Method for producing improved quality bulk SiC single crystals using a SiC seed crystal having a temporary protective oxide layer, and SiC seed crystal having a protective oxide layer

By applying a protective oxide layer to SiC seed crystals and removing it in situ before growth, the method addresses surface impurities, resulting in high-quality SiC bulk single crystals with reduced defects and improved yield.

JP2024539552AInactive Publication Date: 2024-10-29SICRYSTAL GMBH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024518465
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-17
Filing Date
2023-05-17
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The presence of impurities and contaminant particles on the surface of SiC seed crystals during the crystal growth process leads to defects such as dislocations, inclusions, and polytype changes in SiC bulk crystals, reducing their quality and yield.

Method used

A silicon carbide seed crystal with a protective oxide layer having controlled thickness variations is used, which is applied to the growth surface and remains until just before the start of the sublimation process, protecting against impurity deposition, followed by an in situ etch-back process to expose a clean surface for crystal growth.

Benefits of technology

This method produces high-quality SiC bulk single crystals with reduced defects, improving the yield and quality of SiC wafers and semiconductor components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539552000001_ABST
    Figure 2024539552000001_ABST
Patent Text Reader

Abstract

The present invention relates to a silicon carbide substrate for use as a crystal seed, comprising a silicon carbide single crystal disk coated with a protective oxide layer. The protective oxide layer is intended to be removed to expose an ideal and clean surface of the silicon carbide single crystal disk. The present invention also relates to a method for producing at least one silicon carbide bulk single crystal by sublimation growth using a silicon carbide substrate with a protective oxide layer as a seed crystal. The protective oxide layer is removed from the seed crystal surface by a back-etch process performed in situ in a crystal growth crucible, i.e. after the seed crystal is placed inside the growth crucible and before the sublimation deposition on the growth surface starts, to expose the underlying silicon carbide single crystal disk.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicon carbide (SiC) seed crystal having a protective oxide layer for use as a seed crystal in a sublimation process, and a method for producing improved quality bulk SiC single crystals using the SiC seed crystal. [Background technology]

[0002] Silicon carbide (SiC) substrates are commonly used in the semiconductor industry, such as in the manufacture of semiconductors and electronic devices. Traditionally, SiC substrates are made from a bulk SiC single crystal (also called an ingot), which is sliced ​​using a multi-wire saw or other suitable cutting process, such as laser-assisted cutting, to obtain a number of SiC substrates. The surface of the SiC substrate is then prepared by a multi-stage polishing process in preparation for a subsequent epitaxial process in which a single crystal layer of a material, such as SiC or GaN, is deposited on the polished SiC substrate. The physical properties of such a single crystal layer and devices made from such a single crystal layer depend critically on the quality of the underlying SiC substrate, and thus also on the quality of the original bulk SiC single crystal itself.

[0003] SiC bulk single crystals are generally grown by physical vapor deposition (PVT) from a suitable sublimed source material and a seed crystal. For example, a physical vapor deposition (PVT) process for producing SiC bulk crystals is disclosed in U.S. Pat. No. 8,865,324, which uses a SiC single crystal disk as a seed for growing a bulk single crystal. The SiC single crystal seed is placed in a crucible of a PVT growth system together with a suitable source material. The source material is sublimated under controlled temperature and pressure conditions, and the resulting sublimed material is directed toward and deposited on the SiC seed under the influence of a suitable temperature gradient to grow a crystal.

[0004] It should be noted that in this disclosure, the following terms are used to distinguish the different components: First, the SiC starting material placed inside the crucible and on which the sublimated source material grows is called the "seed crystal" or "seed". In this disclosure, this seed crystal constitutes a monocrystalline disk with a growth surface on which the SiC will be deposited in the sublimation process. The grown monocrystalline is also called a "bulk crystal", "silicon carbide bulk monocrystalline", "ingot" or "monocrystalline boule". By slicing the bulk crystal, so-called "substrates" are obtained. These substrates are used by integrated circuit manufacturers to grow epitaxial layers on the substrate to produce so-called "wafers" that may later constitute semiconductor structures. By dicing the wafer, the individual "dies", also called "chips", are produced.

[0005] The condition and quality of the SiC seed, especially the deposition surface, are major factors in the final quality of the crystal grown thereon. In particular, during the polishing process and / or during handling of the seed after the polishing process, various types of impurities, such as contaminating atoms, particles and dirt, can fall and adhere to the surface of the SiC seed. These surface impurities promote the generation of various defects in the bulk crystal grown on the seed, reducing the quality of the crystal grown thereon. For example, impurity atoms, molecules and / or clusters deposited on the seed surface can act as initiation points for dislocations, such as threading screw dislocations (TSDs) and threading edge dislocations (TEDs), on the growing crystal, which continue to grow into the bulk crystal during the growth process. Such dislocations adversely affect the quality of the grown bulk crystal, the SiC substrate produced from the bulk crystal, and ultimately the epitaxial quality of the single crystal layer grown on such SiC substrate.

[0006] Furthermore, particles (e.g., silicon, carbon, and silicon carbide) that remain attached to the surface of the SiC seeds after seed treatment can overgrow during the crystal growth process, leading to the creation of defects known as inclusions, or, depending on their dimensions, can generate dislocations or microtubes within the growing crystal. Furthermore, deposited impurities and particles from materials / elements other than SiC can even result in polytype changes of the growing bulk crystal (e.g., change in crystal structure from 4H to 6H or 15R), depending on the chemical composition of the impurities.

