Coated steel sheet with excellent corrosion resistance and surface appearance and its manufacturing method

A Zn-Mg-Al plated steel sheet with controlled Mg and Al ratios and precise manufacturing processes achieves improved corrosion resistance and surface appearance by optimizing crystal formation, addressing unevenness and spangle issues.

JP2024539571AInactive Publication Date: 2024-10-29POHANG IRON & STEEL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024519266
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-28
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing Zn-Mg-Al zinc alloy plated steel sheets face issues with uneven surface appearance, poor image clarity after painting, and reduced corrosion resistance due to excessive Mg and Al content, leading to spangle formation and decreased adhesion.

Method used

A plated steel sheet with a Zn-Mg-Al based plating layer containing specific ratios of Mg and Al, controlled through X-ray diffraction intensities of crystal peaks, is manufactured using a precise hot-dip galvanizing process with controlled cooling rates and inert gas wiping to optimize crystal formation and surface appearance.

Benefits of technology

The solution results in a plated steel sheet with enhanced corrosion resistance, improved surface appearance, and sharpness after coating, addressing the limitations of conventional Zn-Mg-Al zinc alloy plated steel sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539571000001_ABST
    Figure 2024539571000001_ABST
Patent Text Reader

Abstract

The present invention provides a Zn-Mg-Al plated steel sheet which is excellent in corrosion resistance and at least one of weldability and chemical conversion treatability, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a highly corrosion-resistant plated steel sheet having excellent corrosion resistance and surface appearance, and a method for producing the same. [Background technology]

[0002] When exposed to a corrosive environment, zinc-based plated steel sheets have a sacrificial corrosion protection property in which zinc, which has a lower redox potential than iron, corrodes first, suppressing the corrosion of the steel material. In addition, as the zinc in the plated layer oxidizes, it forms a dense corrosion product on the surface of the steel material, insulating the steel material from the oxidizing atmosphere and improving the corrosion resistance of the steel material. Due to these advantageous properties, the range of applications of zinc-based plated steel sheets has recently expanded to building materials, home appliances, and automotive steel sheets.

[0003] However, the corrosive environment is gradually worsening due to increased air pollution accompanying industrial advancement, and strict regulations on resources and energy conservation are creating a growing need for the development of steel materials with superior corrosion resistance to conventional galvanized steel materials.

[0004] In order to solve these problems, various researches are being conducted on the manufacturing technology of zinc alloy-coated steel sheets that improve the corrosion resistance of steel materials by adding elements such as aluminum (Al) and magnesium (Mg) to the zinc plating bath. A representative example is Zn-Mg-Al zinc alloy-coated steel sheets, which further add Mg to the Zn-Al plating composition.

[0005] However, Zn-Mg-Al zinc alloy plated steel sheets are often used after processing, but the surface of the plated layer is uneven and has high roughness, which results in poor image clarity after painting.

[0006] In addition, Zn-Mg-Al zinc alloy plated steel sheets are prone to spangle formation during slow cooling, which results in an unattractive surface appearance.

[0007] Therefore, no technology has been developed to meet the high-end demands for excellent corrosion resistance, clarity after painting, and surface appearance. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Korean Patent Publication No. 2010-0073819 Summary of the Invention [Problem to be solved by the invention]

[0009] According to one aspect of the present invention, there is provided a plated steel sheet having excellent corrosion resistance and surface appearance, and a method for producing the same.

[0010] According to another aspect of the present invention, there are provided a plated steel sheet which is excellent in all respects in corrosion resistance, surface appearance and image clarity after painting, and a method for producing the same.

[0011] The object of the present invention is not limited to the above. Anyone having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding additional objects of the invention from the entire contents of the specification of the present invention. [Means for solving the problem]

[0012] One aspect of the present invention is Base steel sheet; and a Zn-Mg-Al-based coating layer provided on at least one surface of the base steel sheet; The plating layer contains, by weight percent, 4.0 to 6.3% Mg, 11.0 to 19.5% Al, the balance being Zn and other unavoidable impurities, A plated steel sheet is provided that satisfies the following relational expression 1. [Equation 1] 0.1≦I (110) / I (103) ≦0.25 (In the above Relational Formula 1, the above I (110)indicates the integrated X-ray diffraction intensity of the crystal peak of the (110) plane of the MgZn2 phase, and the above I (103) indicates the integrated X-ray diffraction intensity of the (103) crystal plane of the MgZn2 phase.

