Force-balanced meniscus applicator for depositing crystalline layers and method for printing crystalline patterned features - Patents.com
The force-balanced meniscus applicator addresses the challenge of small grain sizes in organic semiconductor films by controlling deposition to create large crystalline domains and patterned films, enhancing electron carrier mobility and reducing defects in electronic devices.
Patent Information
- Application Number
- JP2024518668
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-23
- Filing Date
- 2022-09-20
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods for depositing organic semiconductor thin films result in small grain sizes, leading to lower electron carrier mobilities and charge trap densities, making them unsuitable for many electronic applications, and there is a need for a low-cost, high-throughput method to produce patterned thin films with large crystalline domains.
A force-balanced meniscus applicator that applies precursor solutions to a surface during relative movement, using a slot with a force balance reservoir and wetting features to control deposition, ensuring solution flows only onto hydrophilic areas and not hydrophobic areas, allowing for the formation of crystalline layers with desired patterns.
The applicator enables the production of high-quality organic films with large crystalline domains and patterned thin films, improving electron carrier mobility and reducing charge trap densities, suitable for high-throughput manufacturing of electronic devices.
Smart Images

Figure 2024539560000001_ABST
Abstract
Description
[Technical field]
[0001] Related Application Data This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 247,605, entitled "Method of forming a patterned crystalline layer on a substrate, and apparatus therefor," filed on September 23, 2021, which is incorporated by reference in its entirety.
[0002] The present disclosure relates generally to the field of semiconductor manufacturing. In particular, the present disclosure is directed to a force-balanced meniscus applicator for depositing crystalline layers and a method for printing crystalline patterned features. [Background technology]
[0003] Organic semiconductor thin films have potential applications in a variety of fields, including organic field effect transistors (OFETs), organic light emitting diodes (OLEDs), electroluminescent displays, low-cost photovoltaic devices, radio frequency (RF) identification tags, sensors, and wearable computers. Thin films deposited from solution by high throughput processes (typically >1 mm / sec) generally have a relatively small grain size and are adversely affected by grain boundary properties. As a result, such films typically have lower electron carrier mobility and larger charge trap density compared to films with larger grain size, making them less useful for many electronic applications. For example, conventional methods of depositing organic semiconductor thin films based on vapor deposition always produce materials with domain dimensions smaller than 10 microns. Observers close to the electronics industry expect that organic microelectronics will eventually find applications in portable and wearable devices because of their ability to utilize flexible, lightweight materials. However, many issues remain to be addressed in the following areas:
[0004] 1) A low-cost, high-throughput method for producing thin film materials. 2) Fabrication of patterned thin films by direct printing. 3) A method for producing high quality materials consisting of large crystalline domains. Summary of the Invention [Problem to be solved by the invention]
[0005] It would therefore be desirable for manufacturers to be able to produce high quality organic films with crystalline domains orders of magnitude larger than previously practical. It would also be desirable for manufacturers to be able to achieve patterned thin films in which certain given functional areas of a substrate are coated with an organic semiconductor thin film having grain sizes comparable to or larger than the dimensions of the individual patterned functional areas. [Means for solving the problem]
[0006] In one embodiment, the present disclosure is directed to an applicator that applies a solution to a surface along a deposition direction when movement occurs between the applicator and the surface along the deposition direction and when the solution forms a meniscus between the applicator and the surface. The applicator includes an applicator slot having a slot opening immediately adjacent to the surface in use. The slot opening has a length at least nominally perpendicular to the deposition direction and a width at least nominally parallel to the deposition direction. The length of the slot opening is at least twice the width of the slot opening. The slot opening is continuous and unobstructed along the length of the slot opening. The applicator includes a force balance reservoir in fluid communication with the applicator slot along the length of the slot opening of the applicator slot and designed and configured to hold a portion of the solution during use of the applicator. The force balance reservoir includes a plurality of wetting features arranged to allow the solution to flow out of the slot opening when movement occurs between the applicator and the solution in the deposition direction and to prevent the solution from flowing out of the slot opening when no movement occurs between the applicator and the surface in the deposition direction.
[0007] In another embodiment, the present disclosure relates to a method of printing features on a substrate using a precursor solution including a depositable material dissolved in a solvent, each feature having an in-plane dimension and an in-plane shape and composed of the depositable material after the solvent has left the feature. The method includes providing a substrate having a print area including a plurality of functional areas surrounded by non-functional areas. The method has a print direction along the substrate. The print area has a width perpendicular to the print direction. The functional areas define the location of the crystalline features. Each of the functional areas is spaced apart from one another along the print direction and perpendicular to the print direction. Each functional area has a hydrophilic surface that is hydrophilic with respect to the precursor solution. The hydrophilic surfaces are sized and shaped to match the in-plane dimensions and the in-plane shape of the corresponding crystalline feature, respectively. Each functional area is defined by a feature boundary formed between a hydrophilic surface and a hydrophobic surface. The hydrophobic surface surrounds the hydrophilic surface and is hydrophobic with respect to the precursor solution. The method also includes moving a meniscus of the precursor solution along the printing direction while in contact with the printing area across the width of the printing direction to deposit a portion of the solution on the hydrophilic surfaces of the functional area and to prevent any of the solution from depositing on the hydrophobic surfaces. [Brief description of the drawings]
[0008] For the purpose of illustrating the invention, the drawings show aspects of one or more embodiments of the invention, it being understood, however, that the invention is not limited to the precise arrangements and instrumentalities shown in the drawings.
