate are suitable for the present invention to function. Fine powders may require a relatively higher amount of silicate than coarse powders, and suitable amounts for different size powders are described in Examples 1, 2, 4, and 6. Average particle sizes above about 75 μm may require only 0.05-0.2 wt% silicate to form a complete coating, while finer average particle sizes may require higher amounts of silicate, such as 0.1-0.5 wt%, as would be expected based on their relative surface area ratios. Higher amounts of silicate can be used, but will not result in a higher coating that is more than adequately coated.
[0103] In another embodiment, in the ferromagnetic powder composition according to any one of the previous embodiments, the β / α molar ratio of the silicate is in the interval 2.5-4.1, preferably 2.9-3.5, more preferably 3.1-3.4.
[0104] Too low a molar ratio will cause poor coating quality and give poor electrical resistivity. Conversely, too high a molar ratio may destabilize the aqueous silicate solution and cause clumping precipitation, thus causing poor coating quality and poor electrical resistivity. By applying the silicate within the preferred interval, the coating quality has been found to be optimal.
[0105] In another embodiment, in the ferromagnetic powder composition according to any one of the preceding claims, the D of the bismuth(III) oxide particles (14) measured according to SS-ISO13320-1 50 are in intervals of 0.5 to 2 μm.
[0106] This amount of bismuth(III) oxide particles is in the preferred range because particles that are too coarse will cause poor distribution within the coating composition which in turn will give poor magnetic and / or mechanical properties, while particles that are too fine will tend to agglomerate and therefore be difficult to handle.
[0107] In another embodiment, a ferromagnetic powder composition according to any one of the previous embodiments is disclosed, wherein the bismuth(III) oxide particles (14) are present in an amount of 0.05 to 0.3 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0108] The amount of bismuth (III) oxide particles is in the preferred range, since too low an amount will give insufficient magnetic and mechanical properties, and too high an amount will mainly give low density and therefore poor magnetic properties. Powders with a fine particle size distribution are preferred over coarse powders (D 50 >70μm; 0.05~0.2wt%) with a higher amount (D 50 <70 μm; 0.15 to 0.3 wt%) may be required.
[0109] In another embodiment, there is disclosed a ferromagnetic powder composition according to any one of the previous embodiments, wherein the potassium silicate is present in an amount of 0.1-0.6 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0110] The amount of this silicate is in the preferred range because too low an amount cannot sufficiently cover the surface of the particles, causing rusting and poor magnetic properties, whereas too high an amount will cause low density and therefore poor magnetic properties (see Example 10).
[0111] In another embodiment, a ferromagnetic powder composition according to any one of the previous embodiments is disclosed, wherein the bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.30 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0112] In another embodiment, there is disclosed a ferromagnetic powder composition according to any one of the previous embodiments, wherein the bismuth(III) oxide particles are present in an amount of 0.10-0.25 wt %, and the metal organic compound is present in an amount of 0.10-0.25 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0113] This embodiment is a particularly preferred embodiment of the present disclosure as the spacing amounts encompass the most frequently used amounts for both fine and coarse iron-based core powders.
[0114] In another embodiment, a ferromagnetic powder composition according to any one of the previous embodiments is disclosed, wherein the metal organic compound (13) is present in an amount of 0.15-0.30 wt %, preferably in the range of 0.10-0.25 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0115] This embodiment is a particularly preferred embodiment of the present disclosure as the spacing amounts encompass the most frequently used amounts for both fine and coarse iron-based core powders.
[0116] In another embodiment, a ferromagnetic powder composition according to any one of the previous embodiments is disclosed, wherein the potassium silicate is present in an amount of 0.1-0.3 wt %, calculated based on the total weight of the ferromagnetic powder composition, the bismuth (III) oxide particles (14) are present in an amount of 0.10-0.20 wt %, and the metal organic compound (13) is present in an amount of 0.10-0.20 wt %.
[0117] In another embodiment, a ferromagnetic powder composition according to any one of the previous embodiments is disclosed, wherein the metal organic compound is selected from the group consisting of alkoxy terminated aminosilsesquioxanes, aminosiloxanes, oligomeric 3-aminopropylalkoxysilanes, 3-aminopropyl / propylalkoxysilanes.
[0118] The metal organic compounds are in one embodiment selected from derivatives, intermediates or oligomers of silanes, siloxanes and silsesquioxanes, or the corresponding titanates, aluminates or zirconates.
[0119] In another embodiment, a ferromagnetic powder composition according to any one of the previous embodiments is disclosed, wherein the metal organic compound is selected from the group consisting of N-aminoethyl-3-aminopropylalkoxysilane and N-aminoethyl-3-aminopropyl / methylalkoxysilane.
[0120] In one embodiment, the average size of the core particles is in the range of 20-75 μm as measured according to ISO 4497:2020, the at least one silicate comprises potassium silicate, the at least one silicate is present in an amount ranging from 0.10 to 1.0 wt%, the bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.30 wt%, and the metal organic compound is present in an amount of 0.15 to 0.30 wt%. Example 6 shows typical amounts of additives for a core powder containing relatively fine sized particles.
[0121] In one embodiment, the average size of the core particles is in the range of 45-150 μm measured according to ISO 4497:2020, potassium silicate is present in an amount of 0.1-0.6 wt%, bismuth(III) oxide particles (14) are present in an amount of 0.10-0.25 wt%, and metal organic compound (13) is present in an amount ranging from 0.10-0.25 wt%. Examples 4 and 5 show typical amounts for core powders containing intermediate size particles.
[0122] In one embodiment, the average size of the core particles (11) is in the range of 75 to 380 μm as measured according to ISO 4497:2020, the potassium silicate is present in an amount in the range of 0.05 to 0.3 wt %, the bismuth (III) oxide particles (14) are present in an amount of 0.10 to 0.20 wt %, and the metal organic compound (13) is present in an amount of 0.10 to 0.20 wt %.
[0123] The total amount of metal organic compound (13) in one embodiment is 0.05-0.6 wt %, preferably 0.05-0.5 wt %, more preferably 0.1-0.4 wt %, and most preferably 0.10-0.20 wt % of the ferromagnetic powder composition. In one embodiment, metal organic compound (13) is present in an amount in the range of 0.15-0.30 wt %, preferably in the range of 0.10-0.25 wt %. This is the amount of as-received liquid metal organic compound relative to the total weight of the powder composition.
[0124] In one embodiment, the bismuth(III) oxide particles are present in an amount of 0.10-0.25 wt %, calculated on the ferromagnetic powder composition, and the metal organic compound is present in an amount of 0.10-0.25 wt %, which is the amount of as-received liquid metal organic compound relative to the total weight of the powder composition.
[0125] In one embodiment, potassium silicate is present in an amount ranging from 0.10 to 0.30 wt %, bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.20 wt %, and metal organic compound (13) is present in an amount of 0.05 to 0.20 wt %.
[0126] The same embodiments disclosed and discussed above are equally applicable to the methods described below, however, some additional aspects related to these methods are discussed herein below.
[0127] In a second aspect and embodiments thereof, the method comprises the following successive steps: a. preparing soft magnetic iron-based core particles (11); b. Soft magnetic iron-based core particles (11) represented by the general formula (MO) α (SiO2) β of (In the formula, M is selected from Li, Na and K; with a first aqueous mixture containing a silicate (wherein α is the moles of MO and β is the moles of SiO, the β / α molar ratio being in the interval 0.5 to 4.1); thereby obtaining a first coating (12a) at least partially covering the core particle (11) which is in direct contact with the surface of the core particle (11); c. removing at least a portion of the water; d. reacting the silicate-coated soft magnetic iron-based core particles (11) with an acidic aqueous solution; Disclosed herein is a method for coating soft magnetic iron-based core particles (11) with an aqueous silicate solution, comprising the step of: the silicate being present in an amount of 0.02 to 1.0 wt %, calculated based on the total weight of the at least partially coated soft magnetic iron-based core particles.
[0128] In a particularly preferred embodiment of the method for coating the soft magnetic iron-based core particles (11) with an aqueous silicate solution, M is potassium (K).
[0129] In one embodiment of the method for coating the soft magnetic iron-based core particles (11) with an aqueous silicate solution, the aqueous acid solution is phosphoric acid or nitric acid, preferably phosphoric acid.