[0013] Another aspect of the present invention is Plating bath temperature (T B ) for T B -10℃~T B A step of immersing the base steel sheet in a coating bath containing, by weight%, 4.0 to 6.3% Mg, 11.0 to 19.5% Al, the balance being Zn and other unavoidable impurities, to hot-dip galvanize the base steel sheet so as to satisfy a drawing temperature of -40°C; supplying an inert gas cooled to 1 to 20°C to the hot-dip galvanized steel sheet to perform air wiping; cooling the air-wiped steel sheet to 420° C. at an average cooling rate of 10 to 15° C. / s; and Secondarily cooling the primarily cooled steel sheet at a temperature range of 300°C or more but less than 420°C at an average cooling rate of 5 to 8°C / s; The present invention provides a method for producing a plated steel sheet, which satisfies the following relational expression 2. [Equation 2] W air ×(1-T / T o )+5≦P air (In the above Relational Formula 2, the above W air represents the distance between the air knives, in mm. air represents the pressure of the air knife in kPa. T represents the temperature of the supplied inert gas in °C. o represents the average temperature of the atmosphere, assumed to be 25°C.) Effect of the Invention

[0014] According to one aspect of the present invention, there is provided a plated steel sheet having excellent corrosion resistance and surface appearance, and a method for producing the same.

[0015] According to another aspect of the present invention, there can be provided a plated steel sheet which is excellent in all of corrosion resistance, surface appearance and image clarity after painting, and a method for producing the same.

[0016] The various yet significant advantages and effects of the present invention are not limited to the above, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0017] [Figure 1] 1 is a graph showing X-ray diffraction peaks versus X-ray diffraction angle (2θ) measured by X-ray diffraction (hereinafter, referred to as "XRD") on the surface of the plating layer for the plated steel sheets obtained in Example 8 and Comparative Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The terms used in this specification are for the purpose of describing particular embodiments and are not intended to limit the present invention. Furthermore, the singular forms used in this specification also include the plural forms unless the relevant definition clearly indicates otherwise.

[0019] The meaning of "comprise" as used in the specification is to specify a feature and does not exclude the presence or addition of other features.

[0020] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. Dictionary-defined terms are to be interpreted as having a meaning consistent with the relevant technical literature and the presently disclosed content.

[0021] Hereinafter, a "plated steel sheet" according to one aspect of the present invention will be described in detail. In the present invention, the content of each element is expressed in percent by weight unless otherwise specified.

[0022] In conventional technology related to Zn-Mg-Al zinc alloy plated steel sheets, magnesium is added to improve corrosion resistance. However, if too much magnesium is added, there is a problem that more dross is generated floating in the plating bath, and the dross must be removed frequently. Therefore, the upper limit of the amount of magnesium that can be added is limited to 3%.

[0023] Therefore, research was conducted to further improve corrosion resistance by increasing the amount of Mg added beyond 3%, but as the amount of Mg and Al added increased, there was a problem that the roughness increased due to non-uniformity between the phases, making it difficult to ensure clear reflection after painting.

[0024] In addition to the problem of poor image clarity after painting, Zn-Mg-Al zinc alloy plated steel sheets have problems with the surface appearance being unattractive due to the generation of spangles caused by accelerated crystal growth during slow cooling during the manufacturing process, limiting their application to home appliances and automobiles.

[0025] Therefore, with the conventional techniques, it has been technically difficult to provide a plated steel sheet which not only ensures corrosion resistance but also has excellent image clarity and surface appearance after painting.

[0026] Therefore, the present inventors conducted extensive research in order to solve the above-mentioned problems and at the same time provide a plated steel sheet that is excellent not only in corrosion resistance but also in image clarity and / or surface appearance after painting. As a result, the inventors discovered that an important factor is not only the composition of the plating layer, but also controlling within a specific range the ratio of the X-ray diffraction integrated intensity of the crystal peak of the (110) plane of the MgZn2 phase, obtained by analyzing the surface of the plating layer by XRD, to the X-ray diffraction integrated intensity of the crystal of the (103) plane of the MgZn2 phase, and thus completed the present invention.

[0027] Therefore, the following will specifically describe the configuration of a plated steel sheet that has excellent corrosion resistance and, at the same time, excellent image clarity and / or surface appearance after painting.

[0028] First, the plated steel sheet according to the present invention includes a base steel sheet; and a Zn-Mg-Al-based plating layer provided on at least one surface of the base steel sheet.

[0029] In the present invention, the type of base steel sheet is not particularly limited. For example, the base steel sheet may be an Fe-based base steel sheet used as a base steel sheet for ordinary zinc-based plated steel sheets, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet, but is not limited thereto. Alternatively, the base steel sheet may be, for example, a carbon steel, an extra-low carbon steel, or a high manganese steel used as a material for construction, home appliances, or automobiles.

[0030] However, as an example, the above-mentioned base steel sheet has, by weight%, C: more than 0% (more preferably, 0.001% or more) and 0.18% or less, Si: more than 0% (more preferably, 0.001% or more) and 1.5% or less, Mn: 0.01 to 2.7%, P: more than 0% (more preferably, 0.001% or more) and 0.07% or less, S: more than 0% (more preferably, 0.001% or more) and 0.015% or less, Al: more than 0% (more preferably, It may have a composition including: Nb: more than 0% (more preferably, 0.001% or more) and 0.06% or less, Cr: more than 0% (more preferably, 0.001% or more) and 1.1% or less, Ti: more than 0% (more preferably, 0.001% or more) and 0.06% or less, B: more than 0% (more preferably, 0.001% or more) and 0.03% or less, and the balance being Fe and other unavoidable impurities.

