Heat-assisted self-piercing riveting for high-strength 7XXX aluminum.
The self-drilling riveting system with a local melt process addresses cracking issues in high-strength aluminum alloys by locally melting the substrate before riveting, resulting in stronger, crack-free joints.
Patent Information
- Application Number
- JP2024522217
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-20
- Filing Date
- 2022-10-13
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional self-drilling riveting processes in high-strength aluminum alloys, such as those used in the automotive and aerospace industries, often result in cracks known as 'button cracks', leading to premature failure of the joints.
A self-drilling riveting system that includes a local melt system, such as a resistance spot welding system, to locally melt the target location on the metal substrates before driving a rivet into the joint, forming a bond without visible material welding.
The system minimizes or eliminates cracking in high-strength aluminum alloys, producing joints with reduced rivet head height and improved minimum thickness, enabling reliable joint formation in materials that conventional methods cannot handle.
Smart Images

Figure 2024538776000001_ABST
Abstract
Description
[Technical field]
[0001] REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 63 / 262,761, filed October 20, 2021, entitled "THERMAL ASSISTED SELF-PIERCING RIVETING FOR HIGH STRENGTH 7XXX ALUMINUM," the entire contents of which are incorporated herein by reference.
[0002] This application relates to self-pierce riveting systems and methods, and more particularly to self-pierce riveting systems and methods for high strength aluminum alloys. [Background technology]
[0003] Various joining techniques can be used to join components together to form various parts or components of the final product. Such joining techniques can include various types of welding (e.g., resistance spot welding, friction stir welding, laser beam welding, ultrasonic welding, etc.), adhesives, and / or mechanical fastening, among others.
[0004] Self-piercing riveting is a type of mechanical fastening technique that typically uses a rivet having a head and a base. During the self-piercing riveting process, the rivet is driven into one or more sheets by a driver such that the base of the rivet penetrates at least one sheet and deforms to form a mechanical interlock. A problem with the conventional self-piercing riveting process is that in high strength materials, such as high strength aluminum alloys, cracks may develop in one or both of the sheets or components joined by the rivet (such cracks are sometimes known as "button cracks"). Such cracks may cause premature failure of the self-piercing riveted joint and may be totally unacceptable in certain industries, particularly in the automotive or aerospace industries. Summary of the Invention
[0005] The embodiments covered by this patent are defined by the claims below, and not by this Summary. This Summary is a high level overview of various embodiments and introduces some of the concepts that are further described in the Detailed Description section below. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used alone to determine the scope of the claimed subject matter. The subject matter should be understood by reference to the entire specification of this patent, any or all of the drawings, and appropriate portions of the claims.
[0006] According to certain embodiments, a self-piercing riveting system includes a local melting system and a driver. The local melting system is capable of locally melting a target location on a metal substrate. In one non-limiting embodiment, the local melting system is a resistance spot welding system. The driver is capable of driving a rivet into the metal substrate at the target location after the target location is locally melted. The rivet driven into the metal substrate forms a joint.
[0007] According to some embodiments, a method of joining at least two metal substrates includes locally melting a target location on the at least two metal substrates, the method includes, after locally melting the target location, driving a rivet into the target location with a driver such that the rivet penetrates the at least two metal substrates at the target location.
[0008] According to various embodiments, a method of joining at least two metal substrates includes welding the at least two metal substrates at a target location for a weld time greater than 0 seconds and less than 1 second such that a temperature at the target location is at least 500° C. The method includes, after welding, driving a rivet at the target location such that the rivet penetrates the at least two metal substrates at the target location.
[0009] The various embodiments described herein may include additional systems, methods, features, and advantages that may not necessarily be expressly disclosed herein, but will be apparent to one of ordinary skill in the art upon review of the following detailed description and the accompanying drawings. It is intended that all such systems, methods, features, and advantages be included within this disclosure and protected by the accompanying claims.