[0130] In one embodiment of the method for coating the soft magnetic iron-based core particles (11) with an aqueous silicate solution, steps b) and c) are repeated at least once.
[0131] In one embodiment of the method for coating the soft magnetic iron-based core particles (11) with an aqueous silicate solution, 0.05-0.5 wt % of silicate, calculated on the total weight of the ferromagnetic powder composition, is added in step b).
[0132] In one embodiment of the method for coating the soft magnetic iron-based core particles (11) with an aqueous silicate solution, the β / α molar ratio of the silicate is in the interval from 2.5 to 4.1, preferably from 2.9 to 3.5, more preferably from 3.1 to 3.4.
[0133] In that embodiment, the successive steps are: a. preparing soft magnetic iron-based core particles (11); b. Soft magnetic iron-based core particles (11) are formed into a compound represented by the general formula (KO) α (SiO2) β where α is the moles of KO and β is the moles of SiO, the β / α molar ratio being in the interval of 0.5 to 4.1, thereby obtaining a first coating (12a) at least partially covering the core particle (11) which is in direct contact with the surface of the core particle (11); c. Removing at least a portion of the water to obtain at least partially coated soft magnetic iron-based core particles (11) suitable for subsequent coating with an insulating aqueous coating; Disclosed herein is a method for coating soft magnetic iron-based core particles (11) with an aqueous silicate solution, comprising the step of: the silicate being present in an amount of 0.02 to 1.0 wt %, calculated based on the total weight of the at least partially coated soft magnetic iron-based core particles.
[0134] The method provides for obtaining an intermediate product, iron-based core particles coated with a first coating (12a), which provides a surface suitable for the application of subsequent coatings that are water-based but not acetone-based as used in the prior art.
[0135] The method may continue in a further step for the case in the next embodiment by applying a further coating with at least an aqueous liquid.
[0136] The core particles are provided uncoated with the first coating. No coating should be applied to the core particles prior to the first coating.
[0137] The core particles are contacted with a first aqueous mixture containing silicate. The silicate is preferably diluted in water to form an aqueous silicate solution with a suitable solid content. The silicate typically forms a polyion in the aqueous solution, and the silicate is distributed and adsorbed on the surface of the core particles. In most cases, essentially all of the silicate molecules are adsorbed on the surface of the core particles.
[0138] After the first coating, water is at least partially removed. It is considered that water typically remains in the powder composition as at least water of crystallization. In one embodiment, water is removed by stirring and heating in a mixer to which silicate is added. In one embodiment, water is removed by drying in a drying cabinet. Also, a combination of different methods of removing water is included. Also, other methods of removing water can be used.
[0139] The water in the composition is not necessarily completely removed. A small portion of water may remain. The water left in the powder composition can be both free water and water bound to various ions, forming hydrates and salts.In one embodiment, all water is removed.
[0140] In a further aspect and embodiment thereof, disclosed herein is a method for obtaining a ferromagnetic powder composition comprising coating a powder comprising at least 80 wt.-% of soft magnetic iron-based core particles (11) having a particle size distribution in the range of 20-1000 μm measured according to ISO 4497:2020 using a method according to detailed aspects and embodiments herein, prior to subsequent process steps of drying and isolating the ferromagnetic powder composition.
[0141] In an embodiment of the method for obtaining a ferromagnetic powder composition, the method further comprises, prior to the subsequent process steps of drying and isolating the ferromagnetic powder composition, the further successive steps of: e. Optionally, contacting the at least partially coated soft magnetic iron-based core particles from step c) with bismuth(III) oxide particles (14), wherein the D of the bismuth(III) oxide particles (14) measured according to SS-ISO13320-1 is 50 are steps with intervals of 0.1 to 10 μm, f. optionally, removing at least a portion of the water; g. A particle having the general formula: (1) R1 [(R1) x (R2) y (M2)] n O n-1 R1 (Wherein, M2 is selected from the group consisting of Si, Ti, Al and Zr; O is oxygen; R1 is a hydrolyzable group; R2 is an organic moiety, and at least one R2 contains at least one amino group; n is the number of repeat units, which is an integer from 1 to 20; x is 0 or 1; and y is 1 or 2; Equipped with.
[0142] In an embodiment of the method for obtaining a ferromagnetic powder composition, M2 is silicon (Si).
[0143] In an embodiment of the method for obtaining a ferromagnetic powder composition, step e) is included.
[0144] In an embodiment of the method for obtaining a ferromagnetic powder composition, step f) is included.
[0145] In an embodiment of the method for obtaining a ferromagnetic powder composition, both steps e) and f) are included.
[0146] In an embodiment of the method for obtaining a ferromagnetic powder composition, at least 80 wt. % of the core particles (11) provided are in the range of 20 to 75 μm measured according to ISO 4497:2020.
[0147] In an embodiment of the method for obtaining a ferromagnetic powder composition, at least 80 wt % of the core particles (11) are in the range of 45 to 150 μm measured according to ISO 4497:2020.
[0148] In one embodiment of the method for obtaining a ferromagnetic powder composition, at least 80 wt % of the core particles (11) are in the range of 75 to 380 μm measured according to ISO 4497:2020.
[0149] In one embodiment of the method for obtaining a ferromagnetic powder composition, the D of the bismuth(III) oxide particles (14) measured according to SS-ISO13320-1 50 are in intervals of 0.5 to 2 μm.
[0150] In one embodiment of the method for obtaining a ferromagnetic powder composition, the bismuth(III) oxide particles (14) are present in an amount of 0.05 to 0.30 wt %, preferably 0.10 to 0.30 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0151] In one embodiment of the method for obtaining a ferromagnetic powder composition, the silicate is present in an amount ranging from 0.10 to 1.0 wt%, preferably 0.10 to 0.6 wt%, calculated based on the total weight of the ferromagnetic powder composition.
[0152] In one embodiment of the method for obtaining a ferromagnetic powder composition, the metal organic compound (13) is present in the range of 0.15 to 0.30 wt %, preferably in the range of 0.10 to 0.25 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0153] In one embodiment of the method for obtaining a ferromagnetic powder composition, the bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.25 wt %, calculated based on the total weight of the ferromagnetic powder composition, and the metal organic compound (13) is present in an amount of 0.10 to 0.25 wt %.
[0154] In one embodiment of the method for obtaining a ferromagnetic powder composition, the silicate is potassium water glass and is present in an amount of 0.10 to 0.30 wt %, the bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.20 wt %, and the metal organic compound is present in an amount of 0.05 to 0.20 wt %.
[0155] In one embodiment of the method of obtaining a ferromagnetic powder composition, the metal organic compound is selected from the group consisting of alkoxy-terminated aminosilsesquioxanes, aminosiloxanes, oligomeric 3-aminopropylalkoxysilanes, 3-aminopropylalkoxysilanes.
[0156] In one embodiment of the method for obtaining a ferromagnetic powder composition, the metal organic compound is selected from the group consisting of N-aminoethyl-3-aminopropylalkoxysilane and N-aminoethyl-3-aminopropylmethylalkoxysilane.
[0157] Further, in one embodiment of the present specification, a method for obtaining a ferromagnetic powder composition is disclosed, comprising: The method further comprises the following successive steps: e. contacting the at least partially coated soft magnetic iron-based core particles from step c) with bismuth(III) oxide particles (14), wherein the D of the bismuth(III) oxide particles (14) measured according to SS-ISO13320-1 50 are steps with intervals of 0.1 to 10 μm, f. removing at least a portion of the water; g. A particle having the general formula: (1) R1 [(R1) x (R2) y (M2)] n O n-1 R1 (Wherein, M2 is selected from the group consisting of Si, Ti, Al and Zr; O is oxygen; R1 is a hydrolyzable group; R2 is an organic moiety, and at least one R2 contains at least one amino group; n is the number of repeat units, which is an integer from 1 to 20; x is 0 or 1; and y is 1 or 2; Equipped with.
[0158] Further, in one embodiment herein, a method for obtaining a ferromagnetic powder composition according to any one of the previous method embodiments is disclosed, the method comprising step d) of adding at least one acid after step c), the acid being selected from the group consisting of phosphoric acid and nitric acid. The effect of treating the powder with an acid, preferably diluted in water, is illustrated in the examples.