[0009] [Figure 1A] FIG. 1 is a side view of a force balanced meniscus (FBM) applicator made in accordance with the present disclosure. [Figure 1B] FIG. 1B is an enlarged cross-sectional view taken along line 1B-1B of FIG. 1A, showing the slots of the FBM applicator. [Figure 1C] FIG. 1C is an enlarged cross-sectional view taken along line 1C-1C in FIG. 1A, showing the slot of the FMB applicator in an oblique orientation relative to the orientation shown in FIG. 1B. [Figure 1D]FIG. 1D is an enlarged cross-sectional view taken along line 1D-1D in FIG. 1A, illustrating an example in which the reservoir of the FBM applicator is an open-path reservoir. [Figure 1E] FIG. 1E is an enlarged cross-sectional view taken along line 1E-1E of FIG. 1A, illustrating an example in which the reservoir of the FBM applicator is a closed-circuit reservoir and the wetting structure is provided by an insertion structure inserted into the reservoir. [Figure 1F] FIG. 1F is an enlarged cross-sectional view taken along line 1F-1F of FIG. 1A, illustrating an example where the reservoir of the FBM applicator is a closed-circuit reservoir and the volume of the reservoir is defined by the volume of the wetting structure. [Figure 2A] FIG. 2 is a longitudinal cross-sectional view of an exemplary embodiment of an FBM applicator of the present disclosure. [Figure 2B] FIG. 2B is a perspective view of the body of the FBM applicator of FIG. 2A. [Figure 2C] FIG. 2C is a cross-sectional view taken along line 2C-2C of FIG. 2B, showing the wetting passage and cover plate. [Figure 2D] FIG. 2B is an enlarged bottom view of the FBM applicator of FIG. 2A. [Diagram 3] FIG. 2E is a perspective view of the FBM applicator of FIGS. 2A-2D mounted on a linear patch coater. [Figure 4A] FIG. 4 is a photograph of a sample crystalline layer written using the linear patch coater of FIG. 3, where the crystalline layer is illuminated with polarized light. [Figure 4B] 4 is a graph of the transfer curve of a field effect transistor (FET) fabricated using the linear patch coater of FIG. 3. [Diagram 5] FIG. 2E is a perspective view of the FBM applicator of FIGS. 2A-2D mounted on a roll coater. [Figure 6A] FIG. 6 is a diagram showing the structure of each of a plurality of field effect transistors (FETs) fabricated using the roll coater of FIG. 5. [Figure 6B] 13 is a polarized optical microscope image of a C8-BTBT thin film on a glass substrate prepared from a 1.5 wt % C8-BTBT-toluene solution at 60° C. and 25 mm / sec writing conditions. [Figure 6C] 6 is a graph of a transfer curve of one of the FETs fabricated using the roll coater of FIG. 5. [Figure 7] 1 is a diagram of the molecular structure of arbitrary semiconductor and dielectric molecules. [Figure 8A] FIG. 1 illustrates a meniscus of an FBM applicator of the present disclosure formed on a hydrophilic surface. [Figure 8B] FIG. 1 illustrates a meniscus of the FBM applicator of the present disclosure formed on a hydrophobic surface. [Figure 8C] 1 shows the meniscus of the FBM applicator of the present disclosure after transition from a hydrophobic surface to a hydrophilic surface and illustrates the pinning of the contact line at the transition between the hydrophobic and hydrophilic surfaces. [Figure 9A] Photograph of the deposition of precursor solutions during the formation of multiple FETs taken with 45° crossed polarizers, showing the interaction of the solutions with hydrophilic and hydrophobic regions. [Figure 9B] Photograph of deposition of precursor solutions during formation of multiple FETs taken with 45° crossed polarizers, showing interaction of the solutions only with hydrophobic regions. [Figure 10A] 13 is a photograph of a patterned feature during initial nucleation of crystallization of a precursor solution written using an FBM applicator of the present disclosure. [Figure 10B] 10B is a photograph of the patterned feature of FIG. 10A after partial crystallization of the patterned feature. [Figure 10C] 10C is a photograph of the patterned features of FIGS. 10A and 10B after complete crystallization of the patterned features. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In some aspects, the present disclosure is directed to force-balanced meniscus (FBM) applicators, or simply "applicators," that apply solution to a surface when there is motion between the applicator and the surface relative to one another, rather than when there is no motion between the applicator and the surface. The term "meniscus" in the composite descriptor "force-balanced meniscus" is directed to a property of the presently disclosed applicators where the applied solution forms a meniscus with the surface, or at least a hydrophilic (with respect to the solution) portion thereof, during deposition. Details of meniscus-type applicators with respect to the formation of a meniscus in the context of organic semiconductor precursor solutions can be found, for example, in U.S. Patent Nos. 7,351,283 and 9,444,049, entitled "System and Method for Producing Crystalline Thin Film Structures" and "Method for Forming One or More Crystalline Layers on a Substrate," issued April 1, 2008 and September 13, 2016, respectively, and U.S. Patent Application Publication No. 2008 / 0138927, entitled "System and Method for Producing Crystalline Thin Film Structures Using Meniscus Growth Techniques," published June 12, 2008, which are incorporated herein by reference for their teachings regarding meniscus geometry, other meniscus properties, and crystal growth from a meniscus, as described below. As described in detail below, the term "force balance" in the above composite descriptor relates to a property of the applicator of the present disclosure where when motion occurs between the applicator and the surface, the relative motion draws the solution out of the applicator and deposits the solution on the surface, but when no relative motion occurs, the solution does not flow out of the applicator and is not drawn back into the applicator, at least to the extent that the solution is no longer in contact with the surface. Thus, there is a balance of forces such as between the applicator and the solution, including any hydrophilic attractive forces between the solution and the deposition surface. This balance of forces can provide improved control of the deposition of the solution, and improved control of the formation of the resulting deposition layer, e.g., an organic semiconductor layer or a hybrid organic-inorganic-semiconductor layer, formed from the deposited solution.
[0011] In some aspects, the present disclosure is directed to printing shaped crystalline features on a surface using a precursor solution for a crystalline layer, and providing hydrophilic (with respect to the precursor solution) functional areas that are sized and shaped to match the desired crystalline features. In some embodiments, providing hydrophilic features may be accomplished by forming a hydrophobic (with respect to the precursor solution) mask on the surface, or by using a template sheet superimposed on the surface, which may or may not be hydrophobic. In some embodiments, the precursor solution may be applied using an FBM applicator of the present disclosure. However, in some embodiments, the precursor solution may be applied using other techniques, such as those disclosed in any of the patent documents incorporated by reference above. The foregoing and other aspects of the present disclosure are described in detail below by way of some non-limiting examples and illustrations.
[0012] Throughout this disclosure and the appended claims, the term "about" when used in conjunction with a corresponding numerical value refers to ±20% of that numerical value, typically ±10% of that numerical value, often ±5% of that numerical value, and most often ±2% of that numerical value. In some embodiments, the term "about" can refer to the numerical value itself.