[0010] This specification refers to the accompanying drawings in which: The use of like reference numbers in different drawings is intended to indicate the same or similar elements. [Brief description of the drawings]
[0011] [Figure 1] 1 illustrates a self-piercing riveting system, according to an embodiment. [Figure 2A] 1 illustrates a metal substrate during a preheating stage of a joining process using a self-piercing riveting system, according to an embodiment. [Figure 2B] 2B shows the metal substrate of FIG. 2A during the riveting stage of the joining process. [Diagram 3] 1A and 1B show a joint formed using a self-piercing riveting system, according to an embodiment. [Figure 4] A and B show a conventional joint formed on two metal substrates, and C and D show a joint formed using the self-piercing riveting system according to the embodiment on the metal substrates of Figures 4A and 4B. [Diagram 5] A and B show a conventional joint formed on two metal substrates, and C and D show a joint formed using the self-piercing riveting system according to the embodiment on the metal substrates of Figures 5A and 5B. [Figure 6] A and B show a conventional joint formed on two metal substrates, and C and D show a joint formed using the self-piercing riveting system according to the embodiment on the metal substrates of Figures 6A and 6B. [Figure 7]A and B show a conventional joint formed on two metal substrates, and C and D show a joint formed using the self-piercing riveting system according to the embodiment on the metal substrates of Figures 7A and 7B. [Figure 8] 1 is a table of results for conventional joints and joints formed using a self-piercing riveting system, according to an embodiment. [Figure 9] 1 illustrates a target location formed by two metal substrates, where the interface of the target location is shown to be partially melted, according to an embodiment. [Figure 10] 10A and 10B show a conventional joint formed between two metal substrates, and C and D show a joint formed using the self-piercing riveting system according to the metal substrate embodiment of FIGS. 10A and 10B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Described herein is a self-piercing riveting (SPR) system and associated method for joining two or more metal substrates. The SPR system provided herein includes a preheating system that locally melts a target location on the metal substrate, and a driver that drives a rivet into the target location on the metal substrate to form a joint that joins the metal substrates. As used herein, locally melting the target location prior to the SPR process refers to heating without visible material welding of the substrates. In certain embodiments, the interface at the target location between the metal substrates may be fully locally melted (e.g., the entire target area may be locally melted) or partially locally melted (e.g., less than the entire target area is locally melted prior to the SPR process / only minor interfacial melting is provided). In some embodiments, the preheating system may be a welding system, including but not limited to a resistance spot welding system, which heats the metal substrate to at least partially melt the target location on the metal substrate to form a melted area. The driver may be any suitable device or mechanism for driving a rivet into the target location. The rivet driven into the metal substrate can be any type of rivet as desired. During the SPR process, a pre-heating system can locally melt (partially or fully) a target location, and a driver drives the rivet into the target location prior to solidification of the target location.
[0013] In certain embodiments, the SPR systems and methods described herein can provide improved joints in metal substrates. In some embodiments, the SPR systems and methods provided herein can produce SPR joints with minimal or no cracks compared to joints formed without preheating. In certain embodiments, riveted joints formed using the SPR systems and methods provided herein can have reduced rivet head heights compared to conventional joints and / or improved minimum thickness without cracks compared to conventional joints. The SPR systems and methods described herein can also enable joint formation in high strength aluminum alloys that would not otherwise be possible or would result in joints with various defects, such as cracks. Various other benefits and advantages can be realized using the SPR systems and methods described herein, and the above benefits and advantages should not be considered limiting.
[0014] FIG. 1 shows an example of an SPR system 100 for joining at least a first substrate 102 to a second substrate 104 with a rivet 106 .
[0015] Although two substrates 102, 104 are shown, in other embodiments, the SPR system 100 can be used to bond any number of substrates as desired. In various examples, the substrates 102, 104 can be metal sheets, metal shates, or other suitable types of workpieces for forming various parts or components of a final product. As used herein, a sheet generally refers to a metal (e.g., aluminum) product having a thickness of less than about 4 mm. For example, a sheet can have a thickness of less than 4 mm, less than 3 mm, less than 2 mm, less than 1 mm, less than 0.5 mm, less than 0.3 mm, or less than 0.1 mm. A shate (also called a sheet plate) generally has a thickness of about 4 mm to about 15 mm. For example, a shate can have a thickness of 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, or 15 mm. In one non-limiting example, the substrates 102, 104 joined by the SPR system 100 can have a thickness of 5 mm or less, such as 3 mm or less, although this need not be the case in other embodiments.
[0016] In some examples, the first substrate 102 and / or the second substrate 104 may be selected from a group including 1xxx aluminum alloys, 2xxx aluminum alloys, 3xxx aluminum alloys, 4xxx aluminum alloys, 5xxx aluminum alloys, 6xxx aluminum alloys, 7xxx aluminum alloys, or 8xxx aluminum alloys. In some examples, the substrates 102, 104 may be different metals (e.g., the first substrate 102 is a 7xxx aluminum alloy and the second substrate 104 is a 6xxx series aluminum alloy). In other examples, the substrates 102, 104 are both aluminum alloys of the same series (e.g., the first and second aluminum alloys are both 7xxx aluminum alloys). In some non-limiting examples, one or more of the substrates 102, 104 may be high-strength aluminum alloys, such as 2xxx aluminum alloys, 5xxx aluminum alloys, 6xxx aluminum alloys, and / or 7xxx aluminum alloys, among others. As described herein, such high strength aluminum alloys will crack during conventional SPR processes, but such cracking can be minimized and / or avoided using SPR system 100.