[0159] In another embodiment of the method, steps b) and c) may be repeated at least once.
[0160] In another embodiment of the method, at least 80 wt% of the provided core particles (11) are in the range of 20-75 μm measured according to ISO 4497:2020.
[0161] In another embodiment of the method, at least 80 wt% of the core particles (11) are in the range of 45 to 150 μm measured according to ISO 4497:2020.
[0162] In another embodiment of the method, at least 80 wt % of the core particles (11) are in the range of 75 to 380 μm measured according to ISO 4497:2020.
[0163] In an embodiment, a method according to any one of the previous embodiments, wherein 0.05-0.5 wt% of silicate, calculated based on the total weight of the ferromagnetic powder composition, is added in step b).
[0164] In an embodiment, a process according to any one of the previous embodiments is disclosed, wherein the β / α molar ratio is in the interval 2.5-4.1, preferably 2.9-3.5, more preferably 3.1-3.4.
[0165] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the D of the bismuth(III) oxide particles (14) measured according to SS-ISO13320-1 is 50 are in intervals of 0.5 to 2 μm.
[0166] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the bismuth(III) oxide particles (14) are present in an amount of 0.05 to 0.3 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0167] In an embodiment, a method according to any one of the preceding claims is disclosed, wherein the silicate is present in an amount in the range of 0.1-1.0 wt %, calculated on the total weight of the ferromagnetic powder composition.
[0168] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the bismuth(III) oxide particles (14) are present in an amount in the range of 0.10 to 0.30 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0169] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the silicate is potassium water glass in an amount ranging from 0.1 to 0.6 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0170] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.25 wt %, calculated based on the total weight of the ferromagnetic powder composition, and the metal organic compound (13) is present in an amount of 0.10 to 0.25 wt %.
[0171] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the metal organic compound (13) is present in the range of 0.15 to 0.30 wt %, preferably in the range of 0.10 to 0.25 wt %, calculated based on the total weight of the ferromagnetic powder composition.
[0172] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the silicate is potassium water glass and is present in an amount of 0.10-0.30 wt %, the bismuth(III) oxide particles (14) are present in an amount of 0.10-0.20 wt %, and the metal organic compound is present in an amount of 0.05-0.20 wt %.
[0173] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the metal organic compound is selected from the group consisting of alkoxy terminated aminosilsesquioxanes, aminosiloxanes, oligomeric 3-aminopropylalkoxysilanes, 3-aminopropyl / propylalkoxysilanes.
[0174] In an embodiment, a method according to any one of the previous embodiments is disclosed, wherein the metal organic compound is selected from the group consisting of N-aminoethyl-3-aminopropylalkoxysilane and N-aminoethyl-3-aminopropylmethylalkoxysilane.
[0175] In a further aspect and embodiment thereof, there is provided a method of producing an object from a ferromagnetic powder composition according to the present disclosure, comprising the steps of: h. taking the ferromagnetic powder composition from step f and mixing the ferromagnetic powder composition with at least one lubricant; i. optionally preheating the die to a temperature below the melting temperature of the added particulate lubricant; j. compressing the composition in the mold at a compression pressure in the range of 300 to 2000 MPa, preferably 400 to 1200 MPa; k. Removing the resulting green body; and l. Heat treating the base material in a non-reducing atmosphere containing preferably 0 to 2.2 wt%, more preferably 0.5 to 2 wt%, O2 at a temperature in the range of 300 to 800 ° C, preferably 400 to 750 ° C, more preferably 600 to 700 ° C. A method is detailed herein comprising:
[0176] In one embodiment, a method of producing an object from a ferromagnetic powder composition comprising the further steps of: g) taking the ferromagnetic powder composition from step f) and mixing the ferromagnetic powder composition with at least one lubricant; h) compressing the composition in the mold at a compression pressure in the range of 300 to 2000 MPa, preferably 400 to 1200 MPa; m. optionally, preheating the die to a temperature below the melting temperature of the added particulate lubricant; n. Removing the obtained green body; and o. Heat treating the base material in a non-reducing atmosphere containing preferably 0 to 2.2 wt%, more preferably 0.5 to 2 wt%, O2 at a temperature in the range of 300 to 800°C, preferably 400 to 750°C, more preferably 600 to 700°C. Disclosed herein is a method comprising:
[0177] After at least partial removal of the water, the ferromagnetic powder composition is contacted with bismuth (III) oxide particles. In one embodiment, this is done by dispersing the bismuth (III) oxide particles in water and adding the dispersion to the powder composition. In one embodiment, the powder composition is mixed in a mixer during and after the addition.
[0178] In another embodiment, the bismuth(III) oxide particles (14) may already be mixed and dispersed with the aqueous silicate solution and coated according to step b, followed by step c. Thus, step d may be omitted.
[0179] The powder composition is then mixed with a compound of general formula (1) R1 [(R1) x (R2) y (M)] n O n-1 The powder composition is contacted with a metal organic compound having R1. In one embodiment, the powder composition is mixed in a mixer at, during, or after the addition. Such continuous mixing has the advantage of a simpler manufacturing process. The bismuth (III) oxide particles and the metal organic compound form a second coating.
[0180] In one embodiment, the method comprises the step of adding at least one acid after step c), the acid being selected from the group consisting of organic acids and mineral acids. In one embodiment, the acid is selected from the group consisting of phosphoric acid and nitric acid. The selected acid is preferably diluted in a prior addition of water.
[0181] In one embodiment, steps b) and c) are repeated at least once, thereby applying two or more layers of the first coating, thereby increasing the probability that each individual core particle is completely covered by the coating.
[0182] In another embodiment, the molar ratio of the silicate solution is different, with the first layer applied in step b having a higher molar ratio than the second layer applied. This procedure may result in a first coating with improved particle coverage.
[0183] The powder composition is in one embodiment dried in step c) prior to step d), which improves application of the metal-organic compound for the second coating.
[0184] In one embodiment, the method comprises a further step comprising compacting the ferromagnetic composition into an object. In one embodiment, the method further comprises further successive steps for producing an object from the ferromagnetic powder composition: g) taking the ferromagnetic powder composition from step f) and mixing the ferromagnetic powder composition with at least one lubricant, h) compacting the composition in a mould at a compaction pressure in the range of 300-2000 MPa, preferably 400-1200 MPa, i) optionally pre-heating the mould to a temperature below the melting temperature of the added particulate lubricant, j) removing the resulting green body, and k) heat treating the green body at a temperature in the range of 300-800°C, preferably 400-750°C, more preferably 600-700°C in a non-reducing atmosphere, preferably nitrogen gas containing 0-2.2 wt%, more preferably 0.5-2 wt% O2 (oxygen gas).
[0185] This method step produces an object from the ferromagnetic powder composition.
[0186] In one embodiment, the lubricant is a particulate lubricant. The particulate lubricant allows compaction without the need to apply die lubrication. The particulate lubricant is, in one embodiment, at least one lubricant selected from the group consisting of primary and secondary fatty acid amides, transamides (bisamides) or fatty acid alcohols. The lubricating moiety of the particulate lubricant may be a saturated or unsaturated chain containing 12 to 22 carbon atoms. The particulate lubricant may be preferably selected from stearamide, erucamide, stearyl erucamide, erucyl-stearamide, behenyl alcohol, erucyl alcohol, ethylene-bisstearamide (i.e., EBS or amide wax). The particulate lubricant may be present in an amount of 0.15 to 0.80% by weight of the composition, preferably 0.20 to 0.40% by weight.
[0187] In one embodiment, the amount of lubricant added is less, e.g., 0.05-1.5 wt%, but compaction (steps m-o) is carried out using die lubrication (DWL), the benefit of which is improved compact density for a particular compaction pressure.
[0188] Thus, in a fourth aspect and embodiments thereof, there is provided a method of producing an object from a ferromagnetic powder composition according to the present disclosure, comprising the steps of: p. taking the ferromagnetic powder composition from step f. and mixing the ferromagnetic powder composition with at least one lubricant; q. optionally preheating the die to a temperature below the melting temperature of the added particulate lubricant; r. compressing the composition in the mold at a compression pressure in the range of 300 to 2000 MPa, preferably 400 to 1200 MPa; s. Removing the resulting green body; and t. Heat treating the base material in a non-reducing atmosphere containing preferably 0 to 2.2 wt%, more preferably 0.5 to 2 wt%, O2 at a temperature in the range of 300 to 800 ° C, preferably 400 to 750 ° C, more preferably 600 to 700 ° C. A method is detailed herein comprising:
[0189] A method for preparing a soft magnetic composite material according to the present invention comprises uniaxially compressing a composition according to the present invention in a die at a compression pressure of at least about 300 MPa, preferably at least 600 MPa; optionally preheating the die to a temperature below the dissolution temperature of the added particulate lubricant; removing the resulting green body; and optionally heat treating the green body.