[0013] Typical FBM applicator configuration
[0014] Turning now to the drawings, FIGS. 1A and 1B provide a high level overview of an exemplary FBM applicator 100 made in accordance with the present disclosure. In this example, the applicator 100 includes a force-balanced reservoir 104 (or simply "reservoir") that contains a solution 108 for application onto a surface, here surface 112, via an elongated application slot 116 (or simply "slot") (FIG. 1B). In this example, the solution 108 is a precursor solution for forming a crystalline layer 108L on the surface 112 (FIG. 1A), which is hydrophilic to the solution. Thus, the solution forms a meniscus 108M between the applicator 100 and the surface before the crystalline components in the solution crystallize at the contact line 108CL to form the crystalline layer. Examples of crystalline layers made of organic and hybrid organic-inorganic semiconductor materials, and precursor solutions for forming such crystalline layers, are as follows. Additionally, the mechanism of crystal growth at the contact line 108CL is described in detail, for example, in any of the patent documents listed above. In the context of applicator 100, the particular composition of solution 108 is not important; rather, the interaction of the solution with surface 112 and the applicator is important to achieve the desired force balance characteristics of the applicator.
[0015] The force balancing property of the exemplary FBM applicator 100 is achieved by providing the reservoir 104 with a wetting feature 104W that is either a structural element located within the reservoir, or has a total volume that effectively defines the reservoir itself, or a combination of both. Generally, the wetting feature 104W has a surface (not shown) that is hydrophilic with respect to the solution 108, and is designed, configured, and positioned to create a force within the solution 104 that acts to counteract forces such as the solution's own weight, surface tension, and other forces associated with the meniscus 108M, which would cause the solution to flow out of the applicator 100 at a higher rate than would be needed or desired in the absence of the wetting feature. For example, during deposition and formation of crystalline layer 108L, without wetting feature 104W, solution 108 would flow out of applicator 100 at a faster rate than necessary for proper deposition and formation, and without wetting feature solution would flow out of applicator 100 when no flow is desired, when deposition is not occurring when there is no motion between applicator 100 and surface 112. Note also that if a different flow rate is desired, wetting feature 104W can be adjusted so that slot 116 applies solution 108 at different flow rates along the length of the slot.
[0016] From a functional standpoint, the wetting features 104W need not take any particular form so long as they perform the necessary force balancing functions described above. However, one skilled in the art will readily appreciate that some forms of wetting features 104W are easier and less expensive to implement than others. As a result, practicality and / or cost may be the driving factor for designing and providing the necessary wetting features 104W. It should be noted that the wetting features 104W, once wetted by the solution 108, by retaining some portion of the solution, are considered part of the reservoir 104 regardless of where they may be located. For example, a wetting feature 104W that appears to be located in a slot 116 is still part of the reservoir 104.
[0017] It should be noted that in some embodiments, all of the countervailing forces required to achieve the desired force balance goal are provided nominally or solely by the wetting feature 104W, and not any other type of force, such as vacuum and / or suction forces. The word "nominal" in the immediately preceding sentence is provided to account for secondary forces that may act as a natural consequence of the non-force balanced features of the applicator 100, such as wetting / capillary forces that may occur in the slot 116 or in a conventional solution distribution line (not shown) that supplies the solution 108 to the slot. The difference is that, in the presence of such secondary forces, the necessary force balance cannot be achieved without the presence of the wetting feature 104W, which is purposefully designed to provide the applicator 100 with the proper force balance for any application of the applicator. Typically, the reservoir 104 is in fluid communication with the surrounding environment, as well as with the same environment in which the deposition of the crystal layer 108L occurs on the surface 112. Thus, both the reservoir 104 and the deposit are subjected to the same ambient pressure (e.g., atmospheric pressure) so that no overall suction force can exist between the solution inlet 104I (FIG. 1A), 104I' (FIG. 1D) to the reservoir 104 and the slot 116.
[0018] The configuration of the wetting feature 104W typically requires consideration of various design parameters, including, but not limited to, the wetting characteristics of the solution 108, the density of the solution, the amount of solution in the slot 116, the cross-sectional dimensions of the slot (i.e., the slot length Ls and slot width Ws (FIG. 1B)), the angle, φ, the distance between the flow axis FAs of the slot and the total flow axis FAr of the reservoir 104, whether the reservoir is open along the top side, the dimensions of the meniscus 108M, any suitable subcombination between others depending on the particular design, and other design parameters. It should be noted that the total flow axis FAr of the reservoir is effectively the axis parallel to the total flow of the solution 108 in and / or through the reservoir 104.
[0019] Exemplary forms that the wetting features 104W may have include, but are not limited to, inter alia, alone or in any suitable combination with one another, channels formed in one or more interior walls of the reservoir, island-like structures formed on one or more walls of the reservoir, column-like structures extending from one wall and in some cases joining an opposing wall, interior walls within the bounding walls of the reservoir (e.g., forming a serpentine, zigzag, or circuitous path within the reservoir), tubular structures within the reservoir, or tubular structures functionally forming a collective reservoir consisting of the sum of the interior volumes of otherwise tubular structures, and open-pore structures within the reservoir, or open-pore structures functionally forming a collective reservoir consisting of the open volumes of otherwise open-pore structures.
[0020] The crystalline layer 108L has a deposition direction 108Dd (FIG. 1B). As one, the other, or both of the applicator 100 and the surface 112 move relative to the other during deposition, the dimensions of the deposited crystalline layer increase along the deposition direction. As described above, the slot 116 has a length Ls and a width Ws, as shown in FIG. 1B. The length Ls is nominally perpendicular to the deposition direction 108Dd, and the width Ws is nominally parallel to the deposition direction 108Dd. With reference to both FIG. 1B and FIG. 1C, the term "nominal" in the immediately preceding sentence is provided to account for the possibility that the actual deposition direction 108Dd' may be at some non-zero skew angle, Δ. The length Ls and width Ws are oriented relative to the design deposition direction 108Dd. Typically, the skew angle Δ is negligibly close to zero.