[0017] In other examples, the substrates 102, 104 may be various other metals or materials welded together, including, but not limited to, aluminum, aluminum alloys, steel, steel-based materials, nickel, nickel-based materials, copper, copper-based materials, cast iron, titanium, titanium-based materials, various other suitable materials, and / or various combinations of materials. In other examples, the first metal sheet 102 and / or the second metal sheet 104 may include various other metals or types of metal sheets, including, but not limited to, aluminum clad alloy sheets, monolithic alloys (aluminum, steel, etc.), roll-bonded alloys, or various other types of metal sheets welded together.
[0018] As shown, the SPR system 100 includes a pre-heating system 108 and a driver 110. During the bonding process, the pre-heating system 108 locally melts a target location 112 on the substrates 102, 104 to form a melted or molten region 114 at the target location 112. The driver 110 then drives the rivet 106 into the target location 112 such that the rivet 106 penetrates the substrates 102, 104, thereby forming a bond.
[0019] The pre-heating system 108 may be a variety of suitable devices or mechanisms for locally melting the target location 112. In certain embodiments, the pre-heating system 108 may heat the target location 112 to a melting temperature for a melting time. In some non-limiting examples, the melting time may be less than 2 seconds, e.g., less than 1 second, e.g., 1000 milliseconds or less, e.g., 500 milliseconds or less. In certain non-limiting examples, the melting time may be less than 500 milliseconds, e.g., 300 milliseconds or less. The melting temperature may be a temperature sufficient to at least partially melt (or cause to be in a molten state) a portion of the substrate 102, 104. In various non-limiting examples, the melting temperature may be at least 500° C., and in some optional embodiments, the melting temperature may be at least 500° C. Optionally, a controller (not shown) may be communicatively coupled to the pre-heating system 108 to control the pre-heating system 108 to heat the substrate 102, 104 to the melting temperature for a melting time. If a controller is included, the controller may be a general processing unit, a processor specially designed for coupling applications, or other suitable processor or computing device. The pre-heating system 108, which pre-heats the target location 112 to a melting temperature for a melting time, can ensure that the substrate is melted locally at the target location 112 while minimizing delays in the overall bonding process. The pre-heating system 108 may optionally allow for additional material to be provided between the substrates 102 and 104. As one non-limiting example, adhesive may be optionally provided between the substrates 102 and 104 or at the target location on the opposing surfaces of the substrates 102, 104 to initially position the substrates 102, 104 relative to one another. In such an embodiment, the adhesive does not need to be removed prior to pre-heating by the pre-heating system 108.
[0020] In the illustrated embodiment, the preheating system 108 is a resistance spot welding (RSW) system having electrodes 116A-116B clamped together in contact with opposing surfaces of the substrates 102, 104. While the electrodes 116A-116B are clamped together, a current is applied through the electrodes 116A-116B and heat generated at the interface of the substrates 102, 104 heats and at least partially melts the substrates 102, 104, thereby forming a molten or melted region 114. Any number of electrodes 116A-116B may be utilized in the RSW system as desired. In other embodiments, the preheating system 108 need not be an RSW system and other types of welding and / or non-welding systems may be used as the preheating system 108 as desired.
[0021] The driver 110 may be any suitable device or mechanism for driving the rivet 106 into the target location 112 such that the rivet 106 penetrates the substrates 102, 104, thereby forming a joint. In various embodiments, the driver 110 drives the rivet 106 into the target location 112 while the target location 112 is at least partially melted and / or unsolidified. In such embodiments, the melted region 114 may facilitate insertion of the rivet 106 into the substrates 102, 104, especially in substrates with high strength. In the illustrated embodiment, the driver 110 is a punch. Optionally, the driver 110 may be provided with a die or guide to facilitate positioning and / or insertion of the rivet 106 into the substrates 102, 104 at the target location 112.
[0022] 1 should not be considered limiting. During the joining process, the driver 110 drives the rivet 106 such that the rivet 106 penetrates the first substrate 102 and at least partially engages the second substrate 104. The base region 118 may splay or otherwise deform outwardly within the second substrate 104 to form a mechanical interlock, thereby forming a joint.