[0190] Compaction may be cold die compaction, warm die compaction, or high speed compaction, preferably controlled die temperature compaction (50-120° C.) is used with unheated powder.
[0191] The heat treatment process may be in a vacuum, non-reducing, inert, or weakly oxidizing atmosphere, for example, 0.01-3 wt% oxygen. In one embodiment, a nitrogen atmosphere is used as the non-reducing atmosphere. In one embodiment, 0-2.2 wt% oxygen, preferably 0.5-2 wt% oxygen, is added. Optionally, the heat treatment is performed in an inert atmosphere and then quickly exposed to an oxidizing atmosphere to form a higher strength surface crust. The temperature may be up to 800° C. in one embodiment.
[0192] It is believed that the heat treatment conditions will allow the lubricant to evaporate as completely as possible. This is usually obtained during the first part of the heat treatment cycle, which is above about 300-500 °C. At higher temperatures, the metal or semi-metallic compounds may react with the metal-organic compounds and partially form a glassy network. This will further improve the mechanical strength and electrical resistivity of the part. At the highest temperatures (more preferably 600-700 °C), the compacts can reach complete stress relaxation, where the coercivity, and therefore the hysteresis losses of the composite, are minimized.
[0193] The first coating, i.e. the coating comprising at least one silicate, is utilized to prepare the powder for application of a further coating, which is applied from an aqueous solution or mixture. It has surprisingly been found that treatment with at least one silicate can prepare the powder for subsequent coating in an aqueous system.
[0194] In another embodiment, the general formula (KO) α (SiO2) β Disclosed is the use of at least one silicate with the formula: where α is the moles of KO and β is the moles of SiO, with a β / α molar ratio in the interval 0.5-4.1, as a first coating (12a), in direct contact with the surface of soft magnetic iron-based particles (14), thereby making the particles suitable for coating with aqueous chemicals or compounds substantially free of any organic solvents, which are often toxic, explosive or environmentally unfriendly.
[0195] Examples of additional coatings that can be applied after the first coating include, but are not limited to, metal salts dissolved in water.
[0196] The above embodiments can be combined with any of the above aspects. Furthermore, each of the above embodiments can be freely combined with one or more of the above embodiments.
[0197] The present invention is further illustrated by the following non-limiting examples, which serve the purpose of illustrating different embodiments of the invention without limiting the scope of the invention. EXAMPLES
[0198] (Example 1) The iron powder used had an apparent density of 3.2 g / cm 3 , D 50 was a 40 mesh water atomized annealed powder with a 200-250 μm spacing measured according to ISO 9276-2:2014. The powder has at least 80 wt% of core particles in the range of 75-380 μm measured according to ISO 4497:2020.
[0199] The powders were first coated with a coating containing potassium silicate (K12 from Sibelco Nordic AB) by adding an aqueous solution of potassium silicate in an amount of 0.05, 0.10, or 0.15 wt% calculated on the weight of the powder composition. The potassium silicate was a potassium silicate with a β / α molar ratio of 3.37. The dry weight of the potassium silicate was used to calculate the amounts. The coating was done with a coating solution consisting of water and potassium silicate. The coating solution was made by taking the potassium silicate solution with a solids content of 34.3 wt% as received and diluting it with water to a solids content of 14 wt%.
[0200] The coating solution was applied to the iron powder in the mixer, followed by mixing for 10 minutes, and the mantle was heated to 80° C. and mixing continued for 30-60 minutes until the powder appeared dry by visual inspection. It should be noted that even if the powder appears dry by visual inspection, water will likely remain, at least as water of crystallization and / or hydrate.
[0201] Further drying was done in a warming cabinet for 60-120 minutes at 120° C. Mixer and warming cabinet drying was done for all samples except sample number 1 which was not dried.
[0202] Then, the diluted phosphoric acid was added, phosphoric acid (85wt%) was diluted with water, and 0.50 or 0.75g phosphoric acid (85wt%) per kg of powder composition was mixed with water. 0, 3 or 10g of water per kg of powder composition was used for mixing with phosphoric acid. The resulting mixture of diluted phosphoric acid was added to the powder composition and then mixed. It was produced in a batch size of 1 kg in a laboratory mixer. The mixing time was 2 minutes.
[0203] Then, a mixture containing particles of Bi2O3 and H2O was added. 50 The particle size was 0.9 μm and was purchased from 5N Plus. The amount of particles was 1.0 g per kg of powder composition. The amount of water was in the interval 0-18 g per kg of powder composition. The powders were then mixed in the same mixer for 5 minutes.
[0204] Afterwards, for all samples except sample no. 6, a drying step was performed at 120° C. for 120 minutes.
[0205] Then, the formula (1) R1 [(R1) x (R2) y (M2)] n O n-1The oligomeric diamino-functional silane according to R1 was added in an amount of 1.5 g per kg of powder composition. The oligomeric diamino-functional silane was Dynasylan® 1146 from Evonik Industries AG, which is the preferred embodiment of the present disclosure. In this metal-organic compound, the central metal is silicon (Si).
[0206] The powders were then mixed in the same mixer for 2 minutes.
[0207] Then, 3 g of H2O was added per kg of powder composition. The powders were then mixed in the same mixer for 5 minutes.
[0208] After a drying step at 120°C for 60-120 minutes, the powder composition was utilized for production test samples.
[0209] The powder composition was mixed with 0.3 wt% lubricant (EBS) based on the total composition. The particulate lubricant was mixed into the coating powder using a paint shaker for 20 seconds and then in a windmill mixer for 10 minutes.
[0210] Compression was carried out at 800 MPa with a die temperature of 100°C.
[0211] The molded parts were heat treated in a belt furnace (all samples except sample numbers 8, 9 and 10) or a batch furnace (sample numbers 8, 9 and 10 only) in a nitrogen atmosphere with an oxygen level of 5000 ppm.
[0212] The belt furnace was operated between 450 and 670° C. with increasing temperature. Residence time for parts molded above 600° C. was approximately 20 minutes.
[0213] The batch furnace has three zones. The first zone had a temperature of 450° C. with a residence time of 30 minutes. The second zone had a temperature of 650° C. with a residence time of 25 minutes. The third zone was a cool-down zone.
[0214] The finished parts were subjected to various property measurements.
[0215] The density was measured using an automatic measuring fixture for the rings (measuring inner and outer diameters and height) and a balance.
[0216] The resistivity was measured on the completed magnetic square toroid by four-point method, with the distance between the measurement points being 20 mm. The specific electrical resistivity was measured on the square toroid sample by four-point measurement method.
[0217] For magnetic measurements, a square toroid was wrapped with 100 drive and 100 sense turns of resin-coated copper wire (diameter 0.63 mm) and measured using a Brockhaus MPG200D. Standards: IEC 60404-4 (DC measurements) and IEC 60404-6 (AC measurements).
[0218] The transverse strength TRS was measured according to SS-ENISO 3325:2000 on bars with dimensions of 30x12x6 mm.
[0219] The different experiments are summarized in Table 1 below.
[0220] Table 1a summarizes the amounts added in the different experiments. The amounts are given in g per kg of powder composition, except for potassium silicate, where the amounts are given in weight percentages (wt%).
[0221] Table 1b summarises the different results in the following columns:
[0222] A comparable commercial powder is Somaloy™ 700HR 5P, the properties of which are given in Table 1b.
[0223] From Table 1b it can be seen that the samples are comparable to the reference material considering all the properties listed in the table. It is concluded that the coating is useful for these relatively coarse particles. [Table 1a]
[0224] In the above table, experiments 1, 2, 5-7 and 9 are replicate experiments, and experiments 8 and 10 are different phosphate concentrations.