[0031] Although not particularly limited, according to one embodiment of the present invention, at least one surface of the base steel sheet may be provided with a Zn-Mg-Al-based plating layer made of a Zn-Mg-Al-based alloy. The plating layer may be formed on only one surface of the base steel sheet, or may be formed on both surfaces of the base steel sheet. In this case, the Zn-Mg-Al-based plating layer refers to a plating layer that contains Mg and Al and mainly contains Zn (i.e., contains 50% or more Zn).

[0032] Although not particularly limited, according to one embodiment of the present invention, the thickness of the Zn-Mg-Al-based coating layer may be 5 to 100 μm, and more preferably 7 to 90 μm. If the thickness of the coating layer is less than 5 μm, the coating layer may become very thin locally due to an error caused by the thickness deviation of the coating layer, and the corrosion resistance may be poor. If the thickness of the coating layer exceeds 100 μm, the cooling of the hot-dip coating layer may be delayed, and there may be a possibility of solidification defects occurring on the surface of the coating layer, such as a sagging shape, and the productivity of the steel sheet may decrease due to solidification of the coating layer.

[0033] Meanwhile, although not particularly limited, according to an embodiment of the present invention, an Fe-Al-based inhibition layer may be further included between the base steel sheet and the Zn-Mg-Al-based coating layer. The Fe-Al-based inhibition layer is a layer mainly containing (for example, 60% or more) an intermetallic compound of Fe and Al, and examples of the intermetallic compound of Fe and Al include FeAl, FeAl3, Fe2Al5, etc. In addition, a component derived from the coating layer such as Zn, Mg, etc. may be further included, for example, 40% or less. The inhibition layer is a layer formed by alloying Fe diffused from the initial coating base steel sheet and coating bath components. The inhibition layer can play a role in improving the adhesion between the base steel sheet and the coating layer, and at the same time, can play a role in preventing Fe diffusion from the base steel sheet to the coating layer. In this case, the inhibition layer can be formed continuously or discontinuously between the base steel sheet and the Zn-Mg-Al-based coating layer. With respect to the inhibition layer, except for the above description, contents commonly known in the art can be similarly applied.

[0034] Although not particularly limited, according to one embodiment of the present invention, the thickness of the inhibition layer may be 0.1 to 1 μm. The inhibition layer prevents alloying and ensures corrosion resistance, but since it is brittle, it may affect workability, and in the present invention, the thickness of the inhibition layer may be 1 μm or less. However, in order to function as an inhibition layer, the thickness may be 0.1 μm or more. From the viewpoint of further improving the above-mentioned effects, preferably, the upper limit of the inhibition layer thickness may be 1.00 μm, or the lower limit of the inhibition layer thickness may be 0.15 μm.

[0035] In this case, the thickness of the inhibition layer may refer to the minimum thickness of the inhibition layer in the thickness direction when a cross-sectional specimen is prepared by cutting the plated steel sheet in the thickness direction (i.e., the direction perpendicular to the rolling direction) and then photographing the cross-section with a scanning electron microscope (hereinafter referred to as "SEM").

[0036] According to the present invention, the plating layer contains, by weight, 4.0-6.3% Mg, 11.0-19.5% Al, and the balance being Zn and other inevitable impurities. The reasons for adding each component and limiting the content thereof will be specifically described below.

[0037] Mg: 4.0% or more and 6.3% or less Mg is an element that plays a role in improving the corrosion resistance of plated steel materials, and in the present invention, the Mg content in the plated layer is controlled to 4.0% or more in order to ensure the desired excellent corrosion resistance. On the other hand, if Mg is added excessively, dross may be generated, so the Mg content can be controlled to 6.3% or less.

[0038] Al: 11.0% or more and 19.5% or less Generally, when Mg is added at 1% or more, it is effective in improving corrosion resistance. However, when Mg is added at 2% or more, the oxidation of Mg in the plating bath increases the generation of floating dross in the plating bath, which requires frequent removal of the dross.

[0039] Due to these problems, in the conventional technology, Zn-Mg-Al zinc alloy plating is added with 1.0% or more of Mg to ensure corrosion resistance, but the upper limit of the Mg content is set at 3.0% in common use.

[0040] However, in the present invention, in order to further improve the corrosion resistance, it is necessary to increase the Mg content to 4% or more. However, if the coating layer contains Mg at 4% or more, there is a problem that dross is generated due to oxidation of Mg in the coating bath, so it is necessary to add Al at 11.0% or more.

[0041] However, if excessive Al is added to suppress dross, the melting point of the coating bath becomes high, and the resulting operating temperature becomes too high, which can cause problems due to high-temperature work such as erosion of the coating bath structure and denaturation of the steel material. In addition, if the Al content in the coating bath is excessive, Al reacts with Fe in the base steel sheet and does not contribute to the formation of an Fe-Al inhibition layer, but instead the reaction between Al and Zn occurs rapidly, causing excessive formation of a lumpy outburst phase, which can actually worsen corrosion resistance. Therefore, it is preferable to control the upper limit of the Al content in the coating layer to 19.5%.