[0023] 2A and 2B are cross-sectional views of metal substrates 202, 204 during a bonding process using the SPR system 100. In this embodiment, each of the metal substrates is a 7xxx aluminum alloy. As shown in FIG. 2A, after preheating with the preheating system 108, a melted or molten region 214 is formed at the interface of the substrates 202, 204. Referring to FIG. 2B, after the riveting stage of the SPR process, a rivet 206 is driven through the molten region 214, thereby forming a joint 222 joining the substrates 202, 204. Compared to the rivet 106, the rivet 206 is completely hollow. As shown in FIG. 2B, the joint 220 did not cause cracks in the substrates 202, 204.
[0024] 3A-3B are photographs of another joint 322 formed using the SPR system 100 according to various embodiments, joining metal substrates 302, 304. In this embodiment, each metal substrate 302, 304 is the same 7xxx aluminum alloy, and each substrate is 2.8 mm thick. As shown in FIG. 3A, a bottom view of joint 322, and FIG. 3B, a cross-sectional view, joint 322 did not crack after rivet 306 was driven through fusion region 314.
[0025] 3B, in certain embodiments, in addition to preventing or minimizing cracking compared to conventional SPR processes, as described in more detail below, the joints formed by the SPR system 100 described herein may have a reduced head height 324, a reduced crack-free minimum thickness 326, and / or improved interlock 328. As referred to herein, head height 324 (HH) is the extent to which the head 320 of the rivet 306 forming the joint 322 extends above or below the first substrate 302, and minimum thickness 326 (T min) is the minimum thickness of the second substrate 304 (which may be, but need not be, immediately adjacent the base region 318 of the rivet 306), and the interlock 328 is the extent to which the base region 318 of the rivet 306 spreads or deforms outwardly from the interface between the substrates 302 and 304. The particular locations shown as being measured for the head height 324, minimum thickness 326, and interlock 328 should not be considered limiting, and the lines for each measurement are for illustrative purposes and are not intended to be specific measurements. Non-limiting examples of these improved measurements are described in detail below with reference to FIGS. 4A-4D, 5A-5D, 6A-6D, and 7A-7D.
[0026] 4A-4D show a non-limiting example comparison of a conventional SPR joint 423 (FIGS. 4A-4B) and an SPR joint 422 (FIGS. 4C-4D) formed using the SPR system 100. In this embodiment, both joints 422, 423 are formed in the same stack of metal substrates, with the top metal substrate 401 being a 6xxx aluminum alloy having a thickness of 2.5 mm and the metal substrate 403 being a 7xxx aluminum alloy having a thickness of 2.8 mm. The same type of rivet 406 was used for both joints 422, 423. In this example, the conventional SPR joint 423 developed a crack 430 in the metal substrates 401, 403, while the SPR joint 422 did not develop a crack in the metal substrates 401, 403. Additionally, the HH of the SPR joint 423 is 0.56 mm, the T min is 1.175 mm, the interlock is 0.713 mm, the HH of the SPR joint 422 is 0.01 mm, and T min In this example, SPR joint 423 has a slightly increased interlock compared to SPR joint 422, but SPR joint 422 does not crack (unlike joint 423), has a reduced HH, and has a higher T min The SPR junction 422 is an improved, better junction since .
[0027] 5A-5D show another non-limiting example of a comparison between a conventional SPR joint 523 (FIGS. 5A-5B) and an SPR joint 522 (FIGS. 5C-5D) formed using the SPR system 100. In this embodiment, both joints 522, 523 are formed in the same stack of metal substrates, where metal substrate 501 is a 6xxx aluminum alloy having a thickness of 2.0 mm and metal substrate 503 is a 7xxx aluminum alloy having a thickness of 1.8 mm. The same type of rivet 506 is used in both joints 522, 523, and compared to rivet 406, rivet 506 is not completely hollow. In this example, conventional SPR joint 523 caused cracks 530 in metal substrates 501, 503. In contrast, SPR joint 522 did not cause cracks in metal substrates 501, 503. Additionally, the HH of SPR joint 523 is −0.02 mm, T min is 0.533 mm, the interlock is 0.16 mm, the HH of the SPR joint 522 is -0.06 mm, and T min From this information, it can be seen that SPR joint 522 did not crack (unlike joint 523), had the lowest HH, and had the lowest T min , had the highest interlock, so was an improved, better joint.