[0225] The initial poor reproducibility is noteworthy from the experiments. Further studies (see Examples 11 and 12) have shown that the silicate-coated iron-based particles react with the acid component and deposit partially or completely neutralized silicate on the surface of the iron-based particles, rather than creating a subsequent layer of solid mineral acid on the first deposited silicate layer.
[0226] In the prior art (see, for example, EP 2252419 B1), it was found that a phosphoric acid layer was formed directly on the metal surface of iron-based particles that had been subjected to a coating procedure using phosphoric acid in acetone.
[0227] Rather, as seen in this experiment, the acidic aqueous solution contributes to a partial or complete silicate coating on the core iron-based particles.
[0228] (Example 2) The iron powder used had an apparent density of 3.4 g / cm 3 , D 50 The powder was an annealed water atomized pure iron powder with a particle diameter in the 200-250 μm interval measured according to ISO 9276-2:2014. The powder has at least 80 wt% of the core particles in the range of 75-380 μm measured according to ISO 4497:2020.
[0229] The powders were first coated with a coating containing potassium silicate as defined in Example 1 by addition of an aqueous solution of potassium silicate (K12 from Sibelco Nordic AB) in an amount of 0.1 or 0.2 wt % relative to the total powder composition. The powders were then partially dried using the same method as in Example 1.
[0230] Phosphoric acid was then added. 0, 0.4, 0.75 or 1.5 g per kg of powder composition of phosphoric acid (85 wt%) was used. Phosphoric acid (85 wt%) was diluted with water. 0, 5 or 10 g per kg of powder composition of H2O was used to dilute phosphoric acid. The diluted phosphoric acid was added to the powder composition. Phosphoric acid was added to all samples except sample number 12, where 0.75 g per kg of powder composition of nitric acid (65%) was added, 10 g per kg of powder composition of H2O was used to dilute nitric acid, and no acid was added in sample numbers 17 and 20. The addition of acid and water was performed in a laboratory mixer with a batch size of 1 kg. The mixing time was 2 minutes. [Table 1b]
[0231] Then, a mixture containing Bi2O3 particles and H2O was added. 50 The particle size was 0.9 μm (submicron at 5N Plus). The amount of particles was 1 g per kg of powder composition. The amount of water was 17 g per kg of powder composition. The powders were then mixed in the same mixer for 5 minutes.
[0232] Then, an oligomeric diamino-functional silane was added in an amount of 1.5 g per kg of powder composition (Dynasylan® 1146). The powders were then mixed in the same mixer for 2 minutes.
[0233] Then, 3 g of H2O was added per kg of powder composition. The powders were then mixed in the same mixer for 5 minutes.
[0234] After a drying step at 120° C. for 60-120 minutes, the powder composition was utilized for production test samples.
[0235] The powder composition was compressed into parts as detailed in Example 1.
[0236] Table 2a summarizes the amounts added in the different experiments. The amounts are given in g per kg of powder composition, except for potassium silicate, where the amounts are given in wt%.
[0237] Table 2b summarizes the different results in the same units with respect to Table 1b.
[0238] A commercially available powder with a comparable size of core particles is Somaloy™ 700HR 5P, the properties of which are given in Table 2b.
[0239] In the experiments reported in Table 2a, for all samples except sample nos. 12, 17 and 20, phosphoric acid (85 wt%) was used. For sample no. 12, nitric acid (65%) was used. For sample no. 17 and sample no. 20, no acid was added. The first number indicates the amount of acid and the second number indicates the amount of water. In the later coatings with B2O3 and silane, the concentrations did not change between experiments. Concentrations in g / kg powder composition.
[0240] (Example 3) As an example of using different acids, we note that sample number 11 and sample number 12 were prepared similarly, but with concentrated phosphoric acid and concentrated nitric acid, respectively. As shown in Table 2b, the use of nitric acid instead of phosphoric acid is comparable in their resulting effectiveness, although the total concentration of available protons from each acid is significantly higher for phosphoric acid than for nitric acid.
[0241] Due to the highly basic nature of the highly silicate, even water is generated in this experiment and acts as an at least partially reactive acid, providing some benefit to subsequent coatings.
[0242] However, it is clear from the experiments that the addition of a highly concentrated mineral acid is superior to the simple addition of water to the silicate coated particles. [Table 2a]
[0243] (Example 4) The iron powder used had an apparent density of 3.4 g / cm 3 , D 50 The powder was an annealed water atomized pure iron powder with a particle size distribution in the 95-100 μm interval measured according to ISO 9276-2:2014. The powder had at least 80 wt% of the core particles in the 75-380 μm range measured according to ISO 4497:2020 with 80% within 45-150 μm on a 100 mesh sieve.
[0244] Powder compositions were prepared for coating parts using the same method as detailed in Example 1, but with varying amounts of Bi2O3, silane, and water. [Table 2b]
[0245] Table 4a summarizes the amounts added in the different experiments. The amounts are given in g per kg of powder composition, except for potassium silicate, where the amounts are given in wt%.
[0246] Table 4b summarizes the different results in the same units as for Table 1b.
[0247] The results in Table 4b show that in order to achieve good resistivity, the amount of coating component needs to be increased for these relatively fine powders compared to the coarser powders. It is concluded that coatings are beneficial for these relatively fine particles. [Table 4a]
[0248] (Example 5) Green parts, sample number 23, were manufactured using the same method as sample number 21. The green parts were then heat treated in a batch furnace according to Example 1, but with oxygen content varied between 0 and 50000 ppm.
[0249] Table 5a summarizes the amounts added in the different experiments. The amounts are given in g per kg of powder composition, except for potassium silicate, where the amounts are given in wt%.
[0250] Table 5b summarizes the different results in the same units as for Table 1b. It can be seen from Table 5b that increased oxygen content in the heat treatment atmosphere gives higher resistivity. However, if the oxygen level is too high (50000 ppm), the coercivity increases, thus resulting in total core loss. [Table 5a]
[0251] (Example 6) The iron powder used had an apparent density of 3.2 g / cm 3 , D 50 The powder was an annealed water atomized pure iron powder with a particle size in the 38-45 μm interval measured according to ISO 9276-2:2014. The powder has at least 80 wt% of the core particles in the 20-75 μm range measured according to ISO 4497:2020.
[0252] Powder compositions were prepared for coating parts using the same method as detailed in Example 1, but with varying amounts of potassium silicate, phosphate, Bi2O3 and silane.
[0253] Table 6a summarizes the amounts added in the different experiments. The amounts are given in g per kg of powder composition, except for potassium silicate, where the amounts are given in wt%. [Table 4b] [Table 5b]
[0254] Table 6b summarizes the different results in the same units as for Table 1b.
[0255] A commercially available powder with a comparable size of core particles is Somaloy™ 110i 5P, the characteristics of which are given in Table 6b.
[0256] The results in Table 6b show that in order to achieve resistivity comparable to the reference material, the amount of coating component needs to be increased for these relatively fine powders compared to the coarser powders. It is concluded that coatings are beneficial for these fine particles. [Table 6a]
[0257] (Example 7) A comparative sample not according to the invention was prepared by repeating the procedure for sample no. 2, but omitting any drying or removal of any water after application of the potassium silicate. This sample is sample no. 1. In Table 1b, the resistivity of the parts was only 24 μΩm for sample no. 1 compared to 1450 μΩm for comparative sample no. 2. Not performing any removal of water after application of the silicate did not produce satisfactory results.
[0258] (Example 8) Comparative samples not according to the invention were prepared by repeating the procedure of sample no. 9. For sample no. 28, acetone was added to the acid instead of water. The powder was treated after application of K-silicate. For sample no. 29, acetone was also added to the acid, but the powder was instead treated before treatment with K-silicate. The examples are summarized in Table 8a.
[0259] The results in Table 8b show that acetone is not necessary and satisfactory results are also achieved without the use of organic solvents such as acetone to deposit the acid coating. It can further be concluded that a phosphoric acid coating under silicate is not suitable for improving the magnetic properties of the powders of the present invention and that the silicate should be applied directly onto the powder as a first coating. [Table 6b] [Table 8b] [Table 8a]
[0260] (Example 9) Comparative examples not according to the invention were prepared by repeating the procedure for sample no. 11, but replacing the phosphoric acid with the same amount of 98% sulfuric acid (sample no. 39) or 60% acetic acid (sample no. 40). As can be seen from Table 9, for sample no. 39, rust appeared on the powder, and it was concluded that sulfuric acid was not suitable. For sample no. 40, the resistivity was 416 μΩm compared to 1364 μΩm for comparative sample no. 11. It was concluded that all acids were not suitable for the process. [Table 9]
[0261] (Example 10) A comparative example not according to the invention was prepared by repeating the procedure outlined in Example 1, except that the powder was dried after application of the phosphoric acid and water mixture.