[0007] All of the above mentioned defects reduce the quality and yield of the grown bulk crystals and SiC substrates, and consequently the quality of the epilayers fabricated on such SiC substrates and the electronic components fabricated therefrom.

[0008] In the past, attempts have been made to improve the quality of bulk crystals grown on seeds, taking into account that impurities accumulate on the surface of the seed crystal during the polishing process of the seed and / or during handling of the seed after processing.

[0009] For example, JP 2008-024554 A describes a method for improving the quality of crystals grown on SiC single crystal seeds. According to this method, dislocations in the SiC single crystal are exposed by selective etching and then overgrown together with an oxide layer and a protective film. An ex-situ anisotropic etch-back is then performed, which exposes the original single crystal seed surface together with the filled etch pits. The dislocations originally present in the seed crystal can no longer be propagated in the subsequent growth process to the crystal subsequently grown thereon. However, although this method aims to reduce the effect of dislocations formed in the seed, it does not eliminate the cause of the formation of such defects, in other words it does not prevent impurity atoms and particles from accumulating on the surface of the seed during various handling processes of the seed (e.g. during the placement of the seed inside the growth crucible) before the actual crystal growth process begins, i.e. before SiC starts to deposit on the seed growth surface. As a result, deposition of impurities on the surface of SiC seeds processed using this technique can still occur during handling of the seeds, thus resulting in the formation of further defects in the crystal grown thereon, such as the creation of new dislocations, and / or causing polytype changes in the SiC crystal structure. In particular, accurate transfer of polytype information from the seed crystal to the crystal grown thereon is an essential prerequisite for polytype growth of SiC single crystals. However, SiC seeds with non-polytype surfaces, such as those produced according to the disclosure of JP2008-024554A, including regions with SiO2 or other oxides to seal etch pits, promote polytype changes during crystal growth, making the grown crystal unusable and thus reducing yields.

[0010] Therefore, there remains a need for techniques that make it possible to improve the quality and yield of SiC bulk single crystals and SiC single crystal substrates by reducing one of the main causes of the occurrence of defects and / or polytype changes on SiC bulk crystals and SiC single crystal layers, namely the actual crystal growth process, and in particular the presence of impurities and contaminating particles on the surface of the SiC seed crystal before the deposition of SiC on the seed growth surface. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2008-024554 A Summary of the Invention

[0012] The present invention has been made in consideration of the shortcomings and drawbacks of the prior art, and has an object to provide a silicon carbide (SiC) single crystal seed crystal in which the amount of impurities and contaminant particles is reduced before SiC is deposited on the seed growth surface, and a method for producing an improved quality SiC bulk single crystal using the silicon carbide (SiC) single crystal seed crystal.

[0013] This object is solved by the subject matter of the independent claims. Advantageous embodiments of the invention are the subject matter of the dependent claims.

[0014] According to the invention, there is provided a silicon carbide seed comprising a silicon carbide single crystal disk and a protective oxide layer covering a region of a first surface of the silicon carbide single crystal disk, the first surface being a growth surface in the volume crystal growth process, the protective oxide layer being further characterized in that along the covered region, the protective oxide layer has a thickness variation above and below an average thickness of the protective oxide layer less than a predetermined tolerance.

[0015] Thus, the ideal property of the SiC single crystal disk, especially the growth surface, is that it is protected by an oxide layer from the deposition of new defect sources, such as dirt, particles, impurity atoms, etc., during further handling operations of the silicon carbide disk used as a seed crystal, such as mounting the seed crystal in a holder for inserting and holding the seed crystal in a growth crucible. The oxide layer remains on the seed until just before the start of the SiC deposition process, but at least after the intended placement in the growth crucible. The growth surface is, for example, the (000-1) plane for 4H crystal growth and the (0001) plane for 6H crystal growth. Other orientations and lattice planes are also intended to be included in the present disclosure.

[0016] According to a further development, the average thickness is the average of the thickness of the protective oxide layer over the entire area covered by the protective oxide layer and / or the average thickness of the protective oxide layer is between 5 nm and 20 nm.

[0017] According to a further development, the protective oxide layer consists of silicon dioxide and has an average thickness between 1 nm and 25 nm, with a predetermined tolerance of 0.5 nm, so that the thickness of the protective oxide layer at any location of the coated area of ​​the first surface does not deviate by more than 0.5 nm above or below the average thickness of the protective oxide layer.

[0018] According to a further development, the deviation in the thickness of the protective oxide layer is no more than 0.3 nm above or below the average thickness.

[0019] According to further developments, the first surface covered with the protective oxide layer corresponds to a crystal volume growth surface of the silicon carbide single crystal disk (e.g. the C-face of 4H crystal growth) and / or the silicon carbide single crystal disk has a thickness of 500 μm to 5000 μm, or 800 μm to 3000 μm and / or the silicon carbide disk has a diameter of 150 mm or more, preferably 200 mm or more.

[0020] According to a further development, the first surface of the silicon carbide single crystal disk has a surface roughness of 0.5 nm to 1 nm in the thickness direction of the silicon carbide single crystal disk.

[0021] According to a further development, the silicon carbide single crystal disk is made of one of the 4H-, 6H-, 15R- and 3C modifications of silicon carbide, preferably the 4H-SiC modification, and / or the silicon carbide single crystal disk has an off-axis orientation characterized by an off-axis angle of 0-4°, preferably 0-2° of the off-axis orientation.