[0021] The slot 116 has an undivided opening 116 adjacent the surface 112 during use of the applicator 100. The area of the opening is defined by a length Ls and a width Ws. In this example, the slot 116 is undivided. Thus, the length Ls is equal to the entire length of the slot. However, in other embodiments, the entire slot 116 may be divided into multiple segments, e.g., segments 116(1)-116(3) by partitions 116D(1) and 116D(2) (FIG. 1B), each of which has a corresponding undivided length Ls and a corresponding undivided opening 116O(1)-116O(3). In some embodiments, the ratio of the length Ls to the width Ws is 2:1 or more, 5:1 or more, 10:1 or more, 20:1 or more, 50:1 or more, 100:1 or more, 500:1 or more, or 1000:1 or more, among other ranges. In some embodiments, including those having the width Ws to length Ls ratios described above, the width Ws of the slot 116 at the opening 116O may range from about 100 microns to about 500 microns for relatively low viscosity solutions and from about 500 microns to about 2500 microns for relatively high viscosity solutions, among others. One of ordinary skill in the art will readily understand how to tailor the width Ws of the slot 116 for a particular application, for example according to the viscosity of the solution 108, without undue experimentation. In this embodiment, the opening 116O is free of obstructions in front of the portion of the applicator 100 immediately adjacent the slot 116. In some embodiments, the opening 116O may have a depth (not shown) in the range of about 0 mm to about 10 mm or more, measured from the front of the opening to the portion of the wetting feature 104W closest to the front. However, at greater depths, the weight of the solution 108 may become a greater factor in designing an appropriate wetting feature 104W. Depending on the depth, the slot 116 may optionally include one or more partitions 116D spaced apart from one another along the length Ls of the slot.
[0022] 1D and 1B, the width Wr of the reservoir 104 in this example is equal to the length Ls of the slot 112. However, in some embodiments, the width Wr of the reservoir 104 in this example may be less than or greater than the length Ls of the slot 112 depending on the design in question. In any of these cases, it should be understood that there is a many-to-one relationship between the number of wetting features 104W and the single slot 112 as a whole, or, if the slot is divided into multiple segments by one or more partitions along its entire length, such as segments 116(1)-116(3) divided by partitions 116D(1) and 116D(2), between the number of wetting features associated with any one of the resulting slot segments and that particular slot segment itself. If the slot is divided into segments, each segment may have any of the slot widths Ws to slot / segment widths Ls, as described above.
[0023] With particular reference to FIG. 1D, this figure illustrates an example of a reservoir 104 that is an open-path reservoir 104(1). Wetting feature 104W(1) is located toward the bottom of the reservoir. In this example, wetting feature 104W(1) is shown as an open path (e.g., straight, serpentine, zigzag, etc.) (collectively designated 120) formed in a bottom wall 104BW(1) of reservoir 104(1). In some embodiments, the open-path reservoir 104(1) may be closed with a suitable closure 104C(1), such as a piece of glass or other transparent material, a piece of plastic, or a piece of metal, among others. In some embodiments that include closure 104C(1), the closure may include its own wetting feature (not shown), which may complement or replace the shown wetting feature 104W(1).
[0024] FIG. 1E shows an example of a reservoir 104 that is a closed-path reservoir 104(2) in which the wetting structure 104W(2) is distributed across the entire height Hr and width Wr of the reservoir. In some examples, the wetting structure 104W(2) may be formed by an open-pore foam or an open-pore sintered structure, among others, and may be a plurality of straight, serpentine, zigzag, etc. closed paths. In this example, the wetting structure 104W(2) is disposed within an insert structure 104IS(2) that is inserted into the reservoir 104(2). In this example, the wetting structure 104W(2) is shown as occupying the entire height Hr of the reservoir 104(2). However, in other embodiments, the wetting structure 104W(2) does not extend across the entire height Hr of the reservoir 104(2).
[0025] FIG. 1F shows an example of a reservoir 104 that is a closed-path reservoir 104(3). The volume of the reservoir is equal to the total volume defined by the wetting structure 104W(3) itself. In general, the reservoir 104(3) of FIG. 1F can be distinguished from the reservoir 104(2) of FIG. 1E in that the reservoir of FIG. 1F is not formed separately to the wetting structure 104W(3) and does not have a volume for holding the solution 108 that may be larger than the total volume provided by the wetting structure. Rather, the volume of the reservoir 104(3) is a volume defined by the wetting structure 104W(3) itself. In some examples, the wetting structure 104W(3) may be formed by an open-pore foam or an open-pore sintered structure, among others, and may be a closed path that is multiple straight, serpentine, zigzag, etc. Such wetting structures may be provided by additive manufacturing techniques (eg, 3D printing) or subtractive manufacturing techniques (eg, milling, drilling, electrical discharge machining, etc.).
[0026] Example of an embodiment of the FMB applicator
[0027] 2A-2D show an example 200 of the FBM applicator 100 of FIGS. 1A-1F (hereinafter, "applicator 200" or "FBM applicator 200"). Referring to FIG. 2A, in this example, the FBM applicator 200 includes a body 204, an end piece 208, and a removable cover plate 212. FIGS. 2B-2D show various details not seen or not fully shown in FIG. 2A, and the reader should refer to each of these additional figures as necessary. The end piece 208 and the body 204 cooperate to form a slot 216, and the cover plate 212 and the body cooperate to form a reservoir 220. In some embodiments, the end piece 208 may be made removable such that it is replaceable with an end piece (not shown) that provides the slot 216 with one or more different characteristics, such as a different length, a different width, a different number of partitions (if any), and / or more or less wetting features that contribute to the volume of the reservoir 220. As best shown in Figures 2B and 2C, the reservoir 220 is formed by a plurality of wetting paths 220W (wetting feature 104W in Figure 1A). Figure 2A shows an FBM applicator 200 applying a solution 224 onto a surface 228S of a substrate 228 to form a liquid film 224F thereon. If the solution 224 is a precursor solution containing crystalline components, the components can be crystallized and the solvent can be evaporated or otherwise removed to form a crystalline layer (not shown). As one skilled in the art will readily appreciate, the substrate 228 can be any suitable flexible or rigid substrate and the liquid film 224F can be provided for any suitable purpose, such as forming a crystalline layer and / or one or more semiconductor layers of a semiconductor device, such as a field effect transistor (FET), a diode, a solar cell, or other photoconductive layer. The surface 228S of the substrate 228 is hydrophilic, at least in the areas where the liquid film 224F is desired. In some embodiments, the cover plate 212 may be transparent so that a user can view the contents of the wet channel 220W and correspondingly the amount of solution 224 in the reservoir 220, for example, to determine when solution needs to be added to the reservoir. As can be seen in FIG. 2D, the slot 216 in this embodiment does not include an interior divider or other interior structure.Leaving the reservoir 220 open to atmospheric pressure allows for easy replenishment of the solution 224 within the reservoir using any suitable replenishment means 232, such as an automatic or manual replenishment system. The materials of construction of each of the body 204, end pieces 208, and cover plate 212 may be any material suitable for a particular application.