[0042] The balance is Zn and other unavoidable impurities. In addition to the above-mentioned composition of the coating layer, the balance may be Zn and other inevitable impurities. The inevitable impurities may include all impurities that are unintentionally mixed in the normal manufacturing process of hot-dip galvanized steel sheets, and the meaning thereof can be easily understood by a person skilled in the art.

[0043] On the other hand, according to the present invention, the above-mentioned plated steel sheet preferably satisfies the following relational expression 1 in order to ensure corrosion resistance and at the same time the desired level of excellent image clarity and beautiful surface appearance after painting. [Equation 1] 0.1≦I (110) / I (103) ≦0.25 (In the above Relational Formula 1, the above I (110)indicates the integrated X-ray diffraction intensity of the crystal peak of the (110) plane of the MgZn2 phase, and the above I (103) indicates the integrated X-ray diffraction intensity of the (103) crystal plane of the MgZn2 phase.

[0044] The inventors have found that the ratio of MgZn2 phase (110) crystal planes and MgZn2 phase (103) crystal planes in the plating layer is an important factor in ensuring excellent image clarity and beautiful surface appearance after painting. That is, by controlling the ratio of the X-ray diffraction integrated intensity of the crystal peak of the MgZn2 phase (110) plane obtained by XRD analysis of the surface of the plating layer to the X-ray diffraction integrated intensity of the crystal peak of the MgZn2 phase (103) plane, so as to satisfy the above-mentioned relational expression 1, it is possible to not only ensure excellent corrosion resistance, but also improve the image clarity and surface appearance after painting.

[0045] Specifically, in the present invention, when there are many crystals on the (103) plane of the MgZn2 phase, this means that there are many areas where crystals have formed in the vertical direction, which prevents the crystals from growing laterally, thereby making it possible to suppress the formation of spangles.

[0046] However, in the component system according to the present invention, the (110) crystal plane of the MgZn2 phase and the (103) crystal plane of the MgZn2 phase, which affect the characteristics of the invention, are essential, and the characteristics of the image clarity and surface appearance after painting are determined by harmonizing these two types of crystal planes.

[0047] Therefore, I defined by the above relation 1 (110) / I (103) If the value is less than 0.1, crystal mismatch will be large, which may cause a problem of reduced adhesion of the plating layer. (110) / I (103)If the value exceeds 0.25, the ratio of MgZn2 phase (110) crystals to MgZn2 phase (103) crystals is excessive, which may result in insufficient sharpness and surface appearance after painting. During quenching, the MgZn2 phase (110) crystals exist at the bottom of the plating layer, promoting the formation of Zn phase (002) crystals upward in the plating layer, and the contact with the MgZn2 phase (103) crystals makes the surface beautiful.

[0048] That is, while the (110) plane crystals of the MgZn2 phase and the (103) plane crystals of the MgZn2 phase are mixed to satisfy the above-mentioned Relational Formula 1, there are more (103) plane crystals of the MgZn2 phase, which have a smaller interplanar spacing than the (002) plane crystals of the Zn phase, in preparation for the (110) plane crystals of the MgZn2 phase. As a result, the addition of Mg improves the corrosion resistance compared to conventional techniques, and at the same time, it is possible to ensure a plated steel sheet having small surface roughness and a beautiful surface appearance.

[0049] Meanwhile, although not particularly limited, according to one embodiment of the present invention, in order to further maximize the above-mentioned effects, it is more preferable that I defined by the above Relation 1 be used. (110) / I (103) The lower limit of the value can be 0.11, or the above I (110) / I (103) The upper limit of the value can be 0.15.

[0050] In this case, the crystal peak of the (110) plane of the MgZn2 phase and the crystal peak of the (103) plane of the MgZn2 phase can be distinguished from the crystal peak of the (110) plane and the crystal peak of the (103) plane by a method known in the art from the X-ray diffraction integrated intensity obtained by analyzing the surface of the coating layer by XRD, and therefore will not be separately defined in this specification.

[0051] Meanwhile, the method for measuring the X-ray diffraction integrated intensity is not particularly limited, and any method known in the art can be applied. For example, the surface of the plating layer can be analyzed by XRD to measure the X-ray diffraction integrated intensity. A RINT2000 diffractometer can be used as an apparatus for measuring the X-ray diffraction integrated intensity. The measurement conditions for the X-ray diffraction integrated intensity are a Cu target, voltage: 40 kV, current: 200 mA, and the X-ray diffraction angle (2θ) can be measured from 10 to 100°. As a representative example, when a Cu target is used, the above I (110) can be defined as the integrated intensity of the peak between 2θ = 34.0° and 34.6°, and the above I (103) can be defined as the integrated intensity of the peak between 2θ=37.0° and 37.5°. However, when the target material is different, such as Mo, the value of 2θ varies depending on the type of target material, and therefore the range of 2θ is not particularly limited in the present invention.