[0022] According to a further development, the first surface of the silicon carbide single crystal disk has a surface roughness of 12000 / cm 2 less than 8000 / cm 2 and / or an etch pit density of less than 2000 / cm 2 less than 1000 / cm 2 has a screw dislocation density of less than

[0023] The present invention also provides a method for producing at least one bulk silicon carbide single crystal by sublimation growth in a growth crucible having at least one crystal growth region for placing at least one seed crystal therein and a source material region for storing powdered or partially consolidated silicon carbide material for sublimation, the method comprising the steps of providing at least one silicon carbide seed crystal with a protective oxide layer according to the present invention for use as at least one seed crystal, fixing the at least one seed crystal to a holding device and inserting the seed crystal fixed to the holding device into the growth region of the growth crucible, surrounding the growth crucible with a thermal insulating material, and sublimating the source material from the source material region. and performing a sublimation growth process in which a silicon carbide bulk single crystal is grown from the silicon carbide growth gas phase by deposition from the SiC growth gas phase on a seed crystal disposed in the crystal growth region, the method being characterized by the step of performing an etch-back process in the crystal growth region after at least one seed crystal having a protective oxide layer is disposed in the crystal growth region and prior to commencing the sublimation growth process, the etch-back process being adapted to remove the protective oxide layer from a surface of the seed crystal and expose the underlying silicon carbide single crystal disk.

[0024] Therefore, the manufacturing process is designed such that, before the start of the growth process, the protective oxide layer is removed in situ from the SiC substrate, e.g., by setting suitable silicon and carbon vapor pressures in the growth chamber, thereby exposing the underlying surface of the SiC single crystal seed free of impurities, particles and impurity atoms, so that the subsequent crystal growth can be initiated on an ideal seed surface and high quality crystals can be produced.

[0025] According to a further development, the step of providing at least one silicon carbide seed with a protective oxide layer comprises a step of performing an oxidation process on the silicon carbide single crystal disk in order to cover said area on the first surface with an oxide layer, the oxidation process being performed before fixing the silicon carbide substrate in a holding fixture and inserting the silicon carbide substrate fixed in the holding fixture into the growth region of the growth crucible.

[0026] According to a further development, at least one silicon carbide seed crystal used as a crystal seed is provided with a first surface which corresponds to a growth surface of the silicon carbide single crystal disk and / or the growth crucible used in the production method is partly made of graphite.

[0027] According to a further development, the etch-back process comprises the steps of: supplying a gaseous atmosphere of an etch-back component to the crystal growth region in the growth crucible and setting a given vapor pressure of the etch-back gaseous atmosphere selected to etch away the protective oxide layer, the etch-back component comprising silicon and / or carbon, and maintaining the etch-back process for a time dependent on the thickness of the protective oxide layer to completely expose the area of ​​the first surface covered by the protective oxide layer. Alternatively, the etch-back is performed as a purely thermal etching process, where no additional etch-back component is added, but where high temperature and vacuum treatment are used to remove the protective oxide layer.

[0028] According to a further development, the etch-back process is performed at (i) a pressure between 0.1 mbar and 100 mbar, and (ii) a pressure between 1×10 -7 mbar~1×10 -3 (iii) in a high vacuum process step at a pressure in the mbar range; (iv) in a purging process step with an inert gas; (v) using a reducing gas selected from the group of reducing gases comprising SF, Cl, CHF, CF, NF, CF or mixtures thereof in a growth crucible or under one or a combination thereof.

[0029] According to a further development, the etch-back process is carried out under one of the following temperature conditions: a temperature above 1200°C and below the sublimation temperature of the source material, preferably below 1400°C, and a temperature above 1650°C and below the sublimation temperature of the source material, preferably below 1850°C.

[0030] According to a further development, the oxidation process comprises one or a combination of the following: dry oxidation with oxygen and possibly an inert gas, the inert gas comprising nitrogen and / or argon; wet oxidation with a mixture of oxygen, water and possibly an inert gas; oxidation at a temperature between 15°C and 50°C (for example 40°C) in a defined gas atmosphere; oxidation with ozone; oxidation with oxygen plasma; and / or oxidation with at least one of Na2CO3, H2O2, NaOH, KIO3, KClO3, KMnO4 and CrO3.

[0031] Overall, the SiC seed crystal according to the invention and the method for producing a bulk SiC single crystal using the same allow for the production of a higher quality bulk SiC single crystal by using a SiC seed crystal having a temporary protective oxide layer that is only removed in situ after the seed crystal is introduced into the growth crucible and before the start of the actual sublimation growth. This allows for a substantial improvement in bulk crystal quality thanks to the surface of the seed crystal exposed by the etch-back, which has a reduced amount of impurities and contaminating particles. Thus, the formation of bulk crystal defects, such as dislocations, inclusions, and / or changes in the SiC crystal structure, does not occur any more or is at least significantly reduced compared to conventionally produced bulk SiC single crystals. Thus, the bulk SiC single crystal produced according to the invention provides a higher quality and thus allows for an improved yield and quality of SiC wafers and semiconductor components produced from the SiC wafers.

[0032] The accompanying drawings are incorporated in and form a part of this specification for the purpose of explaining the principles of the invention, and are not to be construed as limiting the invention to only illustrated and described examples of how the invention can be made and used.