[0028] During use of the FBM applicator 200, solution 224 is introduced into the reservoir 220 and flows into the slot 216 under its own weight. The deposition of a thin film 224F is shown in FIG. 2A. As the applicator 200 and the substrate 228 move relative to one another, the solution 224 is drawn from the slot 216 into a thin film 224F by capillary forces. This force-balanced solution delivery technique has several advantages, including: (i) when the coating or printing process changes speed, the delivery speed automatically adjusts to the new process speed, and (ii) delivery can be stopped momentarily without solution 224 flowing out of the slot 116 during patterned coating where hydrophobic portions of the surface are being coated. Thus, conventional systems including conventional pumping devices are disadvantageous to the FBM applicator of the present disclosure, and even if this disadvantage is mitigated by active control and feedback of the delivery speed, these potentially complex and expensive measures are not necessary with the passive delivery design of the FBM applicator of the present disclosure. Both advantages (i) and (ii) are described in more detail below under the heading "Exemplary Patterning Methods."
[0029] Example of FBM applicator layout
[0030] In some embodiments, the disclosed method using the disclosed FBM applicators, such as FBM applicator 100 of FIG. 1A and FBM applicator 200 of FIG. 2A, involves deposition from a solution containing an organic or hybrid organic-inorganic semiconductor material dissolved in an organic solvent. Such solutions are often colloquially referred to as "electronic ink." For example, 6,13-bis(triisopropylsilylethynyl)pentacene (TIPS-pentacene) can be dissolved in toluene at room temperature up to about 5% by weight. In some embodiments, it is desirable to coat the solution over a large area. Typically, strips are coated, the strips having widths that can range from 1 mm to at least 1 meter, or even greater, if the disclosed FBM applicators are constructed accordingly. Details of the process, referred to as "lateral crystallization," are described in the patent documents incorporated by reference above.
[0031] The regime of more general interest for high throughput deposition is the high speed regime, which exceeds the critical velocity that divides the two coating regimes, as described in U.S. Patent No. 9,444,049, incorporated by reference above. For example, the critical velocity of a TIPS-pentacene solution in toluene at room temperature is about 1 mm / s during deposition by a pen writer or other similar means. Both regimes are considered to be within the capillary coating region of operating parameters. For convenience, in this disclosure, the low speed regime will be referred to as "Type 1" and the high speed regime as "Type 2". In Type 1, crystallization occurs very close to the contact line between the liquid meniscus and the surface being coated. On the other hand, in Type 2, the solution is first coated as a liquid layer that dries into a crystalline film at a significant distance from the meniscus, and there is usually no clear contact line. However, the high speed regime 2 is more difficult to control, as it depends critically on the drying pattern of the liquid thin film. To achieve large grain crystalline thin films at high throughput, it is important to design a process that mitigates this uncontrolled drying. The FBM applicator of the present disclosure is central to such a process.
[0032] The FBM applicator 200 of Figures 2A-2D was tested in several coating apparatuses, specifically a linear patch coater 300 as shown in Figure 3 and a roll coater 500 as shown in Figure 5. The results of the linear patch coater 300 operating in type 1 (deposition rate of 0.05 mm / s) to produce 25.4 mm wide strips (equal to the length of the slot) of crystalline thin films 50 mm to 125 mm long are shown in Figure 4A. Figure 4A shows a portion of one of the produced strips. Figure 4A is a photograph of one of the produced 25.4 mm wide samples, illuminated with polarized light, showing that in type 1 at a deposition rate of 0.05 mm / s very large grain sizes of over 25.4 mm were obtained along the writing direction (perpendicular to the 25.4 mm wide sample). In fact, the largest grains in this sample extended almost along the length of the 125 mm sample along the writing direction. The improved grain dimensions along the writing direction are apparently hypothesized to be a result of increasing the width of the slot to 25.4 mm from prior art pen-writers with either a 1 mm diameter circular capillary or a 5 mm wide rectangular capillary. In these cases, the grains grow from the edge of the strip during deposition. Therefore, the improvement is likely due to minimizing edge effects where new grains nucleate and propagate from the edge of the thin film strip. Figure 4B shows the transfer curve 400 of an organic or hybrid organic-inorganic FET (not shown, but see Figure 6A for the structure of the FET) with a semiconductor layer formed using the FBM applicator 200 of Figures 2A-2D mounted on the linear patch coater 300 of Figure 3. As can be seen in Figure 4B, the charge carrier mobility found is characteristic of TIPS-pentacene with large grains.
[0033] FIG. 6A shows a FET structure 600 of a FET fabricated using the roll coater 500 of FIG. 5. As seen in FIG. 5, a template glass substrate 504, templated to form the semiconductor layer of the FET, is shown attached to the roller 508 of the roll coater 500. As seen in FIG. 6A, the FET structure 600 was fabricated on a flexible glass substrate 604 having a pair of gold contacts 608(1) and 608(2) formed on the glass substrate. A semiconductor layer 612 of C8-BTBT with large grains was deposited on the gold contacts 608(1) and 608(2) and on the glass substrate 604 between the two gold contacts. A dielectric gate layer 616 of Cytop809M was deposited on the semiconductor layer 612, and an aluminum gate electrode 620 was formed over the space between the two gold contacts 608(1) and 608(2). The writing conditions using the roll coater 500 of FIG. 5 in fabricating a FET having the FET structure 600 of FIG. 6A were 25 mm / sec at 60° C. using a 1.5 wt % C8-BTBT solution and a 1:1 ratio of Cytop809m and Cytop100 series solvents (AGC Inc. formerly Asahi Glass Co., Ltd.). The transistor yield was 85% functional and the average carrier mobility of the functional transistors was 1.1 cm. 2 With this in mind, the results of the roll coater 500 of Figure 5 operating in type 2 are shown in Figures 6B and 6C.