[0052] In this specification, the MgZn2 crystal having the (110) plane means a structure in which the (110) plane is present in the hexagonal crystal of the MgZn2 phase on the steel sheet surface, and the MgZn2 crystal having the (103) plane means a structure in which the (103) plane is present in the hexagonal crystal of the MgZn2 phase on the steel sheet surface.

[0053] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the plated steel sheet may be selectively subjected to the above-mentioned I (110) The value of I above can be 85 or less. (110) By satisfying a value of 85 or less, it is possible to increase the proportion of MgZn2 phase (103) crystals relative to the MgZn2 phase (110) crystals within the range that satisfies Relational Formula 1. This makes it possible to suppress the formation of spangles in the plating layer and further increase the influence of the MgZn2 phase (103) crystals, which contribute to ensuring the characteristics of a beautiful surface appearance.

[0054] Therefore, from the viewpoint of maximizing the above-mentioned effects, it is more preferable to use the above-mentioned I (110) The upper limit of the value of may be 80, or (110) The lower limit of the value may be 50.

[0055] Alternatively, although not particularly limited, according to one embodiment of the present invention, the plated steel sheet may be selectively (103) The value of I above can be 525 or more. (103) By satisfying a value of 525 or more, it is possible to increase the proportion of MgZn2 phase (103) crystals relative to the MgZn2 phase (110) crystals within the range that satisfies Relational Formula 1. This makes it possible to suppress the formation of spangles in the plating layer and further improve the effect of the MgZn2 phase (103) crystals, which contribute to ensuring the characteristics of a beautiful surface appearance.

[0056] Therefore, from the viewpoint of maximizing the above-mentioned effects, it is more preferable to use the above-mentioned I (103) The lower limit of the value of may be 530, or the above I (103) The upper limit for the value of can be 600.

[0057] At this time, although there is no particular limitation, the above I (110) The value of I (103) The values ​​are those measured using a RINT2000 diffractometer with a Cu target under the conditions of a voltage of 40 kV and a current of 200 mA.

[0058] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the surface roughness of the plated steel sheet may selectively satisfy the ranges of Ra: 0.3 to 0.6 μm and Rpc: 40 to 90 ( / 10 mm). By adjusting the surface roughness of the plated steel sheet to be small so as to satisfy the above-mentioned ranges, the effect of suppressing spangle formation can be further improved, and more beautiful surface appearance characteristics can be secured.

[0059] Next, a "method for producing a plated steel sheet" according to another aspect of the present invention will be described in detail. However, this does not necessarily mean that the plated steel sheet of the present invention must be produced by the following production method.

[0060] According to an embodiment of the present invention, the method may further include a step of preparing a base steel sheet, and the type of the base steel sheet is not particularly limited. It may be an Fe-based base steel sheet used as a base steel sheet for a typical hot-dip galvanized steel sheet, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet, but is not limited thereto. In addition, the base steel sheet may be, for example, a carbon steel, an extra-low carbon steel, or a high manganese steel used as a material for construction, home appliances, and automobiles, but is not limited thereto. In this case, the above description may be similarly applied to the base steel sheet.

[0061] Next, the prepared base steel sheet is immersed in a coating bath containing, by weight, 4.0 to 6.3% Mg, 11.0 to 19.5% Al, the balance being Zn and other unavoidable impurities, to perform hot-dip galvanizing.

[0062] In this case, the reasons for adding the components and the reasons for limiting the contents in the above-mentioned coating bath can be similarly applied to the explanation for the components of the coating layer described above, except for the small amount of Fe content that can flow in from the base steel sheet.

[0063] Meanwhile, in order to prepare the coating bath having the above composition, a composite ingot containing the desired Zn, Al, and Mg or a Zn-Mg or Zn-Al ingot containing individual components can be used. In order to replenish the coating bath consumed in hot dip coating, the ingot is melted and supplied. In this case, a method of directly immersing the ingot in the coating bath and melting it can be selected, or a method of melting the ingot in a separate port and then replenishing the molten metal to the coating bath can be selected.

[0064] According to the present invention, during the hot dip galvanizing, the drawing temperature of the base steel sheet is set to be equal to or lower than the plating bath temperature (T B) for T B -10℃~T B The drawing temperature of the above base steel sheet is controlled to satisfy the drawing temperature of -40℃. B If the temperature is less than -10°C, the crystal phase is not dense, and the drawing temperature of the base steel sheet is T B If the temperature exceeds -40°C, problems will occur with the plating adhesion.

[0065] At this time, although not particularly limited, the above-mentioned plating bath temperature (T B ) may be in the range of 440 to 500°C. On the other hand, more preferably, the plating bath temperature (T B The lower limit of the plating bath temperature (T B ) may be 490°C.