[0033] Further features and advantages will become apparent from the following more detailed description of the invention, which is illustrated in the accompanying drawings. [Brief description of the drawings]

[0034] [Figure 1] FIG. 2 is a schematic cross-sectional view of a SiC seed crystal having a temporary protective oxide layer in accordance with the present invention.

[0035] [Diagram 2] FIG. 2 is a schematic cross-sectional view of a SiC seed crystal according to the present invention, secured in a holding fixture and showing impurities building up on the surface of the protective oxide layer.

[0036] [Diagram 3] FIG. 3 is a schematic cross-sectional view of a growth apparatus for producing a bulk SiC single crystal by sublimation growth according to the present invention, in which the SiC seed crystal shown in FIG. 2 is placed inside and used as a seed crystal.

[0037] [Figure 4] FIG. 4 is a schematic cross-sectional view of the growth apparatus shown in FIG. 3 at a subsequent manufacturing stage after etching back the protective oxide layer from the SiC seed crystal and before starting the sublimation growth process.

[0038] [Diagram 5] FIG. 5 is a schematic cross-sectional view of the growth apparatus shown in FIG. 4 at a subsequent manufacturing stage, the sublimation growth stage, in which a SiC bulk single crystal is grown on a SiC seed crystal after the protective oxide layer has been removed.

[0039] [Figure 6] 2 is a flow chart showing a sequence of steps of a method for producing bulk SiC single crystals by sublimation growth according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which exemplary embodiments of the invention are shown. The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art. Like numbers refer to like elements throughout.

[0041] With reference to FIG. 1, a SiC seed crystal 100 with a protective oxide layer 110 according to the present invention is shown. The SiC seed crystal 100 has a silicon carbide monocrystalline disk 120 covered with a protective oxide layer 110 on the whole (or part) of its first surface 125, which is the surface intended for growing a SiC bulk crystal. The function of the protective oxide layer 110 is to form a temporary protective surface on which all impurities and contaminant particles 130 from the external environment can adhere, which would otherwise inevitably fall onto the deposition surface 125 of the SiC monocrystalline disk 120 while preparing for the subsequent growth process, for example when the seed crystal is fixed to a holding fixture 140. The SiC seed crystal 100 according to the present invention allows the impurities and contaminant particles 125 to be captured on the protective oxide layer 110, as shown in FIG. 2. The protective oxide layer 110 is intended to be removed before the start of the actual sublimation growth process, i.e. before the start of deposition of SiC on the seed growth surface, but only after the SiC seed crystal 100 with the protective oxide layer 110 has been introduced into the growth crucible, so as to obtain a SiC single crystal layer seed with an impurity-free deposition surface 125.

[0042] The protective oxide layer 110 is preferably made of an oxide material such as silicon dioxide, since it can be easily removed by an etch-back process as described below. In order to efficiently remove the protective oxide layer 110 uniformly over the entire covered surface 125 during a single etch-back process, the protective oxide layer 110 is formed on the SiC single crystal layer 110 by a suitable oxidation process and with selected parameters that allow achieving a uniform oxide thickness over the entire area 125 covered by the oxide layer 110. In particular, the protective oxide layer 110 is formed with a thickness variation along the covered area on the surface 125 below and above an average thickness of the protective oxide layer that is less than a predetermined tolerance, where the average thickness is the average value of the thickness of the protective oxide layer over the entire area covered by the protective oxide layer. Thus, the thickness of the protective oxide layer does not deviate above or below the average thickness at any location on the area of ​​the first surface 125 covered by the protective layer 110 by more than a predetermined tolerance.

[0043] The SiC disk 120 is preferably made of 4H modification of SiC. However, the SiC disk 120 may be made of any of the other SiC structural variants (polytypes), such as the 6H, 15R, and 3C variants of silicon carbide. For example, the deposition surface 125 of the cut SiC disk 120 preferably corresponds to the (000-1) crystal plane (i.e., the C-plane for PVT growth of 4H SiC bulk crystals), which is the preferred crystal plane of seed substrates used in the semiconductor industry for the growth of SiC bulk crystals by PVT. Furthermore, depending on the PVT characteristics required for the subsequent crystal growth, the SiC single crystal disk 120 may be cut and / or processed such that the crystal axis of the C-plane is inclined by an off-axis orientation from a direction perpendicular to the growth surface 125 of the SiC single crystal disk 120. Preferably, the off-axis orientation of the SiC disk 120 is characterized by an off-angle of 0 to 4°.

[0044] The cut SiC single crystal disk 120 can then be treated (all or a combination of individual treatments) by processing steps commonly used in the art, such as grinding, lapping and polishing (by mechanical and / or chemical-mechanical means) of the front and / or back surface of the SiC disk 120 to remove scratches, surface defects and subsurface damage. In order to form a uniform oxide layer 110 thereon, the SiC disk 120 is preferably treated to provide a smooth deposition surface 125 with a surface roughness of 0.5 nm to 1 nm in the thickness direction of the SiC layer 120, and preferably has a thickness of about 500 μm to about 5000 μm as described above. Chamfers can also be added to the front and back surfaces of the cut SiC disk 120. Alignment notches or flats can also be defined. The SiC disk 120 preferably has a substantially circular disk shape, except for the presence of certain dies such as alignment notches and flats, and has sufficient mechanical stability to be self-supporting. The SiC disk 120 thus produced is intended to meet the industrial requirements for manufacturing semiconductor SiC bulk crystals.