[0034] FIG. 6B shows a polarized optical microscope image of the C8-BTBT thin film of the semiconductor layer 612 (FIG. 6A). Because the substrate temperature is held at 60° C., the grain size is larger than what is typically observed at a speed of 25 mm / s. Although the critical velocity can be shifted to a higher speed by heating the substrate, it is clear from the grain morphology that the deposition conditions correspond to type 2, since the grains are not elongated along the coating direction. Thus, the observation of large grains is not due to a shift in the critical velocity higher, but due to crystallization from a transient liquid crystal (LC) phase. This effect is characterized as a thin film that is initially coated as a solution, but does not directly crystallize, but goes through a transient LC phase. The nucleation rate of the crystalline phase controls the final grain size and particle morphology. Although this effect is known to occur in a class of molecules based on the BTBT molecular core that have a liquid crystal phase at high temperatures, it should be emphasized that the effect occurs at substrate temperatures where the crystalline phase is the stable phase and not the transient LC phase. Figure 6C shows an example transfer curve 650 from one of the FETs having the FET structure 600 of Figure 6A, with C8-BTBT as the semiconductor layer 612, from which an estimated charge carrier mobility can be extracted.
[0035] Exemplary Materials for Semiconductor Applications
[0036] When an FBM applicator of the present disclosure, such as applicator 100 of FIG. 1A or applicator 200 of FIG. 2A, is configured for use in making organic and / or hybrid organic-inorganic semiconductor films, any one or more of several organic and hybrid organic-inorganic semiconductor molecules can be used. Such classes of molecules include (I) simple polyaromatic hydrocarbons (PAHs) such as anthracene, (II) TIPS-pentacene, 2,8-difluoro-5,11-bis(triethylsilylethynyl)anthradithiophene (diF-TES-ADT), 2,7-dioctyl[1]benzothieno[3,2-b][1]benzothiophene (C8-BTBT), and 2-decyl-7-phenyl[1]benzothieno[3,2-b][1]benzothiophene (Ph-BTBT-C1 These include PAHs with side groups added to increase solubility in organic solvents and to affect crystal packing, such as (III) PAHs with side groups added to increase solubility in organic solvents and to affect crystal packing, (III) polymers such as poly(3-hexylthiophene) (P3HT) and poly(vinylidene fluoride-co-trifluoroethylene) [P(VDF-TrFE)], and (IV) hybrid organic-inorganic molecules such as hybrid perovskite (e.g., lead halide perovskite (e.g., CH3NH3PbI3)) molecules. Note that P(VDF-TrFE) is a dielectric material and the others are semiconductors. The molecular structures of some of these example molecules are shown in Figure 7.
[0037] Anthracene is the only material listed as class 1 because it is the easiest to crystallize and typically forms the largest crystalline grain size when coated from solution. As described in the present disclosure, special methods are required to obtain very large grain sizes, but good results are obtained for class II. Among class II, there are exceptional cases, for example materials with a BTBT core with an LC phase that may appear as a transient phase during solution deposition under some conditions, such as during deposition on a heated substrate. Another exception is rubrene (not shown in Figure 7). To the inventors' knowledge, large grain crystalline thin films of rubrene have not been obtained by solution coating methods. Polymeric materials (class III) typically show limited crystallinity and orientational alignment along the coating direction.
[0038] Exemplary Patterning Methods
[0039] Semiconductor devices such as FETs and diodes, and portions thereof, can be fabricated by depositing one or more precursor solutions of organic or hybrid organic-inorganic semiconductor materials and / or organic or hybrid organic-inorganic dielectric materials using, inter alia, a meniscus deposition technique such as the immersion technique of U.S. Pat. No. 7,444,049, incorporated by reference above, or a technique using an FBM applicator such as FBM applicator 100 of FIG. 1A or FBM applicator 200 of FIG. 2A. Such a process generally involves providing a substrate with patterned functional areas that are hydrophilic to the precursor solution for each layer of the device deposited using such techniques. Areas surrounding the patterned areas, i.e., non-functional areas, are hydrophobic to the precursor solution. As described in more detail below, the precursor solution does not deposit on the hydrophobic non-functional areas, but does deposit on the hydrophilic patterned functional areas. The crystalline components of the precursor solution crystallize therein with high shape fidelity.
[0040] The hydrophilic patterned functional regions may be defined in any suitable manner. For example, the hydrophilic patterned functional regions may be defined by providing hydrophobic non-functional regions using any suitable technique, for example, by blanket coating the hydrophilic layer with a hydrophobic layer, patterning the hydrophobic layer, and then etching away the patterned functional regions of the hydrophobic layer to expose the hydrophilic material underneath the hydrophobic layer. As another example, the surface of the hydrophilic layer onto which the precursor solution is to be deposited may be treated in a patterned manner to render the hydrophilic layer hydrophobic in areas outside the hydrophilic patterned regions onto which the precursor solution is desired to be deposited. As a further example, a removable and / or reusable hydrophobic template sheet with appropriately patterned openings may be overlaid on or otherwise applied to the hydrophilic surface of the substrate.
[0041] As a detailed example, a method for defining hydrophilic patterned functional areas includes treating a hydrophobic surface with a hydrophobic monolayer, e.g., octadecyltrichlorosilane (OTS) or another self-assembled monolayer. The pattern can be created by several means, such as microcontact stamping or photolithography. This particular example creates the pattern by photolithography, which is accomplished through the following general steps, although the exact method is not critical: (i) spin-coating a positive photoresist onto the surface to be coated, (ii) exposing the positive photoresist to ultraviolet light through a shadow mask, (iii) dissolving the exposed portions of the photoresist using a developer, (iv) treating the newly exposed portions of the surface with a hydrophobic self-assembled monolayer, and (v) removing the remaining photoresist. The patterned functional areas in the final removal step (v) have the properties of the underlying substrate, which is hydrophilic. Thus, using the mask pattern transferred to the photoresist, a molecular template is created on the original surface that contains complementary patterns of hydrophilic and hydrophobic regions that define functional and non-functional areas, respectively.
[0042] 8A-8C show a series of schematics 800, 804, 808, respectively, illustrating how patterning is achieved by controlling the hydrophobic / hydrophilic interactions between a liquid precursor solution and a surface on which patterned features are desired. FIG. 8A shows the coating of a precursor solution 812 onto an untreated hydrophilic surface 816 to form a crystalline film 812F. As long as the contact angle θc (FIGS. 8B and 8C) of the meniscus 812M is small enough, coating occurs. However, while this description of the contact angle θc is appropriate for regime 1, in regime 2 there is no clear contact line as in 812CL of FIG. 8B. Instead, an elongated thin liquid film 812LF, known as a "dynamic meniscus," is observed. As shown in FIG. 8A, the thin liquid film 812LF is then dried by solvent evaporation and transformed into a crystalline solid film 812F.