[0028] 6A-6D show an additional non-limiting example of a comparison between a conventional SPR joint 623 (FIGS. 6A-6B) and an SPR joint 622 (FIGS. 6C-6D) formed using SPR system 100. In this embodiment, both joints 622, 623 were formed in the same stack of metal substrates, where metal substrate 601 was a 6xxx aluminum alloy having a thickness of 2.5 mm and metal substrate 603 was a 7xxx aluminum alloy having a thickness of 2.8 mm. The same type of rivet 606 was used for both joints 622, 623, and similar to rivet 406, rivet 606 is hollow along its length. In this example, conventional SPR joint 623 developed a crack 630 in metal substrates 601, 603, while SPR joint 622 did not. Additionally, the HH of SPR joint 623 was 0.40 mm and the T minis 0.792 mm, the interlock is 0.620 mm, the HH of the SPR joint 622 is -0.06 mm, and T min The interlock was 0.485 mm and 0.602 mm. In this example, SPR joint 622 was an improvement compared to SPR joint 623. Based on these results, SPR joint 622 was an improved, better joint because unlike joint 623, joint 622 did not develop cracks. Additionally, T min is reduced at the SPR joint 622, and the negative HH (i.e., the head of the rivet 606 recessed into the substrate 602) may be beneficial for further processing requiring minimal protrusion.
[0029] 7A-7D show yet another non-limiting example of a comparison between a conventional SPR joint 723 (FIGS. 7A-7B) and an SPR joint 722 (FIGS. 7C-7D) formed using SPR system 100. In this embodiment, both joints 722, 723 were formed in the same stack of metal substrates, where metal substrate 701 was a 6xxx aluminum alloy having a thickness of 2.5 mm and metal substrate 703 was a 7xxx aluminum alloy having a thickness of 2.8 mm. The same type of rivet 706 was used in both joints 722, 723, and unlike rivet 406, rivet 706 is not hollow along its entire length. In this example, conventional SPR joint 723 developed cracks 730 in metal substrates 701, 703, while SPR joint 722 did not. Additionally, the HH of SPR joint 723 was 0.36 mm and the T min is 0.784 mm, the interlock is 0.603 mm, the HH of the SPR joint 722 is -0.20 mm, and T min 0.374 mm, and the interlock was 0.529 mm. From these results, it can be seen that the SPR joint 722 (unlike the joint 723) did not cause cracks, and furthermore, the SPR joint 722 had a T min and HH was reduced (and negative) so it was a better and improved joint.
[0030] FIG. 8 shows additional examples of conventional SPR joints compared to SPR joints formed using SPR system 100. As shown in FIG. 8, material stack 1 has an upper layer of 5xxx aluminum alloy having a thickness of 1.2 mm and a lower layer of 7xxx aluminum alloy having a thickness of 1.8 mm. Material stack 2 has an upper layer of 5xxx aluminum alloy having a thickness of 2.5 mm and a lower layer of 7xxx aluminum alloy having a thickness of 1.8 mm. Both material stack 1 and material stack 2 were subjected to a conventional SPR process and an SPR process using SPR system 100 using the same type of rivet. As shown, during the conventional SPR process, in both material stack 1 and material stack 2, the button of the joint cracked and the interlock was greater than 0.4 mm, and the SPR quality was unacceptable. In contrast, during the SPR process using SPR system 100, in both material stack 1 and material stack 2, the button did not crack, the interlock was greater than 0.4 mm, and the SPR quality was acceptable. Based on these results, the SPR process using SPR system 100 produced improved bonds between the upper and lower layers of both material stack 1 and material stack 2.
[0031] 1 and 2, a method of bonding a first substrate 102 with a second substrate 104 using the SPR system 100 is also described. The method may include positioning the first substrate 102 and the second substrate 104 relative to one another such that the first substrate 102 and the second substrate 104 contact one another. In some embodiments, positioning the substrates 102, 104 may include using an adhesive between the substrates 102 and 104 to facilitate positioning the first substrate 102 relative to the second substrate 104. In some non-limiting examples, at least one of the substrates 102, 104 is a high-strength aluminum alloy. In one non-limiting example, at least one of the substrates 102, 104 is a 7xxx aluminum alloy and / or a 6xxx aluminum alloy.