[0045] Conventionally, the thus treated SiC single crystal disk 120 with the ideal characteristics of the deposition surface 125 is subjected to further operations, such as fixing to a holding fixture 140 for holding the seed in a growth crucible, so that it can be used as a seed crystal for growing a SiC bulk single crystal thereon. However, since these operations cannot be performed in a clean room due to the high concentration of dust, particles and other impurities generated in the atmosphere during these handling operations, the surface 125 of the ideally produced SiC disk 110 is generally recontaminated with metallic and / or non-metallic impurity atoms, inorganic or organic impurities or particles during these operations.

[0046] In order to maintain the ideal properties of the deposition surface 125 of the SiC seed crystal 120 until the deposition of SiC on the seed growth surface 125 starts, the concept underlying the present invention is therefore to form a temporary protective oxide layer 110 on the top of the SiC disk 120, i.e. on the deposition surface 125. More specifically, the oxidation of the deposition surface 125 is performed immediately after the above-mentioned treatment of the SiC slice 120, so that the protective oxide layer 110 is created before dirt, impurity atoms or particles can accumulate on the ideal surface 125 of the SiC slice 120 by physisorption or chemisorption during further handling of the seed.

[0047] For example, a SiC substrate 100 with a protective oxide layer 110 can be manufactured as follows. First, a single crystal slice or disk 120, preferably about 500 μm to about 5000 μm thick, is cut from a high-quality bulk SiC single crystal, for example by sawing or laser-assisted cutting, generally in a direction perpendicular to the longitudinal axis of the bulk SiC single crystal or inclined by a given off-angle. Since the cut SiC disk 120 already has a high crystalline quality of polytype with a low density of inclusions, dislocations and / or microtubes and a low content of impurities, further treatment processes to reduce the adverse effect of existing defects on the subsequent crystal growth, such as the treatment processes described in JP 2008-024554 A, do not further result in significant improvement of the quality of the crystal grown on the seed. For example, before applying the oxide layer 110, the silicon carbide single crystal disk 120 has a lattice density of 12000 / cm 2 less than 8000 / cm 2 and / or has an etch pit density of less than 2000 / cm 2 less than 1000 / cm 2 has a screw dislocation density of less than

[0048] For the oxidation process, the SiC slice (or disk) 120 may be placed in a conventional oxidation chamber. For example, the SiC slice 120 may be placed in a closed chamber with an inlet and an outlet for supplying the oxidizing components, and subjected to a controlled oxidation treatment by setting and maintaining an oxidizing atmosphere of suitable composition and under controlled pressure and temperature. In the oxidation chamber, the gas or chemical composition of the oxidizing atmosphere, as well as the setting of the temperature, atmospheric pressure and oxidation process time, may be controlled. Thus, a protective oxide layer having a desired composition and thickness, i.e. a constant and uniform thickness, may be obtained. For example, an oxide layer having a thickness of 1 nm to 25 nm (measured on the crystal C-face of the SiC disk 120) may be obtained using such a controlled oxidation process, suitable for easy removal by a subsequent etch-back process. To form the protective oxide layer 110 according to the present invention on the SiC single crystal disk 120, several oxidation processes known in the art may be used. For example, one or more of the following processes may be used (alone or in combination): (i) dry oxidation with oxygen and optionally an inert gas, the inert gas comprising nitrogen and / or argon; (ii) wet oxidation with a mixture of oxygen, water and optionally an inert gas; (iii) Oxidation in a specified gas atmosphere at room temperature between 15°C and 50°C; (iv) oxidation by ozone; (v) oxidation with oxygen plasma, and / or (vi) Oxidation with at least one of Na2CO3, H2O2, NaOH, KIO3, KClO3, KMnO4 and CrO3.

[0049] The temperature, pressure and / or process time parameters to achieve a desired final oxide thickness can be determined by experiment and / or simulation analysis depending on the particular composition of the oxide layer 110 being formed, the oxidizing atmosphere, and the characteristics of the oxidation chamber used, such as the chamber volume and associated heating and pressure systems.

[0050] Creating a uniform oxide layer with little variation in thickness across the coated area 125 of the SiC disk 120 is a key factor to ensure that an ideal surface 125 of the SiC single crystal layer 120 is completely exposed for crystal growth after removal of the oxide layer 110 by etch-back.

[0051] The measurement of the oxide layer thickness can be performed non-destructively after the oxidation process is completed, for example by ellipsometry. Advantageously, the thickness measurement may be performed in situ (i.e., on the SiC disk 120 in the oxidation chamber) using an appropriate design of the oxidation chamber. This allows the oxidation process to be terminated when the oxide layer 110 according to the invention reaches a desired thickness.

[0052] Thus, the SiC single crystal disk 120, and more particularly the surface 125 intended to be used for crystal growth, is protected from adsorption of dirt, impurity atoms and particles during handling steps, such as fixing to a holding fixture and / or placing in a growth crucible, that must be performed before starting the deposition of SiC onto the seed growth surface to grow a SiC bulk single crystal.

[0053] Next, a method for producing at least one bulk SiC single crystal using the SiC substrate 100 according to the present invention as a seed crystal for sublimation growth will be described with reference to FIGS.