[0262] From Table 10 we can see that if too much acid is applied the powder will rust. A large amount of potassium silicate will withstand a large amount of phosphoric acid before rusting occurs. [Table 10]
[0263] (Example 11) The iron powder used had an apparent density of 3.4 g / cm 3 , D 50The iron powder was an annealed water atomized pure iron powder with a particle size distribution in the 95-100 μm interval. The iron powder was a ferromagnetic powder composition containing soft magnetic iron-based core particles. The particle size distribution was measured by weighing the different sieve fractions according to ISO 4497:2020. The average particle size was then calculated according to ISO 9276-2:2014.
[0264] The powder composition was coated into parts using the same method as detailed in Example 1.
[0265] Table 11a summarizes the amounts added in the different experiments. The amounts are given in g per kg of powder composition, except for potassium silicate, where the amounts are given in wt%.
[0266] Table 11b summarizes the different results in the same units as for Table 1. [Table 11a]
[0267] Table 11b shows that resistivity increases with the addition of phosphoric acid, but if too much acid is used (sample no. 47), it has a negative effect on the transmittance, TRS and overall core loss (see Figure 2).
[0268] (Example 12) In Example 12, the same iron powder used in Example 11 (designated #100) and Example 2 (designated #40) was used, both with the same first coating, namely, 0.10 wt% potassium silicate.
[0269] 1 ml of the acid solution was added to 100 g of the dry potassium silicate coated powder in a container and the mixture was shaken for 1 minute and rested for 3 minutes.
[0270] Both HNO3 and H3PO4 were used in varying concentrations.
[0271] The powder was then mixed with 200 ml of deionized water and after 3 minutes the pH of the water was measured according to DIN 19268. The turbidity was measured according to ISO 7027-1:2016.
[0272] FIG. 12a shows that the pH decreases and the turbidity increases with the addition of H3PO4, the increase being more evident for the coarser (#40) powder. [Table 11b]
[0273] The increase in turbidity may be caused by acid-induced precipitation of silica particles from the potassium silicate coating, indicating the role of acid treatment (see Figures 3 and 4).
[0274] As observed, too low a pH will destabilize the potassium silicate coating, causing an unacceptable decrease in transmittance and TRS in line with currently required limits on acid concentration.
[0275] (Example 13) Surface inspection using SEM / EDS In this embodiment, the soft magnetic iron-based core particles are formed of the above general formula (K2O) α (SiO2) β The silicate was mixed with an aqueous solution of the silicate having a β / α ratio of 3.1 to 3.4 and a concentration of 0.1 wt % of Example 1. However, no acid treatment was provided.
[0276] Core particles were examined using a field emission gun scanning electron microscope (FEG-SEM) (Hitachi SU6600) equipped with an energy dispersive spectroscopy detector (Oxford Instruments Ultima Max 65 mm).
[0277] Measurements were made at a distance of 10 mm (working distance) using an accelerating voltage of 20 kV with a penetration depth of 1.5 μm and a detection area diameter of 1 μm.
[0278] The results are shown in Figures 5A-C and further summarized in Table 13 below. Herein, Figure 5A shows an SEM image of an iron-based core particle coated with silicate. Figure 5B shows an EDS mapping image of the corresponding core particle showing the potassium (K) content on the surface in light grey to white. It can be observed that the silicate coating varies in thickness on the surface, thus forming thicker areas (patches) with higher K content than outside the same patch and thinner areas between the patches.
[0279] FIG. 5C shows an EDS mapping image of the corresponding core particle showing the silicon (Si) content on the surface in light grey to white. [Table 13]
[0280] SEM / EDS measurements determined the material content at the surface of the particles as well as to some extent within the bulk particles (minimum detection depth at 20 kV is about 1.5 μm, diameter for EDS point analysis is about 1 μm), and differences in measured iron content (Fe) reflect different thicknesses of and between patches.
[0281] As can be seen from the examples, even though potassium silicate does deposit on the surface, the resulting coating is very inhomogeneous and "patchy", barely covering the outer iron surface of the patch.
[0282] (Example 14) In this embodiment, the soft magnetic iron-based core particles are formed of a material having the general formula (KO) α (SiO2) β The silicate was mixed with an aqueous solution of the silicate having a β / α ratio of 3.1 to 3.4 and a concentration of 0.1 wt % as in Example 1 above.
[0283] Core particles were examined using a field emission gun scanning electron microscope (FEG-SEM) (Hitachi SU6600) equipped with an energy dispersive spectroscopy detector (Oxford Instruments Ultima Max 65 mm).
[0284] Measurements were made at a distance of 10 mm (working distance) using an accelerating voltage of 20 kV.
[0285] The results are shown in Figures 6A-C, 7A-D and 8A-B and further summarized below in Table 14. Data are the average of at least 4 but in most cases up to 12 independent EDS measurements. [Table 14]
[0286] At weaker acid concentrations, the potassium silicate patches appear similar to the acid-free sample (see FIG. 5), with sizes up to a few microns.
[0287] At stronger acid concentrations, these patches are much smaller (bottom left image), which is consistent with the changes in surface chemistry also shown in Example 12.
[0288] EDS analysis shows that the phosphor is mainly located in patches / dots with potassium. This was taken to indicate that the patches are potentially nano-deposits of K3PO4 as nano-crystallites rather than potassium silicate.
[0289] Outside the patch, the phosphor is detected at levels about 2-3 times higher than background, but not as high as the observed direct deposition of K3PO4, but this increase is significant and observed at all detection locations, consistent with the general intensity enhancement for the phosphor seen in the EDS images of Figures 8A and B.
[0290] This clearly demonstrates that, in contrast to the phosphate coating layers formed by prior art methods, the presently coated particles achieve their beneficial properties without the presence of a phosphate layer, through a combination of potassium silicate with an insulating aqueous coating, or a combination of potassium silicate with an insulating aqueous coating and interstituent bismuth (III) oxide particles.
[0291] Advantageously, however, this increase in the presence of phosphor over background is evidence of a surface that has been subjected to an acidic aqueous solution treatment of potassium silicate with aqueous phosphoric acid.
[0292] Figure 6 shows progressively higher magnifications for uncoated iron particles up to 5 μm in Figure 6D, and EDS was performed for K, Si, and P. Small amounts, as shown in Table 14, were found for all three elements, consistent with the expected background, as no differences between patch and no patch were observed.
[0293] In Fig. 7, potassium water glass coated iron-based particles are shown, with scales A: 250 μm and B: 100 μm, respectively. The coating with potassium water appears homogeneous and completely covering, as evidenced by EDS for K and Si when compared with SEM images (compare Figs. 6B and 6C), although patches of thicker water glass are present (clear patches).
[0294] FIG. 8 shows the results for water glass treated particles treated with two different phosphoric acid concentrations, A: 8.5 g / l and B: 75 g / l, respectively, and EDS was performed for K, Si and P. Notably, the intensity increase of element signals due to acid treatment is consistent with the results obtained in Example 12.
[0295] Based on the experiments presented herein, it was possible to conclude that the aforementioned chemical changes in the presence of an aqueous acid solution involve at least partial reaction of the deposited silicate to form silica as the first coating. It was further possible to conclude that under optimal reaction conditions, complete conversion of the silicate to silica occurs under the influence of the aqueous acid solution.
[0296] Based on the experiments shown herein, it is possible to define an internal standard which includes a test for when the silicate of the first coating (12a) is treated with an acidic aqueous solution, for example preferably phosphoric acid or nitric acid, most preferably phosphoric acid, i.e. the silicate coated surface shows a significant increase in the detected level of at least one element characteristic of the aqueous acid solution used when measuring the silicate coated surface before and after the treatment with the aqueous acid solution, the detection being carried out by energy dispersive spectroscopy (EDS), the measurements being carried out at a distance of 10 mm (working distance) using an accelerating voltage of 20 kV, a penetration depth of 1.5 μm and a detection area diameter of 1 μm, and the detection result of the detection level of the characteristic element is the average of at least four independent detections.