[0066] Next, the hot-dip galvanized steel sheet is air-wiped by supplying an inert gas cooled to 1 to 20° C. As a result of intensive research, the present inventors have found that, unlike conventional methods, air wiping is performed by supplying an inert gas cooled to a specific temperature range, which has the effect of rapidly cooling the steel sheet without the problem of surface oxidation.

[0067] That is, if the temperature of the inert gas supplied during the air wiping is less than 1° C., a problem of water droplets adhering to peripheral devices may occur, resulting in uneven wiping. On the other hand, if the temperature of the inert gas supplied during the air wiping exceeds 20° C., a problem of a decrease in the effect of rapid cooling may occur, resulting in a failure to form a beautiful surface appearance. From the viewpoint of maximizing the above-mentioned effects, more preferably, the lower limit of the temperature of the nitrogen gas supplied during the air wiping may be 1.0° C., or the upper limit of the temperature of the nitrogen gas supplied during the air wiping may be 5.0° C.

[0068] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the inert gas may be argon (Ar) gas, nitrogen (N2) gas, or a mixture of argon and nitrogen gas, and it is more preferable to use nitrogen gas.

[0069] Further, according to the present invention, the air wiping is controlled so as to satisfy the following relational expression 2. By controlling the air wiping conditions so as to satisfy the following relational expression 2, the formation ratio of MgZn2 phase (110) crystals and MgZn2 phase (103) crystals can be optimized. In addition, it is possible to ensure beautiful roughness characteristics in which the surface shows a milky white color, thereby achieving the effect of making the surface appearance very smooth. In this case, since the following relational expression 2 is an empirically obtained value, no particular unit can be specified, and it can be expressed by the following defined W air The unit of is mm and P air The units of kPa, T and T o It is sufficient to meet the unit of °C. [Equation 2] W air ×(1-T / T o )+5≦P air (In the above Relational Formula 2, the above W air represents the distance between the air knives, in mm. air represents the pressure of the air knife in kPa. T represents the temperature of the supplied inert gas in °C. o represents the average temperature of the atmosphere, assumed to be 25°C.)

[0070] Furthermore, although not particularly limited, according to one embodiment of the present invention, in the air wiping step, the gap between the air knives may be in the range of 10 to 30 mm (more preferably 10 to 20 mm). Alternatively, the pressure of the air knives may be in the range of 5 to 30 kPa (more preferably 15 to 23 kPa). Alternatively, the temperature of the supplied gas may be in the range of 1 to 20° C. (more preferably 1 to 5° C.). By adjusting the air wiping conditions so as to satisfy the above-mentioned ranges, a plated steel sheet having excellent corrosion resistance, clearness after painting, and surface appearance can be effectively manufactured.

[0071] According to the present invention, after the air wiping step, the air wiped steel sheet is primarily cooled to 420° C. at an average cooling rate of 10-15° C. / s, and then the primarily cooled steel sheet is secondary cooled at an average cooling rate of 5-8° C. / s in a temperature range of less than 420° C. and not less than 300° C. Here, the average cooling rate is based on the surface temperature of the steel sheet.

[0072] As a result of extensive research, the inventors have found that by precisely controlling the cooling rate in two stages while performing rapid cooling during the primary cooling, it is possible to further optimize the formation ratio of crystals on the (110) plane of the MgZn2 phase and crystals on the (103) plane of the MgZn2 phase, thereby further improving the characteristics of the surface appearance, while also ensuring the effect of obtaining a uniform surface structure in the width direction of the steel sheet.

[0073] That is, if the average cooling rate during the primary cooling is less than 10.0°C / s, the effect of quenching may be weak, and if the average cooling rate during the primary cooling exceeds 15.0°C / s, the surface may become uneven in the width direction of the steel sheet. Also, if the average cooling rate during the secondary cooling is less than 5.0°C / s, the surface roughness may increase, and if the average cooling rate during the secondary cooling exceeds 8.0°C / s, the surface may become uneven in the width direction of the steel sheet.

[0074] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the cooling conditions may be selectively controlled during the cooling so as to satisfy the following Relational Expressions 3 and 4. By controlling the relationship between the average cooling rates during the primary cooling and secondary cooling to satisfy the following Relational Expressions 3 and 4, it is possible to further suppress the formation of spangles in the plated steel sheet and further improve the appearance characteristics. In this regard, since the following Relational Expressions 3 and 4 are values ​​obtained empirically, no particular units may be determined, and it is sufficient that the units C1 and C2 defined below are satisfied. [Equation 3] 17≦C1+C2 [Equation 4] 5≦C1-C2≦10 (In the above Relational Formula 3, C1 indicates the average cooling rate [°C / s] during the first cooling, and C2 indicates the average cooling rate [°C / s] during the second cooling.)

[0075] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the surface roughness of the plated steel sheet obtained by the secondary cooling can be selectively controlled to the ranges of Ra: 0.3 to 0.6 μm and Rpc: 40 to 90 ( / 10 mm). By controlling the surface roughness Ra and Rpc of the plated steel sheet to satisfy the above ranges, it is possible to ensure the effect of a very beautiful surface and excellent appearance.