[0032] The method includes pre-heating the first substrate 102 and the second substrate 104 at the target location 112 to locally melt the first substrate 102 and the second substrate 104. In some embodiments, pre-heating the substrates 102, 104 includes heating the substrates 102, 104 to a melting temperature for a melting time. In certain aspects, heating the substrates 102, 104 includes heating the substrates 102, 104 for a melting time of less than 2 seconds, e.g., 1000 milliseconds or less, e.g., less than 500 milliseconds, or e.g., less than 300 milliseconds. In various aspects, heating the substrates optionally includes heating the substrates 102, 104 to a melting temperature of at least 500° C. In some embodiments, pre-heating the substrates 102, 104 includes heating the substrates 102, 104 to locally melt the substrates 102, 104 at least at the interface between the substrates 102 and 104. In various embodiments, heating the substrate 102, 104 includes heating the substrate with a RSW system, where the heating includes supplying a current to the electrodes 116A-116B of the RSW system. In some optional examples, supplying a current to the electrodes 116A-116B may include supplying a current of 10 kA to 22 kA. In one non-limiting example, pre-heating the substrate 102, 104 includes supplying a current to the electrodes 116A-116B and heating the substrate 102, 104 to a melting temperature of at least 500° C. for a melting time of less than 1000 milliseconds.
[0033] The method includes holding the substrates 102, 104 and driving the rivet 106 with a driver 110 so that the rivet 106 penetrates the first substrate 102 at a target location 112. In various embodiments, the rivet 106 is driven into the target location 112 before a molten region 114 (formed in a preheating step) solidifies. In this step, the rivet 106 at least partially pierces the second substrate 104 and the base 118 expands or otherwise deforms within the second substrate 104.
[0034] FIG. 9 is a cross-sectional view of metal substrates 902, 904 during a bonding process using the SPR system 100 after preheating and before the SPR process. In this embodiment, each of the metal substrates is a 7xxx aluminum alloy. In the embodiment of FIG. 9, the metal substrates 902, 904 form the target location 112. In certain embodiments, as shown in FIG. 9, the interface 934 of the metal substrates 902, 904 at the target location 112 is partially locally melted (e.g., the interface 934 includes a melted portion 936 and a non-melted portion 938). In some embodiments, the partially locally melted interface 934 may be achieved by controlling the heat applied during preheating by the preheating system. In other embodiments, the entire interface 934 may be locally melted.
[0035] 10A-10D show yet another non-limiting example of a comparison between a conventional SPR joint 1023 (FIGS. 10A-10B) and an SPR joint 1022 (FIGS. 10C-10D) formed using the SPR system 100. In this embodiment, both joints 1022, 1023 are formed in the same stack of metal substrates, where metal substrate 1001 is a 7xxx aluminum alloy having a thickness of 1.8 mm and metal substrate 1003 is a 7xxx aluminum alloy having a thickness of 1.8 mm. The same type of rivet 1006 was used in both joints 1022, 1023. The interface of the target area of SPR joint 1022 was partially melted locally during preheating. In this example, conventional SPR joint 1023 developed cracks 1030 in metal substrates 1001, 1003, while SPR joint 1022 did not. Furthermore, the HH of the SPR junction 1023 is 0.35 mm, and T min is 0.559 mm, the interlock is 0.621 mm, the HH of the SPR joint 1022 is 0.02 mm, and the T minThe thickness was 1.302 mm and the interlock was 0.839 mm. From these results, SPR joint 1022 was a better and improved joint since it did not cause cracks (unlike joint 1023) and further reduced HH and increased interlock. As shown in FIG. 10D, the interface of the metal substrates 1002, 1003 at the target location is clear with slight melting observed, indicating that complete localized melting of the interface at the target location is not required to provide an improved SPR joint according to the embodiment.
[0036] Provided below is a collection of exemplary embodiments, including at least some explicitly listed as "Examples" that provide further description of various exemplary embodiments according to the concepts described herein. These examples are not intended to be mutually exclusive, exhaustive, or limiting, and the present disclosure is not limited to these examples, but rather encompasses all possible modifications and variations within the scope of the presented claims and their equivalents.
[0037] Example 1. A self-piercing riveting system comprising a localized melting system configured to locally melt a target location on a metal substrate, and a driver configured to drive a rivet into the metal substrate at the target location after the target location has locally melted to form a joint.
[0038] Example 2. The self-pierce riveting system of any preceding or subsequent example or combination of examples, wherein the localized melting system comprises a resistance spot welding system.
[0039] Example 3. The self-piercing riveting system of any preceding or subsequent example or combination of examples, wherein the localized melting system is configured to heat the target location to a temperature of at least 500° C. for less than 1 second.