[0054] FIG. 3 shows an embodiment of a crystal growth apparatus 300 for producing a SiC bulk single crystal 301 by a sublimation growth process according to the present invention. The growth apparatus 300 includes a crystal growth crucible 310 into which a SiC seed crystal 100 for producing a SiC bulk single crystal by sublimation (also called physical vapor transport) is inserted. Specifically, the growth crucible 310 is provided with a crystal growth region 320 in which a seed crystal such as the above-mentioned SiC seed crystal 100 is disposed, and a source material region 330 for containing a source material 332 such as powdered, consolidated or partially consolidated silicon carbide that is sublimated during the sublimation growth process. For example, SiC powder may be injected into the source material region 314 as a pre-finished starting material before the start of the sublimation growth process. The seed crystal 100 is fixed to a crucible lid 315 (which is the holding device 140 in this example) and disposed inside the crucible 310 so as to be disposed opposite the SiC source material region 330. In general, the diameter of the seed crystal 100 is selected to be approximately the same as the diameter of the SiC bulk single crystal to be grown thereon. Nevertheless, the diameter of the final SiC bulk single crystal diameter may be smaller or larger than the underlying seed crystal 100 by a small deviation, for example, less than 30%. In particular, in normal wafer crystal growth, the diameter of the seed crystal is equal to or larger than the grown bulk crystal. However, the preparation of the bulk crystal may also be used to manufacture a new seed crystal that is larger. In such a case of diameter enlargement, the seed crystal is smaller than the grown bulk crystal.

[0055] The walls 312 and lid 315 of the growth crucible 310 enclose the crystal growth region 320 and the source material region 330, allowing for the creation of a controlled sublimation atmosphere within the crystal growth region 320. The growth crucible 310 preferably has a SiO2 content of at least 1.75 g / cm3, for example. 3The growth apparatus 300 is made of an electrically and thermally conductive graphite crucible material having a density of 100 / 100 / 100 / 2 ...100 / 200 / 100 / 100 / 100 / 200 / 100 / 100 / 100

[0056] The growth apparatus 300 is then placed in a reaction chamber (not shown), conventionally configured as a tubular vessel such as a quartz glass tube, surrounded by respective cooling and heating systems for generating and controlling the temperature gradients required to sublimate the source material and transport the sublimated components towards the seed crystal 120 during the sublimation growth process. For example, the heating means may be provided as an induction heating coil 12 with a controlled current, which can generate the desired temperature inside the growth crucible 310 by inducing a current circulating in the conductive wall 312 of the growth crucible 310 around the central axis 355. Under growth pressures of 0.1 mbar to 100 mbar, growth temperatures of more than 2000 degrees, in particular about 2400° C., can be achieved during the sublimation process.

[0057] During the sublimation growth process, SiC material is sublimated from the source material region 330 by the induced heat, and the sublimated gaseous components are transported to the crystal growth region 320 under the influence of the thermal gradient generated inside the crucible 310. Thus, a SiC growth gas phase is generated in the crystal growth region 320, from which a SiC bulk single crystal is grown on a seed crystal by deposition from the SiC growth gas phase.

[0058] The growth crucible 310 shown in Figures 3 to 5 is designed to grow one SiC bulk single crystal at a time. However, the SiC seed crystal 100 and the method for manufacturing a SiC bulk crystal using the SiC seed crystal 100 according to the principles of the present invention are intended to be applied to a growth crucible having multiple growth regions designed to simultaneously grow one or more SiC bulk single crystals. For example, it is envisioned to use a growth crucible having a source material region provided in a central region of the crucible and two crystal growth regions located on either side of the source material region to accommodate respective seed crystals therein, to simultaneously grow two SiC bulk crystals from the same source material.

[0059] As described above, in the method of producing at least one SiC bulk single crystal by sublimation growth according to the present invention, before starting the sublimation growth process, a protective oxide layer 110 is first deposited on the deposition surface 125 of the SiC single crystal disk 120, for example on the (000-1) (i.e. carbon) face in the case of 4H crystal growth, and then the deposition surface 125 is fixed in a holding fixture to maintain the high quality of the deposition surface 125. In this way, the deposition surface 125 is temporarily protected from the deposition of impurity atoms, particles and impurities. The SiC seed crystal 100 is then fixed in a holding fixture or crucible lid 315, a powdered or (partially) consolidated SiC source material is placed in the source material area 330, and the growth crucible 310 is covered with a thermally insulated housing 340 and inserted into the reaction chamber.

[0060] The protective oxide layer 110 with adsorbed impurity atoms, impurities and particles is then removed in situ (i.e., inside the growth crucible 310 after the SiC seed crystal 100 is placed inside the growth crucible 310 and the growth apparatus 300 is inserted into the reaction chamber) by performing an etch-back process before starting the crystal growth by sublimation. In particular, the etch-back process is performed, which may include setting the vapor pressure of the gas atmosphere of the etch-back components in the crystal growth region 320. In particular, a temperature gradient is required that promotes the dissolution of silicon dioxide compared to the deposition of SiC. As a result, silicon dioxide evaporates before the deposition of SiC.

[0061] For example, the etch-back can be accomplished by setting a low vapor pressure of an etching species, such as carbon, in the atmosphere of the growth region 320 in which the SiC substrate 100 is located. This etching atmosphere sublimes the previously formed protective oxide layer 110, including all contaminating atoms, particles and impurities that may have been deposited thereon.