[0076] As described above, by precisely controlling the plating composition and manufacturing conditions, it is possible to effectively provide a plated steel sheet that is excellent not only in corrosion resistance but also in bendability and surface appearance. EXAMPLES

[0077] (Example) The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are for illustrative purposes only and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.

[0078] A base steel sheet having a thickness of 1.5 mm and a width of 1200 mm and having a composition of C: 0.018%, Si: 0.01%, Mn: 0.2%, P: 0.009%, S: 0.005%, Al: 0.1%, Nb: 0.02%, Cr: 0.2%, Ti: 0.02%, B: 0.015%, the balance being Fe and impurities, was prepared. The base steel sheet prepared above was immersed in a coating bath under the conditions in Table 1 below to perform hot-dip galvanizing.

[0079] Next, the hot-dip galvanized steel sheet was subjected to an air wiping treatment using nitrogen (N2) gas under the conditions shown in Table 1 below, and then subjected to primary cooling and secondary cooling under the conditions shown in Table 2 below. Thereafter, the steel sheet obtained by the secondary cooling was controlled so as to satisfy the surface roughness shown in Table 2 below.

[0080] [Table 1]

[0081] [Table 2]

[0082] Test pieces of the plated steel sheets obtained by the methods in Tables 1 and 2 above were prepared, and the plated layers were dissolved in a hydrochloric acid solution. The dissolved liquid was then analyzed by a wet analysis (ICP) method to determine the compositions of the plated layers, which are shown in Table 3 below (the remainder corresponds to Zn and impurities).

[0083] In addition, cross-sectional test pieces were prepared by cutting the steel sheet in a direction perpendicular to the rolling direction so that the interface between the coating layer and the base steel could be observed, and photographed with an SEM to confirm that an Fe-Al-based inhibitor layer was formed between the base steel sheet and the Zn-Mg-Al-based coating layer. The thickness of the Fe-Al-based inhibitor layer was measured in a direction perpendicular to the rolling direction of the steel sheet using the SEM, and is shown in Table 3 below.

[0084] In addition, to measure the X-ray diffraction integral intensity of the plating layer, a RINT2000 diffractometer was used to measure the diffraction peaks MgZn2(110) and MgZn2(103) at 2θ=34.0°-38.0° under the conditions of voltage: 40 kV, current: 200 mA with a Cu target, and the integral intensity of the corresponding peaks was calculated. (110) is the value obtained by integrating the peak from 34° to 34.6°, and the integrated intensity I (103) is a value obtained by integrating the peak at 37° to 37.5° (the unit is integrated intensity, which corresponds to cps*2θ), and is shown in Table 3 below.

[0085] [Table 3]

[0086] The characteristics of each of the invention examples and comparative examples were evaluated according to the following criteria, and the evaluation results of each characteristic are shown in Table 4 below.

[0087] <Corrosion resistance> In order to evaluate the corrosion resistance, a salt spray tester (SST) was used in accordance with the test method of ISO14993, and the evaluation was performed according to the following criteria. ○: The time it takes for red rust to appear is 30 to 40 times longer than that of Zn plating of the same thickness. △: The time it takes for red rust to appear is 20 to 30 times longer than that of Zn plating of the same thickness. ×: The time it takes for red rust to appear is less than 20 times longer than that for Zn plating of the same thickness.

[0088] <Image clarity after painting> To evaluate the image clarity after painting, the material in question was cut to 75 mm x 150 mm, the steel plate was degreased and phosphate treated, then electrocoated, and the Wsa (image clarity index) (μm) value was measured. ○:Wsa0.35 or less △: Wsa 0.36 or more and 0.40 or less ×: Wsa0.41 or higher

[0089] <With or without spangles> To evaluate the size of the spangles, an image was taken at 100x magnification using an optical microscope, and the size of the spangles was measured on both the vertical and horizontal axes, and then the average of 10 spangles was taken and evaluated according to the following criteria. ◎: No spangles observed ○: Spangle size (0.1~0.29mm) △: Size of spangles (0.3~0.5mm) ×: Size of spangles (0.5mm or more)

[0090] [Table 4]

[0091] As can be seen from the experimental results in Table 4 above, in the case of Invention Examples 1 to 9, which satisfy the plating composition and manufacturing conditions specified in the present invention, it was confirmed that the corrosion resistance, image clarity after painting, and appearance characteristics are all excellent.

[0092] In particular, among the above-mentioned invention examples, it was confirmed that in the case of invention examples 7 to 9, which satisfy the cooling rates of the relational expressions 3 and 4 defined in the present invention, the surface appearance was more excellent than that of invention examples 1 to 6. This is presumably due to the fact that an appropriate ratio of MgZn2 phase (110) plane crystals and MgZn2 phase (103) plane crystals are formed around the Zn phase (002) plane crystals, while at the same time the presence ratio of MgZn2 phase (103) plane crystals, which greatly contributes to the presence or absence of spangles, is further improved.