[0043] FIG. 8B shows the case of a hydrophobic surface 820. In this case, the surface tension is reduced, the contact angle θc is increased, and there is no significant dynamic meniscus. As a result, no solid thin film is produced. FIG. 8C shows the more complex case of a patterned surface 824 with hydrophilic regions 824(1) and hydrophobic regions 824(2). Here, the trailing contact line 812CL′ is pinned at the boundary 824B between the hydrophilic region 824(1) and the hydrophobic region 824(2). This results in the meniscus 828 being dynamically stretched. As a result, a thin film 832 is deposited only on the hydrophilic regions. The film 832 may be a crystalline solid film if a clear contact line is present (type 1), or it may be a liquid thin film that subsequently crystallizes, possibly by transforming through one or more transient phases before reaching the final crystalline state (type 2). As can be seen in FIG. 8C, membrane 832 is anchored at boundary 824B between hydrophobic region 824(2) and hydrophilic region 824(1).
[0044] Patterns have been used in a variety of different ways, such as to define surface patterns during either wet or dry etching by inhibiting etching in portions of the surface protected by a self-assembled monolayer. In the prior art, considerable attention has been paid to creating surface patterns by etching methods that can be classified as subtractive methods. In the disclosed method, crystalline thin films are created by additive methods using solution coating. As mentioned above, due to the poor wettability of the solution, coating occurs in hydrophilic areas but not in hydrophobic areas. Functional fabrication using the disclosed patterned coating method is highly unique and desirable over the prior art, since most scalable high-throughput coating methods, such as conventional slot-die coating, are designed to completely coat a surface over a wide strip, e.g., at least 1 mm wide. In contrast, the methods disclosed herein can additively create fully patterned semiconductor and other layers over relatively large areas of a substrate where relatively small functional areas are predefined prior to coating.
[0045] For example, Figures 9A and 9B show two images 900 and 904 taken a short time apart to show the movement of a meniscus 908M of precursor solution 908 being applied to a patterned surface having hydrophilic patterned regions 912 and 916 (only a few of each are labeled to avoid confusion) where precursor solution is to be deposited, and hydrophobic regions 920 where precursor solution should not be deposited. Comparing Figures 9A and 9B with each other, it is readily apparent that in regions 908M(1)-908M(4) of the meniscus 908M where precursor solution 908 is still in contact with one of the hydrophilic patterned regions 912, the meniscus is dynamically stretched (see also Figure 8C) to form a nonlinear contact line 908CL (Figure 9A), but when the meniscus is in contact with a hydrophobic region, there is no dynamic stretching due to the much lower wetting forces. The meniscus 908M in Figure 9B has passed well past the end of the hydrophilic patterned region 912, so the contact line 908CL is again linear due to the even distribution of surface tension within the meniscus even then. In this example, the printed patterned regions 912 and 916 contain crystallized C8-BTBT. The printing speed was 0.3 mm / sec for coating type 1.
[0046] 10A-10C show, inter alia, printing with near perfect contrast and fidelity of small features such as features that are greater than or equal to about 200 μm in the maximum direction and less than or equal to about 200 μm in the minimum direction, features that are greater than or equal to about 100 μm in the maximum direction and less than or equal to about 100 μm in the minimum direction, features that are greater than or equal to about 50 μm in the maximum direction and less than or equal to about 50 μm in the minimum direction, or features with maximum dimensions less than 20 μm. These remarkable results appear to be due to the extreme sensitivity of the coating process to the contact angle of the solution at the meniscus (see above) and whether the meniscus is pinned to the boundary of the hydrophilic region. The method also appears to be improved by passive supply of solution. This can be facilitated using FBM applicators of the present disclosure, such as FBM applicator 100 of FIG. 1A and FBM applicator 200 of FIGS. 2A-2D described above.
[0047] Figures 10A-10C show three frames 1000(1)-1000(3), respectively, extracted from a video taken during deposition of patterned C8-BTBT from a 0.5 wt % toluene solution 1004 at 80 °C with a writing speed of 25 mm / s. Frame 1000(1) in Figure 10A corresponds to a moment approximately 1 second after the printing phase has stopped, at which point the single patterned feature 1008 in the figure is composed primarily of solution 1004. An initial nucleation event of the liquid crystalline to crystalline phase can be seen at 1004N. Crystallization of the patterned feature 1008 is observed to propagate from left to right in frames 1000(2) and 1000(3) in Figures 10B and 10C, respectively. The crystallization front 1004CF is shown approximately at the longitudinal center of the patterned feature in frame 1000(2), and the entire patterned feature is fully crystallized in frame 1000(3). These subsequent frames 1000(2) and 1000(3) are separated from each other by about 1 second. Frame 1000(2) is also separated from frame 1000(1) by about 1 second. In this example, the patterned feature is 150 μm by 1 mm. It is noteworthy that this printing was done with coating type 2, which normally results in a thin film of small grains. However, deposition onto a heated substrate forced the C8-BTBT into a transient liquid crystal state, resulting in a large crystalline grain structure. The templating provided here by the hydrophobic regions 1112 surrounding the patterned feature 1008 caused the nucleation of the crystalline phase within the hydrophilic regions (not shown) of the surface underlying the patterned feature. Thus, in this manner, single crystal domains can be placed at any desired location on a surface by utilizing an appropriate template.
[0048] The ability to print high quality crystalline features can prove of great utility for the creation of electronic devices free of grain boundary defects. In particular, Figures 10A-10C demonstrate that the general method is a low-cost, high-throughput method in which large grain thin films are produced by patterned printing, thus satisfying all three of the desired attributes described in the Background section above. Patterning somewhat mitigates the need to obtain very large grain sizes (e.g., >25.4 mm) since grains can be placed at any device location, such as FETs. This provides a means to produce semiconductor layers free of grain boundary defects within the area of the device. This method is also compatible with methods to obtain large grains at high speeds (e.g., >1 mm / sec), such as by utilizing the transient phase phenomenon shown in Figures 10A-10C for patterned thin films.
[0049] As mentioned above, patterning may be achieved by additional means that do not require direct template of the surface. For example, a sheet mask can be created in which the solid portions of the sheet mask have a hydrophobic surface. When the sheet mask is engaged with a hydrophilic substrate surface, the openings in the sheet mask allow portions of the hydrophilic surface to be exposed that are to be coated. Assuming the mask is thinner than the typical dimensions of a meniscus, the sheet mask itself will act as a template in the process described above. The advantage of this approach is that the sheet mask can be easily removed, which facilitates the deposition of multiple layers.