[0297] Because the coatings of Soileau et al. do not rely on further chemical modification, detection of an increased level of at least one element characteristic of the aqueous acid solution used is a sensible means of distinguishing the present coatings from those of Soileau et al.
[0298] From the experiments, it was observed that the acid treatment and associated pH reduction results in the precipitation of nanosilica which promotes the distribution of silicate into complete coverage, as evidenced by turbidity measurements (see Example 12, Figures 3 and 4).The acid treated first coating is thus a covered silicate coating.
[0299] It was observed that the acid treatment caused a concentration of cations (potassium ions (K+) which in the experiments sought unreacted silicate during powder processing (in the experimental stirring)) on the silicate surface, forming nano-sized patches. These patches have a low ratio of (SiO2 / K2O) relative to the background coating between the patches. The patches eventually become smaller and better distributed as the acid concentration is increased, contributing to the observed beneficial effects on tribology (internal lubrication and protection from cold welding during compression) and eventually completing the complete transition from silicate to silica.
[0300] Thus, in an embodiment, the first coating is a silica coating.
[0301] As further observed in the experiments with phosphoric acid, the excess amount of acid eventually reacts further with potassium after the complete conversion of silicate to silica, thereby forming the observed K3PO4 nanocrystallites.
[0302] To that end, an internal test for the reaction of silicate to silica can be defined by comparing the above-defined EDS-measured content of alkali metal ions (in potassium (K) in the experiment) in the patch after coating and before acid treatment with the amount of alkali metal ions after acid treatment, the reduction of alkali metal ions being decisive for the reaction of silicate to silica and the absence of a further reduction of alkali metal ions after the first reduction being decisive for the complete reaction of the silicate present on the coated core particles to silica.
[0303] The measured reductions on the patches (see Table 14) were by factors of 14.4 / 4.2 ≈ 3.4 (8.5 g / l H3PO4) and 14.4 / 0.47 ≈ 30.6 (75 g / l H3PO4) for the partially reacted and fully reacted surfaces, respectively.
[0304] (Example 15) In this embodiment, the soft magnetic iron-based core particles are formed of a material having the general formula (KO) α (SiO2) β The silicate was mixed with an aqueous solution of silicate having a β / α ratio of 3.1 to 3.4 at a concentration of 0.1 wt % according to Example 1. Additionally, particles of bismuth (III) oxide were added to the silicate coated particles.
[0305] As shown in FIG. 9, at the selected bismuth(III) oxide particle concentration, they were distributed without any discernible pattern on the silicate-coated particles, consistent with individual particle deposition from a dilute solution.
[0306] (Example 16) The particles of Example 15 having a potassium silicate coating and surface-attached bismuth(III) oxide were post-coated with Dynasylan™ according to the procedure of Example 1.
[0307] As can be seen from Figure 10, the bismuth(III) oxide particles are indistinguishable beneath the Dynasylan coating, but since EDS is only sensitive to the Si in the Dynasylan molecules, the EDS is constant, indicating a substantially complete coating, and the measured signal will include some contribution from the underlying silicate due to the penetration depth of the EDS beam.
[0308] Conclusion Although the invention has been described in detail for purposes of illustration, it will be understood that such detail is for that purpose only and that modifications may be made by those skilled in the art in practicing the claimed subject matter from a study of the drawings, the disclosure, and the appended claims.
[0309] Where used in the claims, the term "comprising" does not exclude other elements or steps. Where used in the claims, the indefinite articles "a" or "an" do not exclude a plurality. Any signs used in the claims shall not be interpreted as limiting the scope.
Claims
1. A ferromagnetic powder composition comprising soft magnetic iron-based core particles (11), at least 80 wt. % of said core particles (11) have a particle size distribution in the range of 20 to 1000 μm, measured according to ISO 4497:2020; The surface of the core particle (11) is 2 O) α (SiO 2 ) β (In the formula, -α is M 2 is the moles of O, and β is SiO 2 with the β / α molar ratio in the interval from 0.5 to 4.1, - M is selected from Li, Na and K, - said first coating (12a) is in direct contact with the surface of the core particles (11) of ferromagnetic powder; - said silicate is present in an amount of 0.02 to 1.0 wt %, calculated on the total weight of said ferromagnetic powder composition; and - a ferromagnetic powder composition, wherein said first coating (12a) is acid-treated with an aqueous acidic solution after forming said first coating (12a) on said iron-based core particle (11).
2. 2. The ferromagnetic powder composition of claim 1, wherein M is potassium (K).
3. A ferromagnetic powder composition according to any one of claims 1 and 2, wherein the aqueous acid solution is either aqueous phosphoric acid or aqueous nitric acid.
4. A ferromagnetic powder composition according to any one of claims 1 to 3, wherein the acidic aqueous solution is aqueous phosphoric acid.
5. On said first coating (12a) bismuth (III) oxide particles (14) are deposited, said bismuth (III) oxide particles (14) having a D measured according to SS-ISO 13320-1 in intervals of 0.1 to 10 μm. 50 5. A ferromagnetic powder composition according to claim 1, having
6. 6. The ferromagnetic powder composition according to claim 1, wherein the core particle (11) further comprises a second coating (12b), the first coating (12a) on the core particle (11) being located between the core particle (11) and the second coating (12b), the second coating (12b) being formed from at least one insulating water-based organic molecule suitable for depositing as at least a monolayer on the first coating (12a).
7. At least one insulating water-based organic molecule suitable for depositing as at least a monolayer on said first coating (12a) is The following general formula: R 1 [(R 1 ) x (R 2 ) y (M2)] n O n-1 R 1 (Wherein, M2 is selected from the group consisting of Si, Ti, Al and Zr; O is oxygen; R 1 is a hydrolyzable group; R 2 is an organic moiety, and at least one R 2 contains at least one amino group; n is the number of repeat units, which is an integer from 1 to 20; x is 0 or 1; and and y is 1 or 2; 7. A ferromagnetic powder composition according to claim 6.
8. 8. The ferromagnetic powder composition of claim 7, wherein M2 is silicon (Si).
9. A ferromagnetic powder composition according to any one of claims 1 to 8, wherein at least 80 wt% of the core particles are in the range of 20 to 75 μm measured according to ISO 4497:2020.
10. A ferromagnetic powder composition according to any one of claims 1 to 8, wherein at least 80 wt% of the core particles are in the range of 45 to 150 μm measured according to ISO 4497:2020.
11. A ferromagnetic powder composition according to any one of claims 1 to 8, wherein at least 80 wt% of the core particles are in the range of 75 to 380 μm measured according to ISO 4497:2020.
12. 12. A ferromagnetic powder composition according to claim 1, wherein the silicate is present in the ferromagnetic powder composition in an amount of 0.05 to 1.0 wt %, calculated on the total weight of the ferromagnetic powder composition, preferably the silicate is present in an amount of 0.10 to 0.5 wt %.
13. A ferromagnetic powder composition according to any one of claims 1 to 12, wherein potassium silicate is present in an amount of 0.1 to 0.6 wt %, calculated on the total weight of the ferromagnetic powder composition.
14. A ferromagnetic powder composition according to any one of the preceding claims, wherein the β / α molar ratio of said silicates is in the interval from 2.5 to 4.1, preferably from 2.9 to 3.5, more preferably from 3.1 to 3.
4.
15. The D of the bismuth (III) oxide particles (14) measured in accordance with SS-ISO13320-1 50 A ferromagnetic powder composition according to any one of claims 5 to 14, wherein the spacing between the first and second ferromagnetic particles is between 0.5 and 2 µm.
16. 16. A ferromagnetic powder composition according to any one of claims 5 to 15, wherein the bismuth(III) oxide particles (14) are present in an amount of 0.05 to 0.30 wt %, calculated on the total weight of the ferromagnetic powder composition.
17. 17. A ferromagnetic powder composition according to any one of claims 5 to 16, wherein the bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.30 wt. %, calculated on the total weight of the ferromagnetic powder composition.