[0093] On the other hand, in the case of Comparative Examples 1 to 17, which do not satisfy all of the plating compositions and manufacturing conditions specified in the present invention, it was confirmed that one or more of the corrosion resistance, image clarity after painting, and appearance characteristics were deteriorated compared to Invention Examples 1 to 9.

Claims

1. Base steel sheet; and a Zn-Mg-Al-based plating layer provided on at least one surface of the base steel sheet; The plated steel sheet, wherein the plating layer satisfies the following Relational Expressions 1 and 2. [Relationship 1] -10.0≦[Zn] 1/10t -[Zn] s ≦-5.0 (In the above-mentioned relational formula 1, the [Zn] 1/10t represents the weight percent content of Zn at a 1 / 10t position (t is the total thickness of the plating layer) from the surface of the plating layer in the thickness direction, and the [Zn] s represents the weight percent Zn content on the surface of the plating layer.) [Relationship 2] <h2 style=";text-align:left;direction:ltr">+3.0≦[Al]<h2 style=";text-align:left;direction:ltr"> 1/10t <h2 style=";text-align:left;direction:ltr"> -[Al]<h2 style=";text-align:left;direction:ltr"> s <h2 style=";text-align:left;direction:ltr"> ≦+13.0 (In the above-mentioned Relational Formula 2, the above-mentioned [Al] 1/10t represents the weight percent content of Al at a 1 / 10t position (t is the total thickness of the plating layer) from the surface of the plating layer in the thickness direction, and the [Al] s represents the weight percent content of Al on the surface of the plating layer.)

2. The plated steel sheet according to claim 1, further comprising: an Fe-Al-based inhibiting layer provided between the base steel sheet and the Zn-Mg-Al-based plating layer.

3. The plated steel sheet according to claim 1, wherein the plating layer contains, by weight percent, 4.0 to 7.0% Mg, 8.2 to 19.5% Al, and the balance being Zn and other inevitable impurities.

4. The plated steel sheet according to claim 1 , further satisfying the following relational expression 3: [Relationship 3] -1.0≦[Mg] 1/10t -[Mg] s ≦+1.0 (In the above-mentioned Relational Formula 3, the above-mentioned [Mg] 1/10t represents the weight percent content of Mg at a position 1 / 10t from the surface of the plating layer in the thickness direction (t is the total thickness of the plating layer), and the [Mg] s represents the weight percent Mg content on the surface of the plating layer.)

5. 2. The plated steel sheet according to claim 1, wherein the Mg content by weight at a 2 / 3t position from the surface of the plating layer in the thickness direction satisfies ±0.5 wt% of the average Mg content by weight in the plating layer.

6. 2. The plated steel sheet according to claim 1, wherein an area ratio of an Al phase having a Zn solid solution rate of 27 atomic % or more on a surface of the plated layer is 2.0 to 10.1%.

7. performing a first shot blasting process by projecting metal balls having a grain size of 0.6 to 1.0 mm at 400 to 1200 kg / min onto the surface of the base steel sheet in a shot blasting cabin where metal material circulates at a rotation speed of 1200 to 2000 mpm; performing a secondary shot blasting process by projecting metal balls having a grain size of 0.2 to 0.5 mm at 400 to 1200 kg / min onto the surface of the base steel sheet in the shot blasting cabin where the metal material circulates at a rotation speed of 1200 to 2000 mpm; dipping the shot blasted steel sheet in a galvanizing bath containing, by weight, 4.0-7.0% Mg, 8.2-19.5% Al, the balance Zn and other inevitable impurities, and maintained at a temperature of Ts+20°C to Ts+80°C relative to the solidification start temperature (Ts) on the equilibrium diagram, to perform hot-dip galvanizing; and cooling the hot-dip galvanized steel sheet from a solidification start temperature to a solidification finish temperature at an average cooling rate of 2 to 8°C / s using an inert gas.

8. 8. The method for producing a plated steel sheet according to claim 7, further comprising the step of performing pre-temper rolling of the shot blasted base steel sheet by applying a roll reduction of 100 to 400 tons to a steel sheet surface using a dull roll having a surface roughness Ra of 1.8 to 2.8 μm, prior to the hot-dip galvanization.

Citation Information

Patent Citations

  • Hot dip zn-al-mg coated steel sheet excellent in corrosion resistance and external surface appearance, and its production

    JP1998306357A

  • Method for manufacturing hot-dip galvanized steel sheet with excellent press formability

    JP2002266062A

  • METHOD OF PRODUCING Zn-Al-Mg BASED ALLOY PLATED STEEL

    JP2004244650A

  • Hot dip galvanized steel sheet for heat treatment working having excellent phosphate treatability and post-painting corrosion resistance and method for manufacturing the same

    JP2006265706A

  • Plated steel material with excellent abrasion resistance and white rust resistance and its manufacturing method