[0062] The composition and respective pressure of the etch-back gaseous atmosphere are selected according to the composition of the protective oxide layer 110 so as to completely etch away the oxide material from the SiC substrate 100. In particular, several etch-back processes and conditions may be used to in-situ remove the protective oxide layer 110 from the SiC seed crystal 100. For example, the etch-back process may be performed by setting the pressure between 1 mbar and 100 mbar and / or by setting the nucleation temperature between 1200°C and 1400°C, or between 1650°C and 1850°C. The etch-back may also be performed under high vacuum or during purging with an inert gas such as argon. Furthermore, a reducing gas such as SF6, Cl2, CHF3, C2F6, NF3, CF4 or mixtures thereof may be introduced into the growth crucible 310 to selectively remove the oxide layer 110 and thus the impurity atoms, particles and impurities present thereon. Finally, some of the above-mentioned variants of the etch-back process may be combined.

[0063] The etch-back process is then maintained for a duration that depends on parameters such as the thickness and composition of the protective oxide layer, the reactivity of the etch-back gaseous atmosphere, etc., to completely expose the area of ​​the deposition surface 125 of the SiC single crystal disk 120 previously covered by the protective oxide layer 110. Thus, by setting an appropriate etching vapor pressure in the growth region 320 before starting the sublimation growth, i.e., the deposition of SiC on the growth surface, the protective oxide layer 110 that was temporarily formed on the SiC seed crystal 100 can be efficiently removed, thereby exposing the underlying ideally prepared face 125 (which is the C-face in this example) of the SiC single crystal disk 120 without any further impurities, impurity atoms or particles. As a result, it is possible to continue and start the sublimation growth of SiC bulk single crystal on the exposed face 125 of the SiC single crystal disk 120 without any further handling of the SiC single crystal disk 120, and more importantly, without the need to remove the SiC single crystal disk 120 from the growth crucible 310 and expose it to contaminants. This makes it possible to produce bulk SiC single crystals of high quality and with extremely low defect density.

[0064] In summary, the present invention allows the ideal properties of the SiC single crystal disk 120 used as a seed crystal, in particular the properties for PVT growth of the C-side of the 4H-SiC disk, to be preserved from the adverse effects caused by impurity particles and contaminants deposited on the surface 125 intended for crystal growth, by a temporary protective oxide layer formed on the seed crystal surface 125 immediately after the completion of the cutting and polishing treatments performed on the SiC single crystal disk 120 in preparation for the subsequent crystal growth process. The protective oxide layer 110 remains on the SiC seed crystal 100 until just before the start of crystal growth, i.e. just before the deposition of SiC, at least until after the SiC seed crystal 100 is placed in the crystal growth crucible 310. As a result, the deposition of dirt, particles and impurity atoms during handling operations of the SiC seed crystal 100, such as during fixing and inserting the SiC seed crystal 100 into the growth crucible 310, which may cause new crystal defects in the grown crystal, can be prevented.

[0065] Furthermore, since the method for producing a bulk SiC single crystal of the present invention is designed to remove the protective oxide layer 110 in situ before starting the growth of a bulk SiC single crystal on the seed crystal, the crystal growth can be easily started on an ideal surface 125 of the SiC single crystal disk 120, which is a part of the seed crystal 100, i.e., a surface free of impurities, particles, and impurity atoms. This allows the production of a high-quality bulk SiC single crystal.

[0066] Although certain features of the above exemplary embodiments have been described using terms such as "top", "bottom" and "upper", these terms are used solely to facilitate the description of the respective features and their relative orientation within the optical module, and should not be construed as limiting the claimed invention or any of its components to a particular spatial orientation. Furthermore, in the above disclosure, when the terms "about" or "approximately" are applied to a particular value or range, this should be understood to refer to a value or range that is as precise as the method used to measure it. For example, if no measurement error is mentioned, the expression "about 500 μm" should be construed to refer to a value that is approximately the same as "500 μm". [Explanation of symbols]

[0067] 100 SiC seed crystal 110 Protective oxide layer 120 SiC single crystal disk Deposition surface of 125 SiC disk 130 Impurities 140 Holding device 300 Growing Device 301 SiC bulk crystal 310 Crystal growth crucible 312 Crucible Wall 315 Crucible Lid 320 Crystal Growth Area 330 Raw materials area 340 Insulated housing 350 opening 355 Center axis 360 Heating Coil

Claims

1. A silicon carbide seed crystal (100), A silicon carbide single crystal disk (120); a protective oxide layer (110) covering a region of the first surface (125) of the silicon carbide single crystal disk (120); the protective oxide layer (110) is characterized by having a thickness variation along the coated area less than a predetermined tolerance above and below an average thickness of the protective oxide layer (110); Silicon carbide seed crystal (100).

2. the average thickness being the average thickness of the protective oxide layer over the entire area covered by the protective oxide layer (110); and / or the average thickness of the protective oxide layer (110) is between 5 nm and 20 nm; The silicon carbide seed crystal (100) of claim 1.

3. the protective oxide layer (110) is made of silicon dioxide and has an average thickness between 1 nm and 25 nm, and the predetermined tolerance is 0.5 nm such that the thickness of the protective oxide layer at any location of the covered area of ​​the first surface does not deviate by more than 0.5 nm above or below the average thickness of the protective oxide layer. The silicon carbide seed crystal (100) of claim 1 or 2.

4. the deviation in thickness of the protective oxide layer (110) is no more than 0.3 nm above or below the average thickness; The silicon carbide seed crystal (100) of any one of claims 1 to 3.