[0050] Various modifications and additions can be made without departing from the spirit and scope of the present invention. The features of each of the various embodiments described above may be combined with features of other described embodiments as necessary to provide multiple combinations of features in related new embodiments. Furthermore, while the above describes several separate embodiments, what is described herein is merely illustrative of the application of the principles of the present invention. Furthermore, although certain methods herein may be illustrated and / or described as being performed in a particular order, the ordering is highly variable within the scope of one of ordinary skill in the art to achieve aspects of the present disclosure. Thus, this description is meant to be taken only as an example, and not to limit the scope of the present invention.
[0051] Exemplary embodiments have been disclosed above and shown in the accompanying drawings. It will be understood by those skilled in the art that various modifications, omissions and additions can be made to what is specifically disclosed herein without departing from the spirit and scope of the present invention.
Claims
1. 1. An applicator for applying a solution to a surface along a deposition direction when movement occurs between the applicator and the surface along the deposition direction and when the solution forms a meniscus between the applicator and the surface, comprising: an applicator slot having a slot opening immediately adjacent to the surface when the applicator is in use; a force balanced reservoir in fluid communication with the application slot along a length of the slot opening of the application slot, the force balanced reservoir designed and configured to hold a portion of the solution during use of the applicator; Equipped with the slot opening has a length at least nominally perpendicular to the deposition direction and a width at least nominally parallel to the deposition direction, the length of the slot opening being at least twice the width of the slot opening, and the slot opening being continuous and unobstructed along the length of the slot opening; The force balanced reservoir includes a plurality of wetting features arranged to permit the solution to flow out of the slot opening when motion occurs between the applicator and the solution in the application direction and to prevent the solution from flowing out of the slot opening when no motion occurs between the applicator and the surface in the application direction. Applicator.
2. the applicator slot having a flow axis along which the solution flows during use of the applicator; the force balanced reservoir having a general flow axis along which the solution flows within the force balanced reservoir during use of the applicator; The flow axis of the application slot is perpendicular to the total flow axis of the force balance reservoir. The applicator of claim 1 .
3. the applicator slot having a flow axis along which the solution flows during use of the applicator; the force balanced reservoir having a general flow axis along which the solution flows within the force balanced reservoir during use of the applicator; The flow axis of the application slot is parallel to the total flow axis of the force balance reservoir. The applicator of claim 1 .
4. the applicator slot having a flow axis along which the solution flows during use of the applicator; the force balanced reservoir having a general flow axis along which the solution flows within the force balanced reservoir during use of the applicator; The flow axis of the application slot is oblique to the total flow axis of the force balance reservoir. The applicator of claim 1 .
5. the applicator slot having a flow axis along which the solution flows during use of the applicator; the force balanced reservoir having a general flow axis along which the solution flows within the force balanced reservoir during use of the applicator; the flow axis of the application slot forms an angle φ with respect to the total flow axis of the force balanced reservoir; The wetting features are positioned as a function of the angle φ. The applicator of claim 1 .
6. The applicator is designed and configured such that both the force balanced reservoir and the slot opening are open to the ambient atmosphere surrounding the applicator during use. The applicator of claim 1 .
7. The force-balancing reservoir is configured as an open channel having a bottom wall, and the wetting feature is disposed on the bottom wall. The applicator of claim 1 .
8. a transparent closure removably engaged with the open passageway and allowing a user to view the contents of the force balanced reservoir.
8. The applicator of claim 7.
9. The wetting feature is provided as an insert structure that is inserted into the force-balancing reservoir. The applicator of claim 1 .
10. The wetting features have a total volume that defines the volume of the force balance reservoir. The applicator of claim 1 .
11. The wetting features include interconnected apertures. The applicator of claim 1 .
12. The wetting feature comprises a columnar structure within the force-balancing reservoir. The applicator of claim 1 .
13. The wetting feature includes a plurality of open channels. The applicator of claim 1 .
14. The moistening function includes a plurality of blocked passages. The applicator of claim 1 .
15. The wetting feature has a hydrophilic surface that is arranged to contact the solution during use. The applicator of claim 1 .
16. 1. A method for printing features on a substrate using a precursor solution comprising a deposition material dissolved in a solvent, the method comprising: Each feature has an in-plane dimension and an in-plane shape and is comprised of the depositable material after the solvent has left the feature, and the method comprises: providing a substrate having a printed area including a plurality of functional areas surrounded by non-functional areas; The method has a printing direction along the substrate; The printing area has a width perpendicular to the printing direction, the functional region defines a location of the crystalline feature; the functional areas are spaced apart from one another along the printing direction and perpendicular to the printing direction; each functional area having a hydrophilic surface that is hydrophilic with respect to said precursor solution and that is sized and shaped to conform to the in-plane dimensions and in-plane shape, respectively, of said corresponding crystalline feature; each functional region is defined by a plurality of functional boundaries formed between the hydrophilic surface and a hydrophobic surface surrounding the hydrophilic surface and which is hydrophobic with respect to the precursor solution; and moving a meniscus of the precursor solution along the printing direction in contact with the print area across a width of the print area to deposit a portion of the solution on the hydrophilic surfaces of the functional area and to prevent any of the solution from depositing on the hydrophobic surfaces. method.
17. Moving the meniscus includes moving the meniscus force balanced applicator relative to the substrate, moving the substrate relative to the meniscus force balanced applicator, or moving both the meniscus force balanced applicator and the substrate relative to each other.
17. The method of claim 16.
18. The method of claim 17 , wherein the meniscus force balanced applicator has a solution delivery slot that extends across the entire width of the print area.
19. Moving the meniscus includes using a dip coating process.
20. The method of claim 18.
20. The deposit material is a crystalline material.
17. The method of claim 16.
21. The crystalline material is an organic semiconductor material.
21. The method of claim 20.
22. The crystalline material is a hybrid organic-inorganic semiconductor material.
21. The method of claim 20.
23. The meniscus is moved to cause lateral crystal growth contact lines to form on each hydrophilic surface and not form on the hydrophobic surface.
21. The method of claim 20.
24. Any of said functional areas has a maximum dimension of 20 microns or less 17. The method of claim 16.
25. and generating the functional areas using a hydrophobic mask to generate the non-functional areas in the printed areas.
17. The method of claim 16.
26. generating the functional area using a template sheet that is temporarily applied to the print area.
17. The method of claim 16.