[0040] Example 4. The self-pierce riveting system of any preceding or subsequent example or combination of examples, further comprising a controller communicatively coupled to the local melting system and the driver, the controller configured to control the local melting system to apply heat to a melting temperature for a melting time.
[0041] Example 5. The self-pierce riveting system of any preceding or subsequent example or combination of examples, wherein the melt time is greater than 0 seconds and less than or equal to 1000 milliseconds, and the melt temperature is at least 500°C.
[0042] Example 6. The self-piercing riveting system of any preceding or subsequent example or combination of examples, wherein the self-piercing riveting system is configured to form the joint in the metal substrate comprising a 7xxx aluminum alloy less than 5 mm thick.
[0043] Example 7. A method for joining at least two metal substrates, comprising locally melting a target location on the at least two metal substrates, and after locally melting the target location, driving the rivet into the target location using a driver such that the rivet penetrates the at least two metal substrates at the target location.
[0044] Example 8. The method of any preceding or subsequent example or combination of examples, wherein at least one of the two metal substrates comprises a 7xxx aluminum alloy.
[0045] Example 9. The method of any preceding or subsequent example or combination of examples, wherein each of the at least two metal substrates comprises a thickness of 5 mm or less.
[0046] Example 10. The method of any preceding or subsequent example or combination of examples, wherein locally melting the target location includes welding the target location to a melting temperature using a resistance spot welding system for a melting time.
[0047] Example 11. The method of any preceding or subsequent example or combination of examples, wherein the melt time is greater than 0 seconds and less than 1 second.
[0048] Example 12. The method of any preceding or subsequent example or combination of examples, wherein the melt time is greater than 0 seconds and less than or equal to 1000 milliseconds.
[0049] Example 13. The method of any preceding or subsequent example or combination of examples, wherein the melting temperature is at least 500°C.
[0050] Example 14. The method of any preceding or subsequent example or combination of examples, wherein driving the rivet into the target location with the driver after locally melting the target location includes driving the rivet into the target location before the target location solidifies.
[0051] Example 15. A joint formed by the method described in any preceding or subsequent example or combination of examples.
[0052] Example 16. A method for joining at least two metal substrates, comprising: welding the at least two substrates at a target location for a welding time longer than 0 seconds and less than 1 second such that the temperature at the target location is at least 500°C; and after welding, driving the rivet at the target location such that the rivet penetrates the at least two metal substrates at the target location.
[0053] Example 17. The method of any preceding or subsequent example or combination of examples, wherein at least one of the two metal substrates comprises a 7xxx aluminum alloy.
[0054] Example 18. The method of any preceding or subsequent example or combination of examples, wherein each of the at least two metal substrates comprises a thickness of 5 mm or less.
[0055] Example 19. The method of any preceding or subsequent example or combination of examples, wherein the welding time is greater than 0 seconds and less than or equal to 1000 milliseconds.
[0056] Example 20. The method of any preceding or subsequent example or combination of examples, wherein driving the rivet into the target location after welding the target location includes driving the rivet into the target location with a driver before solidification of the target location.
[0057] Example 21. The method of any preceding or subsequent example or combination of examples, further comprising applying an adhesive between the at least two metal substrates at the target location prior to welding.
[0058] Example 22. A joint formed by the method described in any preceding or subsequent example or combination of examples.
[0059] Example 23. The method of any preceding or subsequent example or combination of examples, wherein locally melting the target area and / or welding the target area includes partially locally melting the interface of the metal substrate at the target area.
[0060] Example 23. The method of any preceding or subsequent example or combination of examples, wherein locally melting the target area and / or welding the target area includes locally melting the entire interface of the metal substrate at the target area.
[0061] The subject matter of the embodiments has been described herein with specificity to meet statutory requirements, but this description is not necessarily intended to limit the scope of the claims. The claimed subject matter may be embodied in other ways, may include different elements or steps, and may be used in conjunction with other existing or future technologies. This description should not be construed as implying a particular order or arrangement between the various steps or elements, unless the order of the individual steps or arrangement of the elements is explicitly described. In particular, references to directions such as "upper", "lower", "top", "bottom", "left", "right", "front", and "rear" are intended to refer to the orientation of the components and directions as shown and described in the figure(s) to which reference is made. In the drawings and description, like numerals are intended to represent like elements.