5. the first surface (125) covered by the protective oxide layer (110) corresponds to the C-face of the silicon carbide single crystal disk; and / or the silicon carbide single crystal disk (120) has a thickness of 500 μm to 5000 μm, or 800 μm to 3000 μm; and / or The silicon carbide disk (120) has a diameter of 150 mm or more, preferably 200 mm or more. The silicon carbide seed crystal (100) of any one of the preceding claims.

6. the first surface of the silicon carbide single crystal disk (120) has a surface roughness of 0.5 nm to 1 nm in a thickness direction of the silicon carbide single crystal disk; The silicon carbide seed crystal (100) of any one of the preceding claims.

7. the silicon carbide single crystal disk (120) is made of one of the 4H-, 6H-, 15R- and 3C modifications of silicon carbide, preferably the 4H-SiC modification; and / or the silicon carbide single crystal disk (120) has an off-axis orientation characterized by an off-axis angle of 0° to 4°, preferably 0° to 2°; The silicon carbide seed crystal (100) of any one of the preceding claims.

8. the first surface (125) of the silicon carbide single crystal disk (120) 12000 / cm 2 less than 8000 / cm 2 and / or an etch pit density of less than 2000 / cm 2 less than 1000 / cm 2 8. The silicon carbide seed crystal of claim 1 having a screw dislocation density of less than 0.1 μm.

9. 1. A method for producing at least one silicon carbide bulk single crystal (301) by sublimation growth inside a growth crucible having at least one crystal growth area (320) for placing therein at least one seed crystal (100) and a source material area (330) for storing powdered or partially consolidated silicon carbide material for sublimation, the method comprising: providing a protective oxide layer (110) according to any one of claims 1 to 8 on at least one silicon carbide seed crystal (100) for use as said at least one seed crystal; Fixing the at least one seed crystal (100) to a holding fixture and inserting the seed crystal (100) fixed to the holding fixture into the growth region of the growth crucible; wrapping the growth crucible with an insulating material; performing a sublimation growth process, sublimating the source material from the source material region, transporting the sublimated gaseous material into the crystal growth region to generate a silicon carbide growth vapor in the crystal growth region, and growing a silicon carbide bulk single crystal from the silicon carbide growth vapor onto the seed crystal disposed in the crystal growth region by deposition from the SiC growth vapor; Including, After the at least one seed crystal (100) having the protective oxide layer (110) is placed in the crystal growth zone, and before starting the sublimation growth process, performing an etch-back process in the crystal growth zone adapted to remove the protective oxide layer from a surface of the seed crystal and expose the underlying silicon carbide single crystal disk (120). The method of claim 1,

10. providing at least one silicon carbide seed crystal (100) with a protective oxide layer (110); performing an oxidation process on the silicon carbide single crystal disk to cover the area on the first surface with an oxide layer; the oxidation process is performed prior to fixing the silicon carbide seed crystal in a holding fixture and inserting the silicon carbide seed crystal, fixed in the holding fixture, into the growth region of the growth crucible.

10. The method of claim 9.

11. the at least one silicon carbide seed crystal (100) used as a crystal seed is provided with the first surface corresponding to a growth surface of the silicon carbide single crystal disk; and / or The growth crucible used in the manufacturing method is formed partially from graphite.

11. The method according to claim 9 or 10.

12. The etch-back process comprises: providing a gaseous atmosphere of an etch-back component to the crystal growth region in the growth crucible and setting a given vapor pressure of the etch-back gaseous atmosphere selected to etch away the protective oxide layer, the etch-back component comprising silicon and / or carbon; maintaining the etch-back process for a time dependent on the thickness of the protective oxide layer to completely expose the area of ​​the first surface covered by the protective oxide layer; Including, 12. The method according to any one of claims 9 to 11.

13. The etch-back process comprises: (i) at a pressure between 0.1 mbar and 100 mbar, (ii) 1 x 10 -7 mbar to 1×10 -3 In a high vacuum process step at pressures in the range of mbar, (iii) In the inert gas purging process step, (iv) SF in the growth crucible. 6 , Cl 2 , C.H.F. 3 , C 2 F 6 , N.F. 3 , C.F. 4 or mixtures thereof, The method is carried out under one or a combination of the following conditions:

13. The method according to any one of claims 9 to 12.

14. The etch-back process comprises: (i) a temperature above 1200° C. and below the sublimation temperature of the source material, preferably below 1400° C.; and (ii) a temperature greater than 1650° C. and less than the sublimation temperature of the source material, preferably less than 1850° C. The temperature is determined under any one of the following conditions:

14. The method according to any one of claims 9 to 13.

15. The oxidation process comprises: (i) dry oxidation with oxygen and optionally an inert gas, said inert gas comprising nitrogen and / or argon; (ii) wet oxidation with a mixture of oxygen, water and optionally an inert gas; (iii) oxidation in a specified gas atmosphere at room temperature between 15° C. and 50° C.; (iv) oxidation with ozone; (v) oxidation with oxygen plasma, and / or (vi) Na 2 CO 3 , H 2 O 2 , NaOH, KIO 3 , KClO 3 , KMnO 4 and CrO 3 Oxidation by at least one of or a combination thereof, 14. The method according to any one of claims 8 to 13.

Citation Information

Patent Citations

  • Method for producing single crystal

    JP2014034485A

  • Silicon carbide single crystal substrate

    JP2017190286A

  • Seed crystal for monocrystal 4h-sic growth and processing method for the same

    JP2019127415A

  • Semiconductor device and production method therefor

    WO2003047000A1

  • Method for producing single crystal

    JP2008024554A