18. 18. A ferromagnetic powder composition according to any one of claims 5 to 17, wherein the bismuth (III) oxide particles are present in an amount of 0.10 to 0.25 wt % and the metal organic compound is present in an amount of 0.10 to 0.25 wt %, calculated on the total weight of the ferromagnetic powder composition.
19. 19. Ferromagnetic powder composition according to any one of claims 7 to 18, wherein the metal organic compound (13) is present in an amount of 0.15 to 0.30 wt %, preferably in the range of 0.10 to 0.25 wt %, calculated on the total weight of the ferromagnetic powder composition.
20. 20. A ferromagnetic powder composition according to any one of claims 7 to 19, wherein potassium silicate is present in an amount of 0.10 to 0.30 wt. %, calculated on the total weight of the ferromagnetic powder composition, the bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.20 wt. %, and the metal organic compound (13) is present in an amount of 0.10 to 0.20 wt. %.
21. 21. The ferromagnetic powder composition of claim 7, wherein the metal organic compound is selected from the group consisting of alkoxy terminated aminosilsesquioxanes, aminosiloxanes, oligomeric 3-aminopropylalkoxysilanes, 3-aminopropylalkoxysilanes.
22. 22. A ferromagnetic powder composition according to any one of claims 7 to 21, wherein the metal organic compound is selected from the group consisting of N-aminoethyl-3-aminopropylalkoxysilane and N-aminoethyl-3-aminopropylmethylalkoxysilane.
23. Next successive steps: a. Preparing soft magnetic iron-based core particles (11); b. The soft magnetic iron-based core particles (11) are formed into a compound represented by the general formula (M 2 O) α (SiO 2 ) β (In the formula, M is selected from Li, Na and K; -α is M 2 is the moles of O, and β is SiO 2 with a first aqueous mixture comprising a silicate having a β / α molar ratio in the interval of 0.5 to 4.1; thereby obtaining a first coating (12a) at least partially covering said core particle (11) which is in direct contact with the surface of said core particle (11), c. removing at least a portion of the water; d. reacting the silicate-coated soft magnetic iron-based core particles (11) with an acidic aqueous solution; said silicate being present in an amount of 0.02 to 1.0 wt %, calculated based on the total weight of said at least partially coated soft magnetic iron-based core particles; A method for coating soft magnetic iron-based core particles (11) with an aqueous silicate solution, comprising:
24. 24. The method for coating soft magnetic iron based core particles (11) with an aqueous silicate solution according to claim 23, wherein M is potassium (K).
25. A method for coating soft magnetic iron-based core particles (11) with an aqueous silicate solution according to claim 23 or 24, wherein said aqueous acid solution is phosphoric acid or nitric acid, preferably phosphoric acid.
26. 26. The method of any one of claims 23 to 25, wherein steps b) and c) are repeated at least once.
27. 27. A method according to any one of claims 23 to 26, wherein 0.05 to 0.5 wt. % of said silicate, calculated on the total weight of said ferromagnetic powder composition, is added in step b).
28. 28. The process according to any one of claims 23 to 27, wherein the β / α molar ratio of said silicate is in the interval from 2.5 to 4.1, preferably from 2.9 to 3.5, more preferably from 3.1 to 3.
4.
29. 29. A method for obtaining a ferromagnetic powder composition comprising the step of coating a powder comprising at least 80 wt.-% of soft magnetic iron-based core particles (11) having a particle size distribution in the range of 20-1000 μm measured according to ISO 4497:2020 using the method according to any one of claims 23 to 28, prior to the subsequent process step of drying and isolating the ferromagnetic powder composition.
30. Prior to the next process step of drying and isolating said ferromagnetic powder composition, further successive steps include: e. Optionally, contacting said at least partially coated soft magnetic iron-based core particles from step c) with bismuth (III) oxide particles (14), wherein the D of the bismuth (III) oxide particles (14) measured according to SS-ISO 13320-1 is 50 are steps spaced from 0.1 to 10 μm apart, f. optionally removing at least a portion of said water; g. The particles are formed according to the general formula: R 1 [(R 1 ) x (R 2 ) y (M2)] n O n-1 R 1 (Wherein, M2 is selected from the group consisting of Si, Ti, Al and Zr; O is oxygen; R 1 is a hydrolyzable group; R 2 is an organic moiety, and at least one R 2 contains at least one amino group; n is the number of repeat units, which is an integer from 1 to 20; x is 0 or 1; and y is 1 or 2; 30. A method for obtaining the ferromagnetic powder composition of claim 29, further comprising:
31. 31. The method of claim 29 or 30, wherein M2 is silicon (Si).
32. 32. The method of any one of claims 29 to 31, comprising step e).
33. 33. The method of any one of claims 29 to 32, comprising step f).
34. 34. The method of any one of claims 29 to 33, wherein both steps e) and f) are included.
35. 35. The method according to any one of claims 29 to 34, wherein at least 80 wt.% of the provided core particles (11) are in the range of 20 to 75 μm measured according to ISO 4497:2020.
36. 35. The method according to any one of claims 29 to 34, wherein at least 80 wt.% of the core particles (11) are in the range of 45 to 150 μm measured according to ISO 4497:2020.
37. 35. The method according to any one of claims 29 to 34, wherein at least 80 wt.% of the core particles (11) are in the range of 75 to 380 μm measured according to ISO 4497:2020.
38. The D of the bismuth (III) oxide particles (14) measured in accordance with SS-ISO13320-1 50 The method according to any one of claims 29 to 37, wherein the spacing is between 0.5 and 2 μm.
39. 39. The method according to any one of claims 29 to 38, wherein the bismuth(III) oxide particles (14) are present in an amount of 0.05 to 0.30 wt %, preferably 0.10 to 0.30 wt %, calculated on the total weight of the ferromagnetic powder composition.
40. A method according to any one of claims 29 to 39, wherein said silicate is present in an amount in the range of 0.10 to 1.0 wt%, preferably 0.10 to 0.6 wt%, calculated on the total weight of the ferromagnetic powder composition.
41. 41. The method according to any one of claims 29 to 40, wherein the metal organic compound (13) is present in the range of 0.15 to 0.30 wt %, preferably in the range of 0.10 to 0.25 wt %, calculated on the total weight of the ferromagnetic powder composition.
42. 42. The method according to any one of claims 29 to 41, wherein the bismuth(III) oxide particles (14) are present in an amount of 0.10 to 0.25 wt %, calculated on the total weight of the ferromagnetic powder composition, and the metal organic compound (13) is present in an amount of 0.10 to 0.25 wt %.
43. 43. The method according to any one of claims 29 to 42, wherein the silicate is potassium water glass and is present in an amount of 0.10 to 0.30 wt %, the bismuth (III) oxide particles (14) are present in an amount of 0.10 to 0.20 wt %, and the metal organic compound is present in an amount of 0.05 to 0.20 wt %.
44. 45. The method of any one of claims 29 to 44, wherein the metal organic compound is selected from the group consisting of alkoxy terminated amino silsesquioxanes, amino siloxanes, oligomeric 3-aminopropyl alkoxy silanes, 3-aminopropyl alkoxy silanes.
45. 46. The method of any one of claims 29 to 45, wherein the metal organic compound is selected from the group consisting of N-aminoethyl-3-aminopropylalkoxysilane and N-aminoethyl-3-aminopropyl / methylalkoxysilane.
46. A method for producing an object from a ferromagnetic powder composition according to any one of claims 29 to 45, comprising the steps of: h. taking said ferromagnetic powder composition from step g and mixing said ferromagnetic powder composition with at least one lubricant; i. optionally preheating the die to a temperature below the melting temperature of the added particulate lubricant; j. compressing the composition in the mold at a compression pressure ranging from 300 to 2000 MPa, preferably from 400 to 1200 MPa; k. Removing the resulting green body; and Preferably 0 to 2.2 wt %, more preferably 0.5 to 2 wt % O 2 and heat treating the green body at a temperature in the range of 300 to 800°C, preferably 400 to 750°C, more preferably 600 to 700°C in a non-reducing atmosphere containing A method comprising:
Citation Information
Patent Citations
Ferromagnetic powder composition and method for its production
EP2252419A1
Powdered iron core magnetic devices
US4601753A
Powdered iron core magnetic devices
US4601765A
Ferromagnetic powder composition and method for its production
WO2011032931A1