[0062] Aspects and features of the present disclosure may be used with any suitable metal substrate, including, but not limited to, aluminum, aluminum alloys, steel, steel-based materials, nickel, nickel-based materials, copper, copper-based materials, cast iron, titanium, titanium-based materials, aluminum clad alloys, monolithic alloys, roll-bonded alloys, and / or various other metals or combinations of metals. Aspects and features of the present disclosure may be particularly useful for bonding aluminum and / or aluminum alloys. In this description, reference is made to alloys identified by aluminum industry designations such as "series" or "7xxx". For an understanding of the most commonly used numbering systems in naming and identifying aluminum and its alloys, please refer to "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Compositions Limits for Aluminum Alloys in the Form of Castings and Ingot" (both published by the Aluminum Association).
[0063] The above-mentioned aspects are merely possible examples of implementations and are described merely for a clear understanding of the principles of the present disclosure. Many variations and modifications may be made to the above-mentioned embodiment(s) without substantially departing from the spirit and principles of the present disclosure. All such modifications and modifications are intended to be included herein within the scope of the present disclosure, and all possible claims to individual aspects or combinations of elements or steps are intended to be supported by the present disclosure. Moreover, although specific terms are used in the present specification and the following claims, they are used in a generic and descriptive sense only and not for the purpose of limiting the described embodiments, nor the scope of the following claims.
Claims
1. a localized melting system configured to locally melt a target location on the metal substrate; a driver configured to locally melt the target location and then drive a rivet into the metal substrate at the target location to form a joint; A self-piercing riveting system comprising:
2. The self-pierce riveting system of claim 1 , wherein the localized melting system comprises a resistance spot welding system.
3. The self-pierce riveting system of claim 1 , wherein the localized melting system is configured to heat the target location to a temperature of at least 500° C. for less than 1 second.
4. 2. The self-pierce riveting system of claim 1, further comprising a controller communicatively coupled to the localized melting system and the driver, the controller configured to control the localized melting system to apply heat to a melting temperature for a melting time.
5. 5. The self-pierce riveting system of claim 4, wherein the melt time is greater than 0 seconds and less than or equal to 1000 milliseconds, and the melt temperature is at least 500°C.
6. 2. The self-piercing riveting system of claim 1, wherein the self-piercing riveting system is configured to form the joint in the metal substrate, the metal substrate comprising a 7xxx aluminum alloy having a thickness of less than 5 mm.
7. 1. A method for joining at least two metal substrates, comprising the steps of: locally melting target locations on the at least two metal substrates; after locally melting the target location, driving the rivet into the target location using a driver such that the rivet penetrates the at least two metal substrates at the target location; The method comprising:
8. The method of claim 7 , wherein at least one of the two metal substrates comprises a 7xxx aluminum alloy.
9. The method of claim 7 , wherein each of the at least two metal substrates comprises a thickness of 5 mm or less.
10. The method of claim 7 , wherein locally melting the target location comprises welding the target location with a resistance spot welding system to a melting temperature for a melting time.
11. The method of claim 10, wherein the melting time is greater than 0 seconds and less than 1 second.
12. The method of claim 10, wherein the melt time is greater than 0 seconds and less than or equal to 1000 milliseconds.
13. The method of claim 10, wherein the melting temperature is at least 500°C.
14. 8. The method of claim 7, wherein driving the rivet into the target location with the driver after locally melting the target location comprises driving the rivet into the target location before solidification of the target location.
15. A joint formed by the method of claim 7.
16. 1. A method for joining at least two metal substrates, comprising the steps of: welding the at least two metal substrates at a target location such that the temperature at the target location is at least 500° C. for a welding time greater than 0 seconds and less than 1 second; driving the rivet into the target location after welding such that the rivet penetrates the at least two metal substrates at the target location; The method comprising:
17. 17. The method of claim 16, wherein at least one of the two metal substrates comprises a 7xxx aluminum alloy.
18. The method of claim 16 , wherein each of the at least two metal substrates comprises a thickness of 5 mm or less.
19. 17. The method of claim 16, wherein the welding time is greater than 0 seconds and less than or equal to 1000 milliseconds.
20. 17. The method of claim 16, wherein driving the rivet into the target location after welding the target location comprises driving the rivet into the target location with a driver prior to solidification of the target location.
21. The method of claim 16 , further comprising applying an adhesive between the at least two metal substrates at the target location prior to welding.
22. A joint formed by the method of claim 16.
Citation Information
Patent Citations
Method of joining aluminium alloy sheets of the AA7000-series
US20140290064A1
Method and System for Enhancing Rivetability
US20170044637A1
Mechanical bonding device and mechanical bonding method
WO2017002976A1